Method for treating soft contact lens surfaces
A surface treatment agent for soft contact lenses, formed by reacting poly(meth)acrylic acid with a specific copolymer, addresses hydrophobicity and stability issues, enhancing hydrophilicity and comfort without compromising oxygen permeability.
Patent Information
- Application Number
- JP2021551686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-09
- Filing Date
- 2020-10-07
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-07
Smart Images

Figure 0007567803000001 
Figure 0007567803000002 
Figure 0007567803000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface treatment agent for soft contact lenses, which comprises a reactant obtained by reacting two different polymers having specific structures. [Background technology]
[0002] It is estimated that there are more than 10 million soft contact lens wearers in Japan, and the number of wearers has increased rapidly due to the ease and convenience of contact lenses. However, it has been reported that the ease and convenience of contact lenses has led to an increase in the length of time soft contact lens wear, particularly among younger generations (Non-Patent Document 1). The issues that arise from this increase in the length of time soft contact lens wear are the lack of oxygen to the cornea and the discomfort caused by wearing soft contact lenses. The supply of oxygen to the cornea can be increased by blending a material having a functional group with excellent oxygen permeability, such as a silicone monomer, into the material that constitutes the soft contact lens, and technological developments have been made regarding the blending formulation and manufacturing method of soft contact lenses with excellent oxygen permeability (Patent Document 1, etc.). However, silicone monomers with excellent oxygen permeability are extremely hydrophobic, and as a result, the soft contact lenses give a dry feeling, discomfort, etc. For this reason, technological developments have been made to hydrophilize the surface of silicone hydrogel contact lenses that contain silicone monomers.
[0003] As an example of these techniques, it is conceivable to blend a hydrophilic monomer having a carboxyl group, such as methacrylic acid or acrylic acid, into a silicone hydrogel contact lens. However, when a silicone monomer and a monomer having a carboxyl group are blended at the same time, the hydrolysis reaction of the polymer in the contact lens is accelerated, resulting in poor stability over time, and thus this has not yet been put to practical use. Another technique has been developed in which a copolymer having both a highly reactive functional group such as an amino group, an epoxy group, or a thiol group and a hydrophilic group is produced in advance, and a silicone hydrogel contact lens having a highly reactive functional group is chemically bonded to impart hydrophilicity to the contact lens surface (Patent Document 2). However, this technique requires highly controlled manufacturing equipment, which is economically disadvantageous, and there is also a concern that forming a hydrophilic layer on the contact lens surface may actually reduce oxygen permeability, so it cannot be said that it has been fully deployed in products. Thus, there has been a demand for the development of a surface treatment technique that can provide silicone hydrogel contact lenses that have good hydrophilicity and therefore excellent wearing comfort. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-115005 A [Patent Document 2] Special Publication No. 2012-508902 [Non-patent literature]
[0005] [Non-Patent Document 1] Walline JJ, 2013, Long-term Contact Lens Wear of Children and Teens, Eye & Contact Lens, 39, 283-289. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a soft contact lens that can dramatically improve the hydrophilicity of the surface of the soft contact lens and improve the discomfort of the soft contact lens. Table surface of process How to The purpose of this invention is to provide [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above problems, the inventors have discovered a technology for easily imparting extremely excellent surface hydrophilicity to the surface of a soft contact lens and reducing the feeling of dryness by using a surface treatment agent for a soft contact lens containing a reaction product obtained by reacting poly(meth)acrylic acid with a copolymer (P) having two different types of structural units in a specific ratio, and have completed the present invention. That is, the soft contact lens of the present invention Table surface of process How to That is as follows:
[0008] [1] A method for treating a surface of a soft contact lens, comprising reacting the following poly(meth)acrylic acid with a copolymer (P): Poly(meth)acrylic acid: Poly(meth)acrylic acid with an average molecular weight of 1,000 to 2,000,000 Copolymer (P): A hydrophilic monomer (n A ) and the reactive monomer (n B ) and a hydrophilic monomer (n A ) is 80 to 99 mol %, and the reactive monomer (n B ) is 1 to 20 mol % and the weight average molecular weight is 10,000 to 5,000,000. In formulas (1) and (2), X represents a hydrogen atom or a methyl group. [ka] [ka] [2] The soft contact lenses are silicone hydrogel contact lenses. In The method for treating the surface of a soft contact lens according to the above item [1]. Effect of the Invention
[0009] The soft contact lenses of the present invention Table surface of process How to By using this, it is possible to impart extremely excellent surface hydrophilicity, thereby reducing the dry feeling and discomfort. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The surface treatment agent for soft contact lenses of the present invention is a surface treatment agent for soft contact lenses that contains a reaction product obtained by reacting the poly(meth)acrylic acid shown below with a copolymer (P). Poly(meth)acrylic acid: Poly(meth)acrylic acid with an average molecular weight of 1,000 to 2,000,000 Copolymer (P): A hydrophilic monomer (n A ) and the reactive monomer (n B ) and a hydrophilic monomer (n A ) is 80 to 99 mol %, and the reactive monomer (n B ) is 1 to 20 mol % and the weight average molecular weight is 10,000 to 5,000,000. In formulas (1) and (2), X represents a hydrogen atom or a methyl group. [ka] [ka]
[0011] In this specification, "poly(meth)acrylic acid" means "polyacrylic acid or polymethacrylic acid", and the same applies to other similar terms. In addition, in this specification, when a preferred numerical range (e.g., a range of concentration or weight-average molecular weight) is described in stages, each lower limit and upper limit can be combined independently. For example, in the description "preferably 10 or more, more preferably 20 or more, and preferably 100 or less, more preferably 90 or less," "preferable lower limit: 10" and "more preferable upper limit: 90" can be combined to "10 or more and 90 or less." For example, in the description "preferably 10 to 100, more preferably 20 to 90," it can be similarly expressed as "10 to 90."
[0012] <Poly(meth)acrylic acid> Examples of the poly(meth)acrylic acid used in the production of the reactant contained in the surface treatment agent for soft contact lenses of the present invention include polyacrylic acid and polymethacrylic acid, and preferably polyacrylic acid. The average molecular weight of the poly(meth)acrylic acid used in the surface treatment agent for soft contact lenses of the present invention is 1,000 to 2,000,000, and preferably 5,000 to 1,000,000. Here, the above average molecular weight means the weight average molecular weight measured by gel permeation chromatography (GPC).
[0013] The copolymer (P) used for producing the reaction product contained in the surface treatment agent for soft contact lenses of the present invention is a hydrophilic monomer (n A ) and the reactive monomer (n B The copolymer (P) is obtained by polymerizing the hydrophilic monomer (n A ) is 80 to 99 mol %, and the reactive monomer (n B In particular, the hydrophilic monomer (n A ) is the hydrophilic monomer (n A ) in the copolymer (P), and the reactive monomer (n B ) is the reactive monomer (n BThe molar percentage of each of these structural units in the copolymer (P) can be adjusted by the charge ratio of each monomer. Therefore, the copolymer (P) is a structural unit based on a hydrophilic monomer (n A ) 80 to 99 mol % and a reactive monomer (n B ) 1 to 20 mol % is polymerized, and the weight average molecular weight is 10,000 to 5,000,000. [ka] [ka]
[0014] [Hydrophilic monomer (n A )] The copolymer (P) used in the present invention is a copolymer containing a hydrophilic monomer (n A ), that is, a monomer having a phosphorylcholine structure (hereinafter, simply referred to as "hydrophilic monomer (n A ) is also called ". The copolymer (P) has a hydrophilic monomer (n A ) imparts hydrophilicity to the copolymer (P), and can impart excellent hydrophilicity to the surface of a soft contact lens. Hydrophilic monomer (n A ) is 2-((meth)acryloyloxy)ethyl-2-(trimethylammonio)ethyl phosphate, and preferably 2-(methacryloyloxy)ethyl-2-(trimethylammonio)ethyl phosphate represented by formula (1') (hereinafter also referred to as "2-methacryloyloxyethyl phosphorylcholine"). [ka]
[0015] Hydrophilic monomer (n AThe content of the reactive monomer (n) represented by formula (2) is 80 to 99 mol %. If the content is less than 80 mol %, the effect of improving the hydrophilicity of the soft contact lens surface cannot be expected, and if the content is more than 99 mol %, the amount of the reactive monomer (n) represented by formula (2) is relatively small. B ) in the copolymer (P), and chemical bonding with the poly(meth)acrylic acid of the copolymer (P) is not possible. A The content of ) is preferably 85 mol % or more, more preferably 87 mol % or more, and further preferably 95 mol % or less.
[0016] [Reactive monomer (n B )] The copolymer (P) used in the present invention is a copolymer containing a reactive monomer (n B The copolymer (P) contains a reactive monomer (n B ) makes it easier to react with poly(meth)acrylic acid to produce a reaction product. The reactive monomer (n B ) is 2-aminoethyl (meth)acrylate, and is preferably 2-aminoethyl methacrylate represented by formula (2'). The reactive monomers (n B The amino group in may be in the form of a salt such as a hydrochloride. [ka]
[0017] The reactive monomer (n B The content of is 1 to 20 mol %. If the content is less than 1 mol %, the effect of reacting with poly(meth)acrylic acid cannot be expected, and if the content is more than 20 mol %, high hydrophilicity cannot be expected. From the above viewpoint, the reactive monomer (n B The content of ) is preferably 15 mol % or less, more preferably 13 mol % or less, and further preferably 5 mol % or more. A preferred combination of each monomer in the copolymer (P) used in the present invention is, for example, a hydrophilic monomer (n A ) as 2-(meth)acryloyloxyethyl phosphorylcholine, reactive monomer (n B ) is 2-aminoethyl (meth)acrylate. When the monomers in the copolymer (P) are combined as described above, excellent hydrophilicity and durability can be imparted to the surface of a soft contact lens.
[0018] [Other monomers] The copolymer (P) contains the hydrophilic monomer (n A ) and reactive monomers (n B ), other monomers may be contained, but the hydrophilic monomer (n A ) and reactive monomers (n B ) is preferably a copolymer consisting of only Examples of the other monomer include polymerizable monomers selected from linear or branched alkyl (meth)acrylates, cyclic alkyl (meth)acrylates, aromatic group-containing (meth)acrylates, styrene-based monomers, vinyl ether monomers, vinyl ester monomers, hydrophilic hydroxyl group-containing (meth)acrylates, acid group-containing monomers, and nitrogen-containing group-containing monomers.
[0019] Examples of linear or branched alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. An example of the cyclic alkyl (meth)acrylate is cyclohexyl (meth)acrylate.
[0020] Examples of aromatic group-containing (meth)acrylates include benzyl (meth)acrylate and phenoxyethyl (meth)acrylate. Examples of the styrene monomer include styrene, methylstyrene, and chlorostyrene. Examples of the vinyl ether monomer include methyl vinyl ether and butyl vinyl ether. Examples of vinyl ester monomers include vinyl acetate and vinyl propionate.
[0021] Examples of hydrophilic hydroxyl group-containing (meth)acrylates include polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Examples of the acid group-containing monomer include (meth)acrylic acid, styrenesulfonic acid, and (meth)acryloyloxyphosphonic acid. An example of the nitrogen-containing group-containing monomer is N-vinylpyrrolidone.
[0022] When the copolymer (P) contains other monomers as structural units, the hydrophilic monomer (n A )(Number of moles: N A ) and other monomers (number of moles: N X ) and the molar ratio [N A / N X ] is a hydrophilic monomer (n A ) is taken as 100, and preferably it is 100 / 50 or less. In addition, when the copolymer (P) contains other monomers as structural units, the hydrophilic monomer (n A )(Number of moles: N A ), reactive monomer (n B )(Number of moles: N B ), other monomers (number of moles: N X ) The mole ratio of each structural unit based on A :N B :N X = 50-99:1-50:1-50 is preferable.
[0023] [Weight average molecular weight of copolymer (P)] The weight average molecular weight of the copolymer (P) is 10,000 to 5,000,000, preferably 12,000 or more, more preferably 14,000 or more, even more preferably 16,000 or more, and preferably 4,000,000 or less, more preferably 3,000,000 or less, even more preferably 2,000,000 or less. For example, the weight average molecular weight of the copolymer (P) may be 18,000 to 1,500,000, 30,000 to 1,500,000, or 30,000 to 1,200,000. If the weight-average molecular weight is less than 10,000, it may be difficult to separate impurities during production, whereas if the weight-average molecular weight exceeds 5,000,000, the viscosity may increase, making filtration difficult. The weight average molecular weight of the copolymer (P) is a value measured by gel permeation chromatography (GPC).
[0024] [Production method of copolymer (P)] The copolymer (P) is a copolymer of the hydrophilic monomer (n A ), reactive monomer (n B ) and other monomers used as necessary. The copolymer is usually a random copolymer, but may be an alternating copolymer or a block copolymer in which the monomers are regularly arranged, or may have a graft structure in part. Specifically, for example, the copolymer (P) can be obtained by radically polymerizing a mixture of the monomers in the presence of a radical polymerization initiator under an inert gas atmosphere such as nitrogen, carbon dioxide, argon, or helium.
[0025] The radical polymerization method can be carried out by a known method such as bulk polymerization, suspension polymerization, emulsion polymerization, drop polymerization, solution polymerization, etc. As the radical polymerization method, drop polymerization or solution polymerization is preferred from the viewpoint of purification, etc., and drop polymerization is particularly preferred. The copolymer (P) can be purified by a known purification method such as reprecipitation, dialysis, or ultrafiltration. Examples of the radical polymerization initiator include an azo-based radical polymerization initiator, an organic peroxide, and a persulfate.
[0026] Examples of the azo radical polymerization initiator include 2,2'-azobis(2-diaminopropyl) dihydrochloride, 2,2'-azobis(2-(5-methyl-2-imidazolin-2-yl)propane) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobisisobutyramide dihydrate, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile (AIBN). Examples of organic peroxides include t-butyl peroxyneodecanate, benzoyl peroxide, diisopropyl peroxydicarbonate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxypivalate, t-butyl peroxyisobutyrate, lauroyl peroxide, t-butyl peroxydecanate, and succinic acid peroxide. Examples of persulfate oxides include ammonium persulfate, potassium persulfate, and sodium persulfate.
[0027] These radical polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is usually 0.001 to 10 parts by mass, preferably 0.02 to 5.0 parts by mass, and more preferably 0.03 to 3.0 parts by mass, based on 100 parts by mass of the total of the monomers. The synthesis of the copolymer (P) can be carried out in the presence of a solvent. The solvent is not particularly limited as long as it dissolves each monomer composition and does not adversely affect the reaction, and examples of the solvent include water, alcohol solvents, ketone solvents, ester solvents, linear or cyclic ether solvents, and nitrogen-containing solvents. Examples of alcohol-based solvents include methanol, ethanol, n-propanol, and isopropanol. Examples of the ketone solvent include acetone, methyl ethyl ketone, and diethyl ketone. An example of the ester solvent is ethyl acetate. Examples of linear or cyclic ether solvents include ethyl cellosolve and tetrahydrofuran. Examples of nitrogen-containing solvents include acetonitrile, nitrimethane, and N-methylpyrrolidone. Of these solvents, it is preferable to use water and alcohol-based solvents.
[0028] <Production of reactants> The surface treatment agent for soft contact lenses of the present invention contains a reaction product obtained by reacting the above-mentioned poly(meth)acrylic acid with the copolymer (P). The reaction of the poly(meth)acrylic acid with the copolymer (P) is preferably carried out in the presence of a condensation agent. As the condensing agent, for example, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC), N,N-dicyclohexylcarbodiimide (DCC), 1-cyclohexyl-3-(2-morpholinoethyl)carbodiimide, diisopropylcarbodiimide, or a mixture thereof can be used.
[0029] The reaction product in the present invention is preferably generated in a reaction solution. The reaction solution is a solution containing the above-mentioned poly(meth)acrylic acid, copolymer (P), and a solvent. The reaction solution preferably further contains the above-mentioned condensing agent. In the reaction solution, the poly(meth)acrylic acid and the copolymer (P) react to generate a reaction product. The solvent may be water, and may contain alcohol such as ethanol, n-propanol, and isopropanol other than water. The water may be water that is usually used in the manufacture of pharmaceuticals and medical devices. Specifically, ion-exchanged water, purified water, sterilized purified water, distilled water, and water for injection may be used.
[0030] The concentration of poly(meth)acrylic acid in the reaction solution is preferably 0.00001 w / v% to 1.0 w / v%, more preferably 0.001 w / v% to 0.8 w / v%, and even more preferably 0.1 w / v% to 0.6 w / v%. If the concentration is less than 0.00001 w / v%, the effect of the contact lens surface treatment cannot be expected, and if it is more than 1.0 w / v%, it may take a long time to dissolve the poly(meth)acrylic acid. The concentration of copolymer (P) in the reaction solution is preferably 0.05 w / v% to 4.0 w / v%, more preferably 0.1 w / v% to 2.0 w / v%, and even more preferably 0.2 w / v% to 1.0 w / v%. If the concentration of copolymer (P) is equal to or higher than these lower limits, it becomes easier to obtain the effect of imparting excellent hydrophilicity and durability to soft contact lenses. If it is equal to or lower than these upper limits, it is economically advantageous to obtain an effect commensurate with the blending amount. The concentration of the condensing agent in the reaction solution is preferably 0.05 w / v % to 1.0 w / v %, more preferably 0.1 w / v % to 0.8 w / v %, and even more preferably 0.2 w / v % to 0.6 w / v %. In addition, it is preferable to add a buffer to the reaction solution, and the concentration of the buffer is preferably 0.0001 w / v% to 15.0 w / v%, more preferably 0.001 w / v% to 10.0 w / v%, and even more preferably 0.01 w / v% to 5.0 w / v%. Specific types of buffers will be described later. The concentration of each component in the reaction solution means the concentration of each component before the reaction between poly(meth)acrylic acid and copolymer (P) begins. In the present invention, "w / v%" refers to the mass of a certain component in 100 mL of solution expressed in grams (g). For example, "the solution of the present invention contains 1.0 w / v% copolymer (P)" means that 100 mL of the solution contains 1.0 g of copolymer (P).
[0031] The temperature at which the reaction product is produced in the reaction solution is, for example, 0 to 60° C., and preferably 10 to 50° C. The reaction time is, for example, 10 to 480 minutes, and preferably 60 to 360 minutes.
[0032] The reaction product of the present invention can be produced in the manner described above. The reaction product is contained in a reaction solution, and the reaction product may be isolated by removing the solvent and used, but the reaction solution containing the reaction product may be used as the surface treatment agent for soft contact lenses of the present invention as it is.
[0033] The reaction product can be produced by reacting poly(meth)acrylic acid with the copolymer (P) in a solution as described above. Among them, it is preferable to carry out the reaction product by a process including the following steps (i) to (iii), and to prepare the surface treatment agent for soft contact lenses of the present invention at the same time as obtaining the reaction product.
[0034] (i) A step of separately preparing a poly(meth)acrylic acid solution in which poly(meth)acrylic acid is dissolved in a solvent, and a surface treatment solution in which copolymer (P) is dissolved in a solvent. (ii) A step of immersing a soft contact lens in the poly(meth)acrylic acid solution. (iii) a step of removing the soft contact lens from the poly(meth)acrylic acid solution, immersing the soft contact lens in a surface treatment solution to convert the surface treatment solution into a reaction solution containing poly(meth)acrylic acid, copolymer (P), and a solvent, reacting the poly(meth)acrylic acid with the copolymer (P) in the reaction solution to generate a reaction product, and preparing a surface treatment agent for soft contact lenses containing the reaction product.
[0035] In the above step (iii), a reaction product is generated in the reaction solution, and the reaction solution containing the reaction product corresponds to the surface treatment agent for soft contact lenses of the present invention. In the above step (iii), the surface treatment agent for soft contact lenses is prepared and the surface treatment of the soft contact lenses is performed.
[0036] The concentration of poly(meth)acrylic acid in the poly(meth)acrylic acid solution in step (i) is preferably 0.05 w / v% to 1.0 w / v%, more preferably 0.1 w / v% to 0.8 w / v%, and even more preferably 0.2 w / v% to 0.6 w / v%. Examples of the solvent for dissolving poly(meth)acrylic acid include water, organic solvents, etc. The organic solvent is not particularly limited, but examples thereof include ethers such as tetrahydrofuran, ketones such as acetone and N-methylpyrrolidone, esters such as ethyl acetate, alcohols such as ethanol, and amides such as dimethylformamide, and alcohols are preferred.
[0037] The solvent of the surface treatment solution in the above step (i) may be water, and may contain alcohol such as ethanol, n-propanol, and isopropanol in addition to water. The water may be water that is generally used in the manufacture of pharmaceuticals and medical devices. Specifically, ion-exchanged water, purified water, sterilized purified water, distilled water, and water for injection may be used. The surface treatment solution containing the copolymer (P) in the step (i) preferably contains a condensing agent. The type of the condensing agent is as described above. The surface treatment solution preferably contains a buffer. The concentrations of the copolymer (P), condensing agent and buffer in the surface treatment solution are the same as those in the above-mentioned reaction solution.
[0038] The immersion time in the above step (ii) is not particularly limited, but is preferably 0.1 to 6 minutes.
[0039] In step (iii), the soft contact lens immersed in step (ii) may be taken out of the poly(meth)acrylic acid solution and directly immersed in the surface treatment solution. From the viewpoint of removing excess polymethacrylic acid, however, it is preferable to take it out of the poly(meth)acrylic acid solution, immerse it in water, and then immerse it in the surface treatment solution. The type of the solvent in the reaction solution in step (iii) is the same as that in the surface treatment solution described above, and the concentrations of the poly(meth)acrylic acid, copolymer (P), condensing agent, and buffer in the reaction solution are as described above.
[0040] [Other ingredients] The surface treatment agent for soft contact lenses of the present invention may further contain the following components, if necessary, in addition to the reaction product obtained by reacting poly(meth)acrylic acid with the copolymer (P).
[0041] (Buffer) The surface treatment agent for soft contact lenses of the present invention may contain a buffering agent. By containing a buffering agent in the surface treatment agent for soft contact lenses of the present invention, the pH and osmotic pressure can be adjusted, and deformation of the soft contact lens can be suppressed.
[0042] In the present invention, from the viewpoint of obtaining the above-mentioned effects, one or more buffers selected from a phosphate buffer, a 2-morpholinoethanesulfonic acid buffer, and a borate buffer can be used as the buffer. In this specification, the term "phosphate buffer" refers to a buffer solution consisting of disodium hydrogen phosphate, sodium dihydrogen phosphate, anhydrous sodium dihydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, hydrochloric acid, sodium hydroxide, potassium hydroxide, etc. The term "2-morpholinoethanesulfonic acid buffer" refers to a buffer solution consisting of 2-morpholinoethanesulfonic acid. The term "borate buffer" refers to a buffer solution consisting of boric acid, borax, hydrochloric acid, sodium hydroxide, potassium hydroxide, etc.
[0043] The concentration of the buffer in the surface treatment agent for soft contact lenses of the present invention is preferably 0.0001 w / v% to 15.0 w / v%, more preferably 0.001 w / v% to 10.0 w / v%, and even more preferably 0.01 w / v% to 5.0 w / v%. In particular, when one or more buffers selected from phosphate buffer, 2-morpholinoethanesulfonic acid buffer, and borate buffer are used as the buffer, the concentration thereof is preferably 0.001 w / v% to 10.0 w / v%, more preferably 0.01 w / v% to 5.0 w / v%, and even more preferably 0.1 w / v% to 5.0 w / v%, as the total of the components of the phosphate buffer, 2-morpholinoethanesulfonic acid buffer, and borate buffer.
[0044] (Additives) The surface treating agent for soft contact lenses of the present invention may further contain additives, if necessary. The additives may include those conventionally used in soft contact lenses, such as inorganic salts, acids, bases, antioxidants, stabilizers, and preservatives. Examples of inorganic salts include sodium chloride, potassium chloride, magnesium chloride, and calcium chloride. Examples of the acid include phosphoric acid and sulfuric acid. Examples of the base include trishydroxymethylaminomethane and monoethanolamine. Antioxidants include, for example, tocopherol acetate and dibutylhydroxytoluene. Stabilizers include, for example, sodium edetate and glycine. Examples of preservatives include benzalkonium chloride, chlorhexidine gluconate, potassium sorbate, chlorobutanol, and polyhexanide hydrochloride.
[0045] The surface treatment agent for soft contact lenses of the present invention may further contain polyethylene glycol, poloxamer, sodium alginate, hydroxypropyl methylcellulose, hydroxyethyl cellulose, sodium hyaluronate, sodium chondroitin sulfate, etc., from the viewpoint of moisturizing the soft contact lens and improving the wearing comfort. Among these additives, it is preferable to add inorganic salts such as sodium chloride or potassium chloride from the viewpoint of adjusting the osmotic pressure of the soft contact lens to a suitable range. The inorganic salts can also be used together with a buffer to form a physiological saline solution (e.g., ISO physiological saline solution).
[0046] From the viewpoint of further enhancing the effect of imparting hydrophilicity and its sustainability to the soft contact lens, it is preferable to add polyethylene glycol, sodium alginate, poloxamer, hydroxypropyl methylcellulose, hydroxyethyl cellulose, sodium hyaluronate or sodium chondroitin sulfate. When the surface treatment agent for soft contact lenses of the present invention contains additives, the concentration of the additives is preferably 0.001 w / v% to 10.0 w / v%, more preferably 0.001 w / v% to 7.0 w / v%, in terms of the total of the additive components. In particular, when the surface treatment agent for soft contact lenses of the present invention contains sodium chloride, the concentration is preferably 0.001 w / v% to 1.5 w / v%, more preferably 0.05 w / v% to 1.3 w / v%, and even more preferably 0.1 w / v% to 1.0 w / v%. On the other hand, when the surface treatment agent for soft contact lenses of the present invention contains potassium chloride, the concentration is preferably 0.01 w / v% to 4.0 w / v%, more preferably 0.05 w / v% to 3.5 w / v%, and even more preferably 0.1 w / v% to 3.0 w / v%.
[0047] [Method of manufacturing the surface treatment agent for soft contact lenses] The method for producing the surface treatment agent for soft contact lenses of the present invention is not particularly limited, and the reaction product is generated by reacting poly(meth)acrylic acid with the copolymer (P) in the reaction solution as described above, and the reaction product may be used as it is as the surface treatment agent for soft contact lenses, or the reaction product may be isolated and mixed with a solvent or the like to produce the surface treatment agent for soft contact lenses. Among them, it is preferable to produce the surface treatment agent for soft contact lenses by a process including steps (i) to (iii) as described above.
[0048] [pH of surface treatment agents for soft contact lenses] The pH of the surface treatment agent for soft contact lenses of the present invention is preferably 3.0 to 8.0, more preferably 3.5 to 7.8, even more preferably 4.0 to 7.6, and even more preferably 4.5 to 7.5, from the viewpoint of improving the efficiency of the condensation reaction. In this specification, the pH of the surface treatment agent for soft contact lenses refers to a value measured in accordance with the 17th Edition of the Japanese Pharmacopoeia, General Test Method, 2.54, pH Measurement Method.
[0049] [Osmotic pressure and osmotic pressure ratio of surface treatment agents for soft contact lenses] From the viewpoint of improving the wearing comfort, the osmotic pressure of the surface treatment agent for soft contact lenses of the present invention is preferably 200 to 400 mOsm, more preferably 225 to 375 mOsm, even more preferably 230 to 350 mOsm, and even more preferably 240 to 340 mOsm. The osmotic pressure ratio is preferably 0.7 to 1.4, more preferably 0.7 to 1.3, and even more preferably 0.8 to 1.2. In this specification, the osmotic pressure of the soft contact lens surface treatment agent refers to a value measured in accordance with the 17th Edition of the Japanese Pharmacopoeia, General Test Method 2.47 Osmotic Pressure Measurement Method (Osmolarity Measurement Method), and the osmotic pressure ratio refers to the value obtained by dividing the obtained osmotic pressure value by the osmotic pressure value of 0.9 mass % physiological saline (286 mOsm).
[0050] As described above, the surface treatment agent for soft contact lenses of the present invention can improve the hydrophilicity of the surface of soft contact lenses and reduce the dryness and discomfort felt by the wearer. Therefore, the surface treatment agent for soft contact lenses of the present invention is preferably used for silicone hydrogel contact lenses. EXAMPLES
[0051] The surface treatment agent for contact lenses of the present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited thereto. The copolymers and polymers used in the examples and comparative examples are as follows.
[0052] <Polyacrylic acid> Polyacrylic acid 1··Polyacrylic acid 5,000 (average molecular weight 5,000, Fujifilm Wako Pure Chemical Industries, Ltd.) Polyacrylic acid 2··Polyacrylic acid 25,000 (average molecular weight 25,000, Fujifilm Wako Pure Chemical Industries, Ltd.) Polyacrylic acid 3··Polyacrylic acid 250,000 (average molecular weight 250,000, Fujifilm Wako Pure Chemical Industries, Ltd.) Polyacrylic acid 4··Polyacrylic acid 1,000,000 (average molecular weight 1,000,000, Fujifilm Wako Pure Chemical Industries, Ltd.)
[0053] <Copolymer (P)> As the copolymer (P), the following copolymers (P1) to (P5) were used.
[0054] Copolymer (P1) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B ) (number of moles: Nb) was 2-aminoethyl methacrylate hydrochloride to obtain 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer (copolymer (P1)). Hydrophilic monomer (n A ): 92.5 mol% The reactive monomer (n B ): 7.5 mol% Weight average molecular weight of copolymer (P1): 200,000
[0055] Copolymer (P2) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B ) (number of moles: Nb) was 2-aminoethyl methacrylate hydrochloride to obtain 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer (copolymer (P2)). Hydrophilic monomer (n A ): 95.0 mol% The reactive monomer (n B ): 5.0 mol% Weight average molecular weight of copolymer (P2): 210,000
[0056] Copolymer (P3) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P3), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 97.5 mol% Reactive monomer (n B ): 2.5 mol% Weight average molecular weight of copolymer (P3): 230,000
[0057] Copolymer (P4) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P4), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 95.0 mol% Reactive monomer (n B ): 5.0 mol% Weight average molecular weight of copolymer (P4): 270,000
[0058] Copolymer (P5) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P5), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 95.0 mol% Reactive monomer (n B ): 5.0 mol% Weight average molecular weight of copolymer (P5): 150,000
[0059] Copolymer (P6) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P6), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 90.0 mol% Reactive monomer (n B ): 10.0 mol% Weight average molecular weight of copolymer (P6): 300,000
[0060] Copolymer (P7) Hydrophilic monomer (n A) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P7), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 80.0 mol% Reactive monomer (n B ): 20.0 mol% Weight average molecular weight of copolymer (P7): 1,000,000
[0061] Copolymer (P8) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N b Using 2-aminoethyl methacrylate hydrochloride as the copolymer (P8), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 90.0 mol% Reactive monomer (n B ): 10.0 mol% Weight average molecular weight of copolymer (P8): 1,500,000
[0062] Copolymer (P9) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n B )(Number of moles: N bUsing 2-aminoethyl methacrylate hydrochloride as the copolymer (P9), 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride polymer was obtained. Hydrophilic monomer (n A ): 90.0 mol% Reactive monomer (n B ): 10.0 mol% Weight average molecular weight of copolymer (P9): 10,000
[0063] <Measurement of weight average molecular weight> 5 mg of each of the obtained copolymers (P1) to (P9) was dissolved in 1 g of a 0.1 mol / L aqueous sodium sulfate solution and subjected to GPC measurement. Other measurement conditions were as follows. Column: Shodex (GSM-700) Mobile phase: 0.1 mol / L sodium sulfate aqueous solution Standard substance: Pullulan Detector: Differential refractive index RI-8020 (manufactured by Tosoh Corporation) Calculation method for weight average molecular weight: Molecular weight calculation program (GPC program for SC-8020) Flow rate: 1.0mL per minute Injection volume: 100μL Column oven: 40℃ Measurement time: 30 minutes
[0064] <Comparative polymer for copolymer (P)> As comparative polymers for copolymer (P), the following polymers (A), (B), (C) and (D) were used. Polymer (A) 2-methacryloyloxyethyl phosphorylcholine homopolymer (weight average molecular weight: 200,000) was used. Polymer (B) A commercially available polydimethyldimethylenepyrosidium chloride solution (40% solution) (Polyquaternium-6, ME Polymer H40W (product name) manufactured by Toho Chemical Industry Co., Ltd., weight average molecular weight 250,000) was used.
[0065] Polymer (C) The copolymer of 2-methacryloyloxyethyl phosphorylcholine and methacrylic acid (molar ratio; 2-methacryloyloxyethyl phosphorylcholine:methacrylic acid=3:7) (weight average molecular weight: 288,000) was used. Polymer (D) Hydrophilic monomer (n A ) (molar number: Na) as 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (also known as 2-methacryloyloxyethyl phosphorylcholine), reactive monomer (n b )(Number of moles: N b ) was used as the copolymer, 2-methacryloyloxyethyl phosphorylcholine·2-aminoethyl methacrylate hydrochloride, to obtain copolymer. Hydrophilic monomer (n A ): 40.0 mol% The reactive monomer (n B ): 60.0 mol% Weight average molecular weight: 234,000
[0066] <Polymer concentration adjustment> For the purpose of facilitating handling when used in the Examples and Comparative Examples, the respective polymers were previously adjusted in concentration as follows. Copolymer (P1) to copolymer (P9): Each polymer and purified water were used to adjust the copolymer concentration to 10 w / v%. The solutions thus adjusted are indicated in the tables as "copolymer (P1) solution", etc. Polymer (A): Polymer (A) and purified water were used to adjust the concentration of polymer (A) to 5 w / v %. Polymer (B): Polymer (B) was a 40 w / v % liquid and was used as is. Polymer (C): Polymer (C) and purified water were used to adjust the concentration of polymer (C) to 5 w / v %. Polymer (D): Polymer (D) and purified water were used to adjust the concentration of polymer (D) to 10 w / v %.
[0067] <ISO physiological saline solution> The ISO physiological saline used in each example and comparative example was prepared as follows. According to ISO 18369-3:2006, Ophthalmic Optics-Contact Lenses Part 3: Measurement Methods., an ISO physiological saline solution was prepared. Specifically, 8.3 g of sodium chloride, 5.993 g of disodium hydrogen phosphate dodecahydrate, and 0.528 g of sodium dihydrogen phosphate dihydrate were dissolved in water to make a total volume of 1000 mL, and the ISO physiological saline solution was obtained by filtration. Sodium chloride was manufactured by Kishida Chemical Co., Ltd., disodium hydrogen phosphate dodecahydrate was manufactured by Wako Pure Chemical Industries, Ltd., sodium dihydrogen phosphate dihydrate was manufactured by Fujifilm Wako Pure Chemical Corporation, and ion-exchanged water was used for water.
[0068] <Contact lenses for evaluation> The following contact lenses were used for the surface treatment. (1): Manufactured by Seed Co., Ltd., Seed 2 Week Fine UV (Composition: 2-HEMA, EGDMA, Water content: 38%, FDA classification: I, Oxygen permeability (Dk value): 12) (2): Manufactured by Johnson & Johnson K.K., 2 Week Acuvue (Composition: 2-HEMA, MAA, Water content: 58%, FDA classification: IV, Oxygen permeability (Dk value): 28) (3): Manufactured by Alcon Japan Co., Ltd., Air Optix Aqua (Composition: Betacon, TRIS, DMA, Water content: 33%, FDA classification: I (Silicone hydrogel contact lens), Oxygen permeability (Dk value): 138) (4): Manufactured by Bausch + Lomb Japan Ltd., Medalist FreshFit Comfort Moist (Composition: Monomer modified with TRIS structure, NVP, Water content: 36%, FDA classification: III, Oxygen permeability (Dk value): 130) Note that the above (3) and (4) correspond to silicone hydrogel contact lenses.
[0069] <WBUT (Water Breaking Up Time) test of soft contact lenses> The WBUT test for soft contact lenses was carried out according to the following procedure. (1) 10 mL or more of ISO physiological saline was placed in a 15 mL centrifuge tube, and one soft contact lens treated in the Example was placed in the 15 mL centrifuge tube and shaken for 2 hours. (2) The ISO saline solution in the centrifuge tube was removed, and 10 mL or more of ISO saline solution was added again and shaken overnight. (3) The soft contact lens was removed from the 15 mL centrifuge tube, lightly wiped to remove moisture, and then placed in a contact lens case, to which 1 mL of ISO physiological saline was added. (4) The soft contact lens was grasped with tweezers and slowly pulled up. (5) Time measurement began when the soft contact lens was raised to a height where it was no longer in contact with the liquid surface. (6) When the liquid film formed on the surface of the soft contact lens disappeared, the time measurement was stopped, and the time (seconds) from the start to the end of the time measurement was defined as the WBUT before scrubbing. (7) After the test, the soft contact lens was placed on the index finger and rubbed 20 times using the thumb and index finger. (8) After scrubbing, the soft contact lens was immersed in ISO saline using tweezers. (9) Steps (4), (5) and (6) were repeated and the WBUT after scrubbing was measured. Each measurement was repeated three times, and the average values were evaluated as WBUT (before scrubbing) and WBUT (after scrubbing). A higher WBUT value indicates better hydrophilicity. WBUT: 5 seconds or more was judged to have surface hydrophilicity, 10 seconds or more was judged to have excellent surface hydrophilicity, and 15 seconds or more was judged to have extremely excellent surface hydrophilicity.
[0070] <Oxygen permeability measurement for soft contact lenses> The oxygen permeability of the soft contact lenses was measured using an Oxygen Permeometer model 201T manufactured by Createch / Rehder Dev. Co. In each example, the oxygen permeability was measured for the soft contact lenses before and after treatment with the surface treatment agent.
[0071] Example 1 100 g of water and 0.976 g of 2-morpholinoethanesulfonic acid were weighed and dissolved in a beaker in advance. 20 g of copolymer (P1) solution (10 w / v% aqueous solution) and 0.5 g of water-soluble carbodiimide (1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride) were further added to this liquid and mixed to prepare a surface treatment solution. Separately, 100 g of ethanol and 0.4 g of polyacrylic acid 1 were mixed in a beaker to prepare a polyacrylic acid solution, and 10 pieces of the contact lenses (1) for evaluation were placed in the polyacrylic acid solution and immersed for 1 minute. Thereafter, the contact lenses (1) for evaluation were taken out, placed in 100 g of water, and further immersed for 1 minute. After removing the contact lens (1) for evaluation from the water, the contact lens (1) for evaluation was placed in a previously prepared surface treatment solution and immersed at 37° C. for 60 minutes to produce a surface treatment agent for soft contact lenses containing a reaction product of polyacrylic acid 1 and copolymer (P1), and the contact lens (1) for evaluation was surface-treated with the surface treatment agent. Thereafter, the contact lens (1) for evaluation was removed and immersed in ISO physiological saline to obtain the contact lens of Example 1. A <Soft Contact Lens WBUT (Water Breaking Up Time) Test> was carried out on the contact lens of Example 1. The evaluation results are shown in Table 1. In producing the surface treatment agent for contact lenses in Example 1, the reaction between polyacrylic acid and copolymer (P) was tracked. 13 The results were analyzed by C-NMR, which confirmed that new components other than polyacrylic acid and copolymer (P) were produced, and that a reaction product was produced.
[0072] (Examples 2 to 20) Each soft contact lens of Examples 2 to 20 was prepared in the same manner as in Example 1, except that the compositions of the polyacrylic acid solution, the surface treatment solution, and the surface treatment agent for soft contact lenses, and the types of the contact lenses used for evaluation were changed as shown in Tables 1 to 3. The contact lenses of each Example and Comparative Example were subjected to <WBUT test for soft contact lenses>. The results are shown in Tables 1 to 3.
[0073] Comparative Example 1 An experiment was carried out in the same manner as in Example 1, except that 20 g of a 5 w / v % aqueous solution of polymer (A) was used instead of 20 g of a 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0074] Comparative Example 2 An experiment was carried out in the same manner as in Example 1, except that 20 g of a 40 w / v % aqueous solution of polymer (B) was used instead of 20 g of a 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0075] Comparative Example 3 An experiment was carried out in the same manner as in Example 1, except that 20 g of a 5 w / v % aqueous solution of polymer (C) was used instead of 20 g of a 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0076] Comparative Example 4 An experiment was carried out in the same manner as in Example 1, except that 20 g of a 10 w / v % aqueous solution of polymer (D) was used instead of 20 g of the 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0077] Comparative Example 5 An experiment was carried out in the same manner as in Example 1, except that 1 g of a 10 w / v % aqueous solution of polymer (D) was used instead of 20 g of the 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0078] Comparative Example 6 An experiment was carried out in the same manner as in Example 1, except that 40 g of a 10 w / v % aqueous solution of polymer (D) was used instead of 20 g of the 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0079] Comparative Example 7 An experiment was carried out in the same manner as in Example 1, except that 0.05 g of polyacrylic acid 1 was used instead of 0.4 g of polyacrylic acid 1 used in Example 1, and 20 g of a 10 w / v % aqueous solution of polymer (D) was used instead of 20 g of a 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0080] Comparative Example 8 An experiment was carried out in the same manner as in Example 1, except that 1 g of polyacrylic acid 2 was used instead of 0.4 g of polyacrylic acid 1 used in Example 1, and 20 g of a 10 w / v % aqueous solution of polymer (D) was used instead of 20 g of a 10 w / v % aqueous solution of copolymer (P1) used in Example 1. The results are shown in Table 4.
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] [Table 4]
[0085] The oxygen permeability after the surface treatment was measured for the contact lenses that had been subjected to the surface treatments of Examples 1 to 20. The results are shown in Table 5.
[0086] [Table 5]
[0087] As is clear from the results of Tables 1 to 5, by using a soft contact lens surface treatment agent containing a reaction product obtained by reacting the polyacrylic acid of the present invention with the copolymer (P), it is possible to impart excellent hydrophilicity and its durability to the surface of a soft contact lens. Furthermore, it was found that when the soft contact lens surface treatment agent of the present invention is used on a silicone hydrogel contact lens, it exhibits extremely excellent hydrophilicity and its durability, does not affect oxygen permeability, and provides excellent wearing comfort. [Industrial Applicability]
[0088] By subjecting the surface of a soft contact lens to hydrophilic treatment using the surface treatment agent for soft contact lenses of the present invention, it is possible to impart extremely excellent surface hydrophilicity, and since the imparted surface hydrophilicity also has excellent durability, it is possible to provide a soft contact lens that reduces discomfort and is excellent in wearing comfort.
Claims
1. A method for treating a surface of a soft contact lens, comprising reacting a poly(meth)acrylic acid shown below with a copolymer (P). Poly(meth)acrylic acid: Poly(meth)acrylic acid having an average molecular weight of 1,000 to 2,000,000 Copolymer (P): A hydrophilic monomer (n A ) and a reactive monomer (n B ) and a hydrophilic monomer (n A ) is 80 to 99 mol %, and the reactive monomer (n B %。 In the formula (1) and the formula (2), X represents a hydrogen atom or a methyl group. [Formula 1] [chemical 2]
2. 2. The method for treating a surface of a soft contact lens according to claim 1, wherein the soft contact lens is a silicone hydrogel contact lens.
Citation Information
Patent Citations
Bionic polymer and method for preparing durable double-bionic polymer coating and application thereof
CN109796616A
polymer surface coating
JP1995502053A
Silicone hydrogel material with chemically bonded wetting agent
JP2012508902A
Silicone hydrogel lenses with cross-linked hydrophilic coating
JP2013533518A
Silicone monomer, silicone polymer and medical device using the same, and methods of manufacturing silicone monomer and silicone polymer
JP2017115005A