Coating composition and cured product
Patent Information
- Application Number
- JP2024517478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-07
- Filing Date
- 2023-06-15
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2043-06-15
Smart Images

Figure 0007568169000001 
Figure 0007568169000002 
Figure 0007568169000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating composition and a cured product thereof. In particular, the present invention relates to a coating composition capable of giving a cured product (coating) having excellent substrate adhesion, chemical resistance, and solvent resistance required in various fields such as automobile interior / exterior coatings, home appliances, paints for building materials, and film coating agents, and to a cured product obtained by using the coating composition. [Background technology]
[0002] Coating compositions used in automobiles, home appliances, building materials, etc. are required to have various properties such as chemical resistance, scratch resistance, adhesion to substrates, etc. The NCO-OH curing system, which reacts isocyanate groups (NCO) with hydroxyl groups (OH), is commonly used as a curing system that satisfies these required properties.
[0003] In the NCO-OH curing system, an isocyanate compound is used as a curing agent for paints and the like, and an organic tin compound such as dibutyltin oxide or dibutyltin dilaurate is generally used as a catalyst to promote the curing reaction using an isocyanate compound (see Patent Document 1).
[0004] Although organotin compounds have high catalytic performance, their toxicity has become a problem in recent years, and there is a demand for alternative catalysts to organotin compounds.
[0005] In addition, while the NCO-OH curing system is highly versatile, it has problems with storage stability and handling, such as being susceptible to the effects of moisture in the air and a short pot life after mixing an isocyanate compound as a curing agent.
[0006] Furthermore, isocyanate compounds are also problematic due to their toxicity to the body and a shortage of raw materials, and there is a demand for non-NCO-OH curing systems that do not use isocyanate compounds as curing agents and have excellent adhesion to substrates and chemical resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-307800 A Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to provide a coating composition that can give a cured product (coating) that has excellent substrate adhesion, chemical resistance, and solvent resistance without using an isocyanate-based curing agent, and the cured product. [Means for solving the problem]
[0009] As a result of extensive research, the present inventors have found that a cured product (coating) having excellent adhesion to substrates, chemical resistance, and solvent resistance can be obtained by using a coating composition containing an acrylic resin obtained by blending specific monomers in a specific ratio, an acrylate compound having crosslinking properties, and a specific base catalyst, and have thus completed the present invention.
[0010] That is, the present invention provides a coating composition comprising an acrylic resin (1), an acrylate compound (2), and a quaternary ammonium compound (3), As a monomer component constituting the acrylic resin (1), 5 to 50% by mass of a β-diketone group-containing monomer (A), 0.1 to 0.8 mass% of a carboxyl group-containing monomer (B), and The coating composition comprises 49.5 to 94.5 mass % of a monomer (C) other than the monomer (A) and the monomer (B), which does not contain any functional group such as a hydroxyl group, a nitrile group, or an amide group, and whose homopolymer has a glass transition temperature of 60°C or higher.
[0011] In the coating composition of the present invention, the acrylic resin (1) preferably has a weight average molecular weight of 3,000 to 80,000.
[0012] In the coating composition of the present invention, the acrylic resin (1) preferably has a glass transition temperature of 40 to 100°C.
[0013] The present invention also relates to a cured product of the coating composition. Effect of the Invention
[0014] By using the coating composition of the present invention, a cured product (coating) having excellent substrate adhesion, chemical resistance, and solvent resistance can be obtained, and the composition is useful in fields requiring high durability and safety, such as automobile interiors and exteriors, home electrical appliances, paints for building materials, and film coating agents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Acrylic resin (1)] The coating composition of the present invention is characterized by containing an acrylic resin (1) and, as monomer components constituting the acrylic resin (1), containing 5 to 50 mass% of a β-diketone group-containing monomer (A), 0.1 to 0.8 mass% of a carboxyl group-containing monomer (B), and 49.5 to 94.5 mass% of a monomer (C) other than the monomers (A) and (B), which does not contain any of the functional groups of a hydroxyl group, a nitrile group, and an amide group, and which has a glass transition temperature of a homopolymer of 60°C or higher. The acrylic resin (1) is prepared by using specific monomers in a specific ratio, and a cured product (coating) obtained by using the acrylic resin (1) has excellent substrate adhesion, water resistance, weather resistance, chemical resistance, and solvent resistance, and is therefore useful.
[0016] [β-diketone group-containing monomer (A)] As a monomer component constituting the acrylic resin (1), a β-diketone group-containing monomer (A) (hereinafter, sometimes referred to as "monomer (A)") is contained in an amount of 5 to 50 mass % based on the total amount of the monomer components, preferably 10 to 40 mass %, and more preferably 10 to 20 mass %. By using the monomer (A) in the acrylic resin (1) within the above range, the balance between the cure shrinkage during film formation and the crosslink density is optimized, the obtained cured product exhibits excellent curability, and the adhesion of the cured product to the substrate (substrate adhesion) is also excellent, making it useful. The monomer (A) is different from the monomers (B) to (E) described later.
[0017] The monomer (A) can be used without any particular limitation as long as it is a polymerizable monomer having a β-diketone group, and examples thereof include 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, acetoacetoxybutyl (meth)acrylate, etc., and among these, 2-acetoacetoxyethyl methacrylate (AAEM) is preferred. These may be used alone or in combination of two or more kinds.
[0018] [Carboxyl group-containing monomer (B)] The acrylic resin (1) contains a carboxyl group-containing monomer (B) (hereinafter, sometimes referred to as "monomer (B)") in an amount of 0.1 to 0.8% by mass, preferably 0.1 to 0.5% by mass, and more preferably 0.1 to 0.3% by mass, based on the total amount of the monomer components, of the monomer components. By using the monomer (B) in the acrylic resin (1) within the above range, compatibility with the catalyst and a balance between curability and pot life are achieved, which is useful. Note that when the monomer (B) is used in a large amount (for example, 1.0% by mass), the resulting coating composition is prone to curing defects, which is not preferable. Note that the monomer (B) is different from the monomer (A) and the monomers (C) to (E) described below.
[0019] As the monomer (B), any polymerizable monomer having a carboxyl group can be used without any particular limitation, and examples thereof include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, β-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, etc., unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, etc., or half esters of these unsaturated dicarboxylic acids, and among these, (meth)acrylic acid is more preferred from the viewpoint of copolymerizability with other monomers.These may be used alone or in combination of two or more.
[0020] [Monomer (C) other than the monomer (A) and the monomer (B), which does not contain any of the functional groups of a hydroxyl group, a nitrile group, and an amide group, and which has a glass transition temperature of a homopolymer of 60° C. or higher] As a monomer component constituting the acrylic resin (1), a monomer (C) (hereinafter sometimes referred to as "monomer (C)") other than the monomer (A) and the monomer (B), which does not contain any functional group of a hydroxyl group, a nitrile group, or an amide group, and has a homopolymer glass transition temperature of 60°C or higher is contained in an amount of 49.5 to 94.5 mass%, preferably 52 to 88 mass%, and more preferably 54 to 86 mass%, based on the total amount of monomer components. By using the monomer (C) in the acrylic resin (1) within the above range, the glass transition temperature of the obtained acrylic resin (1) is improved, a coating film having high durability is formed, and the solvent resistance and chemical resistance of the cured product using the obtained coating composition are improved, which is useful. The monomer (C) is different from the monomers (A), (B), and the monomers (D) and (E) described later.
[0021] The monomer (C) can be used without any particular limitation as long as it is a polymerizable monomer other than the monomer (A) and the monomer (B), does not contain any functional group of a hydroxyl group, a nitrile group, or an amide group, and has a homopolymer glass transition temperature of 60° C. or higher, and examples thereof include styrene, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl methacrylate, isobornyl methacrylate, and isobornyl acrylate, and among these, methyl methacrylate is more preferable from the viewpoint of the polarity of the monomer. These may be used alone or in combination of two or more.
[0022] [(Meth)acrylic acid alkyl ester (D) having an alkyl group having 2 to 10 carbon atoms and having a homopolymer glass transition temperature of less than 60°C] The monomer components constituting the acrylic resin (1) may further contain a (meth)acrylic acid alkyl ester (D) (hereinafter, sometimes referred to as "monomer (D)") having an alkyl group with 2 to 10 carbon atoms and a homopolymer glass transition temperature of less than 60° C., and in particular, from the viewpoint of the polarity of the polymer after polymerization and solubility in a solvent, a (meth)acrylic acid alkyl ester having an alkyl group with 2 to 4 carbon atoms and a homopolymer glass transition temperature of less than 60° C. may be contained. The monomer (D) is different from the monomers (A) to (C) and the monomer (E) described later.
[0023] Examples of the monomer (D) include ethyl acrylate, propyl (meth)acrylate, isopropyl acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, and the like. Among these, from the viewpoint of the polarity of the polymer after polymerization and the solubility in the solvent, butyl (meth)acrylate can be more preferably used. These may be used alone or in combination of two or more.
[0024] The content of the monomer (D) is preferably 15% by mass or less, and more preferably 10% by mass or less, based on the total amount of monomer components constituting the acrylic resin (1).
[0025] [Other monomer components] As monomer components constituting the acrylic resin (1), in addition to the monomer (A) and the like, other monomer components (hereinafter sometimes referred to as "monomer (E)") may be used as necessary, such as polymerizable monomers containing a hydroxyl group, an amide group, an amino group, and an epoxy group.
[0026] The content of the monomer (E) is preferably 0 to 5 mass %, more preferably 0 to 3 mass %, based on the total amount of monomer components constituting the acrylic resin (1).
[0027] The acrylic resin (1) can be obtained by polymerizing an appropriate combination of the monomers (A) and the like according to the desired properties. The acrylic resin (1) may include any of random copolymers, block copolymers, graft copolymers, and the like.
[0028] (Polymerization method) As the polymerization method for the acrylic resin (1), any appropriate method can be adopted, for example, solution polymerization, bulk polymerization, emulsion polymerization, and various radical polymerizations. Among them, solution polymerization is preferred from the viewpoint of ease of handling.
[0029] (Radical polymerization initiator) The acrylic resin (1) may contain a radical polymerization initiator when radically polymerizing the acrylic resin (1). The radical polymerization initiator may be, for example, a thermal polymerization initiator that generates free radicals when heated. These may be used alone or in combination of two or more kinds.
[0030] Examples of the radical polymerization initiator include peroxide radical polymerization initiators, azo radical polymerization initiators, etc. Among them, peroxide radical polymerization initiators are preferred.
[0031] Examples of the peroxide radical polymerization initiator include hydroperoxide compounds such as 1,1,3,3-tetramethylbutyl hydroperoxide; dialkyl peroxide compounds such as tert-butylcumyl peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, dicumyl peroxide, 1,4-bis(1-tert-butylperoxy-1-methylethyl)benzene, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; diacyl peroxide compounds such as dilauroyl peroxide, didecanoyl peroxide, dicyclohexyl peroxydicarbonate, and bis(4-tert-butylcyclohexyl)peroxydicarbonate; Examples of peroxyester compounds include peroxyacetate, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxylaurate, (1,1-dimethylpropyl) 2-ethylperhexanoate, tert-butyl 2-ethylperhexanoate, tert-butyl 3,5,5-trimethylperhexanoate, tert-butylperoxy-2-ethylhexyl monocarbonate, and tert-butyl peroxymaleic acid.
[0032] Examples of the azo radical polymerization initiator include azonitrile compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, and 2-phenylazo-4-methoxy-2,4-dimethyl-valeronitrile; 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], and the like. azoamide compounds such as 2,2'-azobis[2-methyl-N-[2-(1-hydroxybutyl)]-propionamide], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], 2,2'-azobis(2-methylpropionamide) dihydrate, 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), and 2,2'-azobis(N-cyclohexyl-2-methylpropionamide); alkyl azo compounds such as 2,2'-azobis(2,4,4-trimethylpentane) and 2,2'-azobis(2-methylpropane); and the like.
[0033] Commercially available examples of the radical polymerization initiator include "Perbutyl C", "Perbutyl A", "Perbutyl P", "Perbutyl L", "Perbutyl O", "Perbutyl ND", "Perbutyl Z", "Perbutyl I", "Percumyl P", "Percumyl D", "Perhexyl D", "Perhexyl A", "Perhexyl I", "Perhexyl Z", "Perhexyl ND", "Perhexyl O", "Perhexyl PV", and "Perhexyl O", all manufactured by NOF Corporation.
[0034] The amount of the polymerization initiator used may be a normal amount, and may be selected, for example, from the range of about 0.3 to 15 parts by mass, and preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total amount of all the monomer components constituting the acrylic resin (1).
[0035] The polymerization temperature and polymerization time can be appropriately selected depending on the type of monomer used, the type of polymerization initiator, etc. For example, the polymerization temperature can be about 80 to 130°C, and the polymerization time can be about 5 to 20 hours.
[0036] (Chain transfer agent) In addition, various conventionally known chain transfer agents (molecular weight regulators or polymerization degree regulators) can be used in the polymerization, if necessary. The chain transfer agent is selected from mercaptans such as n-lauryl mercaptan, t-lauryl mercaptan, glycidyl mercaptan, and 2-mercaptoethanol, and among them, t-lauryl mercaptan is preferably used. These may be used alone or in combination of two or more kinds.
[0037] The amount of the chain transfer agent used may be a normal amount, and may be selected from the range of about 0.1 to 10 parts by mass per 100 parts by mass of the total amount of the monomer components constituting the acrylic resin (1).
[0038] The weight average molecular weight (Mw) of the acrylic resin (1) is preferably 3000 to 80000, more preferably 3500 to 70000, and further preferably 4000 to 60000. When the weight average molecular weight (Mw) is within the above range, the balance between the coating film properties and the workability is good, which is useful.
[0039] The glass transition temperature (Tg) of the acrylic resin (1) is preferably 40 to 100° C., more preferably 45 to 95° C., and even more preferably 50 to 90° C. When the glass transition temperature (Tg) is within the above range, the coating film properties are well balanced, which is useful.
[0040] [Acrylate compound (2)] The coating composition of the present invention is characterized in that it contains, in addition to the acrylic resin (1), an acrylate compound (2) other than the raw material used for the acrylic resin (1). The acrylate compound (2) is different from the acrylic resin (1) and plays a role as a crosslinking agent (crosslinkable monomer), which is important for obtaining a cured product using the coating composition. The acrylate compound (2) may be a compound having one or more (meth)acryloyl groups (having an unsaturated double bond) in one molecule, and preferably has two or more (meth)acryloyl groups in one molecule from the viewpoint of improving chemical resistance and solvent resistance.
[0041] Examples of the acrylate compound (2) include monoesters such as methyl acrylate, lauryl acrylate, stearyl acrylate, isostearyl acrylate, tetrahydrofurfuryl acrylate, (methoxyethyl) acrylate, methoxypolyethylene glycol acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl) acrylate, [{cyclohexanespiro-2-(1,3-dioxolan-4yl)}methyl] acrylate, and {(3-ethyloxetan-3-yl)methyl} acrylate; Glycol diacrylate, Propylene glycol diacrylate, Butanediol diacrylate, Pentanediol diacrylate, Hexanediol diacrylate, Heptanediol diacrylate, Octanediol diacrylate, Nonanediol diacrylate, Decanediol diacrylate, Glycerin-1,2-diacrylate, Glycerin-1,3-diacrylate, Pentaerythritol diacrylate, 2-Hydroxy-3-acryloyloxypropyl methacrylate, Tricyclodecane dimethanoate diesters such as dipropylene glycol diacrylate, dipropylene glycol diacrylate, and tripropylene glycol diacrylate; glycerin triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol triacrylate, ethoxylated isocyanuric acid triacrylate, ethoxylated glycerin triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, Examples of the dipentaerythritol hexaacrylate include ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane trimethacrylate, and trispentaerythritol octaacrylate. Among these, from the viewpoint of compatibility of substrate adhesion, chemical resistance, and solvent resistance, tricyclodecane dimethanol diacrylate, trimethylolpropane triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate are more preferred. These may be used alone or in combination of two or more.
[0042] (Other crosslinking agents (hardening agents)) In addition to the acrylate compound (2), the coating composition may further contain other curing agents (crosslinking agents) as necessary. The crosslinking agents are not particularly limited, and examples thereof include epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, and carbodiimide-based crosslinking agents. The crosslinking agents can be appropriately used depending on the type of functional group contained in the coating composition to be used. It is preferable not to use isocyanate-based crosslinking agents because they have problems such as a shortened pot life of the coating composition. These may be used alone or in combination of two or more.
[0043] The amount of the acrylate compound (2) used may be selected such that the molar ratio of the active proton CH in the β-diketone group-containing monomer (A) constituting the acrylic resin (1) to the unsaturated double bond C═C in the acrylate compound (2) is in the range of 0.5 to 2.0, and is preferably selected from the range of 0.8 to 1.2 from the viewpoint of a balance between adhesion to substrates, chemical resistance, and solvent resistance.
[0044] [Quaternary ammonium compounds (3)] The coating composition of the present invention is characterized in that it contains a quaternary ammonium compound (3) in addition to the acrylic resin (1) and the acrylate compound (2). The quaternary ammonium compound (3) is a base catalyst, and plays a role as a thermal latent curing catalyst (curing accelerator) from the viewpoint of promoting the curing reaction upon heating, and is important for obtaining a cured product using the coating composition. In addition, the quaternary ammonium compound (3) is preferably a quaternary ammonium compound in which the number of carbon atoms in the hydrocarbon group bonded to the nitrogen atom in the quaternary ammonium group (cation group) in the quaternary ammonium compound is 2 or more and the anion ionically bonded to the cationic group is a hydroxide ion (OH - ), acetate ion (RCOO - ), carbonate ion (RCO 3-), alkoxide ions (RO - ) is preferable. The R is preferably a hydrogen atom or an alkyl group.
[0045] Examples of the quaternary ammonium compound (3) include tetra-n-propylammonium hydroxide, tetra-n-butylammonium hydroxide, tetra-n-pentylammonium hydroxide, tetra-n-hexylammonium hydroxide, tetracyclohexylammonium hydroxide, tetrakis(trifluoromethyl)ammonium hydroxide, trimethylcyclohexylammonium hydroxide, trimethyl(trifluoromethyl)ammonium hydroxide, trimethyl t-butylammonium hydroxide, tetra-n-propylphosphonium hydroxide, tetra-n-butylphosphonium hydroxide, tetra-n-pentylphosphonium hydroxide, tetra Examples of the compound include n-hexyl phosphonium hydroxide, tetracyclohexyl phosphonium hydroxide, tetrakis(trifluoromethyl)phosphonium hydroxide, trimethylcyclohexyl phosphonium hydroxide, trimethyl(trifluoromethyl)phosphonium hydroxide, trimethyl t-butyl phosphonium hydroxide, tetrapropyl ammonium acetate, tetrabutyl ammonium acetate, and triethylmethyl ammonium 2-ethylhexane salt. Among these, tetrabutyl ammonium hydroxide, tetrabutyl ammonium acetate, and triethylmethyl ammonium 2-ethylhexane salt are preferred from the viewpoint of both curability and pot life. These compounds may be used alone or in combination of two or more.
[0046] In addition to the quaternary ammonium compound (3), the coating composition may further contain other curing catalysts as necessary. Examples of the other curing catalysts that can be used include amines such as triethylamine, N,N-benzylmethylamine, N,N-dimethylphenylamine, and N,N-dimethylaniline; imidazoles such as methylimidazole, 1,2-dimethylimidazole, and 2-methyl-4-methylimidazole; and phosphines such as triphenylphosphine and tributylphosphine. It is preferable not to use paints or inks that use amidines such as 1,8-diazabicyclo(5.4.0)undec-7-ene (DBU) as a curing catalyst from the viewpoint of the balance between coating film properties and pot life.
[0047] The amount of the quaternary ammonium compound (3) used can be selected from the range of about 0.1 to 6.0 parts by mass, and preferably 0.3 to 3.2 parts by mass, based on 100 parts by mass of the total amount of the monomer components constituting the acrylic resin (1) from the viewpoints of adhesion to the substrate, chemical resistance, and solvent resistance.
[0048] (Other additives) The coating composition may contain other additives as necessary. Examples of the other additives include additives such as silane coupling agents, lubricants, fillers, thixotropic agents, tackifiers, waxes, heat stabilizers, light resistance stabilizers, fluorescent whitening agents, foaming agents, pH adjusters, leveling agents, gelation inhibitors, dispersion stabilizers, antioxidants, radical scavengers, heat resistance agents, inorganic fillers, organic fillers, plasticizers, reinforcing agents, antibacterial agents, fungicides, rust inhibitors, thermoplastic resins, thermosetting resins, pigments, dyes, conductivity agents, antistatic agents, moisture permeability enhancers, water repellents, oil repellents, hollow foams, crystal water-containing compounds, flame retardants, water absorbents, moisture absorbents, deodorants, foam stabilizers, defoamers, antifungal agents, preservatives, anti-algae agents, pigment dispersants, antiblocking agents, hydrolysis inhibitors, etc. The amount of these additives to be added is not particularly limited and can be selected appropriately.
[0049] (solvent) The coating composition may contain a solvent if necessary. Examples of the solvent include acetone, diethyl ketone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, tetrahydrofuran, dioxane, ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, n-pentane, n-hexane, cyclohexane, n-heptane, benzene, toluene, xylene, carbon tetrachloride, dichloromethane, chloroform, trichloroethane, dimethylformamide, N-methylpyrrolidone, acetonitrile, diacetone alcohol, normal butanol, and propylene glycol monomethyl ether acetate. The amount of the solvent is not particularly limited and may be appropriately selected.
[0050] [Coating composition] The coating composition of the present invention comprises an acrylic resin (1), an acrylate compound (2), and a quaternary ammonium compound (3), and contains, as monomer components constituting the acrylic resin (1), 5 to 50 mass% of a β-diketone group-containing monomer (A), 0.1 to 0.8 mass% of a carboxyl group-containing monomer (B), and 49.5 to 94.5 mass% of a monomer (C) other than the monomers (A) and (B), which does not contain any of the functional groups of a hydroxyl group, a nitrile group, and an amide group, and which has a glass transition temperature of a homopolymer of 60°C or higher. The coating composition has thermal latency and undergoes a rapid reaction when heated, and therefore the composition (solution) has a long pot life, excellent storage stability and ease of handling. Furthermore, the cured product (coating) obtained from the coating composition has excellent substrate adhesion, chemical resistance, and solvent resistance, making it useful.
[0051] The method for preparing the coating composition is not particularly limited, and the coating composition can be prepared by a known method. For example, the coating composition can be prepared by uniformly mixing each component such as the acrylic resin (1). More specifically, a solvent is added to the acrylic resin (1) and the acrylate compound (2) to adjust the viscosity, and a quaternary ammonium compound (3) serving as a base catalyst is added thereto to prepare the coating composition (solution). This method is useful because it can avoid partial insolubility or localized high concentration of the base catalyst by adding the base catalyst after viscosity adjustment. In addition, this method can improve the pot life of the coating composition (solution), and is effective for coatability.
[0052] [Cured product] The present invention relates to a cured product of the coating composition. The cured product is a coating film (film) or the like obtained by a crosslinking reaction of the coating composition, and is useful as a cured product (coating) having excellent substrate adhesion, chemical resistance, and solvent resistance.
[0053] The cured product (coating) can be formed by applying and drying the coating composition on the surface of a substrate or the like. Examples of methods for forming the cured product (coating) include a method in which the coating composition is uniformly applied to the surface of the substrate by a roller method, a spray method, an applicator, a bar coater, a brush, or other known methods, and then cured at room temperature or under heat. When the coating composition contains an organic solvent as a solvent, it is preferable to heat-dry the coating composition using a heated roller, hot air, a hot plate, or the like after the coating.
[0054] In addition, when forming a coating film (film) cured by a crosslinking reaction of the coating composition, the curing is preferably performed at, for example, 40 to 120°C, more preferably 60 to 90°C, from the viewpoint of curability. In addition, other curing methods can be performed by, for example, heating (for example, 50 to 120°C) under pressure (for example, 1 to 5 MPa) or by radical polymerization through light irradiation. In such cases, the above-mentioned known crosslinking agents (thermosetting agents and photocuring agents) can also be used in combination.
[0055] [Application] The coating composition of the present invention can give a cured product (coating) having excellent substrate adhesion, chemical resistance, and solvent resistance, and therefore can be used in fields requiring high durability and safety, such as automobile interior and exterior coatings, home electrical appliances, paints for building materials, and film coating agents. EXAMPLES
[0056] The present invention will be described in more detail below with reference to examples. However, the present invention should not be construed as being limited to the following examples as long as the gist of the present invention is not exceeded.
[0057] (Production Example 1) To a flask equipped with a cooling tube, a thermometer, a dropping funnel, and a stirrer, 390.6 parts by mass of butyl acetate was added, and the internal temperature was raised to 110°C. Next, a mixture of 392.6 parts by mass of methyl methacrylate, 60.5 parts by mass of butyl acrylate, 50.4 parts by mass of 2-acetoacetoxyethyl methacrylate, 0.5 parts by mass of methacrylic acid, 98.9 parts by mass of n-butyl acetate, and 5.0 parts by mass of Perbutyl O (t-butylperoxy-2-ethylhexanoate, manufactured by NOF Corp.) was added dropwise over 5 hours. One hour after the end of the dropwise addition, a mixture of 3.9 parts by mass of n-butyl acetate and 0.5 parts by mass of Perbutyl O was added. Then, the polymerization reaction was carried out for 17 hours while maintaining the internal temperature at 110°C. Next, butyl acetate was added to obtain the target resin with a non-volatile content of 50% by mass. The weight average molecular weight (Mw) of the resin was 32,000.
[0058] (Examples 2 to 14) Using the same procedure as in Production Example 1, resins of Production Examples 2 to 14 were prepared using the formulations in Table 1.
[0059] (Examples 1 to 13 and Comparative Examples 1 to 8) (Coating film preparation method: non-NCO-OH curing system) The resins (β-diketone group-containing acrylic resins) obtained in Production Examples 1 to 14 were mixed with a polyfunctional acrylate (acrylate compound), and the viscosity was adjusted to about 10 seconds using a NK-2 Iwata viscosity cup (manufactured by Anest Iwata Corporation) using a mixed solvent of butyl acetate / isobutyl acetate / normal butanol / propylene glycol monomethyl ether acetate (30 / 30 / 30 / 10 (mass ratio)) as the solvent. Next, a quaternary ammonium salt (quaternary ammonium compound) was added as a base catalyst to prepare a coating composition (solution), which was then spray-coated onto a substrate (ABS: acrylonitrile-butadiene-styrene copolymer, and PC: polycarbonate).The coating was then set for 10 minutes, dried at 80°C for 1 hour, and allowed to stand at room temperature (about 23°C) for 7 days to form a coating film (film thickness: 20 to 30 μm (after drying)) on the substrate.
[0060] (Comparative Examples 7 and 8) (Coating film preparation method: NCO-OH curing system) The resin (hydroxyl group-containing acrylic resin) obtained in Production Examples 13 and 14 was mixed with a curing agent, polyisocyanate (Sumidur N-3300, manufactured by Sumika Covestro Urethane Co., Ltd.), and a catalyst (dibutyltin dilaurate). A mixed solvent of diacetone alcohol / isobutyl acetate / ethyl acetate / butyl acetate (30 / 30 / 30 / 10) (mass ratio) was used as the solvent, and the viscosity was adjusted to about 10 seconds in an NK-2 Iwata viscosity cup (manufactured by Anest Iwata Corporation) to obtain a coating composition (solution). Next, the coating composition (solution) was spray-coated onto substrates (ABS and PC). After that, it was set for 10 minutes, dried at 80°C for 1 hour, and then left to stand at room temperature (about 23°C) for about 7 days to form a coating film (film thickness: 20 to 30 μm (after drying)) on the substrate.
[0061] (GPC measurement) The weight average molecular weight (Mw) of the resin obtained in the above Production Examples was measured under the following GPC measurement conditions. [GPC measurement conditions] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 4 mg / mL in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following monodisperse polystyrene. [Monodisperse polystyrene] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0062] (Glass transition temperature (Tg)) The glass transition temperature (hereinafter abbreviated as "design Tg") calculated by the FOX formula improves the sunscreen resistance, solvent resistance, and water resistance of the resulting coating film, so the glass transition temperature (design Tg) of the resin (acrylic resin (1)) obtained in the above Production Example is preferably in the range of 40 to 100°C. In the present invention, the glass transition temperature calculated by the FOX formula is calculated in accordance with the FOX formula: 1 / Tg=W1 / Tg1+W2 / Tg2+... (Tg: glass transition temperature to be determined, W1: weight fraction of component 1, Tg1: glass transition temperature of a homopolymer of component 1). The glass transition temperature of the homopolymer of each component was measured using the values described in Polymer Handbook (4th Edition) by J. Brandrup, EH Immergut, and EA Grulke (Wiley Interscience) and the actual values measured by differential scanning calorimetry (DSC) after synthesizing the homopolymer.
[0063] (Pot Life) As described above, the obtained coating composition (solution) was stored at 23° C., and the viscosity at each time point was measured using an NK-2 Iwata Viscosity Cup (manufactured by Anest Iwata Corporation). A rating of A or B was deemed to be at a level that would not cause any problems in practical use (A being the best rating). (Evaluation Criteria) A: After 24 hours, if there is fluidity and the viscosity is less than twice the initial value B: After 24 hours, there is fluidity, but the viscosity is more than 2 times but less than 4 times the initial viscosity. C: More than 10 hours, no liquidity within 24 hours D: No liquidity within 10 hours after 0 hours
[0064] (Substrate adhesion test) As described above, the coating films obtained on the substrates (ABS and PC) were subjected to a cross-cut test (1 mm, 100 squares, 4 directions) in accordance with JIS K 5600-5-6, and the adhesion of the coating film to the substrates (ABS and PC) was visually confirmed. A rating of 5B was deemed to be at a level that was acceptable for practical use (5B is the best rating). (Evaluation Criteria) 5B: No defects 4B: Defective area is less than 5% 3B: Defects exceed 5% and are within 15% 2B: Defects exceed 15% and are within 35% 1B: Defective area is more than 35% and less than 65% 0B: More than 65 missing parts
[0065] (Water resistance test) The coating films obtained on the substrates (ABS and PC) as described above were immersed in water (tap water) heated to 40°C for 240 hours, and a cross-cut test (1 mm, 100 squares, 4 directions) was performed in accordance with JIS K 5600-5-6, and the adhesion of the coating film to the substrates (ABS and PC) was evaluated visually. A rating of 5B was deemed to be at a level that was acceptable for practical use (5B is the best rating). (Evaluation Criteria) 5B: No defects 4B: Defective area is less than 5% 3B: Defects exceed 5% and are within 15% 2B: Defects exceed 15% and are within 35% 1B: Defective area is more than 35% and less than 65% 0B: More than 65 missing parts
[0066] (Sunscreen resistance test) An evaluation test was conducted using a sunscreen cream (Coppertone Sports Ultra Sweatproof SPF30, manufactured by SSL Healthcare Japan Inc.). The coating film obtained on the substrate (ABS) on which the coating film was formed as described above was cut to a size of 50 mm x 70 mm, and the sunscreen cream was applied uniformly (0.5 g / 100 cm) on the coating film. 2 ) and then dried at 55° C. for 4 hours. After drying, the sunscreen cream was washed with a neutral detergent (manufactured by Kao Corporation, product name "CuCute"), and the appearance of the coating film was visually evaluated according to the following criteria. A rating of A or B was deemed to be at a level that would not cause any problems in practical use (A being the best rating). (Evaluation Criteria) A: No marks left B: Traces remain on some parts of the coating C: Traces remain on the entire coating D: Sunscreen cream doesn't come off
[0067] (Ethanol tolerance test) A rubbing test was carried out in which a felt pad (10mm wide x 10mm high x 40mm deep, manufactured by Valqua Corporation) soaked in ethanol (95% or more, grade 1 reagent) was pressed against the coating film obtained on the substrate (ABS) as described above, and rubbing was performed up to 500 times while applying a load of 1kg. The condition of the coating film after rubbing was visually observed, and was evaluated according to the following criteria depending on the number of times until the base material of the ABS substrate became visible. A rating of A or B was deemed to be at a level that would not cause any problems in practical use (A being the best rating). (Evaluation Criteria) A: More than 500 times B: More than 350 times and less than 500 times C: More than 150 times, but less than 350 times D: 150 times or less
[0068] [Table 1]
[0069] The abbreviations in Tables 2 and 3 are explained below. DPHA: Dipentaerythritol pentaacrylate / dipentaerythritol hexaacrylate (product name: Aronix M-402), manufactured by Toagosei Co., Ltd. TMPTA: Trimethylolpropane triacrylate (product name: Miramar M300), manufactured by MIWON A-DCP: Tricyclodecane dimethanol diacrylate (product name: NK Ester A-DCP), manufactured by Shin-Nakamura Chemical Co., Ltd. N-3300: Hexamethylene diisocyanate nurate (product name: Sumidur N-3300), manufactured by Sumika Covestro Urethane Co., Ltd. tBAOH: Tetrabutylammonium hydroxide, manufactured by Tokyo Chemical Industry Co., Ltd. tBAAc: Tetrabutylammonium acetate, manufactured by Tokyo Chemical Industry Co., Ltd. U-CAT 18X: Triethylmethylammonium 2-ethylhexane salt (product name: U-CAT 18X), manufactured by San-Apro Ltd. DBU: 1,8-diazabicyclo[5.4.0]undec-7-ene, manufactured by Kanto Chemical Co., Ltd. DBTDL: Dibutyltin dilaurate, manufactured by Nitto Kasei Co., Ltd. ABS (plate): Showa Denko Materials Co., Ltd., acrylonitrile-butadiene-styrene copolymer (product name: Kobe Poly Sheet ABS-BKWB) PC (plate): Polycarbonate (product name: PC1600) manufactured by Takiron Corporation
[0070] [Table 2]
[0071] [Table 3]
[0072] From the above evaluation results, it was confirmed that in all Examples, the pot life of the obtained coating composition (solution) was practically satisfactory and had excellent storage stability, and the coating (coating film) obtained using the coating composition was also excellent in substrate adhesion, water resistance, sunscreen resistance (chemical resistance), and ethanol resistance (solvent resistance).
[0073] On the other hand, from the above evaluation results, in Comparative Examples 1 to 4, 7 and 8, resins not using the desired monomer components in the desired mixing ratio were used, so that it was not possible to obtain a composition that simultaneously satisfied all the properties at a level that would not cause problems in practical use. Also, in Comparative Examples 5 to 8, a quaternary ammonium compound was not used as a catalyst, so that the pot life was short and all other properties could not be satisfied.
Claims
1. A coating composition comprising an acrylic resin (1), an acrylate compound (2), and a quaternary ammonium compound (3), As a monomer component constituting the acrylic resin (1), 5 to 50% by mass of a β-diketone group-containing monomer (A), 0.1 to 0.8% by mass of a carboxyl group-containing monomer (B), and The present invention comprises 49.5 to 94.5% by mass of a monomer (C) other than the monomer (A) and the monomer (B), which does not contain any of a hydroxyl group, a nitrile group, and an amide group, and which has a glass transition temperature of a homopolymer of 60° C. or higher, the β-diketone group-containing monomer (A) is one or more monomers selected from the group consisting of 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and acetoacetoxybutyl (meth)acrylate; the carboxyl group-containing monomer (B) is at least one of an unsaturated monocarboxylic acid selected from the group consisting of (meth)acrylic acid, crotonic acid, β-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl succinate, and 2-(meth)acryloyloxyethylhexahydrophthalic acid, an unsaturated dicarboxylic acid selected from the group consisting of maleic acid, fumaric acid, and itaconic acid, and a half ester of the unsaturated dicarboxylic acid; The coating composition, wherein the monomer (C) is one or more monomers selected from the group consisting of styrene, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl methacrylate, isobornyl methacrylate, and isobornyl acrylate.
2. 2. The coating composition according to claim 1, wherein the acrylic resin (1) has a weight average molecular weight of 3,000 to 80,000.
3. 2. The coating composition according to claim 1, wherein the acrylic resin (1) has a glass transition temperature of 40 to 100° C.
4. A cured product of the coating composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Curable resin composition and coating material
JP1998045993A
Curable composition
JP2004018859A
Cationic electrodeposition coating composition, method of managing electrodeposition bath, and electrodeposition coating system
JP2004307800A
Coating composition, cured film thereof, and coated article provided with the same
JP2015140423A
Antifogging agent composition
JP2019038981A