Aliphatic polyester copolymer

A stretched polyester with a specific 3HB-co-4HB molecular structure addresses the brittleness and deterioration issues of biodegradable plastics, offering high shape followability and flexibility.

JP7568231B2Active Publication Date: 2024-10-16MITSUBISHI GAS CHEM CO INC +1
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2021519451
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-13
Filing Date
2020-05-13
Publication Date
2024-10-16
Estimated Expiration
2040-05-13

AI Technical Summary

Technical Problem

Existing biodegradable plastics, such as polyhydroxyalkanoate (PHA), suffer from issues of brittleness, low elasticity, and deterioration due to secondary crystallization, limiting their practical applications and usability.

Method used

A stretched polyester composed of an aliphatic copolymer containing 3-hydroxybutyrate (3HB) and 4-hydroxybutyrate (4HB) units with a specific molecular structure and crystalline orientation, allowing for elastic response and reduced secondary crystallization.

Benefits of technology

The stretched polyester exhibits high shape followability, flexibility, and resistance to deterioration over time, making it suitable for applications requiring stretchability and biodegradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568231000005
    Figure 0007568231000005
  • Figure 0007568231000006
    Figure 0007568231000006
  • Figure 0007568231000007
    Figure 0007568231000007
Patent Text Reader

Abstract

The present invention addresses the problem of providing a stretchable polyester that has flexibility and shape followability through elastic response and that is capable of suppressing degradation over time caused by secondary crystallization. The present invention provides a stretchable polyester that is an aliphatic copolymerization polyester including two or more types of monomer units and that includes an α structure and an amorphous structure, wherein the X-ray orientation degree of the α structure is 50% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretched polyester having high shape conformability, flexibility, and repeated stretchability. [Background technology]

[0002] In recent years, large amounts of synthetic plastics have been produced and discarded, and have been incinerated or landfilled. However, issues such as the generation of toxic gases during combustion, pressure on landfill capacity, and soil loosening have attracted attention. There are also concerns about the adverse effects on ecosystems caused by the disposal and leakage of synthetic plastics into the environment. Due to the diversity of plastic types, sorting and reusing them requires time and cost, and only a small proportion of plastics are recycled. Therefore, biodegradable plastics that decompose in the environment into a carbon source that can be used by living organisms have been attracting attention.

[0003] On the other hand, in the medical field, biodegradable plastics are attracting attention as biodegradable materials such as implant materials that do not require recovery, sustained drug release carriers, and scaffolds in regenerative medicine.

[0004] Biodegradable materials such as polyglycolic acid, polylactic acid, hydroxyapatite, collagen, and hyaluronic acid are used in the medical field. These materials have characteristics such as biocompatibility and bioabsorbability, and have contributed to the improvement of medical care, such as suturing for patients who cannot have their stitches removed or for areas that do not require re-incision, implants that are absorbed and replaced by biological tissue after maintaining their strength for a certain period of time, carriers for sustained release of drugs such as medicines and biologically active substances, and scaffolds in regenerative medicine. However, many of these existing bioabsorbable materials lack elasticity and are often hard as individual materials, so their use has been limited.

[0005] Polyhydroxyalkanoates (PHAs) are thermoplastic polyesters that accumulate in microorganisms, and have attracted attention as biodegradable, biocompatible, and bioabsorbable plastics, and have been the subject of much research (Non-Patent Document 1). More than 100 types of monomer units that make up PHA are known, and the most representative is poly-3-hydroxybutyrate (hereinafter abbreviated as P(3HB)), which is composed of (R)-3-hydroxybutyrate (hereinafter abbreviated as 3HB) (Non-Patent Document 1).

[0006] P(3HB) has a high melting point similar to that of polypropylene (hereafter referred to as PP), and its breaking strength is similar to that of PP, but its breaking elongation is less than 5%, its glass transition point is below room temperature at 4°C, and it is a highly crystalline, hard and brittle material.When trying to use PHA industrially, known methods for improving its physical properties include introducing a second component monomer unit to form a copolymer, and increasing the molecular weight.

[0007] Examples of the method for introducing a second component monomer unit to form a copolymer include copolymers incorporating 3-hydroxyvalerate (hereinafter, 3HV), 3-hydroxyhexanoate (hereinafter, 3HH), 4-hydroxybutyrate (hereinafter, 4HB), lactate (hereinafter, LA), glycolate (hereinafter, GA), 3-hydroxypropionate (hereinafter, 3HP), or even longer chain hydroxyalkanoates.

[0008] Methods for increasing the molecular weight include a method in which the P(3HB) biosynthesis gene (phaCAB) extracted from the P(3HB)-synthesizing bacterium Cupriavidus necator is introduced into Escherichia coli XL1-Blue, which does not have a PHA synthesis or degradation system, and the genetically modified bacteria is cultured at pH 6 to produce ultra-high molecular weight P(3HB) (Non-Patent Document 2), a method in which a strain in which the PHA-degrading enzyme gene of a PHA-producing wild-type strain has been disrupted (Patent Document 1), and a method in which ultra-high molecular weight PHA is obtained by adjusting the culture conditions of a PHA-producing wild-type strain (Patent Document 2).

[0009] Aliphatic polyesters, including PHA, generally have a slow crystallization rate, a glass transition point below room temperature, and after molding, deterioration over time due to secondary crystallization progresses, and the breaking elongation tends to decrease. The amorphous parts that did not crystallize in the first crystallization exist between the lamellar crystals, and secondary crystallization refers to the molecular chains of the amorphous parts being incorporated into the crystalline parts by molecular motion, improving the crystallinity. In addition, annealing, a heat treatment to eliminate distortion inside the plastic after molding, is sometimes performed, and the crystallization that progresses during this heat treatment is also called secondary crystallization. It is known that secondary crystallization applies tension to the molecular chains of the amorphous parts, causing cracks and deterioration over time. In addition, when the crystals themselves become large, a large force is applied to the tie molecules that connect the crystals, and the overall structure may become weaker. P(3HB) is a polymer that has a slow crystallization rate but high crystallinity, a glass transition point of 4°C, which is below room temperature, and secondary crystallization occurs during storage, making it hard and brittle, and its physical properties deteriorate over time. By copolymerizing 3-hydroxyvalerate (3HV) units, P(3HB-co-3HV) has shown improvements in flexibility, but the 3HB unit and the 3HV unit can exist in the same crystal lattice, and the glass transition point tends to decrease further through copolymerization, and it is known that deterioration over time due to secondary crystallization after molding continues.

[0010] Copolymerized PHAs composed of second component units that do not co-crystallize with 3HB units, such as 4-hydroxybutyrate (4HB) units and 3-hydroxyhexanoate (3HH) units, can be expected to have improved extensibility and flexibility compared to copolymers with 3HV units by changing the ratio of the second unit components. However, their glass transition points are below room temperature, and they still have the tendency to undergo secondary crystallization after molding, mainly in the 3HB-rich regions, and the problem of deterioration of mechanical properties such as elongation over time remains.

[0011] Therefore, there have been proposals to promote crystallization by blending inorganic substances such as boron nitride, titanium oxide, talc, layered silicate, calcium carbonate, sodium chloride, and metal phosphate with PHA polymer (Patent Document 3), and to blend sorbitol acetal, a compound having an amide bond, and pentaerythritol (Patent Document 4). These are measures taken to promote the slow crystallization rate of PHA and improve processability during molding, but the effects are insufficient, such as causing a decrease in strength and worsening the surface appearance of the molded product, and problems such as the need to add additives and deterioration over time due to secondary crystallization still remain. In addition, there is no description of the elasticity of the molded product.

[0012] Examples of biodegradable plastics that exhibit elasticity include P(3HB-co-4HB) (Non-Patent Documents 3 and 4), P(3HB-co-3HH) (Patent Document 5), and materials obtained by attaching photoreactive acrylate and / or methacrylate groups to copolymers of caprolactone and lactic acid and / or glycolic acid and then photocuring them (Patent Document 6).

[0013] It is already known that P(3HB-co-4HB) copolymers containing 3 to 60% 4HB units are highly flexible, and flexible and tough molded products can be obtained using this copolymer (Patent Document 7). The ratio of 4HB can also be adjusted as desired (Patent Documents 8, 9, and 10), and Patent Document 11 also describes the application of stretching to molded products formed from P(3HB). However, when the stretching force is released, the product almost completely relaxes and does not shrink, and even in P(3HB-co-3HV), the stretchability is less than 100% due to the high crystallinity that co-crystallizes, and there is almost no stretchability. In addition, the problem of deterioration over time due to secondary crystallization remains.

[0014] Non-Patent Document 3 reports that a P(3HB-co-4HB) copolymer solvent cast film with a 4HB ratio of 31% was stretched and then showed elasticity, returning to almost its original shape, but it is believed that the problem of deterioration over time due to secondary crystallization still remains. Non-Patent Document 4 describes that a copolymer of 4HB and 3HB (4HB content of about 20 to 35%) is elastomeric and is a material that stretches and returns to its original shape when force is applied, but it is believed that the problem of deterioration over time due to secondary crystallization still remains. Neither document shows hysteresis, which indicates repeated stretching.

[0015] Patent Document 12 describes a molded product of a 3HB and 4HB copolymer (4HB ratio of 60% to 95%) or a mixed polyester with a crystalline biodegradable polyester, which is obtained by stretching and is a molded product that combines biodegradability and a low initial elastic modulus at low strain, and is flexible, tough, and biodegradable. It describes that the stretched heat-treated yarn and film shrink to 60 to 70% of the size immediately after stretching, but it is unclear whether they are elastic bodies that are repeatedly stretched and contracted, and it is believed that the problem of deterioration over time due to secondary crystallization still remains.

[0016] Patent Document 13 describes that a copolymer of 3HB and 4HB (30% to 99% 4HB) has good biocompatibility, elasticity, and flexibility, and can be used as a medical material for soft tissues without causing safety problems such as cytotoxicity, but it is unclear whether it is an elastic body that is repeatedly stretched, and it is thought that the problem of deterioration over time due to secondary crystallization still remains. In addition, there are descriptions of composites with other fiber composite knitted and woven fabrics such as polyethylene terephthalate, and composites with fiber composites such as polyglycolic acid and polylactic acid, but they are not necessarily aimed at complete degradability.

[0017] Patent Document 14 describes that when melt-spinning P(3HB-co-3HH) copolymer, the melt-extruded filament is quenched below the glass transition temperature, and then partially crystallized at a temperature above the glass transition temperature to obtain a pre-drawn filament that can be further drawn and exhibits elasticity and has the property of suppressing the growth of spherulites. It is described that this method requires quenching below the glass transition temperature, and that even if left at room temperature for a while, it does not grow into three-dimensional spherulites and tends not to be brittle, but it is presumed that at this stage, deterioration over time due to secondary crystallization will still progress. In addition, the degree of elasticity is not clear.

[0018] It is also known that a stretchable material can be obtained by adding an acrylate group or the like to a copolymer of caprolactone and lactic acid and / or glycolic acid and then photocuring it (Patent Document 6). However, when a lactic acid-caprolactone copolymer with a molecular weight of 2000 to 10000 is used, the material elastically deforms only up to a strain of about 20 to 60%, and the stress at that time is 2 to 0.2 N / mm 2 or less (Non-Patent Document 5), which is not a sufficiently high molecular weight substance and cannot be used in areas where greater strength and elasticity are required. Furthermore, the copolymer of caprolactone with lactic acid and / or glycolic acid is obtained by chemical synthesis using a polymerization catalyst such as tin octoate (tin 2-ethylhexanoate), and care must be taken with the amount of catalyst used in medical applications.

[0019] A biodegradable material exhibiting elastic deformation has also been obtained by crosslinking the copolymer obtained by copolymerizing cyclic depsipeptide and ε-caprolactone with polyisocyanates (Patent Document 15). A polymerization catalyst such as tin 2-ethylhexanoate is used in the synthesis of the copolymer, and it is not known whether the crosslinked body can be melt-molded after it is created, and it is unclear whether it is suitable for practical use. [Prior art documents] [Patent documents]

[0020] [Patent Document 1] International Publication WO2014 / 065253 [Patent Document 2] International Publication WO2019 / 044837 [Patent Document 3] International Publication WO2008 / 099586 [Patent Document 4] Patent No. 6368245 [Patent Document 5] Patent No. 4562316 [Patent Document 6] Patent No. 3680132 [Patent Document 7] Japanese Patent Publication No. 64-48821 [Patent Document 8] Japanese Patent Application Publication No. 3-216193 [Patent Document 9] Japanese Patent Application Publication No. 3-292889 [Patent Document 10] Japanese Patent Publication No. 5-64591 [Patent Document 11] Japanese Patent Publication No. 59-059419 [Patent Document 12] Japanese Patent Application Publication No. 6-336523 [Patent Document 13] Japanese Patent Application Publication No. 7-275344 [Patent Document 14] Patent No. 4562316 [Patent Document 15] Patent Publication No. 2008-120888 [Non-patent literature]

[0021] [Non-Patent Document 1] Alistair J. Anderson et al.,Microbiological Reviews,Vol.54,No.4,450-472,1990 [Non-Patent Document 2] S. Kusaka et al., Applied Microbiology and Biotechnology, Vol. 47, 140-143, 1997 [Non-Patent Document 3] Kai-Hee Huong et al.,International Journal of Biological Macromolecules,Vol.101 ,983-995,2017 [Non-Patent Document 4] David P. Martin et al.,Biochemical Engineering Journal, Vol.16,97-105,2003 [Non-Patent Document 5] Takashi Ushida, Journal of the Japan Society of Mechanical Engineers, Vol.106, 897, 2003 Summary of the Invention [Problem to be solved by the invention]

[0022] An object of the present invention is to provide a stretched polyester having shape conformability and flexibility due to its elastic response. [Means for solving the problem]

[0023] As a result of intensive research to solve the above problems, the inventors have found that P(3HB-co-4HB) copolymer molded products retain an α structure (α crystals) showing random orientation, and the period of the α crystals is not uniform, but when the molded product is deformed by stretching after a certain period of crystallization treatment, the degree of orientation of the α crystals is increased in the stretched direction while maintaining the X-ray orientation degree of the α structure at 50% or more, and at the same time, the molecular chains of the amorphous part between the α crystals are stretched to produce a β structure (planar zigzag structure), and when the load is removed, the β structure is reduced or eliminated while maintaining the degree of orientation of the α crystals, resulting in a molded product showing elastic response, which led to the completion of the present invention. Here, the α structure is a folded lamellar crystal, and the β structure is a planar zigzag extended chain structure.

[0024] According to the present invention, the following inventions are provided. <1> A stretched polyester which is an aliphatic copolyester containing two or more types of monomer units, and which contains an α structure and an amorphous structure, and in which the degree of X-ray orientation of the α structure is 50% or more. <2> In the stretched state, β structure is detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement, and in the unloaded state, the β structure is significantly reduced or no β structure is detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement compared to the stretched state. <1> Stretched polyester according to claim 1. <3> The elasticity is such that the tensile elongation recovery rate is 20% or more and 100% or less. <1> or <2> Stretched polyester according to claim 1. <4> A stretched polyester which is an aliphatic copolymer polyester containing two or more types of monomer units and has a stretchability of 20% or more and 100% or less of tensile elongation recovery rate. <5> After crystallization, the material is stretched, and after the load is removed, it exhibits elasticity. <1> from <4> 13. The stretched polyester according to any one of the above. <6> The crystal structure is oriented by stretching. <1> from <5> 13. The stretched polyester according to any one of the above. <7> The crystal structure is oriented by stretching 2 to 20 times. <5> or <6> Stretched polyester according to claim 1. <8> The polymer contains a lamellar crystal structure and an amorphous structure, and exhibits a specific extended chain structure during stretching, and when the tensile load is removed, the extended chain structure is significantly reduced or disappears. <1> from <7> 13. The stretched polyester according to any one of the above. <9> The extended chain structure is a planar zigzag structure. <1> from <8> 13. The stretched polyester according to any one of the above. <10> The lamellar crystal structure is composed of helical folding. <1> from <9> 13. The stretched polyester according to any one of the above. <11> The two or more types of monomer units are a combination of two or more types of monomer units having different main chain lengths. <1> from <10> 13. The stretched polyester according to any one of the above. <12> The polyester contains 3-hydroxybutyrate units as monomer units. <1> from <11> 13. The stretched polyester according to any one of the above. <13> The polyester further comprises 4-hydroxybutyrate units as monomer units. <12> Stretched polyester according to claim 1. <14> The ratio of 4-hydroxybutyrate units to all monomer units is 10 mol% to 30 mol%. <13> Stretched polyester according to claim 1. <15> The weight average molecular weight as measured by gel permeation chromatography in terms of polystyrene is 100,000 to 3,000,000. <1> from <14> 13. The stretched polyester according to any one of the above. <16> It is biodegradable, <1> from <15> 13. The stretched polyester according to any one of the above. <17> It is bioabsorbable; <1> from <16> 13. The stretched polyester according to any one of the above. <18> of biological or chemical synthetic origin; <1> from <17> 13. The stretched polyester according to any one of the above. <19> <1> from <18> A film comprising the stretched polyester according to any one of the above. <20> <1> from <18> A fiber comprising the stretched polyester according to any one of the above. <21> <1> from <18> A molded article comprising the stretched polyester according to any one of the above items. <22> A stretching step of orienting an aliphatic copolymer polyester containing two or more types of monomer units by stretching after crystallization; and An unloading step of unloading the tensile load of the polyester oriented by the stretching step: Including, <1> from <18> 2. A method for producing the stretched polyester according to claim 1 . <23> The form of the produced oriented polyester is a film, a fiber or a molded article. <22> The method described above. Effect of the Invention

[0025] The aliphatic oriented polyester of the present invention can be deformed by stretching and can exhibit an elastic response by unloading, and has shape conformability and flexibility due to its elastic response even without the addition of a crosslinking agent. By using the stretched polyester of the present invention, which has not been put to practical use until now, it becomes possible to manufacture environmentally degradable and bioabsorbable instruments and devices having elasticity. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 shows stress-strain curves of the tensile test for the films of Production Examples 1 to 12 and 14. [Diagram 2] Figure 2 shows the results of WAXD and SAXS measurements of the film molded product of the sample from Production Example 1. The top side shows WAXD measurements, and the bottom side shows SAXS measurements. Original indicates the film molded product before stretching, ×5 indicates the film being stretched 5 times, ×10 indicates the film being stretched 10 times, After release indicates the film after unloading, and Drawing again indicates the film being stretched again. [Diagram 3] Figure 3 shows the change in the crystal structure of a PHA polymer. When unstretched, the α structures (α crystals) in the molded product are in a randomly oriented state, but they become oriented when stretched, and the amorphous chains between them become extended β structures. When the load is removed, the α structures maintain their orientation, and the β structures between the α structures return to being amorphous. This causes a peak in the (121) plane. When stretched again, the amorphous parts return to being extended β structures, and when the load is removed again, they return to being amorphous again. [Figure 4] FIG. 4 shows the procedure for evaluating the stretchability of a film. [Diagram 5] FIG. 5 shows a stress-strain curve (strain 0% to 100%) of the PHA fiber of Example 15 (Production Example 2). [Figure 6] FIG. 6 shows a stress-strain curve (strain 0% to 100%) of the PHA fiber of Example 16 (Production Example 5). [Figure 7] FIG. 7 shows the stress-strain curve (strain 0% to 100%) of the PHA fiber of Example 17 (Production Example 13). [Figure 8] FIG. 8 shows a stress-strain curve (strain 0% to 100%) of the PHA fiber of Example 17 (Production Example 13). [Figure 9] FIG. 9 shows the stress-strain curve (strain 0% to 10%) of the PHA fiber of Example 17 (Production Example 13). [Figure 10] FIG. 10 shows a stress-strain curve (strain 0% to 1000%) of the PHA film of Example 2 (Production Example 2). [Figure 11]FIG. 11 shows a stress-strain curve (strain 0% to 1000%) of the PHA film of Example 5 (Production Example 5). [Figure 12] FIG. 12 shows a stress-strain curve (strain 0% to 1000%) of the PHA film of Example 14 (Production Example 14). [Figure 13] FIG. 13 shows the results of WAXD measurement and SAXS measurement of the film molded article of the sample of Production Example 2. [Figure 14] FIG. 14 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 3. [Figure 15] FIG. 15 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 4. [Figure 16] FIG. 16 shows the results of WAXD measurement and SAXS measurement of the film molded article of the sample of Production Example 5. [Figure 17] FIG. 17 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 6. [Figure 18] FIG. 18 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 7. [Figure 19] FIG. 19 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 8. [Figure 20] FIG. 20 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 9. [Figure 21] FIG. 21 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 10. [Figure 22] FIG. 22 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 11. [Figure 23] FIG. 23 shows the results of WAXD measurement and SAXS measurement of the film molded product of the sample of Production Example 12. [Figure 24] FIG. 24 is a diagram showing a method for calculating the degree of orientation. [Diagram 25]FIG. 25 shows the results of WAXD measurement of the P(3HB-co-3HV) fibers prepared in Example 19. [Figure 26] FIG. 26 shows the stress-strain curve of the P(3HB-co-3HV) fiber produced in Example 19. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described in detail below. Note that the following embodiments are merely examples for explaining the present invention, and the present invention is not limited to these embodiments.

[0028] [polyester] The polyester of the present invention is an aliphatic copolyester containing two or more kinds of monomer units, and is a stretched polyester containing an α-structure and an amorphous structure, in which the degree of X-ray orientation of the α-structure is 50% or more. The use of an aliphatic copolyester containing two or more types of monomer units and containing an α-structure and an amorphous structure enable the stretched polyester of the present invention to have shape conformability and flexibility. Furthermore, the stretched polyester of the present invention can suppress deterioration over time due to secondary crystallization even without the addition of a crystal nucleating agent or the like. The polyester of the present invention contains two or more kinds of monomer units, and preferably the two or more kinds of monomer units are a combination of two or more kinds of monomer units having different main chain lengths. The polymerized units preferably contain 3-hydroxybutyrate units. The polymerized units preferably contain 4-hydroxybutyrate units in addition to 3-hydroxybutyrate units.

[0029] The weight average molecular weight measured by gel permeation chromatography in terms of polystyrene is preferably 100,000 or more, more preferably 200,000 or more, and may be 300,000 or more, 400,000 or more, or 500,000 or more. The weight average molecular weight measured by gel permeation chromatography in terms of polystyrene may be 600,000 or more, 700,000 or more, 800,000 or more, 900,000 or more, 1 million or more, 1.1 million or more, 1.2 million or more, 1.3 million or more, 1.4 million or more, 1.5 million or more, 2 million or more, 3 million or more, or 4 million or more. The upper limit of the weight average molecular weight measured by gel permeation chromatography in terms of polystyrene is not particularly limited, but it is generally 20 million or less, and may be 10 million or less, 8 million or less, 7 million or less, 6 million or less, 5 million or less, 4 million or less, or 3 million or less. However, when melt molding is performed, taking into consideration the decrease in molecular weight due to thermal decomposition and the fact that the viscosity during melting is not too high, the weight average molecular weight as measured by gel permeation chromatography in terms of polystyrene is desirably 400,000 or more and 2,500,000 or less, more preferably 500,000 or more and 2,200,000 or less, and even more preferably 600,000 or more and 2,000,000 or less.

[0030] The aliphatic stretched polyester of the present invention preferably contains 3-hydroxybutyrate units, more preferably 3-hydroxybutyrate units and 4-hydroxybutyrate units, as polymerization units. When the polyester of the present invention contains 3-hydroxybutyrate units, and when the polyester of the present invention contains 3-hydroxybutyrate units and 4-hydroxybutyrate units, the polyester may contain other polymerization units other than 3-hydroxybutyrate units and 4-hydroxybutyrate units as polymerization units. Examples of the other polymerization units include lactate (LA), glycolate (GA), 3-hydroxypropionate (3HP), 3-hydroxyvalerate (3HV), 5-hydroxyvalerate (5HV), 5-hydroxyhexanoate (5HH), 6-hydroxyhexanoate (6HH), 3-hydroxyhexanoate (3HH), or hydroxyalkanoates having 7 or more carbon atoms. Also, terpolymers or multipolymers containing the above polymerization units can be used instead of binary copolymers. The above copolymer compositions may also be mixed in any desired ratio.

[0031] In the present invention, the 3-hydroxybutyrate unit and the 4-hydroxybutyrate unit are represented by the following formulas, respectively. 3-Hydroxybutyrate unit: -OCH(CH 3 )CH 2 C(=O)- 4-Hydroxybutyrate unit: -OCH 2 CH 2 CH 2 C(=O)-

[0032] In the case where the stretched polyester of the present invention contains 4-hydroxybutyrate units, the ratio of the 4-hydroxybutyrate units to the total monomer units is preferably 10 mol% to 30 mol%. The ratio of the 4-hydroxybutyrate units to the total monomer units may be 11 mol% or more, 12 mol% or more, 13 mol% or more, 14 mol% or more, 15 mol% or more, or 16 mol% or more, or 17 mol% or more, 18 mol% or more, 19 mol% or more, or 20 mol% or more. The ratio of the 4-hydroxybutyrate units to the total monomer units may be 30 mol% or less, 29 mol% or less, 28 mol% or less, 27 mol% or less, 26 mol% or less, 25 mol% or less, 24 mol% or less, 23 mol% or less, 22 mol% or less, or 21 mol% or less.

[0033] The ratio of 4-hydroxybutyrate units to the total monomer units can be measured according to the method described in the Examples below. The polyesters of the present invention may be random, block, alternating or graft polymers, but are preferably random polymers.

[0034] It is known that P(3HB-co-4HB) is extensible and flexible, but the present invention has found that when the copolymer is crystallized for a certain period of time and then stretched, it is elastically deformed and extensible, and is stretchable. Furthermore, it has been found that, according to a preferred embodiment of the present invention, deterioration over time due to secondary crystallization is suppressed.

[0035] Preferably, the stretched polyester of the present invention contains an α-structure and an amorphous structure, and the degree of X-ray orientation of the α-structure is 50% or more. The degree of X-ray orientation can be calculated according to the method described in [Calculation of the degree of orientation] in the examples described later. The degree of X-ray orientation of the α structure may be 50% or more, but may be 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, or 85% or more. The upper limit of the degree of X-ray orientation of the α structure is not particularly limited, but is generally 95% or less, and may be 90% or less.

[0036] Preferably, the stretched polyester of the present invention has elasticity. Elasticity is a property of returning to the original state when an external force is applied to an elastic polyester to stretch it, and then the external force is removed. The polyester of the present invention has elasticity with a tensile elongation recovery rate of 20% or more and 100% or less. The lower limit of the tensile elongation recovery rate may be 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, or 50% or more. The upper limit of the tensile elongation recovery rate is not particularly limited, but may be 95% or less, 90% or less, 85% or less, or 80% or less.

[0037] In the case of fibers, the tensile elongation recovery rate means the tensile elongation recovery rate when evaluated by the method described in the "Elasticity evaluation: fibers" section of the Examples below. That is, a cyclic test is performed on a fiber having a length of 3 cm and a fiber diameter of about 0.1 to 0.3 mm, using a tensile tester, under conditions of a temperature of 23°C and an initial length of 10 mm. The fiber is stretched at a tensile speed of 20 mm / min to a strain of 100% (20 mm, which is twice the initial length, i.e., a displacement length of 10 mm), and then the gripper is moved at the same speed to the original length to shrink the fiber. This operation is repeated. If the displacement length at the start of the second elongation (i.e., approximately equal to the end of the first contraction) is X mm, the tensile elongation recovery rate R (%) is given by R = [(20-(X+10)) / 10] x 100 As shown in the figure.

[0038] In the case of cast film, the tensile elongation recovery rate means the tensile elongation recovery rate when evaluated by the method described in the "Elasticity Evaluation: Film" in the Examples below. That is, a film cut to a length of 3 cm and a width of 3 mm is subjected to a cycle test using a tensile tester under the conditions of a temperature of 23°C and an initial length of 10 mm. The film is stretched to a strain of 1000% (110 mm, which is 11 times the initial length, i.e., a displacement length of 100 mm) at a tensile speed of 20 mm / min, and then the gripper is moved to the original length at the same speed to shrink the film. This operation is repeated. The cast film is an unstretched film, and corresponds to the invention of the present application from the end of the first stretching operation (stretching to a displacement length of 100 mm) in the tensile test. If the displacement length at the start of the second stretching (i.e., approximately equal to the end of the first shrinkage) is y mm, the deemed tensile elongation recovery rate r (%) based on the displacement length of 0 mm of the unstretched film is: r = [(110-(y+10)) / 100] x 100 As shown in the figure. However, the present invention is a stretched polyester, and if the displacement length of the film after the first stretching is set as 0 mm, The tensile elongation recovery rate R (%) is R=r 2 / r 1 ×100 where r 1 is the assumed tensile elongation recovery rate after the first stretching, and r 2 is the assumed tensile elongation recovery rate after the second stretching.

[0039] As described in the examples below, the stretched polyester of the present invention is stretched after crystallization, and can exhibit stretchability after unloading. In the polyester of the present invention, the crystal structure is oriented by the above-mentioned stretching. As the stretching treatment, it is preferable to stretch 2 to 20 times within a range where the polyester does not break, and more preferably, it is preferable to stretch 2 to 15 times, and more preferably, it is possible to stretch 2 to 10 times (for example, 2 times, 5 times, or 10 times). The stretching ratio and the number of times of stretching may be appropriately adjusted according to the required stretch width.

[0040] The stretched polyester of the present invention preferably contains a lamellar crystal structure (a structure consisting of folded helical structures: also referred to as an α structure) and an amorphous structure, and develops a specific extended chain structure (a planar zigzag structure: also referred to as a β structure) during stretching, and the extended chain structure is significantly reduced or eliminated upon unloading.

[0041] The extended chain structure (β structure) can be measured by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement described in the Examples below. In the stretched polyester of the present invention, the β structure is preferably detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement in the stretched state, but in the unloaded state, the β structure is significantly reduced or no β structure is detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement compared to the stretched state.

[0042] In the polyester of the present invention after stretching and unloading, it is preferable that the extended chain structure is not detected by wide-angle X-ray diffraction measurement, but it is sufficient that the signal derived from the extended chain structure is reduced after unloading.

[0043] The crystallinity of the stretched polyester of the present invention is not particularly limited, but is preferably 10% or more, and may be 20% or more, 30% or more, or 40% or more. The upper limit of the crystallinity is not particularly limited, but is generally 80% or less.

[0044] The stretched polyester of the present invention is preferably biodegradable, more preferably bioabsorbable. Biodegradable means that it can be decomposed by microorganisms or enzymes in the natural environment (e.g., soil, compost, lakes, marshes, seawater, etc.) or can be decomposed into non-toxic components in the living body. Bioabsorbable means that it can be metabolized by the living body such as human or animal.

[0045] The present invention provides a stretched polyester that has shape conformability and flexibility due to elastic response and can suppress deterioration over time due to secondary crystallization without the addition of crosslinking agents, crystal nucleating agents, etc., but these can also be added as long as they do not destroy the physical properties.

[0046] [Manufacturing method of polyester] Generally, methods for synthesizing PHAs include fermentation synthesis (biosynthesis) and chemical synthesis. The method for producing the aliphatic polyester of the present invention may be either fermentation synthesis (biosynthesis) or chemical synthesis, but the fermentation synthesis (biosynthesis) is preferred in order to obtain a polyester with a large molecular weight.

[0047] The chemical synthesis method is a method of chemically synthesizing PHAs according to the method of normal organic synthesis.Specific examples of the chemical synthesis method include (R)-β-butyrolactone, ε-caprolactone, and other fatty acid lactones are ring-opened under a catalyst to synthesize P(3HB-co-6HHx) (Abe et al., Macromolecules, 28, 7630 (1995)), (R)-β-butyrolactone, γ-butyrolactone, and other fatty acid lactones are ring-opened under a catalyst to synthesize P(3HB-co-4HB) (Hori et al., Polymer,36, 4703(1995)), and glycolide and lactide are ring-opened under a catalyst to synthesize P(GA-co-LA) (Gilding et al., Polymer 20, 1459 (1979)).

[0048] The fermentation synthesis method (biosynthesis method) is a method for synthesizing PHAs biologically according to conventional culture engineering techniques. Specifically, for example, the polyester containing 4HB of the present invention can be produced by culturing a microorganism capable of producing P(3HB) as a carbon source in the presence of ε-caprolactone (also known as 6-hexanolactone) or its saponification product 6-hydroxyhexanoate or a salt thereof, γ-butyrolactone or its saponification product 4-hydroxybutyrate or a salt thereof, butyric acid derivatives such as 4-chlorobutyrate and 4-bromobutyrate, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, and other even-numbered α,ω-alkanediols having 4 or more carbon atoms (Saito et al., Polymer International 39, 169 (1996), and International Publication WO2019 / 044837).

[0049] Microorganisms capable of producing P(3HB) include those of the genera Cupriavidus, Alcaligenes, Ralstonia, Delftia, Comamonas, Hydrogenophaga, Microorganisms known to synthesize P(3HB), such as Burkholderia, Escherichia, Azotobacter, Methylobacterium, Paracoccos, Acinetobacter, Aeromonas, Allochromatium, Azorhizobium, Bacillus, Caulobacter, Chromobacterium, Ectothiorhodospira, Klebsiella, Nocardia, Pseudomonas, Rhodobacter, Rhodococcus, Rhodospirillum, Rickettsia, Sinorhizobium, Sphingomonas, Synechocystis, Thiococcus, Thiocystis, Vibrio, and Wautersia, can be used. Among the above, the Cupriavidus genus is preferred, and Cupriavidus necator is more preferred. As an example, Cupriavidus necator strain H16 (ATCC17699) can be used.

[0050] In addition, Cupriavidus necator H16 wild type strain can sufficiently incorporate 3HB, 3HV, 3HP, 4HB, 5HV, etc. into PHA, but if a genetically modified strain into which a PHA polymerase gene with different substrate specificity is introduced is used, other hydroxy acids can also be polymerized into PHA. Therefore, not only Cupriavidus necator H16 strain, but also its genetically modified strains and, as mentioned above, other hydroxy acids of the genera Cupriavidus, Alcaligenes, Ralstonia, Delftia, Comamonas, Hydrogenophaga, It is also possible to use microorganisms that have the ability to polymerize PHA or that have been imparted with the ability to polymerize PHA, such as the genera Burkholderia, Escherichia, Azotobacter, Methylobacterium, Paracoccos, Acinetobacter, Aeromonas, Allochromatium, Azorhizobium, Bacillus, Caulobacter, Chromobacterium, Ectothiorhodospira, Klebsiella, Nocardia, Pseudomonas, Rhodobacter, Rhodococcus, Rhodospirillum, Rickettsia, Sinorhizobium, Sphingomonas, Synechocystis, Thiococcus, Thiocystis, Vibrio, and Wautersia.

[0051] The pH of the culture medium is generally about 4 to about 10, preferably about 5 to about 8, and more preferably about 5.8 to about 7.5. The culture temperature is generally 15° C. to 45° C., preferably 20° C. to 40° C., and more preferably 25° C. to 38° C. The culture method may be any of batch culture, fed-batch culture, and continuous culture.

[0052] There are no particular limitations on the medium components, so long as they are substances that can be assimilated by the microorganisms used. Examples of carbon sources that can be used include sugars such as arabinose, glucose, mannose, fructose, and galactose; sugar alcohols such as sorbitol, mannitol, and inositol; alcohols such as methanol, ethanol, and butanol; organic carbon sources such as acetic acid, butyric acid, fatty acids, and vegetable oils; inorganic carbon sources such as carbon dioxide; and natural products such as yeast extract, molasses, peptone, and meat extract.

[0053] Nitrogen sources that can be used include inorganic nitrogen compounds such as ammonia, ammonium salts (ammonium chloride, ammonium sulfate, ammonium phosphate), nitrates, etc., and / or organic nitrogen-containing substances such as urea, corn steep liquor, casein, peptone, yeast extract, meat extract, etc.

[0054] Examples of the inorganic component are selected from calcium salts, magnesium salts, potassium salts, sodium salts, phosphates, manganese salts, zinc salts, iron salts, copper salts, molybdenum salts, cobalt salts, nickel salts, chromium salts, boron compounds, and iodine compounds, and more specific examples include monopotassium phosphate, dipotassium phosphate, magnesium phosphate, magnesium sulfate, sodium chloride, and the like. Other organic nutrient sources include, for example, amino acids such as glycine, alanine, serine, threonine, and proline, vitamins such as vitamin B1, vitamin B12, folic acid, and vitamin C, and the like.

[0055] Methods for producing 4HB-containing PHA include culturing a PHA-producing wild strain with a precursor that can become 4HB-CoA, and culturing the wild strain with a precursor that can become 4HB-CoA, and introducing a 4HB-CoA supply pathway by genetic recombination. In the present invention, a method of culturing a PHA-producing wild strain with a precursor that can become 4HB-CoA may be adopted, or a 4HB-CoA supply pathway may be introduced by genetic recombination. Precursors that can become 4HB-CoA include ε-caprolactone (also known as 6-hexanolactone), or its saponification product 6-hydroxyhexanoate or its salt, γ-butyrolactone, or its saponification product 4-hydroxybutyrate or its salt, butyric acid derivatives such as 4-chlorobutyrate and 4-bromobutyrate, and even-chain α, ω-alkanediols having 4 or more carbon atoms such as 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, and 1,10-decanediol. By culturing a microorganism capable of synthesizing P(3HB) in the presence of these, 4HB-containing PHA can be produced (International Publication WO2019 / 044837, and Polymer International 39, 169-174(1996)). The amount of precursors that can become 4HB-CoA is not particularly limited, but they can be supplied in a batch, continuous, or intermittent manner so long as they do not cause growth inhibition. In general, the ratio of 4HB in PHA can be changed by changing the amount, concentration, and supply rate of these precursors. In addition, a method shown by Li et al. can be used to produce 4HB-containing PHA by incorporating a 4HB-CoA supply pathway and a PHA synthesis pathway into E. coli from a carbon source structurally different from 4HB through genetic recombination (Metabolic Engineering, Volume 12, 352-359 (2010)).

[0056] Fermentation synthesis methods for producing PHAs containing monomer units other than 3HB and 4HB can include a method of incorporating 3HV, 3HP, or 5HV monomer units using propionic acid, valeric acid, 1,3-propanediol, 1,5-pentanediol, propanol, pentanol, etc., or a method of incorporating 3HH monomer units using a carbon source that can supply 3HH-CoA via the β-oxidation pathway using a microorganism that has a PHA polymerase with broad substrate specificity that can recognize 3HB-CoA and 3HH-CoA. Furthermore, genetically modified bacteria that can incorporate lactic acid, glycolic acid, 3HH monomer units, etc. by changing the substrate specificity of the PHA polymerase by gene replacement can also be used. By combining the method for producing 4HB-containing PHA with the method for introducing these other monomer units, it is possible to synthesize by fermentation not only binary copolymers such as P(3HB-co-3HV), P(3HB-co-3HP), P(3HB-co-4HB), P(3HB-co-3HH), P(3HB-co-5HV), P(3HB-co-6HH), P(3HB-co-LA), and P(3HB-co-GA), but also terpolymers and further multipolymers combining 3HB, 3HV, 3HP, 3HH, 4HB, 5HV, 6HH, LA, GA, or even longer chain hydroxyalkanoates.

[0057] PHA can be produced in a so-called growth-uncoupled manner, in which the bacterial cells are grown prior to cultivation for PHA production, and then the medium is changed or the culture medium is changed to a PHA accumulation condition in which nutrients such as phosphorus and nitrogen sources are limited as the cells grow. Alternatively, growth-coupled production can be performed in which the bacterial cells grow and PHA accumulates simultaneously.

[0058] From the culture obtained by the above-mentioned cultivation, the cells are separated and collected by a conventional solid-liquid separation means such as filtration and centrifugation, and the cells are washed and dried to obtain dry cells. From the dried cells, the polyester produced is extracted by a conventional method, for example, with an organic solvent such as chloroform, and the PHA is precipitated and collected by adding a poor solvent such as hexane to the extract.

[0059] Alternatively, the recovered bacterial cells can be subjected to a known method, such as physical disruption using a high-pressure homogenizer or ultrasonic treatment, alkali treatment using sodium hydroxide, potassium hydroxide, sodium hypochlorite, etc., surfactant treatment, enzyme treatment using protease, lysozyme, lipase, etc., oxidation treatment using an oxidizing agent such as hydrogen peroxide, washing with a solvent such as methanol, ethanol, acetone, etc., and drying, to remove components other than PHA and recover PHA.

[0060] [Creating elastic molded bodies] The above PHA can be used as a raw material and subjected to melt processing steps such as melt spinning, melt extrusion, injection molding, etc. The molded product can be crystallized by heat treatment and then stretched to obtain fibers, films, and molded products with rubber elasticity.

[0061] As melting conditions, it is desirable for manufacturing and processing that the melting temperature is between 100°C and 220°C, the melting time is 20 minutes or less, and the mold temperature and winding temperature are in the range of 5°C to 50°C. The fibers, films, and molded bodies thus melt-processed are subjected to a crystallization treatment. As conditions for this crystallization treatment, if the crystallization temperature is in the range of 20°C to 120°C and the crystallization time is in the range of 1 minute to 120 minutes, it is possible to proceed to the next stretching process. When a film or other molded article is produced by the solvent casting method, crystallization occurs simultaneously with evaporation of the solvent, so that the film can proceed to the next stretching process.

[0062] Crystallized fibers, films, and other molded articles are stretched at a stretch ratio of 2 times or more (for example, 5 times or more) to develop rubber elasticity. For example, after melting at a melting temperature of 180°C for 5 minutes, the fiber is wound up at 23°C, crystallized at 23°C for 30 minutes, and then stretched approximately 5 times to produce a fiber with rubber elasticity. If the length of the fiber after melt spinning, crystallization, and drawing is taken as 100% (the length at the end of all steps, not before drawing, is taken as 100%), it can be stretched to approximately 200% (strain 100%) without breaking, and then, by removing the load, it shows the property of recovering strain to nearly 130-150% (strain 30-50%), with a stretch recovery rate (%) of about 70% to about 50%. The stretch ratio and number of stretches can be adjusted appropriately to match the required stretch range.

[0063] Alternatively, a film having rubber elasticity can be produced by melt-molding the film in a hot press at 180° C. for 2 to 5 minutes, crystallizing the film at 23° C. for 60 minutes, and stretching the film 2 to 10 times. If the length of the film after it has been created through melt molding, crystallization, and stretching is taken as 100% (the length after it has been stretched and shrunk is taken as 100%), it can be stretched up to approximately 200% (strain 100%) without breaking, and when the load is then removed, it has the property of recovering to nearly 140% (strain 40%). The fibers and films produced in this manner retain good elastic response even after long-term storage of six months or more, and are molded articles in which deterioration over time due to secondary crystallization is suppressed.

[0064] The present invention will be described in more detail with reference to the following Production Examples and Examples, but the present invention is not particularly limited to the following Examples. EXAMPLES

[0065] [Polymer production (jar culture)] <Production Example 1> Cupriavidus necator strain H16 (ATCC17699) was used to produce PHA. KH 2 PO 4 2.72g / L, Na 2 HPO 4 4.26 g / L, NaHCO 3 0.3g / L, (NH 4 ) 2 SO 42g / L, MgSO 4 7H 2 Sterilized medium 1 was made of 0.2 g / L O, 0.2 g / L yeast extract, and 3.5 mL of the mineral solution described below, to which fructose was added at 14.24 g / L. Test tube shaking culture was carried out at 30°C for 24 hours to obtain a pre-preculture solution. Mineral solution: FeC 6 H 5 O 7 xH 2 O 6g / L, ZnSO 4 7H 2 O 2g / L, CuSO 4 5H 2 O 0.1g / L, MnCl 2 4H 2 O 1g / L, KI 0.1g / L, (NH 4 ) 6 Mo 7 O 24 4H 2 O 0.1g / L, CoCl 2 6H 2 O 0.1g / L, H 3 BO 3 0.2g / L, NaCl 5g / L, CaCl 2 2H 2 O 4g / L dissolved in water.

[0066] 1 mL of the pre-preculture solution was inoculated into a 500 mL Erlenmeyer flask containing 100 mL of the above-mentioned medium 1 to which fructose was added at 14.24 g / L, or medium to which fructose was added at 8.86 g / L and ε-caprolactone at 5.38 g / L, or medium to which fructose was added at 8.86 g / L and γ-butyrolactone at 5.38 g / L, and cultured at 30°C and 150 rpm for 48 to 96 hours to prepare the main culture medium (preculture solution).

[0067] The above medium 1 (NH 4 ) 2 SO 4A 3-L jar fermenter was prepared with 2 L of a medium containing 7.5 g / L of fructose and γ-butyrolactone, which were then aseptically fed through a sterile filter (PTFE 0.2 μm pores). The carbon source feed rate and feeding ratio could be set at will, but to avoid bacterial growth being halted due to the carbon source not being consumed by the bacteria and remaining in excess in the culture tank, the culture was started at low flow rates of 1-2 g / h (0.5-1 g / h L) for 42% fructose and 0.2-0.5 g / h (0.1-0.25 g / h L) for γ-butyrolactone, and the feed rates were increased stepwise or continuously in accordance with the growth of the bacteria. The aeration rate was controlled at 0.2-0.3 L / min, the stirring speed at 500-700 rpm, the culture temperature at 36°C, the lower limit of culture pH at 6.0, and 2N NaOH solution was used as an alkali for pH adjustment. The ratio of γ-butyrolactone:fructose was about 0.5. The culture was completed 140 hours after the start of the culture.

[0068] After the cultivation, the cells were collected by centrifugation, frozen at -20°C, and then freeze-dried. The method for extracting and purifying PHA from the cells was as follows. In a glass Erlenmeyer flask with a screw cap, about 4 to 10 g of freeze-dried cells were suspended in 400 mL of chloroform, and extraction was carried out at 30°C for 24 to 48 hours. The resulting viscous solution was filtered through filter paper to remove the cell residue. The resulting clear liquid was concentrated to about 100 to 200 mL using an evaporator, and PHA was precipitated using 5 times the amount of hexane, a poor solvent. The resulting white precipitate was washed with ethanol and then vacuum dried to obtain purified PHA.

[0069] <Production Example 2> The same procedure as in Production Example 1 was repeated, except that the culture time in the jar culture was 170 hours.

[0070] <Production Example 3> The same procedure as in Production Example 1 was repeated, except that the culture time in the jar culture was 96 hours.

[0071] <Production Example 4> The same procedure as in Production Example 1 was repeated, except that the culture time in the jar culture was 120 hours.

[0072] <Production Example 5> The same procedure as in Production Example 1 was repeated, except that the culture time in the jar culture was 144 hours.

[0073] <Production Example 6> In the jar culture medium (NH 4 ) 2 SO 4 The same procedures as in Production Example 1 were carried out except that a medium containing 12.5 g / L of fructose was used, a 42 mass% fructose solution and ε-caprolactone were used as fed-batch carbon sources with an ε-caprolactone:fructose ratio of approximately 0.4, 12.5% ​​aqueous ammonia was used as the alkali for adjusting the pH, and the culture time was 149 hours.

[0074] <Production Example 7> The same procedures as in Production Example 6 were carried out, except that the culture time in the jar culture was 172 hours and the ratio of ε-caprolactone:fructose was about 0.5.

[0075] <Production Example 8> The same procedures as in Production Example 6 were carried out, except that the culture time in the jar culture was 172 hours and the ratio of ε-caprolactone:fructose was about 0.6.

[0076] <Production Example 9> The same procedures as in Production Example 6 were carried out, except that the culture time in the jar culture was 205 hours and the ratio of ε-caprolactone:fructose was about 0.6.

[0077] <Production Example 9> The same procedures as in Production Example 6 were carried out, except that the culture time in the jar culture was 205 hours and the ratio of ε-caprolactone:fructose was about 0.6.

[0078] <Production Example 10> The same procedures as in Production Example 1 were carried out except that the culture time in the jar culture was 114 hours, the ratio of ε-caprolactone:fructose was about 0.4, and purification was performed after culture by combining high-pressure crushing treatment, alkali treatment, oxidizing agent treatment, solvent washing, etc.

[0079] <Production Example 11> The same procedures as in Production Example 10 were carried out except that the culture time in the jar culture was 111 hours and the ratio of ε-caprolactone:fructose was about 0.5.

[0080] <Production Example 12> The same procedures as in Production Example 10 were carried out except that the culture time in the jar culture was 113 hours and the ratio of ε-caprolactone:fructose was about 0.5.

[0081] <Production Example 13> The same procedures as in Production Example 10 were carried out except that the culture time in the jar culture was 113 hours and the ratio of ε-caprolactone:fructose was about 0.4.

[0082] <Production Example 14> The same procedures as in Production Example 6 were carried out except that the culture time in the jar culture was 113 hours and the ratio of ε-caprolactone:fructose was about 0.5.

[0083] [PHA molecular weight measurement] The molecular weight of PHA (weight average molecular weight Mw and number average molecular weight Mn) was measured by gel permeation chromatography as follows. The measurement results of the molecular weight (Mw and Mn) of the PHA of each production example are shown in Table 1 below. The purified PHA was dissolved in chloroform at 60°C for 4 hours, and then cooled to room temperature. The solution was filtered through a PTFE filter with a pore size of 0.2 μm to remove insoluble matter, and used as a measurement sample. The GPC conditions were as follows: Equipment: Shimadzu HPLC Prominence system Column: Showa Denko Shodex K-806L (2 columns in series) Column temperature: 40℃ Mobile phase: Chloroform (1ml / min) Detector: RI (40℃) Standard: Shodex polystyrene molecular weight standard (6.87 million to 1270) Injection volume: 60μl Analysis time: 30 minutes

[0084] [Polymer analysis] < 1 H-NMR> The composition of the purified PHA in each production example was determined using a nuclear magnetic resonance spectrometer (JASCO ECA500). The purified PHA was dissolved in CDCl at a concentration of 1.5% by mass. 3 The resulting solution was used as a measurement sample. 1 H-NMR spectra were measured at 500 MHz at room temperature.

[0085] The 4HB ratios measured by NMR for the PHA of each production example are shown in Table 1 below.

[0086] [Measurement of thermal properties] The glass transition temperature (Tg) and melting point (Tm) were measured using a differential scanning calorimeter (PerkinElmer, DSC8500) equipped with an intracooler. The measurement atmosphere was nitrogen (20 ml / min), and the sample was heated from -50°C to 200°C at 20°C / min and held for 1 minute to completely melt the sample. The sample was then rapidly cooled to -50°C at 200°C / min, held for 3 minutes, and then heated again to 200°C at 20°C / min (this heating was taken as the second run). Tg and Tm were measured using the DSC curve (thermogram) measured in the second run. When the temperature was raised from the glassy state in the rapidly cooled state, the baseline fluctuated when the glassy state transitioned to the amorphous state, and the temperature at which this fluctuation occurred was read to determine Tg. When the temperature was further raised, a melting peak (endothermic peak) appeared as a downward convex peak on the DSC curve, and the temperature at the apex of the peak was taken as Tm. The sample was about 1 mg, and an aluminum sample pan was used. Indium was used for temperature calibration. The measurement results are shown in Table 1 below.

[0087] [Table 1]

[0088] <Examples 1 to 14> [Film crystallization] The P(3HB-co-4HB) polymers (0.25 g each) obtained in Production Examples 1 to 14 were dissolved in 10 ml of chloroform, and the obtained polymer solutions were poured into a Teflon petri dish with a diameter of 5 cm, covered with a film (aluminum foil) with holes, and the solvent was evaporated for about one day to produce a solvent cast film. The obtained film was left to stand at 23°C for one week to promote crystallization, and a PHA cast film was obtained. When the film is produced by melt molding such as hot pressing, it is heated and melted at 180°C for 2 to 5 minutes, and then allowed to crystallize at 23°C for about 1 to 120 minutes before moving on to the next stretching process.

[0089] [Stretching process] The PHA film obtained above was cut into a strip of 3 cm in length and 3 mm in width, and stretched at 23° C. to an arbitrary ratio, for example, 2 times, 5 times, 10 times, etc., using a stretching machine. If necessary, the stretching was stopped and unloaded, and the stretching operation was repeated again. The PHA cast films produced using the P(3HB-co-4HB) polymers obtained in Production Examples 1 to 14 were stretched as described above to obtain the films of Examples 1 to 14, respectively.

[0090] [Wide-angle X-ray diffraction (WAXD) and small-angle X-ray scattering (SAXS) measurements] For the PHA cast films made from the PHAs of Production Examples 1 to 12, the structure of the films before stretching, during stretching, after unloading, and during re-stretching was analyzed by wide-angle X-ray diffraction (WAXD) measurement and small-angle X-ray scattering (SAXS) measurement.

[0091] WAXD and SAXS measurements were performed at the SPring-8 synchrotron radiation facility with an X-ray wavelength of 0.1 nm and a camera length of 250 mm. The film was placed perpendicular to the X-ray beam and parallel to the detector. For SAXS measurements, the X-ray wavelength was 0.1 nm and the camera length was 2500 mm.

[0092] The results of WAXD and SAXS measurements for the samples of Production Examples 1 to 12 are shown in Figure 2 and Figures 13 to 23. The upper side shows WAXD measurements and the lower side shows SAXS measurements. "Original" indicates the film before stretching, "x5" indicates the film being stretched 5 times, "x10" indicates the film being stretched 10 times, "After release" or "Zero stress" indicates the film after unloading, and "Drawing again" indicates the film being stretched again.

[0093] In the WAXD measurement, the ring pattern areas with strong intensity indicate peaks diffracted by crystals, while the areas with weak intensity indicate areas derived from amorphous matter. As a result of the WAXD measurement, in the film molded body before stretching, concentric (ring pattern) diffraction due to the double helical structure (α structure) was observed, and the α structure was present in a disordered manner. Therefore, it can be seen that the film before stretching contains α structure and amorphous structure (note that 100% crystallinity is impossible for a polymer, so it naturally contains amorphous structure). At this point, no diffraction due to the planar zigzag structure (β structure) was observed. In contrast, in the WAXD analysis results after stretching 5 and 10 times, the α structure begins to be slightly oriented in the stretching direction, but the period of the α crystals is not uniform. In the case of 5-fold and 10-fold stretching and re-stretching after unloading, diffraction points due to the β structure were observed on the WAXD equator, which revealed that the molecular chains of the amorphous parts between the α structures were stretched to produce a β structure (planar zigzag structure). The diffraction points due to the β structure disappeared when the tensile load was removed and the elongation was restored, and it was considered that the β structure returned to a random coil again in the unloaded state. Even after unloading and shrinking, diffraction points due to the oriented α structure generated by the first stretching were observed, indicating that the α structure remains oriented. After unloading and shrinking, diffraction points due to the oriented α structure were also observed when re-stretching with a tensile load applied again. As described above, it can be seen that the film after stretching contains an α structure and an amorphous structure.

[0094] The SAXS measurements of these films showed that the unloaded films showed drop-like patterns on the meridian parallel to the stretching direction. This indicates that the lamellar crystals have a specific period and are oriented in the stretching direction. The WAXD results showed that a ring pattern originating from the lamellar crystals was generated before stretching, and when this was stretched, a cross orientation of the crystals formed with an α structure and the appearance of a β structure were observed, and when the load was removed, the degree of orientation decreased and the β structure disappeared. The SAXS results showed that there was no clear scattering peak before stretching (random orientation of the laminated lamellae), and meridian scattering that appeared during the stretching process and a clear meridian drop-like scattering pattern observed in the film after unloading were observed. From the above results, it is thought that in this film, the laminated lamellar structure that existed before stretching rotates as it is stretched and becomes oriented horizontally or perpendicularly to the stretching direction. At this time, it is thought that the tie molecular chains present between the lamellar crystals become in a tensioned state and gather together due to the increase in the stretch ratio, resulting in the appearance of a β structure (strong equatorial diffraction in WAXD). This β structure is not stable, so it is expected to melt and return to normal tie molecular chains when the tension is released. Furthermore, after unloading, the entire film shrinks due to rubber elasticity. At this time, the higher-order structure composed of lamellar crystals can dynamically rearrange, so it is expected to become a structure with some periodicity, which is thought to be the reason why a strong scattering pattern is observed along the meridian in the SAXS measurement of the film after unloading.

[0095] [Calculation of the degree of orientation] In the wide-angle X-ray diffraction (WAXD) measurement described above, a ring-shaped area including a specific diffraction point (in this case, the (020) plane) in the WAXD image measured was selected, and all diffraction intensities with the same azimuth angle were integrated. This intensity was then plotted against the azimuth angle to create a one-dimensional azimuth angle profile. A normal distribution-like curve with a peak is obtained where the diffraction point exists, and the full width at half maximum (FWHM: peak width at half the height of the peak) is measured (see Figure 24). If the full width at half maximum is β, then the degree of orientation F [%] is given by F = (180-β) / 180 × 100[%] It is expressed as:

[0096] The orientation degrees [%] of the films of Examples 1 to 12 were measured, and the results are shown in Table 2.

[0097] [Table 2]

[0098] [Tensile test: film] PHA film cut into strips 3 cm long and 3 mm wide was subjected to tensile testing until the film broke using a tensile testing machine AGS-X or EZ-Test (Shimadzu Corporation) at a temperature of 23°C, a test speed of 20 mm / min, and an initial length of 10 mm. Of the 3 cm length in the longitudinal direction, a region of 1 cm from each end of the film was used to fix the film, and the central 1 cm (10 mm) was used for the tensile test, with this 10 mm portion being the initial length. The stress-strain curve results are shown in Figure 1.

[0099] [Evaluation of film elasticity] The stretchability of the films of Examples 2, 4, 5, 6, 8 and 14 was evaluated by the method shown in Figure 4. The films were cut into strips of 3 cm in length and 3 mm in width, and the strain L when stretched 11 times to 11 cm (strain 1000%, displacement length 10 cm) was 0% when the chuck distance (distance between the fixtures) was 1 cm. 1 (%), and the strain L when stretched again to 11 times (strain 1000%) and then released 2 The strain (%) is summarized in Table 3. The strain was calculated by dividing the displacement length by the distance between the fixtures (1 cm).

[0100] [Table 3]

[0101] <Examples 15 to 18> [Fiber crystallization] The P(3HB-co-4HB) obtained in Production Examples 2, 5, and 13 was heated at 170°C to 180°C for 5 to 10 minutes to melt, and then extruded from a 2 mm discharge die. Specifically, a high-temperature melt extrusion spinning device (IMC-19F8) manufactured by Imoto Manufacturing Co., Ltd. (Kyoto) was used, and about 5 g of polymer was filled into a cylinder with a diameter of 6 mm, and extruded at a piston extrusion speed of 0.5 mm / s. The polymer was wound on a roller at 23°C, and left to stand for 30 minutes at 23°C while wound on the roller to crystallize, to obtain a primary PHA fiber. The crystallization time depends on the ratio of 4HB and the crystallization temperature, but if the P(3HB-co-4HB) has a 4HB ratio of about 10 mol% to 30 mol%, it takes about 1 to 120 minutes to proceed to the next drawing step.

[0102] [Stretching after crystallization] The primary PHA fiber was stretched about 5 times while being pressed against a metal pin (a stainless steel or chrome-plated pin with a circular cross section of 7-8 mm in diameter and a smooth surface) heated to 60°C to obtain a fiber. The fibers were left to stand at 23°C for one month, and are designated as Examples 15, 16, and 17, respectively. As in the case of the film, the degree of X-ray orientation of the α structure of the fibers of Examples 15 to 17 is presumed to be 50% or more. It has been reported that the breaking elongation of an unstretched film of a homopolymer of poly(3-hydroxybutyrate), which is in the form of a film, is significantly reduced by deterioration over time (GJM de Koning et al., POLYMER, 1993, Vol.34, No.19, 4089-4094, Figure 2). [Evaluation of long-term stability] The fiber produced in Example 17 was stored at 23° C. for half a year to obtain the fiber of Example 18.

[0103] [Tensile test: fiber] Stretched PHA fibers (Examples 17 and 18) with a length of 3 cm and a fiber diameter of approximately 0.1 to 0.3 mm were subjected to tensile tests up to fiber breakage using a tensile tester AGS-X or EZ-Test (manufactured by Shimadzu Corporation) at a temperature of 23°C, a test speed of 20 mm / min, and an initial length of 10 mm. The results of the tensile tests are shown in Table 4. As a result of the tensile tests, the breaking strain (breaking elongation) was approximately the same, and deterioration over time was almost suppressed.

[0104] [Table 4]

[0105] [Elasticity evaluation: fiber] The PHA fibers prepared in Examples 15 to 17 were evaluated by a cycle test in which the fibers were repeatedly stretched and contracted. Stretched PHA fibers with a length of 3 cm and a fiber diameter of about 0.1 to 0.3 mm were subjected to a cycle test at a temperature of 23°C and an initial length of 10 mm using a tensile tester AGS-X or EZ-Test (manufactured by Shimadzu Corporation). The fibers were stretched to a strain of 100% (twice the length) at a tensile speed of 20 mm / min, and then the clamps were moved to the original length at the same speed to shrink the PHA fibers. This was repeated five times. The stress-strain curves during the second to fifth contractions are shown in Figures 5 to 7.

[0106] The PHA fiber from Manufacturing Example 2 produced in Example 15 had a tensile elongation recovery rate (%) of approximately 70% at the start of the second elongation (i.e., considered to be approximately equal to the end of the first contraction), and a tensile elongation recovery rate (%) of approximately 70% to approximately 60% at the start of the third to fifth elongations (Figure 5). The PHA fiber from Manufacturing Example 5 produced in Example 16 had a tensile elongation recovery rate (%) of approximately 65% ​​at the start of the second elongation (i.e., considered to be approximately equal to the end of the first contraction), and a tensile elongation recovery rate (%) of approximately 65% ​​to approximately 60% at the start of the third to fifth elongations (Figure 6). The PHA fiber from Manufacturing Example 13 produced in Example 17 had a tensile elongation recovery rate (%) of approximately 60% at the start of the second elongation (i.e., considered to be approximately equal to the end of the first contraction), and a tensile elongation recovery rate (%) of approximately 60% to approximately 55% at the start of the third to fifth elongations (Figure 7).

[0107] Similarly, the PHA fiber prepared in Example 17 was stretched to 100% strain (twice the length) at a tensile speed of 20 mm / min, and then the clamp was moved at the same speed to 90% strain, causing the PHA fiber to shrink. This was repeated five times. The stress-strain curves during the first to fifth stretches are shown in Figure 8. The PHA fiber prepared in Example 17 was stretched to a strain of 100% and then repeatedly stretched to approximately 90%.

[0108] Similarly, the PHA fiber prepared in Example 17 was stretched to a strain of 10% (1.1 times the length) at a tensile speed of 20 mm / min, and then the clamp was moved to the original length at the same speed to shrink the PHA fiber. This was repeated five times. The stress-strain curves during the first to fifth stretches are shown in Figure 9. The PHA fiber prepared in Example 17 was stretched to a strain of 10%, and then repeatedly stretched to approximately 1% (1.01 times).

[0109] [Elasticity evaluation: film] The PHA film from Production Example 2 was evaluated by a cycle test in which it was repeatedly stretched and contracted. A PHA film cut to a length of 3 cm and a width of 3 mm was subjected to a cycle test using a tensile tester AGS-X or EZ-Test (manufactured by Shimadzu Corporation) at a temperature of 23°C and an initial length of 10 mm. The film was stretched to a strain of 1000% (11 times the length) at a tensile speed of 20 mm / min, and then the gripper was moved to the original length at the same speed to shrink the PHA film. This was repeated five times. The stress-strain curves during the second to fifth stretches are shown in Figure 10.

[0110] The PHA cast film produced from Production Example 2 had a deemed tensile elongation recovery rate (%) of about 50% at the beginning of the second elongation (i.e., deemed to be approximately equal to the end of the first contraction), and a deemed tensile elongation recovery rate (%) of about 45% to about 40% at the beginning of the third to fifth elongations (Figure 10). When the tensile elongation recovery rate (%) is calculated based on the displacement of 0 mm at the beginning of the second elongation, the tensile elongation recovery rate (%) at the third cycle test is 92%, at the fourth cycle test is 88%, and at the fifth cycle test is 85%.

[0111] The PHA film obtained in Production Example 5 was evaluated in a cycle test in the same manner as above. The stress-strain curves during the second to fifth contractions are shown in FIG. The PHA film from Production Example 5 had a deemed tensile elongation recovery rate (%) of about 50% at the beginning of the second elongation (i.e., deemed to be approximately equal to the end of the first contraction), and a deemed tensile elongation recovery rate (%) of about 45% to about 40% at the beginning of the third to fifth elongations. When the tensile elongation recovery rate (%) is calculated based on the displacement of 0 mm at the beginning of the second elongation, the tensile elongation recovery rate (%) in the third cycle test is 91%, in the fourth cycle test is 87%, and in the fifth cycle test is 85%.

[0112] The PHA film from Production Example 14 was evaluated in a cycle test in the same manner as above. The stress-strain curves during the second to fifth contractions are shown in FIG. The PHA film from Production Example 14 had a deemed tensile elongation recovery rate (%) of about 50% at the beginning of the second elongation (i.e., deemed to be approximately equal to the end of the first contraction), and had a deemed tensile elongation recovery rate (%) of about 50% to about 40% at the beginning of the third to fifth elongations. When the tensile elongation recovery rate (%) was calculated based on the displacement of 0 mm at the beginning of the second elongation, the tensile elongation recovery rate (%) in the third cycle test was 96%, in the fourth cycle test was 94%, and in the fifth cycle test was 92%.

[0113] Example 19: Preparation of elastic P(3HB-co-3HV) fibers and their structural analysis <Experiment> P(3HB-co-12%-3HV) (Metabolix) was melted at 150°C for 5 minutes using a melt spinning apparatus. The extruded resin was then necked and stretched by hand up to 5 times to produce a fiber with elasticity that could be stretched up to 2 times. The resulting stretchable fiber was irradiated with X-rays while undergoing a cycle test at the large synchrotron radiation facility SPring-8 (FSBL03XU) and structural analysis was performed. Specifically, a cycle test was performed as follows: 0.5N → 2N → 0.5N → 4N → 0.5N → 6N → 0.5N → 10N → 0.5N, and the relationship between elasticity and molecular chain structure was analyzed. Furthermore, the resulting fiber was stretched 1 time, 1.5 times, and 2 times, and annealed at 100°C for 24 hours. The stretching and structural analysis were specifically performed in the same manner as in Examples 1 to 14. As a result, two-stage drawn heat-treated fibers were produced at 1x, 1.5x, and 2x stretching, and their physical properties and structure were evaluated using a tensile tester and X-ray diffraction.

[0114] <Results and Discussion> [Relationship between elasticity and molecular chain structure] A dynamic test was conducted in which the stretchable fiber was irradiated with X-rays while undergoing a cyclic test, and a structural analysis was performed. WAXD showed that a strong peak of β crystals appeared when a load was applied, but the peak decreased when the load was removed (Figure 25). SAXS showed that the long period between α crystals increased when a load was applied, and decreased when the load was removed. Furthermore, the periodic change in the long period almost coincided with the change in the distance between the grippers of the fiber. From this, it is thought that when loading is applied, the tie molecules between the α crystals stretch out to the point where β crystals appear, but when loading is removed, the β crystals that had appeared return to tie molecules. From these results, it is thought that the cause of stretchability is the reversible change between tie molecules and β crystals.

[0115] [Study on increasing the strength of elastic fibers] Tensile tests were performed on the fibers that were heat-treated by two-step stretching at 1x, 1.5x, and 2x. The breaking strength increased with increasing stretch ratio, and the breaking strength of the fiber that was heat-treated by two-step stretching at 2x was 302MPa. On the other hand, the breaking elongation of the fiber decreased with increasing stretch ratio (Figure 26). As a result of structural analysis of these fibers, it was found that, for the fibers that were heat-treated by two-step stretching at 1.5x and 2x from WAXD, the tie molecules in the amorphous region between the α crystals (lamellar crystals consisting of a double helix structure) and the α crystals were fully stretched, and β crystals (planar zigzag structure) derived from the extended chains of the molecules were expressed. Furthermore, SAXS showed streak scattering in the fibers that were heat-treated by two-step stretching at 1.5x and 2x, which indicated that the shish part of the shish kebab structure was regularly packed. From the above, it is considered that the increase in breaking strength is due to the molecular chains of the shish part being regularly packed while being fully stretched to form β crystals, and the decrease in breaking elongation is due to the molecular chains being fully extended. [Industrial Applicability]

[0116] The films, fibers, and other molded articles exhibiting biodegradability, biocompatibility, and bioabsorbability of the present invention are flexible and can follow external forces and shapes, and are useful in industrial applications such as films, fibers, textiles, and film and fiber composites that require elasticity, etc. They can be used in applications that take advantage of the biodegradability and bioabsorbability of plastics used in agriculture, fisheries, commerce, industry, medicine, etc.

Claims

1. A polyester containing 3-hydroxybutyrate units and 4-hydroxybutyrate units, the ratio of the 4-hydroxybutyrate units to the total monomer units being 10 mol% to 30 mol%, the polyester containing an α structure and an amorphous structure, the degree of X-ray orientation of the α structure being 50% or more and 95% or less, In the stretched state, a β structure is detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement, and in the unloaded state, the β structure is reduced or no β structure is detected by wide-angle X-ray diffraction measurement and small-angle X-ray scattering measurement compared to the stretched state; The elasticity is such that the tensile elongation recovery rate measured by the following method is 20% or more and 100% or less. Stretched polyester: In the case of fibers, a fiber with a length of 3 cm and a fiber diameter of approximately 0.1 to 0.3 mm is used for the tensile test. Then, under the conditions of a temperature of 23°C and an initial length of 10 mm, the fiber is stretched at 20 mm / min to a strain of 100% (20 mm, which is twice the initial length, i.e., a displacement length of 10 mm), and then the gripping tools are moved at the same speed to the original length to contract the fiber. If the displacement length at the start of the second stretching is X mm, the tensile stretch recovery rate R (%) is expressed as R = [(20 - (X + 10)) / 10] x 100. In the case of cast film, a film cut to a length of 3 cm and a width of 3 mm is stretched using a tensile tester at a temperature of 23° C. and an initial length of 10 mm at a tension speed of 20 mm / min to a strain of 1000% (110 mm, which is 11 times the initial length, i.e., a displacement length of 100 mm), and then the gripper is moved at the same speed to the original length to shrink the film. If the displacement length at the start of the second stretching is y mm, the assumed tensile elongation recovery rate r (%) based on the displacement length of 0 mm of the unstretched film is is expressed by r = [(110 - (y + 10)) / 100] x 100. The tensile elongation recovery rate R (%) is expressed by R = r 2 / r 1 x 100 where r 1 is the deemed tensile elongation recovery rate after the first stretching, and r 2 is the deemed tensile elongation recovery rate after the second stretching.

2. 2. The stretched polyester according to claim 1, which is stretched after crystallization and exhibits stretchability after the load is removed.

3. 3. The stretched polyester according to claim 1, wherein the crystal structure of the stretched polyester is oriented by stretching.

4. 4. The stretched polyester according to claim 2 or 3, wherein the crystal structure has been oriented by stretching at a ratio of 2 to 20.

5. The polymer according to any one of claims 1 to 4, which comprises a lamellar crystal structure and an amorphous structure, develops a specific extended chain structure during stretching, and the extended chain structure significantly decreases or disappears when the tensile load is removed. Stretched polyester.

6. 6. The stretched polyester according to claim 1, wherein the extended chain structure is a planar zigzag structure.

7. 7. The oriented polyester according to claim 1, wherein the lamellar crystalline structure comprises a helical folding structure.

8. 8. The stretched polyester according to claim 1, which has a weight average molecular weight of 100,000 to 3,000,000 as measured by gel permeation chromatography relative to polystyrene standards.

9. 9. The stretched polyester of claim 1 which is biodegradable.

10. 10. The stretched polyester of claim 1 which is bioabsorbable.

11. 11. The stretched polyester according to claim 1, which is of biological or chemical synthetic origin.

12. A film comprising the stretched polyester of claim 1 .

13. A fiber comprising the oriented polyester of claim 1 .

14. A molded article comprising the stretched polyester according to claim 1 .

15. A stretching step of orienting a polyester containing 3-hydroxybutyrate units and 4-hydroxybutyrate units, the ratio of the 4-hydroxybutyrate units to the total monomer units being 10 mol % to 30 mol %, by stretching after crystallization; and An unloading step of unloading the tensile load of the polyester oriented by the stretching step: A method for producing the oriented polyester of claim 1 , comprising:

16. 16. The method according to claim 15, wherein the oriented polyester produced is in the form of a film, fiber or molded article.

Citation Information

Patent Citations

  • 3-hydroxybutyrate polymer

    JP1984059419A

  • Production of polyester film

    JP1986120724A

  • Copper alloy filament and its production

    JP1988068245A

  • Polyester copolymer and its production

    JP1989048821A

  • Preparation of copolyester

    JP1991216193A