Reinforced thermoplastic molding composition

The polyamide molding composition, with optimized polyamide, glass fibers, and glass flakes, addresses the challenge of maintaining mechanical and surface properties in both dry and conditioned states, achieving high tensile modulus, breaking stress, and impact resistance with consistent gloss.

JP7568418B2Active Publication Date: 2024-10-16EMS PATENT AG
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2020072760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-16
Filing Date
2020-04-15
Publication Date
2024-10-16
Estimated Expiration
2040-04-15

AI Technical Summary

Technical Problem

Existing polyamide molding compositions lack simultaneous good mechanical properties and surface properties in both dry and conditioned states, particularly in terms of impact resistance, stiffness, strength, and gloss, with existing technologies not adequately addressing these requirements.

Method used

A polyamide molding composition comprising specific ratios of polyamide, glass fibers, and glass flakes, along with a heat stabilizer, optimized to achieve high impact resistance, stiffness, and strength, with minimal change in properties between dry and conditioned states, and improved gloss.

Benefits of technology

The composition maintains excellent mechanical properties and surface quality under varying conditions, ensuring high tensile modulus, breaking stress, and impact resistance, with gloss remaining consistent in both dry and conditioned states.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568418000001
    Figure 0007568418000001
  • Figure 0007568418000002
    Figure 0007568418000002
  • Figure 0007568418000003
    Figure 0007568418000003
Patent Text Reader

Abstract

To provide a polyamide molding composition better than the prior art.SOLUTION: A polyamide molding composition comprises the following components: (A) 28.0-64.9 mass% of at least one polyamide; (B) 15.0-40.0 mass% of glass fibers; (C) 15.0-35.0 mass% of glass flakes having a particle thickness in the range of 0.3-2.0 μm; (D) 0.1-2.0 mass% of a heat stabilizer; and (E) 0-5.0 mass% of additives; with the proviso that the sum of the components (B) and (C) is in the range of 35.0 to 65.0 mass%, based on the sum of the components (A) to (E), and the sum of the components (A) to (E) makes 100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass-fiber-reinforced polyamide molding composition having good mechanical properties in the dry and conditioned state and good surface properties. [Background technology]

[0002] US3499955 describes the possibility of using glass fibres and glass flakes together with a crosslinking agent in a partially thermoplastic moulding composition, the aim being to be as steam-free as possible, the matrix being subsequently crosslinked. WO-A-94 / 22942 discloses polyamide molding compositions mixed with glass fibres and glass flakes. The matrices disclosed are only aliphatic polyamides, and surface and mechanical properties are reported, but no comparison between the dry and conditioned states is included. EP-A-0741762 is directed to glass fiber reinforced polyamide molding compositions based in part on a mixture of polyamide 66 and polyamide 6T / DT. Both the mechanical and surface properties are given in the dry state, with no comparison to the conditioned state. DE-A-10352319 discloses polyamide molding compositions containing glass fibers and further particulate fillers, which are weather-resistant and jet-black and are pigmented with carbon black. Small particulate fillers with a minimum diameter of 30 μm are preferably used. As the examples show, the appearance and weather resistance of the molded parts are substantially determined by the properties of the carbon black used. US-A-2008 / 0119603 describes a polyamide-based material for telephone housings that contains glass fibres and glass flakes. No data are disclosed on the surface or mechanical behaviour in the dry state compared to the conditioned state. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] US3499955 [Patent Document 2] WO-A-94 / 22942 [Patent Document 3] EP-A-0741762 [Patent Document 4] DE-A-10352319 [Patent Document 5] US-A-2008 / 0119603 Summary of the Invention

[0004] It is therefore an object of the present invention to provide a polyamide molding composition which is improved over the prior art. In particular, the aim is to achieve good mechanical properties and good surface properties, preferably in the dry and conditioned state. The molding composition preferably has high impact resistance, including under humid conditions, with sufficient stiffness and strength, and also has good surface quality. This means in detail that the tensile modulus in the dry state is preferably at least 15000 MPa, and in the conditioned state is not more than 1500 MPa, or more than 1100 MPa below the value in the dry state. Additionally or alternatively, the breaking stress in the dry state is preferably at least 150 MPa, preferably at least 200 MPa, and in the conditioned state is not more than 50 MPa, or more than 40 MPa below the value in the dry state. Additionally or alternatively, the impact resistance in the dry state is preferably at least 50 kJ / m 2 or at least 60 kJ / m 2 and 15 kJ / m in the adjusted state. 2 or less than 12 kJ / m on a dry basis 2 These conditions for tensile modulus, stress at break and impact resistance preferably hold simultaneously. In the context of mechanical properties, conditioning means that the specimens were stored at 72° C. and 62% relative humidity for 14 days before each measurement. Additionally, the gloss, measured preferably at an angle of 60° in the dry state (DAM) and after conditioning (80° C., 80% relative humidity, 120 hours), is at least 70%. This object is achieved by a polyamide moulding composition according to claim 1.

[0005] The subject of the present invention is therefore a composition comprising (A) 28.0 to 64.9% by mass of at least one polyamide, (B) 15.0 to 40.0 mass% glass fiber, (C) 15.0 to 35.0 mass % of glass flakes having a particle thickness in the range of 0.3 to 2.0 μm, in particular 0.4 to 1.7 μm; (D) 0.1 to 2.0 mass % of a heat stabilizer, (E) 0 to 5.0 mass% of additives A polyamide molding composition comprising: A polyamide molding composition, provided that the total of components (B) and (C) is in the range of 35.0 to 65.0% by mass based on the total of components (A) to (E), where the total of components (A) to (E) is 100% by mass.

[0006] The total of components (B) and (C) is preferably in the range of 40.0 to 60.0 mass %, more preferably in the range of 42.0 to 57.0 mass % or 45.0 to 55.0 mass %, based on the total of components (A) to (E) in each case. The molding composition is preferably free of impact modifiers, ie, (E) does not contain any impact modifiers. Component (A): Component (A) is composed of at least one polyamide, preferably at least one semicrystalline aliphatic or semiaromatic polyamide, or of a mixture of polyamides, more preferably a mixture of at least one semicrystalline polyamide and at least one amorphous or microcrystalline polyamide. The polyamide molding composition contains at least one polyamide (A), preferably in an amount of 34.0 to 59.8% by weight, particularly preferably 38.2 to 57.8 or 41.5 to 54.7% by weight, based in each case on the total of the components (A) to (E). The notations and abbreviations used herein for polyamides and their monomers are specified in the ISO standard ISO 16396-1:2015. Thus, inter alia, the following abbreviations are used for diamines: MXD stands for m-xylenediamine, MPMD stands for 2-methyl-1,5-pentanediamine, MOD stands for 2-methyl-1,8-octanediamine, MACM stands for bis(4-amino-3-methyl-cyclohexyl)methane, PACM stands for bis(4-amino-cyclohexyl)methane, TMDC stands for bis(4-amino-3,5-dimethyl-cyclohexyl)methane, Bac stands for 1,3-bis(aminomethyl)cyclohexane, ND stands for 2,2,4-trimethylhexamethylenediamine, and IND stands for 2,4,4-trimethylhexamethylenediamine.

[0007] The present invention encompasses both polyamides with a balanced end group ratio of carboxyl and amino groups, and polyamides with an unbalanced end group ratio of carboxyl and amino groups, i.e., with an excess of amino or carboxyl end groups. To provide polyamides with specific end group structures, it is preferred to use, for example, an excess of diamine or dicarboxylic acid in the preparation, especially in the molar ratio of diamine to dicarboxylic acid in the range of 0.90-1.10, more preferably 0.94-1.06, and very preferably 0.97-1.03. Therefore, it is preferred to use monofunctional adducts of amines and monocarboxylic acids to adjust the end groups of the polyamide. The amounts of monomers should be understood to mean that the corresponding molar ratios of monomers used in polycondensation are also found in the polyamides prepared accordingly by polycondensation. When lactams or amino carboxylic acids are used, there is no excess of one component. Instead, the amine or carboxylic acid is carefully added to the starting material to adjust the end group ratio. In one preferred embodiment, the at least one polyamide (A) is selected from the group consisting of semicrystalline and amorphous polyamides, or mixtures thereof. The at least one polyamide (A) is preferably a semicrystalline polyamide or a mixture of semicrystalline polyamides. It is also preferred to design component (A) as a mixture of a semicrystalline polyamide and an amorphous polyamide. A mixture of at least two amorphous polyamides is also suitable as component (A).

[0008] Semicrystalline polyamides as referred to herein differ from amorphous polyamides in that they have a pronounced melting point (or melting temperature), which can be determined, for example, by heating the melt using differential scanning calorimetry (DSC). Semicrystalline plastics may have, for example, a crystalline fraction of 10-80% and may have both a glass transition temperature below which the amorphous phase freezes out and a melting temperature below which the crystalline phase melts. The melting point of semicrystalline polyamides is preferably in the range of 160-330°C, more preferably in the range of 170-300°C, and more particularly in the range of 175-280°C, in each case determined according to ISO 11357-3:2013 at a heating rate of 20 K / min. Semicrystalline polyamides preferably have an enthalpy of fusion of >30 J / g, determined according to ISO 11357-3:2013. In contrast, the amorphous polyamides referred to herein do not have a determinable melting point, but only a glass transition temperature. Semicrystalline polyamides differ from amorphous polyamides in that they are opaque, whereas amorphous polyamides are transparent. Amorphous polyamides preferably exhibit a heat of fusion of less than 5 J / g in differential scanning calorimetry (DSC) according to ISO11357-3:2013 at a heating rate of 20 K / min. Amorphous polyamides do not have a melting point due to their amorphous nature.

[0009] The microcrystalline polyamides referred to herein can be considered as a combination of semicrystalline and amorphous polyamides. They are semicrystalline polyamides and therefore have a melting point. However, their morphology is such that the crystallite diameter is so small that the plates produced are still transparent even with a thickness of 2 mm, i.e. the light transmission measured according to ASTM D 1003:2013 is at least 75%. In differential scanning calorimetry (DSC) according to ISO 11357-3:2013 at a heating rate of 20 K / min, the microcrystalline polyamides preferably exhibit a heat of fusion of 5 to 30 J / g. When polyamides are referred to herein as microcrystalline, they are in fact essentially semicrystalline but have the heat of fusion indicated above. The glass transition temperature of the amorphous or microcrystalline polyamide is preferably 40-220°C, more preferably 60-200°C, very preferably 100-170°C, measured according to ISO 11357-2:2013 at a heating rate of 20 K / min.

[0010] For the purposes of the preferred embodiments of the present invention, preferred semicrystalline polyamides on the one hand and, collectively, preferred amorphous and microcrystalline polyamides are considered below. Exemplary particularly preferred semicrystalline polyamides (A1: aliphatic, A2: semi-aromatic) are herein designated PA 46, PA 49, PA 410, PA 411, PA 412, PA 413, PA 414, PA 415, PA 416, PA 418, PA 436, PA 56, PA 510, PA 66, PA 69, PA 610, PA 611, PA 612, PA 613, PA 614, PA 615, PA 616, PA 617, PA 618, PA 1010, PA 1011, PA 1012, PA 1013, PA 1014, PA 1015, PA 1016, PA 66 / 6, PA 6 / 66 / 610, PA 6 / 66 / 12, PA 6 / 12, PA 11, PA 12, PA 912, PA 1212, PA MXD6, PA MXD9, PA MXD10, PA MXD11, PA MXD12, PA MXD13, PA MXD14, PA MXD15, PA MXD16, PA MXD17, PA MXD18, PA MXD36, copolyamides thereof or mixtures, blends or alloys thereof, polyamides having 4T repeat units, polyamides having 5T repeat units, polyamides having 6T repeat units, polyamides having 8T repeat units, polyamides having 9T repeat units, polyamides having 10T repeat units, PA 4T / 6T, PA 4T / 8T, PA 6T / 8T, PA 4T / MPMDT, PA 4T / 4I, PA 5T / 5I, PA 6T / 6I, PA 9T, PA 9T / MODT, PA 9T / 9I, PA 10T, PA 10T / 6T, PA 10T / 610, PA 10T / 612, PA 10T / 11, PA 10T / 12, PA 10T / 6T / 10I / 6I, PA 12T, PA MPMDT / 6T, PA 6T / 6I(>50mol% 6T), PA 10T / 10I, PA 12T / 12I, PA 4T / 6T / 8T, PA 4T / 6T / 10T, PA 4T / 8T / 10T, PA6T / 8T / 10T, PA 4T / 6T / MPMDT, PA 6T / 6, PA 6T / 66, PA 4T / 66, PA 5T / 66, PA 6T / 6I / 6, PA 66 / 6I / 6T, PA 10T / 6T / 1012 / 612, PA 6T / BacT / Bac6 / 66, PA 6T / 610 / BacT / Bac10, PA6T / 612 / BacT / Bac12, PA 6T / BacT / 6I / BacI, polyetheramides, polyetheresteramides, polyesteramides, and mixtures or copolymers thereof.

[0011] Copolyamide in the above sense refers to a polyamide having a plurality of the stated monomer units. The relative viscosity of the semi-crystalline polyamides (A1) and (A2), measured on a solution of 0.5 g polyamide in 100 ml m-cresol at 20° C. according to ISO 307:2013, is preferably 1.40 to 2.70, more preferably 1.50 to 2.40, very preferably 1.60 to 2.20.

[0012] The amount of oxygen (A3) in PA 6I / 6TPA (65% I / 60% IPA) 6I / 6T / 6N、PA MXDI / 6I、PA MXDI / MXDT / 6I / 6T、PA MXDI / 12I、PA MXDI、PA MXDI / MXD6、PA MACM10、PA MACM12 PA MACM14、PA MACM18、PA MXDI / MXDT / PAD TMDC10、PA TMDC12、PA TMDC14、PA TMDC18、PA PACM12、PA PACM14、PA PACM18、PA PACM10 / 11、PA PACM10 / 12、PA PACM12 / 612、PACM12 / PACM12 / 614 / PACM14 MACMI / 12、PA MACMT / 12、PA MACMI / MACM12、PA MACMI / MACMN、PA MACMT / MACM12、PA MACMT / MACMN、PA MACM36、PA TMDC36、PA MACMI / MACM36、PA MACMI / MACM36、PA MACMI / MACM12、PA MACMT / MACM36、PA MACMI / MACMT / 12、PA 6I / 6T / MACMI / MACMT、PA 6I / 6T / MACMI / MACMT / 12、PA MACM6 / 11、PA MACM6 / 12、PA MACM10 / 11、PA MACM10 / 12、PA MACM10 / 1010、PA MACM12 / 1012、PA MACM12 / 1212、PA MACM14 / 1014、PA MACM14 / 1214、PA MACM18 / 1018、PA 6I / 6T / MACMI / MACMT / MACM12 / PACM12、 6I / 6T / MACMI / MACMT / MACM12、PA MACMI / MACMT / MACM12 / 12、PA MACMI / MACMT / MACM12、PA 6I / 6T / MACMI / MACMT / 12、PA 6I / 6T / 6N / MACMI / MACMT / MACM1、PACM TMDC12 / TMDCT / TMDC36、PA TMDC12 / TMDCI、PA TMDC12 / TMDCI / TMDC36、よびPAIt is preferred that the MACM is selected from the group consisting of TMDC12 / TMDCT and mixtures or copolymers thereof, in which the MACM may be completely replaced, preferably up to 50 mol %, more particularly up to 35 mol %, by PACM and / or TMDC and / or the laurolactam may be totally or partially replaced by caprolactam. The above mentioned systems PA 6T / 6I(A2, semi-crystalline) and PA 6I / 6T(A3, amorphous) differ in that in the former polyamide the proportion of 6T repeat units is greater than that of 6I repeat units, while the opposite is true for the latter polyamide.

[0013] Particularly preferred are polyamides 66, 610, 612, 10T / 6T, 66 / 6I / 6T, 6T / 66 / BacT / Bac6, 6I / 6T, also MACMX and PACMX with X=10 to 16, and also polyamides 11 and 12. Very particular preference is given to PA 66, PA 66 / 6I / 6T, PA 6T / 66 / BacT / Bac6, PA 6I / 6T / MACMI / MACMT / MACM12 / 612 and PA 10T / 6T. The relative viscosity of the amorphous or microcrystalline polyamide A3, measured on a solution of 0.5 g polyamide in 100 ml m-cresol at 20° C. according to ISO 307:2013, is preferably 1.35 to 2.20, more preferably 1.40 to 2.10, very preferably 1.45 to 2.00 and particularly preferably 1.50 to 1.90. Component (A) may also comprise a mixture of semicrystalline polyamides (A1) and / or (A2) and amorphous and / or microcrystalline polyamides (A3), in which case the proportion of semicrystalline polyamides in component (A) is in each case preferably in the range from 30.0 to 98.0% by weight, more preferably in the range from 40.0 to 95.0% by weight, very preferably in the range from 50.0 to 90.0% by weight, based on the total weight of component (A).

[0014] These mixtures of semicrystalline polyamides (A1) and / or (A2) with amorphous or microcrystalline polyamides (A3) are preferably selected from the group consisting of mixtures of PA 66 and PA 6I / 6T, mixtures of PA66 and PA 6T / 66 / BacT / Bac6, mixtures of PA66 and PA 6I / 6T / MACMI / MACMT / MACM12 / 612, mixtures of PA 66 / 6I / 6T and PA 6I / 6T, mixtures of PA 66 / 6I / 6T and PA 6T / 66 / BacT / Bac6, mixtures of PA12 and PA MACM12, mixtures of PA12 and PA PACM12, and mixtures of PA66 and PA 6T / 66 / BacT / Bac6 and PA 6I / 6T / MACMI / MACMT / MACM12 / 612. In another particularly preferred embodiment of the polyamide molding composition of the invention, component (A) comprises a mixture of at least one semicrystalline aliphatic polyamide (A1) and at least one semicrystalline semiaromatic polyamide (A2) based on the diamines 1,6-hexanediamine and bis(aminomethyl)cyclohexane, in particular 1,3-bis(aminomethyl)cyclohexane, and further based on the dicarboxylic acids terephthalic acid, isophthalic acid and / or two or more aliphatic dicarboxylic acids having 6 to 18 carbons. Particularly preferred aliphatic polyamides (A1) are PA66, PA610 and PA612, particularly preferred semiaromatic polyamides (A2) are 6T / 66 / BacT / Bac6, 6T / 610 / BacT / Bac10, 6T / 612 / BacT / Bac12 and 6T / BacT / 6I / BacI.

[0015] In another particularly preferred embodiment of the polyamide molding composition of the invention, component (A) comprises a semicrystalline polyamide (A1) or (A2) or a mixture thereof. Particular preference is given to the polyamides PA 66, PA 610, PA 612, PA 10T / 6T, PA 66 / 6I / 6T, PA 6T / 66 / BacT / Bac6, PA 6T / 610 / BacT / Bac10, PA 6T / 612 / BacT / Bac12, 6T / BacT / 6I / BacI, as well as mixtures thereof, with a relative viscosity in the range from 1.60 to 2.30. In another particularly preferred embodiment of the polyamide molding composition of the invention, component (A) comprises a mixture of semicrystalline polyamides (A1) and / or (A2) with amorphous or microcrystalline polyamides (A3), in which case, as semicrystalline polyamides (A1), PA 66, PA 610, PA 612, PA 616, PA12 with a relative viscosity in the range of 1.60 to 2.30, as polyamides (A2), PA 10T / 6T and PA 66 / 6I / 6T, and as amorphous or microcrystalline polyamides (A3), PA 6I / 6T, PA 6I / 6T / MACMI / MACMT / MACM12 / 612, PA MACM12 and PA PACM12 are particularly preferred.

[0016] According to the invention, the following polyamide mixtures are therefore particularly preferred as polyamides of component (A): Mixture (i): (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A3) 10 to 50 mass % of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol % of hexamethylene isophthalamide units and 15 to 45 mol % of hexamethylene terephthalamide units; (wherein the fractions (A1) and (A3) constitute 100% by weight of the polyamide mixture (A)).

[0017] Mixture (ii): (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 10 to 50% by weight of the semi-crystalline, semi-aromatic polyamide 6T / 66 / BacT / Bac6, 6T / 6I / BacT / BacI or 6T / 66 / 6I / BacT / Bac6 / BacI, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, in particular 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and further 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction. and (wherein the fractions (A1) and (A2) constitute 100% by weight of the polyamide mixture (A)). Mixture (iii): (A2) 50 to 90% by mass of semi-crystalline semi-aromatic polyamide 10T / 6T; (A3) 10 to 50 mass % of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol % of hexamethylene isophthalamide units and 15 to 45 mol % of hexamethylene terephthalamide units; (wherein the fractions (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)).

[0018] Mixture (iii): (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 8 to 30% by weight of a semi-crystalline, semi-aromatic polyamide PA 6T / BacT / 66 / Bac6, 6T / BacT / 6I / BacI or 6T / BacT / 6I / BacI / 66 / Bac6, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, in particular 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid and further 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction, (A3) 2-20% by weight of amorphous polyamide 6I / 6T / 612 / MACMI / MACMT / MACM12 (wherein the composition preferably contains 18-30 mol% each of 6I and 6T units, 12-26 mol% of 612 units, and further 6-16 mol% each of MACM12, MACMI and MACMT units, where the sum of all PA units is 100 mol%); (wherein the fractions (A1), (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)).

[0019] The polyamide molding composition necessarily contains, in the form of component (B), a fibrous reinforcing material in the form of glass fibers in a proportion of at least 15.0 and at most 40.0 percent by weight. According to one preferred embodiment, the polyamide molding composition is characterized in that component (B) is present in a proportion in the range of 17.0 to 35.0% by mass, preferably in the range of 18.0 to 32.0% by mass or 20.0 to 30.0% by mass, based on the sum of components (A) to (E). In this case, the glass fibers (B) may have a circular cross section, particularly preferably with a diameter in the range from 5 to 20 μm, or in the range from 5 to 13 μm or 6 to 10 μm, or a noncircular cross section, in which case the dimensional ratio of the main cross-sectional axis to the secondary cross-sectional axis perpendicular thereto is preferentially greater than 2.5, particularly preferably in the range from 2.5 to 6 or 3 to 5. The glass fibers (B) can be used, for example, in the form of short fibers (e.g., chopped glass having a length of 0.2 to 20 mm) or continuous filament fibers (rovings). The glass fibers (B) can have various cross sections, with circular cross sections (round fibers) and non-circular cross sections (flat fibers) being preferred.

[0020] Glass fibers with a circular cross section, i.e. round glass fibers, have a diameter preferentially in the range of 5 to 20 μm, preferably in the range of 5 to 13 μm, more preferably in the range of 6 to 10 μm. The glass fibers are preferably used in the form of short glass fibers (chopped glass with a length of 0.2 to 20 mm, preferably 2 to 12 mm). In the case of flattened glass fibers, i.e. glass fibers with a noncircular cross section, preference is given to using glass fibers whose dimensional ratio of the main cross-sectional axis to the secondary cross-sectional axis perpendicular thereto is greater than 2.5, preferably in the range from 2.5 to 6, in particular in the range from 3 to 5. These so-called flattened glass fibers have an oval, elliptical, elliptical with one or more waists (so-called cocoon fibers), polygonal, rectangular or approximately rectangular cross section. A further preferred characteristic configuration of the flattened glass fibers used is that the length of the main cross-sectional axis is preferably in the range from 6 to 40 μm, in particular in the range from 15 to 30 μm, and the length of the secondary cross-sectional axis is in the range from 3 to 20 μm, in particular in the range from 4 to 10 μm. At the same time, the flattened glass fibers have a very high packing density, which means that the cross section of the glass fills an imaginary rectangle and surrounds the cross section of the glass fiber as accurately as possible to the extent of at least 70%, preferably at least 80%, particularly preferably at least 85%.

[0021] To reinforce the molding composition of the invention, it is also possible to use a mixture of glass fibers with a circular cross section and glass fibers with a non-circular cross section, in which case the proportion of flat glass fibers preferentially predominates, i.e. represents more than 50% by weight of the total fiber weight. Preferably, component (B) is selected from the group consisting of: E-glass fibres (according to ASTM D578-00, consisting of 52-62% silicon dioxide, 12-16% aluminium oxide, 16-25% calcium oxide, 0-10% borax, 0-5% magnesium oxide, 0-2% alkali metal oxides, 0-1.5% titanium dioxide and 0-0.3% iron oxide, preferably with a density of 2.58±0.04 g / cm 3 , tensile modulus of elasticity 70-75 GPa, tensile strength 3000-3500 MPa, elongation at break 4.5-4.8%), A-glass fiber (63-72% silicon dioxide, 6-10% calcium oxide, 14-16% sodium and potassium oxide, 0-6% aluminum oxide, 0-6% boron oxide, 0-4% magnesium oxide), C-glass fiber (64-68% silicon dioxide, 11-15% calcium oxide, 7-10% sodium and potassium oxide, 3-5% aluminum oxide, 4-6% boron oxide, 2-4% magnesium oxide), D-glass fiber (72-75% silicon dioxide, 0-1 % calcium oxide, 0-4% sodium and potassium oxides, 0-1% aluminum oxide, and 21-24% boron oxide), basalt fibers (mineral fibers with the following approximate composition: 52% SiO2, 17% Al2O3, 9% CaO, 5% MgO, 5% Na2O, 5% iron oxide, plus other metal oxides), AR-glass fibers (55-75% silicon dioxide, 1-10% calcium oxide, 11-21% sodium and potassium oxides, 0-5% aluminum oxide, 0-8% boron oxide, 0-12% titanium dioxide, 1-18% zirconium oxide, and 0-5% iron oxide), and mixtures of these.

[0022] One preferred embodiment of component (B) is a high-strength glass fiber based on a ternary system of silicon dioxide-aluminum oxide-magnesium oxide or a quaternary system of silicon dioxide-aluminum oxide-magnesium oxide-calcium oxide, in which the sum of the amounts of silicon dioxide, aluminum oxide and magnesium oxide is at least 78% by weight, preferably at least 87%, more preferably at least 92%, based on the total glass composition. For example, a composition of 58-70% by weight of silicon dioxide (SiO2), 15-30% by weight of aluminum oxide (Al2O3), 5-15% by weight of magnesium oxide (MgO), 0-10% by weight of calcium oxide (CaO) and 0-2% by weight of further oxides, such as zirconium dioxide (ZrO2), boron oxide (B2O3), titanium dioxide (TiO2) or lithium oxide (Li2O), is particularly preferably used. In another embodiment, the high strength glass fibers have a composition of 60-67% by weight silicon dioxide (SiO2), 20-28% by weight aluminum oxide (Al2O3), 7-12% by weight magnesium oxide (MgO), 0-9% by weight calcium oxide (CaO), and 0-1.5% by weight of additional oxides, such as zirconium dioxide (ZrO2), boron oxide (BO3), titanium dioxide (TiO2), lithium oxide (Li2O), etc.

[0023] In particular, it is preferred that the high-strength glass fibres have the following composition: 62-66% by weight of silicon dioxide (SiO2), 22-27% by weight of aluminium oxide (Al2O3), 8-12% by weight of magnesium oxide (MgO), 0-5% by weight of calcium oxide (CaO), 0-1% by weight of further oxides such as zirconium dioxide (ZrO2), boron oxide (B2O3), titanium dioxide (TiO2), lithium oxide (Li2O), etc. The high strength glass fibers have a tensile strength of 3700 MPa or more, preferably at least 3800 or 4000 MPa, an elongation at break of at least 4.8%, preferably at least 4.9 or 5.0%, and a tensile modulus of greater than 75 GPa, preferably greater than 78 or 80 GPa, with these glass properties being determined using individual fibers (original monofilaments) with a diameter of 10 μm and a length of 12.7 mm at a temperature of 23° C. and a relative humidity of 50%. Specific examples of these high strength glass fibers of component (B1) are S-glass fiber of size 995 from Owens Corning, T-glass fiber from Nittobo, HiPertex from 3B, HS4-glass fiber from Sinoma Jinjing Fiberglass, R-glass fiber from Vetrotex, and S-1- and S-2-glass fibers from AGY.

[0024] The glass fibers used in the form of rovings (continuous filament fibers) have, for example, preferentially, a diameter (in the case of round glass fibers) or a secondary cross-sectional axis (in the case of flattened glass fibers) of 6 to 20 μm, preferably 12 to 18 μm, the cross section of the glass fibers can be round, oval, elliptical, elliptical with single or multiple waists, polygonal, rectangular or approximately rectangular. Particularly preferred are so-called flattened glass fibers, whose cross-sectional axis ratio, i.e. the ratio of the main cross-sectional axis to the secondary cross-sectional axis, is 2.5 to 5. The continuous filament fibers can be produced from the various glasses mentioned above, with preference being given to continuous filament fibers based on E-glass and various high-strength glasses. These continuous filament fibers are incorporated into the polyamide molding composition of the invention by known methods for producing elongated long-fiber reinforced pellets, in particular by the pultrusion process, in which a continuous filament fiber strand (roving) is completely saturated with a polymer melt and then cooled and chopped. The elongated long fiber reinforced pellets thus obtained, preferably with a pellet length of 3 to 25 mm, in particular 4 to 12 mm, can be further processed into shaped parts by customary processing methods (e.g. injection molding, compression molding, etc.).

[0025] As component (B), preference is given to glass fibres of E-glass having a non-circular cross section (flat fibres) and an axial ratio of the main cross section axis to the secondary cross section axis of at least 2.5, and / or high-strength glass fibres having a circular or non-circular cross section, as well as glass composites substantially based on silicon dioxide, aluminium oxide and magnesium oxide components, the proportion of magnesium oxide (MgO) being 5-15% by weight and the proportion of calcium oxide being 0-10% by weight. In the form of flat E-glass fibers, the glass fibers of component (B) preferably have a density of 2.54 to 2.62 g / cm 3 , tensile modulus of 70-75 GPa, tensile strength of 3000-3500 MPa, and elongation at break of 4.5-4.8%. These mechanical properties are determined using individual fibers with a diameter of 10 μm and a length of 12.7 mm at 23 °C and 50% relative humidity.

[0026] As component (B), E-glass glass fibers having a circular cross section (round fiber) and a diameter in the range of 6 to 10 μm are particularly preferred. The glass fibers of the present invention may be provided in sizes suitable for thermoplastic resins, particularly polyamides, that contain adhesion promoters based on aminosilane or epoxysilane compounds. The polyamide molding composition preferably contains 16.0 to 33.0 mass %, more preferably 18.0 to 32.0 mass %, and more preferably 20.0 to 30.0 mass % of glass flakes (component (C)), in each case based on the total of components (A) to (E). The particle thickness of the glass flakes of component (C) is preferably in the range of 0.4 to 1.7 μm, more preferably in the range of 0.5 to 1.6 μm, and particularly preferably in the range of 0.5 to 1.5 μm. The particle thickness of the glass flakes preferably means the average particle thickness. This average particle thickness is obtained as the arithmetic mean by determining the thickness by scanning electron microscopy using at least 100 individual glass flakes. With regard to the variation width of the particle thickness, it is further preferred that at least 50% by mass, in particular at least 70% by mass of the glass flakes are included in the particle thickness range from half the average particle thickness (0.5 × average particle thickness) to 1.5 times the average particle thickness (1.5 × average particle thickness). Thus, glass flakes of component (C) having an average particle thickness in the range of 0.3 to 2.0 μm, more preferably in the range of 0.4 to 1.7 μm, more preferably in the range of 0.5 to 1.6 μm, and particularly preferably in the range of 0.5 to 1.5 μm are preferred.

[0027] Glass flakes are thin, transparent, irregularly shaped, plate-like pieces of glass with a wide particle size distribution and a high aspect ratio (ratio of average particle size to particle thickness). The particle thickness of a single glass flake has minimal variation. The particle size of the individual glass particles is typically 10-2000 or 10-4000 μm, with an average particle size (D50) ranging from 20-300, 30-300, or 15-600 μm. It should be understood that this dimension and the dimensions mentioned above are based on the glass flakes in the starting material and / or molding composition. Conventional glass flakes, which are mainly used in paints or coatings for anticorrosive or reinforced plastics, have a thickness of 3-7 μm. Glass flakes are produced, for example, by breaking glass bubbles or by crushing a liquid glass melt in a centrifuge, followed by grinding ribbon-like glass pieces. Glass flakes are characterized based on the particle size distribution, average particle size, and thickness of the glass particles. Furthermore, the glass flakes can be produced from a variety of different glasses, such as E-glass, S-glass, ECR-glass and C-glass. A typical representative of thick glass flakes is Microglas REF-160A from NGF Europe, where the particle size distribution is as follows: 10% of the glass particles are 300-1700 μm in diameter, 65% are in the range of 45-300 μm in diameter and 25% are below 45 μm in particle size. Here, the thickness is 5 μm. The type of glass used is E-glass. The glass flakes can be surface coated in various sizes, for example with aminosilanes or epoxysilanes, to improve their adhesion to the polymer matrix.

[0028] The glass flakes used in the present invention preferably have an average particle size and particle size distribution approximately as described above, but due to the relatively large aspect ratio, the particle thickness is much smaller. The thickness of the glass flakes of the present invention is only 0.3 to 2.0 μm. These very thin glass flakes are currently used only in the field of cosmetics and virtually exclusively in pigment coatings for vehicles. An example of this kind of very thin glass flake is E-glass type MEG160FY-M03 from Nippon Sheet Glass Co. (Japan) with an average particle size (d50) of 160 μm, a thickness of 0.7 μm, and a particle size distribution with 20% of the glass particles in the range of 2000-1400 μm, 60% in the range of 150-1400 μm, and 20% smaller than 150 μm, coated with 3-aminopropyltriethoxysilane, or E-glass flake type GF100E-A from Glass Flake Ltd. with an average particle size of 160 μm, 80% of the glass particles in the range of 150-1700 μm, and 20% smaller than 150 μm, a particle thickness of 1.0-1.3 μm, coated with 3-aminopropyltriethoxysilane. Also suitable is ECR-glass flake type GF100MECR-A from Glass Flake Ltd., with an average particle size of 120 μm, a particle size distribution with 10% of the glass particles in the range 300-1000 μm, 65% in the range 50-300 μm, and 25% smaller than 50 μm, a particle thickness of 1.0-1.3 μm, and coated with 3-aminopropyltriethoxysilane.

[0029] Preferably herein the glass flakes consist of E-, S-, C- or ECR-glass, with glass flakes of E-glass being particularly preferred. The glass flakes may have different particle sizes depending on whether they are crushed, micronized or uncrushed. An average particle size (D50) of 20-300 μm, more preferably 50-200 μm, particularly preferably 80-170 μm is preferred. The average particle sizes stated for the glass flakes are based on the raw materials (component (C)) and / or the finished molding composition used and were determined using laser diffraction particle size analysis. The glass flakes used are preferably provided with a coating based on aminosilanes, vinylsilanes, epoxysilanes or acrylosilanes, with a surface coating with aminosilanes being particularly preferred. The amount of silane is preferably 0.1-1.0% by weight, more preferably 0.3-0.9% by weight, based on the amount of glass flakes.

[0030] The polyamide molding composition further comprises a heat stabilizer in the form of component (D), distinct from the other constituents (B), (C) and (E), in a proportion of 0.1 to 2.0 percent by weight. Component (D) is preferentially present in a proportion in the range of 0.2 to 2.0% by weight, particularly preferably in the range of 0.2 to 1.8 or 0.3 to 1.5% by weight, relative to the sum of components (A) to (E). According to one preferred embodiment, component (D) may be selected from the following group: Compounds of mono- or divalent copper, in particular salts of mono- or divalent copper with inorganic or organic acids or with mono- or divalent phenols, oxides of mono- or divalent copper, or complex compounds of copper salts with ammonia, amines, amides, lactams, cyanides or phosphines, preferably the Cu(I) or Cu(II) salts of hydrohalic acids, of hydrocyanic acid or of copper salts of aliphatic carboxylic acids, very preferably the monovalent copper compounds CuCl, CuBr, CuI, CuCN and Cu2O, and also the divalent copper compounds CuCl2, CuSO4, CuO, copper(II) acetate or copper(II) stearate, or mixtures of these compounds, where these copper compounds are used on their own or, preferentially, in the form of concentrates. In this specification, concentrate refers to a polymer containing a high concentration of copper salts or copper compounds, preferably having the same or substantially the same chemical properties as component (A). In particular, preferentially, the copper compound is used in combination with further metal halides, including alkali metal halides, such as NaI, KI, NaBr, KBr, where the molar ratio of metal halide to copper is between 0.5 and 20, preferably between 1 and 10, more preferably between 2 and 7; · Stabilizers based on secondary aromatic amines; · Stabilizers based on sterically hindered phenols; · Phosphites and phosphonites; · A mixture of the aforementioned stabilizers.

[0031] Thus, preferentially, the compounds of interest are compounds of mono- or divalent copper, such as salts of mono- or divalent copper with inorganic or organic acids or with mono- or divalent phenols, oxides of mono- or divalent copper, or complex compounds of copper salts with ammonia, amines, amides, lactams, cyanides or phosphines, preferably Cu(I) or Cu(II) salts of hydrohalic acids, of hydrocyanic acid or of copper salts of aliphatic carboxylic acids. The monovalent copper compounds CuCl, CuBr, CuI, CuCN and Cu2O, as well as the divalent copper compounds CuCl2, CuSO4, CuO, copper(II) acetate or copper(II) stearate are particularly preferred. The copper compound may be used on its own or in the form of a concentrate. A concentrate in this context is a polymer, preferably of the same chemical nature as component (A), containing a high concentration of copper salts. The copper compound is advantageously used in combination with other metal halides, in particular alkali metal halides, such as NaI, KI, NaBr, KBr, where the molar ratio of metal halide to copper is 0.5 to 20, preferably 1 to 10, more preferably 2 to 7. It is preferred to use a combination of CuI and KI in a total concentration of 0.1 to 0.7% by weight, in particular 0.2 to 0.5% by weight, based on the molding composition.

[0032] Likewise, stabilizers based on secondary aromatic amines are also contemplated, in which case the stabilizer is preferably present in an amount of 0.2 to 2, preferably 0.2 to 1.5% by weight. Furthermore, stabilizers based on sterically hindered phenols are contemplated, which are preferably present in an amount of 0.1 to 1.5, more preferably 0.2 to 1.0% by weight. Phosphites and phosphonites are also contemplated. Likewise, mixtures of the above mentioned heat stabilizers are contemplated. Particularly preferred examples of stabilizers based on secondary aromatic amines which may be used in the present invention are the adduct of phenylenediamine with acetone (Naugard A), the adduct of phenylenediamine with linolene, Naugard 445, N,N'-dinaphthyl-p-phenylenediamine, N-phenyl-N'-cyclohexyl-p-phenylenediamine, or mixtures of two or more thereof.

[0033] Preferred examples of stabilizers based on sterically hindered phenols which can be used in the present invention are N,N'-hexamethylene-bis-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide, glycol bis(3,3-bis(4'-hydroxy-3'-tert-butylphenyl)butanoate), 2,1'-thioethyl bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), 4-4'-butylidene-bis-(3-methyl-6-tert-butylphenol), triethylene glycol 3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, or a mixture of two or more of these stabilizers.

[0034] Preferred phosphites and phosphonites are triphenyl phosphite, diphenyl alkyl phosphites, phenyl dialkyl phosphites, tris(nonylphenyl) phosphite, trilauryl phosphite, trioctadecyl phosphite, distearyl pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl) phosphite, diisodecyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite, diisodecyloxy pentaerythritol diphosphite, bis(2,4-di-tert-butyl-6-methylphenyl) pentaerythritol diphosphite, bis(2,4,6-tris(tert-butylphenyl) pentaerythritol diphosphite, tristearyl sorbitol Triphosphite, Tetrakis(2,4-di-tert-butylphenyl) 4,4'-biphenylene diphosphonite, 6-isooctyloxy-2,4,8,10-tetra-tert-butyl-12H-dibenzo[d,g]-1,3,2-dioxaphosphocin, 6-fluoro-2,4,8,10-tetra-tert-butyl-12-methyldibenzo[d,g]-1,3,2-dioxaphosphocin, Bis(2,4-di-tert-butyl-6-methylphenyl) Particularly preferred are tris[2-tert-butyl-4-thio(2'-methyl-4'-hydroxy-5'-tert-butyl)phenyl-5-methyl]phenyl phosphite and tris(2,4-di-tert-butylphenyl)phosphite (available as Hostanox® PAR24 from Clariant, Basel).

[0035] A preferred embodiment of the heat stabilizer is a combination of Irgatec NC 66 (available from BASF) and a copper stabilizer based on CuI and KI. Heat stabilizers based only on CuI and KI are particularly preferred. With the exception of the use of organic heat stabilizers and / or copper or copper compounds, the use of further transition metals or further transition metal compounds of groups VB, VIB, VIIB and / or VIIIB of the periodic table is preferably excluded. According to a further preferred embodiment, the heat stabilizer of component (D) is selected from the group of phenolic heat stabilizers, phosphite heat stabilizers, amine heat stabilizers, or mixtures or combinations thereof, component (D) being particularly preferably selected from the following group: triethylene glycol bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), N,N'-hexamethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionamide], tris(2,4-di-tert-butylphenyl)phosphite, or mixtures thereof.

[0036] Preferred organic stabilizers are phenolic and / or phosphite compounds, such as Irganox 245, Irganox 1010, Irganox 1098, Hostanox PAR 24 or Irgafos 168. Component (D) is preferably a mixture of 10 parts by weight of a mixture of Irganox 1010 (CAS 6683-19-8, phenolic antioxidant) and Anox 20 (CAS 6683-19-8, phenolic antioxidant) in a ratio of 7:3, and further 2 parts by weight of Hostanox PAR24 (CAS:31570-04-4, tris(2,4-di-tert-butylphenyl)phosphite), the concentration being 0.3-1.5% by weight based on the total of components (A)-(E). The polyamide moulding composition may also comprise further auxiliaries and / or additives in the form of component (E), which are distinct from the other constituents (A) to (D), preferably in a proportion of at most 4 percent by weight. According to one preferred embodiment, component (E) is present in a proportion in the range of 0 to 4.0 mass %, more preferably in the range of 0 to 3.0 mass %, particularly preferably in the range of 0 to 2.0 or 0.1 to 2.0 mass %, based on the sum of components (A) to (E). Component (E) is preferentially selected from the following group: crystallization accelerators or retarders, flow aids, lubricants, mold release agents, pigments, dyes, taggants, processing aids, antistatic agents, carbon black, graphite, carbon nanotubes, residues from the polymerization process such as catalysts, salts and their derivatives. Preferentially, component (E) does not comprise polyamides, in particular semi-crystalline, semi-aromatic, aliphatic, microcrystalline or amorphous polyamides, and does not comprise impact modifiers.

[0037] As already evident above, the proposed polyamide moulding compositions are characterised in that they are particularly suitable for applications in the automotive and electrical / electronics sectors, in particular when processed into shaped articles, preferably by injection moulding or extrusion. The invention therefore also relates to a shaped article produced from the above-mentioned polyamide molding composition, preferably by injection molding or extrusion, or having at least one region or coating of the above-mentioned polyamide molding composition. The thermoplastic molding compositions of the invention and the shaped articles produced therefrom are notable for their good mechanical properties and good surface properties in the dry and conditioned state, respectively. The shaped articles have good impact resistance with sufficient stiffness and strength, including under humid conditions, and also have good surface quality. The shaped articles of interest are preferably those for which good surface quality is important. More particularly, the shaped articles are Exterior The shaped articles are selected from the group consisting of parts and / or visible housings, covers or frames. These shaped articles can be manufactured by several methods, such as injection molding or injection compression molding, or by extrusion. They can also be further machined, such as by cutting, drilling, milling, laser marking, laser welding or laser cutting.

[0038] The polyamide molding compositions of the invention find application in the production of shaped articles, in particular parts of electrical or electronic components, parts of housings or parts of housing components, preferably housings or housing parts of portable electronic devices, panels or covers, household goods, household machines, eyeglass frames, eyeglass edgings, sunglasses, cameras, spectacles for hyperopia, decorative articles, devices and equipment for telecommunications and household appliances, interior and exterior parts in the field of the automotive segment and other means of transport, interior and exterior parts, preferably with a transport or mechanical function, in the fields of electrical goods, furniture, sports, mechanical engineering, sanitation and hygiene, medicine, energy and propulsion technology, particularly preferably mobile phones, smartphones, personal organizers, laptop computers, notebook computers, tablet computers, radios, cameras, timepieces, calculators, sensor housings, measuring devices, music or video playback devices, navigation devices, GPS devices, electronic photo frames, external hard drives and other electronic storage media. Further embodiments are set forth in the dependent claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] Preferred embodiments of the invention are described below with reference to examples which are merely illustrative and should not be construed as limiting. Preparation of the molding composition and test specimens: The molding compositions with the composition according to Tables 1 and 2 below were produced using a ZSK25 twin screw extruder from Werner u. Pfleiderer. The various polyamide pellets were mixed with the stabilizers and additives and metered into the inlet zone. The fillers (glass fibres, mica, kaolin, calcium carbonate, hollow glass beads and glass flakes) were metered into the polymer melt via a side feeder three-barrel unit in front of the die. The barrel temperature was set as an increasing profile up to 290°C (up to 320°C for PA-4 and PA-5). Compounding was carried out at 200 rpm with a throughput of 15 kg / h. The extruded strands were pelletized after cooling in a water bath and the pellets obtained were dried at 100°C for 24 hours. Test specimens were produced using an Arburg Allrounder 320-210-750 injection molding unit with the cylinder temperature set at 275-280 °C (up to 310 °C for PA-4 and PA-5) and the screw speed set at 250 rpm. The mold temperature was 100 °C (130 °C for PA-4 and PA-5).

[0040] Measurement of characteristics: Measurements were carried out using the following test specimens according to the following criteria: The test specimens in the dry state after injection moulding are stored in a dry environment, ie on silica gel, at room temperature for at least 48 hours. The conditioned specimens, with the exception of those for the gloss measurement, are stored for 14 days at 72° C. and 62% relative humidity according to DIN EN ISO 1110:1998. Thermal behavior, melting point (Tm), enthalpy of fusion (ΔHm) and glass transition temperature (Tg) were measured on pellets according to ISO standard 11357-1, -2 and -3 (2013-04). Differential scanning calorimetry (DSC) was performed at a heating rate of 20 K / min. The relative viscosity (ηrel) was determined according to DIN EN ISO 307 (2013-08) using a solution of 0.5 g of polymer in 100 ml of m-cresol at a temperature of 20° C. The samples were used in pellet form.

[0041] The tensile modulus, stress at break and elongation at break were determined in the dry and conditioned state at 23 °C using ISO tensile test specimens of type A1, 170 x 20 / 10 x 4 mm, according to ISO / CD 3167 (2014-11), at a tensile speed of 1 mm / min (tensile modulus) or 5 mm / min (stress at break, elongation at break) according to ISO 527 (2012-06). The Charpy impact resistance was determined in the dry and conditioned state according to ISO 179 / 2*eU (1997, *2 = instrumented) at 23 °C using ISO test specimens, type B1 (dimensions 80 x 10 x 4 mm) manufactured according to the ISO / CD 3167 (2003) standard. The gloss was determined according to ISO 2813 (2015-02) using a Minolta Multi Gloss 268 instrument with plates of dimensions 60 x 60 x 2 mm at an angle of 60° and a temperature of 23 °C. The gloss values ​​are reported in dimensionless gloss units (GU). The dry specimens were stored after injection molding in a dry environment, i.e. on silica gel, at room temperature for 48 h. For conditioning, the plates were stored at 85 °C and 85% relative humidity for 120 h.

[0042] [Table 1]

[0043] [Table 2]

[0044] [Table 3]

[0045] Discussion of results: The examples B1-B8 using the compositions according to the invention show consistently good mechanical properties (modulus, stress at break, elongation at break, impact resistance) with small differences between the dry and conditioned state. The good properties are also evident in particular in the gloss, which is consequently almost independent of whether the material is in the dry or conditioned state. These properties are demonstrated for various glass fiber contents as well as for glass fibers with a round cross section (type B) and for glass fibers with a flat cross section (type A). Flat glass fibers show better properties, especially in terms of gloss. The properties are also demonstrated in the examples for various polyamide matrix compositions, which give slightly different properties. Particularly good conditioned gloss values ​​are obtained for the mixtures of amorphous 6I / 6T and 10T / 6T (B7), and particularly good dry gloss values ​​are obtained for the matrix only with 66 / 6I / 6T (B6). In addition, the properties are demonstrated for various glass flake contents. The use of a high proportion of glass flakes can increase the modulus and stress at break as well as the gloss. The elongation at break and the impact resistance are only retained (compare B2 with B4 and B1 with B5).

[0046] In VB1 to VB4, alternative fillers are used for component (C) or for (B) and (C). In VB1 and VB2, starting from essentially the same composition as B3, the glass flakes are replaced by kaolin and calcium carbonate, respectively, in substantially the same proportions. As a result, the mechanical properties are consistently worse and the gloss in the conditioned state is also deteriorated. For example VB3, starting from example B3, the glass fibers and glass flakes are replaced by glass beads. As a result, the mechanical properties and the gloss are worse. For VB4, starting from B2, the glass flakes are replaced by mica, but here too the mechanical properties obtained are consistently worse and the gloss obtained is also worse. For VB5, starting from B3, the glass flakes are replaced by glass fibers. As a result, the values ​​of the modulus and the stress at break are improved, but the values ​​of the elongation at break are worse and the values ​​of the impact resistance are approximately the same. In particular the gloss, and especially the gloss in the conditioned state, is very poor. Comparing comparative example VB6 with B7 (where the round glass fibres and glass flakes of B7 are replaced by flat glass fibres), here too the results are improved values ​​of modulus and stress at break, worse values ​​of elongation at break and almost the same values ​​of impact resistance. The gloss is good in the dry state but unacceptable in the conditioned state. Thus, in all these comparative examples VB1-VB4, the stiffness (modulus), strength (stress at break) and impact resistance are significantly reduced compared to examples B1-B5. On the other hand, the gloss can be generally satisfactory especially in the dry state, but in the conditioned state the values ​​drop significantly in some cases. VB5-VB7, which used only glass fibres as filler, are noteworthy as the mechanical properties are good, except that the elongation at break is low in these cases. In contrast, the gloss values ​​change significantly when the specimens are conditioned.

[0047] In VB8 and VB9, in addition to glass fibers, glass flakes with a particle thickness of 5 μm, which are not according to the invention, are used. Comparing B2 and VB8, it is clear that the mechanical properties, especially impact resistance, are consistently worse in VB8. The gloss after adjustment also drops significantly. Here, it becomes clear that the thin glass flakes according to the invention have a positive effect. If an impact modifier is additionally used, as in VB9, the mechanical properties, including impact resistance, are significantly reduced. The gloss also drops to an unacceptable level due to this use. Yet another aspect of the present invention may be as follows. [1] The following ingredients (A) 28.0 to 64.9% by mass of at least one polyamide, (B) 15.0 to 40.0 mass% glass fiber, (C) 15.0 to 35.0 mass% of glass flakes having a particle thickness in the range of 0.3 to 2.0 μm; (D) 0.1 to 2.0 mass % of a heat stabilizer, (E) 0 to 5.0 mass% of additives A polyamide molding composition comprising: The polyamide molding composition as described above, provided that the total of components (B) and (C) is within the range of 35.0 to 65.0 mass% based on the total of components (A) to (E), and the total of components (A) to (E) is 100 mass%. [2] The polyamide molding composition according to [1] above, characterized in that the proportion of component (A) is in any case within the range of 34.0 to 59.8% by mass, preferably within the range of 38.2 to 57.8% by mass or 41.5 to 54.7% by mass, based on the total of components (A) to (E). [3] Component (A) is selected from the group consisting of semi-crystalline aliphatic polyamides (A1), semi-crystalline semi-aromatic polyamides (A2) and amorphous and / or microcrystalline polyamides (A3) or mixtures thereof, preferably component (A) is a mixture of at least one semi-crystalline polyamide (A1, A2) and at least one amorphous or microcrystalline polyamide (A3), more preferably the proportion of semi-crystalline polyamides (A1, A2) in component (A) is in each case 30.0 to 98.0% by weight, more preferably 40.0 to 95.0% by weight, very preferably 50.0 to 90.0% by weight, based on the total weight of component (A); and / or The polyamide molding composition according to [1] or [2] above, characterized in that component (A) is composed of a semi-crystalline aliphatic polyamide (A1) or a semi-crystalline semi-aromatic polyamide (A2) or a mixture thereof, preferably selected from the group consisting of PA 66, PA 610, PA 612, PA 10T / 6T, PA 66 / 6I / 6T, PA 6T / 66 / BacT / Bac6, PA 6T / 610 / BacT / Bac10, PA 6T / 612 / BacT / Bac12, PA 6T / BacT / 6I / BacI, and mixtures thereof, having a relative viscosity preferably in the range of 1.60 to 2.30. [4] Component (A) is a mixture of the following: (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A3) 10 to 50 mass % of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol % of hexamethylene isophthalamide units and 15 to 45 mol % of hexamethylene terephthalamide units; (wherein the fractions (A1) and (A3) constitute 100% by weight of the polyamide mixture (A)); or (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 10 to 50% by mass of semicrystalline semiaromatic polyamide 6T / 66 / BacT / Bac6, 6T / 6I / BacT / BacI or 6T / 66 / 6I / BacT / Bac6 / BacI, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, in particular 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction. and (wherein the fractions (A1) and (A2) constitute 100% by weight of the polyamide mixture (A)); or (A2) 50 to 90% by mass of semi-crystalline semi-aromatic polyamide 10T / 6T; (A3) 10 to 50 mass % of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol % of hexamethylene isophthalamide units and 15 to 45 mol % of hexamethylene terephthalamide units; (wherein the fractions (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)); or (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 8 to 30% by mass of a semi-crystalline semi-aromatic polyamide PA 6T / BacT / 66 / Bac6, 6T / BacT / 6I / BacI or 6T / BacT / 6I / BacI / 66 / Bac6, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, in particular 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction, (A3) 2-20% by weight of amorphous polyamide 6I / 6T / 612 / MACMI / MACMT / MACM12 (wherein the composition preferably contains 18-30 mol% each of 6I and 6T units, 12-26 mol% of 612 units, and 6-16 mol% each of MACM12, MACMI and MACMT units, where the sum of all PA units amounts to 100 mol%); (wherein the fractions (A1), (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)). The polyamide molding composition according to any one of the above [1] to [3], characterized in that it comprises one of the following: [5] The polyamide molding composition according to any one of the above [1] to [4], characterized in that the proportion of component (B) is in the range of 17.0 to 35.0 mass%, preferably 18.0 to 32.0 mass% or 20.0 to 30.0 mass%, based on the total of components (A) to (E) in any case. [6] The glass fibers of component (B) are E-glass fibers or S-glass fibers; and / or Component (B) is composed of glass fibers having a circular cross section, particularly preferably with a diameter in the range of 5 to 20 μm, or in the range of 5 to 13 μm or 6 to 10 μm; and / or The polyamide molding composition according to any one of the above [1] to [5], characterized in that the glass fibers of component (B) are fibers having a non-circular cross section, the dimensional ratio of the main cross section axis to the secondary cross section axis perpendicular thereto being preferentially greater than 2.5, particularly preferably in the range of 2.5 to 6 or 3 to 5. [7] The polyamide molding composition according to any one of the above [1] to [6], characterized in that the proportion of component (C) is in the range of 16.0 to 33.0 mass%, preferably in the range of 18.0 to 32.0 or 20.0 to 30.0 mass%, based on the total of components (A) to (E) in any case. [8] The average particle size (d50) of component (C) is within the range of 20 to 300 μm, more preferably within the range of 50 to 200 μm, or particularly preferably within the range of 80 to 170 μm; and / or The polyamide molding composition according to any one of the above [1] to [7], characterized in that the particle thickness of component (C) is within the range of 0.4 to 1.7 μm, particularly preferably 0.5 to 1.5 μm. [9] The polyamide molding composition according to any one of the above [1] to [8], characterized in that the total of the components (B) and (C) is within the range of 40.0 to 60.0 mass%, preferably within the range of 42.0 to 57.0 mass% or 45.0 to 55.0 mass%, based on the total of the components (A) to (E).

[10] The polyamide molding composition according to any one of the above [1] to [9], characterized in that the proportion of component (D) is in the range of 0.2 to 2.0 mass%, preferably 0.2 to 1.8 or 0.3 to 1.5 mass%, based on the total of components (A) to (E) in any case.

[11] Component (D) comprises an organic stabilizer, preferably an organic stabilizer that does not contain Cu oxide or Cu salt; and / or Component (D) is selected from the group: Compounds of mono- or divalent copper, in particular salts of mono- or divalent copper with inorganic or organic acids or with mono- or divalent phenols, oxides of mono- or divalent copper or complex compounds of copper salts with ammonia, amines, amides, lactams, cyanides or phosphines, preferably the Cu(I) or Cu(II) salts of hydrohalic acids, of hydrocyanic acid or of copper salts of aliphatic carboxylic acids, very preferably the monovalent copper compounds CuCl, CuBr, CuI, CuCN and Cu2O, and the divalent copper compounds CuCl2, CuSO4, CuO, copper(II) acetate or stearic acid. copper(II), or mixtures of these compounds (wherein these copper compounds are used on their own or, preferentially, in the form of concentrates, where concentrates refer to polymers, which preferably have the same or substantially the same chemical properties as component (A), containing copper salts in high concentrations, and where, particularly preferentially, the copper compounds are used in combination with further metal halides, including alkali metal halides, such as NaI, KI, NaBr, KBr, where the molar ratio of metal halide to copper is between 0.5 and 20, preferably between 1 and 10, more preferably between 2 and 7); Stabilizers based on secondary aromatic amines; Stabilizers based on sterically hindered phenols; Phosphites and phosphonites; and Mixtures of the aforementioned stabilizers The polyamide molding composition according to any one of the above [1] to

[10] , characterized in that it is selected from the following:

[12] The polyamide molding composition according to any one of the above [1] to

[11] , characterized in that the component (E) is present in an amount within the range of 0 to 4.0 mass%, preferably within the range of 0 to 3.0 mass%, and particularly preferably within the range of 0 to 2.0 or 0.1 to 2.0 mass%, based on the total amount of the components (A) to (E).

[13] The polyamide molding composition according to any one of the above [1] to

[12] , characterized in that the component (E) is selected from the following group: crystallization accelerators or retarders, flow aids, lubricants, mold release agents, pigments, dyes, taggants, processing aids, antistatic agents, carbon black, graphite, carbon nanotubes, residues from polymerization processes, such as catalysts, salts and derivatives thereof.

[14] A shaped article made of the polyamide molding composition according to any one of [1] to

[13] above, or comprising at least one region or coating made from the polyamide molding composition according to any one of [1] to

[13] above, preferably produced by injection molding, extrusion molding or blow molding, Preferably exterior parts and / or visible housings, covers or frames, in particular parts of electrical or electronic components, parts of housings or parts of housing components, preferably housings or housing parts, panels or covers of portable electronic devices, household goods, household machines, eyeglass frames, eyeglass edgings, sunglasses, cameras, telescoping glasses, decorative articles, devices and equipment for telecommunications and household appliances, interior and exterior parts in the field of the automobile segment and other means of transport, interior and exterior parts, preferably with a transport or mechanical function, in the fields of electrical goods, furniture, sports, mechanical engineering, sanitation and hygiene, medicine, energy and propulsion technology, particularly preferably shaped articles in the field of mobile phones, smartphones, personal organizers, laptop computers, notebook computers, tablet computers, radios, cameras, timepieces, calculators, sensor housings, measuring devices, music and / or video playback devices, navigation devices, GPS devices, electronic photo frames, external hard drives and other electronic storage media, The shaped product.

[15] Use of the polyamide molding composition according to any one of [1] to

[13] for producing the shaped article according to

[14] above, or a method for producing the shaped article according to

[14] above, comprising: The above-mentioned use or method, characterized in that the molding composition according to any one of the above-mentioned [1] to

[13] is introduced in molten form, and the shaped part is formed from this molding composition by extrusion molding, injection molding or blow molding.

Claims

1. The following ingredients (A) 28.0 to 64.9% by weight of at least one polyamide; (B) 15.0 to 40.0 mass% glass fibers, (C) 15.0 to 35.0% by mass of glass flakes having a particle thickness in the range of 0.3 to 2.0 μm; (D) 0.1 to 2.0% by mass of a heat stabilizer, (E) 0 to 5.0% by mass of additives A polyamide molding composition comprising: The polyamide molding composition as described above, provided that the total of components (B) and (C) is in the range of 35.0 to 65.0% by mass based on the total of components (A) to (E), and the total of components (A) to (E) is 100% by mass.

2. 2. The polyamide molding composition according to claim 1, characterized in that the proportion of component (A) is in the range from 34.0 to 59.8% by weight, based on the sum of components (A) to (E).

3. A polyamide molding composition as described in claim 1 or 2, characterized in that the proportion of component (A) is in the range of 38.2 to 57.8 mass% or 41.5 to 54.7 mass% in each case relative to the sum of components (A) to (E).

4. Component (A) is a mixture of at least one semicrystalline polyamide (A1, A2) and at least one amorphous or microcrystalline polyamide (A3); and / or 4. Polyamide molding composition according to claim 1, characterized in that component (A) consists of a semi-crystalline, aliphatic polyamide (A1) or a semi-crystalline, semi-aromatic polyamide (A2) or a mixture thereof.

5. Component (A) is a mixture of at least one semi-crystalline polyamide (A1, A2) and at least one amorphous or microcrystalline polyamide (A3), in which the proportion of the semi-crystalline polyamide (A1, A2) in component (A) is in the range of 30.0 to 98.0% by weight, or 40.0 to 95.0% by weight, or 50.0 to 90.0% by weight, in each case based on the total weight of component (A); and / or 5. Polyamide molding composition according to claim 1, characterized in that component (A) consists of a semi-crystalline, aliphatic polyamide (A1) or a semi-crystalline, semi-aromatic polyamide (A2) selected from the group consisting of PA 66, PA 610, PA 612, PA 10T / 6T, PA 66 / 6I / 6T, PA 6T / 66 / BacT / Bac6, PA 6T / 610 / BacT / Bac10, PA 6T / 612 / BacT / Bac12, PA 6T / BacT / 6I / BacI, and mixtures thereof, having a relative viscosity in the range from 1.60 to 2.30, or a mixture thereof.

6. Component (A) is a mixture of: (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A3) 10 to 50% by mass of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol% of hexamethylene isophthalamide units and 15 to 45 mol% of hexamethylene terephthalamide units; (wherein the fractions (A1) and (A3) constitute 100% by weight of the polyamide mixture (A)); or (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 10 to 50% by weight of semi-crystalline, semi-aromatic polyamide 6T / 66 / BacT / Bac6, 6T / 6I / BacT / BacI or 6T / 66 / 6I / BacT / Bac6 / BacI, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is composed of 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction. and wherein the fractions (A1) and (A2) constitute 100% by weight of the polyamide mixture (A); or (A2) 50 to 90% by mass of semicrystalline semi-aromatic polyamide 10T / 6T; (A3) 10 to 50% by mass of amorphous semi-aromatic polyamide 6I / 6T having 55 to 85 mol% of hexamethylene isophthalamide units and 15 to 45 mol% of hexamethylene terephthalamide units; (wherein the fractions (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)); or (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 8 to 30% by weight of a semi-crystalline, semi-aromatic polyamide PA 6T / BacT / 66 / Bac6, 6T / BacT / 6I / BacI or 6T / BacT / 6I / BacI / 66 / Bac6, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is composed of 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction, (A3) 2 to 20% by mass of amorphous polyamide 6I / 6T / 612 / MACMI / MACMT / MACM12; (wherein the fractions (A1), (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)).

6. The polyamide molding composition according to claim 1, wherein the polyamide molding composition comprises one of the following:

7. Component (A) is a mixture of: (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 10 to 50% by weight of semi-crystalline, semi-aromatic polyamide 6T / 66 / BacT / Bac6, 6T / 6I / BacT / BacI or 6T / 66 / 6I / BacT / Bac6 / BacI, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is composed of 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction. (wherein the fractions (A1) and (A2) constitute 100% by weight of the polyamide mixture (A)); or (A1) 50 to 90% by mass of semi-crystalline aliphatic polyamide 66; (A2) 8 to 30% by weight of a semi-crystalline, semi-aromatic polyamide PA 6T / BacT / 66 / Bac6, 6T / BacT / 6I / BacI or 6T / BacT / 6I / BacI / 66 / Bac6, in which the diamine component is selected from 65 to 85 mole fraction of 1,6-hexanediamine and 15 to 35 mole fraction of 1,3-bis(aminomethyl)cyclohexane, and the dicarboxylic acid component is composed of 64 to 100 mole fraction of terephthalic acid, 0 to 18 mole fraction of isophthalic acid, and 0 to 18 mole fraction of one or more aliphatic dicarboxylic acids having 6 to 18 carbons, in which the sum of each of the diamine component and the dicarboxylic acid component is 100 mole fraction, (A3) 2-20% by weight of amorphous polyamide 6I / 6T / 612 / MACMI / MACMT / MACM12 (wherein the composition comprises 18-30 mol% each of 6I and 6T units, 12-26 mol% of 612 units, and 6-16 mol% each of MACM12, MACMI and MACMT units, the sum of all PA units adding up to 100 mol%) (wherein the fractions (A1), (A2) and (A3) constitute 100% by weight of the polyamide mixture (A)).

7. The polyamide molding composition according to claim 1, characterized in that it consists of one of the following:

8. 8. The polyamide molding composition according to claim 1, wherein the proportion of component (B) is in the range of 17.0 to 35.0% by weight, based on the sum of components (A) to (E).

9. A polyamide molding composition according to any one of claims 1 to 8, characterized in that the proportion of component (B) is in the range of 18.0 to 32.0 mass% or 20.0 to 30.0 mass%, in each case relative to the sum of components (A) to (E).

10. The glass fibers of component (B) are E-glass fibers or S-glass fibers; and / or Component (B) is composed of glass fibers having a circular cross section; and / or 10. Polyamide molding composition according to claim 1, characterized in that the glass fibres of component (B) are fibres with a non-circular cross section.

11. Component (B) is composed of glass fibers having a circular cross section and a diameter within the range of 5 to 20 μm, 5 to 13 μm, or 6 to 10 μm. and / or 11. Polyamide molding composition according to claim 1, characterized in that the glass fibres of component (B) are fibres with a non-circular cross section, in which the dimensional ratio of the main cross section axis to the secondary cross section axis perpendicular thereto is greater than 2.5 or in the range from 2.5 to 6 or from 3 to 5.

12. 12. The polyamide molding composition according to claim 1, wherein the proportion of component (C) is in the range from 16.0 to 33.0% by weight, based on the sum of components (A) to (E).

13. A polyamide molding composition according to any one of claims 1 to 12, characterized in that the proportion of component (C) is in the range of 18.0 to 32.0 mass% or 20.0 to 30.0 mass%, in each case relative to the sum of components (A) to (E).

14. The average particle size (d50) of component (C) is in the range of 50 to 200 μm or in the range of 80 to 170 μm; and / or 14. Polyamide molding composition according to claim 1, characterized in that the particle thickness of component (C) is in the range of 0.4 to 1.7 μm or 0.5 to 1.5 μm.

15. 15. The polyamide molding composition according to claim 1, wherein the sum of components (B) and (C) is in the range of 40.0 to 60.0% by weight, based on the sum of components (A) to (E).

16. A polyamide molding composition according to any one of claims 1 to 15, characterized in that the sum of components (B) and (C) is within the range of 42.0 to 57.0 mass% or 45.0 to 55.0 mass%, relative to the sum of components (A) to (E).

17. 17. Polyamide molding composition according to claim 1, characterized in that the proportion of component (D) is in the range from 0.2 to 2.0% by weight, based on the sum of components (A) to (E).

18. A polyamide molding composition according to any one of claims 1 to 17, characterized in that the proportion of component (D) is in each case within the range of 0.2 to 1.8 mass% or 0.3 to 1.5 mass%, relative to the sum of components (A) to (E).

19. Component (D) comprises an organic stabilizer; and / or Component (D) is selected from the group consisting of: Compounds of monovalent or divalent copper; Stabilizers based on secondary aromatic amines; Stabilizers based on sterically hindered phenols; Phosphites and phosphonites; and Mixtures of the aforementioned stabilizers 19. The polyamide molding composition according to claim 1, wherein the polyamide molding composition is selected from the group consisting of

20. Component (D) comprises an organic stabilizer that does not contain Cu oxides or Cu salts; and / or Component (D) is selected from the group consisting of: Salts of mono- or divalent copper with inorganic or organic acids or mono- or divalent phenols (e.g. Cu(I) or Cu(II) salts of hydrohalic acids (e.g. CuCl, CuBr, CuI, and CuCl2), Cu(I) or Cu(II) salts of hydrocyanic acid (e.g. CuCN), copper salts of aliphatic carboxylic acids (e.g. copper(II) acetate and copper(II) stearate), and CuSO4), oxides of mono- or divalent copper (e.g. Cu2O and CuO), or complex compounds of copper salts with ammonia, amines, amides, lactams, cyanides or phosphines, or mixtures of these compounds, wherein these copper compounds are used by themselves or in the form of concentrates, where concentrate refers to a polymer of the same or substantially the same chemical nature as component (A) containing a high concentration of copper salts, where the copper compounds may be used in combination with additional metal halides (e.g., alkali metal halides (e.g., NaI, KI, NaBr, KBr)), where the molar ratio of metal halide to copper is 0.5 to 20, or 1 to 10, or 2 to 7; 20. The polyamide molding composition according to claim 1 ,

21. 21. The polyamide molding composition according to claim 1, wherein component (E) is present in a proportion ranging from 0 to 4.0% by weight, based on the sum of components (A) to (E).

22. A polyamide molding composition according to any one of claims 1 to 21, characterized in that component (E) is present in an amount within the range of 0 to 3.0 mass%, 0 to 2.0 mass%, or 0.1 to 2.0 mass%, relative to the sum of components (A) to (E).

23. 23. Polyamide moulding composition according to any one of claims 1 to 22, characterized in that component (E) is selected from the following group: crystallization accelerators or retarders, flow aids, lubricants, release agents, pigments, dyes, taggants, processing aids, antistatic agents, carbon black, graphite, carbon nanotubes and residues from the polymerization process (for example catalysts, salts and their derivatives).

24. Made from a polyamide moulding composition according to any one of claims 1 to 23, or At least one area or coating made of the polyamide molding composition according to any one of claims 1 to 23, Modeled item.

25. The shaped article of claim 24, produced by injection molding, extrusion molding or blow molding.

26. A shaped article as described in claim 24 or 25, which is a shaped article in the field of exterior parts and / or visible housings, covers or frames (e.g. parts of electrical or electronic components, parts of housings or parts of housing components).

27. ​​In the form of housings or housing parts, panels or covers for portable electronic devices, household goods, household machines, eyeglass frames, eyeglass edgings, sunglasses, cameras, farsighted spectacles, decorative articles, devices and equipment for telecommunications and household appliances, interior and exterior parts in the field of automotive segments and other means of transport, interior and exterior parts in the fields of electrical goods, furniture, sports, mechanical engineering, sanitation and hygiene, medicine, energy and propulsion technology (e.g. mobile phones, smartphones, personal organizers, laptop computers, notebook computers, tablet computers, radios, cameras, timepieces, calculators, sensor housings, measuring devices, music and / or video playback devices, navigation devices, GPS devices, electronic photo frames, external hard drives and other electronic storage media), The shaped article according to any one of claims 24 to 26.

28. Use of the polyamide moulding composition according to any one of claims 1 to 23 for producing a shaped article according to any one of claims 24 to 27, comprising 24. The use, characterized in that the polyamide molding composition according to any one of claims 1 to 23 is introduced in molten form and the shaped article is formed from this molding composition by extrusion, injection molding or blow molding processes.

29. A method for producing a shaped article according to any one of claims 24 to 27, comprising the steps of: The process according to any one of claims 1 to 23, wherein the polyamide moulding composition is introduced in molten form and the shaped article is formed from this moulding composition by extrusion, injection moulding or blow moulding.

Citation Information

Patent Citations

  • Heat-resistant polyamide reinforced material with low water absorption rate and preparation method thereof

    CN109929243A

  • polyamide resin composition

    DE10352319A1

  • Polyamide resin composition and molding thereof

    EP0741762A1

  • Vibration fusion bonded hollow molding made of polyamide resin

    JP1996281827A

  • Mobile phone housing containing polyamide resin composition

    JP2010510374A