Manufacturing method of meltblown nonwoven fabric

A thermoplastic resin composition with polyolefin and a soluble crystal nucleating agent addresses the challenge of reducing fiber diameter and enhancing water pressure resistance and filterability in melt-blown nonwoven fabrics, suitable for absorbent articles and separation membranes.

JP7568429B2Active Publication Date: 2024-10-16KAO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020107365
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-22
Publication Date
2024-10-16
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

Existing methods for producing melt-blown nonwoven fabrics face challenges in reducing fiber diameter efficiently while maintaining cost-effectiveness and preventing manufacturing issues such as filter clogging, and there is a need for improved water pressure resistance and filterability.

Method used

A method involving a thermoplastic resin composition containing polyolefin and a soluble crystal nucleating agent, with specific precipitation temperature and complex viscosity ratios, is used to produce fibers with diameters of 900 nm or less, enhancing water pressure resistance and filterability.

Benefits of technology

The method achieves fibers with reduced diameters, improving water pressure resistance and filterability, suitable for absorbent articles and separation membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568429000001
    Figure 0007568429000001
  • Figure 0007568429000002
    Figure 0007568429000002
  • Figure 0007568429000003
    Figure 0007568429000003
Patent Text Reader

Abstract

To manufacture a meltblow nonwoven fabric having improved water pressure resistance and filter properties while reducing a diameter of a constituent fiber.SOLUTION: A meltblow nonwoven fabric manufacturing method has a spinning process to melt a thermoplastic resin composition by heating, subsequently cause the molten material to be discharged from a nozzle, cause the discharged molten material to be fibrous by stretching the discharged molten material by airflow. The thermoplastic resin composition contains polyolefin, which is a thermoplastic resin, and a dissolved-type crystal nucleating agent. A precipitation temperature at which the dissolved-type crystal nucleating agent is precipitated from the thermoplastic resin composition in a molten state is 150°C or higher and 185°C or less. The thermoplastic resin composition has a complex viscosity of ηT-10 at a temperature lower by 10°C than the precipitation temperature. When the complex viscosity at the precipitation temperature is ηT, ηT-10 / ηT, which is a ratio of ηT-10 to ηT, is 1.5 or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a melt-blown nonwoven fabric, and more particularly to a method for producing a melt-blown nonwoven fabric, a method for producing an absorbent article using the same, a melt-blown nonwoven fabric, and an absorbent article. [Background technology]

[0002] The melt-blowing method is a method in which molten resin is blown out from a die having multiple nozzles with a high-temperature, high-velocity air current, and the resin stretched into fibers is fused together to form a nonwoven fabric, and is suitable for producing nonwoven fabrics with fine fibers. Melt-blown nonwoven fabrics are nonwoven fabrics produced by the melt-blowing method. Regarding the technology for producing melt-blown nonwoven fabrics, Patent Document 1 discloses a method for producing melt-blown nonwoven fabrics by blending a phosphoric acid-based dispersion-type crystal nucleating agent with a thermoplastic resin. In the examples of Patent Document 2, a method for producing melt-blown nonwoven fabrics by blending a soluble crystal nucleating agent with a thermoplastic resin is described. Patent Document 3 describes a granular polyolefin additive composition in which a crystal nucleating agent, which is a dibenzylidene sorbitol, is blended with a polyolefin, and a method for producing the same. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO2014 / 030730 publication [Patent Document 2] JP 2018-141244 A [Patent Document 3] JP 2002-332359 A Summary of the Invention [Problem to be solved by the invention]

[0004] As mentioned above, the melt-blowing method is suitable for producing nonwoven fabrics made of fine fibers, and in recent years, research has been conducted toward mass production of nonwoven fabrics made of ultrafine fibers or nanofibers, which have even smaller fiber diameters. However, in order to obtain a fiber with a small fiber diameter, it is necessary to increase the amount of hot air used, which tends to increase the production cost. The technology of Patent Document 2 is a technology that can reduce the diameter of the constituent fibers, but it does not necessarily fully meet the need for even smaller diameters. In addition, when a dispersion-type crystal nucleating agent is used as in Patent Document 1, production problems tend to occur when trying to reduce the diameter of the fiber, such as clogging of the filter arranged in the path from the extruder to the die. Patent Document 3 does not describe the production of a nonwoven fabric.

[0005] Therefore, an object of the present invention is to provide a method for producing a melt-blown nonwoven fabric that can eliminate the above-mentioned drawbacks of the conventional techniques. [Means for solving the problem]

[0006] The present invention provides a method for producing a melt-blown nonwoven fabric, comprising a spinning step of heating and melting a thermoplastic resin composition, extruding the molten material from a nozzle, and stretching the extruding molten material with an airflow to form fibers. The thermoplastic resin composition preferably contains a polyolefin as a thermoplastic resin and a soluble crystal nucleating agent. The precipitation temperature at which the soluble crystal nucleating agent precipitates from the molten state of the thermoplastic resin composition is preferably 150°C or higher and 185°C or lower. The thermoplastic resin composition has a complex viscosity η at a temperature 10°C lower than the precipitation temperature. T-10 The complex viscosity at the precipitation temperature is η T Then, η T-10 η T The ratio to η T-10 / η T It is preferable that the value is 1.5 or more.

[0007] The present invention provides a method for producing an absorbent article, which comprises a step of laminating a melt-blown nonwoven fabric produced by the above-mentioned method for producing a melt-blown nonwoven fabric on an absorbent core of the absorbent article. The present invention provides a melt-blown nonwoven fabric comprising polypropylene and a soluble crystal nucleating agent, and having an average fiber diameter of 900 nm or less. The present invention also provides an absorbent article comprising the above-mentioned meltblown nonwoven fabric. Effect of the Invention

[0008] According to the method for producing a melt-blown nonwoven fabric of the present invention, the diameter of the constituent fibers can be efficiently reduced, and a melt-blown nonwoven fabric having improved water pressure resistance and filtering properties can be efficiently produced. According to the melt-blown nonwoven fabric of the present invention, it is possible to provide a melt-blown nonwoven fabric having finer fibers and improved water pressure resistance and filtering properties. According to the absorbent article and the manufacturing method thereof of the present invention, it is possible to provide an absorbent article which contains a meltblown nonwoven fabric whose constituent fibers have a fine diameter and have improved water pressure resistance, and which has excellent properties such as preventing liquid leakage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will now be described based on its preferred embodiments. The method for producing a melt-blown nonwoven fabric of the present invention is a method for producing a nonwoven fabric by a melt-blowing method, and includes a spinning step in which a thermoplastic resin composition is heated and melted, then the melt is discharged from a nozzle, and the discharged melt is stretched by an air flow to form fibers. In a collection step, the fibrous melt is deposited on a known collection means such as a net conveyor or a collection screen, and is bonded to each other by fusion to form a nonwoven fabric.

[0010] The method for producing the melt-blown nonwoven fabric according to the present embodiment can be carried out in the same manner as the conventional method for producing the melt-blown nonwoven fabric, except that the specific thermoplastic resin composition described below is used. As for the nonwoven fabric production apparatus, a known melt-blown nonwoven fabric production apparatus conventionally used for the production of the melt-blown nonwoven fabric can be used.

[0011] The thermoplastic resin composition used as a raw material in the method for producing the melt-blown nonwoven fabric of the present invention will now be described. The thermoplastic resin composition used in the present embodiment contains (1) a polyolefin as a thermoplastic resin, and (2) a soluble crystal nucleating agent.

[0012] (1) Polyolefin The thermoplastic resin composition contains a polyolefin as the thermoplastic resin, which is preferred from the viewpoint of reducing the diameter of the constituent fibers of the nonwoven fabric obtained by the melt-blowing method. As the polyolefin, any thermoplastic resin that is commonly used as a material for the constituent fibers of meltblown nonwoven fabrics can be used without any particular limitation. Examples of polyolefin include polyethylene, polypropylene, polymethylpentene such as poly4-methyl-1-pentene, polybutene, etc. In addition, copolymers of polymerizable monomers constituting these resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and their esters and acid anhydrides can also be used. Polypropylene includes propylene homopolymers as well as propylene-based copolymers of propylene and other monomers such as α-olefins. Examples of propylene-based copolymers include propylene-α-olefin random copolymers and propylene block copolymers. Examples of polyethylene include linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ultra-high molecular weight polyethylene (UHMWPE). The polyolefins can be used alone or in combination of two or more kinds as a copolymer or blend.

[0013] Among polyolefins, polypropylene is preferred from the viewpoint of achieving a finer fiber diameter and a good balance between price and performance, and propylene homopolymer is more preferred from the viewpoint of achieving a finer fiber diameter more efficiently. The weight average molecular weight of the polypropylene is preferably 25,000 or more, more preferably 35,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less.

[0014] The polyolefin used in the thermoplastic resin composition has a melt flow rate of 500 g / mol at a temperature of 230°C and a load of 2160 g. 10 min or more from the viewpoint of reducing the amount of hot air used and decreasing the fiber diameter of the resulting nonwoven fabric. Hereinafter, the melt flow rate at a temperature of 230° C. and a load of 2160 g will be simply referred to as “MFR”. The MFR of polyolefin is 750g / 10 min or more is preferable, and 1000g / 10 The MFR of the polyolefin is preferably 2500 g / min or more from the viewpoint of preventing thread breakage. 10 Minutes or less are preferable, and 2000g / 10 The MFR of the polyolefin is the MFR of the polyolefin when the thermoplastic resin composition contains only one type of polyolefin, and is the MFR of the mixture of the polyolefins when the thermoplastic resin composition contains two or more types of polyolefins. The MFR is measured at a test temperature and load in accordance with, for example, JIS K 7210. The MFR of the constituent resins can also be measured by remelting the completed nonwoven fabric and performing the measurement in the same manner.

[0015] (2) Soluble crystal nucleating agents Nucleating agents are roughly divided into organic nucleating agents and inorganic nucleating agents, with organic nucleating agents being preferred. Organic nucleating agents have superior dispersibility compared to inorganic nucleating agents such as talc and silica, and are therefore more effective with a small amount. Organic nucleating agents can be divided into soluble type and dispersed type. In the present invention, the soluble type nucleating agent (also called soluble type nucleating agent) is used.

[0016] The soluble crystal nucleating agent is capable of dissolving in the molten thermoplastic resin in relation to the main thermoplastic resin in the thermoplastic resin composition. Here, the main thermoplastic resin is the polyolefin contained in the largest amount in the thermoplastic resin composition, and is preferably 60 mass% or more, more preferably 75 mass% or more, and even more preferably 90 mass% or more of the total mass of the thermoplastic resin contained in the thermoplastic resin composition. As the soluble crystal nucleating agent, commercially available ones can be used as the soluble crystal nucleating agent of the main thermoplastic resin in the thermoplastic resin composition. For example, when the main thermoplastic resin contained in the thermoplastic resin composition is polypropylene, various commercially available crystal nucleating agents can be used as the soluble crystal nucleating agent of polypropylene. For example, "Gelall D", "Gelall MD", "Gelall DXR" and "Rikaclear PC1" from New Japan Chemical Co., Ltd., and "IRGACLEAR XT386" from BASF can be used. As the soluble crystal nucleating agent of polyolefin represented by polypropylene, it is preferable to use a sorbitol-based or amide-based crystal nucleating agent. As the sorbitol-based crystal nucleating agent, crystal nucleating agents that are dibenzylidene sorbitols, for example, "Gelall D", "Gelall MD", and "Gelall DXR" mentioned above can be mentioned, and as the crystal nucleating agent that is an amide-based compound, for example, "Rikaclear PC1" and "IRGACLEAR XT386" mentioned above can be mentioned. As the soluble crystal nucleating agent, it is preferable to use a sorbitol-based compound such as dibenzylidene sorbitol or an amide-based compound, since the fibrous molten material discharged from the nozzle can be efficiently thinned, and it is even more preferable to use 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol, since the fibrous molten material discharged from the nozzle can be even more efficiently thinned. The soluble crystal nucleating agents may be used alone or in combination of two or more.

[0017] The inclusion of a soluble crystal nucleating agent can be confirmed by analyzing the thermoplastic resin composition obtained by remelting the meltblown nonwoven fabric using a differential scanning calorimeter measurement or the like. In addition, the soluble crystal nucleating agent can be extracted from the remelted thermoplastic resin composition using a high boiling point solvent, and the compound type can be identified by a known analytical method such as high performance liquid chromatography or nuclear magnetic resonance. If the soluble crystal nucleating agent is used, no aggregates of the soluble crystal nucleating agent are observed even when the thermoplastic resin composition is sufficiently heated to above the dissolution temperature.

[0018] The thermoplastic resin composition used in the present embodiment may contain other components in addition to the thermoplastic resin and the soluble crystal nucleating agent, as long as the effects of the present invention are not impaired. For example, it may contain an antibacterial agent, an antifungal agent, a flame retardant, a light stabilizer, a hydrophilic agent, a water repellent agent, a pigment, etc.

[0019] The method for producing the melt-blown nonwoven fabric according to the present embodiment can be carried out in the same manner as the conventional method for producing a melt-blown nonwoven fabric, except that the above-mentioned thermoplastic resin composition is used. For example, the nonwoven fabric can be produced using a known nonwoven fabric production apparatus equipped with an extruder equipped with a barrel having a built-in screw and a raw material input section, and a die connected to the extruder directly or via a gear pump or the like. In that case, preferably, the thermoplastic resin composition is fed into the extruder from the raw material input section as, for example, pellets, heated in the extruder to become molten, and the molten material is fed to the die from the extruder directly or via a gear pump or the like. The die is formed with a plurality of nozzles arranged in series for discharging the molten material, and the molten material fed to the die is discharged from the plurality of nozzles and stretched by high-temperature and high-pressure airflows sprayed from the outlets located on both sides of the nozzles, and becomes fibrous. The fibrous molten material is then deposited on the known collection means described above, and the fibers are fused to each other to become a melt-blown nonwoven fabric. The plurality of nozzles provided in the die are preferably arranged in series at regular intervals. The high-temperature and high-pressure airflow is preferably an airflow, but may be an airflow of other gases.

[0020] The thermoplastic resin composition used in the present embodiment has a precipitation temperature T at which the solution-type crystal nucleating agent precipitates from the molten thermoplastic resin composition of 150° C. or higher and 185° C. or lower. The thermoplastic resin composition used in this embodiment has a complex viscosity η at a temperature 10° C. lower than the precipitation temperature T T-10 The complex viscosity at the precipitation temperature T is η T Then, η T-10 η T The ratio to η T-10 / η T The value of is 1.5 or more. Hereinafter, η T-10 η T The ratio to is also simply called the complex viscosity ratio.

[0021] The present inventors have discovered that by setting the precipitation temperature of the soluble crystal nucleating agent within a specific range and setting the value of the complex viscosity ratio within a specific range, the fiber diameter of the constituent fibers of the obtained melt-blown nonwoven fabric can be significantly reduced, and the water pressure resistance of the obtained melt-blown nonwoven fabric can also be improved. Conventionally, the combination of a thermoplastic resin and a soluble crystal nucleating agent to prepare a thermoplastic resin composition has been disclosed in Patent Document 2. However, in the present embodiment, the precipitation temperature of the soluble crystal nucleating agent is set to a specific range, and in relation to the precipitation temperature, the complex viscosity η of the thermoplastic resin composition at a temperature 10° C. lower than the precipitation temperature is set to a specific range. T-10 and the complex viscosity at the precipitation temperature η T Relative to η T-10 / η T There is no known technique for setting the value of in a specific range.

[0022] According to the method for producing the melt-blown nonwoven fabric of the present embodiment, by setting the precipitation temperature of the soluble crystal nucleating agent in the above-mentioned specific range and setting the value of the complex viscosity ratio in the above-mentioned specific range, the fiber diameter of the constituent fibers of the obtained melt-blown nonwoven fabric can be increased to one layer. This also makes it possible to produce a melt-blown nonwoven fabric with improved water pressure resistance and filtering properties.

[0023] The reason for this is unclear, but is speculated as follows. It has been reported that the soluble crystal nucleating agent forms a network structure during the cooling process. On the other hand, in a melt-blown nonwoven fabric manufacturing device, the molten thermoplastic resin composition discharged from the nozzle generally has low viscosity and high fluidity, so that the discharged molten material is relatively easily stretched when it is subjected to an air flow. The molten thermoplastic resin composition discharged from the nozzle is hereinafter also simply referred to as the molten material. The dissolved crystal nucleating agent in the melt discharged from the nozzle precipitates during the cooling process of the melt and forms a network structure within the melt. When the crystal nucleating agent precipitates in the melt, a network structure is formed and the melt thickens, suppressing subsequent stretching. Therefore, if the crystal nucleating agent precipitates immediately after the melt is discharged from the nozzle, the melt is not sufficiently stretched and subsequent stretching is inhibited, making it difficult to reduce the diameter. On the other hand, if the crystal nucleating agent does not precipitate even after the melt discharged from the nozzle is stretched to a certain extent, the melt, which has already become thin to a certain extent, breaks without forming a network structure, and further stretching is not possible. In this way, when the precipitation temperature is close to the temperature of the thermoplastic resin composition discharged from the nozzle [high temperature], precipitation occurs quickly and the thinning of the fibers tends to be suppressed, whereas when the precipitation temperature is far from the temperature of the thermoplastic resin composition [low temperature], precipitation occurs slowly, making the incorporation of a soluble crystal nucleating agent meaningless.

[0024] In contrast, according to the manufacturing method of the melt-blown nonwoven fabric of the present embodiment, the precipitation temperature of the soluble crystal nucleating agent is set to the above-mentioned specific range, and the value of the ratio of the complex viscosity is set to the above-mentioned specific range, so that the melt discharged from the nozzle is efficiently stretched by the air flow while maintaining a low viscosity, and the melt is thickened by the formation of a network structure due to the precipitation of the crystal nucleating agent near the breaking point where it would normally break, and the breakage of the melt is suppressed. As a result, after further stretching of the melt occurs, the balance between the resistance force due to the thickening and the stretching force due to the air flow is lost, and the melt breaks. In this way, it is presumed that the melt is greatly stretched and then broken, resulting in a fiber with an even thinner diameter. It is presumed that such fibers with a small diameter are arranged in the planar direction of the nonwoven fabric, thereby increasing the fiber density per unit area, and improving the water pressure resistance (water resistance) and filterability.

[0025] From the viewpoint of efficiently stretching the molten material discharged from the nozzle to further reduce the diameter of the constituent fibers, the precipitation temperature of the soluble crystal nucleating agent is more preferably 155°C or higher, even more preferably 160°C or higher, more preferably 180°C or lower, even more preferably 175°C or lower, and even more preferably 155°C or higher and 180°C or lower, even more preferably 160°C or higher and 175°C or lower.

[0026] From the viewpoint of efficiently stretching the molten material discharged from the nozzle to further reduce the diameter of the constituent fibers, it is preferable that the thermoplastic resin composition has a sudden increase in viscosity near the cutting point when no soluble crystal nucleating agent is blended. From this viewpoint, the value of the complex viscosity ratio is 1.5 or more, more preferably 1.6 or more, and even more preferably 2.0 or more, as described above. The upper limit of the value of the complex viscosity ratio is not particularly limited, but is, for example, preferably 5.0 or less, and even more preferably 4.0 or less.

[0027] The temperature of the thermoplastic resin composition before being discharged from the nozzle is at least equal to or higher than the precipitation temperature (° C.) of the soluble crystal nucleating agent. From the viewpoint of more reliably obtaining fine fibers, the temperature of the thermoplastic resin composition before being discharged from the nozzle is preferably 200° C. or higher. From the viewpoint of precipitating the crystal nucleating agent at an appropriate timing to more efficiently thin the fibers, the difference between the temperature of the thermoplastic resin composition discharged from the nozzle and the precipitation temperature (°C) is preferably 15°C or more, more preferably 20°C or more, and is also preferably 120°C or less, more preferably 105°C or less, and is also preferably 15°C or more and 120°C or less, more preferably 20°C or more and 105°C or less.

[0028] [Measurement of Precipitation Temperature of Dissolved Crystal Nucleating Agent] The precipitation temperature of the soluble crystal nucleating agent can be measured by the following method. Measurements are performed using a rotational rheometer (Rheo stress 6000, manufactured by Thermo Fisher Scientific) with parallel plates of φ60 mm. First, the temperature of the sample stage and the parallel plate is raised to 270° C. After the temperature is raised, the sample stage and the parallel plate are brought into contact with each other to perform zero point adjustment. Next, the sample stage and the parallel plate are separated, and about 1.5 g of a sample of the thermoplastic resin composition is placed on the sample stage and melted. The sample of the thermoplastic resin composition can be in any form, such as powder, pellets, or nonwoven fabric. After the sample of the thermoplastic resin composition is melted, the gap between the sample stage and the parallel plate is immediately set to 0.5 mm, and the molten resin is sandwiched between the sample stage and the parallel plate and left to stand for 30 seconds. Then, while lowering the temperature from 270°C to at least 145°C at -0.5°C / sec, a strain of 0.8±0.2 is applied to the parallel plate at a frequency of 10 Hz, and the parallel plate is vibrated in the rotational direction to obtain the storage modulus G' (Pa) and complex viscosity η (Pa·s) at each temperature. Using the storage modulus G' for the obtained temperature, the storage modulus G' at temperatures of 265°C in increments of -5°C (260, 255, 250···) is obtained, and the slope of the storage modulus G' at temperatures of -5°C increments is calculated using the following formula (1). The temperature at which the value of formula (1) became −2.5 Pa or less was determined as the precipitation temperature of the crystal nucleating agent.

number

[0029] [Method of calculating complex viscosity at precipitation temperature of soluble crystal nucleating agent] In equation (1), G' T is the storage modulus at the precipitation temperature (265°C to -5°C intervals), and G' is T-5 is the storage modulus at the precipitation temperature -5℃. In addition, the complex viscosity η with respect to temperature is the complex viscosity η at the precipitation temperature of the nucleating agent. T , complex viscosity at precipitation temperature -10℃ η T-10 The ratio can be calculated by using the following formula (2).

number

[0030] The ratio η T-10 / η T can be adjusted to the above-mentioned specific range mainly by using a soluble crystal nucleating agent and adjusting the amount of the agent added. The ratio ηT-10 / η T From the viewpoint of keeping within the above-mentioned preferred range, the amount of the soluble crystal nucleating agent added in the thermoplastic resin composition is preferably more than 0.1% by mass and less than 1.0% by mass. Here, the amount of the soluble crystal nucleating agent added is the mass ratio (mass%) of the crystal nucleating agent to the total amount of all components of the thermoplastic resin composition excluding the crystal nucleating agent. If the amount of the soluble crystal nucleating agent is large, the viscosity increases in the high temperature region where the fiber is stretched, making it difficult to narrow the fiber diameter, and if the amount of the soluble crystal nucleating agent is too small, the viscosity increases in the low temperature region after the fiber breaks, and there is no sufficient precipitation, so the fiber diameter does not narrow, resulting in a decrease in the amount of fiber, and the water pressure resistance or filterability tends to decrease. Therefore, taking into account the balance between the precipitation temperature, the range of the complex viscosity ratio, and the fiber diameter, the amount of the soluble crystal nucleating agent added in the thermoplastic resin composition is preferably more than 0.1% by mass, more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, and also preferably less than 1.0% by mass, more preferably 0.9% by mass or less, even more preferably 0.5% by mass or less, and more specifically, preferably more than 0.1% by mass and less than 1.0% by mass, more preferably 0.2% by mass or more and 0.9% by mass or less, and even more preferably 0.3% by mass or more and 0.5% by mass or less. In this way, by setting the amount of the soluble crystal nucleating agent to be added within the above range, it is possible to more reliably make the fiber diameter sufficiently small and improve the water pressure resistance and filtering properties of the resulting nonwoven fabric.

[0031] In a preferred embodiment, the temperature of the thermoplastic resin composition before being discharged from the nozzle is 200°C or higher. For example, a method for producing a melt-blown nonwoven fabric in which the temperature of the molten thermoplastic resin composition when being discharged from the nozzle is 200°C or higher and the temperature of the airflow is 200°C or higher is also possible, in which the energy consumption is significantly reduced. In addition, the lower limit of the temperature when being discharged from the nozzle needs to be equal to or higher than the melting point of the resin, and the higher the temperature, the thinner the fibers tend to be. The temperature when being discharged from the nozzle is, for example, the temperature of the molten material immediately before being discharged from the nozzle, and the temperature of the thermoplastic resin composition is usually measured by a temperature sensor inserted into the nozzle. The temperature of the airflow is the temperature of the gas sprayed from the outlet arranged near the nozzle.

[0032] The melt-blown nonwoven fabric produced by the method for producing a melt-blown nonwoven fabric of the present invention preferably has constituent fibers with an average fiber diameter of 900 nm or less. According to the manufacturing method of the melt-blown nonwoven fabric of the present embodiment, it is possible to manufacture a melt-blown nonwoven fabric which is made of fibers with small fiber diameters in which the molten material is greatly stretched while suppressing the amount of hot air used, and which has improved water pressure resistance and filtering properties while reducing the diameter of the constituent fibers. When the average fiber diameter of the constituent fibers of the melt-blown nonwoven fabric is 900 nm or less, which is smaller than that of conventional melt-blown nonwoven fabrics, the melt-blown nonwoven fabric has excellent (a) water resistance (water pressure resistance) and (b) filtering properties.

[0033] (a) Excellent water resistance has the advantage of increasing leak resistance when used, for example, as the backsheet of absorbent articles such as sanitary napkins and disposable diapers, or as a component sheet of three-dimensional guards placed at the front, rear, or sides. (a) Its excellent filtering properties are advantageous in that it can efficiently capture foreign matter to be removed when used in various separation membranes, sanitary masks, etc. From the viewpoint of improving water resistance (water pressure resistance) and filtering properties, the average fiber diameter of the constituent fibers of the meltblown nonwoven fabric is preferably 100 nm or more, more preferably 300 nm or more, and is preferably 900 nm or less, more preferably 850 nm or less.

[0034] The average fiber diameter of the constituent fibers of the meltblown nonwoven fabric can be determined by the following method. [Method of measuring average fiber diameter] When obtaining a nonwoven fabric to be measured from a diaper or the like, the hot melt is deactivated with a cold spray or an organic solvent, and the nonwoven fabric to be measured is carefully peeled off and isolated. This process is common to all measurements in this specification unless otherwise specified. The average fiber diameter is determined by first randomly collecting five small samples from the nonwoven fabric. Next, a photograph is taken with a scanning electron microscope at 1,000 to 10,000 times magnification so that 20 to 60 fibers are visible in the field of view. The fiber diameter is measured so that each fiber in the field of view is counted once, and the average fiber diameter for 100 or more fibers is calculated in nanometer order and rounded off to the first decimal place.

[0035] The meltblown nonwoven fabric according to the present invention may be a laminated nonwoven fabric having a multi-layer structure including a meltblown layer produced by the method of the present invention. Examples of the multilayered laminated nonwoven fabric include a structure in which a base layer made of a spunbonded nonwoven fabric or an air-through nonwoven fabric and a meltblown nonwoven fabric (meltblown layer) produced by the method of the present invention are laminated in the thickness direction. More specifically, examples of the laminated nonwoven fabric include a laminated nonwoven fabric having a layer structure of spunbonded (S)-meltblown (M)-spunbonded (S), a laminated nonwoven fabric having a layer structure of spunbonded (S)-meltblown (M)-air-through (AT), and a laminated nonwoven fabric having a layer structure of air-through (AT)-meltblown (M)-air-through (AT). A laminated nonwoven fabric including a meltblown layer can be produced, for example, by depositing fibers containing a crystal nucleating agent spun by the method of the present invention on a substrate layer made of a spunbonded nonwoven fabric, an air-through nonwoven fabric, etc. to form a meltblown nonwoven fabric (meltblown layer), or by laminating one or more other layers thereon. Between the meltblown layer and a layer other than the meltblown layer, for example, between the substrate layer and the meltblown layer, or between any layers of the laminated nonwoven fabric, any joining means, for example, heat embossing, may be integrated. When the nonwoven fabric to be measured has a multi-layer structure integrated with a substrate such as a spunbonded nonwoven fabric or an air-through nonwoven fabric, the average fiber diameter of the constituent fibers is measured with the focus on the meltblown layer.

[0036] The water pressure resistance of the meltblown nonwoven fabric produced by the production method according to this embodiment will be described. The water pressure resistance can be measured by the following measurement method. [Method of measuring water pressure resistance] Water pressure resistance is measured in accordance with the water resistance test specified in JIS L 1092. If the size of the test piece does not meet the regulation, a device with a reduced measurement area can be assembled so that water hits the test piece of a sampleable area, and the measurement can be performed in the same manner. Measurements are made on 10 test pieces, and the average value is regarded as the water pressure resistance of the sample.

[0037] The meltblown nonwoven fabric according to the present embodiment has excellent water pressure resistance and is useful, for example, as a back sheet of absorbent articles such as sanitary napkins and disposable diapers, a constituent sheet of a three-dimensional guard, etc. In addition, it has excellent filtering properties and is useful as a filter material for various separation membranes and sanitary masks, etc.

[0038] The uses of the melt-blown nonwoven fabric according to the present invention are not particularly limited, and it can be used for various purposes by making the most of its characteristics. For example, the meltblown nonwoven fabric according to the present invention is laminated on an absorbent body of an absorbent article. The absorbent article is used mainly to absorb and retain liquids discharged from the body, such as urine and menstrual blood. Furthermore, according to the absorbent article and its manufacturing method of the present invention, by including a step of laminating the meltblown nonwoven fabric on the absorbent body of the absorbent article, it is possible to provide an absorbent article that is less likely to leak liquid by laminating the meltblown nonwoven fabric with finer fibers and improved water pressure resistance on the absorbent body. An absorbent article typically comprises a top sheet, a back sheet, and a liquid-retentive absorbent interposed between the two sheets. The absorbent article may further comprise various members according to the specific use of the absorbent article. Such members are known to those skilled in the art. For example, when the absorbent article is a disposable diaper, a sanitary napkin, or an incontinence pad, one or more pairs of three-dimensional guards can be arranged on both sides in the longitudinal direction along the front-rear direction of the wearer. The three-dimensional guard has a fixed end and a free end, and preferably an elastic member is arranged near the free end.

[0039] The melt-blown nonwoven fabric according to the present invention can be used as a back sheet or a constituent sheet of a three-dimensional guard, which are required to be water-resistant, a top sheet or a constituent sheet of a back sheet or a three-dimensional guard, which are required to be able to conceal the color of menstrual blood, urine, etc., of such absorbent articles. When the back sheet of an absorbent article is formed from a laminated sheet of a resin film and an exterior nonwoven fabric covering the non-skin-facing side thereof, the melt-blown nonwoven fabric according to the present invention may be used in place of the resin film, the exterior nonwoven fabric, or the entire back sheet. It can also be used as a filter material for a sanitary mask.

[0040] The melt-blown nonwoven fabric manufacturing method, the absorbent article manufacturing method, the melt-blown nonwoven fabric, and the absorbent article of the present invention are not limited to the above-mentioned embodiments and can be appropriately modified. For example, the melt-blown nonwoven fabric of the present invention may be excellent in only one of water resistance and filtering property. EXAMPLES

[0041] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "mass % (wt%)". In Examples 1 to 4 and Comparative Examples 1 and 2 in Table 1, the spinning conditions were the same, polypropylene resin (PP) with MFR of 1200 g / 10 min was used as the thermoplastic resin, Gelall MD was used as the dissolution type crystal nucleating agent, and the amount of nucleating agent added was changed. The nucleating agent precipitation temperature T [°C] and the complex viscosity ratio (η T-10 / η T ), average fiber diameter [nm] and water pressure resistance [mmAq.] for the examples and comparative examples are shown. In Reference Example 1 in Table 1, the spinning conditions are as shown in Table 1, polypropylene resin (PP) with MFR of 1300 g / 10 min is used as the thermoplastic resin, Gelall MD is used as the soluble crystal nucleating agent, and the amount of nucleating agent added is 0.1 mass %. The measurement results of the reference example of the average fiber diameter [nm] and water pressure resistance [mmAq.] are shown.

[0042] [Examples 1 to 4] In Examples 1 and 2, the amount of nucleating agent added was 0.3 mass%, and in Examples 3 and 4, the amount of nucleating agent added was 0.5 mass%. Note that Examples 1 and 2, and Examples 3 and 4, have different basis weights. Basis weight is mass per unit area, and is synonymous with grammage. In Examples 1 and 3, the basis weight was 5 g / m 2 In Examples 2 and 4, the basis weight is 10 g / m 2 did.

[0043] [Comparative Examples 1-2, Reference Example 1] Comparative Example 1 shows a case where no soluble crystal nucleating agent was added, and Comparative Example 2 shows a case where the amount of nucleating agent added was 1.0 mass%. Reference Example 1 shows a case where the MFR of polypropylene resin (PP) was 1300 g / 10 min and the amount of nucleating agent added was 0.1 mass%. 〔evaluation〕 For each of the melt-blown nonwoven fabrics obtained in the Examples, Comparative Examples, and Reference Examples, the nucleating agent precipitation temperature, the complex viscosity ratio, the average fiber diameter of the constituent fibers, and the water pressure resistance were measured by the methods described above. The results are shown in Table 1.

[0044] [Table 1]

[0045] As is clear from the measurement results shown in Table 1, the melt-blown nonwoven fabrics obtained in Examples 1 to 4, which contain a thermoplastic resin polyolefin and a soluble crystal nucleating agent as a thermoplastic resin composition and have a precipitation temperature of 150°C to 185°C, have an average fiber diameter significantly smaller than those in Comparative Examples 1 and 2 and Reference Example 1. Normally, in order to reduce the average fiber diameter, it is necessary to increase the amount of hot air used, but in the manufacturing method of the present invention, the average fiber diameter can be reduced with the same amount of hot air used. For example, comparing Example 1 with Comparative Example 2, it can be seen that the average fiber diameter of Example 1 is smaller by 100 nm or more. The complex viscosity ratio value of the thermoplastic resin composition is 1.5 or more in Examples 1 to 4 and Comparative Example 2. In Comparative Example 2, the complex viscosity ratio value satisfies 1.5 or more, but the fiber diameter is not smaller than that in Examples 1 to 4. In the case of Comparative Example 2, it is presumed that the precipitation temperature is as high as 195°C, so that the molten material discharged from the nozzle hardens before it can be sufficiently stretched, and thus the fiber diameter is suppressed from being thinned to the fiber diameter of Examples 1 to 4.

[0046] In the case of Comparative Example 1, in which the thermoplastic resin composition does not contain a soluble crystal nucleating agent, the fiber diameter was larger than those of Examples 1 to 4 because no soluble crystal nucleating agent was blended. In Reference Example 1, the amount of soluble crystal nucleating agent added was small at 0.1 mass %, so the precipitation temperature was 150° C. or less, as shown in Table 2 below. It is presumed that the nucleating agent was not sufficiently precipitated in the region where the yarn breakage occurred, and the diameter was not sufficiently reduced. In addition, in Examples 1 and 3, the water pressure resistance is higher than that of Comparative Examples 1 and 2 at the same basis weight. 2 Despite this, the weight is 10g / m 2It is believed that this is due to the fact that the fiber diameter is made thinner, which increases the density of the accumulated fibers. In Examples 2 and 4, at the same basis weight, the water pressure resistance is higher than that of Reference Example 1. This is presumably due to the fact that the fiber diameter is similarly made thinner, resulting in a higher density of the deposited fibers.

[0047] From these results, it can be seen that in order to improve the water pressure resistance while reducing the fiber diameter, it is important that the precipitation temperature of the soluble crystal nucleating agent is 150°C or higher and 185°C or lower, and that the complex viscosity ratio of the thermoplastic resin composition is 1.5 or higher, as in the manufacturing method of the melt-blown nonwoven fabric described in this embodiment.

[0048] Next, the relationship between the type of soluble crystal nucleating agent and the viscosity of the thermoplastic resin composition when the soluble crystal nucleating agent precipitates will be described with reference to Table 2. Table 2 shows the results of an experiment on the relationship between the type and amount of soluble crystal nucleating agent, and the precipitation temperature and the complex viscosity ratio when the MFR of polypropylene resin (PP) was changed.

[0049] [Table 2]

[0050] The nonwoven fabric of Experiment 1 corresponds to the nonwoven fabric of Reference Example 1 in Table 1, the nonwoven fabric of Experiment 2 corresponds to the nonwoven fabric of Examples 1 and 2 in Table 1, the nonwoven fabric of Experiment 3 corresponds to the nonwoven fabric of Examples 3 and 4 in Table 1, and the nonwoven fabric of Experiment 4 corresponds to the nonwoven fabric of Comparative Example 2 in Table 1, and each was produced under the spinning conditions shown in Table 1. In Experiments 5 and 9, the MFR of polypropylene resin (PP), the type of soluble crystal nucleating agent, and the amount of nucleating agent added were changed as shown in Table 2, and the nonwoven fabric was produced under the same spinning conditions as in Reference Example 1 in Table 1. In Experiments 6, 7, 8, and 10, the MFR of polypropylene resin (PP), the type of soluble crystal nucleating agent, and the amount of nucleating agent added were changed as shown in Table 2, and the nonwoven fabric was produced under the same spinning conditions as in Example 1 in Table 1. The nonwoven fabrics in Experiments 1 to 4 were made using Gelall MD as a molten crystal nucleating agent to be blended into the thermoplastic resin composition, whereas different types of molten crystal nucleating agents were used in Experiments 5 to 10. The nonwoven fabrics in Experiments 5 and 6 used Gelall D as a molten crystal nucleating agent, those in Experiments 7 and 8 used Gelall DXR as a molten crystal nucleating agent, and those in Experiments 9 and 10 used Rikaclear PC1 as a molten crystal nucleating agent.

[0051] Comparing Experiment 2 with Experiments 6, 8, and 10, it can be seen that even if the type of soluble crystal nucleating agent is different, by setting the amount added within an appropriate range, for example, the above-mentioned preferred range of more than 0.1% and not more than 1.0%, the precipitation temperature and the complex viscosity ratio can be set to values ​​within the preferred ranges specified in the present invention (precipitation temperature of 150°C or higher and 185°C or lower, complex viscosity ratio of 1.5 or higher). On the other hand, as in Experiment 1 corresponding to Reference Example 1 in Table 1, when the soluble nucleating agent is only 0.1% by mass, the precipitation temperature and the complex viscosity ratio are outside the preferred ranges defined in the present invention. The same can be said for Experiments 5 and 9 in which the type of soluble nucleating agent was changed. Also, as in Experiment 7, when the soluble nucleating agent is Gelall DXR, the precipitation temperature and the complex viscosity ratio are outside the preferred ranges defined in the present invention even when the amount added is 0.3% by mass. Since the precipitation temperature and the complex viscosity ratio increase when the amount added of the soluble nucleating agent is increased, when the soluble nucleating agent is Gelall DXR, the precipitation temperature and the complex viscosity ratio are outside the preferred ranges defined in the present invention even when the amount added is 0.1% by mass.

[0052] From these results, even if the type of soluble nucleating agent is different, by appropriately adjusting the amount of addition, the precipitation temperature of the soluble nucleating agent can be within the preferred range specified in the present invention. In addition, since the complex viscosity increases as its value increases, the viscosity increases, it can be seen that the material used for the molten nucleating agent is not limited to Gelall MD, and other types of molten nucleating agents can also achieve the same effect as Gelall MD.

[0053] In the melt-blown nonwoven fabric produced by the production method of the present invention and the melt-blown nonwoven fabric of the present invention, the basis weight (grammage) of the produced melt-blown nonwoven fabric is 5 g / m 2 In the case of , the water pressure resistance is 900mmAq. or more, and the basis weight of the melt-blown nonwoven fabric to be manufactured is 10g / m 2 In this case, it is preferable that the water pressure resistance is 1100mmAq. or more. The melt-blown nonwoven fabric produced by the production method of the present invention and the melt-blown nonwoven fabric of the present invention preferably have a basis weight (grammage) of 12 g / m from the viewpoint of suppressing the amount of raw materials used and producing a nonwoven fabric that is lightweight yet has high water resistance (water pressure resistance). 2 Less than 10 g / m 2 Less than 8 g / m, more preferably 2 , particularly preferably 7 g / m 2 The lower limit is not particularly limited, but from the viewpoint of securing strength, for example, 2 g / m 2 More preferably, it is 3 g / m 2 More preferably, 4 g / m 2 More preferably, 5 g / m 2 That's all. From the viewpoint of productivity, it is preferable that the total discharge rate of the resin discharged from the nozzle is 10 kg / m / hr or more, and from the viewpoint of reducing the diameter, it is preferable that the single-hole discharge rate of the resin discharged from the nozzle is 0.1 g / min / hole or less.

Claims

1. A method for producing a melt-blown nonwoven fabric, comprising a spinning step of heating and melting a thermoplastic resin composition, discharging the melt from a nozzle, and stretching the discharged melt by an air current to form a fiber, The thermoplastic resin composition contains a polyolefin as a thermoplastic resin and a soluble crystal nucleating agent, the precipitation temperature at which the solution-type crystal nucleating agent precipitates from the molten state of the thermoplastic resin composition is 150° C. or higher and 185° C. or lower; The thermoplastic resin composition has a complex viscosity η at a temperature 10° C. lower than the precipitation temperature. T-10 The complex viscosity at the precipitation temperature is η T Then, η T-10 η T The ratio to η T-10 / T is 1.5 or more, The polyolefin is polypropylene (provided that the following (a) to (f) (a) [mmmm]=20 to 60 mol% (b) [rrrr] / (1-[mmmm])≦0.1 (c) [rmrm]>2.5 mol% (d) [mm]×[rr] / [mr] 2 ≦2.0 (e) Mass average molecular weight (Mw) = 10,000 to 200,000 (f) Molecular weight distribution (Mw / Mn)<4 (excluding low crystalline polypropylene satisfying the above.) A method for producing a meltblown nonwoven fabric.

2. The method for producing a melt-blown nonwoven fabric according to claim 1, wherein the soluble crystal nucleating agent is a dibenzylidene sorbitol or an amide compound.

3. The method for producing a melt-blown nonwoven fabric according to claim 1 or 2, wherein the soluble crystal nucleating agent is 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol.

4. The method for producing a melt-blown nonwoven fabric according to any one of claims 1 to 3, wherein the amount of the soluble crystal nucleating agent added in the thermoplastic resin composition is more than 0.1% by mass and less than 1.0% by mass.

5. The method for producing a melt-blown nonwoven fabric according to any one of claims 1 to 4, wherein the temperature of the thermoplastic resin composition before being discharged from the nozzle is 200°C or higher.

6. The method for producing a melt-blown nonwoven fabric according to any one of claims 1 to 5, wherein the average fiber diameter of the melt-blown nonwoven fabric produced is 900 nm or less.

7. A method for producing a melt-blown nonwoven fabric described in any one of claims 1 to 6, wherein the polypropylene has a melt flow rate of 500 g / 10 min or more at a temperature of 230°C and a load of 2160 g.

8. A method for producing a melt-blown nonwoven fabric described in any one of claims 1 to 7, wherein the single-hole discharge rate of the thermoplastic resin composition discharged from the nozzle is 0.1 g / min / hole or less.

9. A method for manufacturing an absorbent article, comprising a step of laminating a meltblown nonwoven fabric manufactured by the manufacturing method according to any one of claims 1 to 8 on an absorbent body of the absorbent article.

Citation Information

Patent Citations

  • Production of polypropylene ultrafine fiber

    JP1988006107A

  • Production of polyolefin fiber

    JP1990084531A

  • Particulate additive composition for polyolefin, its preparation process, polyolefin resin composition containing the additive composition and its molded body

    JP2002332359A

  • Elastic nonwoven fabric, process for producing the same, and textile product

    JP2009079341A

  • Melt-blown nonwoven fabric

    JP2018095973A