Apparatus for producing raw materials for blast furnace equipped with a chute and method for producing raw materials for blast furnace

The chute with a gas injection device and diffusion section addresses the segregation issue in carbonization furnaces, enhancing the uniformity of material distribution and carbonization efficiency.

JP7567832B2Active Publication Date: 2024-10-16JFE STEEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022025365
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-22
Publication Date
2024-10-16
Estimated Expiration
2042-02-22

AI Technical Summary

Technical Problem

Existing carbonization furnaces face challenges in achieving uniform distribution of molded materials due to segregation of powder and larger particles, leading to non-uniform gas flow and impaired carbonization efficiency.

Method used

A chute equipped with a gas injection device that blows gas onto larger molded particles to mix with powder, ensuring they enter the furnace together, combined with a diffusion section to disperse the materials in the width direction.

Benefits of technology

This approach suppresses powder segregation, improving the quality and productivity of blast furnace raw materials by ensuring uniform charging and consistent gas flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567832000001
    Figure 0007567832000001
  • Figure 0007567832000002
    Figure 0007567832000002
  • Figure 0007567832000003
    Figure 0007567832000003
Patent Text Reader

Abstract

To provide a chute which improves distribution of a molding in a dry distillation furnace at the time of manufacture of the raw material for the blast furnace such as a ferro coke, that is, can suppress segregation of powder and molding particles having a larger particle diameter than the powder, and to provide an apparatus and a method for manufacturing a raw material for a blast furnace provided with the chute.SOLUTION: In a chute 3 for charging a molding into a charged part 1, the molding has powder SP and molding particles LP having a larger particle diameter than the powder SP, and a gas jet device 6 for jetting gas toward the molding, and thereby bowing off the powder SP so as to be placed on the molding particles LP is provided.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chute, and a manufacturing apparatus and method for producing raw material for a blast furnace, the apparatus being provided with the chute. [Background technology]

[0002] In recent years, the steel industry has been required to reduce CO2 gas emissions in order to prevent global warming, and there is an urgent need to reduce the use of fossil fuels. In the steel industry, molten iron is produced in a blast furnace by reducing iron ore with coke, which is carbon, i.e., coal, in a coke oven. To reduce the coke consumption, technology is being developed to use ferro-coke as a raw material for blast furnaces. Ferro-coke is a molded coke made by mixing a certain amount of iron ore with coal and forming it into agglomerates, then carbonizing it to disperse fine metallic iron particles in the coke, and increasing the reactivity of the coke through the catalytic action of the metallic iron.

[0003] As a method for carbonizing ferro-coke, a method using a vertical carbonization furnace (hereinafter, simply referred to as a carbonization furnace) has been proposed. For example, Patent Document 1 discloses a method for producing ferro-coke using a carbonization furnace having a carbonization zone at the top and a cooling zone at the bottom. This method includes a charging step of charging molded materials made of a carbon-containing material and an iron-containing material into the carbonization furnace from the top of the furnace, a carbonization step of carbonizing the molded materials in the carbonization zone by blowing in a heated gas to produce ferro-coke, a cooling step of cooling the ferro-coke by blowing in a cooling gas, an in-furnace gas discharge step of discharging in-furnace gas from an outlet at the top of the furnace, and a ferro-coke discharge step of discharging the ferro-coke from the bottom of the cooling zone. In the carbonization step, the molded materials are heated by blowing in a low-temperature gas from a low-temperature gas blowing tuyeres in the middle of the carbonization zone and a high-temperature gas from a high-temperature gas blowing tuyeres in the bottom of the carbonization zone into the furnace. In the cooling process, the ferro-coke is cooled by injecting cooling gas from the cooling gas injection tuyeres at the bottom of the cooling zone. In order to increase the production volume of ferro-coke, the volume of the carbonization furnace must be increased, but the heating gas and the cooling gas are injected in the depth direction of the carbonization furnace, that is, parallel to the horizontal component of the direction in which the molded materials are charged, in other words, in the thickness direction of the carbonization furnace. Therefore, in order to allow the above-mentioned gases to penetrate to the center of the furnace in the depth direction, it is necessary to keep the inner dimension in the depth direction below a certain value. Therefore, the carbonization furnace has a shape in which the furnace width direction (the direction perpendicular to the depth direction in the cross section of the carbonization furnace) is longer than the depth direction. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-57970 A [Patent Document 2] JP 2011-162271 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, in a carbonization furnace having a structure in which the furnace width direction is longer than the depth direction, it is difficult to obtain a uniform distribution of the molded materials even if multiple rows of molded material charging inlets are arranged in the furnace width direction. In particular, the powder generated by the collision of the molded materials with the wall surface of the chute through which the molded materials are charged into the carbonization furnace, or the collision of the molded materials with each other during the process of transporting the molded materials into the carbonization furnace including the chute, tends to segregate and tend to be concentrated at the charging inlet side in the carbonization furnace. This is because most of the powder slips through the molded materials and settles, and the molded materials are separated into two layers by the time they reach the carbonization furnace: a layer of molded material particles with a particle size larger than the powder (hereinafter referred to as the molded material layer) and a powder layer located below the molded material layer. Specifically, when 1 ton of molded materials is charged into the carbonization furnace, the thickness of the charged materials when entering the carbonization furnace, that is, the combined thickness of the molded material layer and the powder layer, is about 150 mm at the maximum. The compact particles are charged into the carbonization furnace from a high position due to the powder present below them, so they tend to fly to a position far from the carbonization furnace's charging port, while the powder in the lower layer falls near the charging port. The compact particles form mountains according to their angle of repose, so they are distributed more uniformly than the powder, but the powder is fixed in position by slipping between the compact particles, so if the powder falls concentrated at one point, for example near the charging port, significant powder segregation occurs. One problem caused by powder segregation is that the gas flow in the furnace becomes uneven, affecting the carbonization of the compacts.

[0006] As an example of a method for uniformly charging materials, Patent Document 2 discloses a method for dispersing materials radially by providing a dispersion induction section with an inclined surface that slopes radially downward from the center of the width direction of the conveying path toward the outlet side in a conveying furnace. This technology is specialized for improving dispersion in the furnace width direction. The presence or absence of a dispersion induction section does not affect the flying distance of the powder, so the installation of a dispersion induction section cannot eliminate powder segregation at the charging inlet side.

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide a chute that can improve the distribution of shaped products in a carbonization furnace during the production of blast furnace raw materials such as ferro-coke, i.e., that can suppress segregation of powder and shaped product particles having a particle size larger than that of the powder, and a manufacturing apparatus and manufacturing method for blast furnace raw materials equipped with the chute. [Means for solving the problem]

[0008] In order to achieve the above object, the present invention provides [1] A chute for loading a molded material into a loading section, the molded material having a powder and molded material particles having a larger particle size than the powder, and the chute is equipped with a gas injection device that injects gas toward the molded material to blow the powder off so that it lies on top of the molded material particles.

[0009] [2] In the chute described in [1] above, the gas injection device is configured to inject the gas from below the molded product.

[0010] [3] The chute described in [1] or [2] above, wherein the gas injection speed by the gas injection device is 20 m / s or more and 30 m / s or less.

[0011] [4] An apparatus for manufacturing raw materials for a blast furnace, comprising a chute as described in any one of [1] to [3] above, wherein the loading section is a carbonization furnace for carbonizing the molded materials, and the gas injection device is configured to continuously inject the gas onto the molded materials for a predetermined period of time while the molded materials are flowing into the chute.

[0012] [5] In the apparatus for manufacturing raw materials for blast furnaces described in [4] above, the gas injection device is provided upstream of the outlet of the chute in the direction of charging the molded material from the chute to the carbonization furnace.

[0013] [6] In the manufacturing apparatus for blast furnace raw materials according to the above [4] or [5], This is an apparatus for manufacturing raw materials for a blast furnace, in which a diffusion section for diffusing the molded materials in the width direction of the carbonization furnace is provided downstream of the outlet of the chute in the charging direction of the molded materials.

[0014] [7] In the apparatus for manufacturing blast furnace raw material described in any one of [4] to [6] above, the molded product contains a carbon-containing material and an iron-containing material as components.

[0015] [8] A method for producing blast furnace raw materials using an apparatus for producing blast furnace raw materials described in any one of [4] to [7] above. Effect of the Invention

[0016] According to the present invention, even if the molded product is separated to some extent into two layers, a layer of powder (hereinafter referred to as the powder layer) and a layer of molded product particles (hereinafter referred to as the molded product particle layer) during the transportation process, the powder is blown off and placed on the molded product particles by injecting gas onto the molded product. Alternatively, the molded product particles and the powder are mixed to some extent by the gas. Therefore, the molded product particles and the powder are unlikely to be charged into the carbonization furnace in a two-layer state, and segregation of the molded product particles and the powder in the carbonization furnace can be suppressed. This can suppress the adverse effect on the carbonization of the molded product caused by the segregation of the molded product particles and the powder. As a result, the quality of the raw material for the blast furnace charged into the blast furnace can be improved, and the productivity of the raw material for the blast furnace can be improved. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a side view of the ferro-coke producing apparatus according to the present invention. [Diagram 2] FIG. 13 is a diagram showing the correlation between the maximum powder rate and the installation position of the gas injection device. [Diagram 3] FIG. 13 is a diagram showing the correlation between the maximum powder rate and the timing of gas injection. [Figure 4]FIG. 13 is a diagram showing the correlation between the maximum powder rate and the gas injection velocity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The briquettes in the embodiment of the present invention are carbonized to become a raw material for a blast furnace, and an example of the raw material for a blast furnace is briquettes. Specifically, ferro coke, which is a type of briquettes, can be mentioned. Hereinafter, an embodiment of the present invention will be described using a manufacturing process of ferro coke as an example. Note that the drawings in the following description are schematic and may differ from the actual process. In addition, the following embodiment exemplifies an apparatus and a method for embodying the technical idea of ​​the present invention, and the present invention is not limited to the embodiment described below. In other words, the present invention can be modified in various ways within the technical scope of the present invention described in the claims.

[0019] Fig. 1 is a side view of a ferro-coke manufacturing apparatus (hereinafter, simply referred to as the manufacturing apparatus) according to the present invention. The manufacturing apparatus shown in Fig. 1 includes a carbonization furnace 1 that carbonizes briquettes in an upper carbonization zone and cools the ferro-coke produced by carbonizing the briquettes in a lower cooling zone (not shown), and a charging port 2 is formed on the side of the upper part of the carbonization furnace 1. The left-right direction in Fig. 1 indicates the depth direction and thickness direction of the carbonization furnace 1, and the up-down direction in Fig. 1 indicates the up-down direction of the carbonization furnace 1. The above-mentioned carbonization furnace 1 corresponds to a charging port in an embodiment of the present invention.

[0020] As described above, the molded product in the embodiment of the present invention is turned into ferro-coke by carbonization, and contains carbon-containing materials (such as coal) and iron-containing materials (such as iron ore) as components. The molded product is formed by agglomerating the above-mentioned materials by an agglomerating means (not shown), and is transported to the carbonization furnace 1 in this state by a transporting means (not shown). In addition, the molded product may be partially turned into powder by colliding with the transporting means or with each other due to vibration during the transport process. Therefore, when the molded product is charged into the carbonization furnace 1, the molded product contains powder SP and molded product particles LP having a particle size larger than that of the powder SP. The powder SP may move to the lower side of the molded product particles LP through gaps between the molded product particles LP due to vibration during the transport process, and may form a layer of the powder SP (hereinafter referred to as the powder layer) and a layer of the molded product particles LP (hereinafter referred to as the molded product particle layer). The above-mentioned agglomerating means and conveying means may be configured in the same manner as conventionally known agglomerating means and conveying means.

[0021] A chute 3 is connected to the inlet 2, which charges the molded material conveyed by the conveying means into the carbonization furnace 1. In the example shown in FIG. 1, the chute 3 has an inclined surface that slopes downward from above, and the molded material conveyed by the conveying means is charged into the carbonization furnace 1 along the inclined surface. Specifically, the chute 3 shown in FIG. 1 has two inclined surfaces 3A and 3B with different inclination angles in the charging direction of the molded material. The inclination angle of the second inclined surface 3B on the downstream side with respect to the horizontal plane (not shown) is set smaller than that of the first inclined surface 3A on the upstream side in the charging direction. This is to make it easier to charge the molded material on the side opposite the inlet 2 in the depth direction of the carbonization furnace 1. The inclination angles of these inclined surfaces 3A and 3B are set in advance.

[0022] A gate 4 for charging the molded material into the carbonization furnace 1 is provided near the outlet of the chute 3 in the charging direction of the molded material into the carbonization furnace 1. The gate 4 is a mechanism for charging the molded material into the carbonization furnace 1, or a mechanism for temporarily storing the molded material to be charged into the carbonization furnace 1 and adjusting the charging amount of the molded material. That is, the gate 4 is not particularly limited as long as it can charge the molded material into the carbonization furnace 1 or can adjust the charging amount of the molded material. In the example shown here, the gate 4 is in the form of a door configured to rotate around a predetermined rotation center axis. Specifically, the gate 4 is provided on the upper inner surface of the inner surface of the chute 3, and is configured to open toward the carbonization furnace 1 side upon receiving a torque transmitted from an actuator (not shown). This is to avoid the possibility that the gate 4 may hinder the charging of the molded material when the gate 4 is opened and the molded material is charged into the carbonization furnace 1 if the gate 4 is provided on the lower inner surface of the inner surface of the chute 3. Furthermore, the gate 4 may be configured so that its opening degree can be changed continuously or stepwise. When the gate 4 is configured so that its opening degree can be changed, the amount of the molded material charged into the carbonization furnace 1 can be controlled by controlling the opening degree of the gate 4. Furthermore, the gate 4 is provided near the exit of the chute 3 in order to prevent the powder SP from passing between the molded material particles LP and moving to the lower side of the molded material particles LP if the molded material has a long travel distance before passing through the gate 4 and reaching the carbonization furnace 1, that is, if the powder SP is blown away by gas and placed on the molded material particles LP, as described below.

[0023] The diffusion section 5 is provided downstream of the gate 4 in the charging direction of the molded material. The diffusion section 5 diffuses or disperses the molded material that has passed through the gate 4 in the width direction of the dry distillation furnace 1 (hereinafter referred to as the furnace width direction) when the molded material is charged into the inside of the dry distillation furnace 1. Specifically, the diffusion section 5 is provided between the first inclined surface 3A and the second inclined surface 3B of the chute 3 in the charging direction of the molded material. Although not shown in detail, the diffusion section 5 has a quadrangular pyramid shape as an example, and includes a triangular front inclined surface facing the dry distillation furnace 1 and triangular side inclined surfaces located on both sides of the front inclined surface. Each of the front inclined surface and the two side inclined surfaces descends from the chute 3 toward the charging port 2 side, and is a passing surface for the molded material. The furnace width direction is a direction perpendicular to each of the vertical direction and the depth direction of the dry distillation furnace 1.

[0024] At least a part of the chute 3 upstream of the gate 4 is provided with a gas injection device 6 that injects gas onto the molded product temporarily stored inside the chute 3, and blows off the powder SP of the molded product so that it lands on the molded product particles LP. The gas injection device 6 is connected to a gas supply source via a gas pipe (not shown), and an on-off valve (not shown) is provided on the gas pipe. The gas from the gas supply source is supplied to the chute 3 by opening the on-off valve, and the gas supply is stopped by closing the valve. Specifically, in the example shown in FIG. 1, a plurality of gas injection ports (not shown) are formed on the inner surface of the lower side of the chute 3 at regular intervals along the charging direction of the molded product, penetrating the chute 3 in the plate thickness direction. The gas injection ports are connected to the gas pipes and gas supply source described above, and gas is injected from each gas injection port into the inside of the chute 3, that is, from below the powder SP, by opening the on-off valve. Note that gas pipes may be installed inside the chute 3 along the inner surface of the lower side of the chute 3, and a plurality of gas injection ports may be formed on the gas pipes arranged in the chute 3. The gas injection device 6 is only required to be configured to inject gas into the inside of the chute 3, and to blow away the powder SP that tends to move below the molding particles LP so that it lands on top of the molding particles LP. The length of the gas injection device 6 in the charging direction of the moldings and the interval between the gas injection ports are preset by experiment.

[0025] The gas injection speed is set, for example, to a speed at which the powder SP is blown onto the molding particles LP, but the molding particles LP are not blown away, or the molding particles LP vibrate slightly, but do not particularly rise up. Specifically, the gas injection speed is set to 20 m / s or more and 30 m / s or less. If the gas injection speed is below 20 m / s, the powder SP cannot be blown away, and if it exceeds 30 m / s, the molding particles LP may also be blown away and collide with the inner surface of the chute 3, resulting in powderization.

[0026] Moreover, the gas injection device 6 is preferably configured to inject gas into the inside of the chute 3 when the gate 4 is closed, the molded products are supplied into the inside of the chute 3, and the molded products are flowing. This is to avoid the fact that if gas is injected when the molded products supplied into the inside of the chute 3 are completely or almost still, the amount of powder SP blown away by the gas and moving onto the molded product particle layer is reduced due to the large thickness of the molded product particle layer on the powder layer. In other words, when the molded products supplied into the inside of the chute 3 are completely or almost still, the molded product particle layer functions to suppress the movement of the powder SP caused by the gas, and this is to avoid this. Therefore, the gas injection device 6 is preferably configured to inject gas into the inside of the chute 3 when the gate 4 is closed and the powder SP and molded product particles LP supplied into the inside of the chute 3 maintain or hold their kinetic energy.

[0027] Furthermore, it is preferable that the gas injection device 6 continuously injects gas at least while the molded products are being supplied near the gate 4, that is, during the period from when the gate 4 is closed and the molded products start to be supplied inside the chute 3 until the gate is filled with the molded products. Alternatively, it is preferable to continuously inject gas during the period from when the molded products start to be supplied near the gate 4 until all the molded products to be charged into the dry distillation furnace 1 reach the vicinity of the gate 4. The above period is the period during which the molded products near the gate 4 continue to move, and this period can be obtained in advance by experiment. Also, since the thickness of the molded product particle layer near the gate 4 is relatively small or the molded product particles LP are in a floating state while the molded products are moving, the efficiency of moving the powder SP by the gas is improved.

[0028] The gas injected from the gas injection device 6 into the chute 3 is preferably an inert gas such as nitrogen, carbon dioxide, or a rare gas. Examples of rare gases include helium, neon, argon, krypton, and xenon. This is to suppress a reaction between the gas and the molded products when the molded products are dry distilled in the dry distillation furnace 1.

[0029] Next, the operation of the manufacturing apparatus shown in Fig. 1 will be described. Molded products containing carbon-containing materials (such as coal) and iron-containing materials (such as iron ore) that are raw materials for ferro-coke are supplied from a conveying means toward the chute 3. Here, as described above, a part of the molded product becomes powder SP during the conveying process, and the powder SP moves to the lower side of the molded product particles LP through the gaps between the molded product particles LP. Therefore, by the time the molded product reaches the chute 3, the molded product is in two layers: a layer of molded product particles LP (hereinafter referred to as molded product particle layer) and a layer of powder SP below it (hereinafter referred to as powder layer).

[0030] When the molded products are charged into the chute 3, the gate 4 provided on the outlet side of the chute 3 is in a closed state, and one batch of molded products is accumulated on the upstream side of the gate 4. If no external force such as gas injection is applied to the molded products from when they are supplied to the chute 3 until they are accumulated on the upstream side of the gate 4, the molded products accumulated on the upstream side of the gate 4 will be in a state of being separated into two layers, a molded product particle layer (upper layer) and a powder layer (lower layer). As described above, if the molded products separated into two layers are charged into the inside of the carbonization furnace 1 as they are, the molded product particles LP of the upper layer will fly to a position away from the charging port 2, while the powder SP of the lower layer may segregate near the charging port 2 of the carbonization furnace 1. Therefore, in the present invention, gas is injected from below onto the powder SP on the upstream side of the gate 4 to blow the powder SP onto the molded product particles LP.

[0031] Specifically, gas is injected from a plurality of injection ports during a certain period during which the molded product continues to move, from when the molded product starts being supplied to the inside of the chute 3 until the gate 4 is filled with the molded product. In this manner, the powder SP is blown off and floated up. Although a portion of the powder SP is restrained from moving by the molded product particles LP and remains below the lower layer, i.e., the molded product particle layer, most of the powder SP is blown off onto the upper layer of the molded product particle layer. FIG. 1 shows this state. After the gas is injected, the operator opens the gate 4, and the molded product moves toward the dry distillation furnace 1 with the powder layer on top of the molded product particle layer. The injection of gas may start when the operator starts supplying the molded product to the chute 3. Alternatively, a timing sensor (not shown) that detects that the molded product has been supplied to the chute 3 and outputs a signal may be provided upstream of the chute 3, and the gas injection device 6 may be started according to the output signal of the timing sensor to inject gas.

[0032] The molded products that have passed through the gate 4 pass through a diffusion section 5 that promotes dispersion or diffusion in the furnace width direction before falling into the interior of the carbonization furnace 1, which is installed at a lower position than the chute 3. Therefore, the molded products are charged into the carbonization furnace 1 from the charging opening 2 in a dispersed or diffused state in the furnace width direction. The diffusion section 5 has a structure in which its length in the furnace width direction is longer than that of the chute 3.

[0033] Therefore, according to the embodiment of the present invention, complete settling of the powder SP can be prevented or suppressed by injecting gas onto the powder SP near the outlet of the chute 3. That is, the molded material can be charged into the carbonization furnace 1 in a state where the powder layer and the molded material particle layer are upside down or in a state where the powder SP has entered the molded material particle layer. As a result, the powder SP is supplied both to a position away from the charging port 2 in the depth direction of the carbonization furnace 1 and to a position near the charging port 2 of the carbonization furnace 1, and segregation of the powder SP is mitigated. Therefore, it is possible to suppress the adverse effect of the segregation of the powder SP on the carbonization of the molded material, improve the quality of the blast furnace raw material charged into the blast furnace, and increase the productivity of the blast furnace raw material.

[0034] Next, an example carried out to confirm the action and effect of the present invention will be described. In this example, a test device simulating the ferro-coke manufacturing device shown in FIG. 1 was used, and the distribution of the molded materials in the depth direction of the test device when the molded materials were charged into the test device was investigated. Specifically, the molded material charging device, i.e., the chute, had a shape almost identical to that of the chute actually installed in the carbonization furnace 1. The chute was configured to inject nitrogen gas into the inside, and a gate was installed on the outlet side of the chute and a gas injection device was installed upstream of the gate. Furthermore, a diffusion section was installed downstream of the gate, and a collection box, which resembled the carbonization furnace 1, was installed downstream of the diffusion section.

[0035] A predetermined amount of molded products was charged into the collection box from the chute. The collection box was divided into four equal parts in the depth direction and five equal parts in the width direction (corresponding to the furnace width direction of the above-mentioned dry distillation furnace 1) to divide it into a total of twenty parts. The particle size of the molded products present in each divided space was investigated. Specifically, the molded products in each space were collected and sieved, the molded products remaining on the sieve were defined as molded product particles LP, and the molded products below the sieve were defined as powder SP, and the weights of the molded product particles LP and the powder SP were measured. A sieve with 20 mm mesh was used to sieve the molded products. Therefore, the particle size of the molded product particles LP was 20 mm or more in diameter, and the particle size of the powder SP was less than 20 mm in diameter. The powder ratio, that is, the weight ratio of the powder SP to the total amount of molded products in each space, was calculated. The powder ratio is obtained for each of the twenty spaces described above, but in the following description, the "maximum powder ratio" is shown as an index of segregation of the powder SP. The "maximum powder ratio" is the maximum value of the powder ratio obtained by comparing the powder ratios of the twenty spaces.

[0036] [Example 1] In Example 1, the effect of the installation position of the gas injection device on the maximum powder rate was investigated. The amount of molded material charged was set to 250 kg, the gas injection speed was set to 25 m / s, and the distance D between the downstream end of the gas injection device and the outlet of the chute, specifically, the diffusion section, was changed in the charging direction of the molded material. Gas was continuously injected by the gas injection device while the molded material was flowing in the vicinity of the gate. The gas injection time was set to 5 seconds. That is, gas injection was started almost at the same time as the supply of the molded material to the chute 3 was started, and this state was maintained for 5 seconds. The results are shown in FIG. 2. From the results shown in FIG. 2, it was recognized that in order to improve the dispersibility of the powder SP, it is preferable to install the gas injection device closer to the outlet of the chute.

[0037] [Example 2] In Example 2, the effect of the timing of gas injection on the maximum powder ratio was investigated. The amount of molded material charged was 250 kg, the gas injection speed was 25 m / s, the distance D between the downstream end of the gas injection device and the diffusion section in the charging direction of the molded material was 100 mm, and the gas injection time was 5 seconds. Then, (1) the case where gas injection was started while the molded material was flowing in the vicinity of the gate, that is, almost simultaneously with the start of supplying the molded material to the chute, and (2) the case where gas was injected after the molded material had completely stopped moving upstream of the gate were compared. The results are shown in FIG. 3. From the results shown in FIG. 3, it was recognized that (1) continuous gas injection while the molded material was flowing in the vicinity of the gate was effective in dispersing the powder SP.

[0038] [Example 3] In Example 3, the effect of the gas injection speed on the maximum powder ratio was investigated. The amount of molded material charged was 250 kg, the distance D between the downstream end of the gas injection device and the diffusion section in the charging direction of the molded material was set to 100 mm, the gas injection time was set to 5 seconds, and the gas injection speed was changed. The gas was injected continuously while the molded material was flowing in the vicinity of the gate. The results are shown in FIG. 4. From the results shown in FIG. 4, it was confirmed that the segregation of the powder SP can be suppressed by setting the gas injection speed to 20 m / s or more and 30 m / s or less. In FIG. 4, the cases where the gas injection speed is less than 20 m / s and the cases where it is more than 30 m / s are hatched. [Explanation of symbols]

[0039] 1. Carbonization furnace 2 charging ports 3 SHOTS 4 Gate 5 Diffusion section 6 Gas Injection Device SP powder LP molded particles

Claims

1. A manufacturing apparatus for blast furnace raw materials, comprising a chute for charging molded materials into a charging section, The molded product has a powder and molded product particles having a particle size larger than that of the powder, The charging section is a carbonization furnace for carbonizing the molded product, The chute is provided with a gas injection device that, while the molded product is flowing into the chute, continuously injects gas toward the molded product for a predetermined period of time, thereby blowing off the powder so that it lies on top of the molded product particles.

2. In the apparatus for producing raw materials for a blast furnace, the apparatus is provided with the chute according to claim 1, The gas injection device is configured to inject the gas from below the molded product, and the gas injection device is provided with a chute.

3. In the apparatus for producing raw materials for a blast furnace, the apparatus is provided with the chute according to claim 1 or 2, An apparatus for producing raw material for a blast furnace, comprising a chute, wherein the gas injection speed by the gas injection device is 20 m / s or more and 30 m / s or less.

4. In an apparatus for producing raw materials for a blast furnace, the apparatus is provided with the chute according to any one of claims 1 to 3, The gas injection device is provided upstream of a gate provided on the chute in the charging direction of the shaped material from the chute to the carbonization furnace.

5. In an apparatus for producing raw materials for a blast furnace, the apparatus is provided with the chute according to any one of claims 1 to 4, A manufacturing apparatus for blast furnace raw materials equipped with a chute, in which a diffusion section for diffusing the molded material in the width direction of the carbonization furnace is provided downstream of a gate provided on the chute in the charging direction of the molded material.

6. In an apparatus for producing raw materials for a blast furnace, the apparatus is provided with the chute according to any one of claims 1 to 5, The molding contains a carbon-containing material and an iron-containing material as components, and the molding is provided with a chute.

7. A method for producing raw materials for a blast furnace, comprising producing raw materials for a blast furnace using an apparatus for producing raw materials for a blast furnace, the apparatus comprising the chute according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Even distributing device of cascaded mixed coal low temperature pyrolysis

    CN207313530U

  • JP1979161345U

  • Dry dust separation device

    JP1980002497U

  • Apparatus for evenly feeding coal into coke oven