Plating defect estimation method and semiconductor device manufacturing method

The plating defect estimation method measures underlayer properties to predict spike occurrence, enhancing semiconductor device yield and reliability by avoiding defective plating processes.

JP7568342B2Active Publication Date: 2024-10-16MINEBEA POWER SEMICON DEVICE INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021159508
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-10-16
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing methods for manufacturing semiconductor devices fail to effectively estimate the degree of plating defects, particularly the spike phenomenon, before the plating process, leading to potential adhesion issues and electrical short circuits, which negatively impact yield and product life.

Method used

A plating defect estimation method that measures the physical properties of the underlayer before plating pretreatment, using optical and X-ray diffraction techniques to estimate the degree of spike occurrence based on correlations established with known plating materials, allowing for informed decision-making on whether to proceed with the plating process.

Benefits of technology

Enables the estimation of spike occurrence before forming the plating film, thereby improving yield by preventing defective plating processes and ensuring high adhesion and reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568342000001
    Figure 0007568342000001
  • Figure 0007568342000002
    Figure 0007568342000002
  • Figure 0007568342000003
    Figure 0007568342000003
Patent Text Reader

Abstract

To provide a method for estimating plating defects, which can estimate the degree of occurrence of spikes that are caused by plating, before a plating film is formed; and a method for producing a semiconductor device with the use of the method.SOLUTION: The method for estimating plating defects includes: a measurement step of measuring physical properties of a surface of a ground layer before a pretreatment step for plating, which subjects the ground layer to pretreatment for plating; and an estimation step of estimating the degree of occurrence of the spikes that occur on the ground layer by plating, on the basis of the measured physical properties. The method for producing a semiconductor device includes: a ground layer forming step of forming the ground layer on a surface of a semiconductor wafer; a pretreatment step for plating, which subjects the ground layer to pretreatment for the plating; a plating step of subjecting the pretreated ground layer to the plating; the measurement step of measuring the physical properties of the surface of the ground layer, before the pretreatment step for the plating; and the estimation step of estimating the degree of occurrence of the spikes that occur on the ground layer by plating, on the basis of the measured physical properties.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plating defect estimation method for estimating the occurrence rate of spikes that occur on an underlayer due to plating, and a manufacturing method of a semiconductor device using the same. [Background technology]

[0002] Conventionally, various plating processes have been developed to form uniform plating films with few defects. Electrolytic plating and electroless plating are used for various purposes such as improving the appearance of products, improving wear resistance and corrosion resistance, and constructing fine structures of semiconductor devices. Nickel plating is used in various fields because of its excellent mechanical properties, corrosion resistance, and good adhesion.

[0003] Patent Document 1 describes a black luster material using an electroless nickel plating method or an electroless nickel alloy plating method, and a manufacturing method thereof. Examples of the substrate include aluminum pieces. It is said that the desired luster can be obtained by adjusting the reflectance of the black luster material in visible light.

[0004] Patent Document 2 describes a roughened nickel-plated sheet. The substrate includes an aluminum sheet, etc. It is said that excellent adhesion can be obtained by adjusting the surface brightness of the roughened nickel phase.

[0005] Patent Document 3 describes a wear-resistant member having a hard plating film and a power transmission part using the member. The hard plating film is formed by Ni-P plating. Examples of the substrate include aluminum alloys. It is said that adjusting the average crystallite size of the Ni-P plating film ensures wear resistance, fatigue life, plating adhesion, and the like.

[0006] Patent Document 4 describes the spike phenomenon that occurs during nickel plating. It describes that when the aluminum base is etched into a concave shape during the pre-treatment stage of plating, nickel from the plating enters the concave shape and is observed as a spike shape. It is said that a metal replacement treatment solution containing quaternary ammonium hydroxide suppresses attacks on the aluminum base and the occurrence of cracks. [Prior art documents] [Non-patent literature]

[0007] [Patent Document 1] JP 2002-363771 A [Patent Document 2] International Publication No. 2020 / 017655 [Patent Document 3] JP 2007-023316 A [Patent Document 4] JP 2009-127101 A Summary of the Invention [Problem to be solved by the invention]

[0008] In the manufacturing process of semiconductor devices, the surface of electrodes that connect semiconductor elements may be plated. Currently, in various fields including the manufacturing of semiconductor devices, it is desirable to grasp the occurrence degree of plating defects at an early stage. If plating defects are detected during product inspection after plating, the plating process itself becomes a waste, which greatly affects the yield. Therefore, there is a demand to estimate the occurrence degree of plating defects from the physical properties of the plating base, rather than from the inspection of the plating film itself.

[0009] In Patent Documents 1 to 3, the reflectance, brightness, crystallite size, etc. are adjusted to form an appropriate plating film. However, these physical properties are the surface properties of the plating film, and are only known after plating. The method of measuring the surface properties of the plating film as in Patent Documents 1 to 3 cannot improve the yield including the plating process. There is a demand for a technology that can estimate the occurrence degree of plating defects before the plating process and determine whether or not to carry out the plating process depending on the risk of plating defects occurring.

[0010] The spike phenomenon is a particularly problematic plating defect. The spike phenomenon is a phenomenon in which the plating film penetrates into the surface of the base material in a spike-like shape. The spike phenomenon occurs when pitting corrosion occurs in the metal of the base material during pre-treatment for plating, and the plating metal precipitates in the pits during plating. Countless protruding, needle-like, or other spikes are formed at the interface between the base material and the plating film. When spikes are formed, there is a risk that the adhesion of the plating film will decrease or an electrical short circuit will occur, which may shorten the product life.

[0011] Therefore, an object of the present invention is to provide a plating defect estimation method that can estimate the occurrence rate of spikes caused by plating before a plating film is formed, and a manufacturing method of a semiconductor device using the same. [Means for solving the problem]

[0012] In order to solve the above problem, the plating defect estimation method of the present invention includes a measurement process for measuring physical properties of the surface of a base layer prior to a plating pretreatment process in which a base layer is pretreated for plating, and an estimation process for estimating the degree of occurrence of spikes caused on the base layer by plating based on the measured physical properties.

[0013] In addition, a manufacturing method for a semiconductor device according to the present invention includes a base layer formation step of forming a base layer on a surface of a semiconductor wafer, a plating pretreatment step of performing a plating pretreatment on the base layer, a plating step of performing plating on the pretreated base layer, a measurement step of measuring physical properties of the surface of the base layer prior to the plating pretreatment step, and an estimation step of estimating the degree of occurrence of spikes caused on the base layer by plating based on the measured physical properties. Effect of the Invention

[0014] According to the present invention, it is possible to provide a plating defect estimation method capable of estimating the occurrence rate of spikes caused by plating before a plating film is formed, and a manufacturing method of a semiconductor device using the same. [Brief description of the drawings]

[0015] [Figure 1] 1 is a flowchart showing a plating defect estimation method according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view illustrating a schematic example of a configuration of a semiconductor device. [Figure 3A] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after an oxide film has been formed). [Figure 3B] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after a p-type semiconductor layer has been formed). [Figure 3C] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after a metal underlayer has been formed). [Figure 4A] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after a resin layer has been formed). [Figure 4B] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after a metal underlayer has been formed). [Figure 4C] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor device (after a plating layer has been formed). [Diagram 5] 1 is a flow chart showing an electroless plating process. [Figure 6] FIG. 13 is a diagram showing the relationship between the measurement results of the surface brightness of the underlayer and the evaluation results of the occurrence rate of spikes. [Figure 7] FIG. 13 is a diagram showing the relationship between the measurement results of the reflectance of the surface of the underlayer and the evaluation results of the occurrence rate of spikes. [Figure 8] FIG. 13 is a diagram showing the relationship between the measurement results of the crystallite size on the surface of the underlayer and the evaluation results of the occurrence rate of spikes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a plating defect estimation method according to an embodiment of the present invention and a semiconductor device manufacturing method using the same will be described with reference to the drawings. Note that the same reference numerals are used to designate the same components in the following drawings, and duplicated descriptions will be omitted.

[0017] FIG. 1 is a flowchart showing a plating defect estimation method according to an embodiment of the present invention. 1, the plating defect estimation method according to the present embodiment is carried out as a plating defect estimation step S120 accompanying a base layer forming step S110, a plating pretreatment step S130, and a plating step S140. The plating defect estimation step S120 includes a measurement step S10, an estimation step S20, and a determination step S30. Depending on the result of the determination step S30, a predetermined plating pretreatment step S130 and a plating step S140 are performed, or the predetermined plating pretreatment step S130 and a plating step S140 are stopped.

[0018] The plating defect estimation method according to the present embodiment is a method for estimating the occurrence rate of spikes caused by plating. In the plating defect estimation method according to the present embodiment, the occurrence rate of spikes is estimated from the physical properties of the surface of the base layer to be plated. The occurrence rate of spikes can be estimated before the formation of a plating film, without actually forming the plating film. Therefore, it becomes possible to determine whether or not to perform plating before the formation of the plating film.

[0019] Spikes are caused by the spiking phenomenon, where the plating film penetrates the surface of the underlayer in a spike-like form. Spikes are formed when pitting occurs in the underlayer, which is made of metal, during pretreatment for plating, and the plating metal precipitates in the pits during plating. The spikes are made of the plating metal, and appear in countless protruding, needle-like, or other shapes that protrude toward the underlayer at the interface between the underlayer and the plating film.

[0020] If spikes are formed, there is a risk of reducing the adhesion of the plating film and causing an electrical short circuit via the underlayer. This may shorten the product life of the plated product. However, according to the plating defect estimation method of this embodiment, the occurrence rate of spikes can be estimated before the formation of the plating film, so that it is possible to determine in advance whether to perform the plating pretreatment step S130 and the plating step S140 based on the estimation result of the occurrence rate of spikes. This makes it possible to improve the product yield.

[0021] The occurrence rate of spikes can be evaluated, for example, as the number of spikes. The number of spikes can be defined as the number of spikes that cross the interface between the underlayer and the plating film per unit length of a virtual line along the interface. For example, if the number of spikes per 1 μm of interface length is about one, the occurrence rate of spikes can be said to be low. On the other hand, if the number of spikes exceeds several, the occurrence rate of spikes can be said to be high. Alternatively, the occurrence rate of spikes can also be evaluated as the number of spikes that cross the interface between the underlayer and the plating film per unit area.

[0022] In the plating defect estimation method according to the present embodiment, the correlation between the surface properties of the underlayer and the occurrence rate of spikes is determined before estimation. The correlation is determined using a plating material with a known occurrence rate of spikes, i.e., a plating material on which spikes have already occurred. The correlation between the surface properties of the underlayer of a plating material on which spikes have already occurred and the occurrence rate of spikes is determined by measuring each of them.

[0023] The degree of spike occurrence is estimated for a plated material before it is subjected to pre-treatment for plating. For a plated material (base layer) whose degree of spike occurrence is unknown, the physical properties of the base layer surface are measured, and the measurement results are applied to the correlation obtained using a plated material whose degree of spike occurrence is known, and the approximate number of spikes per unit length at the interface between the base layer and the plated layer can be obtained as an estimate of the degree of spike occurrence.

[0024] The underlayer forming step S110 is a step of forming an underlayer made of metal on a workpiece to be plated.

[0025] Examples of metals that form the underlayer include aluminum, aluminum alloys, magnesium, and magnesium alloys. These metals are base metals that have a lower standard electrode potential than zinc and are prone to electrochemical corrosion. These metals are prone to pitting corrosion, which is a cause of spikes, so estimating the occurrence rate of spikes in underlayers made of these metals can greatly improve product yields.

[0026] The measurement step S10 is a step for measuring the surface properties of the undercoat layer prior to pretreatment for plating. In the pretreatment step S130, pitting corrosion, which is a cause of the spike phenomenon, may occur depending on the type of metal forming the undercoat layer and the type of acid solution, alkaline solution, chemical solution, etc. used in the treatment. In the measurement step S10, the surface properties of the undercoat layer are measured to provide information for estimating the degree of occurrence of such pitting corrosion or spikes before the occurrence of pitting corrosion.

[0027] The measurement step S10 can be either a step of optically measuring the surface of the underlayer or a step of X-ray diffraction measuring the surface of the underlayer. In the optical measurement, the reflectance or brightness of the surface of the underlayer is measured. In the X-ray diffraction measurement, the X-ray diffraction spectrum is measured, the full width at half maximum of an appropriate peak due to the metal of the underlayer is obtained, and the crystallite diameter of the surface of the underlayer is calculated using the full width at half maximum.

[0028] The reflectance of the surface of the undercoat layer, the brightness of the surface of the undercoat layer, and the crystallite size of the surface of the undercoat layer indirectly indicate the possibility of pitting corrosion, and have been confirmed by the present inventors to be correlated with the degree of spike occurrence. When these physical properties are measured for a plated material whose degree of spike occurrence is known, a correlation between these physical properties and the degree of spike occurrence can be obtained. When these physical properties are measured for a plated material whose degree of spike occurrence is unknown and applied to the correlation, the unknown degree of spike occurrence can be estimated.

[0029] The estimation step S20 is a step of estimating the occurrence rate of spikes on the underlayer due to plating based on the measured physical properties of the surface of the underlayer. In the estimation step S20, the measurement result of the plated material, whose occurrence rate of spikes is unknown, is applied to the correlation obtained using the plated material, whose occurrence rate of spikes is known, to obtain an estimation result of the occurrence rate of spikes on the plated material.

[0030] The correlation between the surface properties of the underlayer and the incidence of spikes can be plotted as a biaxial graph or the like. This correlation can be subjected to regression analysis using the least squares method or the like, and applied to estimation as a linear correlation. It can also be applied to estimation using machine learning techniques. The estimation result of the incidence of spikes on the plated material can be obtained as an estimated value of the approximate number of spikes per unit length at the interface between the underlayer and the plating film, an estimated range of the approximate number, etc.

[0031] In the estimation step S20, in order to estimate the degree of spike occurrence, a regression model formula expressing a linear correlation or the like can be created from the correlation obtained using a plating material with a known degree of spike occurrence. By substituting the measurement results of the physical properties of the surface of the base layer of a plated material with an unknown degree of spike occurrence into the regression model formula, it is possible to obtain an estimate of the approximate number of spikes per unit length at the interface between the base layer and the plating film, an estimated range of the approximate number, etc.

[0032] The determination step S30 is a step of comparing the estimated spike occurrence rate with a predetermined standard to determine the amount of spikes that are likely to occur. By comparing the estimated spike occurrence rate for the plated material with a predetermined standard or the like according to the product, the disposal of the plated material can be sorted according to the risk of spike occurrence.

[0033] The comparison criteria may be the number of spikes per unit length of the interface between the underlayer and the plating film, or the range of the number, and any value or range of values ​​may be set. For example, in the case of a plating layer formed on an electrode to which a semiconductor element is connected, if the number of spikes per 1 μm of interface length exceeds several, there is a high possibility of an electrical short circuit through the underlayer. Therefore, the comparison criteria may be 1, 0.5, or the like, in terms of the number of spikes per 1 μm of interface length.

[0034] As shown in FIG. 1, when the estimated result of the occurrence rate of spikes is greater than the threshold (determination step S30; YES), the predetermined plating pretreatment step S130 and plating step S140 can be stopped. Instead of simply stopping and discarding, the contents of the plating pretreatment step S130 may be changed depending on whether the estimated result of the occurrence rate of spikes is greater than or less than the threshold. As an example of changing the contents of the plating pretreatment step S130, for example, the plating pretreatment step S130 may be performed under conditions different from the predetermined plating pretreatment step S130. As another example of changing the contents of the plating pretreatment step S130, for example, before the predetermined plating pretreatment step S130, a resurface treatment step may be performed as an additional plating pretreatment step, in which an appropriate resurface treatment such as heat treatment, mechanical polishing, chemical polishing, or electrolytic polishing is performed on the surface of the base layer, and then the predetermined plating pretreatment step S130 similar to the normal case may be performed on the plated material that has been subjected to the resurface treatment. Thereafter, the plating process S140 can be performed. On the other hand, if the estimated result of the occurrence rate of spikes is less than the threshold value (determination process S30: NO), the predetermined plating pretreatment process S130 and plating process S140 can be performed.

[0035] The plating pretreatment step S130 is a step of performing pretreatment for plating on the base layer formed of metal. In the plating pretreatment step S130, an acid solution, an alkaline solution, or other chemical solution is used to perform cleaning and surface treatment on the surface of the base layer before plating. The plating pretreatment step S130 electrochemically corrodes the metal of the base layer to cause pitting corrosion, which is a cause of spikes. The plating pretreatment step S130 may be composed of a single step or multiple steps.

[0036] The treatments constituting the plating pretreatment process S130 include a degreasing and cleaning treatment to remove oils and greases from the surface of the base layer, an alkaline cleaning treatment to remove oxide films and the like on the surface of the base layer using an alkaline solution, an acid cleaning treatment to remove smut and the like using an acid solution, and a zincate treatment to replace the surface of the base layer with a zinc film.

[0037] Zincate treatment is carried out when the underlayer is made of aluminum or an aluminum alloy. In the zincate treatment, the oxide film on the surface of the underlayer is removed, and a zinc film is formed on the surface of the underlayer. When the zinc film is formed, zinc is replaced by the plating metal during plating, accelerating the deposition of the plating film. In the zincate treatment process, a zincate solution that corrodes metal is used.

[0038] The plating step S140 is a step of plating the surface of the underlayer. The plating method may be either electrolytic plating or electroless plating. However, electroless plating is preferred from the viewpoint of forming a plating layer with high uniformity in thickness and composition, and from the viewpoint of reducing the cost of the plating step.

[0039] The plating metal for forming the plating layer may be nickel, copper, chromium, iron, tin, silver, palladium, platinum, gold, alloys of these, etc. When using these plating metals, the correlation between the occurrence rate of spikes and the reflectance of the metal surface, the brightness of the metal surface, and the crystallite size of the metal surface is determined in advance for each type of plating metal.

[0040] According to the plating defect estimation method of the present embodiment, the occurrence rate of spikes is estimated from the physical properties of the surface of the underlayer, so that the occurrence rate of spikes can be estimated before the formation of the plating film. Since it is possible to plate only the plated material that is estimated to have few spikes, it is possible to obtain a product with a long product life that is less likely to cause a decrease in adhesion of the plating film or an electrical short circuit through the underlayer. In addition, if the estimated result of the occurrence rate of spikes is high, the plating process can be stopped or the conditions of the plating pretreatment process can be changed, so that the product yield can be improved.

[0041] Next, a method for manufacturing a semiconductor device using the plating defect estimation method will be described with reference to the drawings.

[0042] The plating defect estimation method can be incorporated into a manufacturing process of a semiconductor device, and can be used to estimate the occurrence rate of spikes in a plating layer formed during the manufacturing process of a semiconductor device.

[0043] 1, the method for manufacturing a semiconductor device includes an underlayer forming step S110, a plating defect estimating step S120, a plating pretreatment step S130, and a plating step S140. The plating defect estimating step S120 is composed of the plating defect estimating process described above, and includes a measuring step S10, an estimating step S20, and a determining step S30.

[0044] The method for manufacturing a semiconductor device includes a semiconductor element forming process (not shown) in which semiconductor elements such as switching elements and diode elements are formed on a semiconductor wafer.

[0045] In the underlayer formation step S110, an underlayer made of metal is formed on the semiconductor wafer. The underlayer can be formed by using a sputtering method, a deposition method, a chemical vapor deposition (CVD) method, or the like. The underlayer constitutes, for example, a part of an electrode of a semiconductor element. The underlayer may be formed on the surface of the semiconductor wafer, or may be formed on the surface of a functional layer such as a semiconductor element or an insulating film formed on the surface of the semiconductor wafer.

[0046] The semiconductor device may be a semiconductor chip or a semiconductor module. In the case of a semiconductor module, a step of electrically connecting the semiconductor chip to an insulating substrate may be included. In the case of a semiconductor module, the semiconductor device is completed by mounting the semiconductor chip on an insulating substrate, electrically connecting electrodes formed on the semiconductor chip to wiring formed on the insulating substrate to form a circuit, and housing them in a housing and sealing them with an insulating sealing resin.

[0047] FIG. 2 is a cross-sectional view illustrating a schematic example of a configuration of a semiconductor device. 2 shows a semiconductor device 100 equipped with a freewheel diode, which is a semiconductor element. The semiconductor device 100 is equipped with electrodes on the front and back surfaces of a semiconductor chip, on which plating layers 104, 112 are formed for electrical connection. One or both of the plating layers 104, 112 equipped on the semiconductor device 100 are used to estimate the occurrence rate of spikes.

[0048] 2 shows an example in which a silicon substrate, which is an n-type semiconductor, is used as the substrate of the semiconductor element. However, a silicon substrate, which is a p-type semiconductor, may also be used as the substrate of the semiconductor element. As the semiconductor, wide-gap semiconductors such as silicon carbide (SiC), gallium nitride (GaN), and gallium oxide (GaO) can also be used in addition to silicon.

[0049] Although a freewheel diode is shown in FIG. 2, a semiconductor element such as a metal-oxide-semiconductor field-effect transistor (MOSFET) or an insulated gate bipolar transistor (IGBT) may be included.

[0050] 2, the semiconductor device 100 includes an insulating substrate 101, a conductive member 102, a semiconductor substrate 108, a cathode electrode 113, an anode electrode 114, a resin layer 111, etc. The cathode electrode 113 is formed, for example, of a plating layer 104, a metal underlayer 105, a copper diffusion prevention layer 106, and a metal layer 107. The anode electrode 114 is formed, for example, of a metal underlayer 109 and a plating layer 112.

[0051] The semiconductor substrate 108 has a structure in which a p-type semiconductor layer 108a, an n-type drift layer 108b, and an n+ type drift layer 108c are stacked in this order from the top surface side to the bottom surface side. The semiconductor substrate 108 forms a semiconductor element 150 by bonding these semiconductor layers together. The p-type semiconductor layer 108a is doped with p-type impurities. The n- type drift layer 108b is doped with low-concentration n-type impurities. The n+ type drift layer 108c is doped with high-concentration n-type impurities.

[0052] On the lower surface of the semiconductor substrate 108, a metal layer 107, a copper diffusion prevention layer 106, a metal underlayer 105, and a plating layer 104 are laminated in this order from the downward direction. The metal layer 107, the copper diffusion prevention layer 106, the metal underlayer 105, and the plating layer 104 form a cathode electrode 113, which is an electrode structure on the cathode side. These layers and the semiconductor substrate 108 are electrically connected to each other.

[0053] Metal layer 107 forms the main body of the electrode, and is made of aluminum or an aluminum alloy such as an aluminum-silicon alloy. Copper diffusion prevention layer 106 is a layer that prevents thermally diffused copper from penetrating into semiconductor substrate 108, and is made of titanium, titanium nitride, tungsten, titanium tungsten, nickel, or the like. Providing copper diffusion prevention layer 106 can prevent copper, which has a high diffusion coefficient, from diffusing from bonding layer 103, etc., into semiconductor substrate 108. This can improve the long-term reliability of semiconductor element 150.

[0054] The metal underlayer 105 is a underlayer to be plated, and is made of aluminum or an aluminum alloy such as an aluminum-silicon alloy. The plating layer 104 is a plating film formed by plating, and is made of a nickel-phosphorus alloy (Ni-P alloy), a nickel-boron alloy (Ni-B alloy), or the like. From the viewpoints of uniformity, corrosion resistance, and the like, the plating layer 104 is preferably made of a nickel-phosphorus alloy.

[0055] An oxide film 110 is formed on the upper surface of the semiconductor substrate 108. The oxide film 110 is formed on a part of the upper surface of the semiconductor substrate 108. A contact region is formed on the upper surface of the semiconductor substrate 108 where the semiconductor substrate 108 is not covered with the oxide film 110, and the semiconductor substrate 108 is partially exposed. A metal base layer 109 and a plating layer 112 are laminated in this order on the exposed upper surface of the semiconductor substrate 108. The metal base layer 109 and the plating layer 112 are electrically connected to the semiconductor substrate 108.

[0056] An oxide film 110 is formed around the metal base layer 109, and a termination region is formed in which the semiconductor substrate 108 is covered with the oxide film 110. A resin layer 111 is formed on the surface of the oxide film 110 around the metal base layer 109. The oxide film 110 is an electrically insulating layer and is made of silicon dioxide. The resin layer 111 is an electrically insulating layer and is made of an insulating resin such as polyimide.

[0057] The metal underlayer 109 is a underlayer to be plated, and is made of aluminum or an aluminum alloy such as an aluminum-silicon alloy or an aluminum-copper alloy.

[0058] The plating layer 112 is a plating film formed by plating, and is made of a nickel-phosphorus alloy (Ni-P alloy), a nickel-boron alloy (Ni-B alloy), etc. From the viewpoints of uniformity, corrosion resistance, etc., the plating layer 112 is preferably made of a nickel-phosphorus alloy.

[0059] The semiconductor element 150 formed by the semiconductor substrate 108 constitutes a semiconductor chip together with the cathode electrode 113, the anode electrode 114, the resin layer 111, etc., and is mounted on the insulating substrate 101. A conductive member 102 is bonded to the upper surface of the insulating substrate 101. The plating layer 104 of the cathode electrode 113 is bonded to the upper surface of the conductive member 102 via a bonding layer 103. The plating layer 104 is electrically connected to the conductive member 102 and the semiconductor substrate 108.

[0060] The insulating substrate 101 is a substrate that supports the semiconductor element 150 and electrically insulates the semiconductor element 150 from the surroundings, and is made of, for example, ceramics. The conductive member 102 has a pattern that forms wiring on the cathode side, and is made of copper. The bonding layer 103 thermally connects the semiconductor element 150 and the insulating substrate 101, and is made of, for example, a sintered metal such as copper, cupric oxide, or silver. The bonding layer 103 may also be made of solder.

[0061] The plating layer 112 of the anode electrode 114 is not covered with the resin layer 111 and is exposed above the semiconductor device 100. A wire (not shown) forming wiring on the anode side is electrically connected to the upper surface of the plating layer 112. The semiconductor element 150 is connected to other elements, etc. by wire bonding to form a predetermined circuit.

[0062] 3A to 3C are diagrams showing a method for manufacturing a semiconductor device. Fig. 3A is a cross-sectional view showing a state in which an oxide film has been formed on a semiconductor wafer. Fig. 3B is a cross-sectional view showing a state in which a p-type semiconductor layer has been formed. Fig. 3C is a diagram showing a state in which a metal base layer on the anode side has been formed.

[0063] As shown in FIG. 3A, in manufacturing the semiconductor device 100, first, a silicon wafer 90 is prepared. Before the state shown in FIG. 3A is reached, an oxide film (not shown) is formed on the surface of the silicon wafer 90 by thermal oxidation. The silicon wafer 90 with the oxide film formed on its surface is subjected to a photolithography process. In the photolithography process, a resist material is applied to the surface of the silicon wafer 90 with the oxide film formed on it. The resist material is then exposed to light, and a resist with a predetermined pattern is developed. When the exposed areas not protected by the resist are etched, the oxide film in the area where the semiconductor element 150 is to be formed is removed.

[0064] Next, the region from which the oxide film has been removed is doped with p-type impurities such as boron or aluminum. Then, after the resist is removed and annealing is performed, a p-type semiconductor layer 108a is formed in a predetermined region on the upper surface side of the silicon wafer 90, as shown in Fig. 3A. Since the silicon wafer 90 has a high resistivity, when the p-type semiconductor layer 108a is formed on one side of the silicon wafer 90, the other side becomes an n-type semiconductor layer (n-type drift layer 108b).

[0065] 3B, an oxide film 110 is formed on one surface of the silicon wafer 90. The oxide film 110 can be formed by, for example, a thermal oxidation method, a CVD method, or the like. When the oxide film 110 is subjected to the same photolithography and etching steps as the silicon wafer 90, a part of the oxide film 110 is removed, and a contact region for connecting the p-type semiconductor layer 108a and the metal base layer 109 is formed.

[0066] 3C, a metal base layer 109 is formed on the surface of the p-type semiconductor layer 108a. The metal base layer 109 can be formed by, for example, a sputtering method, a vapor deposition method, a CVD method, or the like. When the formed metal film is subjected to a photolithography process and an etching process similar to those for the silicon wafer 90, a patterned metal base layer 109 is obtained.

[0067] Next, a resin layer 111 is formed on the surface of the oxide film 110 around the metal base layer 109. The resin layer 111 can be formed, for example, by applying a solution containing a polyimide precursor and a photosensitive material to the surface of the oxide film 110 or the metal base layer 109, and exposing the solution to polyimide. When the termination region is exposed to light, the periphery of the metal base layer 109 is sealed with the resin layer 111 as shown in FIG. 4A.

[0068] Figures 4A to 4C are diagrams showing a method for manufacturing a semiconductor device. Figure 4A is a diagram showing a state after a resin layer has been formed. Figure 4B is a diagram showing a state after a metal underlayer on the cathode side has been formed. Figure 4C is a diagram showing a state after a plating layer on the anode side and a plating layer on the cathode side have been formed.

[0069] As shown in Fig. 4A, the lower surface side of the n-type drift layer 108b is doped with n-type impurities such as phosphorus and arsenic. Then, when annealing is performed with a laser or the like, an n+ type drift layer 108c containing a higher concentration of n-type impurities than the n-type drift layer 108b is formed on the lower surface side of the silicon wafer 90. A depletion layer is secured by the n- type drift layer 108b and the n+ type drift layer 108c. The surface side of the n-type drift layer 108b is ground to reduce the wafer thickness before doping with the n-type impurities.

[0070] 4B, a metal layer 107 is formed on the surface of the n+ type drift layer 108c. A copper diffusion prevention layer 106 is formed on the surface of the metal layer 107. A metal base layer 105 is formed on the surface of the copper diffusion prevention layer 106. The metal layer 107, the copper diffusion prevention layer 106, and the metal base layer 105 can be formed by, for example, a sputtering method, a vapor deposition method, a CVD method, or the like. For example, the thickness of the metal base layer 105 can be about 2.0 μm when an Al-Si alloy is used.

[0071] 4C, a plating layer 104 is formed on the surface of the metal base layer 105 on the cathode side. Also, a plating layer 112 is formed on the surface of the metal base layer 109 on the anode side. When forming the plating layers 104, 112, the degree of spike occurrence caused by plating is estimated by the plating defect estimation method described above, and a plated material on which an appropriate metal base layer 105, 109 is formed is used according to the risk of spike occurrence.

[0072] As shown in Fig. 1, when estimating plating defects, first, the physical properties of the surfaces of the metal base layers 105, 109 are measured. Then, based on the measured physical properties of the surfaces of the metal base layers 105, 109, the occurrence degree of spikes caused by plating on the metal base layers 105, 109 is estimated. After that, the estimated occurrence degree of spikes is compared with a standard to determine the amount of spikes.

[0073] If the determination step S30 estimates that the occurrence of spikes is low, the plating layers 104, 112 are formed under the default conditions. On the other hand, if the determination step S30 estimates that the occurrence of spikes is high, the formation of the plating layers 104, 112 under the default conditions is stopped. Alternatively, before the plating pretreatment step S130 under the default conditions, the plating pretreatment step S130 may be performed with different contents, such as performing a resurface treatment such as a heat treatment on the surface of the metal base layer 105, 109, as an additional pretreatment step, and the plating layers 104, 112 may be formed through the plating step S140.

[0074] The plating layer 104 on the cathode side and the plating layer 112 on the anode side may be formed by either electrolytic plating or electroless plating, but is preferably formed by electroless plating. By using electroless plating, plating layers with good thickness symmetry can be formed on the cathode side and the anode side. Good thickness symmetry can reduce warping of the semiconductor element 150 due to stress generated in the plating layer and thermal warping during soldering to connect wiring. This can improve the manufacturability of the semiconductor device 100.

[0075] The thickness of the plating layers 104, 112 is preferably 1 μm or more and 10 μm or less from the viewpoint of preventing melting of the metal base layers 105, 109 during soldering such as wire bonding, etc. However, the thickness of the plating layers 104, 112 may be increased to a thickness exceeding 10 μm.

[0076] When the plating layers 104, 112 are to be thickened, layers made of copper may be laminated to form a multi-layer structure. When layers made of copper are laminated, it is preferable to form a copper diffusion prevention layer between the copper layer and the semiconductor substrate 108, similar to the copper diffusion prevention layer 106, in order to prevent thermally diffused copper from penetrating into the semiconductor substrate 108.

[0077] In Fig. 4C, the plating layer is formed on both the cathode side and the anode side, but it may be formed only on the cathode side or only on the anode side. When the plating layer is formed only on one side, plating can be performed with a surface protection tape attached to the side not to be formed. The surfaces of the plating layers 104, 112 can be further plated with gold or the like.

[0078] The semiconductor device 100 can be mounted on a power module, which is a main component of a power converter such as an inverter. The power module can be used for various purposes such as a driving power source for hybrid cars, electric cars, trains, ships, etc., a power storage system for natural energy power generation such as solar power generation, wind power generation, and geothermal power generation, a stationary power storage system, and a power conditioner for an uninterruptible power supply system.

[0079] FIG. 5 is a flow chart showing the electroless plating process. 5, the electroless plating process includes a degreasing and cleaning step S131, an etching step S132, a first pickling step S133, a first zincating step S134, a second pickling step S135, a second zincating step S136, and an electroless plating step S141. The electroless plating step S141 includes a step of performing Ni-P electroless plating.

[0080] The degreasing and cleaning process S131, the etching process S132, the first pickling process S133, the first zincating process S134, the second pickling process S135, and the second zincating process S136 constitute a plating pretreatment process S130. Note that one or more of these processes may be omitted.

[0081] In the degreasing and cleaning step S131, the surface of the base layer is cleaned with an alkaline degreasing agent to remove oil adhering to the surface of the base layer. As the alkaline degreasing agent, for example, a solution containing an alkali such as sodium hydroxide or a surfactant is used.

[0082] In the etching step S132, the surface of the underlayer is etched with, for example, a strong alkaline solution to remove the oxide film on the surface of the underlayer. As the strong alkaline solution, for example, a solution containing an alkali such as sodium hydroxide, a surfactant, a complexing agent, etc. is used.

[0083] In the first pickling process S133, the surface of the underlayer is washed with an acid solution to remove impurities such as aluminum hydroxide (Al(OH)3) that are generated by removing the oxide film. As the acid solution, a solution containing sulfuric acid, nitric acid, hydrofluoric acid, etc. is used.

[0084] In the first zincating process S134, the surface of the underlayer is immersed in a zincate solution to deposit zinc on the surface of the underlayer. When zinc is deposited, the zinc is replaced with nickel during plating, so that a highly uniform plating film can be formed. As the zincate solution, for example, a solution containing zinc oxide, sodium hydroxide, iron chloride, etc. is used.

[0085] In the second pickling process S135, the surface of the undercoat layer is washed with an acid solution to remove a part of the zinc precipitated on the surface of the undercoat layer. By removing a part of the precipitated zinc, a more uniform and dense zinc film can be formed during the second zincating. As the acid solution, a solution containing nitric acid or the like is used.

[0086] In the second zincating step S136, the surface of the undercoat layer from which part of the precipitated zinc has been removed is immersed in a zincating solution to precipitate zinc on the surface of the undercoat layer. If zinc is precipitated again after part of the precipitated zinc has been removed, the zinc coating becomes uniform and dense, so that the uniformity and density of the plating metal substituted by zinc also increases. The second zincating can be performed using the same zincating solution, treatment time, and treatment temperature as the first zincating, but may also be a treatment shorter than the first zincating.

[0087] In the electroless plating process shown in FIG. 5, a double zincate treatment is performed. The metal underlayer 105 on the cathode side and the metal underlayer 109 on the anode side are made of aluminum or an aluminum alloy, and therefore an oxide film is easily formed on the surface. However, when the double zincate treatment is performed, the oxide film on the surface is removed, and a plating film with high uniformity and density is formed. Therefore, the adhesion between the metal underlayers 105, 109 and the plating layers 104, 112 can be improved.

[0088] In the electroless plating step S141, a plating layer is formed on the surface of the underlayer. As the plating solution, for example, a solution containing nickel salt such as nickel sulfate, hypophosphite such as sodium hypophosphite, a surfactant, a complexing agent, etc. The thickness of the plating layer 104 on the cathode side and the plating layer 112 on the anode side can be, for example, about 3 μm.

[0089] In electroless nickel-phosphorus plating, the oxidation-reduction reactions represented by the following formulas (1) and (2) occur. The reducing agent, hypophosphite, is oxidized to phosphite and releases electrons. Nickel ions are reduced to metallic nickel, and nickel containing phosphorus is deposited as a plating film. H2PO2 - +H2O → H2PO3 - + 2H + + 2e - (1) Ni 2+ + 2e - → Ni (2)

[0090] The plating solutions used in electroless nickel-phosphorus plating include low-phosphorus concentration types with a phosphorus content of about 1 to 4%, medium-phosphorus concentration types with a phosphorus content of about 5 to 11%, and high-phosphorus concentration types with a phosphorus content of over 12%. Depending on the phosphorus content, various plating films with different solder wettability, corrosion resistance, etc. can be obtained.

[0091] For example, a low phosphorus concentration electroless nickel plating solution "TOP UBP NICORON MLP" (manufactured by Okuno Chemical Industries Co., Ltd.) can be used as a plating solution for forming the plating layer 104 on the cathode side and the plating layer 112 on the anode side. However, for forming these plating layers 104, 112, any of low phosphorus concentration types, medium phosphorus concentration types, and high phosphorus concentration types may be used depending on the required plating film characteristics, etc.

[0092] Next, the results of an investigation into the relationship between the surface properties of the undercoat layer and the incidence of spikes will be described with reference to the drawings.

[0093] In the plating pretreatment process S130, the surface of the base layer formed of metal is corroded by an alkaline solution, an acid solution, a zincate solution, or the like. In particular, in the 1st zincate process S14 and the 2nd zincate process S136, a strongly alkaline zincate solution is used, so that pitting corrosion is likely to occur on the surface of the base layer. When the plating metal precipitates in the pit-like holes, spikes are formed. When spikes occur, there is a risk that the adhesion of the plating film will decrease or an electrical short circuit will occur.

[0094] In order to clarify the relationship between the physical properties of the surface of the underlayer formed of a metal and the occurrence rate of spikes, the inventors created semiconductor wafers with different conditions of the surface of the underlayer, and after applying low-phosphorus concentration electroless nickel-phosphorus plating to these semiconductor wafers, evaluated the occurrence rate of spikes formed of nickel-phosphorus alloy.

[0095] The underlayer was formed of an aluminum-silicon alloy by sputtering. Argon gas was used as the carrier gas. As test materials, several types of underlayers with different surface conditions were created by changing the flow rate of the carrier gas in the chamber and the deposition rate among the sputtering conditions. The deposition rate was adjusted by adjusting the energy of the magnetron that generates the electromagnetic field.

[0096] The smaller the flow rate of the carrier gas, the longer the mean free path of the sputtered metal, and the larger the particle size of the metal film formed. Also, the higher the film formation rate, the higher the kinetic energy of the sputtered metal, and the larger the particle size of the metal film formed. If the particle size of the metal forming the underlayer is large, local corrosion is less likely to progress, and resistance to pitting corrosion is increased. Therefore, it is considered that the smaller the flow rate of the carrier gas and the higher the film formation rate, the less likely spikes will occur.

[0097] Since there is a correlation between the particle size of a metal and the reflectance, brightness, and crystallite size of the metal surface, it was predicted that the degree of spike generation could be estimated by measuring the physical properties of the surface of the underlayer. Therefore, various semiconductor wafers with different physical properties of the surface of the underlayer were produced, and the physical properties of the surface of the underlayer were measured for these test materials, and the degree of spike generation was evaluated to verify the validity of the estimation of the degree of spike generation.

[0098] The occurrence of spikes was evaluated by observing the cross section of the plated underlayer. Cross-sectional samples were prepared by cutting a semiconductor wafer on which a underlayer was formed along a diameter line passing through the center, embedding the wafer in resin, and polishing and ion milling the cut surface. The cross sections of the test materials were observed with a scanning electron microscope (SEM) (Hitachi High-Tech, S-4300 or SU8030).

[0099] The incidence of spikes was determined by observing the interface between the undercoat layer and the plating layer on an SEM image, and calculating the number of spikes that intersect per 1 μm of imaginary line length along the interface. The physical properties of the undercoat layer surface were measured by optical measurement or X-ray diffraction measurement. In the optical measurement, the brightness or reflectance of the undercoat layer surface was determined. In the X-ray diffraction measurement, the crystallite size of the undercoat layer surface was determined.

[0100] <Measurement of the surface brightness of the base layer> The surface brightness of the undercoat layer was measured using a spectrophotometer (Konica Minolta, CM-2600d). A xenon lamp was used as the light source. The observation light source was standard light source D65. The measurement positions were on a diameter line passing through the center of the orientation flat of the semiconductor wafer, and nine points were equally spaced from the top to the bottom, with the orientation flat at the bottom. Of these nine points, the surface result of the fifth point in the center was used.

[0101] Generally, there are two methods for measuring reflected light: the SCI (Specular Component Include) method, which includes specular reflected light, and the SCE (Specular Component Exclude) method, which excludes specular reflected light. The SCI method, which is generally used to manage the color of the material itself, was used to measure the lightness of the surface of the base layer. * a * b * Lightness in the color system (SCI-L * ) was sought.

[0102] FIG. 6 is a diagram showing the relationship between the measurement results of the lightness of the surface of the underlayer and the evaluation results of the occurrence rate of spikes. In FIG. 6, the vertical axis represents the number of spikes N per 1 μm of interface length between the undercoat layer and the plating layer [number / μm], and the horizontal axis represents the surface brightness L of the undercoat layer (SCI-L * ) is shown.

[0103] As shown in Figure 6, the higher the surface brightness of the base layer, the fewer the number of spikes per 1 μm length at the interface between the base layer and the plating layer. If the surface brightness of the base layer is measured before the plating pretreatment process, it can be said that the occurrence rate of spikes, which are plating defects, can be estimated from the correlation between the surface brightness of the base layer and the occurrence rate of spikes.

[0104] From the viewpoint of ensuring adhesion of the plating layer, the number of spikes per 1 μm at the interface between the underlayer and the plating layer is preferably 1 or less. Therefore, under these measurement conditions, the brightness of the surface of the underlayer is preferably 94 or more.

[0105] As the light source, in addition to a xenon lamp, a tungsten lamp, a deuterium discharge tube, a fluorescent lamp, a xenon flash lamp, a halogen lamp, a low-pressure mercury lamp, a laser excited plasma light source, a laser light source, a light emitting diode (LED), etc. can be used.

[0106] As the observation illuminant, in addition to standard illuminant D65, standard illuminant A, standard illuminant C, standard illuminant D50, standard illuminant F2, standard illuminant F6, standard illuminant F7, standard illuminant F8, standard illuminant F10, standard illuminant F11, standard illuminant F12, etc. can be used. As the measurement method, the SCE method may be used as long as a sufficiently high brightness can be ensured. As the color system, the CIE L * a * b * In addition to CIE L * c * h, Hunter Lab, CIE L * u * v * etc. can be used.

[0107] The measurement position may be any position on the surface of the underlayer. However, from the viewpoint of more reliably estimating the occurrence of spikes, a position where the surface has low brightness and where spikes are likely to occur is preferable. When estimating spikes in a semiconductor wafer having underlayers formed on both sides, the measurement position may be the surface of the semiconductor wafer or the back side of the semiconductor wafer.

[0108] In addition, when estimating spikes in a semiconductor wafer, the measurement position may be the surface of the underlayer in the center of the semiconductor wafer, or the surface of the underlayer in the peripheral portion of the semiconductor wafer. The center and peripheral portions of the semiconductor wafer may differ from each other in terms of the deposition conditions of the underlayer. Measuring the side where spikes are likely to occur increases the accuracy of estimating the degree of spike occurrence.

[0109] When estimating the spike occurrence rate of a target sample, the correlation between the surface brightness of the metal underlayer and the spike occurrence rate, i.e., the number of spikes per unit length or unit area of ​​the interface between the underlayer and the plating layer, is determined in advance using a reference test material. A semiconductor wafer with an underlayer of the same chemical composition is used as the reference test material. The correlation is determined individually depending on the light source, observation light source, measurement method, color system, measurement position, etc.

[0110] <Measurement of the reflectance of the surface of the base layer> The reflectance of the surface of the undercoat layer was measured using a spectrophotometer (Konica Minolta, CM-2600d). A xenon lamp was used as the light source. The observation light source was standard light source D65. The measurement positions were on a diameter line passing through the center of the orientation flat of the semiconductor wafer, and nine points were equally spaced from the top to the bottom, with the orientation flat at the bottom. Of these nine points, the result of the fifth point in the center was used.

[0111] The reflectance of the surface of the base layer was measured using the SCI method, which is generally used to manage the color of the material itself. Using the SCI method, the reflectance of reflected light with a wavelength of 600 nm was obtained. The reflectance of light from aluminum generally shows a positive correlation with the wavelength. A wavelength of 600 nm is a condition that produces a relatively high reflectance when using a normal light source.

[0112] FIG. 7 is a diagram showing the relationship between the measurement results of the reflectance of the surface of the underlayer and the evaluation results of the occurrence rate of spikes. In FIG. 7, the vertical axis represents the number of spikes N [number / μm] per 1 μm length of the interface between the underlayer and the plating layer, and the horizontal axis represents the reflectance R [%] of reflected light with a wavelength of 600 nm from the surface of the underlayer.

[0113] As shown in Figure 7, the higher the reflectivity of the base layer surface, the fewer the number of spikes per 1 μm length at the interface between the base layer and the plating layer. If the reflectivity of the metal base layer surface is measured before the plating pretreatment process, it can be said that the incidence of spikes, which are plating defects, can be estimated from the correlation between the reflectivity of the base layer surface and the incidence of spikes.

[0114] From the viewpoint of ensuring adhesion of the plating layer, the number of spikes per 1 μm at the interface between the underlayer and the plating layer is preferably 1 or less. Therefore, under these measurement conditions, the reflectance of the surface of the underlayer is preferably 86% or more.

[0115] As the light source, in addition to a xenon lamp, a tungsten lamp, a deuterium discharge tube, a fluorescent lamp, a xenon flash lamp, a halogen lamp, a low-pressure mercury lamp, a laser excited plasma light source, a laser light source, a light emitting diode (LED), etc. can be used.

[0116] As the observation light source, in addition to standard light source D65, standard light source A, standard light source C, standard light source D50, standard light source F2, standard light source F6, standard light source F7, standard light source F8, standard light source F10, standard light source F11, standard light source F12, etc. can be used.

[0117] The reflected light may have a wavelength of 600 nm or any other suitable wavelength that is not easily absorbed by the metal forming the undercoat layer. The reflected light may be in any wavelength range, such as the ultraviolet range, the visible light range, or the infrared range. The reflected light may be measured using a total reflectometer, a spectral reflectometer, or the like, in addition to a spectrophotometer.

[0118] The measurement position may be any position on the surface of the underlayer. However, from the viewpoint of more reliably estimating the occurrence of spikes, a position where the reflectance of the surface is low and where spikes are likely to occur is preferable. When estimating spikes in a semiconductor wafer having underlayers formed on both sides, the measurement position may be the surface of the semiconductor wafer or the back side of the semiconductor wafer.

[0119] In addition, when estimating spikes in a semiconductor wafer, the measurement position may be the surface of the underlayer in the center of the semiconductor wafer, or the surface of the underlayer in the peripheral portion of the semiconductor wafer. The center and peripheral portions of the semiconductor wafer may differ from each other in terms of the deposition conditions of the underlayer. Measuring the side where spikes are likely to occur increases the accuracy of estimating the degree of spike occurrence.

[0120] When estimating the occurrence rate of spikes in a target sample, the correlation between the reflectance of the surface of the metal underlayer and the occurrence rate of spikes, i.e., the number of spikes per unit length or unit area of ​​the interface between the underlayer and the plating layer, is determined in advance using a reference test material. A semiconductor wafer with an underlayer of the same chemical composition is used as the reference test material. The correlation is determined individually depending on the light source, observation light source, measurement method, measurement position, etc.

[0121] <Measurement of crystallite size on the surface of the undercoat layer> The crystallite diameter of the surface of the underlayer was measured using an X-ray diffraction (XRD) measuring device (Rigaku Corporation, RINT2500HL). In the measured X-ray diffraction spectrum, the peak with the highest diffraction intensity was a diffraction peak assigned to the (200) plane of aluminum. The full width at half maximum of this diffraction peak was used to determine the crystallite diameter of the surface of the underlayer.

[0122] The crystallite diameter on the surface of the underlayer was determined by the Scherrer method. The crystallite diameter D [nm] of the metal present on the surface of the underlayer satisfies the Scherrer formula represented by the following mathematical formula (I). D = K λ / β cosθ (I) In formula (I), K is a constant, λ is the wavelength of the X-ray [nm], β is the full width at half maximum [rad], and θ is the Bragg angle [rad].

[0123] FIG. 8 is a diagram showing the relationship between the measurement results of the crystallite size on the surface of the underlayer and the evaluation results of the incidence of spikes. In FIG. 8, the vertical axis represents the number of spikes N [number / μm] per 1 μm length of the interface between the underlayer and the plating layer, and the horizontal axis represents the aluminum crystallite diameter D [nm] on the surface of the underlayer.

[0124] As shown in Figure 8, the larger the crystallite diameter on the surface of the base layer, the fewer the number of spikes per 1 μm length at the interface between the base layer and the plating layer. If the crystallite diameter on the surface of the base layer is measured before the plating pretreatment process, it can be said that the occurrence of spikes, which are plating defects, can be estimated from the correlation between the crystallite diameter on the surface of the base layer and the occurrence of spikes.

[0125] From the viewpoint of ensuring the adhesion of the plating layer, the number of spikes per 1 μm of the interface between the underlayer and the plating layer is preferably 1 or less. Therefore, under these measurement conditions, the crystallite diameter on the surface of the underlayer is preferably 400 nm or more.

[0126] The crystallite diameter on the surface of the underlayer may be determined by the Hall method. The crystallite diameter D [nm] of the metal present on the surface of the underlayer satisfies the Williamson-Hall formula represented by the following mathematical formula (II). β·cosθ / λ=2ε·sinθ / λ+K·D···(II) In the formula (II), K is a constant, λ is the wavelength of the X-ray [nm], β is the full width at half maximum [rad], θ is the Bragg angle [rad], and ε is the lattice distortion.

[0127] As the diffraction line of aluminum, in addition to the (200) plane, a diffraction line from a diffraction plane with appropriate Miller indices such as the (220) plane can be used as long as an appropriate diffraction peak is obtained. If the underlayer is formed of a material other than aluminum, a diffraction line according to the metal forming the underlayer can be used. However, from the viewpoint of more reliably estimating the occurrence of spikes, it is preferable to use a diffraction line with high diffraction intensity.

[0128] The measurement position may be any position on the surface of the underlayer. However, from the viewpoint of more reliably estimating the occurrence of spikes, it is preferable to use a position on the surface where the crystallite diameter is small and where spikes are likely to occur. When estimating spikes in a semiconductor wafer having underlayers formed on both sides, the measurement position may be the surface of the semiconductor wafer or the back side of the semiconductor wafer.

[0129] In addition, when estimating spikes in a semiconductor wafer, the measurement position may be the surface of the underlayer in the center of the semiconductor wafer, or the surface of the underlayer in the peripheral portion of the semiconductor wafer. The center and peripheral portions of the semiconductor wafer may differ from each other in terms of the deposition conditions of the underlayer. Measuring the side where spikes are likely to occur increases the accuracy of estimating the degree of spike occurrence.

[0130] When estimating the occurrence rate of spikes in a target sample, the correlation between the crystallite diameter on the surface of the underlayer and the occurrence rate of spikes, i.e., the number of spikes per unit length or unit area of ​​the interface between the underlayer and the plating layer, is determined in advance using a reference test material. As the reference test material, a semiconductor wafer on which an underlayer with the same chemical composition is formed is used. The correlation is determined individually depending on the type of diffraction line, the calculation method, the measurement position, etc.

[0131] As shown in Figures 6, 7 and 8, the physical properties of the surface of the undercoat were measured, and it was confirmed that the degree of spike occurrence correlates with the reflectance of the metal surface, the brightness of the metal surface, and the crystallite size of the metal surface. It was confirmed that when the reflectance of the metal surface, the brightness of the metal surface, or the crystallite size of the metal surface are measured for a plated material with an unknown degree of spike occurrence, the degree of spike occurrence can be estimated by applying the results to the correlation obtained using a plated material with a known degree of spike occurrence.

[0132] The plating defect estimation method according to the present embodiment can be widely applied to various plating defects. As long as the correlation between the surface properties of the underlayer and the occurrence rate of plating defects can be utilized, it is possible to estimate plating defects caused by erosion, crevice corrosion, etc., in addition to the spike phenomenon in which the plating film penetrates into the surface of the underlayer in the form of a protrusion, needle, etc.

[0133] According to the plating defect estimation method and semiconductor device manufacturing method of the present embodiment, the occurrence rate of spikes caused by plating can be estimated from the physical properties of the surface of the substrate before the plating film is formed. The occurrence rate of spikes can be estimated based on non-destructive measurements. Since it is possible to plate only the plated material that is estimated to have few spikes, it is possible to provide a highly reliable semiconductor device and a manufacturing method thereof. Since the product yield can be improved, semiconductor devices and the like can be provided at low cost. In addition, since the adhesion of the plating film is less likely to decrease and electrical short circuits through the substrate layer are less likely to occur, it is possible to reduce the size and improve the reliability of power conversion devices equipped with semiconductor devices.

[0134] Although the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the present invention. For example, the present invention is not necessarily limited to those having all the configurations of the above-described embodiment. It is possible to replace a part of the configuration of a certain embodiment with another configuration, add a part of the configuration of a certain embodiment to another form, or omit a part of the configuration of a certain embodiment. [Explanation of symbols]

[0135] 90 Silicon Wafers 100 Semiconductor device 101 Insulating substrate 102 Conductive material 103 Bonding layer 104 Plating layer 105 Metal base layer 106 Copper diffusion prevention layer 107 Metal layer 108 Semiconductor Substrate 108a p-type semiconductor layer 108b n-type drift layer 108c n+ type drift layer 109 Metal base layer 110 Oxide film 111 Resin layer 112 Plating layer 113 Cathode Electrode 114 Anode Electrode 150 Semiconductor elements

Claims

1. a measuring step of measuring physical properties of a surface of the underlayer prior to a plating pretreatment step of subjecting the underlayer to a plating pretreatment; and an estimation step of estimating the occurrence rate of spikes caused on the underlayer by plating based on the measured physical properties.

2. The plating defect estimation method according to claim 1, The plating defect estimating method, wherein the measuring step is a step of optically measuring the surface of the base layer.

3. The plating defect estimation method according to claim 2, A plating defect estimation method for estimating that the occurrence rate of the spikes is low when the reflectance of the surface of the base layer is equal to or higher than a threshold value.

4. The plating defect estimation method according to claim 2, The plating defect estimation method estimates that the occurrence rate of the spikes is low when the brightness of the surface of the base layer is equal to or higher than a threshold value.

5. The plating defect estimation method according to claim 1, The plating defect estimating method, wherein the measuring step is a step of subjecting the surface of the base layer to X-ray diffraction measurement.

6. The plating defect estimation method according to claim 5, A plating defect estimation method for estimating that the occurrence rate of the spikes is low when the crystallite diameter on the surface of the underlayer is equal to or greater than a threshold value.

7. The plating defect estimation method according to claim 1, The plating defect estimation method, wherein the underlayer is formed of aluminum or an aluminum alloy.

8. The plating defect estimation method according to claim 1, The plating defect estimating method, wherein the plating is nickel plating or nickel alloy plating.

9. a base layer forming step of forming a base layer on a semiconductor wafer; a plating pretreatment step of subjecting the underlayer to a plating pretreatment; a plating step of plating the pretreated underlayer; a measuring step of measuring physical properties of a surface of the underlayer prior to the plating pretreatment step; and estimating a degree of occurrence of spikes caused on the underlayer by plating based on the measured physical properties.

10. 10. The method of manufacturing a semiconductor device according to claim 9, The method for manufacturing a semiconductor device, wherein the measuring step is a step of measuring physical properties of the surface of the underlayer at the center of the semiconductor wafer.

11. 10. The method of manufacturing a semiconductor device according to claim 9, The method for manufacturing a semiconductor device, wherein the measuring step is a step of measuring physical properties of the surface of the underlayer in the peripheral portion of the semiconductor wafer.

12. 10. The method of manufacturing a semiconductor device according to claim 9, When the occurrence rate of the spike estimated in the estimation step is greater than a predetermined threshold value, the plating pretreatment step and the plating step are stopped.

13. 10. The method of manufacturing a semiconductor device according to claim 9, The method for manufacturing a semiconductor device includes changing the content of the plating pretreatment step depending on whether the occurrence rate of the spikes estimated in the estimation step is higher or lower than a predetermined threshold value.

Citation Information

Patent Citations

  • Black bright material and production method therefor

    JP2002363771A

  • Substrate processing method and apparatus

    JP2005015885A

  • Wear-resistant member and motive-power transmitting component

    JP2007023316A

  • Solution for processing of metal replacement with aluminum or aluminum alloy and method for surface processing using such solution

    JP2009127101A

  • Semiconductor device and method for manufacturing semiconductor device

    JP2019145667A