Manufacturing method of piezoelectric laminate
The piezoelectric laminate with KNN and AlN films addresses the performance limitations of ultrasonic sensors by enabling deep penetration and high resolution through a non-overlapping, MEMS-manufactured design, simplifying production and integration.
Patent Information
- Application Number
- JP2020068252
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-06
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-04-06
AI Technical Summary
Existing ultrasonic sensors face challenges in achieving high performance with deep ultrasonic penetration and high resolution due to limitations in piezoelectric materials, leading to complex manufacturing processes and limited integration capabilities.
A piezoelectric laminate structure is designed with an output side piezoelectric film made of potassium sodium niobate (KNN) oxide and an input side film made of aluminum nitride (AlN) nitride, arranged to not overlap, allowing independent operation and optimized for deep penetration and high sensitivity, manufactured using MEMS processes.
The laminate structure enables a high-performance ultrasonic sensor with deep penetration and high resolution, simplifying the manufacturing process and enhancing integration, while minimizing interference between output and input sections.
Smart Images

Figure 0007568417000001 
Figure 0007568417000002 
Figure 0007568417000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element. [Background technology]
[0002] Piezoelectric bodies are sometimes used in ultrasonic sensors such as p-MUTs (Piezoelectric Micromachined Ultrasonic Transducers). Ferroelectrics such as lead zirconate titanate (PZT) are widely used as materials for piezoelectric bodies (see, for example, Patent Document 1). In addition, potassium sodium niobate (KNN) ferroelectrics or aluminum nitride (AlN) are sometimes used as piezoelectric materials for ultrasonic sensors (see, for example, Patent Document 2). In recent years, there has been a demand for ultrasonic sensors having piezoelectric bodies with higher performance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-146020 A [Patent Document 2] JP 2019-165307 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a piezoelectric laminate or the like that can provide a high-performance ultrasonic sensor. [Means for solving the problem]
[0005] According to one aspect of the present invention, A substrate; an output-side lower electrode film provided on the substrate; an output-side piezoelectric film that is an oxide film and is provided on the output-side lower electrode film; an output-side upper electrode film provided on the output-side piezoelectric film; an input side lower electrode film provided on the substrate; an input-side piezoelectric film that is a nitride film and is provided on the input-side lower electrode film; an input-side upper electrode film provided on the input-side piezoelectric film, A piezoelectric laminate, a piezoelectric element, and an ultrasonic sensor are provided in which an ultrasonic output section constituted by a laminated section having the output side lower electrode film, the output side piezoelectric film, and the output side upper electrode film, and an ultrasonic input section constituted by a laminated section having the input side lower electrode film, the input side piezoelectric film, and the input side upper electrode film are arranged so as not to overlap each other when viewed from above the substrate.
[0006] According to another aspect of the present invention, forming an output-side lower electrode film and an input-side lower electrode film on a substrate; forming an output-side piezoelectric film, which is an oxide film, on the output-side lower electrode film; forming a protective film for protecting the output-side piezoelectric film; forming an input-side piezoelectric film, which is a nitride film, on the input-side lower electrode film; removing the protective film by etching to expose the output-side piezoelectric film; forming an output-side upper electrode film on the output-side piezoelectric film, and forming an input-side upper electrode film on the input-side piezoelectric film, A method for manufacturing a piezoelectric laminate is provided, which includes a step of producing a laminate in which an ultrasonic output section constituted by a laminate portion having the output side lower electrode film, the output side piezoelectric film, and the output side upper electrode film, and an ultrasonic input section constituted by a laminate portion having the input side lower electrode film, the input side piezoelectric film, and the input side upper electrode film are arranged so as not to overlap each other when viewed from the top of the substrate. Effect of the Invention
[0007] According to the present invention, it is possible to obtain a piezoelectric laminate and a piezoelectric element that can provide a high-performance ultrasonic sensor. [Brief description of the drawings]
[0008] [Figure 1] 1 is a diagram showing an example of a cross-sectional structure of a piezoelectric laminate according to an embodiment of the present invention. [Diagram 2] 11A and 11B are diagrams showing modified examples of the cross-sectional structure of the piezoelectric laminate according to one embodiment of the present invention. [Diagram 3] 1 is a diagram showing an example of a schematic configuration of an ultrasonic sensor according to an embodiment of the present invention; [Figure 4] 1A is a diagram showing an example of the cross-sectional structure of the laminate 10a before the output side piezoelectric film is formed, (b) is a diagram showing an example of the cross-sectional structure of the laminate 10b after the output side piezoelectric film is formed, (c) is a diagram showing an example of the cross-sectional structure of the laminate 10c after the output side piezoelectric film is formed into a predetermined shape, (d) is a diagram showing an example of the cross-sectional structure of the laminate 10d after a protective film is formed, (e) is a diagram showing an example of the cross-sectional structure of the laminate 10e after the input side piezoelectric film is formed, and (f) is a diagram showing an example of the cross-sectional structure of the laminate 10f after the protective film is removed. [Diagram 5] FIG. 13 is a diagram showing a cross-sectional structure of a piezoelectric laminate according to a modified example of an embodiment of the present invention. [Figure 6] 1A is a diagram showing an example of the cross-sectional structure of the laminate 40a before the output side piezoelectric film is formed, (b) is a diagram showing an example of the cross-sectional structure of the laminate 40b after the output side piezoelectric film has been formed and molded into a specified shape, (c) is a diagram showing an example of the cross-sectional structure of the laminate 40c after a protective film has been formed, (d) is a diagram showing an example of the cross-sectional structure of the laminate 40d after the input side lower electrode film has been formed, (e) is a diagram showing an example of the cross-sectional structure of the laminate 40e after the input side piezoelectric film has been formed, and (f) is a diagram showing an example of the cross-sectional structure of the laminate 40f after the protective film has been removed. [Figure 7] FIG. 13 is a diagram showing a cross-sectional structure of a piezoelectric laminate according to a modified example of an embodiment of the present invention. [Figure 8] FIG. 13 is a diagram showing a cross-sectional structure of a piezoelectric laminate according to a modified example of an embodiment of the present invention. [Figure 9]1A is a diagram showing an example of the cross-sectional structure of laminate 42a before the output side piezoelectric film is formed, (b) is a diagram showing an example of the cross-sectional structure of laminate 42b after the output side piezoelectric film is formed, (c) is a diagram showing an example of the cross-sectional structure of laminate 42c after the protective film is formed, (d) is a diagram showing an example of the cross-sectional structure of laminate 42d after the input side piezoelectric film is formed, and (e) is a diagram showing an example of the cross-sectional structure of laminate 42e after the protective film is removed. [Figure 10] FIG. 13 is a diagram showing a cross-sectional structure of a piezoelectric laminate according to a modified example of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <One embodiment of the present invention> Hereinafter, one embodiment of the present invention will be described with reference to FIGS.
[0010] (1) Structure of the piezoelectric laminate 1, a laminate (laminate substrate) 10 having a piezoelectric film according to this embodiment (hereinafter also referred to as piezoelectric laminate 10) is configured to include a substrate 1, a lower electrode film 2 provided (deposited) on the substrate 1, an output side piezoelectric film 3A provided (deposited) on the lower electrode film 2, an output side upper electrode film 4A provided (deposited) on the output side piezoelectric film 3A, an input side piezoelectric film 3B provided (deposited) on the lower electrode film 2, and an input side upper electrode film 4B provided (deposited) on the input side piezoelectric film 3B. In this embodiment, the lower electrode film 2 functions as the output side lower electrode film 2A and also as the input side lower electrode film 2B.
[0011] The substrate 1 is a substrate having a surface oxide film (SiO 2 A single crystal silicon (Si) substrate 1a on which a surface oxide film 1b is formed, that is, a Si substrate having a surface oxide film, can be preferably used. 2Alternatively, a Si substrate 1a having an insulating film 1d formed of an insulating material other than SiO 2 can be used. Alternatively, a Si substrate 1a having an exposed Si(100) surface or Si(111) surface, i.e., a Si substrate having no surface oxide film 1b or insulating film 1d can be used. Alternatively, a silicon on insulator (SOI) substrate, quartz glass (SiO 2 ) substrate, gallium arsenide (GaAs) substrate, sapphire (Al 2 O 3 Alternatively, a metal substrate made of a metal material such as a silicon substrate (Si substrate) or stainless steel (SUS) may be used. The thickness of the single crystal Si substrate 1a may be, for example, 300 μm or more and 1000 μm or less, and the thickness of the surface oxide film 1b may be, for example, 1 nm or more and 4000 nm or less.
[0012] The lower electrode film 2 can be formed by using, for example, platinum (Pt). The lower electrode film 2 is a single crystal film or a polycrystalline film (hereinafter, these are also referred to as Pt film). It is preferable that the crystals constituting the Pt film are preferentially oriented in the (111) plane direction with respect to the surface of the substrate 1. In other words, it is preferable that the surface of the lower electrode film (Pt film) 2 (the surface serving as the base of the output-side piezoelectric film 3A) is mainly composed of the Pt (111) plane. The Pt film can be formed by using a method such as sputtering or vapor deposition. The lower electrode film 2 can be formed by using various metals other than Pt, such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys mainly composed of these metals, strontium ruthenate (SrRuO 3 , abbreviation: SRO) or lanthanum nickel oxide (LaNiO 3 Alternatively, the lower electrode film 2 may be a single layer film formed using the above-mentioned metals or metal oxides, or may be a laminate of a Pt film and a film made of LNO provided on the Pt film, or a laminate of a Pt film and a film made of SRO provided on the Pt film. The thickness of the lower electrode film 2 may be, for example, 100 nm to 400 nm.
[0013] Between the substrate 1 and the lower electrode film 2, for example, titanium (Ti), tantalum (Ta), titanium oxide (TiO 2 ), nickel (Ni), ruthenium oxide (RuO 2 ), iridium oxide (IrO 2 An adhesive layer 6 mainly composed of, for example, ZnO, Cr, or the like may be provided. The adhesive layer 6 can be formed by a method such as sputtering or vapor deposition. The thickness of the adhesive layer 6 can be, for example, 1 nm or more and 200 nm or less.
[0014] The output side piezoelectric film 3A is composed of a film containing oxygen (O) and not nitrogen (N), that is, an oxide film. The term "film not containing N" as used herein includes a film containing no N at all, as well as a film containing a small amount of N as an unavoidable impurity. The output side piezoelectric film 3A is preferably a film having a high piezoelectric constant. This allows the output side piezoelectric film 3A to be greatly deformed when a predetermined voltage is applied by the voltage application unit 11a described below, and allows the output side vibration unit described below to be greatly vibrated. As a result, it is possible to increase the intensity of the ultrasonic waves transmitted from the ultrasonic output unit described below, and to deepen the vibration depth (depth) of the ultrasonic waves with respect to the test object. The piezoelectric constant of the output side piezoelectric film 3A can be, for example, 100 pm / V or more, preferably 170 pm / V or more. The upper limit of the piezoelectric constant of the output side piezoelectric film 3A is not particularly limited, but with current technology, the upper limit is about 200 pm / V. In addition, it is preferable that the output side piezoelectric film 3A has a higher piezoelectric constant than the input side piezoelectric film 3B.
[0015] The output-side piezoelectric film 3A is, for example, potassium sodium niobate (KNN), that is, contains potassium (K), sodium (Na), and niobium (Nb) and has a composition formula (K 1-x Na x ) y NbO 3A film can be formed using the alkali niobium oxide represented by the following. The coefficient x [= Na / (K + Na)] in the above composition formula should be in the range of 0 < x < 1. Preferably, the coefficient x in the above composition formula is in the range of 0 < x < 1, and the coefficient y [= (K + Na) / Nb] is in the range of 0.7 ≦ y ≦ 1.50. The output-side piezoelectric film 3A is a polycrystalline film of KNN (hereinafter also referred to as the KNN film 3A). The crystal structure of KNN is a perovskite structure. The KNN film 3A can be formed using techniques such as sputtering, PLD (Pulsed Laser Deposition), and sol-gel methods. The thickness of the KNN film 3A can be, for example, 0.5 μm or more and 5 μm or less.
[0016] The crystals constituting the KNN film 3A are preferably preferentially oriented in the (001) plane orientation with respect to the surface of the substrate 1 (when the substrate 1 is, for example, an Si substrate 1a having a surface oxide film 1b or an insulating film 1d, etc., it is the surface of the Si substrate 1a, and the same applies hereinafter). That is, the surface of the KNN film 3A (the surface that serves as the base for the output-side upper electrode film 4A) is preferably mainly composed of the KNN (001) plane orientation. By directly forming the KNN film 3A on a Pt film preferentially oriented in the (111) plane orientation with respect to the surface of the substrate 1, it becomes easy to preferentially orient the crystals constituting the KNN film 3A in the (001) plane orientation with respect to the surface of the substrate 1. For example, it becomes easy to orient 80% or more of the crystals in the crystal group constituting the KNN film 3A in the (001) plane orientation with respect to the surface of the substrate 1, and to make 80% or more of the region of the surface of the KNN film 3A the KNN (001) plane.
[0017] Preferably, more than half of the crystals in the crystal group constituting the KNN film 3A have a columnar structure. Also, the boundaries between the crystals constituting the KNN film 3A, that is, the grain boundaries present in the KNN film 3A, preferably penetrate in the thickness direction of the KNN film 3A. For example, in the KNN film 3A, it is preferable that the grain boundaries penetrating in the thickness direction are more numerous than the grain boundaries that do not penetrate in the thickness direction of the KNN film 3A (for example, the grain boundaries parallel to the plane direction of the substrate 1).
[0018] The KNN film 3A preferably contains at least one metal element (hereinafter simply referred to as "metal element") selected from the group consisting of copper (Cu), manganese (Mn), iron (Fe), and vanadium (V). The KNN film 3A more preferably contains at least one of Cu and Mn. "Containing at least one of Cu and Mn" may mean that only Cu is contained, only Mn is contained, or both Cu and Mn are contained.
[0019] The KNN film 3A preferably contains the above metal elements at a concentration within a range of, for example, 0.2 at% to 2.0 at% relative to the amount of niobium (Nb) in the KNN film 3A. That is, the concentration of the above metal elements in the KNN film 3A is preferably, for example, 0.2 at% to 2.0 at%. Note that when the KNN film 3A contains multiple types of metal elements from among Cu, Mn, Fe, and V, the concentration of the metal elements is the total concentration of the multiple types of metal elements.
[0020] By setting the concentration of the metal element in the KNN film 3A to 0.2 at % or more, it is possible to improve the insulating property (leak resistance) of the KNN film 3A while improving the resistance (etching resistance) to a fluorine-based etching solution. By improving the insulating property of the KNN film 3A, it becomes possible to apply a higher voltage by the voltage application unit 11a described below. As a result, it becomes possible to increase the amount of deformation of the KNN film 3A. By improving the etching resistance of the KNN film 3A, that is, by making the KNN film 3A less susceptible to etching, it is possible to suppress a decrease in the piezoelectric performance and quality of the KNN film 3A during the manufacturing process of the piezoelectric stack 10.
[0021] By making the concentration of metal elements in the KNN film 3A 2.0 at % or less, the relative dielectric constant of the KNN film 3A can be made suitable for applications such as an ultrasonic wave generating vibrator, and as described later, it becomes possible to suppress an increase in power consumption when the KNN film 3A is applied to an ultrasonic wave generating vibrator.
[0022] The KNN film 3A may contain secondary components other than K, Na, Nb, and the above metal elements within a range that does not impair the effects obtained by adding the above metal elements within a predetermined range, for example, within a range of 5 at% or less (when multiple types of secondary components are included, the total concentration of the secondary components is within a range of 5 at% or less). Examples of secondary components include lithium (Li), Ta, and antimony (Sb).
[0023] The output-side upper electrode film 4A (hereinafter also referred to as the upper electrode film 4A) can be formed using various metals such as Pt, Au, aluminum (Al), Cu, etc., or alloys thereof. The upper electrode film 4A can be formed using techniques such as sputtering, vapor deposition, plating, metal paste, etc. The upper electrode film 4A does not have a significant effect on the crystal structure of the KNN film 3A, unlike the lower electrode film 2A. Therefore, the material, crystal structure, and film formation technique of the upper electrode film 4A are not particularly limited. Note that, in order to increase the adhesion between the KNN film 3A and the upper electrode film 4A, for example, Ti, Ta, TiO 2 , Ni, RuO 2 , IrO 2 The thickness of the upper electrode film 4A may be, for example, 10 nm or more and 5000 nm or less, and when an adhesive layer is provided, the thickness of the adhesive layer may be, for example, 1 nm or more and 200 nm or less.
[0024] The input side piezoelectric film 3B is composed of a film containing nitrogen (N) and not oxygen (O), that is, a nitride film. In addition, the term "film not containing O" as used herein includes a film containing no O at all, as well as a film containing a small amount of O as an unavoidable impurity. The input side piezoelectric film 3B is preferably a film with a low relative dielectric constant. This makes it possible to increase the reception sensitivity of ultrasonic waves. Specifically, even if the vibration of the input side vibration part described below is small, it is possible to deform the input side piezoelectric film 3B and generate a voltage by the deformation. The relative dielectric constant of the input side piezoelectric film 3B can be, for example, 25 or less, preferably 15 or less. The lower limit of the relative dielectric constant of the input side piezoelectric film 3B is not particularly limited, but with current technology, the lower limit is about 8. In addition, the input side piezoelectric film 3B preferably has a lower relative dielectric constant than the output side piezoelectric film 3A.
[0025] The input side piezoelectric film 3B can be formed, for example, using a nitride containing aluminum (Al), that is, aluminum nitride (AlN). The input side piezoelectric film 3B is an AlN polycrystalline film (hereinafter also referred to as AlN film 3B). The AlN film 3B can be formed using a method such as a sputtering method, a PLD (Pulsed Laser Deposition) method, a MOCVD (Metal Organic Chemical Vapor Deposition) method, or a HVPE (Hydride Vapor Phase Epitaxy) method. The thickness of the AlN film 3B can be, for example, 0.3 μm or more and 5 μm or less. It is preferable that the thickness of the AlN film 3B is as thick as possible within the above range, which makes it possible to increase the reception sensitivity of ultrasonic waves.
[0026] The crystals constituting the AlN film 3B are preferably preferentially oriented in the (001) plane with respect to the surface of the substrate 1. That is, the surface of the AlN film 3B (the surface serving as the base of the input-side upper electrode film 4B) is preferably mainly composed of the AlN (001) plane. By directly depositing the AlN film 3B on the lower electrode film 2B preferentially oriented in the (111) plane with respect to the surface of the substrate 1, it becomes easy to preferentially orient the crystals constituting the AlN film 3B in the (001) plane with respect to the surface of the substrate 1. For example, it becomes easy to orient 80% or more of the crystals constituting the AlN film 3B in the (001) plane with respect to the surface of the substrate 1, and to make 80% or more of the surface of the AlN film 3B the AlN (001) plane.
[0027] It is preferable that more than half of the crystals in the crystal group constituting the AlN film 3B have a columnar structure. Also, it is preferable that the boundaries between the crystals constituting the AlN film 3B, i.e., the crystal grain boundaries present in the AlN film 3B, run through the AlN film 3B in the thickness direction. For example, it is preferable that the number of crystal grain boundaries running through the thickness direction of the AlN film 3B is greater than the number of crystal grain boundaries that do not run through the AlN film 3B in the thickness direction (for example, crystal grain boundaries parallel to the plane direction of the substrate 1).
[0028] The AlN film 3B may be an AlN film containing scandium (Sc) (Sc-AlN film), an AlN film containing magnesium (Mg) and zirconium (Zr) (MgZr-AlN film), or an AlN film containing Mg and hafnium (Hf) (MgHf-AlN film). This can improve the piezoelectric constant of the AlN film 3B, and as a result, it is possible to reliably increase the ultrasonic receiving sensitivity.
[0029] The input-side upper electrode film 4B (hereinafter also referred to as the upper electrode film 4B) can have the same configuration as the above-mentioned upper electrode film 4A. That is, the upper electrode film 4B can be formed using various metals such as Pt, Au, Al, Cu, etc., or alloys thereof. The upper electrode film 4B can also be formed using various metals such as molybdenum (Mo), Ru, etc., or alloys thereof. For example, the upper electrode film 4B can be formed using a method such as a sputtering method, a vapor deposition method, a plating method, or a metal paste method. The upper electrode film 4B does not have a significant effect on the crystal structure of the AlN film 3B, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4B are not particularly limited. Note that, in order to increase the adhesion between the AlN film 3B and the upper electrode film 4B, for example, Ti, Ta, TiO 2 An adhesion layer mainly composed of Ni or the like may be provided. The thickness of the upper electrode film 4B may be, for example, 10 nm or more and 5000 nm or less, and when an adhesion layer is provided, the thickness of the adhesion layer may be, for example, 1 nm or more and 200 nm or less.
[0030] An ultrasonic output section (hereinafter also referred to as "output section") is configured by a laminated section including the lower electrode film 2, the KNN film 3A, and the upper electrode film 4A. The output section may also include the adhesion layer 6 and an output side vibration section formed on the substrate 1, which will be described later. The output section is a section that generates and transmits (outputs) ultrasonic waves. The output section is configured to deform the KNN film 3A by applying an electric field (voltage) between the lower electrode film 2 and the upper electrode film 4A by a voltage application section 11a, which will be described later and is connected between the lower electrode film 2 and the upper electrode film 4A, and the output side vibration section vibrates due to the deformation of the KNN film 3A, and outputs ultrasonic waves generated by the vibration of the output side vibration section.
[0031] The ultrasonic input section (hereinafter also referred to as "input section") is configured by a laminated section including the lower electrode film 2, the AlN film 3B, and the upper electrode film 4B. The input section may also include the adhesion layer 6 and the input side vibration section formed on the substrate 1, which will be described later. The input section is a section that receives (inputs) ultrasonic waves output from the output section and reflected by the test object. The input section is configured so that upon receiving ultrasonic waves, the input side vibration section vibrates, causing the AlN film 3B to deform. This deformation of the AlN film 3B generates a voltage between the lower electrode film 2 and the upper electrode film 4B.
[0032] The output section and the input section are arranged so as not to overlap each other when the substrate 1 (piezoelectric laminate 10) is viewed from above. This makes it possible to suppress interference between the output section and the input section. As a result, it is possible to improve the sensing accuracy of the ultrasonic sensor 30 (described later) manufactured using the piezoelectric laminate 10. Here, "when the substrate 1 is viewed from above" means "when the main surface of the substrate 1 on which the KNN film 3A, the AlN film 3B, etc. are provided is viewed from above in the vertical direction." Note that the "vertical direction" here is a direction that coincides with at least one of the propagation direction of the ultrasonic waves transmitted from the output section or the propagation direction of the ultrasonic waves received by the input section.
[0033] The distance d between the output section and the input section is preferably as short as possible so that they do not interfere with each other (do not contact each other). In other words, the output section and the input section are not in contact with each other, but it is preferable that the distance d between them is as short as possible. For example, it is preferable that the distance (maximum distance) d between the output section and the input section is 500 μm or less. It is more preferable that the output section and the input section are located as close as possible to each other using MEMS manufacturing technology. This makes it possible to increase the integration density of the output section and the input section and to reduce the size of the ultrasonic sensor 30 described below while improving the performance.
[0034] (2) Piezoelectric element and ultrasonic sensor configuration 3 shows a schematic configuration diagram of an ultrasonic sensor 30 according to this embodiment. The ultrasonic sensor 30 includes at least one piezoelectric element 20, and a voltage application unit 11a and a voltage detection unit 11b connected to the piezoelectric element 20. Examples of applications of the ultrasonic sensor 30 include p-MUTs and the like.
[0035] The piezoelectric element 20 means an element having an output-side piezoelectric film 3A and an input-side piezoelectric film 3B, and is obtained by forming the above-mentioned piezoelectric laminate 10 into a predetermined shape. When forming the piezoelectric laminate 10 into a predetermined shape, for example, an output-side vibration part is formed at a position on the substrate 1 corresponding to the output part, and an input-side vibration part is formed at a position on the substrate 1 corresponding to the input part. The output-side vibration part and the input-side vibration part can be formed by forming, for example, a membrane structure or a cantilever structure on the substrate 1 of the piezoelectric laminate 10. FIG. 3 illustrates a piezoelectric element 20 in which a membrane structure is formed on the substrate 1.
[0036] The resonance frequencies of the output side vibration section and the input side vibration section may be the same or different. For example, the width of the output side vibration section and the input side vibration section may be made different from each other depending on the resonance frequency, such as making the width of the output side vibration section larger than the width of the input side vibration section. Also, the thickness of the substrate 1 constituting the output side vibration section and the input side vibration section may be made different from each other depending on the resonance frequency, such as making the thickness of the substrate 1 at a position corresponding to the output section thicker than the thickness of the substrate 1 at a position corresponding to the input section.
[0037] The voltage application unit 11a is a means for applying a voltage between the lower electrode film 2 (output side lower electrode film 2A) and the upper electrode film 4A, and the voltage detection unit 11b is a means for detecting a voltage generated between the lower electrode film 2 (input side lower electrode film 2B) and the upper electrode film 4B. Various known means can be used as the voltage application unit 11a and the voltage detection unit 11b.
[0038] By connecting the voltage application unit 11a between the lower electrode film 2 and the upper electrode film 4A of the piezoelectric element 20, the output unit can function as a vibrator for generating ultrasonic waves. By applying a voltage between the lower electrode film 2 and the upper electrode film 4A by the voltage application unit 11a, the KNN film 3A can be deformed. This deformation action causes the output vibration unit to vibrate, and this vibration can generate ultrasonic waves.
[0039] By connecting the voltage detection unit 11b between the lower electrode film 2 and the upper electrode film 4B of the piezoelectric element 20, the input unit can function as a sensor. When the input unit receives ultrasonic waves and the input-side vibration unit vibrates, the AlN film 3B deforms, and a voltage is generated between the lower electrode film 2 and the upper electrode film 4B due to the deformation. By detecting this voltage with the voltage detection unit 11b, the magnitude of the ultrasonic waves received by the input unit can be measured.
[0040] The ultrasonic sensor 30 is configured to transmit ultrasonic waves from the output unit toward the test object, and receive the ultrasonic waves reflected by the test object at the input unit. Therefore, for example, the presence or absence of the test object can be determined by detecting the magnitude of the voltage detected by the voltage detection unit 11b multiple times and observing the change in the voltage. Also, for example, the distance to the test object can be known by measuring the time from the start of voltage application by the voltage application unit 11a to the detection of the voltage by the voltage detection unit 11b multiple times and observing the change in this time.
[0041] (3) Methods for manufacturing piezoelectric laminates, piezoelectric elements, and ultrasonic sensors Hereinafter, a method for manufacturing the above-mentioned piezoelectric laminate 10, piezoelectric element 20, and ultrasonic sensor 30 will be described with reference to FIGS. 4(a) to 4(f).
[0042] (Deposition of the lower electrode film) First, a substrate 1 is prepared, and an adhesion layer 6 (Ti layer) and a lower electrode film 2 (Pt film) are formed in this order on one of the main surfaces of the substrate 1 by, for example, a sputtering method. This results in a laminate 10a as shown in Fig. 4(a). Note that a substrate 1 (i.e., laminate 10a) on which an adhesion layer 6 and a lower electrode film 2 have been formed in advance on one of the main surfaces may be prepared.
[0043] The conditions for forming the adhesion layer 6 are exemplified as follows. Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Discharge power: 1000W or more and 1500W or less, preferably 1100W or more and 1300W or less Atmosphere: Argon (Ar) gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Time: 30 seconds or more and 3 minutes or less, preferably 30 seconds or more and 2 minutes or less
[0044] The following conditions are exemplified as conditions for depositing the lower electrode film 2. As a target used for depositing the film by sputtering, for example, a metal target made of Pt can be used. Film-forming temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Discharge power: 1000W or more and 1500W or less, preferably 1100W or more and 1300W or less Film deposition atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Film formation time: 3 to 10 minutes, preferably 4 to 7 minutes
[0045] (Deposition of output side piezoelectric film) After the deposition of the lower electrode film 2 is completed, a KNN film 3A is deposited on the laminate 10a (on the lower electrode film 2) by, for example, a sputtering method. The composition ratio of the KNN film 3A can be adjusted by controlling the composition of the target material used during the sputtering deposition. 2CO 3 Powder, Sodium 2 CO 3 powder, Nb 2 O 5 Powder, Cu powder (or CuO powder, Cu 2 The target can be made by mixing and sintering a mixture of K, MnO, and MnO powder. 2 CO 3 Powder, Sodium 2 CO 3 powder, Nb 2 O 5 Powder, Cu powder (or CuO powder, Cu 2 The powder content can be controlled by adjusting the mixing ratio of powder such as MnO powder, MnO powder, etc.
[0046] The conditions for forming the KNN film 3A are exemplified as follows: The film formation time is appropriately set according to the thickness of the KNN film 3A to be formed. Film-forming temperature (substrate temperature): More than 350°C and less than 700°C, preferably 550°C or more and 650°C or less Discharge power: 2000W or more and 2400W or less, preferably 2100W or more and 2300W or less Film deposition atmosphere: Ar gas + oxygen (O 2 ) gas mixture atmosphere (oxygen (O)-containing atmosphere) Ambient pressure: 0.2 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less O 2 The partial pressure of Ar gas relative to the gas (Ar / O 2 Partial pressure ratio): 30 / 1 to 20 / 1, preferably 27 / 1 to 23 / 1 Film-forming speed: 0.5 μm / hr or more and 2 μm / hr or less, preferably 0.5 μm / hr or more and 1.5 μm / hr or less
[0047] This results in a laminate 10b as shown in Fig. 4(b). By depositing the KNN film 3A under the above-mentioned conditions, it is possible to deposit a high-quality KNN film 3A, for example, a KNN film 3A having a piezoelectric constant of 100 pm / V or more.
[0048] After the deposition of the KNN film 3A is completed, the KNN film 3A is shaped into a predetermined shape (predetermined pattern) by etching, etc. This results in a stack 10c as shown in FIG.
[0049] (Protective film formation) Next, a protective film 12 is formed to protect the KNN film 3A. The protective film 12 is provided so as to protect (cover) the KNN film 3A.
[0050] The protective film 12 is a material that can protect the KNN film 3A without being reduced, i.e., without being deteriorated, in the deposition atmosphere (N-containing atmosphere) of the AlN film 3B, and can be deposited using a material that can be easily removed by wet etching using an etching solution containing, for example, fluorine (F). The protective film 12 can be deposited using, for example, silicon oxide (SiO 2 ) can be used for the deposition. The protective film 12 can be deposited by a CVD (Chemical Vapor Deposition) method, a sputtering method, a vapor deposition method, or the like. The thickness of the protective film 12 can be set to a thickness that can continuously cover the surface of the KNN film 3A, that is, a thickness that makes the protective film 12 a continuous film. In the following, the "deposition atmosphere of the AlN film 3B" is also referred to as the "N-containing atmosphere".
[0051] The conditions for forming the protective film 12 by the plasma CVD method are exemplified as follows. Film-forming temperature (substrate temperature): 200° C. or higher and 400° C. or lower, preferably 300° C. or higher and 400° C. or lower, more preferably 350° C. Discharge power: 70W or more and 150W or less, preferably 70W or more and 120W or less, more preferably 100W Raw material: Tetraethoxysilane (abbreviation: TEOS) Film deposition atmosphere: O 2 Gas atmosphere Atmospheric pressure: 50 Pa or more and 100 Pa or less, preferably 60 Pa or more and 70 Pa or less, more preferably 67 Pa
[0052] The deposition time is appropriately set depending on the thickness of the protective film 12 to be deposited. The deposition time can be, for example, 5 minutes or more and 15 minutes or less. Specifically, when depositing a protective film 12 with a thickness of 400 nm, the deposition time can be 11 minutes.
[0053] By forming the protective film 12 under the above-mentioned conditions, the protective film 12 can be formed as a continuous film that covers the KNN film 3A. The protective film 12 acts as a film that suppresses the reduction of the KNN film 3A in an N-containing atmosphere, and protects the KNN film 3A. This protective effect can prevent the KNN film 3A from being exposed to an N-containing atmosphere during the formation of the AlN film 3B. This makes it possible to prevent the KNN film 3A from being reduced and deteriorated by N elements during the formation of the AlN film 3B, that is, the KNN film 3A from being deteriorated due to the removal of oxygen in the KNN film 3A by N elements. As a result, it is possible to prevent changes in the piezoelectric performance and quality of the KNN film 3A (for example, deterioration of insulating properties).
[0054] After the deposition of the protective film 12 is completed, the protective film 12 is shaped into a predetermined pattern. For example, the protective film 12 is removed by etching or the like from the position on the substrate 1 where the AlN film 3B is to be deposited. This results in a stacked body 10d as shown in FIG. 4(d).
[0055] (Deposition of the input side piezoelectric film) Then, the AlN film 3B is formed by, for example, sputtering. As the target material, for example, a metal target made of Al can be used.
[0056] The conditions for depositing the AlN film 3B are exemplified as follows: The deposition time is appropriately set according to the thickness of the AlN film 3B to be deposited. Film forming temperature (substrate temperature): 300℃ or higher and 350℃ or lower Discharge power: 600W or more and 900W or less, preferably 700W or more and 800W or less Film deposition atmosphere: Ar gas + nitrogen (N 2 ) gas mixture atmosphere (N-containing atmosphere) Ambient pressure: 0.5 Pa or more and 2.0 Pa or less, preferably 0.7 Pa or more and 1.0 Pa or less N 2 The partial pressure of Ar gas relative to the gas (Ar / N 2 Partial pressure ratio): 1 / 10 to 1 / 2, preferably 1 / 7 to 1 / 3, more preferably 1 / 6 to 1 / 4 Film-forming speed: 0.3 μm / hr or more and 2 μm / hr or less, preferably 0.3 μm / hr or more and 1 μm / hr or less, more preferably 0.3 μm / hr or more and 0.5 μm / hr or less The deposition atmosphere was a mixture of Ar gas and ammonia (NH 3 ) gas may be used.
[0057] As a result, a laminate 10e as shown in Fig. 4(e) is obtained. Moreover, by forming the AlN film 3B under the above-mentioned conditions, it is possible to form a high-quality AlN film 3B, for example, an AlN film 3B having a relative dielectric constant of 25 or less. As described above, since the KNN film 3A is covered with the protective film 12, the KNN film 3A is hardly reduced by N elements present in the N-containing atmosphere.
[0058] After the formation of the AlN film 3B is completed, the protective film 12 is removed by wet etching using an etching solution containing, for example, fluorine (F). This exposes the KNN film 3A. Furthermore, the unnecessary AlN film 3B formed on the protective film 12 is removed using the protective film 12 as a lift-off layer. In other words, the AlN film 3B is left only in the region where the AlN film 3B is to be formed. As a result, a stacked body 10f as shown in FIG. 4(f) is obtained. Note that, as an etching solution containing F, for example, 4.32 mol / L hydrogen fluoride (HF), ammonium fluoride (NH 4 A buffered hydrofluoric acid (BHF) solution containing 10.67 mol / L of F can be used.
[0059] (Deposition of upper electrode film) Then, Pt films are formed as upper electrode films 4A and 4B on the KNN film 3A and the AlN film 3B by, for example, a sputtering method. The conditions for forming the upper electrode films 4A and 4B can be the same as those for forming the lower electrode film 2. This results in a piezoelectric stack 10 as shown in FIG.
[0060] Then, by forming this piezoelectric stack 10 into a predetermined shape by etching or the like, a piezoelectric element 20 as shown in FIG. 3 is obtained, and by connecting at least one of a voltage application unit 11a or a voltage detection unit 11b to the piezoelectric element 20, an ultrasonic sensor 30 is obtained.
[0061] (4) Effects Obtained by the Present Embodiment According to this embodiment, one or more of the following advantages can be obtained.
[0062] (a) The piezoelectric laminate 10 has an output side piezoelectric film 3A (KNN film 3A) and an input side piezoelectric film 3B (AlN film 3B), and the output part formed by the laminate part having the KNN film 3A and the input part formed by the laminate part having the AlN film 3B do not overlap each other when the substrate 1 is viewed from the top. This makes it possible to drive the KNN film 3A and the AlN film 3B independently. In addition, in the piezoelectric laminate 10, the output side piezoelectric film 3A is made of an oxide film (i.e., the KNN film 3A) having a relatively high piezoelectric constant, and the input side piezoelectric film 3B is made of a nitride film (i.e., the AlN film 3B) having a relatively low relative dielectric constant. By using such a piezoelectric laminate 10, it is possible to obtain an ultrasonic sensor 30 that has a deep penetration depth of ultrasonic waves into the test object and has high resolution (high reception sensitivity). In other words, it is possible to obtain a high-performance ultrasonic sensor 30.
[0063] (b) According to this embodiment, the piezoelectric stack 10 having an output section and an input section, the piezoelectric element 20 obtained by processing the piezoelectric stack 10, and the ultrasonic sensor 30 manufactured using the piezoelectric element 20 can be formed in one step during the MEMS manufacturing process. In other words, it is possible to manufacture a high-performance ultrasonic sensor 30 without complicating the manufacturing process.
[0064] (c) Since the output section and the input section are not in contact with each other, it is possible to suppress interference between the output section and the input section. For example, it is possible to suppress the vibration of the output side vibration section from being transmitted to the input side vibration section. This makes it possible to improve the sensing accuracy of the ultrasonic sensor 30. In other words, it is possible to improve the performance of the ultrasonic sensor 30.
[0065] (d) In the piezoelectric laminate 10, the distance between the output section and the input section is, for example, 500 μm or less, and preferably 300 μm or less. Preferably, the output section and the input section are as close together as possible with MEMS manufacturing technology. This makes it possible to increase the integration degree of the output section and the input section while improving the sensing accuracy of the ultrasonic sensor 30. In other words, it is possible to obtain a high-performance, small-sized ultrasonic sensor 30.
[0066] (e) By providing a protective film 12 for protecting the KNN film 3A after the KNN film 3A is formed and before the AlN film 3B is formed, the KNN film 3A can be prevented from being exposed to an N-containing atmosphere during the formation of the AlN film 3B. This prevents the KNN film 3A from being reduced and deteriorated by N elements in the N-containing atmosphere, and as a result, the piezoelectric performance and quality of the KNN film 3A can be prevented from being reduced. That is, a piezoelectric laminate 10 can be obtained that includes a KNN film 3A having a high-quality and high-performance KNN film 3A and an AlN film 3B having a high-quality and high-performance KNN film 3A. For example, a piezoelectric laminate 10 can be obtained that includes a KNN film 3A having a high piezoelectric constant and an AlN film 3B having a low relative dielectric constant.
[0067] (f) Since the KNN film 3A contains at least one metal element selected from the group consisting of Cu, Mn, Fe, and V, the etching resistance of the KNN film 3A to a fluorine-based etching solution such as a BHF solution can be improved. This makes it possible to prevent the KNN film 3A from being etched when the protective film 12 is removed by wet etching using a BHF solution or the like. As a result, it becomes possible to reliably suppress deterioration in the piezoelectric performance and quality of the KNN film 3A. The inventors of the present application have confirmed that the effect of improving the etching resistance of the KNN film 3A can be particularly enhanced when Cu, among the above metal elements, is added to the KNN film 3A.
[0068] Here, for reference, a conventional ultrasonic sensor will be described. In the conventional ultrasonic sensor, a piezoelectric element having a piezoelectric film made of an oxide film such as a PZT film is used to transmit and receive ultrasonic waves. However, in such an ultrasonic sensor, although the penetration depth of ultrasonic waves is deep, the relative dielectric constant of the piezoelectric film is high, and the resolution of the sensor is low (i.e., the reception sensitivity is low). On the other hand, in order to increase the resolution of the conventional ultrasonic sensor, it is possible to transmit and receive ultrasonic waves using a piezoelectric element having a piezoelectric film made of a nitride film such as an AlN film. However, in such an ultrasonic sensor, although the resolution is high, the piezoelectric constant of the piezoelectric film is low, and the penetration depth of ultrasonic waves is shallow. To address this issue, in this embodiment, an output side piezoelectric film 3A (KNN film 3A) made of an oxide film and an input side piezoelectric film 3B (AlN film 3B) made of a nitride film are provided, and ultrasonic waves are transmitted at the output section including the KNN film 3A, and ultrasonic waves are received at the input section including the AlN film 3B. As a result, according to this embodiment, it is possible to obtain a high-performance ultrasonic sensor 30 or the like having a deep penetration depth of ultrasonic waves and high resolution.
[0069] It is also possible to prepare at least two separate piezoelectric elements, an element for transmitting ultrasonic waves having a piezoelectric film made of an oxide film, and an element for receiving ultrasonic waves having a piezoelectric film made of a nitride film, and provide these at least two piezoelectric elements on the vibration part of the substrate on which the vibration part is formed, to configure an ultrasonic sensor. However, when manufacturing such an ultrasonic sensor, a process of attaching (adhering) the piezoelectric element to the substrate is required. This may complicate the manufacturing process of the ultrasonic sensor. In addition, in the process of attaching the piezoelectric element to the substrate, the distance between adjacent piezoelectric elements can only be about 1 mm, and at the shortest, about 500 μm, so there is also a problem that it is difficult to increase the integration degree of multiple piezoelectric elements. In contrast, according to this embodiment, it is possible to manufacture the piezoelectric laminate 10 (piezoelectric element 20, ultrasonic sensor 30) having an output part including the KNN film 3A and an input part including the AlN film 3B in a batch in the MEMS manufacturing process. In other words, according to this embodiment, it is possible to manufacture a high-performance ultrasonic sensor 30 with a deep penetration depth of ultrasonic waves and high resolution without complicating the manufacturing process. In addition, in this embodiment, since the piezoelectric stack 10 and the like are fabricated in a batch in the MEMS manufacturing process, it is possible to bring the output section and the input section as close as possible to the distance that is possible with the MEMS manufacturing technology. In this way, according to this embodiment, it is possible to fabricate a high-performance, small-sized ultrasonic sensor 30 in a batch in the MEMS manufacturing process.
[0070] (5) Variations This embodiment can be modified as follows: In the following description of the modifications, the same components as those in the above-described embodiment are denoted by the same reference numerals, and the description thereof will be omitted.
[0071] (Variation 1) As shown in FIG. 5, the piezoelectric laminate 40 may be configured to include an output-side lower electrode film 2A (hereinafter also referred to as the lower electrode film 2A) and an input-side lower electrode film 2B (hereinafter also referred to as the lower electrode film 2B) provided on the lower electrode film 2A.
[0072] The lower electrode film 2A can have the same configuration as the lower electrode film 2 in the above-described embodiment.
[0073] The lower electrode film 2B can be formed using at least one of hafnium (Hf) and molybdenum (Mo), for example. The lower electrode film 2B is a single crystal film or a polycrystalline film. The crystals constituting the lower electrode film 2B are preferably preferentially oriented in the (111) plane direction with respect to the surface of the substrate 1. That is, the surface of the lower electrode film 2B (the surface serving as the base of the input-side piezoelectric film 3B) is preferably mainly composed of the Hf (111) plane or the Mo (111) plane. The lower electrode film 2B can be formed using a method such as a sputtering method or a vapor deposition method. The lower electrode film 2B can also be configured in the same manner as the above-mentioned lower electrode film 2. The lower electrode film 2B can also be formed using, for example, Pt. The lower electrode film 2B can also be formed using, for example, Al, Cu, or silver (Ag). The thickness of the lower electrode film 2B can be, for example, 100 nm or more and 400 nm or less. Although not shown in FIG. 5, an adhesive layer similar to the adhesive layer 6 described above may be provided between the lower electrode film 2A and the lower electrode film 2B in order to improve adhesion therebetween.
[0074] In this modification, the output section is composed of a laminated section including the lower electrode film 2A, the KNN film 3A, and the upper electrode film 4A. The input section is composed of a laminated section including the lower electrode film 2B, the AlN film 3B, and the upper electrode film 4B. The lower electrode film 2A located below the AlN film 3B may be included in the input section.
[0075] A method for manufacturing the piezoelectric laminate 40 shown in FIG. 5 will be described with reference to FIGS. 6(a) to (f).
[0076] First, a substrate 1 is prepared, and an adhesion layer 6 (Ti layer) and a lower electrode film 2A are formed in this order on one of the main surfaces of the substrate 1 by, for example, a sputtering method. The adhesion layer 6 and the lower electrode film 2A can be formed under the same conditions as those for forming the adhesion layer 6 and the lower electrode film 2 in the above-mentioned embodiment. As a result, a stacked body 40a as shown in FIG. 6(a) is obtained.
[0077] Next, the KNN film 3A is formed by the same procedure and conditions as in the above embodiment, and the KNN film 3A is shaped into a predetermined pattern. This results in a laminate 40b as shown in FIG. 6(b). Thereafter, the protective film 12 is formed by the same procedure and conditions as in the above embodiment, and is shaped into a predetermined pattern. This results in a laminate 40c as shown in FIG. 6(c).
[0078] Then, the lower electrode film 2B is formed by, for example, a sputtering method. As a result, a stacked body 40d as shown in Fig. 6(d) is obtained. In this modification, the lower electrode film 2B is also formed on the protective film 12 as shown in Fig. 6(d).
[0079] The conditions for depositing the lower electrode film 2B are exemplified as follows: As a target used for depositing the lower electrode film 2B by sputtering, a metal target made of, for example, Hf or Mo can be used. Film-forming temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Discharge power: 1000W or more and 1500W or less, preferably 1100W or more and 1300W or less Film deposition atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Film formation time: 3 to 10 minutes, preferably 4 to 7 minutes
[0080] Then, the AlN film 3B is formed by the same procedure and conditions as in the above-mentioned embodiment. As a result, a stack 40e as shown in FIG. 6(e) is obtained. After that, the protective film 12 is removed by the same procedure and conditions as in the above-mentioned embodiment. As a result, the KNN film 3A is exposed. In addition, the unnecessary lower electrode film 2B and AlN film 3B formed on the protective film 12 are also removed by using the protective film 12 as a lift-off layer. That is, the lower electrode film 2B and AlN film 3B are left only in the region where the lower electrode film 2B and AlN film 3B should be formed. As a result, a stack 40f as shown in FIG. 6(f) is obtained. After that, the upper electrode films 4A and 4B are formed by the same procedure and conditions as in the above-mentioned embodiment. As a result, a piezoelectric stack 40 as shown in FIG. 5 is obtained.
[0081] In other respects, the configuration and manufacturing method can be the same as those of the above-mentioned embodiment. The present modification can also provide the same effects as those of the above-mentioned embodiment. That is, the present modification can also provide a high-performance ultrasonic sensor 30, and such ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process.
[0082] (Variation 2) 7, a piezoelectric laminate 41 may be formed in such a manner that the lower electrode film 2A is provided only at a position on the substrate 1 facing the KNN film 3A, and the lower electrode film 2B is provided only at a position on the substrate 1 facing the AlN film 3B. The lower electrode film 2A may have the same configuration as the lower electrode film 2, and the lower electrode film 2B may have the same configuration as the above-mentioned modified example 1.
[0083] In this modification, an output section is formed of a laminated section including a lower electrode film 2A, a KNN film 3A, and an upper electrode film 4A. An input section is formed of a laminated section including a lower electrode film 2B, an AlN film 3B, and an upper electrode film 4B.
[0084] Other points can be the same as those of the above-mentioned embodiment and modified examples. This modified example can also obtain the same effects as those of the above-mentioned embodiment. That is, this modified example can also obtain a high-performance ultrasonic sensor 30, and such ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process.
[0085] Furthermore, according to this modification, while transmitting ultrasonic waves from the output unit toward the test object, it is also possible for the input unit to receive ultrasonic waves reflected by the test object. This makes it possible, for example, for the ultrasonic sensor 30 to continuously detect the magnitude of the voltage detected by the voltage detection unit 11b. Also, for example, it becomes possible for the ultrasonic sensor 30 to continuously measure the time from the start of voltage application by the voltage application unit 11a to the detection of the voltage by the voltage detection unit 11b. In this way, according to this modification, it is also possible to increase the degree of freedom of transmission and reception of ultrasonic waves in the ultrasonic sensor 30.
[0086] (Variation 3) As shown in FIG. 8, a piezoelectric laminate 42 may be formed by providing an AlN film 3B on a KNN film 3A.
[0087] In this modification, the output section is formed of a laminated section including the lower electrode film 2, the KNN film 3A, and the upper electrode film 4A. The input section is formed of a laminated section including the lower electrode film 2, the AlN film 3B, and the upper electrode film 4B. The KNN film 3A located below the AlN film 3B may be included in the input section.
[0088] A method for manufacturing the piezoelectric laminate 42 shown in FIG. 8 will be described with reference to FIGS. 9(a) to (e).
[0089] First, a substrate 1 is prepared, and an adhesion layer 6 (Ti layer) and a lower electrode film 2 are formed in this order on one of the main surfaces of the substrate 1 by, for example, a sputtering method using the same procedures and conditions as in the above-described embodiment. This results in a stacked body 42a as shown in FIG. 9(a).
[0090] Next, the KNN film 3A is formed by the same procedure and conditions as in the above-mentioned embodiment. As a result, a stack 42b as shown in FIG. 9(b) is obtained. Then, the protective film 12 is formed on the KNN film 3A by the same procedure and conditions as in the above-mentioned embodiment. Then, the protective film 12 is shaped into a predetermined pattern. For example, the protective film 12 is removed by etching or the like from the position on the substrate 1 where the AlN film 3B is to be formed, that is, from the position on the KNN film 3A. As a result, a stack 42c as shown in FIG. 9(c) is obtained. Then, the AlN film 3B is formed by the same procedure and conditions as in the above-mentioned embodiment. As a result, a stack 42d as shown in FIG. 9(d) is obtained. Then, the protective film 12 is removed by the same procedure and conditions as in the above-mentioned embodiment. As a result, a predetermined region of the KNN film 3A is exposed. In addition, the unnecessary AlN film 3B formed on the protective film 12 is also removed by using the protective film 12 as a lift-off layer. That is, the AlN film 3B is left only in the region where the AlN film 3B is to be formed. As a result, a laminate 42e as shown in Fig. 9(e) is obtained. Thereafter, the upper electrode films 4A and 4B are formed by the same procedure and conditions as in the above-mentioned embodiment. This results in a piezoelectric laminate 42 as shown in Fig. 8.
[0091] The other points can be the same as those of the above-mentioned embodiment and modified examples. This modified example can also obtain the same effects as those of the above-mentioned embodiment and modified examples. That is, this modified example can also obtain a high-performance ultrasonic sensor 30, and such an ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process. The inventors of the present application have confirmed that even when the AlN film 3B is provided on the KNN film 3A as in this modified example, the input section can detect the vibration of the input-side vibration section with good sensitivity.
[0092] This modification is not limited to the embodiment shown in Fig. 8. For example, the lower electrode film 2 shown in Fig. 8 may function as the lower electrode film 2A, and a lower electrode film 2B having the same configuration as in the modification 1 may be provided between the KNN film 3A and the AlN film 3B.
[0093] (Variation 4) In the above embodiment, the AlN film 3B is formed after the KNN film 3A is formed, but the present invention is not limited to this. That is, the KNN film 3A may be formed after the AlN film 3B is formed.
[0094] In this modification, after the AlN film 3B is formed and before the KNN film 3A is formed, the protective film 12 is formed to cover the AlN film 3B by the same procedure and conditions as in the above embodiment. Then, the protective film 12 is removed by etching or the like from the position on the substrate 1 (lower electrode film 2) where the KNN film 3A is to be formed, and the protective film 12 is shaped into a predetermined pattern. Then, the KNN film 3A is formed by the same procedure and conditions as in the above embodiment. When the formation of the KNN film 3A is completed, the protective film 12 is removed by the same procedure and conditions as in the above embodiment. This exposes the AlN film 3B and removes the unnecessary KNN film 3A formed on the protective film 12. Thus, in this modification, the protective film 12 functions as a lift-off layer that removes the unnecessary KNN film 3A.
[0095] Other points can be the same as those of the above-mentioned embodiment and modified examples. This modified example can also obtain the same effects as those of the above-mentioned embodiment. That is, this modified example can also obtain a high-performance ultrasonic sensor 30, and such ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process.
[0096] (Variation 5) As shown in FIG. 10, the piezoelectric laminate 43 may be configured to include a substrate 1, a lower electrode film 2B provided on the substrate 1, an input side piezoelectric film (AlN film) 3B provided on the lower electrode film 2B, an output side lower electrode film 2A provided on the input side piezoelectric film 3B, an output side piezoelectric film (KNN film) 3A provided on the output side lower electrode film 2A, an upper electrode film 4A provided on the output side piezoelectric film 3A, and an upper electrode film 4B provided on the input side piezoelectric film 3B.
[0097] In this modification, the output section is composed of a laminated section including the lower electrode film 2A, the KNN film 3A, and the upper electrode film 4A. The lower electrode film 2B and the AlN film 3B located below the KNN film 3A may be considered to be included in the output section. The input section is composed of a laminated section including the lower electrode film 2B, the AlN film 3B, and the upper electrode film 4B.
[0098] Other points can be the same as those of the above-mentioned embodiment and modification. This modification can also provide the same effects as those of the above-mentioned embodiment and modification, that is, this modification can also provide a high-performance ultrasonic sensor 30, and such ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process.
[0099] In this modification, the lower electrode film 2A is provided on the AlN film 3B, and the KNN film 3A is provided on the lower electrode film 2A. As a result, in this modification, the KNN film 3A is also formed directly on the lower electrode film 2A, i.e., on the Pt film, so that it is easy to preferentially orient the crystals constituting the KNN film 3A in the (001) plane direction. However, the lower electrode film 2A does not have to be provided. That is, the lower electrode film 2B may be configured in the same manner as the lower electrode film 2 in the above embodiment, and the lower electrode film 2 may function as the output-side lower electrode film 2A and also as the input-side lower electrode film 2B.
[0100] (Variation 6) A substrate on which a semiconductor circuit such as CMOS is formed can also be used as the substrate 1. When the KNN film 3A is formed on the substrate 1 on which a circuit such as CMOS is formed, it is preferable to form the film under a temperature condition of less than 500°C, more preferably, at or above the deposition temperature of the AlN film 3B and below 500°C, from the viewpoint of suppressing the destruction of the semiconductor circuit such as CMOS. By forming the KNN film 3A under a temperature condition of less than 500°C, it is possible to suppress the destruction of the semiconductor circuit formed on the substrate 1 during the deposition of the KNN film 3A. By forming the KNN film 3A under a temperature condition of at or above the deposition temperature of the AlN film 3B, it is possible to reliably suppress the KNN film 3A from being reduced in the deposition atmosphere of the AlN film 3B, even when the AlN film 3B is deposited after the KNN film 3A is deposited, as in the above-mentioned embodiment. The inventors of the present application have confirmed that the KNN film 3A having a piezoelectric constant of 100 pm / V or more can be obtained even when the KNN film 3A is deposited at a low temperature of less than 500°C.
[0101] Other points can be the same as those of the above-mentioned embodiment and modified examples. This modified example also provides the same effects as those of the above-mentioned embodiment. That is, this modified example also provides a high-performance ultrasonic sensor 30, and such ultrasonic sensor 30 can be fabricated in a batch in the MEMS manufacturing process.
[0102] (Variation 7) The output section and the input section may be in contact with each other. In addition, since the output side vibration section and the input side vibration section are formed separately and independently, it is possible to suppress interference between the output side vibration section and the input side vibration section. This modification also makes it possible to obtain a high-performance ultrasonic sensor 30, and such an ultrasonic sensor 30 can be manufactured in a batch in the MEMS manufacturing process. However, from the viewpoint of reliably suppressing interference between the output section and the input section and reliably suppressing deterioration in the sensor performance of the ultrasonic sensor 30, it is preferable that the output section and the input section are not in contact with each other.
[0103] (Variation 8) In the above-described embodiment, the case where the AlN film 3B is a polycrystalline film of AlN has been described. However, the AlN film 3B may be a single-crystalline film of AlN. Also according to this modification example, the same effects as those of the above-described embodiment, modification examples, etc. can be obtained.
[0104] <Other Embodiments> As described above, the embodiments of the present invention have been specifically described. However, the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the gist thereof.
[0105] In the above-described embodiment and modification examples, the case where the output-side piezoelectric film 3A is a KNN film has been described. However, it is not limited thereto. The output-side piezoelectric film 3A may be, in addition to the above KNN, lead zirconate titanate (PZT), that is, lead (Pb), zirconium (Zr), titanium (Ti), and has a composition formula Pb(Zr 1-x Ti x )O 3 (0 < x < 1). A film can also be formed using the compound represented by Further, the output-side piezoelectric film 3A may be bismuth sodium titanate (BNT), that is, bismuth (Bi), Na, Ti, and has a composition formula (Bi 1-x Na x )TiO 3 (0 < x < 1). A film can also be formed using the compound represented by Further, the output-side piezoelectric film 3A may be bismuth ferrite (BFO), that is, a film can be formed using the compound represented by the composition formula BiFeO 3 . Even when the output-side piezoelectric film 3A is formed using PZT, BNT, or BFO, the same effects as those of the above-described embodiment, etc. can be obtained. That is, a high-performance ultrasonic sensor 30 can be obtained, and such an ultrasonic sensor 30 can be manufactured in a batch in the process of MEMS manufacturing.
[0106] In the above-described embodiment and modification examples, the case where the input-side piezoelectric film 3B is an AlN film has been described. However, it is not limited thereto. The input-side piezoelectric film 3B may be another nitride film exhibiting piezoelectric performance equivalent to that of the AlN film.
[0107] Furthermore, for example, the output-side piezoelectric film 3A may contain, in addition to or instead of the above-mentioned metal elements such as Cu and Mn, other metal elements that have the same effect as the above-mentioned metal elements at a predetermined concentration.
[0108] In the above embodiment, the ultrasonic sensor 30 is obtained using the piezoelectric laminate 10 and the piezoelectric element 20, but the present invention is not limited to this. The piezoelectric laminate 10 and the piezoelectric element 20 may be used to obtain a piezoelectric device for use in an inkjet printer head, a MEMS mirror for a scanner, an angular velocity sensor, a pressure sensor, an acceleration sensor, or the like.
[0109] <Preferred embodiment of the present invention> Preferred aspects of the present invention will be described below.
[0110] (Appendix 1) According to one aspect of the present invention, A substrate; an output-side lower electrode film provided on the substrate; an output-side piezoelectric film that is an oxide film and is provided on the output-side lower electrode film; an output-side upper electrode film provided on the output-side piezoelectric film; an input side lower electrode film provided on the substrate; an input-side piezoelectric film that is a nitride film and is provided on the input-side lower electrode film; an input-side upper electrode film provided on the input-side piezoelectric film, A piezoelectric laminate is provided in which an ultrasonic output section constituted by a laminate having the output side lower electrode film, the output side piezoelectric film and the output side upper electrode film, and an ultrasonic input section constituted by a laminate having the input side lower electrode film, the input side piezoelectric film and the input side upper electrode film are arranged so as not to overlap each other when viewed from the top of the substrate.
[0111] (Appendix 2) The piezoelectric laminate according to claim 1, preferably The ultrasonic output section and the ultrasonic input section are not in contact with each other.
[0112] (Appendix 3) The piezoelectric laminate according to claim 1 or 2, preferably The output-side piezoelectric film has a larger piezoelectric constant than the input-side piezoelectric film, and the input-side piezoelectric film has a lower relative dielectric constant than the output-side piezoelectric film.
[0113] (Appendix 4) The piezoelectric laminate according to any one of Supplementary Notes 1 to 3, preferably The output-side piezoelectric film is formed using any one of potassium sodium niobate, lead zirconate titanate, bismuth sodium titanate, and bismuth ferrite.
[0114] (Appendix 5) The piezoelectric laminate according to any one of claims 1 to 4, preferably The output-side piezoelectric film is formed using potassium sodium niobate, and contains at least one of Cu and Mn in a concentration of 0.2 at % or more and 2.0 at % or less with respect to the amount of niobium contained in the output-side piezoelectric film.
[0115] (Appendix 6) The piezoelectric laminate according to any one of claims 1 to 5, preferably The input side piezoelectric film is made of aluminum nitride.
[0116] (Appendix 7) The piezoelectric laminate according to claim 6, preferably The input-side piezoelectric film contains scandium (Sc), magnesium (Mg) and zirconium (Zr), or magnesium (Mg) and hafnium (Hf).
[0117] (Appendix 8) The piezoelectric laminate according to any one of claims 1 to 7, preferably A semiconductor circuit is formed on the substrate.
[0118] (Appendix 9) According to another aspect of the present invention, forming an output-side lower electrode film and an input-side lower electrode film on a substrate; forming an output-side piezoelectric film, which is an oxide film, on the output-side lower electrode film; forming a protective film for protecting the output-side piezoelectric film; forming an input-side piezoelectric film, which is a nitride film, on the input-side lower electrode film; removing the protective film by etching to expose the output-side piezoelectric film; forming an output-side upper electrode film on the output-side piezoelectric film, and forming an input-side upper electrode film on the input-side piezoelectric film, The present invention provides a method for manufacturing a piezoelectric laminate, which includes a step of producing a laminate in which an ultrasonic output section constituted by a laminate portion having the output side lower electrode film, the output side piezoelectric film, and the output side upper electrode film, and an ultrasonic input section constituted by a laminate portion having the input side lower electrode film, the input side piezoelectric film, and the input side upper electrode film are arranged so as not to overlap each other when viewed from above the substrate.
[0119] (Appendix 10) The method according to claim 9, preferably comprising: The protective film is made of silicon dioxide (SiO 2 ) is a membrane consisting of
[0120] (Appendix 11) The method according to claim 9 or 10, preferably comprising A substrate on which a semiconductor circuit is formed is prepared as the substrate; In the step of depositing the output-side piezoelectric film, the output-side piezoelectric film is deposited under a temperature condition of less than 500° C. Preferably, in the step of depositing the output-side piezoelectric film, the output-side piezoelectric film is deposited under a temperature condition of equal to or higher than the deposition temperature of the input-side piezoelectric film in the step of depositing the input-side piezoelectric film and less than 500° C.
[0121] (Appendix 12) According to yet another aspect of the present invention, A piezoelectric laminate according to any one of claims 1 to 8, a voltage application means connected between the output-side lower electrode film and the output-side upper electrode film; a voltage detection means connected between the input side lower electrode film and the input side upper electrode film, A piezoelectric element and ultrasonic sensor are provided in which the output side piezoelectric film is deformed by applying a predetermined electric field between the output side lower electrode film and the output side upper electrode film by the voltage application means, ultrasonic waves generated by the deformation of the output side piezoelectric film are transmitted from the ultrasonic output section, the ultrasonic waves reflected by the test object are received by the ultrasonic input section, and the voltage generated between the input side lower electrode film and the input side upper electrode film by the deformation of the input side piezoelectric film is detected by the voltage detection means.
[0122] (Appendix 13) The device according to claim 12, preferably A vibration section (for example, a membrane structure or a cantilever structure) is formed at a position on the substrate corresponding to the ultrasonic output section and at a position on the substrate corresponding to the ultrasonic input section. [Explanation of symbols]
[0123] 1 Board 2A Output side lower electrode film 2B Input side lower electrode film 3A output side piezoelectric film (KNN film) 3B Input side piezoelectric film (AlN film) 4A Output side upper electrode film 4B Input side upper electrode film 10,40~43 Piezoelectric laminate
Claims
1. forming an output-side lower electrode film and an input-side lower electrode film on a substrate; forming an output-side piezoelectric film, which is an oxide film, on the output-side lower electrode film; forming a protective film for protecting the output-side piezoelectric film; forming an input-side piezoelectric film, which is a nitride film, on the input-side lower electrode film; removing the protective film by etching to expose the output-side piezoelectric film; forming an output-side upper electrode film on the output-side piezoelectric film, and forming an input-side upper electrode film on the input-side piezoelectric film, A method for manufacturing a piezoelectric laminate, comprising the step of producing a laminate in which an ultrasonic output section constituted by a laminate portion having the output side lower electrode film, the output side piezoelectric film, and the output side upper electrode film, and an ultrasonic input section constituted by a laminate portion having the input side lower electrode film, the input side piezoelectric film, and the input side upper electrode film are arranged so as not to overlap each other when viewed from the top of the substrate.
2. The method for producing a piezoelectric laminate according to claim 1 , wherein the protective film is a film made of silicon dioxide.
Citation Information
Patent Citations
Electronic equipment, ultrasonic fingerprint identification device and manufacturing method thereof
CN107194345A
Piezoelectric element and method of manufacturing the same
JP2018170343A
Ultrasonic sensor, ultrasonic device, and method for manufacturing ultrasonic sensor
JP2019146020A
Ultrasonic sensor
JP2019165307A
Ultrasonic sensor
US20200055088A1