Thermoplastic norbornene resin, molded body and method for producing same
A thermoplastic norbornene resin with controlled molecular weight and glass transition temperature enhances adhesive strength and retardation in optical films, addressing the issues of low bonding strength and insufficient retardation in existing norbornene-based films.
Patent Information
- Application Number
- JP2023081986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2023-05-18
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2039-09-20
AI Technical Summary
Optical films made from thermoplastic norbornene resins often have low adhesive strength when bonded to other films and do not exhibit sufficient retardation properties, particularly in the thickness direction, which is crucial for image display devices like liquid crystal displays.
A thermoplastic norbornene resin with specific molecular weight and glass transition temperature ranges, containing a norbornene polymer hydride with controlled low molecular weight components, is developed to enhance birefringence and adhesive strength after stretching.
The resin achieves high adhesive strength and large retardation in the thickness direction, improving the performance of optical films in image display devices by suppressing delamination and maintaining optical properties in high-temperature environments.
Smart Images

Figure 0007567983000001 
Figure 0007567983000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic norbornene-based resin containing a hydrogenated norbornene-based polymer, a molded article thereof, and a method for producing the molded article. [Background technology]
[0002] Conventionally, optical films made of thermoplastic resins have been known. For example, Patent Documents 1 to 5 describe optical films made of thermoplastic norbornene-based resins. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-043740 A [Patent Document 2] JP 2006-235085 A [Patent Document 3] JP 2006-327112 A [Patent Document 4] JP 2008-114369 A [Patent Document 5] JP 2003-238705 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, optical films for use in image display devices such as liquid crystal display devices are required to have excellent retardation expression, and in particular, films that have excellent retardation Rth expression in the thickness direction are required. Therefore, from the viewpoint of realizing such films that have excellent retardation Rth expression in the thickness direction, there is a demand for the development of thermoplastic norbornene-based resins that have excellent birefringence expression.
[0005] In addition, optical films using thermoplastic norbornene-based resins are generally produced as stretched films. However, stretched films formed from thermoplastic norbornene-based resins tend to have low adhesive strength when bonded to other films. Therefore, there is a demand for the development of thermoplastic norbornene-based resins that can produce optical films with high adhesive strength.
[0006] The present invention has been made in view of the above-mentioned problems, and has an object to provide a thermoplastic norbornene-based resin which is excellent in the ability to express birefringence and which can obtain high adhesive strength after stretching; and a molded article formed from the thermoplastic norbornene-based resin and a method for producing the same. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that a thermoplastic norbornene-based resin that has a weight-average molecular weight Mw in a predetermined range, contains a hydrogenated norbornene-based polymer with a small amount of low-molecular-weight components having a molecular weight of 10,000 or less, and has a glass transition temperature Tg in a predetermined range, is excellent in the expression of birefringence, and can obtain high adhesive strength after stretching, thereby completing the present invention. That is, the present invention includes the following.
[0008] [1] A thermoplastic norbornene-based resin containing a hydrogenated norbornene-based polymer, The glass transition temperature Tg of the thermoplastic norbornene-based resin satisfies the following formula (1), The weight average molecular weight Mw of the hydrogenated product satisfies the following formula (2), A thermoplastic norbornene-based resin, wherein a ratio L of the hydrogenated species having a molecular weight of 10,000 or less to an amount (100%) of the hydrogenated species contained in the thermoplastic norbornene-based resin satisfies the following formula (3): (1) 105°C≦Tg≦120°C (2) 36,000 or less Mw (3) L≦10.5% [2] The birefringence Δn that appears when the thermoplastic norbornene resin is subjected to free end uniaxial stretching at 1.5 times the original length for 1 minute at Tg+15°C R The thermoplastic norbornene-based resin according to [1], which satisfies the following formula (4): (4) 0.0025≦Δn R [3] A molded article formed from the thermoplastic norbornene-based resin according to [1] or [2]. [4] The molded article according to [3], which is an optical film. [5] The molded article according to [4], wherein the photoelastic coefficient C of the optical film satisfies the following formula (5): (5) C≦10 Brewster [6] The molded article according to [4] or [5], wherein a retardation Rth in a thickness direction of the optical film and a thickness d of the optical film satisfy the following formula (6): (6) Rth / d≧3.5×10 -3 [7] A method for producing the molded article according to any one of [4] to [6], A step of preparing a pre-stretched film formed of the thermoplastic norbornene-based resin according to [1] or [2]; and stretching the unstretched film at a temperature equal to or higher than the glass transition temperature (Tg) of the thermoplastic norbornene-based resin + 9°C and at a stretching ratio of 1.8 times or more. Effect of the Invention
[0009] According to the present invention, it is possible to provide a thermoplastic norbornene-based resin which is excellent in the ability to express birefringence and which can obtain high adhesive strength after stretching; and a molded article formed from the thermoplastic norbornene-based resin and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below with reference to the embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0011] In the following description, the in-plane retardation Re of the film is a value expressed by Re = (nx - ny) x d, unless otherwise specified. The retardation Rth in the thickness direction of the film is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d, unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the film (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction perpendicular to the direction of nx. nz represents the refractive index in the thickness direction. d represents the thickness of the film. The measurement wavelength is 550 nm, unless otherwise specified.
[0012] In the following description, a "long" film refers to a film having a length of 5 times or more, preferably 10 times or more, the length of the film's width, specifically a film having a length sufficient to be wound into a roll for storage or transportation. The upper limit of the ratio of the length to the film's width is not particularly limited, but may be, for example, 100,000 times or less.
[0013] In the following description, unless otherwise specified, the term "polarizing plate" includes not only a rigid member but also a flexible member such as a resin film.
[0014] [1. Overview of thermoplastic norbornene resins] The thermoplastic norbornene resin according to one embodiment of the present invention is a thermoplastic resin containing a hydrogenated norbornene polymer. In the following description, the hydrogenated norbornene polymer contained in the thermoplastic norbornene resin may be referred to as a "norbornene hydrogenated product" as appropriate. The thermoplastic norbornene resin satisfies the following first to third requirements.
[0015] First, the glass transition temperature Tg of the thermoplastic norbornene-based resin satisfies the following formula (1). (1) 105°C≦Tg≦120°C
[0016] Secondly, the weight average molecular weight Mw of the norbornene hydride contained in the thermoplastic norbornene resin satisfies the following formula (2). (2) 36,000 or less Mw
[0017] Thirdly, the ratio L of norbornene hydrides having a molecular weight of 10,000 or less to the amount of norbornene hydrides contained in the thermoplastic norbornene resin (100%) satisfies the following formula (3). Hereinafter, the ratio L may be referred to as the "low molecular weight ratio L". (3) L≦10.5%
[0018] The thermoplastic norbornene-based resin according to the present embodiment, which satisfies the first to third requirements, is excellent in the expression of birefringence by stretching. In addition, the thermoplastic norbornene-based resin can obtain high adhesive strength after stretching. Therefore, by using the thermoplastic norbornene-based resin according to the present embodiment, an optical film having large retardation in the thickness direction and high adhesive strength can be obtained.
[0019] [2. Hydrogenated norbornene polymers] The norbornene-based hydrogenated product contained in the thermoplastic norbornene-based resin according to the present embodiment is a polymer containing a structure obtained by hydrogenating a norbornene-based polymer obtained by polymerizing a norbornene-based monomer. Thus, the norbornene-based hydrogenated product usually contains a structure obtained by hydrogenating a repeating structure obtained by polymerizing a norbornene-based monomer. Such norbornene-based hydrogenated products include, for example, hydrogenated products of one or more ring-opening polymers selected from the group consisting of a ring-opening polymer of a norbornene-based monomer and a ring-opening copolymer of a norbornene-based monomer and an arbitrary monomer; hydrogenated products of one or more addition polymers selected from the group consisting of an addition polymer of a norbornene-based monomer and an addition copolymer of a norbornene-based monomer and an arbitrary monomer; and the like. The norbornene-based hydrogenated product contained in the thermoplastic norbornene-based resin may be one type or two or more types.
[0020] A norbornene monomer is a monomer that contains a norbornene structure in the molecule. Examples of such norbornene monomers include bicyclo[2.2.1]hept-2-ene (common name: norbornene), tricyclo[4.3.0.1 2,5 ]Deca-3,7-diene (common name: dicyclopentadiene), tetracyclo[4.4.0.1 2,5 .1 7,10]Dodec-3-ene (trivial name: tetracyclododecene), and other norbornene monomers that do not contain an aromatic ring structure; norbornene monomers that have an aromatic substituent, such as 5-phenyl-2-norbornene, 5-(4-methylphenyl)-2-norbornene, 5-(1-naphthyl)-2-norbornene, and 9-(2-norbornen-5-yl)-carbazole; 1,4-methano-1,4,4a,4b,5,8,8a,9a-octahydrofluorene, 1,4-methano-1,4,4a,9a-tetrahydrofluorene (trivial name: meth norbornene-based monomers containing a norbornene ring structure and an aromatic ring structure in a condensed polycyclic structure, such as 1,4-methano-1,4,4a,9a-tetrahydrofluorene, 1,4-methano-1,4,4a,9a-tetrahydrodibenzofuran, 1,4-methano-1,4,4a,9a-tetrahydrocarbazole, 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene, and 1,4-methano-1,4,4a,9,10,10a-hexahydrophenanthrene; as well as derivatives of these compounds (for example, those having a substituent on the ring).
[0021] Examples of the substituent include alkyl groups such as methyl, ethyl, propyl, and isopropyl groups; alkylidene groups; alkenyl groups; and polar groups. Examples of the polar group include heteroatoms and atomic groups having heteroatoms. Examples of the heteroatoms include oxygen atoms, nitrogen atoms, sulfur atoms, silicon atoms, and halogen atoms. Specific examples of the polar group include halogen groups such as fluoro, chloro, bromo, and iodine groups; carboxyl groups; carbonyloxycarbonyl groups; epoxy groups; hydroxy groups; oxy groups; alkoxy groups; ester groups; silanol groups; silyl groups; amino groups; nitrile groups; sulfone groups; cyano groups; amide groups; and imide groups. The number of the substituents may be 1 or 2 or more. The types of the two or more substituents may be the same or different. However, from the viewpoint of obtaining a thermoplastic norbornene-based resin having a low saturated water absorption rate and excellent moisture resistance, it is preferable that the norbornene-based monomer has a small amount of polar groups, and it is more preferable that the norbornene-based monomer has no polar groups.
[0022] The norbornene monomer may be used alone or in combination of two or more kinds in any ratio.
[0023] The specific type and polymerization ratio of the norbornene monomer are preferably selected so as to obtain a thermoplastic norbornene resin having a desired glass transition temperature Tg. Usually, the glass transition temperature of a norbornene hydride depends on the type and polymerization ratio of the norbornene monomer that is the raw material of the norbornene hydride. Therefore, by appropriately adjusting the type and polymerization ratio of the norbornene monomer, the glass transition temperature of the norbornene hydride can be adjusted, so that the glass transition temperature Tg of the thermoplastic norbornene resin containing the norbornene hydride can be adjusted to satisfy formula (1).
[0024] From the viewpoint of obtaining high birefringence expression by setting the glass transition temperature Tg of the thermoplastic norbornene resin within the range of formula (1), it is preferable to use a tetracyclododecene monomer as the norbornene monomer. Therefore, the norbornene hydrogenated product is preferably a hydrogenated polymer of a monomer containing a tetracyclododecene monomer. Such a norbornene hydrogenated product usually contains a structure obtained by hydrogenating a repeating structure obtained by polymerizing a tetracyclododecene monomer (hereinafter, may be appropriately referred to as a "tetracyclododecene hydrogenated structure").
[0025] The tetracyclododecene monomer refers to a monomer selected from the group consisting of tetracyclododecene and tetracyclododecene derivatives. The tetracyclododecene derivative is a compound having a structure in which a substituent is bonded to the ring of tetracyclododecene. The number of the substituents may be one or more. The types of the two or more substituents may be the same or different. A preferred tetracyclododecene derivative is, for example, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ]-Dodec-3-ene (common name: ethylidenetetracyclododecene) 8-Ethyl-tetracyclo〔4.4.0.1 2,5 .1 7,10]-Dodec-3-ene, 8-ethoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene, 8-methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 The tetracyclododecene monomer may be used alone or in combination of two or more.
[0026] The proportion (polymerization ratio) of the tetracyclododecene monomer contained in the total amount of monomers as raw materials for the norbornene hydride (100% by weight) is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, particularly preferably 25% by weight or more, and preferably 50% by weight or less, more preferably 45% by weight or less, even more preferably 40% by weight or less, particularly preferably 35% by weight or less. When the polymerization ratio of the tetracyclododecene monomer is within the above range, the glass transition temperature of the norbornene hydride can be increased, and therefore the glass transition temperature Tg of the thermoplastic norbornene resin can be easily kept within the range of formula (1).
[0027] Usually, the ratio of a repeating structure (monomer unit) derived from a certain monomer in a norbornene-based hydrogenated product is equal to the ratio (polymerization ratio) of that monomer in the total amount of monomers. Therefore, the ratio of a tetracyclododecene-based hydrogenated structure in a norbornene-based hydrogenated product is equal to the polymerization ratio of the tetracyclododecene-based monomer to the total amount of monomers. Therefore, the ratio of the tetracyclododecene-based hydrogenated structure to 100% by weight of a norbornene-based hydrogenated product is preferably within the same range as the polymerization ratio of the tetracyclododecene-based monomer.
[0028] Furthermore, from the viewpoint of obtaining high birefringence expression by setting the glass transition temperature Tg of the thermoplastic norbornene resin within the range of formula (1), it is preferable to use a dicyclopentadiene monomer as the norbornene monomer. Therefore, the norbornene hydrogenated product is preferably a hydrogenated polymer of a monomer containing a dicyclopentadiene monomer. Such a norbornene hydrogenated product usually contains a structure obtained by hydrogenating a repeating structure obtained by polymerizing a dicyclopentadiene monomer (hereinafter, may be appropriately referred to as a "dicyclopentadiene hydrogenated structure").
[0029] The dicyclopentadiene monomer refers to a monomer selected from the group consisting of dicyclopentadiene and dicyclopentadiene derivatives. The dicyclopentadiene derivative is a compound having a structure in which a substituent is bonded to a dicyclopentadiene ring. The number of the substituents may be one or more. The types of the two or more substituents may be the same or different. The dicyclopentadiene monomer may be used alone or in combination of two or more.
[0030] The proportion (polymerization ratio) of the dicyclopentadiene monomer contained in the total amount of monomers as raw materials for the norbornene hydride (100% by weight) is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, particularly preferably 65% by weight or more, and is preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, particularly preferably 75% by weight or less. When the polymerization ratio of the dicyclopentadiene monomer is within the above range, the glass transition temperature of the norbornene hydride can be increased, and therefore the glass transition temperature Tg of the thermoplastic norbornene resin can be easily kept within the range of formula (1).
[0031] Usually, the ratio of the dicyclopentadiene-based hydrogenated structure in the norbornene-based hydrogenated product is equal to the polymerization ratio of the dicyclopentadiene-based monomer to the total amount of monomers. Therefore, the ratio of the dicyclopentadiene-based hydrogenated structure to 100% by weight of the norbornene-based hydrogenated product is preferably within the same range as the polymerization ratio of the dicyclopentadiene-based monomer.
[0032] In particular, when a tetracyclododecene monomer and a dicyclopentadiene monomer are used in combination as a norbornene monomer, it is preferable that the ratio of the amounts thereof is within a predetermined range. Specifically, the amount of the dicyclopentadiene monomer is preferably 100 parts by weight or more, more preferably 125 parts by weight or more, particularly preferably 150 parts by weight or more, and preferably 500 parts by weight or less, more preferably 450 parts by weight or less, and particularly preferably 400 parts by weight or less, relative to 100 parts by weight of the tetracyclododecene monomer. Therefore, in the norbornene hydrogenated product, the amount of the dicyclopentadiene hydrogenated structure is preferably 100 parts by weight or more, more preferably 125 parts by weight or more, particularly preferably 150 parts by weight or more, and preferably 500 parts by weight or less, more preferably 450 parts by weight or less, and particularly preferably 400 parts by weight or less, relative to 100 parts by weight of the tetracyclododecene hydrogenated structure. When the ratio is within the above range, the glass transition temperature of the norbornene hydride can be increased, so that the glass transition temperature Tg of the thermoplastic norbornene resin can be easily kept within the range of formula (1).
[0033] When using an arbitrary monomer to be copolymerized with a norbornene-based monomer, the type of the arbitrary monomer is not limited as long as a thermoplastic norbornene-based resin having a desired glass transition temperature Tg can be obtained. Examples of the arbitrary monomer capable of ring-opening copolymerization with a norbornene-based monomer include monocyclic olefins and derivatives thereof such as cyclohexene, cycloheptene, and cyclooctene; cyclic conjugated dienes and derivatives thereof such as cyclohexadiene and cycloheptadiene; and the like. Examples of the arbitrary monomer capable of addition copolymerization with a norbornene-based monomer include α-olefins having 2 to 20 carbon atoms such as ethylene, propylene, and 1-butene and derivatives thereof; cycloolefins and derivatives thereof such as cyclobutene, cyclopentene, and cyclohexene; non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, and 5-methyl-1,4-hexadiene; and the like. The optional monomers may be used alone or in combination of two or more kinds.
[0034] The norbornene-based hydrogenated product may be a norbornene-based polymer in which the non-aromatic unsaturated bond is hydrogenated, or a norbornene-based polymer in which the aromatic unsaturated bond is hydrogenated, or a norbornene-based polymer in which both the non-aromatic unsaturated bond and the aromatic unsaturated bond are hydrogenated. Among them, a norbornene-based hydrogenated product in which both the non-aromatic unsaturated bond and the aromatic unsaturated bond in the norbornene-based polymer are hydrogenated is preferred. By using a norbornene-based hydrogenated product in which both the non-aromatic unsaturated bond and the aromatic unsaturated bond are hydrogenated in this way, the photoelastic coefficient can be reduced. Furthermore, the mechanical strength, moisture resistance, heat resistance, and other properties of the thermoplastic norbornene-based resin can usually be effectively improved.
[0035] The glass transition temperature of the norbornene-based hydride is preferably 105°C or higher, more preferably 106°C or higher, particularly preferably 107°C or higher, and preferably 120°C or lower, more preferably 118°C or lower, particularly preferably 117°C or lower. A thermoplastic norbornene-based resin containing a norbornene-based hydride in which the type and polymerization ratio of the norbornene-based monomer are adjusted so as to have a glass transition temperature within the above range can increase the expression of birefringence due to stretching. Therefore, by using this thermoplastic norbornene-based resin, it is possible to obtain an optical film with a large retardation Rth in the thickness direction. In addition, usually, by using a norbornene-based hydride having such a high glass transition temperature, relaxation of the orientation of the norbornene-based hydride in a high-temperature environment can be suppressed. Therefore, excellent heat resistance can be achieved, and the change in the retardation Rth in the thickness direction of the optical film in a high-temperature environment can be suppressed.
[0036] The glass transition temperature of the norbornene-based hydride can be measured using a differential scanning calorimeter in accordance with JIS K 6911 at a temperature rise rate of 10° C. / min.
[0037] The glass transition temperature of the norbornene hydride can be adjusted, for example, by the type and polymerization ratio of the norbornene monomers used as the raw material of the norbornene hydride, and further by the low molecular weight fraction L.
[0038] The norbornene-based hydrogenated product has a weight-average molecular weight Mw that satisfies the above formula (2). In detail, the weight-average molecular weight Mw of the norbornene-based hydrogenated product is usually 36,000 or more, preferably 37,000 or more, and particularly preferably 38,000 or more. When the norbornene-based hydrogenated product having a large weight-average molecular weight Mw is contained as described above, the thermoplastic norbornene-based resin can exhibit a high degree of birefringence due to stretching. Furthermore, when the weight-average molecular weight Mw of the norbornene-based hydrogenated product is large in this way, the adhesive strength of the thermoplastic norbornene-based resin after stretching can be increased. The upper limit of the weight-average molecular weight Mw of the norbornene-based hydrogenated product is not particularly limited, but is preferably 50,000 or less, more preferably 47,000 or less, and particularly preferably 45,000 or less. When the weight-average molecular weight Mw of the norbornene-based hydrogenated product is equal to or less than the above upper limit, the moldability of the thermoplastic norbornene-based resin can be improved.
[0039] The weight average molecular weight Mw of norbornene hydrides can be measured in terms of polyisoprene by gel permeation chromatography using cyclohexane as the eluent. If norbornene hydrides are not soluble in cyclohexane, toluene can be used as the eluent. When the eluent is toluene, the weight average molecular weight Mw can be measured in terms of polystyrene.
[0040] The weight average molecular weight Mw of the norbornene-based hydride in the above range can be achieved, for example, by adjusting the polymerization conditions of the norbornene-based polymer so as to obtain a norbornene-based polymer with a high molecular weight, or by removing low molecular weight components from the norbornene-based hydride using an appropriate separation method. An example of the method of adjusting the polymerization conditions of the norbornene-based polymer so as to obtain a norbornene-based polymer with a high molecular weight is a method of reducing the amount of a chain transfer material. Also, an example of the method of removing low molecular weight components from the norbornene-based hydride using an appropriate separation method is a method of dissolving the norbornene-based hydride in a good solvent, then adding a poor solvent, and taking only the precipitated high molecular weight components.
[0041] The ratio (low molecular weight ratio) L of norbornene-based hydrides having a molecular weight of 10,000 or less to the amount of norbornene-based hydrides contained in the thermoplastic norbornene-based resin (100%) satisfies the following formula (3). In detail, the low molecular weight ratio L is usually 10.5% or less, preferably 10.3% or less, and particularly preferably 10% or less. The low molecular weight ratio L being small as described above indicates that the norbornene-based hydrides contain few low molecular weight components having a molecular weight of 10,000 or less. When the low molecular weight components of the norbornene-based hydrides are small in this way, the thermoplastic norbornene-based resin can increase the birefringence caused by stretching. Furthermore, when the low molecular weight components of the norbornene-based hydrides are small, the adhesive strength of the thermoplastic norbornene-based resin after stretching can be increased. There is no particular lower limit to the low molecular weight ratio L, and it is ideally 0%, but is usually 1% or more.
[0042] The low molecular weight fraction L can be calculated by measuring the molecular weight of the norbornene hydride by the gel permeation chromatography and integrating the amount of components with a molecular weight of 10,000 or less from the measured value.
[0043] The low molecular weight ratio L of the norbornene-based hydride in the above range can be achieved, for example, by adjusting the polymerization conditions of the norbornene-based polymer so as to obtain a norbornene-based polymer with a high molecular weight, or by removing low molecular weight components from the norbornene-based hydride using an appropriate separation method. An example of the method of adjusting the polymerization conditions of the norbornene-based polymer so as to obtain a norbornene-based polymer with a high molecular weight is to reduce the amount of a chain transfer material. Also, an example of the method of removing low molecular weight components from the norbornene-based hydride using an appropriate separation method is to dissolve the norbornene-based hydride in a good solvent, add a poor solvent, and then remove only the precipitated high molecular weight components.
[0044] The molecular weight distribution Mw / Mn of the norbornene-based hydride is preferably 2.4 or less, more preferably 2.3 or less, and particularly preferably 2.2 or less. When the molecular weight distribution Mw / Mn of the norbornene-based hydride is within the above range, the adhesive strength of the thermoplastic norbornene-based resin after stretching can be effectively increased. The molecular weight distribution is the ratio of the weight average molecular weight to the number average molecular weight, and is expressed as "weight average molecular weight Mw / number average molecular weight Mn". The lower limit of the molecular weight distribution of the norbornene-based hydride is usually 1.0 or more.
[0045] The molecular weight distribution Mw / Mn of norbornene-based hydrides can be calculated from the weight-average molecular weight Mw and number-average molecular weight Mn of norbornene-based hydrides. The number-average molecular weight Mn of norbornene-based hydrides can be measured in polyisoprene equivalent by gel permeation chromatography using cyclohexane as the eluent. If norbornene-based hydrides are not soluble in cyclohexane, toluene can be used as the eluent. When the eluent is toluene, the number-average molecular weight Mn can be measured in polystyrene equivalent.
[0046] Norbornene hydrides are excellent in the development of birefringence due to stretching. Therefore, norbornene hydrides usually have a large evaluated birefringence. The evaluated birefringence represents the birefringence developed when a material is subjected to free-end uniaxial stretching of 1.5 times for 1 minute at a stretching temperature 15°C higher than the glass transition temperature of the material.
[0047] In detail, the evaluated birefringence of the norbornene-based hydride is preferably 0.0025 or more, more preferably 0.00255 or more, and particularly preferably 0.0026 or more. A thermoplastic norbornene-based resin containing a norbornene-based hydride having such a large evaluated birefringence can exhibit a large birefringence by stretching. Therefore, an optical film having a large retardation Rth in the thickness direction can be easily manufactured. The upper limit of the evaluated birefringence of the norbornene-based hydride is not particularly limited, but is preferably 0.006 or less, more preferably 0.005 or less, and particularly preferably 0.004 or less. When the evaluated birefringence of the norbornene-based hydride is equal to or less than the upper limit, the retardation of the norbornene-based hydride can be easily adjusted.
[0048] Evaluation of norbornene-based hydrides The birefringence can be measured by the following method. A norbornene-based hydride is molded to obtain a sheet. This sheet is subjected to free-end uniaxial stretching. Free-end uniaxial stretching refers to stretching in one direction, in which no restraining force is applied to the sheet in any direction other than the stretching direction. The stretching temperature of the free-end uniaxial stretching is 15°C higher than the glass transition temperature of the norbornene-based hydride. The stretching time is 1 minute, and the stretching ratio of the free-end uniaxial stretching is 1.5 times. After stretching, the in-plane retardation of the center of the sheet is measured at a measurement wavelength of 550 nm, and the evaluated birefringence is obtained by dividing this in-plane retardation by the thickness of the center of the sheet.
[0049] The evaluated birefringence of the norbornene hydride can be adjusted, for example, by the type and polymerization ratio of the norbornene monomers used as raw materials for the norbornene hydride, as well as the weight average molecular weight Mw and low molecular weight proportion L of the norbornene hydride.
[0050] The stress birefringence of the norbornene-based hydride is preferably 2150×10 -12 Pa -1 More preferably, 2200×10 -12 Pa -1 More preferably, 2250×10 -12 Pa -1or more, preferably 4000×10 -12 Pa -1 Less than or equal to 3600×10 -12 Pa -1 Below, particularly preferably 3200×10 -12 Pa -1 or less. When the stress birefringence of the norbornene-based hydride is equal to or greater than the lower limit of the above range, the expression of birefringence by stretching the thermoplastic norbornene-based resin can be increased. Therefore, the thermoplastic norbornene-based resin can be used to easily manufacture an optical film having a large retardation Rth in the thickness direction. In addition, when the stress birefringence of the norbornene-based hydride is equal to or less than the upper limit of the above range, the retardation Re and Rth of the optical film manufactured using the thermoplastic norbornene-based resin can be easily controlled, and the in-plane variation of the retardation can be suppressed.
[0051] The stress birefringence of a norbornene-based hydride can be measured by the following method. A norbornene-based hydride is formed into a sheet to obtain a sheet. Both ends of the sheet are fixed with clips, and then a weight of a predetermined weight (for example, 55 g) is fixed to one of the clips. Next, the sheet is hung in an oven set to a predetermined temperature (for example, a temperature 15° C. higher than the glass transition temperature of the norbornene-based hydride) from the clip to which the weight is not fixed for a predetermined time (for example, 1 hour) to perform a stretching process. The sheet that has been stretched is slowly cooled to room temperature. The in-plane retardation of the sheet at the center of the sheet is measured at a measurement wavelength of 650 nm, and the in-plane retardation is divided by the thickness of the center of the sheet to calculate the δn value. Then, the stress birefringence can be obtained by dividing the δn value by the stress applied to the sheet (in the above case, the stress applied when the predetermined weight is fixed).
[0052] The stress birefringence of the norbornene hydride can be adjusted, for example, by the type and polymerization ratio of the norbornene monomers used as raw materials for the norbornene hydride, as well as the weight average molecular weight Mw and low molecular weight proportion L of the norbornene hydride.
[0053] The norbornene polymer can be produced, for example, by a production method including polymerizing a norbornene monomer and any optional monomer used as necessary in the presence of a suitable catalyst, and then contacting the obtained norbornene polymer with hydrogen in the presence of a hydrogenation catalyst containing a transition metal such as nickel, palladium, or ruthenium to hydrogenate the carbon-carbon unsaturated bonds, thereby producing the above-mentioned norbornene hydride.
[0054] The ratio of the norbornene hydride contained in the thermoplastic norbornene resin is not particularly limited. From the viewpoint of utilizing the excellent properties of the norbornene hydride, the ratio of the norbornene hydride contained in the thermoplastic norbornene resin is preferably 80% by weight to 100% by weight, more preferably 90% by weight to 100% by weight, and particularly preferably 95% by weight to 100% by weight.
[0055] [3. Optional components that may be contained in thermoplastic norbornene-based resin] The thermoplastic norbornene resin may contain any component other than the norbornene hydride in combination with the norbornene hydride. Examples of the optional components include ultraviolet absorbers, antioxidants, heat stabilizers, light stabilizers, antistatic agents, dispersants, chlorine scavengers, flame retardants, crystallization nucleating agents, reinforcing agents, antiblocking agents, antifogging agents, mold release agents, pigments, organic or inorganic fillers, neutralizing agents, lubricants, decomposers, metal deactivators, antifouling agents, and antibacterial agents. One type of optional component may be used alone, or two or more types may be used in combination at any ratio.
[0056] [4. Characteristics of thermoplastic norbornene resins] The thermoplastic norbornene resin has a glass transition temperature Tg that satisfies the above formula (1). In detail, the glass transition temperature Tg of the thermoplastic norbornene resin is usually 105°C or higher, preferably 106°C or higher, particularly preferably 107°C or higher, and usually 120°C or lower, preferably 118°C or lower, particularly preferably 117°C or lower. The thermoplastic norbornene resin having a glass transition temperature Tg in the above range can increase the expression of birefringence by stretching. Therefore, by using this thermoplastic norbornene resin, it is possible to obtain an optical film having a large retardation Rth in the thickness direction. In addition, by using a thermoplastic norbornene resin having such a high glass transition temperature Tg, the orientation relaxation of the norbornene hydride in a high temperature environment can usually be suppressed. Therefore, excellent heat resistance can be achieved, and the change in the retardation Rth in the thickness direction of the optical film in a high temperature environment can be suppressed.
[0057] The glass transition temperature Tg of the thermoplastic norbornene-based resin can be measured using a differential scanning calorimeter in accordance with JIS K 6911 at a temperature rise rate of 10° C. / min.
[0058] The glass transition temperature Tg of the thermoplastic norbornene resin can be adjusted, for example, by the type and polymerization ratio of the norbornene monomer used as the raw material of the norbornene hydride, the low molecular weight fraction L, and the content of the norbornene hydride.
[0059] Thermoplastic norbornene-based resins have a high tendency to develop birefringence due to stretching. Therefore, when a thermoplastic norbornene-based resin is stretched, a large birefringence is developed. For example, the thermoplastic norbornene-based resin preferably has an evaluated birefringence Δn that satisfies the following formula (4): R has. (4) 0.0025≦Δn R
[0060] In detail, the birefringence Δn of the thermoplastic norbornene resin is evaluated. Ris preferably 0.0025 or more, more preferably 0.00255 or more, and particularly preferably 0.0026 or more. R Thermoplastic norbornene-based resins having this structure can exhibit large birefringence by stretching. Therefore, optical films having large retardation Rth in the thickness direction can be easily manufactured. Evaluation of thermoplastic norbornene-based resins Birefringence Δn R The upper limit of is not particularly limited, but is preferably 0.006 or less, more preferably 0.005 or less, and particularly preferably 0.004 or less. R When it is equal to or less than the upper limit, the retardation of the thermoplastic norbornene resin can be easily adjusted.
[0061] Evaluation of thermoplastic norbornene resin birefringence Δn R can be measured by the following method. A thermoplastic norbornene resin is molded to obtain a sheet. This sheet is subjected to free-end uniaxial stretching. The stretching temperature of the free-end uniaxial stretching is a temperature 15°C higher than the glass transition temperature Tg of the thermoplastic norbornene resin (i.e., Tg+15°C). The stretching time is 1 minute, and the stretching ratio of the free-end uniaxial stretching is 1.5 times. After stretching, the in-plane retardation Re(a) at the center of the sheet is measured at a measurement wavelength of 550 nm, and the in-plane retardation Re(a) is divided by the thickness T(a) of the center of the sheet to obtain an evaluated birefringence Δn R is obtained.
[0062] Evaluation of thermoplastic norbornene resin birefringence Δn R can be adjusted, for example, by the type and polymerization ratio of the norbornene monomer used as the raw material of the norbornene hydride, the weight average molecular weight Mw and low molecular weight ratio L of the norbornene hydride, and the content of the norbornene hydride.
[0063] The thermoplastic norbornene resin has excellent adhesive strength after stretching. Therefore, when the thermoplastic norbornene resin is stretched and the stretched thermoplastic norbornene resin is bonded to any member, delamination can be suppressed. Considering that conventional resins containing norbornene polymers or their hydrogenated products are generally prone to delamination after stretching, the fact that the thermoplastic norbornene resin according to the present embodiment can suppress delamination after stretching is one of its excellent advantages.
[0064] Since the thermoplastic norbornene resin has a high glass transition temperature Tg, it usually has excellent heat resistance. Therefore, the thermoplastic norbornene resin is unlikely to cause molecular orientation relaxation in a high-temperature environment. Therefore, by using the thermoplastic norbornene resin, it is possible to realize an optical film capable of suppressing the change in the thickness direction retardation Rth in a high-temperature environment.
[0065] Stress birefringence C of thermoplastic norbornene resin R is preferably 2150 x 10 -12 Pa -1 More preferably, 2200×10 -12 Pa -1 More preferably, 2250×10 -12 Pa -1 or more, preferably 4000×10 -12 Pa -1 Less than or equal to 3600×10 -12 Pa -1 Below, particularly preferably 3200×10 -12 Pa -1 The stress birefringence C of thermoplastic norbornene resin is as follows. R When the stress birefringence C of the thermoplastic norbornene resin is larger than the lower limit of the range, the expression of birefringence by stretching the thermoplastic norbornene resin can be increased. Therefore, the thermoplastic norbornene resin can be used to easily produce an optical film having a large retardation Rth in the thickness direction. RWhen is equal to or less than the upper limit of the above range, the retardation Re and Rth of the optical film produced using the thermoplastic norbornene-based resin can be easily controlled, and the in-plane variation of the retardation can be suppressed.
[0066] Stress birefringence C of thermoplastic norbornene resin R can be measured by the following method. A thermoplastic norbornene resin is molded into a sheet to obtain a sheet. Both ends of the sheet are fixed with clips, and then a weight of a predetermined weight (for example, 55 g) is fixed to one of the clips. Next, the sheet is hung in an oven set to a predetermined temperature (for example, a temperature 15° C. higher than the glass transition temperature Tg of the thermoplastic norbornene resin) from the clip that does not have the weight fixed as the starting point for a predetermined time (for example, 1 hour) to perform a stretching process. The sheet that has been stretched is slowly cooled to room temperature. The in-plane retardation Re(b) of the sheet at the center is measured at a measurement wavelength of 650 nm, and the in-plane retardation Re(b) is divided by the thickness T(b) [mm] of the sheet center to calculate the Δn value. Then, the Δn value is divided by the stress applied to the sheet (in the above case, the stress applied when the predetermined weight is fixed) to obtain the stress birefringence C R can be sought.
[0067] Stress birefringence C R can be adjusted, for example, by the type and polymerization ratio of the norbornene monomer used as the raw material of the norbornene hydride, the weight average molecular weight Mw and low molecular weight ratio L of the norbornene hydride, and the content of the norbornene hydride.
[0068] [5. Molded body] The molded article according to one embodiment of the present invention is formed by the above-mentioned thermoplastic norbornene-based resin. The shape of the molded article is arbitrary, and may be a film, a syringe, a bag, a cup, a tube, or the like. In particular, from the viewpoint of utilizing the advantages of the thermoplastic norbornene-based resin, that is, excellent birefringence expression during stretching and high adhesive strength can be obtained after stretching, the molded article is preferably a molded article produced by a production method including a stretching process, more preferably a stretched film, and particularly preferably an optical film.
[0069] [6. Optical films] The optical film according to one embodiment of the present invention is a film formed of the above-mentioned thermoplastic norbornene-based resin. By utilizing the excellent birefringence expression of the thermoplastic norbornene-based resin, this optical film is preferably a retardation film having retardation. Furthermore, it is particularly preferable that the optical film has a large retardation Rth in the thickness direction.
[0070] The specific retardation Rth of the optical film in the thickness direction is preferably 150 nm or more, more preferably 200 nm or more, particularly preferably 250 nm or more, and is preferably 450 nm or less, more preferably 400 nm or less, particularly preferably 350 nm or less. When the retardation Rth of the optical film in the thickness direction is equal to or greater than the lower limit of the above range, the contrast in the oblique direction of the image display device including the optical film can be increased. When the retardation Rth of the optical film in the thickness direction is equal to or less than the upper limit of the above range, the in-plane variation of the retardation Rth and the orientation angle of the optical film in the thickness direction can be suppressed.
[0071] Furthermore, by utilizing the fact that the thermoplastic norbornene-based resin has a high birefringence, the optical film preferably has a large retardation Rth in the thickness direction per thickness d of the optical film. Specifically, the thickness d of the optical film and the retardation Rth in the thickness direction of the optical film preferably satisfy the following formula (6). (6) Rth / d≧3.5×10 -3
[0072] In particular, the ratio Rth / d is preferably 3.5×10 -3 More than 3.7×10 -3 More preferably, 3.8×10 -3 When the ratio Rth / d is equal to or greater than the lower limit, a thin optical film having a large retardation Rth in the thickness direction is realized. There is no particular upper limit to the ratio Rth / d, but from the viewpoint of reducing the stretching ratio and increasing the orientation angle precision of the optical film, it is preferably 8.0×10 -3 Less than or equal to 6.0×10 -3 The following is the result.
[0073] Furthermore, when the optical film is attached to a film such as a polarizing plate using an adhesive, the adhesive strength can be increased, making it difficult for the optical film to peel off, and thus suppressing delamination of the optical film.
[0074] It is preferable that the optical film has a small photoelastic coefficient C. Specifically, it is preferable that the photoelastic coefficient C of the optical film satisfies the following formula (5), where 1 Brewster=1×10 -13 cm 2 / dyn. (5) C≦10 Brewster
[0075] In detail, the specific photoelastic coefficient C of the optical film is preferably 10 Brewster or less, more preferably 9 Brewster or less, and particularly preferably 8 Brewster or less. When the photoelastic coefficient C of the optical film is small, the optical properties such as retardation are unlikely to change even if the optical film is warped. Therefore, when the optical film is provided in a liquid crystal display device, the occurrence of light leakage due to the warping of the optical film can be suppressed. Light leakage refers to a phenomenon in which, when the liquid crystal display device is in a black display state, light that should be blocked leaks out of the screen, making the screen brighter. There is no particular limit to the lower limit of the photoelastic coefficient, but it is preferably 0 Brewster or more, more preferably 0.5 Brewster or more, and particularly preferably 1 Brewster or more.
[0076] The photoelastic coefficient C of the optical film can be measured by an ellipsometer.
[0077] An optical film having a small photoelastic coefficient C can be realized, for example, by the optical film containing a norbornene-based hydride.
[0078] The in-plane retardation Re of the optical film is arbitrary depending on the use of the optical film. In terms of specific ranges, the in-plane retardation Re of the optical film is preferably 40 nm or more, more preferably 45 nm or more, particularly preferably 50 nm or more, and preferably 80 nm or less, more preferably 75 nm or less, particularly preferably 70 nm or less. When the in-plane retardation Re of the optical film is equal to or more than the lower limit of the above range, the optical compensation of the liquid crystal cell is easy to be performed. Also, when the in-plane retardation Re of the optical film is equal to or less than the upper limit of the above range, the in-plane variation of the retardation can be suppressed.
[0079] The optical film preferably has a high total light transmittance. The specific total light transmittance of the optical film is preferably 85% to 100%, more preferably 87% to 100%, and particularly preferably 90% to 100%. The total light transmittance can be measured in the wavelength range of 400 nm to 700 nm using a commercially available spectrophotometer.
[0080] The optical film preferably has a small haze in order to improve the image clarity of an image display device when the optical film is provided in the image display device. The haze of the optical film is preferably 1% or less, more preferably 0.8% or less, and particularly preferably 0.5% or less. The haze can be measured using a turbidimeter in accordance with JIS K7361-1997.
[0081] Since the optical film is formed of a thermoplastic norbornene resin having a high glass transition temperature Tg, the optical film usually has excellent heat resistance. Therefore, the molecules of the norbornene hydride contained in the optical film are unlikely to undergo orientation relaxation even in a high-temperature environment. Therefore, the optical film usually can suppress the change in the retardation Rth in the thickness direction in a high-temperature environment. The optical film having excellent heat resistance can be applied to an image display device that can be used in a high-temperature environment.
[0082] The heat resistance of the optical film can be evaluated by the change rate of the retardation Rth in the thickness direction due to a durability test in a high temperature environment. For example, after measuring the retardation Rth0 in the thickness direction of the optical film, the optical film is subjected to a durability test in which the optical film is stored in an environment of 85° C. for 500 hours. After the durability test, the retardation Rth1 in the thickness direction of the optical film is measured. Then, the change amount Rth1-Rth0 of the retardation in the thickness direction of the optical film due to the durability test is divided by the retardation Rth0 in the thickness direction of the optical film before the durability test to calculate the change rate. According to the optical film according to this embodiment, the change rate of the retardation Rth in the thickness direction can be preferably -3.0% to 3.0%, more preferably -2.9% to 2.9%, and particularly preferably -2.8% to 2.8%.
[0083] The optical film is preferably thin. By using the above-mentioned thermoplastic norbornene-based resin, even if the optical film is thin, a large retardation Rth in the thickness direction can be obtained. In addition, when the optical film is thin, the warping of the optical film can be suppressed, so that the change in optical properties such as retardation due to the warping can be reduced. Therefore, when the optical film is provided in a liquid crystal display device, the occurrence of light leakage due to the warping of the optical film can be suppressed. The specific thickness d of the optical film is preferably 120 μm or less, more preferably 100 μm or less, and particularly preferably 80 μm or less. There is no particular limit to the lower limit of the thickness d, but from the viewpoint of suppressing delamination, it is preferably 20 μm or more, more preferably 30 μm or more, and particularly preferably 40 μm or more.
[0084] The optical film described above can be produced, for example, by a production method including a step of preparing a resin film formed of a thermoplastic norbornene-based resin and a step of stretching the resin film. In order to distinguish the resin film before stretching from the optical film obtained after stretching, the resin film before stretching may be referred to as a "film before stretching" as appropriate hereinafter.
[0085] The step of preparing a pre-stretched film usually includes forming a thermoplastic norbornene-based resin to obtain a pre-stretched film. In this case, there is no limitation on the method of forming the thermoplastic norbornene-based resin. Examples of the forming method include extrusion molding, solution casting, and inflation molding. Among them, extrusion molding and solution casting are preferred, and extrusion molding is particularly preferred.
[0086] After preparing the pre-stretched film, a process of stretching the pre-stretched film is carried out. This stretching orients the norbornene-based hydride molecules in the film, so that an optical film having the above-mentioned optical properties is obtained. The stretching conditions in the process of stretching the pre-stretched film can be set arbitrarily within a range in which a desired optical film can be obtained.
[0087] The stretching mode of the pre-stretched film may be, for example, uniaxial stretching in which stretching is performed in one direction, or biaxial stretching in which stretching is performed in two non-parallel directions. The biaxial stretching may be simultaneous biaxial stretching in which stretching is performed simultaneously in two directions, or sequential biaxial stretching in which stretching is performed in one direction and then stretching in the other direction. Among these, from the viewpoint of easily producing an optical film having a large retardation Rth in the thickness direction, biaxial stretching is preferred, and sequential biaxial stretching is more preferred.
[0088] The stretching direction of the pre-stretched film can be set arbitrarily. For example, when the pre-stretched film is a long film, the stretching direction may be a longitudinal direction, a transverse direction, or an oblique direction. The longitudinal direction refers to the length direction of the long film, the transverse direction refers to the width direction of the long film, and the oblique direction refers to a direction that is neither parallel nor perpendicular to the length direction of the long film.
[0089] The stretching ratio of the film before stretching is preferably 1.8 or more, more preferably 1.9 or more, particularly preferably 2.0 or more, and preferably 2.6 or less, more preferably 2.5 or less, particularly preferably 2.4 or less. When the stretching ratio is equal to or more than the lower limit of the above range, an optical film having a large retardation Rth in the thickness direction can be easily obtained. When the stretching ratio is equal to or less than the upper limit of the above range, the orientation angle precision of the optical film can be easily improved. When performing biaxial stretching, it is preferable that the total stretching ratio, which is expressed as the product of the stretching ratio in one direction and the stretching ratio in the other direction, falls within the above range.
[0090] The stretching temperature of the film before stretching is preferably Tg+9° C. or more, more preferably Tg+9.5° C. or more, particularly preferably Tg+10° C. or more, and is preferably Tg+25° C. or less, more preferably Tg+23° C. or less, particularly preferably Tg+20° C. or less. When the stretching temperature is within the above range, it is easy to make the thickness of the optical film uniform.
[0091] In the above-mentioned production method, as described above, an optical film can be obtained by stretching the pre-stretched film, but the above-mentioned production method may further include any optional step. For example, the manufacturing method may include a step of trimming the optical film, a step of subjecting the optical film to a surface treatment, and the like.
[0092] [7. Optical laminate] The optical laminate can be obtained by using the optical film described above. This optical laminate includes the optical film described above and a polarizing plate. Since the optical film can be thinned even if the retardation Rth in the thickness direction is large, the optical laminate can be thinned and warping of the optical laminate can be suppressed. In addition, since the optical film has high adhesive strength, peeling between the optical film and the polarizing plate can be suppressed. Furthermore, since the optical film has high heat resistance, the optical laminate can also have high heat resistance. Such an optical laminate can be suitably applied to an image display device such as a liquid crystal display device.
[0093] The polarizing plate may be, for example, a film having a polarizer layer. The polarizer layer may be, for example, a film of a suitable vinyl alcohol polymer that has been subjected to suitable treatment in a suitable order and manner. Examples of such vinyl alcohol polymers include polyvinyl alcohol and partially formalized polyvinyl alcohol. Examples of film treatments include dyeing with iodine and a dichroic substance such as a dichroic dye, stretching, and crosslinking. The polarizer layer is capable of absorbing linearly polarized light having a vibration direction parallel to the absorption axis, and is preferably excellent in polarization degree. The thickness of the polarizer layer is generally 5 μm to 80 μm, but is not limited thereto.
[0094] The polarizing plate may have a protective film layer on one or both sides of the polarizer layer to protect the polarizer layer. Any transparent film layer can be used as the protective film layer. Among them, a film layer of a resin excellent in transparency, mechanical strength, thermal stability, moisture shielding property, etc. is preferable. Examples of such resins include acetate resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, thermoplastic norbornene resins, (meth)acrylic resins, etc. Among them, acetate resins, thermoplastic norbornene resins, and (meth)acrylic resins are preferable in terms of small birefringence, and thermoplastic norbornene resins are particularly preferable in terms of transparency, low moisture absorption, dimensional stability, light weight, etc.
[0095] The polarizing plate can be produced, for example, by laminating a polarizer layer and a protective film layer. When laminating them, an adhesive may be used, if necessary.
[0096] The optical laminate may further include any optional member in combination with the optical film and the polarizing plate. For example, the optical laminate may include an adhesive layer for bonding the optical film and the polarizing plate together.
[0097] The thickness of the optical laminate is not particularly limited, but is preferably 30 μm or more, more preferably 50 μm or more, and is preferably 150 μm or less, more preferably 130 μm or less.
[0098] [8.Liquid crystal display device] The optical laminate described above can be provided in a liquid crystal display device. As described above, the optical film provided in the optical laminate can be made thin, so the optical laminate is less likely to warp. Therefore, it is possible to suppress the occurrence of light leakage due to changes in the optical properties of the optical film at the warped portion. The warping is generally likely to occur at the corners of the screen of a liquid crystal display device, but a liquid crystal display device provided with the optical laminate can suppress light leakage at such corners. In addition, since the optical film has high heat resistance, the liquid crystal display device can suppress changes in display properties in a high-temperature environment.
[0099] Typically, a liquid crystal display device includes a liquid crystal cell and an optical laminate on at least one side of the liquid crystal cell. In particular, the optical laminate is preferably provided such that the liquid crystal cell, the optical film, and the viewing-side polarizer are arranged in this order. In such a configuration, the optical film can function as a viewing angle compensation film.
[0100] The liquid crystal cell may be in any mode, such as in-plane switching (IPS) mode, vertical alignment (VA) mode, multi-domain vertical alignment (MVA) mode, continuous spin wheel alignment (CPA) mode, hybrid alignment nematic (HAN) mode, twisted nematic (TN) mode, super twisted nematic (STN) mode, or optically compensated bend (OCB) mode. EXAMPLES
[0101] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and may be modified and practiced as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. The following operations were carried out in air at room temperature and normal pressure unless otherwise specified.
[0102] [I. Methods for measuring and calculating physical properties of polymers] (Method of measuring weight average molecular weight Mw of polymer) The weight-average molecular weight Mw of the polymer was measured by gel permeation chromatography (GPC) using cyclohexane as an eluent, and was calculated in terms of standard polyisoprene. As the standard polyisoprene, standard polyisoprene manufactured by Tosoh Corporation (Mw=602, 1390, 3920, 8050, 13800, 22700, 58800, 71300, 109000, 280000) was used. The measurements were performed using three Tosoh columns (TSKgel G5000HXL, TSKgel G4000HXL, and TSKgel G2000HXL) connected in series under conditions of a flow rate of 1.0 mL / min, a sample injection amount of 100 μL, and a column temperature of 40°C.
[0103] (Method for measuring the low molecular weight fraction L of a polymer) The low molecular weight fraction L of the polymer was calculated by integrating the amount of components having a molecular weight of 10,000 or less from the measured molecular weight measured by GPC in the above (Method for measuring weight average molecular weight Mw of polymer).
[0104] (Method of measuring glass transition temperature Tg) The glass transition temperature Tg was measured using a differential scanning calorimeter ("DSC6220SII" manufactured by Nano Technology Corporation) in accordance with JIS K 6911 at a temperature rise rate of 10°C / min.
[0105] (Evaluated birefringence Δn R (Method of measurement) The resin was molded into a sheet of 50 mm length × 100 mm width × 100 μm thickness to obtain a sample sheet. The sample sheet was subjected to free-end uniaxial stretching using a thermostatic tensile tester (Instron Japan Co., Ltd. "5564"). The stretching conditions were as follows. Stretching temperature: Tg+15℃ Chuck distance: 65mm Stretching ratio: 1.5x (stretching distance 32.5mm) Extension time: 1 minute Stretching speed: 32.5mm / min
[0106] After the stretching treatment, the stretched sample sheet was returned to room temperature to obtain a measurement sample.
[0107] The in-plane retardation Re(a) [nm] of the center of the measurement sample was measured at a wavelength of 550 nm using a phase difference meter (AXOMETRICS "AXOSCAN"). The thickness T(a) [mm] of the center of the measurement sample was also measured. Using these measured values Re(a) and T(a), the evaluated birefringence Δn of the resin was calculated according to the following formula (X1): R was calculated. Δn R =Re(a)×(1 / T(a))×10 -6 (X1)
[0108] (Stress birefringence C R (Method of measurement) The resin was molded into a sheet of 35 mm length x 10 mm width x 1 mm thickness to obtain a sample sheet. Both ends of the sample sheet were fixed with clips, and then a weight of 55 g was fixed to one of the clips. Next, the sample sheet was hung for 1 hour in an oven set to the glass transition temperature Tg+15°C of the resin, starting from the clip to which the weight was not fixed, and stretched. The sample sheet was then slowly cooled to room temperature to obtain a measurement sample.
[0109] The in-plane retardation Re(b) [nm] of the center of the sample was measured at a wavelength of 650 nm using a birefringence meter (Photonic Lattice's "WPA-100"). The thickness T(b) [mm] of the center of the sample was also measured. Using these measured values Re(b) and T(b), the Δn value was calculated according to the following formula (X2). δn=Re(b)×(1 / T(b))×10 -6 (X2) Using the Δn value and the stress F applied to the sample, the stress birefringence C is calculated by the following formula (X3). R was calculated. CR =δn / F (X3)
[0110] [II. Evaluation method of optical film properties] (Method of measuring retardation Rth, Re of optical film) The retardation in the thickness direction Rth and the in-plane retardation Re of the optical film were measured at a measurement wavelength of 550 nm using a phase difference meter (AXOMETRICS "AXOSCAN").
[0111] (Method of measuring film thickness) The thickness of the film was measured using a snap gauge ("ID-C112BS" manufactured by Mitutoyo Corporation).
[0112] (Method of measuring the photoelastic coefficient of optical film) The photoelastic coefficient of the optical film was measured by an ellipsometer.
[0113] (Method for measuring the rate of change in retardation Rth in the thickness direction of an optical film after 500 hours at 85°C) Before the durability test described below, the retardation Rth0 in the thickness direction of the optical film was measured. Then, the optical film was subjected to a durability test in which the optical film was stored in an environment of 85°C for 500 hours. After the durability test, the retardation Rth1 in the thickness direction of the optical film was measured. From these measured values Rth0 and Rth1, the change rate of retardation in the thickness direction of the optical film due to the durability test (Rth change rate) was calculated according to the following formula (X4). The closer the Rth change rate is to zero, the more excellent the heat resistance of the optical film is. Rth change rate (%)={(Rth1-Rth0) / Rth0}×100 (X4)
[0114] (Method of measuring adhesive strength of optical film) As an adherend, an unstretched film formed of a resin containing a norbornene-based polymer ("ZEONORFILM" manufactured by ZEON CORPORATION, thickness 100 μm, glass transition temperature of resin 160° C., not stretched) was prepared. One side of the optical film as the measurement target film and one side of the unstretched film were subjected to corona treatment. An adhesive (UV adhesive CRB series manufactured by TOYOCHEM CORPORATION) was attached to both the corona-treated side of the optical film and the corona-treated side of the unstretched film. The adhesive-attached sides were then bonded together. Thereafter, the adhesive was irradiated with ultraviolet light using an electrodeless UV irradiation device (manufactured by Heraeus) to cure the adhesive. The ultraviolet light irradiation was performed using a D bulb as a lamp with a peak illuminance of 100 mW / cm. 2 , Accumulated light intensity 3000mJ / cm 2 As a result, a sample film having a layer structure of unstretched film / adhesive layer / optical film was obtained.
[0115] The obtained sample films were subjected to a 90 degree peel test according to the following procedure. The sample film was cut to a width of 15 mm to obtain a film piece. The optical film side of this film piece was attached to the surface of a slide glass using an adhesive. In this case, a double-sided adhesive tape (manufactured by Nitto Denko Corporation, product number "CS9621") was used as the adhesive. The unstretched film included in the film piece was clamped at the tip of a high-performance digital force gauge (manufactured by Imada Co., Ltd., "ZP-5N"), and the unstretched film was pulled at a speed of 300 mm / min in the normal direction to the surface of the slide glass, and the magnitude of the pulling force was measured as the adhesive strength.
[0116] [Example 1] (1-1) Preparation of norbornene ring-opening polymer: In a glass reaction vessel with the inside replaced with nitrogen, 200 parts of dehydrated cyclohexane, 0.7 mol% of 1-hexene, 0.15 mol% of diisopropyl ether, and 0.44 mol% of triisobutylaluminum were placed in the reactor at room temperature relative to 100 parts by weight of the monomers described below, and mixed. Thereafter, while maintaining the temperature at 45°C, 70 wt% of dicyclopentadiene (DCPD) and 30 wt% of tetracyclododecene (TCD) as monomers, and 0.02 mol% of tungsten hexachloride (0.65 wt% toluene solution) were continuously added in parallel to the reactor over a period of 2 hours to polymerize. Next, 0.2 mol% of isopropyl alcohol was added to the polymerization solution to inactivate the polymerization catalyst and terminate the polymerization reaction. In the above explanation, the amount indicated by the unit "mol%" is a value based on 100 mol% of the total amount of the monomers. The weight average molecular weight Mw of the obtained norbornene ring-opening polymer was 3.1 x 10 4 The conversion rate of the monomer to the polymer was 100%.
[0117] (1-2) Production of norbornene-based hydrides by hydrogenation: Next, 67 g of cyclohexane was added to 183 g of the reaction solution containing the norbornene-based ring-opening polymer obtained in the above step (1-1), and 1.8 wt % of a nickel catalyst supported on diatomaceous earth ("T8400RL" manufactured by JGC Chemical Industries, Ltd., nickel loading rate 57%) was further added as a hydrogenation catalyst. The amount of hydrogenation catalyst is expressed as a value relative to 100 wt % of the norbornene-based ring-opening polymer contained in the reaction solution. Thereafter, the reaction solution was pressurized to 4.5 MPa with hydrogen and heated to a temperature of 190° C. while stirring, and the hydrogenation reaction was carried out for 8 hours. As a result, a reaction solution containing a norbornene-based hydrogenated product as a hydrogenated product of the norbornene-based ring-opening polymer was obtained.
[0118] The reaction solution was filtered under pressure at a pressure of 0.25 MPa (Fundaback Filter, manufactured by Ishikawajima-Harima Heavy Industries Co., Ltd.) using Radiolite #500 as a filter bed to remove the hydrogenation catalyst, and a colorless, transparent solution was obtained. The resulting solution was poured into a large amount of isopropanol to precipitate a norbornene-based hydrogenated product. After filtering out the precipitated norbornene-based hydrogenated product, 2.0 parts of a xylene solution containing 0.1 parts of an antioxidant [pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Ciba Specialty Chemicals, product name "Irganox (registered trademark) 1010") was added per 100 parts of norbornene-based hydrogenated product. The mixture was then dried in a vacuum dryer (200°C, 1 Torr) for 6 hours to obtain a thermoplastic norbornene-based resin. The weight-average molecular weight of the norbornene-based hydrogenated product was 4.4 × 10 4 The proportion L of low molecular weight molecules with a molecular weight of 10,000 or less was 10%.
[0119] Glass transition temperature Tg and evaluated birefringence Δn of thermoplastic norbornene resin R , and stress birefringence C R The glass transition temperature Tg of the thermoplastic norbornene resin was 115.5°C, and the evaluated birefringence Δn R is 0.0030, stress birefringence C R is 2360 x 10 -12 Pa -1 It was.
[0120] (1-3) Preparation of pre-stretched film: The thermoplastic norbornene resin obtained in the above step was fed into a twin-screw extruder and molded into a strand-shaped molded body by hot melt extrusion molding. The molded body was chopped with a strand cutter to obtain pellets of the thermoplastic norbornene resin.
[0121] The pellets were dried at 80° C. for 5 hours. Thereafter, the pellets were fed to an extruder by a conventional method and melted at 250° C. The molten thermoplastic norbornene-based resin was extruded from a die onto a cooling drum to obtain a long unstretched film having a thickness of 150 μm.
[0122] (1-4) Manufacturing of optical films: A longitudinal stretching machine using a float method between rolls was prepared. Using this longitudinal stretching machine, the pre-stretched film was stretched in the longitudinal direction by 1.35 times to obtain an intermediate film. The stretching temperature in the longitudinal stretching machine was 125.5°C, which was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene resin (Tg+10°C).
[0123] The intermediate film was then fed to a transverse stretching machine using a tenter method, and stretched 1.65 times in the transverse direction while adjusting the take-up tension and the tenter chain tension to obtain an optical film as a biaxially stretched film. The stretching temperature in the transverse stretching machine was 131.5°C, which was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene resin (Tg+16°C). The obtained optical film had an in-plane retardation Re of 60 nm, a thickness retardation Rth of 360 nm, and a thickness d of 78 μm. The obtained optical film was evaluated by the above-mentioned methods.
[0124] [Example 2] The combination of monomers used in the above step (1-1) was changed to 29% by weight of tetracyclododecene (TCD), 68% by weight of dicyclopentadiene (DCPD), and 3% by weight of ethylidenetetracyclododecene (ETD). In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 123.7°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 129.7°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0125] [Example 3] The combination of monomers used in the above step (1-1) was changed to 29% by weight of tetracyclododecene (TCD), 70% by weight of dicyclopentadiene (DCPD), and 1% by weight of norbornene (NB). In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 120.5°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 126.5°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0126] [Example 4] The combination of monomers used in the above step (1-1) was changed to 28% by weight of tetracyclododecene (TCD), 70% by weight of dicyclopentadiene (DCPD), and 2% by weight of norbornene (NB). In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 117.6°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 123.6°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0127] [Comparative Example 1] The combination of monomers used in the step (1-1) was changed to 10% by weight of methanotetrahydrofluorene (MTF), 40% by weight of tetracyclododecene (TCD), and 50% by weight of dicyclopentadiene (DCPD). Furthermore, the polymerization temperature in the step (1-1) was changed to 55°C. In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 137.5°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 143.5°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0128] [Comparative Example 2] The combination of monomers used in the step (1-1) was changed to 5% by weight of tetracyclododecene (TCD), 80% by weight of dicyclopentadiene (DCPD), and 15% by weight of ethylidenetetracyclododecene (ETD). Furthermore, the polymerization temperature in the step (1-1) was changed to 55°C. In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 114.2°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 120.2°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0129] [Comparative Example 3] The combination of monomers used in the above step (1-1) was changed to 29% by weight of tetracyclododecene (TCD), 68% by weight of dicyclopentadiene (DCPD), and 3% by weight of ethylidenetetracyclododecene (ETD). In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 123°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 129.0°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0130] [Comparative Example 4] The combination of monomers used in the above step (1-1) was changed to 29% by weight of tetracyclododecene (TCD), 68% by weight of dicyclopentadiene (DCPD), and 3% by weight of ethylidenetetracyclododecene (ETD). Furthermore, the amount of 1-hexene was changed to 0.68 mol%. In the above-mentioned step (1-4), the stretching temperature in the machine direction was changed to 123°C. This stretching temperature was 10°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+10°C). In addition, in the above-mentioned step (1-4), the stretching temperature in the transverse direction was changed to 129.0°C. This stretching temperature was 16°C higher than the glass transition temperature Tg of the thermoplastic norbornene-based resin (Tg+16°C). Except for the above, the same procedures as in Example 1 were carried out to produce and evaluate a thermoplastic norbornene-based resin and an optical film.
[0131] [result] The results of the above-mentioned Examples and Comparative Examples are shown in Tables 1 and 2 below.
[0132] [Table 1]
[0133] [Table 2]
Claims
1. A molded article formed from a norbornene-based resin, The norbornene-based resin is a thermoplastic norbornene-based resin containing a hydrogenated norbornene-based polymer, The glass transition temperature Tg of the thermoplastic norbornene-based resin satisfies the following formula (1), The weight average molecular weight Mw of the hydrogenated product satisfies the following formula (2): a ratio L of the hydrogenated substance having a molecular weight of 10,000 or less to the amount of the hydrogenated substance contained in the thermoplastic norbornene-based resin (100%) satisfies the following formula (3): The birefringence Δn that appears when the thermoplastic norbornene resin is subjected to free end uniaxial stretching at 1.5 times its original length for 1 minute at Tg+15° C. R satisfies the following formula (4), (1) 105° C.≦Tg≦120° C. (2) 36,000≦Mw (3) L≦10.5% (4)0.0025≦Δn R The stress birefringence C of the thermoplastic norbornene resin R is 2250 x 10 -12 P -1 That's all. The molded article is an optical film, The photoelastic coefficient C of the optical film satisfies the following formula (5): (5) C≦10 Brewster
2. The molded article according to claim 1 , wherein a retardation Rth in a thickness direction of the optical film and a thickness d of the optical film satisfy the following formula (6): (6)Rth / d≧3.5×10 -3
3. A method for producing the molded body according to claim 1 or 2, preparing a pre-stretched film formed of the thermoplastic norbornene-based resin; and stretching the pre-stretched film at a temperature equal to or higher than a glass transition temperature (Tg) of the thermoplastic norbornene-based resin + 9°C to a stretching ratio of 1.8 times or more.
Citation Information
Patent Citations
Norbornene-based polymer and its production
JP1998139865A
Thermoplastic norbornene resin optical film
JP2003238705A
Optical compensation film and liquid crystal display device
JP2005043740A
Oriented polyolefin film
JP2006235085A
Three-component norbornene-based polymer excellent in strength in adhesion of sebum and method for producing the same
JP2006241204A