Mesophase pitch manufacturing process

The heat treatment and solvent extraction process for mesophase pitch production addresses the issue of poor mechanical properties in carbon fibers by increasing the formation of mesophase aggregates, resulting in fibers with enhanced molecular orientation and mechanical performance.

JP7568867B2Active Publication Date: 2024-10-16EXXONMOBIL CHEMICAL PATENTS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023542942
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-15
Filing Date
2022-01-04
Publication Date
2024-10-16
Estimated Expiration
2042-01-04

AI Technical Summary

Technical Problem

Existing methods for producing mesophase pitch for carbon fiber production yield carbon fibers with poor mechanical properties due to low molecular orientation, necessitating improved systems and methods for producing mesophase pitch.

Method used

A process involving heat treatment of heavy feedstocks under severe conditions, followed by solvent extraction, to increase the formation of mesophase pitch precursor molecules, resulting in mesophase aggregates with enhanced mechanical properties.

Benefits of technology

The process enhances the yield of mesophase pitch, leading to carbon fibers with improved molecular orientation and superior mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568867000011
    Figure 0007568867000011
  • Figure 0007568867000012
    Figure 0007568867000012
  • Figure 0007568867000013
    Figure 0007568867000013
Patent Text Reader

Abstract

A process for producing mesophase pitch is described. The process generally includes providing a feedstock having a T5≧400° F. (204° C.) and a T95≦1,400° F. (760° C.) and heating the feedstock at a temperature in the range of about 420° C. to about 520° C. to produce a heat-treated product comprising an isotropic pitch. Generally, the heating is conducted under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time of heating and Y is the bromine number of the feedstock as measured in accordance with ASTM D1159. The process generally includes providing an isotropic pitch having a solubility blending number (S SU) of at least about 10 SU. BN under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising mesophase pitch, and recovering the mesophase pitch.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of and priority to U.S. Provisional Application No. 63 / 138,051, filed January 15, 2021, the disclosure of which is incorporated herein by reference.

[0002] Field This disclosure relates generally to the production of mesophase pitch for use in the production of carbon fibers. [Background technology]

[0003] background Isotropic pitch and mesophase pitch are carbon-containing feedstocks that can be formed from residues produced during the processing of coal or petroleum feedstocks or by other processes such as acid-catalyzed condensation of small aromatic species. For some grades of carbon fiber, isotropic pitch can be used as the initial feedstock. However, carbon fibers produced from isotropic pitch generally exhibit little molecular orientation and relatively poor mechanical properties. In contrast to carbon fibers formed from isotropic pitch, carbon fibers produced from mesophase pitch exhibit very favorable molecular orientation and relatively superior mechanical properties. Therefore, it would be beneficial to identify systems and / or methods that can improve the ability to produce mesophase pitch suitable for the production of carbon fibers. No. 4,208,267 describes a method for forming mesophase pitch. An isotropic pitch sample is solvent extracted. The extract is then exposed to elevated temperatures in the range of 230° C. to about 400° C. to form mesophase pitch. No. 5,032,250 describes a process for isolating mesophase pitch: isotropic pitch containing mesogens is mixed with a solvent and exposed to dense phase or supercritical conditions to phase separate the mesogens. U.S. Pat. No. 5,259,947 describes a method for forming a solvated mesophase comprising the steps of: (1) combining a carbonaceous aromatic isotropic pitch with a solvent; (2) applying sufficient agitation and sufficient heat to cause any insoluble material in the mixture to form liquid solvated mesophase droplets; and (3) recovering the insoluble material as a solid or fluid solvated mesophase. Other references that may be of interest include U.S. Patent No. 9,222,027, U.S. Patent Publication No. 2019 / 0382665, and U.S. Patent Publication No. 2020 / 0181497. [Brief description of the drawings]

[0004] [Figure 1] 1 is a schematic diagram of a non-limiting example of a process of the present disclosure. [Diagram 2] 1 is a polarizing optical microscope photograph of the isotropic pitch (Pitch A) used to carry out Example 2. [Diagram 3] 1 is a polarizing optical microscope photograph of the isotropic pitch (Pitch B) used to carry out Example 3. [Figure 4] 1 is a polarizing optical microscope photograph of the solid product recovered in Example 2. [Diagram 5] 1 is a polarizing optical microscope photograph of the solid product recovered in Example 3. Summary of the Invention

[0005] overview In accordance with the present disclosure, it has now been discovered that thermal treatment of a heavy feedstock under conditions of sufficient severity relative to the bromine number of the feedstock advantageously enables increased formation of mesophase pitch precursor molecules which can then be made into mesophase aggregates via solvent extraction. Accordingly, in one aspect, the disclosure provides a process for producing mesophase pitch, comprising the steps of providing a feedstock having a T5≧400° F. (204° C.) and a T95≦1,400° F. (760° C.); heating the feedstock at a temperature in the range of about 420° C. to about 520° C. to produce a heat-treated product comprising an isotropic pitch, the heating being conducted under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time of heating and Y is the bromine number of the feedstock as measured in accordance with ASTM D1159; and treating the isotropic pitch to a solubility blending number (S SU) of at least about 10 SU. BN ), under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising mesophase pitch, and recovering the mesophase pitch.

[0006] In a further aspect, the present disclosure relates to a mesophase pitch produced by the aforementioned process. In a further aspect, the present disclosure relates to carbon fibers produced from the aforementioned mesophase pitch. In yet another aspect, the disclosure provides a process for producing mesophase pitch comprising the steps of providing a feedstock comprising at least one member selected from the group consisting of main column bottoms (MCB), hydroprocessed MCB, steam cracker tar, hydrotreated steam cracker tar, vacuum resid, deasphalted residue or rock, and mixtures or combinations thereof; and heating the feedstock at a temperature in the range of about 420° C. to about 520° C. to produce a heat-treated product comprising isotropic pitch, the heating satisfying the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time of heating and Y is the equivalent reaction time of the ASTM A2014-10022 equivalent reaction time. D1159), contacting the isotropic pitch with a solvent selected from the group consisting of single ring aromatics, two ring aromatics, paraffins, midcut solvents, and mixtures or combinations thereof, under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising mesophase pitch; and recovering the mesophase pitch. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Various embodiments described herein provide a process for the production of mesophase pitch via solvent extraction of an isotropic pitch formed by heat treating a heavy feedstock having a T5≧400° F. (204° C.) and a T95≦1,400° F. (760° C.) under sufficiently severe conditions. Without wishing to be bound by theory, it is believed that the isotropic pitch has a solubility blending number (S ) of a minimum of 10 solvency units (“SU”). BN) is believed to advantageously permit dissolution of large aromatic molecules with low hydrogen content in the isotropic pitch without interfering with the development of mesophase aggregates. Typically, heat treatment of the heavy feedstock is conducted at a temperature in the range of about 420° C. to about 520° C. and for a residence time of 5 minutes to 8 hours, more preferably about 5 minutes to about 1 hour, and most preferably 5 minutes to 30 minutes, for example about 10 minutes to about 30 minutes. Without wishing to be bound by theory, it is believed that heat treatment of the heavy feedstock at a sufficiently high severity relative to the reactivity of the heavy feedstock as measured by its bromine number advantageously results in increased formation of mesophase pitch precursor molecules that can then be converted into mesophase aggregates via solvent extraction, thereby increasing the mesophase pitch yield in the solid product recovered from the insoluble fraction.

[0008] All numerical values ​​in the detailed description and claims of this application are modified by the term "about" or "approximately" to account for experimental error and variations that one of ordinary skill in the art would expect. Unless otherwise indicated, room temperature is about 23° C. As used herein, "wt%" means percentage by weight, "vol%" means percentage by volume, "mol%" means percentage by mole, "ppm" means parts per million, and "ppm wt" and "wppm" are used interchangeably to mean parts per million on a mass basis. All "ppm" as used herein is ppm by weight unless otherwise specified. All concentrations herein are expressed based on the total amount of the composition in question. All ranges described herein should include the endpoints as two specific embodiments, unless otherwise specified or indicated to the contrary.

[0009] definition For purposes of this specification and the appended claims, the following terms are defined. As used herein, the term "asphaltene" refers to a material that can be obtained from crude oil and has an initial boiling point of about 1,200° F. (650° C.) and is insoluble in straight-chain alkanes, i.e., paraffinic solvents, such as hexane and heptane. As used herein, the term "equivalent reaction time (ERT)" refers to the severity of an operation expressed as the number of seconds of residence time for a reaction having an activation energy of 54 kcal / mole in a reactor operating at 468° C. The ERT of an operation is calculated as follows:

[0010]

number

[0011] where W is the residence time of the operation in seconds; e is 2.71828; E a is 225,936 J / mol; R is 8.3145 J mol -1 ·K -1 ;T rxn is the operating temperature expressed in Kelvin. In very general terms, the reaction rate doubles for every 12-13°C increase in temperature. Thus, a residence time of 60 seconds at 468°C is equivalent to 60 ERT, and increasing the temperature to 501°C would increase the operation severity by a factor of five, or 300 ERT. Expressed another way, 300 seconds at 468°C is equivalent to 60 seconds at 501°C, and both sets of conditions should result in the same product mixture and distribution.

[0012] As used herein, the term "pitch" refers to a viscoelastic carbonaceous residue obtained from the distillation of petroleum, coal tar, or organic materials. Unless otherwise specified herein, the term "pitch" refers to petroleum pitch (i.e., pitch obtained from the distillation of petroleum). As used herein, the term "isotropic pitch" refers to a pitch that includes molecules that are not aligned in an optically ordered liquid crystal state. As used herein, the term "main column bottoms (MCB)" refers to the bottoms fraction from a fluid catalytic cracking process. As used herein, the term "mesogen" refers to a mesophase pitch former or a mesophase pitch precursor. As used herein, the term "mesophase pitch" refers to pitch that is structurally ordered, optically isotropic liquid crystal. The mesophase structure can be described and characterized by a variety of techniques, such as optical birefringence, light scattering, or other scattering techniques. As used herein, "mid-cut solvent" refers to the recycled portion of the product produced during the upgrading of steam cracker tar, the recycled portion having an atmospheric boiling point range of about 350°F (177°C) to about 850°F (454°C).

[0013] Test Method Solubility Blending Number (S BN ) and insoluble count (I N ) Solubility Blending Number (S BN ) and insoluble count (I N ) is a value that can be used to characterize the solubility properties of the deasphalting solvents described herein. The first step in determining the insolubility number and solubility blending number for the deasphalting solvent described herein is to determine whether the deasphalting solvent contains n-heptane insoluble asphaltenes. This is accomplished by blending one volume of the deasphalting solvent with five volumes of n-heptane and determining whether the asphaltenes are insoluble. Any conventional method may be utilized. One possibility is to observe a drop of the test liquid mixture and deasphalting solvent blend between a glass slide and a glass cover slip under an optical microscope at 50-600x magnification. If the asphaltenes are in solution, very few, if any, dark particles will be observed. If the asphaltenes are insoluble, many dark, usually brownish, particles, usually 0.5-10 microns in size, will be observed. Another possible method is to place a drop of the test liquid mixture and deasphalting solvent blend on a piece of filter paper and allow it to dry. If the asphaltenes are insoluble, a dark ring or annulus will be seen around the center of the tan spot created by the solvent. If the asphaltenes are soluble, the color of the solvent spot will be relatively non-uniform. If the deasphalting solvent is found to contain n-heptane insoluble asphaltenes, continue with the procedures described in the next three paragraphs to determine the insolubility number and solubility blending number. If the deasphalting solvent is found to not contain n-heptane insoluble asphaltenes, assign a value of zero to the insolubility number and determine the solubility blending number by the procedures described in the section labeled "Deasphalting Solvent Without Asphaltenes."

[0014] Asphaltene-containing deasphalting solvent I. Deasphalting Solvents Containing Asphaltene, for example Heavy Oils Including Residual Oils N and S BNDetermination of solubility requires examining the solubility of the deasphalting solvent in the test liquid mixture at least in two volume ratios of the deasphalting solvent to the test liquid mixture. The test liquid mixtures are prepared by mixing two liquids in various ratios. One liquid is non-polar (Test Solvent A) and is a solvent for the asphaltenes in the deasphalting solvent. The other liquid is non-polar (Test Solvent B) and is a non-solvent for the asphaltenes in the deasphalting solvent. Test Solvent A is typically toluene and Test Solvent B is typically n-heptane.

[0015] A convenient volume ratio of oil to test liquid mixture is, for example, 1 ml of oil to 5 ml of test liquid mixture for the first test. Various mixtures of the test liquid mixture are then prepared by blending n-heptane and toluene in various known ratios. Each of these is mixed with the deasphalting solvent in a selected volume ratio of deasphalting solvent to test liquid mixture. Each of these is then determined to be soluble or insoluble in asphaltenes. Any convenient method may be utilized. For example, a drop of the blend of test liquid mixture and deasphalting solvent can be observed under an optical microscope using transmitted light between a glass slide and a glass cover slip at 50-600x magnification. If the asphaltenes are in solution, very few, if any, dark particles will be observed. If the asphaltenes are insoluble, many dark, usually brownish, particles, usually 0.5-10 microns in size, will be observed. The results of blending the deasphalting solvent with all the test liquid mixtures are regular as the toluene percentage in the test liquid mixture increases. The desired value will be between the minimum toluene percentage that will dissolve the asphaltene and the maximum toluene percentage that will precipitate the asphaltene. Further test liquid mixtures with toluene percentages between these limits are prepared and blended with oil at the selected volume ratio of oil to test liquid mixture to determine whether the asphaltene is soluble or insoluble. The desired value will be between the minimum toluene percentage that will dissolve the asphaltene and the maximum toluene percentage that will precipitate the asphaltene. This process continues until the desired value is measured within the desired accuracy. Finally, the desired value is considered to be the average of the minimum toluene percentage that will dissolve the asphaltene and the maximum toluene percentage that will precipitate the asphaltene. This is done by adding the volume ratio R of the selected oil to the test liquid mixture. 1 The first data point T in 1 This test is called the toluene equivalence test.

[0016] The second data point can be determined by the same process as the first data point, simply by selecting a different volume ratio of the deasphalting solvent to the test liquid mixture. Alternatively, a lower toluene percentage can be selected than that determined for the first data point, and the test liquid mixture can be added to a known volume of oil until asphaltenes just begin to precipitate. At that point, the selected toluene percentage T in the test liquid mixture can be selected. 2 The volume ratio R of the oil and test liquid mixture in 2 is the second data point. Since the precision of the final numerical value increases as the second data point is further away from the first data point, the preferred test liquid mixtures for determining the second data point are 0% toluene or 100% n-heptane. This test is called the heptane dilution test. Insoluble number I N is defined as follows:

[0017]

number

[0018] Soluble Blending Number I N is defined as follows:

[0019]

number

[0020] Asphaltene-free deasphalting solvent If the deasphalting solvent does not contain asphaltenes, the insolubility number is zero. However, the determination of the solubility blending number for a deasphalting solvent that does not contain asphaltenes requires the use of a test oil containing asphaltenes for which the insolubility number and solubility blending number have already been determined using the procedure just described. First, blend one volume of the test oil with five volumes of the deasphalting solvent. Insoluble asphaltenes can be detected by the microscope or spot techniques described above. If the oils are very viscous (greater than 100 centipoise), they may be heated to 100°C during blending and then cooled to room temperature to look for insoluble asphaltenes. Spot tests may also be performed at 50°C to 70°C in an oven for viscous oil blends. If insoluble asphaltenes are detected, the deasphalting solvent is a non-solvent for the test oil and the procedure in the next paragraph should be followed. However, if no insoluble asphaltenes are detected, the deasphalting solvent is a solvent for the test oil and the procedure in the paragraph following the next paragraph should be followed.

[0021] If insoluble asphaltenes are detected when blending one volume of test oil with five volumes of deasphalting solvent, add small volume increments of deasphalting solvent to 5 ml of test oil until insoluble asphaltenes are detected. NSO is equal to the average of the total volume of deasphalting solvent added for the volume increment just before insoluble asphaltenes are detected and the total volume added when insoluble asphaltenes are first detected. The magnitude of the volume increment may be reduced to the volume increment required for the desired accuracy. This is called the non-solvent oil dilution test. S BNTO is the solubility blending number of the test oil, and I NTO If is the insolubility number of the test oil, then the solubility blending number S of the non-solvent oil BN is given by the following formula:

[0022]

number

[0023] If no insoluble asphaltenes are detected when one volume of the test oil is blended with five volumes of the deasphalting solvent, the deasphalting solvent is a solvent oil for the test oil. The volume ratio R of the same oil to the test liquid mixture used to determine the insolubility number and solubility blending number for the test oil is TO However, now, instead of toluene and n-heptane, various mixtures of test liquids are prepared by blending various known ratios of petroleum and n-heptane. Each of these mixtures is compared with R TO Each of these mixtures is then examined by microscopy or the spot test method described above to determine whether the asphaltene is soluble or insoluble. The results of blending the oil with all test liquid mixtures are orderly with increasing percentage of deasphalted solvent in the test liquid mixture. The desired value will be between the minimum percentage of oil that will dissolve the asphaltene and the maximum percentage of deasphalted solvent that will precipitate the asphaltene. Further test liquid mixtures are prepared with percentages of deasphalted solvent between these limits, and the volume ratio of the selected test oil to test liquid mixture (R TO ) with the test oil to determine whether the asphaltene is soluble or insoluble. The desired value will be between the minimum deasphalted solvent percentage that will dissolve the asphaltene and the maximum deasphalted solvent percentage that will precipitate the asphaltene. This process continues until the desired value is determined within the desired accuracy. Ultimately, the desired value is deemed to be the average of the minimum deasphalted solvent percentage that will dissolve the asphaltene and the maximum deasphalted solvent percentage that will precipitate the asphaltene. This is done by blending the selected test oil with the test liquid mixture by volume R TO Data point T at SO This test is called the solvent oil equivalence test. TO The test oil and test liquid mixture volume ratio R TOIf the data points are already measured, the solubility blending number S of the deasphalting solvent BN is given by the following formula:

[0024]

number

[0025] Mesophase pitch content by optical microscopy. Unless otherwise specified herein, the mesophase pitch content of a sample is determined by optical microscopy according to the following procedure: A digital image of the sample is made using an optical microscope. A histogram of the total number of pixels of the digital image is then created by color intensity in the light intensity regions corresponding to mesophase pitch due to its high refractive index. The image is then divided into mesophase pitch and non-mesophase pitch areas by thresholding in areas having an intensity below a certain threshold corresponding to mesophase pitch. The non-mesophase pitch area of ​​the image is then subtracted, and then the total amount of mesophase pitch area of ​​the image is divided by the total area of ​​the image to obtain an estimate of the mesophase pitch content of the sample in area % (which can be extrapolated to correspond to a vol % estimate). The following provides a more detailed description of certain aspects of the present invention. Although the following description is directed to certain aspects, it will be appreciated by those skilled in the art that these are merely exemplary and that the present invention can be implemented in other ways. References to the "invention" may refer to one or more, but not necessarily all, of the inventions defined by the claims. The use of headings is merely for convenience and should not be construed as limiting the scope of the invention to certain aspects.

[0026] heavy raw materials In the process of the present disclosure, the heavy feed may be characterized by a boiling range. One option for defining the boiling range is to use the initial boiling point of the feed and / or the final boiling point of the feed. Another option, which may in some cases provide a more representative description of the feed, is to characterize the feed based on the amount of the feed boiling at one or more temperatures. For example, the "T5" boiling point of a feed is defined as the temperature at which 5 wt% of the feed boils. Similarly, the "T95" boiling point is the temperature at which 95 wt% of the feed boils. The percentage of the feed boiling at a given temperature can be determined, for example, by the method specified in ASTM D2887 (or by the method of ASTM D7169 if ASTM D2887 is not suitable for a particular cut). In general, the heavy feed may have a T5 ≧ 400°F (204°C) and a T95 ≦ 1,400°F (760°C). Examples of such heavy feeds include those having a 1,050° F.+ (566° C.+) fraction. In some embodiments, the 566° C.+ fraction may represent 1 wt. % or more (i.e., T99 of 566° C. or more), or 2 wt. % or more (T98 of 566° C. or more), or 10 wt. % or more (T90 of 566° C. or more), or 15 wt. % or more (T85 of 566° C. or more), or 30 wt. % or more (T70 of 566° C. or more), or 40 wt. % or more (T60 of 566° C. or more), for example, from about 1 wt. % to about 40 wt. %, or from about 2 wt. % to about 30 wt. % of the heavy feed.

[0027] The heavy feedstock of the present disclosure may be characterized by its reactivity as measured by its bromine number. The heavy feedstock of the present disclosure may have a bromine number of ≧3, or ≧5, or ≧10, or ≧30, or ≧40, for example, from about 3 to about 50, or from about 5 to about 40, or from about 10 to about 30, as measured according to ASTM D1159. The heavy feedstock of the present disclosure may be characterized by its aromatic content. The heavy feedstock of the present disclosure may contain about 40 mol% or more, or about 50 mol% or more, or about 60 mol% or more, for example, up to about 75 mol% or perhaps even more, of aromatic carbon. The aromatic carbon content of the heavy feedstock may be determined according to ASTM D5186. The heavy feedstock of the present disclosure may be characterized by an average carbon number. The heavy feedstock of the present disclosure may be composed of hydrocarbons having an average carbon number of about 33 to about 45 (e.g., about 35 to about 40, or about 37 to about 42, or about 40 to about 45). Heavy feedstocks of the present disclosure may be characterized by a microcarbon residue (MCR) as measured by ASTM D4530-15. Heavy feedstocks of the present disclosure may have an MCR of about 5 wt% or greater (e.g., about 5 wt% to about 45 wt%, or about 10 wt% to about 45 wt%). The heavy feedstocks of the present disclosure may be characterized by their hydrogen content. The heavy feedstocks of the present disclosure generally have a hydrogen content of about 6 wt% to about 11 wt%, for example, about 6 wt% to about 10 wt%. The heavy feedstock of the present disclosure may be characterized by a cumulative concentration of polynuclear aromatic hydrocarbons (PNAs) and polycyclic aromatic hydrocarbons (PAHs). The heavy feedstock of the present disclosure may have a cumulative concentration of partially hydrogenated PNAs and partially hydrogenated PAHs of about 20 wt% or more (e.g., about 50 wt% to about 90 wt%).

[0028] In some embodiments, suitable heavy feedstocks can contain from about 50 wppm to about 10,000 wppm or more elemental nitrogen (i.e., the mass of nitrogen in the various nitrogen-containing compounds in the feedstock). Additionally or alternatively, the heavy feedstock can contain from about 100 wppm to about 20,000 wppm elemental sulfur, preferably from about 100 wppm to about 5,000 wppm elemental sulfur. The sulfur will typically be present as organically bound sulfur. Examples of such sulfur compounds include the class of heterocyclic sulfur compounds, such as thiophene, tetrahydrothiophene, benzothiophene, and the like, and their homologs and analogs. Other organically bound sulfur compounds include aliphatic, naphthenic, and aromatic mercaptans, sulfides, and disulfides and polysulfides. Examples of suitable heavy feedstocks include, but are not limited to, main column bottoms (MCB), steam cracker tar, vacuum resid, deasphalted residue or lock, hydroprocessed or hydrotreated forms of any of the foregoing, and combinations of any of the foregoing. A preferred heavy feedstock may be hydroprocessed MCB. Another preferred example of a heavy feedstock is hydrotreated steam cracker tar. Steam cracker tar and subsequent hydroprocessing may be produced / carried out by any suitable method, for example, as disclosed in U.S. Pat. No. 8,105,479, the entire contents of which are incorporated herein by reference.

[0029] Heat Treatment In the disclosed process, the heavy feedstock typically undergoes a heat treatment step to dealkylate and / or dehydrogenate the heavy feedstock to produce an isotropic pitch. As noted above, without wishing to be bound by theory, it is believed that the heat treatment step, when carried out under conditions of sufficient severity relative to the reactivity of the feedstock, advantageously results in the formation of mesogens in the resulting isotropic pitch that can then be made into mesophase aggregates via solvent extraction. In many cases, the conditions are more severe than those utilized in visbreaking. More specifically, the heat treatment may typically be carried out at a temperature ranging from about 420° C. to about 520° C., preferably from about 480° C. to about 510° C., and with a residence time ranging from about 5 minutes to 8 hours, more preferably from about 5 minutes to about 1 hour, and most preferably from about 5 minutes to about 30 minutes, for example from about 10 minutes to about 30 minutes. Generally, the severity required for the heat treatment step depends on the bromine number of the heavy feedstock. Typically, the severity of the heat treatment conditions required increases as the bromine number of the heavy feedstock decreases. Generally, the heat treatment is carried out under conditions sufficient to satisfy the relationship [X*Y] ≥ 20,000 seconds (e.g., ≥ 30,000 seconds, or ≥ 50,000 seconds, or ≥ 70,000 seconds, or ≥ 200,000 seconds, or ≥ 500,000 seconds, or ≥ 700,000 seconds), where X is the equivalent reaction time of heating and Y is the bromine number of the feedstock. For example, [X*Y] may range from about 20,000 to about 1,000,000 seconds, e.g., from about 30,000 seconds to about 700,000 seconds, or from about 50,000 seconds to about 500,000 seconds, or from about 50,000 seconds to about 100,000 seconds. For example, in embodiments where the heavy feedstock has a bromine number > 10, the minimum ERT of the heat treatment step may be less than or equal to about 2,000 seconds, such as a minimum ERT of 500 seconds. In embodiments where the heavy feedstock has a bromine number < 10, the minimum ERT of the heat treatment step may be greater than about 2,000 seconds, such as a minimum ERT of 10,000 seconds, or alternatively a minimum ERT of 8,000 seconds.

[0030] Suitable pressures for the heat treatment step may range from about 200 psig (1,380 kPa-g) to about 2,000 psig (13,800 kPa-g), for example, from about 400 psig (2,760 kPa-g) to about 1,800 psig (12,400 kPa-g). The heat treatment may be carried out in any vessel, such as a tank, pipe, tubular reactor, or distillation column. Examples of suitable reactor configurations that may be utilized to carry out the heat treatment are described in U.S. Pat. No. 9,222,027, the entire contents of which are incorporated herein by reference. Typically, the thermally treated product is a liquid. In certain embodiments, the thermally treated product may be further processed, such as by flashing, distillation, fractionation, another type of separation based on boiling range, and the like, preferably by vacuum distillation, to produce the isotropic pitch described herein. For example, the thermally treated product will often contain one or more light fractions containing diesel and / or gasoline components and a heavy fraction containing the isotropic pitch described herein. In such embodiments, the yield of the heavy isotropic pitch-containing fraction is typically greater than about 50 wt.%, such as greater than about 60 wt.%, and preferably greater than about 80 wt.%, of the thermally treated product.

[0031] Isotropic Pitch The isotropic pitch resulting from the heat treatment (and any subsequent optional separation steps) may be characterized by a microcarbon residue (MCR) as measured according to ASTM D4530-15. Generally, the isotropic pitch of the present disclosure may have an MCR of 30 wt% or more (e.g., preferably about 50 wt% or more, more preferably about 60 wt% or more). For example, a suitable isotropic pitch may have an MCR in the range of about 30 wt% to about 90 wt%, preferably about 50 wt% to about 90 wt%, more preferably about 60 wt% to about 90 wt%. Typically, the isotropic pitch has an MCR at least 5% greater than the MCR of the heavy feedstock, e.g., at least 10% greater, more preferably at least 20% greater. The isotropic pitch of the present disclosure may be characterized by a softening point measured according to ASTM D3104-14. In general, the isotropic pitch of the present disclosure may have a softening point of about 80° C. or higher, preferably about 100° C. or higher, more preferably about 120° C. or higher, and even more preferably about 200° C. or higher (e.g., preferably in the range of about 80° C. to about 250° C., more preferably in the range of about 100° C. to about 250° C., and even more preferably in the range of about 150° C. to about 250° C.).

[0032] The isotropic pitch of the present disclosure may be characterized by a quinoline insoluble content as measured in accordance with ASTM D2318-15. Generally, the isotropic pitch of the present disclosure may have a quinoline insoluble content of about 1 wt% or more (e.g., preferably about 2 wt% or more, even more preferably about 5 wt% or more, e.g., about 1 wt% to about 10 wt%). The isotropic pitch of the present disclosure may be characterized by a mesophase pitch content. In many cases, the isotropic pitch of the present disclosure may have a mesophase pitch content of greater than about 0.5 wt% and / or greater than about 0.5 vol%, for example, about 0.5 wt% to about 1 wt%, as measured in accordance with ASTM D4616-95(2018). Alternatively, the isotropic pitch of the present disclosure may have a mesophase pitch content of less than 0.5 wt%, for example, about 0 wt% or about 0 vol%, as measured in accordance with ASTM D4616-95(2018). The isotropic pitch of the present disclosure may be characterized by its hydrogen content. In general, the isotropic pitch of the present disclosure may have a hydrogen content of less than about 8 wt% (e.g., preferably less than about 6 wt%, e.g., about 4 wt% to about 6 wt%). The isotropic pitch of the present disclosure may be characterized by a sulfur content. Generally, the isotropic pitch of the present disclosure may have a sulfur content of less than about 2 wt% (e.g., preferably about 1 wt% or less, even more preferably about 0.5 wt% or less), for example, about 0 wt% to about 2 wt%.

[0033] Asphalted solvent In the process of the present disclosure, a suitable deasphalting solvent has a solubility blending number (S BNTypically, the deasphalting solvent has a minimum S of about 10 Solvent Power Units ("SU"). BN For example, suitable deasphalting solvents have an S of about 10 to about 150 SU, such as about 10 to about 130 SU, or about 10 to about 70 SU, or about 10 to about 50 SU, or about 70 to about 130 SU. BN may have: The deasphalting solvent of the present disclosure may be characterized by a boiling point range. In some embodiments, the deasphalting solvent may have an atmospheric boiling point range of approximately 65° C. to 200° C., e.g., about 100° C. to about 175° C. Advantageously, the atmospheric boiling point range of the deasphalting solvent may be less than about 200° C. to facilitate recovery of the solvent from the extraction process described herein, e.g., by distillation.

[0034] Examples of suitable deasphalting solvents include, but are not limited to, C 2 -C 10 Paraffins such as pentane, heptane, and butane; single ring aromatics such as toluene, xylene, ethylbenzene, and trimethylbenzene; polycyclic aromatics such as naphthalene, methylnaphthalene, indane, tetralin, and anthracene; aromatics containing heteroatoms such as pyridine; other heteroatom compounds such as tetrahydrofuran; heavy naphtha, kerosene, and / or light diesel fractions; recycled portions of products generated during the upgrading of heavy oil feedstocks such as steam cracker tar; and other hydrocarbons or hydrocarbon-like fractions having suitable boiling ranges. When the recycled portion of products generated during the upgrading of steam cracker tar is included in the deasphalting solvent, the distillation cut point for the recycled portion can be adjusted to obtain the appropriate boiling range and / or suitable S. BNTypically, the atmospheric boiling range suitable for the recycle portion ranges from about 350°F (177°C) to about 850°F (454°C), i.e., mid-cut solvent. A preferred heavy oil feedstock upgrading process to obtain a mid-cut solvent is further described in U.S. Patent Publication No. 2020 / 0071627, the entire contents of which are incorporated herein by reference. In some embodiments, a paraffin such as hexane or heptane may be included as a co-solvent to improve the solubility parameter of the solvent mixture, preferably in an amount of up to about 90 vol%, for example about 10 vol%, based on the total volume of the solvent. For example, a preferred deasphalting solvent may contain about 0 to about 90 vol% paraffin, such as n-heptane, and about 10 to about 100 vol% toluene, such as 90 vol% toluene and 10 vol% n-heptane, or 80 vol% toluene and 20 vol% n-heptane, or 70 vol% toluene and 30 vol% n-heptane, or 10 vol% toluene and 90 vol% n-heptane. Examples of preferred deasphalting solvents are listed below in their respective related S. BN The values ​​are shown in Table 1 below.

[0035] [Table 1]

[0036] Solvent extraction In the process of the present disclosure, typical solvent extraction conditions include mixing the isotropic pitch with the deasphalting solvent in a volume ratio of about 10:1 to about 1:1, such as about 8:1 or less (deasphalting solvent:isotropic pitch). Typically, the extraction is carried out under conditions suitable for maintaining the solvent in a liquid phase. For example, the extraction may be carried out under extraction conditions including a temperature preferably in the range of about 90°C to about 350°C, preferably about 150°C to about 350°C, even more preferably about 200°C to about 350°C; a total pressure in the range of about 15 psig (about 105 kPa-g) to about 800 psig (about 5,600 kPa-g); and a residence time of about 5 minutes to about 5 hours. Typically, the extraction may be carried out under stirring, such as mechanical stirring using a rotary stirrer. Suitable stirring speeds may range from about 10 RPM to about 8,500 RPM, such as from about 50 RPM to about 5,000 RPM.

[0037] The isotropic pitch is contacted with a deasphalting solvent to produce at least two types of product streams. One type of product stream can be a solvent phase fraction containing the majority of the deasphalting solvent and the majority of the portion of the thermal treatment product or resulting heavy fraction that is soluble in the deasphalting solvent. At least a portion of the deasphalting solvent is typically recovered from the solvent phase fraction, for example by distillation, for recycling and reuse of the recovered deasphalting solvent for solvent extraction. The resulting portion of the solvent phase after recovery of the deasphalting solvent generally contains a supplemental pitch product, otherwise known as deasphalted oil (DAO), which may optionally be recycled to the thermal treatment step. The insoluble fraction (second type of product stream), otherwise known as rock, contains the remaining portion of the isotropic pitch, i.e., the portion that is not soluble in the deasphalting solvent. Typically, the insoluble fraction contains not only mesophase pitch, but also entrained residual solvent and mesophase pitch precursors. In some cases, the softening point of the insoluble fraction may be lowered by mixing the insoluble fraction with a low softening point isotropic pitch (e.g., <200°C) or a low boiling point solvent (e.g., having an atmospheric boiling point in the range of about 200°F (93.3°C) to about 650°F (343°C)). In such embodiments, the low softening point isotropic pitch or low boiling point solvent may be mixed with the insoluble fraction in an amount ranging from about 10 vol% to about 60 vol%, more preferably from about 10 vol% to about 40 vol%, and even more preferably from about 10 vol% to about 20 vol%, based on the total volume of the mixture. Additionally or alternatively, the insoluble fraction may be subsequently subjected to a heat treatment step to convert residual mesophase precursors to mesophase pitch. This optional heat treatment step may be carried out at a temperature ranging from about 300° C. to about 350° C., and may be carried out in the presence of a solvent, preferably a low boiling solvent (e.g., having an atmospheric boiling point ranging from about 200° F. (93.3° C.) to about 650° F. (343° C.)). Any convenient form of separation may be utilized to remove the residual solvent from the insoluble fraction, such as, for example, drying, distillation, fractionation, or another type of separation based on boiling point range. In some cases, the resulting recovered residual solvent may be recycled and reused for solvent extraction.Generally, the yield of the residual solid product recovered from the insoluble fraction obtained after the residual solvent is removed is at least about 10 wt%, preferably at least about 15 wt%, for example, about 10 wt% to about 50 wt%, or about 20 wt% to about 40 wt%. The recovered solid product typically contains about 30 vol% or more of the optically active fraction, for example, about 30 vol% to about 95 vol%, or about 50 vol% to about 85 vol%. In some embodiments, the amount of quinoline insolubles in the recovered solid product can be about 75 wt% or less, or about 50 wt% or less, or about 30 wt% or less, for example, about 0 wt% to about 30 wt%. Additionally or alternatively, the amount of toluene insolubles in the recovered solid product can be about 80 wt% or less, or about 60 wt% or less, or about 40 wt% or less, or about 30 wt% or less, for example, about 0 wt% to about 30 wt%.

[0038] Carbon Fiber The mesophase pitch resulting from the solvent extraction process described herein can be used to form carbon fibers, for example by utilizing a conventional melt spinning process. Melt spinning for the formation of carbon fibers is a known technique. For example, the book "Carbon-Carbon Materials and Composites" contains a chapter by DD Edie and RJ Diefendorf entitled "Carbon Fiber Manufacturing". Another example is the article "Melt Spinning Pitch-Based Carbon Fibers", Carbon, 27(5), p 647, (1989).

[0039] Process Overview The process disclosed herein may be a batch, semi-batch, continuous, semi-continuous process, or any combination thereof, and is preferably a continuous process. FIG. 1 shows an overview of a non-limiting process example 100 of the present disclosure. A heavy feedstock 102 undergoes a heat treatment step in a vessel 104 under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time of heating and Y is the bromine number of the feedstock 102. The heat treatment step carried out in the vessel 104 results in the formation of a heat treatment product 106 comprising isotropic pitch. Often (but not necessarily), the heat treatment product 106 can undergo a separation step to form a heavy fraction 108 comprising isotropic pitch and a light fraction 110. Optionally, the light fraction 110 can be blended with fuel oil. The resulting heat treatment product 106 or the heavy fraction 108 is passed into a solvent extractor 112 along with a deasphalting solvent 114. This results in the formation of a solvent phase fraction 116 that contains most of the deasphalting solvent 114 and most of the portion of the thermally treated product 106 or heavy fraction 108 that is soluble in the deasphalting solvent 114. An insoluble fraction 118, i.e., rock, is also formed that contains most of the insoluble portion of the thermally treated product 106 or heavy fraction 108. Typically, the insoluble fraction 118 contains not only mesophase pitch, but also entrained residual solvent and mesophase pitch precursors. Often, but not necessarily, the insoluble fraction 118 can undergo a subsequent heat treatment stitch (not shown) to convert residual mesophase precursors to mesophase pitch and / or a blending step (not shown) to reduce the softening point of the insoluble fraction 118, as described herein. Often, but not necessarily, a portion of the solvent phase fraction 116 can undergo a separation step to form a recovered solvent stream 122 and a deasphalted oil (DAO) 120. Optionally, at least a portion of the recovered deasphalted solvent stream 122 may be recycled to the solvent extractor 112, either with the deasphalted solvent stream 112 or via a separate stream. Additionally, at least a portion of the DAO 120 and / or at least a portion of the insoluble fraction 118 may be optionally recycled to the vessel 104, either with the heavy feedstock 102 or via a separate stream. The following examples demonstrate the invention, it being understood that numerical modifications and variations are possible and that, within the scope of the appended claims, the invention may be practiced otherwise than as specifically described herein. EXAMPLES

[0040] Example 1: Preparation of isotropic pitch Five isotropic pitch examples (Pitch A, Pitch B, Pitch C, Pitch D, and Pitch E) and one comparative isotropic pitch example (Pitch F) were prepared by thermally treating a heavy feedstock having the properties summarized in Table 2 below under the conditions summarized in Table 3 below. For Pitch A and Pitch B, the heavy fraction was separated by vacuum distillation after thermal treatment (not for Pitch C, Pitch D, Pitch E, or Pitch F). The heavy feedstock used for Pitch A and B was a product resulting from the upgrading of steam cracker tar according to the method described in U.S. Patent Publication No. 2020 / 0071627, the heavy feedstock used for Pitch C, Pitch D, and Pitch F was hydroprocessed MCB, and the heavy feedstock used for Pitch E was (non-hydroprocessed) MCB.

[0041] [Table 2]

[0042] [Table 3]

[0043] Figures 2 and 3 show optical micrographs of pitch A and pitch B, respectively. As is evident from these figures, little or no mesophase was observed. Table 4 below shows the properties of the resulting isotropic pitch examples (pitches A-E) and a comparative pitch example (pitch F).

[0044] [Table 4]

[0045] As can be seen from Table 4, pitches A and C exhibited moderate MCRs, while pitches B and D exhibited high MCRs. These results were expected, considering the higher severity of the heat treatment conditions used to form pitches B and D compared to pitches A and C.

[0046] Examples 2-6 & Comparative Example: Solvent Extraction of Isotropic Pitch In each of Examples 2 to 6 and the Comparative Example, an isotropic pitch (respectively, pitch A, pitch B, pitch C, pitch D, pitch E, or pitch F) was introduced into a 500 ML Hastelloy™ C276 autoclave, and then toluene, i.e., 100 SU of S BN A deasphalting solvent having the formula: ##STR1## was introduced at a ratio of 8 ml of toluene per gram of isotropic pitch. The resulting mixture was sealed in an autoclave and placed under an inert nitrogen atmosphere. The solvent extraction process was carried out in an autoclave under autogenous pressure at 230°C for Examples 2, 3, and 6, and at 280°C for Examples 4, 5, and the Comparative Example. The solvent / isotropic pitch mixture was stirred for 1 hour for Examples 2, 3, 4, and 6, 85 minutes for Example 5, and 3 hours for the Comparative Example, and then cooled to room temperature in each case. During the extraction, pressures of 160 psig (1,100 kPa-g) and 350 psig (2,410 kPa-g) were generated for the experiments carried out at 230°C and 280°C, respectively. The insoluble phase fraction (if any) was collected after decanting the solvent phase fraction and subsequently dried for 30 minutes to remove residual solvent and produce a recovered solid product. As shown in Figures 1 and 2, little or no mesophase pitch was observed in the isotropic pitch, demonstrating the formation of mesophase pitch during the solvent extraction process. Figures 4 and 5 show optical microscope photographs of the solid products recovered from Examples 2 and 3, respectively. The results of the solid products recovered for each of Examples 2-6 and the Comparative Example are summarized in Table 5 below.

[0047] [Table 5]

[0048] As can be seen from Table 5, solid products were recovered in each of Examples 2-6, but not in the Comparative Example. These results were expected given the higher ERT x Bromine values ​​for each of Pitches A-E compared to Pitch F.

[0049] Example 7: Solvent extraction of isotropic pitch with 10SU deasphalting solvent In Example 7, an isotropic pitch was prepared by heat treating a heavy fluid tar feedstock having the following properties: an MCR of 24.2%, a hydrogen content of 6.9 wt%, and a bromine number of about 40. The heat treatment was conducted under the following conditions: a temperature of 460° C., a pressure of 1,000 psig (6,900 kPa-g), a residence time of 35 minutes, and an ERT of 1,387 seconds. The resulting isotropic pitch exhibited the following properties: an MCR of 35.1%, a hydrogen content of 5.32 wt%, a softening point of <30° C., and a mesophase pitch content of 0 vol%. The resulting isotropic pitch was introduced into a 500 ML Hastelloy C276 autoclave and then mixed with a 90 vol%:10 vol% n-heptane:toluene mixture, i.e., 10 SU of S BN A deasphalting solvent having the formula: was introduced at a ratio of 8 ml of solvent per gram of isotropic pitch. The resulting mixture was sealed in an autoclave and placed under an inert nitrogen atmosphere.

[0050] The solvent extraction process was carried out in an autoclave at 280°C under autogenous pressure. The solvent / isotropic pitch mixture was stirred for 1 hour and then cooled to room temperature. During the extraction, a pressure of 350 psig (2,410 kPa-g) was generated. The insoluble phase fraction was collected after decanting the solvent phase fraction and subsequently dried for 30 minutes to remove residual solvent and yield a recovered solid product. The resulting solid product recovered exhibited the following properties: 21 wt% yield; 90 area% optically active fraction; and a softening point of >400° C. These results demonstrate the effectiveness of the 10 SU S in producing a solid product containing mesophase pitch. BN This demonstrates that a deasphalting solvent having

[0051] All documents described herein, including any priority documents and / or testing procedures, are incorporated herein by reference to the extent that they do not contradict this text. As is apparent from the general description and specific embodiments above, the form of the disclosure has been illustrated and described, but various modifications can be made without departing from the spirit and scope of the disclosure. Accordingly, it is not intended that the disclosure be limited thereby. Similarly, the term "comprising" is considered synonymous with the term "including" for purposes of U.S. law. Similarly, whenever a composition, element, or group of elements is preceded by the transition phrase "comprising," there is a common understanding that the same composition or group of elements is also contemplated with the transition phrase "consisting essentially of," "consisting of," "selected from the group consisting of," or "is," preceding the description of the composition, element, or group of elements, and vice versa. Yet another aspect of the present invention may be as follows. [1] A process for producing mesophase pitch, comprising: providing a feedstock having a T5≧400° F. (204° C.) and a T95≦1,400° F. (760° C.); heating the feedstock at a temperature in the range of about 420° C. to about 520° C. to produce a heat-treated product comprising isotropic pitch, the heating being conducted under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time (ERT) of the heating and Y is the bromine number of the feedstock as measured in accordance with ASTM D1159; The isotropic pitch has a solubility blending number (S BN under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising mesophase pitch; recovering the mesophase pitch; The process comprising: [2] The process of [1] above, wherein the feedstock has a bromine number of 10 or more, and the heating is carried out at an ERT of at least about 2,000 seconds. [3] The process of [1], wherein the feedstock has a bromine number of less than 10 and the heating is carried out at an ERT of at least about 4,000 seconds. [4] The process according to any one of [1] to [3] above, wherein the heating is carried out at a temperature in the range of about 420°C to about 510°C. [5] The process according to any one of [1] to [4], wherein the feedstock contains a fraction having a boiling point of 1,050°F (566°C) or higher in the range of about 1 wt% to about 40 wt% based on the mass of the feedstock. [6] The process according to any one of [1] to [5], wherein the feedstock comprises at least one member selected from the group consisting of main column bottoms (MCB), hydroprocessed MCB, steam cracker tar, hydrotreated steam cracker tar, vacuum resid, deasphalted residue or rock, and mixtures or combinations thereof. [7] The isotropic pitch has the following characteristics: (a) microcarbon residue (MCR), as measured in accordance with ASTM D4530-15, ranging from about 30% to about 90%; (b) a softening point, as measured in accordance with ASTM D3104-14, in the range of about 80°C to about 250°C; (c) a mesophase pitch content, as measured in accordance with ASTM D4616-95(2018), greater than about 0.5 vol.%; and (d) greater than about 1 wt. % quinoline insolubles as determined in accordance with ASTM D2318-15 The process according to any one of [1] to [6] above, comprising at least one of the following: [8] The process according to [7], wherein the isotropic pitch has a microcarbon residue (MCR) of at least about 60% as measured in accordance with ASTM D4530-15. [9] The process according to any one of [1] to [8], further comprising a step of separating the heat-treated product to produce a heavy fraction containing the isotropic pitch and a light fraction.

[10] The process according to any one of [1] to [9], wherein the insoluble fraction contains a residual amount of the solvent, and the step of recovering the mesophase pitch comprises removing at least a portion of the residual solvent to form a recovered solid product.

[11] The process described in

[10] , wherein the yield of the recovered solid product is at least about 10 wt %, and the recovered solid product contains at least about 30 vol % of an optically active fraction.

[12] The process according to any one of [1] to

[11] above, wherein the ratio of the isotropic pitch to the solvent during the contact is in the range of about 10:1 to about 1:1 by volume.

[13] The solvent has an S in the range of about 10 SU to about 130 SU. BN The process according to any one of [1] to

[12] above, comprising:

[14] The solvent has an S in the range of about 10 SU to about 100 SU. BN The process according to any one of [1] to

[13] above, comprising:

[15] The process according to any one of [1] to

[14] above, wherein the solvent is selected from the group consisting of monocyclic aromatic compounds, bicyclic aromatic compounds, paraffins, mid-cut solvents, and mixtures or combinations thereof.

[16] The process according to

[15] , wherein the solvent comprises about 10 to about 100 vol.% of a monocyclic aromatic compound and about 0 to about 90 vol.% of n-heptane, based on the volume of the solvent.

[17] The process according to any one of [1] to

[16] above, wherein the contacting is carried out at a temperature in the range of about 90°C to about 350°C.

[18] The process according to any one of [1] to

[17] above, wherein the contacting is carried out at a temperature in the range of about 150°C to about 350°C, at a pressure in the range of about 15 psig (about 105 kPa-g) to about 800 psig (about 5,600 kPa-g), and for a residence time of about 5 minutes to about 5 hours.

[19] The process according to any one of [1] to

[18] , further comprising a step of separating the solvent phase to form a recovered solvent stream and a deasphalted oil stream.

[20] The process described in

[19] , further comprising a step of recycling at least a portion of the recovered solvent stream to the solvent extraction.

[21] The process described in

[19] or

[20] above, further comprising a step of recycling at least a portion of the deasphalted oil stream to the heat treatment.

[22] The mesophase pitch produced by the process described in any one of [1] to

[21] above.

[23] Carbon fibers produced from the mesophase pitch described in

[22] .

[24] A process for producing mesophase pitch, comprising: providing a feedstock comprising at least one member selected from the group consisting of main column bottoms (MCB), hydroprocessed MCB, steam cracker tar, hydrotreated steam cracker tar, vacuum resid, deasphalted residue or rock, and mixtures or combinations thereof; heating the feedstock at a temperature in the range of about 420° C. to about 520° C. to produce a heat-treated product comprising isotropic pitch, wherein the heating is conducted under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time of the heating and Y is the bromine number of the feedstock as measured in accordance with ASTM D1159; contacting the isotropic pitch with a solvent selected from the group consisting of single ring aromatics, two ring aromatics, paraffins, mid-cut solvents, and mixtures or combinations thereof under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising a mesophase pitch; recovering the mesophase pitch; The process comprising:

Claims

1. 1. A process for producing mesophase pitch, comprising: providing a feedstock having a T5≧400°F (204°C) and a T95≦1,400°F (760°C), the feedstock including in the range of 1 wt% to 40 wt%, based on the weight of the feedstock, a fraction having a boiling point equal to or greater than 1,050°F (566°C); heating the feedstock at a temperature in the range of 420° C. to 520° C. to produce a heat-treated product comprising isotropic pitch, said heating being conducted under conditions sufficient to satisfy the relationship [X*Y]≧20,000 seconds, where X is the equivalent reaction time (ERT) of said heating and Y is the bromine number of said feedstock as measured in accordance with ASTM D1159; The isotropic pitch is dissolved in water to obtain a solubility blending number (S BN under conditions sufficient to produce a solvent fraction comprising the solvent and an insoluble fraction comprising mesophase pitch; recovering the mesophase pitch; The process comprising:

2. 2. The process of claim 1, wherein the feedstock has a bromine number of 10 or greater and the heating is at an ERT of at least 2,000 seconds.

3. 3. The process of any one of claims 1 to 2, wherein the feedstock comprises at least one member selected from the group consisting of main column bottoms (MCB), hydroprocessed MCB, steam cracker tar, hydrotreated steam cracker tar, vacuum resid, deasphalted residue or rock, and mixtures or combinations thereof.

4. The isotropic pitch has the following characteristics: (a) Microcarbon Residue (MCR), measured in accordance with ASTM D4530-15, in the range of 30% to 90%; (b) a softening point, measured in accordance with ASTM D3104-14, in the range of 80°C to 250°C; (c) a mesophase pitch content, as determined in accordance with ASTM D4616-95(2018), greater than 0.5 vol.%; and (d) greater than 1 wt. % quinoline insolubles as determined in accordance with ASTM D2318-15 The process according to any one of claims 1 to 3, comprising at least one of:

5. 5. The process of claim 1, further comprising separating the heat treated product to produce a heavy fraction comprising the isotropic pitch and a light fraction comprising the isotropic pitch, the insoluble fraction comprises a residual amount of the solvent, and recovering the mesophase pitch comprises removing at least a portion of the residual solvent to form a recovered solids product; The process, wherein the yield of the recovered solid product is at least 10 wt. % and the recovered solid product comprises at least 30 vol. % of an optically active fraction.

6. the ratio of said isotropic pitch to said solvent during said contacting is in the range of 10:1 to 1:1 by volume; The solvent has an S in the range of 10SU to 130SU. BN The process according to any one of claims 1 to 5, comprising:

7. the solvent is selected from the group consisting of single ring aromatics, two ring aromatics, paraffins, mid-cut solvents, and mixtures or combinations thereof; 7. The process of any one of claims 1 to 6, wherein the solvent comprises 10 to 100 vol.% single ring aromatic compound and 0 to 90 vol.% n-heptane, based on the volume of the solvent.

8. 8. The process of any one of claims 1 to 7, wherein the contacting is conducted at a temperature ranging from 150°C to 350°C, a pressure ranging from 15 psig (105 kPa-g) to 800 psig (5,600 kPa-g), and a residence time of from 5 minutes to 5 hours.

9. 9. The process of any one of claims 1 to 8, further comprising separating a solvent phase to form a recovered solvent stream and a deasphalted oil stream, recycling at least a portion of the recovered solvent stream to the solvent extraction, and recycling at least a portion of the deasphalted oil stream to the heat treatment.

Citation Information

Patent Citations

  • Preparation of highhpurity petroleum pitch or coke

    JP1980157679A

  • Production of carbon fiber using high pressure treatment of precursor substance

    JP1982191327A

  • Preparation of pitch for carbon material

    JP1986026692A

  • Improved method for producing solvated mesophase pitch

    JP1997048978A

  • Method for isolating mesophase pitch

    JP1998508635A