Production of carbon fiber mesophase pitch using supercritical carbon dioxide
Through supercritical carbon dioxide and toluene extraction and quinoline washing, the problem of improving the relative quantity and quality of mesophase bitumen is solved, the production efficiency and quality of carbon fibers are improved, and the production of high-quality fibers is achieved.
Patent Information
- Application Number
- CN202411051804.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-05
- Filing Date
- 2020-03-17
- Publication Date
- 2024-11-12
AI Technical Summary
When the prior art uses supercritical carbon dioxide to produce intermediate phase asphalt of carbon fiber, it is difficult to effectively improve the relative amount and quality of intermediate phase asphalt, affecting the production efficiency and quality of carbon fiber.
Supercritical carbon dioxide and toluene are used to extract coal tar, separate toluene insoluble fractions, and the mesophase asphalt is separated and processed through steps such as extrusion and quinoline washing to form high-quality fibers.
The relative amount and quality of mesophase asphalt is significantly improved, the production efficiency and quality of carbon fibers are improved, the presence of low molecular weight compounds is reduced, and the overall performance of carbon fibers is improved.
Smart Images

Figure CN118931574A_ABST
Abstract
Description
[0001] This application is a divisional application of an application with an application date of March 17, 2020, application number 202080019786.5, and invention name “Mesophase Pitch for Producing Carbon Fibers Using Supercritical Carbon Dioxide”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application was filed as a PCT international patent application on March 17, 2020, and claims the benefit of U.S. Provisional Patent Application No. 62 / 820,162 filed on March 18, 2019; and also claims priority to U.S. Patent Application No. 16 / 532,334 filed on August 5, 2019; the disclosure of which is hereby incorporated by reference in its entirety.
[0004] introduction
[0005] Pyrolysis refers to the thermochemical decomposition of organic materials at high temperatures in the absence of oxygen. Depending on how the pyrolysis system is configured and operated, different pyrolysis products can be obtained. There are systems and methods for producing coal tar via the pyrolysis of coal using supercritical carbon dioxide. In some of those systems and methods, the resulting coal tar product includes at least some mesophase material that can be used to produce mesophase pitch. Mesophase pitch refers to an anisotropic liquid crystal phase of pitch, characterized by pre-graphitic order, high density and high softening temperature. Mesophase pitch can be used to prepare high-performance carbon fibers.
[0006] Using supercritical carbon dioxide to improve mesophase pitch for carbon fiber production
[0007] Embodiments of methods for improving mesophase pitch for carbon fiber production using supercritical carbon dioxide are described. The methods improve the relative amount and quality of mesophase pitch in a feedstock, such as coal tar, that already has at least some mesophase pitch. A particular method includes subjecting the coal tar to sCO2 / toluene extraction to obtain a toluene insoluble fraction of the coal tar; mixing the toluene insoluble fraction with sCO2 to obtain a sCO2 / toluene insoluble fraction mixture; and extruding the sCO2 / toluene insoluble fraction mixture to separate the sCO2 from the toluene insoluble fraction to obtain fibers of the mesophase pitch. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The following drawings, which constitute a part of this application, illustrate the described technology and are not meant to limit in any way the scope of the invention as claimed, which should be based on the appended claims.
[0010] Figure 1A simplified embodiment of a pyrolysis process that increases the relative amount of bitumen produced from a given feedstock is illustrated at a high level.
[0011] Figure 2 The figure shows Figure 1 A more detailed embodiment of the pyrolysis method.
[0012] Figure 3 is an example of a system suitable for the asphalt production method described above.
[0013] Figure 4 The figure shows a process flow diagram of a batch embodiment of a flexible pyrolysis system that can be adjusted to change the pyrolysis products obtained from a given feedstock.
[0014] Figure 5A-5C The figure shows Figure 4 Experimental performance of an embodiment of the system shown in .
[0015] Figure 6 The diagram illustrates an embodiment of a broad process for pyrolyzing a carbonaceous feedstock using CO2 to obtain reaction products.
[0016] Figure 7 is a more detailed embodiment of a method for pyrolyzing coal using supercritical CO2.
[0017] Figure 8 An embodiment of a method for using supercritical carbon dioxide to improve mesophase pitch for carbon fiber production is shown. Detailed Description
[0019] Before disclosing and describing systems and methods for preparing improved mesophase pitch for carbon fiber production using supercritical carbon dioxide, it should be understood that the present disclosure is not limited to the specific structures, process steps or materials disclosed herein, but extends to their equivalents, as will be recognized by a person of ordinary skill in the relevant art. It should also be understood that the terms employed herein are used only for the purpose of describing specific embodiments and are not intended to be limiting. It must be noted that, as used in this specification, the singular forms "a", "an" and "the" include plural indicators unless the context clearly indicates otherwise. Thus, for example, a reference to "lithium hydroxide" should not be considered as a quantitative or source limitation, a reference to a "step" may include multiple steps, a reference to the "production" or "product" of a reaction should not be considered as all products of the reaction, and a reference to a "reaction" may include a reference to one or more of such reaction steps. Thus, a step of a reaction may include multiple reactions or repeated reactions of similar materials to produce a determined reaction product.
[0020] Bitumen refers to a collection of hydrocarbons, including polyaromatic hydrocarbons, that can be made from coal, wood, and other organic materials. Bitumen is characterized by having a high (>80% by weight) elemental carbon composition, a high concentration of polycyclic aromatic hydrocarbons (PAH), and a softening temperature, wherein the softening temperature can range from 100°C to greater than 250°C (measured using Vicat method ASTM-D 1525). Typically, a pitch suitable for carbon fiber will be able to form a high concentration of anisotropic mesophase pitch. It can be used as a base for coatings and paints, for roofing and paving, and as a binder for asphalt products. Bitumen can also be used to make carbon fibers, as discussed in more detail below.
[0021] Although the following systems and methods will be presented in terms of a supercritical carbon dioxide embodiment, any supercritical fluid may be used, such as carbon dioxide, water, methane, nitrous oxide, ethane, propane, ethylene, propylene, methanol, ethanol, acetone, etc., or mixtures of supercritical fluids.
[0022] Figure 1 A simplified embodiment of a pyrolysis process is illustrated at a high level that increases the relative amount of pitch produced from a given feedstock. In the illustrated method 100, a carbonaceous feedstock material and water undergo a two-stage pyrolysis. Water can exist as moisture content in the feedstock. Alternatively, additional water can be added to the feedstock prior to pyrolysis or at some point during pyrolysis.
[0023] The first stage is a low temperature pyrolysis operation 102 to remove C1-C4 gases from the feedstock. In this stage 102, pyrolysis is performed at a relatively low temperature (e.g., 150°C-350°C, from 7MPa-30MPa). The feedstock is heated to the first stage temperature and maintained at that temperature to generate and remove C1-C4 gases from the feedstock. In an embodiment, the gases in the pyrolysis reaction chamber are monitored, and when it is determined based on operator criteria that the C1-C4 gas concentration has begun to level off, a higher temperature pyrolysis operation 104 is performed.
[0024] The first stage temperature may be selected based on a priori knowledge of the properties of the feedstock, or may be automatically determined based on real-time analysis of the pyrolysis reaction and the products being produced. Depending on the embodiment, the first stage temperature may have a lower range selected from 150°C, 175°C, 200°C, 225°C, 250°C, 275°C, 300°C, and 325°C, and may have a higher range selected from 175°C, 200°C, 225°C, 250°C, 275°C, 300°C, 325°C, and 350°C, such that any combination of the lower and higher ranges may be used.
[0025] In the second stage pyrolysis operation 104, the temperature is raised to from 350°C to 550°C at from 7MPa to 30MPa, for example from 7MPa to 12MPa, and maintained at the temperature for a period of time sufficient to produce asphalt. As in the first stage, the amount of pyrolysis reaction products produced will level off over time as the system reaches equilibrium, and the length of the second pyrolysis operation 104 is determined by the operator.
[0026] The second stage temperature may be selected based on a priori knowledge of the properties of the feedstock, or may be automatically determined based on real-time analysis of the pyrolysis reaction and the products being produced. Depending on the embodiment, the second stage temperature may have a lower range selected from 350°C, 375°C, 400°C, 425°C, 450°C, and 480°C, and may have a higher range selected from 375°C, 400°C, 425°C, 450°C, 450°C, 480°C, 500°C, 525°C, and 550°C, such that any combination of the lower and higher ranges may be used.
[0027] The bitumen is then obtained in extraction and separation operation 106. In extraction and separation operation 106, the bitumen is extracted using a solvent such as supercritical carbon dioxide (sCO2), the solvent and dissolved bitumen are removed from the reaction chamber, and then separated to produce a bitumen product.
[0028] To obtain carbon fibers from the pitch, an optional extrusion operation 108 (illustrated by dashed lines in the drawing) may be performed, wherein the pitch is extruded into fibers having a desired cross-sectional profile and allowed to cool. The pitch may or may not be washed first, such as by washing with toluene or other solvents, to remove unwanted products and further refine the pitch.
[0029] Figure 1 Experimental data from the two-stage process indicate that the amount of bitumen produced from a given feedstock is greater than the amount of bitumen that would otherwise be obtained from the same feedstock using a single-stage pyrolysis at a higher temperature. Without being bound by any particular theory, the two-stage process above appears to remove lighter hydrocarbons from the feedstock in the first stage, which renders them unavailable for reaction with larger hydrocarbon chains and aromatics during the second stage, and this increases the relative amount of bitumen produced.
[0030] The raw material can include any carbonaceous material known in the art. For example, the raw material can include, but is not limited to, coal, biomass, biomaterials of mixed origin, peat, tar, plastics, garbage and landfill waste. For example, in the case of coal, the raw material can include, but is not limited to, bituminous coal, sub-bituminous coal, lignite, anthracite and the like. By another example, in the case of biomass, the raw material can include wood materials, such as, but not limited to, softwood or hardwood. In the detailed embodiment experiments discussed herein, the raw material is presented as coal. However, it will be understood that pitch can be similarly produced by any other type of raw material, and is subsequently used to produce carbon fiber in the same manner as described with respect to coal.
[0031] It should be noted that any carbonaceous feedstock, such as coal, may include a certain amount of water. In addition, water may be added to the feedstock prior to pyrolysis or during pyrolysis in any of the methods and systems discussed herein to alter the products produced by the reaction. Likewise, the feedstock may be dried prior to pyrolysis to reduce the amount of water available during the pyrolysis operation, and such drying operations may be part of any of the methods and systems discussed herein.
[0032] Figure 2 The figure shows Figure 1 A more detailed embodiment of the pyrolysis method.
[0033] Method 200 begins with placing feedstock material and water in a pyrolysis reaction chamber in a loading operation 202. In an embodiment, the feedstock material and / or water may be preheated before being placed in the pyrolysis reaction chamber. The amount of water used may be from 1%-1000% of the weight of the dry feedstock material. In an embodiment, the amount of water may be from 10%, 20%, 30%, 40% or 50% of the weight of the dry feedstock material at the low end, and up to 100%, 200% or 500% at the high end. Water may be added separately or may already be in the feedstock material. For example, in an embodiment, the feedstock material used is coal half-saturated with water, so that more than 10% of the weight of the feedstock material is water, and the water in the coal is used as water for loading operation 202.
[0034] The loading operation may also include pressurizing the pyrolysis reaction chamber to an operating pressure (e.g., 7 MPa-12 MPa). In an embodiment, this may include removing oxygen and adding pressurized CO2 to the reaction chamber. In this embodiment, the pressurized CO2 may then be used as a solvent for extracting and removing asphalt and other soluble reaction products from the chamber.
[0035] The method 200 also includes heating the pyrolysis reaction chamber to an intermediate temperature of from 150° C. to 350° C. at from 7 MPa to 12 MPa in an initial heating operation 204. A narrower temperature range may be used, such as from 160, 170, 180, 190, 200, 210, 220, 230, or 240 at the lower end of the range to 250, 260, 270, 280, 290, 300, 310, 320, 330, or 340 at the upper end of the range. The initial heating operation 204 may be performed before the loading operation 202 or after the loading operation 202. In an embodiment, the operation 204 may be performed to increase the temperature as quickly as possible with a given device so that reactions at temperatures below the intermediate temperature are reduced.
[0036] Then, in the first temperature holding operation 206, the intermediate temperature is maintained for a period of time. The holding time can be pre-selected to be, for example, 10 minutes, 15 minutes, 30 minutes, 60 minutes, 120 minutes or even 240 minutes. For example, the pre-selected holding time can be based on previous experiments. Alternatively, the holding time can be determined by monitoring the gas in the pyrolysis reaction chamber. For example, in an embodiment, the concentration of one or more pyrolysis reaction product gases such as methane, ethane, butane, propane or any other light gas reaction product (light gas reaction product) is monitored. The concentration of the monitored one or more gases will initially rise, and eventually begin to stabilize roughly according to an exponential curve. The holding time can be based on the change of the monitored one or more gas concentrations over time. For example, in an embodiment, when it is observed that the concentration of the monitored one or more gases has increased by less than a certain threshold amount (for example, 2% or 100ppm) in a predetermined time period (for example, 10 seconds, 1 minute, 5 minutes, etc.), the first temperature holding operation 206 can terminate. In yet another embodiment, the amount of energy input into the chamber to maintain the pyrolysis temperature or any other parameter, such as the visual or physical condition of the feedstock material, may also be monitored to determine that the reaction has proceeded to the operator's satisfaction.
[0037] Then, a second heating operation 208 is performed. In the second heating operation 208, the temperature of the pyrolysis chamber and the feedstock material is increased to a pyrolysis temperature of from 300° C. to 550° C. For example, the second heating operation 208 may include heating the reaction chamber to from 325° C., 350° C., 375° C., or 400° C. at the low end of the range to from 425° C., 450° C., 475° C., 500° C., 525° C., or 550° C. at the high end.
[0038] Then in the second temperature holding operation 210, the pyrolysis temperature (which may also be referred to as the asphalt production temperature) is maintained for a second time period of from 1 minute to 24 hours. Again, the second holding time can be preselected, for example based on previous experiments. Alternatively, the holding time can be determined by monitoring one or more gases in the pyrolysis reaction chamber, which may or may not be the same one or more gases monitored during the first temperature holding operation 206. In yet another embodiment, the amount of energy input into the chamber to maintain the pyrolysis temperature or any other parameter, such as the visual or physical condition of the feedstock material, can also be monitored to determine that the reaction has proceeded to the extent that the operator is satisfied.
[0039] At the end of the second holding time, the bitumen may be extracted in an extraction operation 212 and removed from the pyrolysis chamber.
[0040] A separation operation 214 may then be performed to separate the extracted asphalt from the solvent. In an embodiment, if the solvent is sCO2, the separation operation 214 may include removing the sCO2 and dissolved pyrolysis reaction products from the chamber, and reducing the temperature and pressure of the solvent until the asphalt is obtained. For example, the sCO2 may pass through a series of collection chambers, each with a different pressure-temperature combination, so as to fractionally remove components in the reaction products that have different solubility in carbon dioxide, including asphalt. One of the separation chambers may be maintained at a temperature and pressure specific to the condensation of asphalt from the solvent. For example, in an embodiment, asphalt is obtained from a CO2 solvent in a chamber maintained at a temperature of 350°C or higher and a pressure of 7.39MPa or higher.
[0041] To obtain carbon fibers from the pitch, an optional extrusion operation 216 (illustrated by dashed lines in the accompanying drawings) may be performed, in which the pitch is extruded into fibers having a desired cross-sectional profile and allowed to cool. The pitch may or may not be washed first to remove unwanted products, and the pitch may be further refined before or after extrusion. In addition, the extruded pitch may be stretched, dried, cooled, baked, heat treated (in an oxidizing environment or an inert environment), or otherwise post-treated to improve the properties of the fiber bundle.
[0042] The method 200 described above is described according to a batch process in a single pyrolysis reaction chamber. In an alternative embodiment, the method can be performed as a continuous process or a semi-continuous process using one or more pyrolysis reaction chambers. For example, in an embodiment, the initial heating operation 204 and the first temperature holding operation 206 can be performed in the first reaction chamber, and then the contents can be transferred to the second chamber for the second heating operation 208 and the second temperature holding operation 210.
[0043] Figure 3 is an example of a system 300 suitable for the asphalt production method described above. Figure 3 The figure shows a block diagram view of a system 300 for converting a carbonaceous material into one or more reaction products. In one embodiment, the system 300 includes a thermochemical conversion system 302. In one embodiment, the thermochemical conversion system 302 includes a thermochemical reaction chamber 304, such as a pyrolysis reaction chamber, which is suitable for accommodating a volume of feedstock material and water 305 (e.g., carbonaceous material) and converting the feedstock material into one or more reaction products including pitch.
[0044] In the illustrated embodiment, the system 300 includes one or more heat sources 308 and a thermal energy transfer system 306 for transferring thermal energy from one or more heat sources 308 to a volume of feedstock 305 contained within the thermochemical reaction chamber 304. The thermal energy transfer system 306 includes a heat transfer element 307. For example, the heat transfer element 307 may include, but is not limited to, a heat transfer loop, a heat transfer line, and the like. For example, the heat transfer element 307 may include, but is not limited to, a heat transfer loop filled with a supercritical fluid (e.g., sCO2), the supercritical fluid being placed in thermal communication (e.g., directly or indirectly) with one or more portions of the one or more heat sources 308.
[0045] In one embodiment, the thermal energy transfer system is arranged to selectively place a volume of supercritical fluid in thermal communication with a volume of feedstock contained within the thermochemical reaction chamber. In this regard, the thermal energy transfer system 306 can selectively transfer thermal energy from one or more heat sources 308 to a volume of feedstock 305 contained within at least one thermochemical reaction chamber 304. In another embodiment, the thermochemical reaction chamber 304 can pyrolyze at least a portion of the feedstock 305 using the thermal energy carried to the feedstock via the supercritical fluid to obtain one or more reaction products.
[0046] The supercritical fluid of system 300 may include any supercritical fluid known in the art suitable for transferring energy from one or more heat sources 308 to feedstock 305 contained in thermochemical reaction chamber 304. In one embodiment, supercritical fluids include, but are not limited to, sCO2. In another embodiment, supercritical fluids include, but are not limited to, water, methanol, ethanol, propanol, acetone. In another embodiment, the supercritical fluid is pressurized to a high pressure in at least one of heat transfer element 307 and thermochemical reaction chamber 304.
[0047] It is noted herein that the supercritical fluid of system 300, such as but not limited to CO2, can have low viscosity and surface tension, allowing such supercritical fluid to easily penetrate organic materials (e.g., coal). The penetration of supercritical fluid into raw material 305 reduces the demand for converting raw material 305 into fine particles before thermochemical reaction, thereby saving energy in the preparation of raw material materials. In one embodiment, in which the supercritical fluid is supercritical CO2, the supercritical fluid can be pressurized to be higher than its critical pressure (7.39MPa) and critical temperature (31°C). It is noted herein that, beyond these conditions, CO2 will show a unique solvency property similar to organic solvents such as hexane, heptane, benzene and toluene. The non-polar nature of supercritical CO2 can be beneficial to control the undesirable ion side reactions that usually occur in aqueous environments. In addition, when the system is decompressed below the critical condition, CO2 will volatilize, which is beneficial to the recovery of oil with low content of water. Again, this can significantly reduce the energy consumption during the reaction product-supercritical fluid separation described in addition herein after pyrolysis. It is also noted herein that the supercritical fluid of system 300 applies heated and pressurized CO2 to feedstock material 305, which provides better control over reaction conditions (e.g., time, pressure, and temperature), thereby allowing better selectivity for high-value target compounds or fuel intermediates.
[0048] In another embodiment, supercritical fluids such as supercritical CO2 can provide strong temperature and reaction time control via injecting a cooler supercritical fluid into the thermochemical reaction chamber 304 to quench the reaction or injecting a hotter supercritical fluid to accelerate the reaction. It is also recognized that since many supercritical fluids such as supercritical CO2 can be effectively compressed, the pressure conditions within the thermochemical reaction chamber 304 can also be used to control the thermochemical reaction within the thermochemical reaction chamber 304.
[0049] In another embodiment, the solubility of one or more reaction products such as asphalt in a supercritical fluid can be controlled by adding a polar material to the supercritical fluid or removing the polar material in the supercritical fluid. For example, the solubility of one or more oils in supercritical carbon dioxide can be controlled by adding / removing one or more materials containing polar molecules, such as but not limited to H2O, ethanol, methanol, higher alcohols and the like. By way of another example, in the case where the feedstock material includes coal, the solubility of one or more oils in sCO2 can be controlled by adding / removing one or more materials containing hydrogen donor molecules, such as but not limited to H2, H2O, formic acid, tetralin and any other hydrogen donor solvents known in the art.
[0050] It should be recognized herein that the feedstock 305 contained within the thermochemical reaction chamber 304 may include sufficient moisture and polar properties to adequately dissolve one or more reaction products (e.g., bio-oil) in the supercritical fluid. As further discussed herein, the "dryness" of the feedstock may be controlled by the thermochemical conversion system 302 (e.g., via the dryer 134), allowing the thermochemical conversion system 302 to maintain a moisture content level within the feedstock 305 sufficient to adequately dissolve one or more reaction products in the supercritical fluid.
[0051] In another embodiment, the supercritical fluid can include one or more materials for enhancing one or more physical reactions or thermochemical reactions in the system 300. For example, the supercritical fluid can include one or more catalysts, such as, but not limited to, metals, metal salts, and organics. By way of another example, the supercritical fluid can include one or more solutes, such as, but not limited to, alcohols, oils, hydrogen, and hydrocarbons.
[0052] The one or more heat sources 308 may include any heat source known in the art suitable for providing thermal energy sufficient to heat the feedstock 305 to the selected temperatures used in the two pyrolysis stages.
[0053] In one embodiment, one or more heat sources 308 include non-CO2 emitting heat sources. In one embodiment, one or more heat sources 308 include one or more nuclear reactors. One or more heat sources 308 may include any nuclear reactor known in the art. For example, one or more heat sources 308 may include liquid metal cooled nuclear reactors, molten salt cooled nuclear reactors, high temperature water cooled nuclear reactors, gas cooled nuclear reactors and the like. By another example, one or more heat sources 308 may include pool reactors. By another example, one or more heat sources 308 may include modular reactors.
[0054] It should be recognized herein that a nuclear reactor can generate temperatures sufficient to implement pyrolysis (e.g., fast pyrolysis) of feedstock 305. For example, a nuclear reactor heat source can generate temperatures in excess of 350° C.-600° C. In this regard, a nuclear reactor can be used to transfer thermal energy (e.g., at temperatures in excess of 350° C.-600° C.) to a supercritical fluid. In turn, the supercritical fluid can transfer the thermal energy generated by the nuclear reactor to feedstock 305 contained within thermochemical reaction chamber 304.
[0055] It is also noted herein that a nuclear reactor heat source can be particularly advantageous as a heat source in the context of system 300 because the thermochemical reaction temperatures of system 300 are within the range of operating temperatures for many nuclear reactors. Nuclear reactor heat can be used to produce reaction products (e.g., asphalt) at high efficiency in thermochemical reaction chamber 304 because the nuclear reactor operates at reaction temperatures for thermochemical conversion (i.e., heat added at the thermochemical reaction temperature supplies the required reaction enthalpy).
[0056] In one embodiment, Figure 3 , the thermal energy transfer system 306 includes a direct heat exchange system configured to transfer thermal energy directly from one or more heat sources 308 to a volume of a supercritical fluid of a heat transfer element 307. For example, the heat transfer element 307 can be placed in direct thermal communication with a portion of the one or more heat sources 308. For example, in the case where one or more heat sources 308 include a nuclear reactor, one or more coolant systems of the nuclear reactor can be integrated with the thermal energy transfer system 306. In this regard, the nuclear reactor can utilize a supercritical fluid in one or more coolant systems, which can then be directly coupled to the thermochemical reaction chamber 304. For example, a primary coolant loop or an intermediate coolant loop of a nuclear reactor can include a coolant fluid composed of a supercritical fluid, such as supercritical CO2. In addition, the coolant loop of the nuclear reactor can be directly coupled to the thermochemical reaction chamber 304 via the thermal energy transfer system 306 so as to mix the supercritical fluid of the coolant loop of the nuclear reactor with the feedstock material 305 contained within the thermochemical reaction chamber 304. In turn, the thermal energy transfer system 306 can circulate the supercritical fluid coolant back to the nuclear reactor via the return path 318 while transferring thermal energy from the nuclear reactor to the feedstock material 305. It is also contemplated herein that the thermal energy transfer system 306 can include any number of filtering elements so as to avoid transfer of feedstock and / or reaction products to the coolant system of the nuclear reactor.
[0057] In another embodiment not shown, the thermal energy transfer system 306 comprises an indirect heat exchange system. In one embodiment, the indirect heat exchange system is configured to indirectly transfer thermal energy from one or more heat sources 308 to a volume of supercritical fluid contained within the heat transfer element 307. In one embodiment, the indirect heat exchange system comprises an intermediate heat transfer element (not shown) configured to transfer thermal energy from one or more heat sources 308 to the intermediate heat transfer element. In turn, the intermediate heat transfer element can transfer thermal energy from the intermediate heat transfer element to a volume of supercritical fluid contained within the heat transfer element 307.
[0058] In an embodiment, the intermediate heat transfer element may include an intermediate heat transfer loop and one or more heat exchangers. The intermediate heat transfer loop may include any working fluid known in the art suitable for transferring thermal energy. For example, the working fluid of the intermediate heat transfer loop may include, but is not limited to, liquid salt, liquid metal, gas, supercritical fluid (e.g., supercritical CO2) or water.
[0059] Furthermore, as previously described herein, the heat transfer element 307 of the heat transfer system 306 can mix the supercritical fluid contained within the heat transfer element 307 with the feedstock material 305 contained within the thermochemical reaction chamber 304. In turn, the thermal energy transfer system 306 can recirculate the supercritical fluid coolant via the return path 318 while transferring thermal energy from the heat source 308 to the feedstock material 305 via the heat transfer element 307.
[0060] It is noted herein that the above description of direct and indirect coupling between one or more heat sources 308 and feedstock 305 is not limiting and is provided for illustrative purposes only. It is recognized herein that, in general, the integration between one or more heat sources (e.g., a nuclear reactor) and the thermochemical reaction chamber 304 can occur by transferring heat from a primary heat transfer system, an intermediate heat transfer system, or a tertiary heat transfer system (e.g., a coolant system) of one or more heat sources 308 to a working fluid, such as supercritical CO2, of the thermochemical conversion system 302. It is also recognized herein that such integration can be implemented using any heat transfer system or device known in the art, such as, but not limited to, one or more heat transfer loops, one or more radiators, one or more heat exchangers, and the like.
[0061] In one embodiment, the thermal energy transfer system 306 includes a flow control system 310. The flow control system 310 can be arranged to selectively place the supercritical fluid in thermal communication with a volume of feedstock contained within the thermochemical reaction chamber 304. In this regard, the flow control system 310 can selectively transfer thermal energy from one or more heat sources 308 to a volume of feedstock contained within the thermochemical reaction chamber 304. For example, the flow control system 310 can be positioned along a heat transfer element 307 (e.g., a heat transfer loop) to control the flow of the supercritical fluid through the heat transfer element 307. In this regard, the flow control system 310 can control the flow of the supercritical fluid to the volume of feedstock 305, thereby controlling the transfer of thermal energy to the feedstock 305.
[0062] The flow control system 310 may include any flow control system known in the art suitable for controlling the flow of a supercritical fluid from a first location to a second location. For example, the flow control system 310 may include, but is not limited to, one or more control valves operably coupled to the heat transfer element 307 and suitable for establishing and stopping flow through the heat transfer element 307. For example, the flow control system 310 may include a manual control valve, a valve / valve actuator, and the like.
[0063] In another embodiment, the flow control system 310 can couple the thermal energy from one or more heat sources 308 to a power generation system (not shown). For example, the flow control system 310 can establish a parallel coupling of the heat generated by the heat source 308 to the turbine power system and the thermochemical conversion system 302. In one embodiment, the thermochemical conversion system 302 can include a plurality of batch reaction systems that can receive heat from one or more heat sources 308 (e.g., nuclear reactors). In this way, multiple batch processes that address the overall heat and feedstock conversion needs can be run simultaneously or sequentially. In another embodiment, heat can be transferred to one or more continuous thermochemical reactors while being coupled in parallel to one or more turbine power systems.
[0064] In one embodiment, system 300 includes a feedstock supply system 312. In one embodiment, feedstock supply system 312 is operably coupled to thermochemical reaction chamber 304 of thermochemical conversion system 302. In another embodiment, feedstock supply system 312 provides a volume of feedstock material and water 305 to the interior of thermochemical reaction chamber 304. Feedstock supply system 312 may include any supply system known in the art suitable for transferring a selected amount of feedstock material (e.g., solid material, particulate material, or liquid material) from one or more feedstock sources to the interior of thermochemical reaction chamber 304. For example, feedstock supply system 312 may include, but is not limited to, a conveyor system, a fluid transfer system, and the like.
[0065] The feedstock supply system 312 may include a separate system for transferring feedstock and additional water in an amount required for the desired reaction. In an alternative embodiment, water may be added to the feedstock prior to transferring the feedstock into the reaction chamber 304. This may be done in the feedstock supply system 312 or prior to being received by the feedstock supply system 312.
[0066] A moisture control system (not shown) may be provided to determine the moisture of the feedstock and add water if necessary. Such a system may include a moisture detector that continuously or periodically determines the moisture of the feedstock, compares the moisture to a target moisture range, and adds water if the moisture is below the target range. A dryer may also be provided for drying the feedstock material 305 in the event that the moisture is above the target range.
[0067] The feedstock material 305 may include any carbonaceous material known in the art. For example, the feedstock material 305 may include, but is not limited to, coal, biomass, biomass of mixed origin, peat, tar, plastic, garbage, and landfill waste. For example, in the case of coal, the feedstock may include, but is not limited to, bituminous coal, sub-bituminous coal, lignite, anthracite, and the like. By way of another example, in the case of biomass, the feedstock may include wood materials, such as, but not limited to, softwood or hardwood.
[0068] It is noted herein that the ability to control temperature, pressure, reaction time, pretreatment options, and post-organic product generation options can allow multiple types of carbonaceous feedstocks to be used within system 300. Additionally, the ability to co-utilize or convert between these types of feedstocks can increase the utilization of available resources and improve the overall economics of asphalt production.
[0069] Reference again Figure 3 , the thermochemical conversion system 302 includes any thermochemical reaction chamber 304 suitable for performing pyrolysis. In one embodiment, the thermochemical reaction chamber 304 is configured to perform a pyrolysis reaction on the feedstock 305. In another embodiment, the thermochemical reaction chamber 304 includes a pyrolysis chamber. In another embodiment, the thermochemical reaction chamber 304 includes a non-combustion pyrolysis chamber or a low-combustion pyrolysis chamber. The pyrolysis chamber of the system 300 can encompass any thermochemical reaction chamber suitable for performing thermochemical decomposition of organic molecules in the absence of oxygen or in a low-oxygen environment.
[0070] In one embodiment, the thermochemical reaction chamber 304 includes a fast pyrolysis reactor suitable for converting raw material 305, such as coal, into a reaction product including asphalt. The fast pyrolysis reactor can include any thermochemical reaction chamber capable of implementing the thermochemical decomposition of organic molecules in about two seconds in the absence of oxygen (or in a reduced oxygen environment). Fast pyrolysis is generally described by Roel JM Westerhof et al. in "Effect of Temperature in Fluidized Bed Fast Pyrolysis of Biomass: Oil Quality Assessment in Test Units," Industrial & Engineering Chemistry Research, Vol. 49, No. 3 (2010), pp. 1160-1168, which is incorporated herein by reference in its entirety. Pyrolysis and fast pyrolysis are also generally described by Ayhan Demirbas et al. in "An Overview of Biomass Pyrolysis" Energy Sources, Vol. 24, No. 3 (2002), pp. 471-482, which is incorporated herein by reference in its entirety.
[0071] In another embodiment, the thermochemical reaction chamber 304 includes a supercritical pyrolysis reactor suitable for converting feedstock 305, such as coal or biomass, into reaction products such as asphalt. For the purposes of this disclosure, 'supercritical pyrolysis reactor' is interpreted to encompass any reactor, reaction vessel, or reaction chamber suitable for carrying out a pyrolysis reaction of a feedstock material using thermal energy supplied by a supercritical fluid. In another embodiment, the thermochemical reaction chamber 304 may include, but is not limited to, a fluidized bed reactor.
[0072] In another embodiment, the thermochemical reaction chamber 304 can implement one or more extraction processes on the feedstock. In another embodiment, an extraction chamber operably coupled to the thermochemical reaction chamber 304 can implement one or more extraction processes on the feedstock after the first or second stage of pyrolysis. In one embodiment, the thermochemical reaction chamber 304 is configured to remove additional compounds from the feedstock material before pyrolysis. For example, the thermochemical reaction chamber 304 can be configured to remove at least one of oil and lipids, sugars or other oxidized compounds. In another embodiment, the extracted compounds can be collected and stored for use in forming additional bio-derived products.
[0073] Removing sugars from the feedstock material 305 can be advantageous. It is recognized herein that sugars caramelize at high temperatures and can serve to block supercritical fluids, such as supercritical CO, from entering the cellulosic structure of the feedstock material 305. Additionally, sugars present in the thermochemical conversion system 302 can also serve to damage downstream catalyst beds, if any. It is noted herein that removal of sugars helps avoid the formation of oxidized compounds such as, but not limited to, furfural, hydroxymethalfurfural, vanillin, and the like.
[0074] In one embodiment, the thermochemical conversion system 302 can extract material from the feedstock 305 at a temperature below 200° C. It is noted herein that extracting sugars at a temperature below 200° C. is beneficial because fructose, sucrose, and maltose each caramelize at temperatures below about 180° C. In this regard, supercritical fluids can be used to extract sugars from the feedstock 305 before the temperature is raised during pyrolysis by deconstructing the cellulosic material and removing the sugars.
[0075] In another embodiment, the thermochemical reaction chamber 304 is configured to preheat the feedstock 305 prior to thermal decomposition. In another embodiment, a preheating chamber operably coupled to the thermochemical reaction chamber 304 is configured to preheat the feedstock 305 prior to thermal decomposition. For example, the thermochemical reaction chamber 304 (or preheating chamber) can preheat the feedstock material to a temperature at or near a temperature required for liquefaction and / or pyrolysis.
[0076] In another embodiment, the thermochemical reaction chamber 304 is configured to pre-treat the feedstock 305 prior to thermal decomposition. For example, the thermochemical reaction chamber 304 can pre-hydrotreat the feedstock material with hydrogen prior to liquefaction and / or pyrolysis. For example, pre-treating the feedstock material with hydrogen can help remove materials such as, but not limited to, sulfur, as well as for supplying hydrogen to the reactive species (i.e., stabilizing free radicals).
[0077] In an alternative embodiment not shown, the thermochemical conversion system 302 is divided into multiple process chambers for implementing various steps of the multi-stage thermochemical process of the system 300. For example, in one embodiment, a first chamber is provided for a first stage of pyrolysis at an intermediate temperature, a second stage is provided for a second stage of pyrolysis at a pyrolysis temperature, and an extraction chamber is provided for solvent contact and extraction of the solvent with the desired bitumen product. The feedstock 305 can be transferred between the chambers continuously or as a batch process.
[0078] Applicants note that, although the above description indicates that, in certain embodiments, the pyrolysis reaction chamber and the extraction chamber can exist as separate chambers, this should not be construed as limiting. Rather, it is contemplated herein that two or more of the thermochemical steps can each be implemented in a single reaction chamber.
[0079] In one embodiment, the thermochemical reaction chamber 304 includes a multi-stage single thermochemical reaction chamber. In one embodiment, the thermochemical conversion system 306 is configured to transfer multiple portions of the supercritical fluid across multiple temperature ranges to a volume of feedstock 305 contained in the multi-stage single thermochemical reaction chamber 304 to perform a set of thermochemical reaction processes on at least a portion of the volume of feedstock.
[0080] In another embodiment, the thermal energy transfer system 306 is configured to transfer a first portion of the supercritical fluid in the second temperature range to a volume of feedstock 305 contained within the single thermochemical reaction chamber 304 to perform a preheating process on at least a portion of the volume of feedstock.
[0081] In another embodiment, the thermal energy transfer system 306 is configured to transfer a second portion of the supercritical fluid within the first temperature range to a volume of feedstock 305 contained within the single thermochemical reaction chamber 304 to perform a first stage pyrolysis on at least a portion of the volume of feedstock.
[0082] In another embodiment, the thermal energy transfer system 306 is configured to transfer a third portion of the supercritical fluid in the second temperature range to a volume of feedstock 305 contained within the single thermochemical reaction chamber 304 to perform a second stage pyrolysis on at least a portion of the volume of feedstock.
[0083] In one embodiment, the flow rate and temperature of the supercritical fluid change spatially across the thermochemical reaction chamber 304. For example, in order to change the flow rate and / or temperature across the reaction chamber 304, a plurality of supercritical fluid streams at different temperatures can be established before entering a single reaction chamber. In this regard, in a vertical reaction chamber, the flow rate and temperature at many spatial locations corresponding to each thermochemical stage can be changed. By another example, the temperature of the supercritical fluid can be changed along the length of the thermochemical reaction chamber 304 by making the supercritical fluid flow along the length of the thermochemical reaction chamber 304. For example, the flow of low-temperature supercritical CO2 can be combined with the flow of CO2 at a higher temperature (for example, between 70°C and 150°C) to dissolve sugar. At another point downstream (for example, 1-3 meters downstream, wherein the average flow rate is 0.25-4m / s), at the pyrolysis temperature or at a supercritical CO2 higher than the pyrolysis temperature is mixed into the chamber. By grading the temperature of each thermochemical reaction step according to the length, the flow rate can be used to control the reaction time.
[0084] It is also contemplated that two or more thermochemical steps, such as pyrolysis, extraction, and separation, are performed in the thermochemical chamber 304 , while additional steps, such as drying and preheating, are performed in dedicated chambers operably coupled to the thermochemical reaction chamber 304 .
[0085] According to one or more embodiments of system 300, the reaction chamber can include one or more outlets 319. Figure 3 In the embodiment shown, the reaction chamber 304 is provided with an outlet for removing the feedstock residue remaining after the second stage of pyrolysis and another outlet for removing the solvent loaded with asphalt and other dissolved pyrolysis products. In one embodiment, the outlet for the feedstock residue remaining after the second stage of pyrolysis is completed is arranged to remove the residue and transfer it to a residue storage system 314. In an embodiment, the residue storage system 314 can be as simple as a drum, rail car, Conex box or other portable container. In an optional embodiment, the residue can be stored in piles for later transportation.
[0086] The solvent outlet 319 transfers the solvent (sCO2 in this embodiment) to the separation system 320. In an embodiment, the outlet includes a valve that controls the flow of gas from the reaction chamber 304 to the separation system 320.
[0087] In an embodiment, separation system 320 reduces temperature and / or pressure in a continuous step to obtain different dissolved components. For example, optionally, a heat rejection heat exchanger can be used before separation system 320 or after separation system 320. In one of these steps, asphalt is condensed and transferred to asphalt extruder 326. Asphalt can be stored in a holding container in the middle. Alternatively, asphalt can be immediately transferred to extruder 326 when condensing out sCO2.
[0088] In embodiments, each step corresponds to a collection chamber maintained at different temperature and pressure conditions, wherein dissolved products are allowed to condense from the solvent. Each chamber then collects those products that condense at the temperature and pressure of that chamber. In embodiments, asphalt is obtained from a chamber maintained at a temperature of 350°C or higher and a pressure of 7.39 MPa or higher.
[0089] As discussed above, a pitch extruder extrude the pitch into fibers which are then allowed to cool for use either directly or indirectly as carbon fibers.
[0090] Other compounds in the solvent stream removed from reaction chamber 304 are collected for further processing or sale in product collection system 322. In one embodiment, a volatile gas separator and storage system can be provided as a part of product collection system 322 or separation system 320. A volatile gas separator can separate one or more volatile gases from the remainder of one or more reaction products. For example, a volatile gas separator can separate volatile gases such as but not limited to CH4, C2H4, C2H6, CO, CO2, H2 and / or H2O from a solid reaction product or a liquid reaction product. It is noted herein that a volatile gas separator can include any volatile gas separation device or process known in the art. It is further recognized that these gases can be cooled, cleaned, collected and stored for future use. Volatile gases can be produced to provide a source of hydrogen.
[0091] In the illustrated embodiment, after removing dissolved products in a closed loop system, CO2 is returned 318 to the heat source 308 for reuse. In an alternative embodiment, CO2 is simply vented.
[0092] In another embodiment not shown, system 300 includes a heat recovery system. In the case of recovery, the system can recover heat from sCO2 via a heat transfer loop before separation system 320 or as a part of separation system 320 (or any other suitable subsystem of system 300), and the heat transfer loop is used to thermally couple sCO2 and a heat recovery system. In one embodiment, the recovered heat can be used as a recuperator or regenerator. In another embodiment, energy can be recovered after the thermochemical process implemented by chamber 304. In another embodiment, the recovered energy can be used to preheat feedstock materials before thermochemical processing. In another embodiment, the recovered energy can be used to generate auxiliary power (e.g., mechanical power or electrical power) for one or more subsystems of system 300.
[0093] Figure 4 The figure shows a process flow diagram for a batch embodiment of a flexible pyrolysis system that can be adjusted to change the pyrolysis products obtained from a given feedstock. In the embodiment shown, the feedstock will be presented as coal. However, the reader will understand that any carbonaceous feedstock, such as biomass, can be used.
[0094] Figure 4 The figure shows a closed loop CO2 pyrolysis system similar in operation to those described above. Figure 4 In the illustrated embodiment, the pyrolysis chamber is a column 402 filled with coal 404. An inlet stream of a supercritical fluid such as sCO2 enters the top of the column and flows through the coal 404. As is known in the art, by controlling the flow rate of sCO2, the residence time or contact time of sCO2 with the coal can be controlled to control the amount of reaction products dissolved in the sCO2 observed in the outlet stream of the chamber. In an embodiment, the sCO2 entering the pyrolysis chamber 402 can be at a temperature range of from 300°C-600°C and a pressure range of from 7.39MPa-12MPa, so that pyrolysis occurs in a CO2 atmosphere in a supercritical state. Higher temperatures and pressures can also be used.
[0095] In a batch system, the pyrolysis chamber may be a simple cylindrical chamber without any internal parts except a screen to hold the coal in place. Multiple chambers may be provided in parallel so that one chamber may be in use while charcoal is removed from other chambers and they are reloaded with new coal. In an alternative embodiment, the chamber may be provided with an agitator or screw for moving the coal during pyrolysis.
[0096] After contacting and pyrolyzing coal 404, sCO2 leaves the bottom of tower 402 together with dissolved pyrolysis products, as described above. Then, the output sCO2 passes through a recuperation and condensation loop, which removes dissolved pyrolysis products and then recuperates CO2 for reuse in pyrolysis chamber 402. The recuperation and condensation loop includes a series of one or more recuperators 406, which simultaneously cool the CO2 stream output by pyrolysis chamber 402, while preheating the inlet stream / return stream of CO2 delivered to chamber 402 (wherein the product has been mostly condensed from the stream). In the illustrated system 400, four recuperators 406 are illustrated, a first-stage recuperator 406a, a second-stage recuperator 406b, a third-stage recuperator 406c, and a fourth-stage recuperator 406d. More or fewer recuperators 406 can be used as needed, as described below.
[0097] The recuperators 406 can be any type of heat exchanger now known or later developed. For example, in an embodiment, the recuperators 406 are each tube-in-tube heat exchangers, where the output CO2 is in the outer tube and the cooler inlet CO2 stream flows through the inner tube. However, any type of heat exchanger can be used in any configuration determined to be beneficial or desired.
[0098] In addition to the recuperator 406, an optional final cooling heat exchanger 408 stage may be provided as part of the recuperation and condensation loop to perform a final reduction in the temperature of the CO2 to the desired low temperature of the loop. This is accomplished using a coolant, such as cooling water from a cooling water system 424 as shown, to perform a final cooling of the output stream. As with the recuperator 406, the final heat exchanger 408, if used, may be any type of heat exchanger.
[0099] As mentioned above, supercritical conditions for CO2 are temperatures above 31.1°C and pressures above 7.39MPa. In describing the system, CO2 will be referred to as supercritical, even though conditions may drop below the critical point of the temperature or pressure at certain points in the system. At these points, it will be understood that CO2 may be in a gaseous state or a liquid state, depending on the temperature and pressure conditions. Such a state may occur, for example, downstream of the pyrolyzer 402, such as in the fourth recuperator 406 or the final heat exchanger 408.
[0100] For example, in an embodiment, the low sCO2 loop temperature can be lower than 50°C, such as room temperature (20°C), and the low pressure can be from 6MPa-8MPa. Lower temperature and pressure can also be used. In this embodiment, CO2 is allowed to enter subcriticality so as to remove as much pyrolysis product as possible. In an optional embodiment, loop temperature and pressure are maintained so that CO2 is maintained in a supercritical state throughout the system 400.
[0101] In the illustrated embodiment, after each heat exchanger in the loop, there is a condensation collection container 410. From left to right, each container is at a subsequently lower temperature. Condensation container 410 can be any type of active condensation device or passive condensation device. For example, in the illustrated embodiment, condensation container 410 is a cold finger condenser, which provides a temperature controlled surface on which CO2 flows. This causes any pyrolysis product that can be condensed at or above the controlled temperature to be collected in condensation container 410. In an optional embodiment, a cyclone separator can be used to replace the finger condenser. Other possible condensation containers include Liebig condenser, Graham condenser, coil condenser and Allin condenser, to name a few.
[0102] Where appropriate, the term "process stream" will be used to refer to the CO2 stream in the CO2 loop portion, where CO2 flows from the pyrolysis chamber 402 through the final condensation collection vessel 410, while "return stream" or "inlet / return stream" will be used to refer to the CO2 stream that flows from the final condensation vessel through the loop, through the pump 420, and ultimately back into the pyrolysis chamber 402. It should be noted that the return stream may not be completely pure CO2, but will likely contain at least trace amounts of reaction products, water, or other compounds that are not completely collected in the condensation vessel. On the other hand, depending on the position in the loop, the process stream will contain at least some and possibly very large amounts of pyrolysis reaction products, which will be removed sequentially through various condensation vessels 410.
[0103] In the illustrated embodiment, different recuperators can operate at different temperatures. For example, in an embodiment, the first recuperator 406a can receive a process stream of CO2 and dissolved reaction products at about 550°C and discharge it at 450°C. The second recuperator 406b can receive a stream at 450°C and discharge it at 300°C. The third recuperator 406c can receive a stream at 300°C and discharge it at 150°C. The fourth recuperator 406d can receive a stream at 150°C and output it at 50°C.
[0104] The return stream of CO2 is partially reconditioned by pump / compressor 420 and heater 422, which brings CO2 back to the operating pressure (e.g., about 10MPa), and heater 422 provides additional heat to CO2 to bring it to the desired pyrolysis temperature. For example, in an embodiment, pump / compressor 420 receives about 10MPa of CO2 and compresses the stream to about 12MPa, which provides enough pressure to maintain the flow through the entire CO2 loop without any additional pump. Depending on the operator's preference, heater 422 can be a single heating unit or multiple units in parallel and / or series. For example, in an embodiment, three separate heaters in series are provided, which receive the CO2 stream of recuperation from the first recuperator 406a, and heat the stream from an inlet temperature of about 450°C to about 550°C. Similarly, as shown, there can be a single pump 420, or multiple pumps distributed throughout the CO2 loop. For example, in embodiments where a portion of the loop is below supercritical conditions, a dedicated heater and / or compressor (not shown) may be provided to purely recondition the CO2 to supercriticality.
[0105] By providing multiple stages of paired heat exchangers 406, 408, followed by a condensation vessel 410, the pyrolysis products can be fractionated and collected by condensation temperature. This allows the desired specific fractions to be easily separated as part of the recuperation process. By providing more or fewer stages, greater or lesser differences in fractions can be achieved, as well as controlling the makeup of each fraction.
[0106] In addition to having multi-stage heat exchangers 406, 408 and subsequent condensation vessels 410, additional flexibility is obtained by using a bypass loop produced by a plurality of bypass valves 412 in the output CO2 portion of the loop and the inlet / return CO2 portion of the loop. In an embodiment, one or more of the heat exchangers are equipped with a bypass capability (bypass capability), which allows the exchanger to be completely or partially bypassed by any one or two of the pyrolysis output stream and the inlet / return stream. In the illustrated embodiment, various bypass valves 412 are provided, which allow the operator to completely or partially bypass each in different stages as required. At any bypass valve 412, the operator can choose how many input streams are directed to any outlet of the valve. This level of flow control provides significant flexibility in the operation of system 400, and allows additional operational control to be performed at the position where the various fractions of pyrolysis products are collected in the system.
[0107] The pyrolysis system 400 can also be provided with an additive injection system for injecting additives into the CO2 inlet / return stream prior to delivery to the pyrolysis chamber 402. In the illustrated embodiment, two additive injection systems are shown, each of which includes an injection pump 414 and an additive supply 416. Examples of additives described in more detail above include H2, H2O, formic acid, and tetralin. In an embodiment, the injection pump 414 is an HPLC injection pump.
[0108] In yet another embodiment (not shown), bypass valve 412 may be provided to allow one or more condensation vessels 410 to be bypassed. This allows the collection of reaction products to be combined into fewer vessels as desired, thereby further increasing the flexibility of system 400.
[0109] The controller 430 Figure 4 4. In an embodiment, the controller 430 is a programmable logic controller configured to monitor and control the pyrolysis system 400 to achieve the desired results. The controller can be implemented in many different ways, from a purpose-built hardware controller to a general-purpose computing device that executes control software. Process controllers are well known in the art, and any suitable controller design or combination of designs now known or later developed can be used.
[0110] Controller 430 controls the distribution of the flow of the process stream and the return stream through each stage of the recuperator. In this way, the inlet temperature and outlet temperature of the stream at each stage can be changed. The heat transfer equations that control the heat exchange between the hot stream and the cold stream in the heat exchanger are well known, and any form of these equations can be used by the controller to determine the distribution of the flow between each stage in order to obtain a specific temperature at a specific location in the CO2 loop. For example, a basic heat exchange equation that can be used is the general counterflow heat exchange equation that describes the transfer of heat through a:
[0111]
[0112] in is the mass flow rate of the process stream, c pa is the specific heat of the process stream, T a1 is the inlet (high) temperature of the process stream entering the recuperator stage, T a2 is the outlet (low) temperature of the process stream, is the mass flow rate of the return flow, c pb is the specific heat of the return flow, T b1is the inlet (low) temperature of the return flow entering the recuperator stage, and T b2 is the outlet (high) temperature of the return flow. As is known in the art, from the above equations, additional equations can be derived that mathematically describe the performance of a recuperator, typically in terms of the overall heat transfer coefficient of the recuperator, based on the size and characteristics of the recuperator. In many cases, performance equations for heat exchangers can be provided by the manufacturer. Such equations are solved by the controller as needed to determine how to distribute the flows through the recuperator stages in order to achieve the goals set by the operator, examples of which are provided below.
[0113] In an embodiment, the controller 430 is connected and capable of controlling the bypass valve 412, the heater 422, the cooling water system 424, the additive pump 414, and other components of the system 400. In addition, the controller 430 may be connected to or otherwise receive information or signals from one or more monitoring devices 426 from which the controller 430 receives data regarding the status of the system 400.
[0114] Figure 4 The figure shows several monitoring devices 426 at different locations throughout the system 400. The monitoring device 426 can be any type of process monitor, analyzer or sensor, such as, for example, a flow sensor, a temperature sensor, a pressure sensor, a balance, a pH sensor, a spectrometer, a photoionization detector, a gas chromatograph, a catalytic sensor, an infrared sensor, and a flame ionization detector, to name a few. The monitoring device 426 can be located at any position in the system 400 as desired. For example, in an embodiment, a gas chromatograph can be used to periodically or continuously monitor and determine different compounds and their relative amounts in the reaction products in the sCO2 leaving the reaction chamber 402. Optionally, a liquid level sensor can be provided on each condensation vessel, and from these data, the relative productivity of the condensate of each recuperator stage can be determined.
[0115] Based on the information received from the monitoring device 426, the controller 430 can change the flow through one or more bypass valves and the temperature of one or more streams to obtain a desired hydrocarbon condensate fraction (i.e., a range of molecular weights) in one or more condensation vessels. For example, in an embodiment, the controller can be directed to separate and recover hydrocarbons having a boiling point from 300°C to 350°C. In this embodiment, the flow through the various bypass valves can be adjusted so that the process stream is discharged from the first recuperator 406a at a temperature of 350°C (as opposed to 450°C as mentioned above) and discharged from the second recuperator 406b at a temperature of 300°C. This can be achieved by bypassing a portion of the return flow around the second recuperator 406b so that a relatively large and cooler return flow is driven through the first recuperator 406a, which increases the relative amount of cooling performed by the first stage. In this way, reaction products having a boiling point higher than 350° C. are collected in the condensation vessel 410 between the first recuperator 406a and the second recuperator 406b, while reaction products having a boiling point from 300° C. to 350° C. are collected in the condensation vessel 410 after the second recuperator 406b.
[0116] As can be seen from the examples above, by using the controller 430 and the flexibility achieved by the design of the system, the operating configuration of the system 400 can be changed in real time to achieve different goals. In addition, by basing the control of the system 400 on real-time knowledge reported by sensors and monitoring devices, the system 400 can be adjusted over time in response to changing conditions (e.g., changing feedstock quality). In this regard, through the controller 430 and multiple stages of recuperators and condensing vessels, the system 400 can be easily configured to separate and collect different fractions of hydrocarbons into different condensing vessels. By providing more stages, even more differences can be provided as needed. Because the controller 430 can easily reconfigure the bypass valve 412, the system 400 is uniquely capable of handling different output requirements or changes in feedstock characteristics.
[0117] In addition, controller 430 can also be used to control and optimize the reaction products obtained from the pyrolysis reaction. For example, in an embodiment, controller 430 can directly or indirectly control the temperature and / or pressure in reaction chamber 402 to change the relative amount of different reaction products. In an embodiment, the change of temperature or pressure in the reaction chamber can be carried out in real time based on the monitoring information received from the sensor and the monitoring device. For example, the type and amount of monitoring data indicating the different reaction products in the sCO2 leaving the reaction chamber 402 can be provided to controller 430. In response to a preset target, such as optimizing a subset of reaction products (for example, maximizing the production of reaction products with a boiling point from 250°C to 350°C), controller 430 can then iteratively change the temperature and / or pressure in the reaction chamber until the optimal distribution of reaction products is obtained based on the current target of system 400.
[0118] Figure 5A-5C The figure shows Figure 4 The experimental performance of an embodiment of the system shown in FIG. In the figure, the system is alternatively referred to as a multi-stage supercritical liquefaction system. In the experiment, Figure 4 The embodiment of the system shown in was created at laboratory scale using four recuperators and a final cooling water heat exchanger, as illustrated. A sample of 1 kg of Power River Basin subbituminous coal was placed in the tower and pyrolyzed using sCO2, as described above. A fine screen was set at the bottom of the tower to prevent solids from leaving the chamber.
[0119] For startup, a bypass loop was used to isolate the pyrolysis chamber until the system reached the desired thermal conditions. After the loop reached the test temperature, the bypass was disabled and the pyrolysis chamber was placed in the loop. The outlet temperature of the sCO2 leaving the pyrolysis chamber was about 490°C, and the inlet temperature of the sCO2 delivered to the pyrolysis chamber was about 500°C. During the experiment, the pressure of the sCO2 in the pyrolysis chamber was about 10 MPa, and the mass flow rate of sCO2 circulating through the loop was between 4.5 kg / min and 10 kg / min. The system was operated without bypassing any of the five heat exchangers so that the entire flow of CO2 passed through each exchanger / condensation vessel stage. The condenser vessels were cold fingers and were designated bottles 1-5, which were maintained at Figure 5A-5C The system is operated for a period of time and then the condensed pyrolysis products from the condensation vessel are analyzed.
[0120] Figure 5A The graph shows representative liquid yields obtained from pyrolyzing a batch of coal through the condenser vessel temperatures. The condenser vessels are finger-shaped condensers and are designated bottles 1-5, which are maintained at Figure 5A The temperatures shown in .
[0121] The condensate fractions obtained from bottles 2 and 5 were subjected to mass spectrometry analysis. Figure 5B The results for bottle 2 are shown, and Figure 5B Results for bottle 5 are shown. As expected, the results show that a significantly higher molecular weight product distribution was condensed in the higher temperature bottle 2 compared to the product distribution obtained in the lower temperature bottle 5. This demonstrates that the multi-stage separation system successfully produces and fractionates different pyrolysis products from the carbonaceous feedstock.
[0122] Figure 6 The figure shows an embodiment of a broad method for pyrolyzing a carbonaceous feedstock using CO2 to obtain a reaction product. The illustrated embodiment is discussed in terms of an ongoing process that reconditions and recycles CO2 for reuse in a closed loop. Figure 6 The process in FIG. 6 is illustrated as starting from a contacting operation 602. In the contacting operation 602, the carbonaceous feedstock is maintained in contact with supercritical carbon dioxide for a certain contact period at a pyrolysis temperature and pressure sufficient to maintain the CO2 in a supercritical state and to cause pyrolysis. The resulting pyrolysis results in conversion of at least some of the feedstock into char and produces a certain amount of pyrolysis reaction products that are dissolved into the CO2.
[0123] The contact period or residence time used can be selected by the operator. The contact can be static, in that CO2 does not flow through the contact chamber during pyrolysis. Instead, the chamber is loaded with CO2 and feedstock and then allowed to react with or without internal stirring or other mixing. In this case, the contact time is the time that the CO2 is supercritical and in contact with the feedstock in the contact chamber. Alternatively, the contact can be dynamic, in that CO2 continuously flows through the chamber containing the feedstock. In dynamic contact, the residence time is calculated by the flow rate of CO2 and the volume of the contact chamber.
[0124] The chemical composition of the pyrolysis reaction product can be changed to a certain extent by changing the pyrolysis conditions. For example, the relatively high temperature and pressure used in contact operation 602 can be conducive to the generation of some reaction products (for example, heavier hydrocarbons, such as oil) relative to other reaction products (for example, medium weight oil or lighter hydrocarbon gas). In addition, additives such as water, formic acid, hydrogen or some other hydrogen donors can be used to increase the availability of hydrogen during pyrolysis, which will also change the chemical composition of the reaction product. Other additives can also be used to affect the pyrolysis reaction and change the chemical composition of the reaction product.
[0125] After the contact time, the supercritical CO2, now containing dissolved pyrolysis reaction products, is separated from the char in a separation operation 604. The separation operation may take the form of removing the char from the CO2 or removing the CO2 from the char.
[0126] After separation operation 604, supercritical CO2 is then cooled to a first temperature and a first pressure in a first cooling operation 606. For example, in an embodiment, the pyrolysis temperature and pressure are 540°C and 11MPa, respectively, and the first temperature and the first pressure are 450°C and 10.9MPa. The first cooling operation 606 may include reducing the temperature of CO2 from the pyrolysis temperature and pressure used in contact operation 602 or reducing the temperature and pressure of CO2. In addition, although referred to as cooling operation 606 in an embodiment, "cooling" may only include reducing the pressure of CO2 while maintaining the temperature at or near the pyrolysis temperature. Regardless of whether temperature, pressure or both are reduced, cooling operation 606 will cause the solubility of the dissolved reaction product to change, and any reaction product that is no longer soluble in CO2 at the first temperature and the first pressure will be condensed out from CO2 as a condensate.
[0127] As part of the first cooling operation 606 or after the first cooling operation 606, the condensate produced by the first cooling operation 606 can be collected and stored for later use. The content of the condensate will be determined by the reaction product produced by the pyrolysis reaction and the first temperature and the first pressure of the first cooling operation 606. Therefore, as described above, by selecting the first temperature and the first pressure, the chemical composition of the condensate produced by the first cooling operation 606 can be controlled to obtain a specific fraction of the pyrolysis reaction product. Once the temperature is known, in an embodiment, the heat exchange equation can be used to determine the relative flow rates of the return flow and the process flow of the different recuperators necessary to reach these temperatures, and thus determine the desired condensate. Based on this information, the controller can then set the position of the bypass valve as needed to obtain a determined flow rate.
[0128] Then, the CO2 with the remaining reaction products undergoes a second cooling operation 608. Similar to the first cooling operation 606, the second cooling operation 608 reduces the CO2 from a first temperature and a first pressure to a second temperature and a second pressure. Again, this may include reducing the temperature, pressure, or both of the CO2. The second cooling operation may be performed using the same equipment as the first cooling operation 606 or by passing the CO2 to a second set of equipment (e.g., a heat exchanger, a cooling vessel, etc.) in which the second cooling operation is performed.
[0129] As part of or after the second cooling operation 608, the condensate produced by the second cooling operation 608 can be collected and stored for later use. The content of the second condensate will be determined by the reaction products produced by the pyrolysis reaction, the first temperature and the first pressure used in the first cooling operation 606, and the second temperature and the second pressure of the second cooling operation 608. Therefore, as described above, by selecting the first temperature and the first pressure and the second temperature and the second pressure, the chemical composition of the condensate produced by the second cooling operation 606 can be controlled to obtain a specific fraction of the pyrolysis reaction product. Once the temperature is known, in an embodiment, the heat exchange equation can be used to determine the relative flow rates of the return flow and the process flow of the different recuperators necessary to reach those temperatures, and thus determine the desired condensate. Based on this information, the controller can then set the position of the bypass valve as needed to obtain a determined flow rate.
[0130] Additional cooling operations (not shown) may be performed. By using additional cooling operations, the fractionation and collection of the reaction products may be tightly controlled. For example, 25 cooling operations may be used to obtain a very finely fractionated condensate. Any number of cooling operations may be used as desired, depending on the operator's goals. Figure 4 , Figure 4 A system with the potential for five cooling operations is shown, and the chemical composition of the condensate of each of the five stages can be changed by changing the relative temperatures and pressures of the operations. For example, in one configuration, the first four cooling operations can be completed with very narrow temperature and / or pressure differences - for example, the first temperature can be 10°C below the pyrolysis temperature, the second temperature can be 20°C below the pyrolysis temperature, the third temperature can be 30°C below the pyrolysis temperature, and the fourth temperature can be 40°C below the pyrolysis temperature, while the last temperature can be 30°C, which will fractionate the higher temperature reaction products (i.e., the reaction products condensed from CO2 at higher temperatures). In another configuration, the temperature difference can be more uniform (even) between the stages, and in yet another configuration, the temperature can be focused on fractionating the lower temperature products. Thus, as part of the method, the temperature and pressure of the different cooling operations can be controlled to obtain specific desired fractions of the reaction products.
[0131] Finally, the CO2 is recycled and reused for additional pyrolysis is a recycling operation 610. Recycling can be accomplished in a continuous system where the CO2 is recycled in a continuous system such as Figure 4 Flows continuously in the loop shown in . Optionally, the CO2 can be stored for later reuse in a batch system or a semi-batch system.
[0132] As part of method 600, CO2 can be maintained in a supercritical state throughout the entire method. Optionally, CO2 can be brought to a subcritical state, such as in a final cooling operation, in order to condense and remove as many reaction products as possible before CO2 is returned to a supercritical state in a reuse operation 610.
[0133] Figure 7 is a more detailed embodiment of a method for pyrolyzing coal using supercritical CO2. Figure 6 The method 600 is written more broadly to cover any batch pyrolysis process, semi-batch pyrolysis process, or continuous pyrolysis process, but Figure 7 Method 700 is more directed to a continuous pyrolysis process for fractionating pyrolysis products from coal and recycling CO2 in a continuous flow loop.
[0134] exist Figure 7 In the embodiment shown in , method 700 begins by flowing an inlet stream of carbon dioxide (CO2) into a reaction chamber containing coal in a supercritical CO2 injection operation 702. In an embodiment, the temperature of the inlet CO2 stream is from 300°C-600°C and the pressure is from 7MPa-12MPa.
[0135] The reaction chamber is maintained at a pyrolysis temperature and pyrolysis pressure sufficient to maintain the CO2 in the reaction chamber in a supercritical state. Figure 7 , illustrated by pyrolysis operation 704. Pyrolysis operation 704 may include actively controlling the temperature and pressure of the reaction chamber. For example, an internal heater or an external heater may be used to directly add heat to the reaction chamber to control its temperature. Similarly, the pressure may be controlled by adjusting the flow rates of the inlet CO2 stream and the outlet CO2 stream. Alternatively, the temperature and pressure of the reaction chamber may be indirectly controlled only by controlling the temperature and flow rate of the inlet stream. Thus, in pyrolysis operation 704, coal is pyrolyzed to obtain char and supercritical CO2 containing dissolved pyrolysis products. As described above with reference to Figure 6 As discussed, the chemical composition of the reaction products can be controlled to a certain extent by varying the temperature and pressure in the reaction chamber and by using certain additives.
[0136] After a contact period determined by the CO 2 flow rate through the reaction chamber and the volume of CO 2 in the chamber, the supercritical CO 2 containing dissolved pyrolysis products then flows from the reaction chamber through an outlet as a reactor outlet stream in an outlet stream discharge operation 706 .
[0137] Then, in a first recuperation and collection operation 706a, the outlet stream is sent to a first recuperator. In this operation 706a, the reactor outlet stream is cooled in the first recuperator by transferring heat to a return stream of CO2 that is on its way back to the reaction chamber. Based on the temperature and flow rate of the two CO2 streams (i.e., the outlet stream and the return stream) passing through the first recuperator, the outlet stream is cooled to a first temperature that is lower than the pyrolysis reaction temperature.
[0138] The act of cooling the outlet stream causes dissolved reaction products (if any) in the outlet stream that condense at a temperature above the first temperature to condense from the CO2. The first recuperative heat exchange and collection operation 706a includes cooling the outlet stream in a collector (e.g., Figure 4 The first stage condensate is collected in a collection vessel (shown in FIG. 1 ). It also includes discharging a first stage CO 2 effluent stream, which contains any dissolved reaction products that are not removed as the first stage condensate.
[0139] It should be noted that not all of the outlet stream can be processed in the first recuperation and collection operation 706a. In an embodiment, some portion of the outlet stream can be sent to a recuperator of a subsequent stage and processed in a subsequent recuperation and collection operation. This splitting of some of the outlet stream can be done to control the chemical composition of the condensate obtained from different stages.
[0140] Then, in a second recuperation and collection operation 706b, the first stage CO2 effluent stream is transferred to a second recuperator. In this operation 706b, the reactor first stage CO2 effluent stream is cooled in the second recuperator by transferring heat to the return stream of CO2 that is on its way back to the reaction chamber. The first stage CO2 effluent stream is cooled to a second temperature that is lower than the first temperature based on the temperature and flow rate of the two CO2 streams (i.e., the first stage CO2 effluent stream and the return stream) passing through the second recuperator.
[0141] Again, the act of cooling the outlet stream causes those dissolved reaction products (if any) remaining in the first stage CO2 effluent stream that condense at a temperature above the second temperature to condense from the CO2. The second recuperation and collection operation 706b includes cooling the CO2 in a collector (e.g., Figure 4 The second stage condensate is collected in a collection vessel (shown in FIG. 1 ). It also includes discharging a second stage CO 2 effluent stream, which contains any remaining dissolved reaction products that are not removed as the second stage condensate.
[0142] Again, not all of the first stage CO2 effluent stream needs to be passed to the second recuperator, and some portion of the first stage CO2 effluent stream may be diverted to subsequent recuperation and collection operations in order to change the chemical composition of subsequent stage condensates.
[0143] Any number of additional recuperation and collection operations may be performed in method 700. Figure 7 , and the nth stage of recuperation and collection operations 706a-n are illustrated in FIG. Each of the recuperation and collection operations 706a-n can be identical except for the operating temperature and pressure of the two CO2 streams involved. The condensate recovered from each of the operations 706a-n can be controlled by diverting portions of the process stream and / or return stream around and to the various operations 706a-n to obtain the desired condensate. The distribution of the flows through the different recuperation and collection operations 706a-n can be controlled manually or automatically by a controller so that different fractions are collected at different stages, as described above.
[0144] Note that Figure 7 One or more of the operations 706a-n, such as, for example, the final recuperation and collection operation 706n, may not include recuperation of heat from the process stream. That is, rather than transferring heat to a return stream of CO2 and effectively recycling that energy, the heat may simply be removed, such as by transferring it to a cold water stream, and either discarded or recycled for another purpose.
[0145] Furthermore, not all recuperation and collection operations 706a-n need to include collecting condensate in a separate vessel. Instead, some condensate may be directed to a subsequent stage heat exchanger for later collection in a downstream recuperation and collection operation.
[0146] After the final recuperation and collection operation 706n, the final stage CO2 effluent stream is then reconditioned by passing it through the various recuperation stages as a return stream in a reconditioning operation 708. The reconditioning operation 708 may include compressing the return stream and / or heating the return stream at one or more points in the CO2 return loop of the system. For example, Figure 4 , the return stream is compressed by pump 420 just after the fifth recuperation and collection operation (not true recuperation in this case since heat is removed using a cold water stream) and is heated by heater 422 just before being injected into reaction chamber 402.
[0147] Note that the reconditioning operation 708 may or may not purge any remaining reaction products from the CO 2. In an embodiment, when the CO 2 return stream is injected into the reaction chamber, some trace amounts of reaction products and / or other compounds such as water remain in the CO 2 return stream.
[0148] After reconditioning, the CO2 return stream is then injected into the reaction chamber as an inlet stream in injection operation 402. Figure 7 This is illustrated by the return arrow from the reconditioning operation 708 to the injection operation 702.
[0149] Figure 8 The figure shows an embodiment of a method for improving mesophase pitch for carbon fiber production using supercritical carbon dioxide. The method uses some or all of a coal tar product having at least some mesophase pitch as a raw material, including those discussed above. In an optional embodiment, any raw material having at least some mesophase pitch, whether derived from coal, any other biomass or hydrocarbon material, can be used as a raw material. For the remainder of this specification, "coal tar" is a material / oil from the pyrolysis or coking of coal. The material extracted from coal tar is referred to as "coal tar pitch".
[0150] In general, the following method 800 improves the quality of coal tar products by separating and recovering high molecular weight (MW) coal tar, for example, by contacting the feedstock with a mixture of a supercritical fluid solvent and a co-solvent from the above Figure 4 The system 400 shown is separated and reclaimed high molecular weight (MW) coal tar to improve the quality of coal tar products. High molecular weight refers to compounds with 1,000amu or higher molecular weight. The high MW hydrocarbons of coal tar are mesophase precursor materials. Although supercritical fluid can be any supercritical fluid as described above, and cosolvent can be any cosolvent or mixture of cosolvents, cosolvent includes aromatic organic solvents (such as, for example, benzene, xylene, tetralin, tetrahydrofuran, pyridine, quinoline, isoquinoline and the like), the remainder of this specification will discuss the specific embodiment of supercritical carbon dioxide (sCO ) / toluene solvent / cosolvent combination. Those skilled in the art will recognize that the present disclosure is not limited to the specific embodiments described below.
[0151] Method 800 begins (operation 802) by placing raw coal tar in a reactor vessel, such as vessel 404 above. In an embodiment, any particular fraction or combination of fractions of coal tar may be used as the initial raw material. For example, in an embodiment, all coal tar produced by system 400 of the disclosed application may be used. Alternatively, all coal tar condensed above a certain threshold temperature may be used. For example, all coal tar condensed at 50°C, 100°C, 150°C, or 200°C or above 50°C, 100°C, 150°C, or 200°C may be used. Alternatively, coal tar condensed between some defined temperature ranges may be used.
[0152] The reactor vessel is then raised to operating temperature and operating pressure (as described above), and in sCO2 / toluene extraction operation 804, sCO2 / toluene solvent passes through reactor vessel 404 and condensation loop. From the sCO2 / toluene solvent of the flow that leaves reaction vessel by condensation loop, collect and reclaim toluene soluble (TS) fraction. Flow keeps a certain time period, such as for example 1 minute, 1 hour, 2 hours, 4 hours, 10 hours, 24 hours etc., and it is selected by operator. The time period can be fixed, or can determine based on the amount of the TS fraction material reclaimed over time. For example, when the amount of TS fraction material per minute drops to below threshold value, extraction can be considered to be completed. After this time period, flow is terminated, and reactor conditions are reduced to below supercritical condition.
[0153] Optionally, the material remaining in the reaction vessel can then be washed with toluene as a final step in operation 804. Alternatively, after the temperature and pressure conditions have been reduced to below supercritical conditions, a solvent other than toluene or a combination of solvents (e.g., toluene and xylene) can be used.
[0154] After the sCO2 / toluene extraction operation 804, the remaining toluene insoluble (TI) fraction in the reaction vessel can be washed with quinoline in the quinoline soluble fraction extraction operation 806. In an alternative embodiment, the extraction operation 806 can be completed in a different reaction vessel, which requires a transfer operation between the vessels.
[0155] In a kind of embodiment of this operation 806, quinoline is added in the remaining material in the container, and remains on a certain temperature and pressure and continues a certain time period.In selectable embodiments, quinoline circulation continues a certain time period by the reaction vessel that remains on a certain temperature and pressure.After the time period of expectation, for any time period, for example, be less than or up to 1 minute, 1 hour, 2 hours, 4 hours, 10 hours, 24 hours etc., quinoline is removed, thereby removes any quinoline soluble (QS) material, quinoline insoluble (QI) material is stayed in the reaction vessel.
[0156] Quinoline and any dissolved QS components are then distilled in a distillation operation, such as using rotary evaporation, to separate quinoline from the QS compounds. The QS compounds recovered from the distillation of quinoline (referred to herein as the QS fraction) represent an improved coal tar product suitable for producing anisotropic mesophase pitch suitable for carbon fiber formation / spinning.
[0157] After distillation, the QS fraction is heat treated to prepare mesophase pitch before being added to the extruder. If mesophase material already exists, the heat treatment operation 807 produces a mesophase structure or increases the amount of mesophase material. In an embodiment, the heat treatment operation 807 can be carried out under vacuum conditions, atmospheric conditions or pressurized conditions (e.g., from 1.01atm to 500atm), and includes heating the QS fraction to from 300°C to 400°C and maintaining it at this temperature for a period of time sufficient to produce a mesophase structure. For example, in one embodiment, temperature-controlled sCO2 can be used to heat the QS fraction in the reactor vessel. Through this step, a mesophase structure (70%-100%) is produced. Operation 807 can also produce some additional quinoline-insoluble (QI) materials, which can be separated from the QS fraction before the next operation as shown. This can be accomplished by performing a second extraction operation 806.
[0158] In alternative embodiments, the heat treatment operation 807 can heat the QS fraction to any temperature from 200° C. to 800° C. for any period of time, e.g., less than or up to 1 minute, 1 hour, 2 hours, 4 hours, 10 hours, 24 hours, etc., as selected by the operator. The period of time can be fixed or can be determined based on the amount of mesophase generated.
[0159] The QS fraction is then thoroughly mixed and extruded under fixed conditions in a mixing operation 808. This can be accomplished using any commercial mixer or extruder such as, for example, a HAAKE TM MiniLab 3 micro mixer or Pharma 11 twin screw extruder (both from Thermo In this operation, the QS fraction is thoroughly mixed in a sCO2 environment under supercritical conditions for a desired amount of time. After the desired amount of mixing, the QS fraction and sCO2 mixture is extruded. When the material leaves the mixer / extruder, at a certain temperature, the sCO2 solvent evaporates from the mixture, taking away any compounds dissolved in the sCO2, leaving fibers of the mesophase pitch. It is believed that most (if not all) of the remaining extruded material will be mesophase pitch, and for this reason, it is called the mesophase fraction. Without being bound by any particular theory, it is also believed that extrusion with sCO2 at a certain temperature can potentially serve as both an oxidant and a catalyst for the remaining unwanted light MW compounds (representing impurities in the mesophase pitch solution), which can eventually form coke or poor crystallization when graphitized, resulting in poor carbon fiber quality.
[0160] In the mixing operation 808 described above, mixing and extruding are carried out simultaneously as a combined process. In an optional embodiment, mixing and extruding can be handled as a separate operation. In this embodiment, mixing is carried out under supercritical conditions and in the sCO environment for a period of time such as the time necessary for the complete mixing of the QS fraction. After it is fully mixed, the QS fraction and sCO then pass through an extruder, which separates sCO from the mesophase fraction and produces the fiber of the mesophase fraction. The pressure, partial pressure, concentration of sCO can be adjusted before extruding. The sCO of the separation of the low MW compounds that may comprise at least some dissolving is removed as the sCO fraction.
[0161] In yet another embodiment, the extrusion process can be performed with an amount of CO2 solvent and a co-solvent (e.g., quinoline or toluene) from the sCO2 / toluene extraction operation 804 with a mesophase fraction. The mesophase fraction can then be melt spun or otherwise extruded directly into fibers as known in the art.
[0162] In yet another embodiment, the extrusion process can be replaced by a simple separation process in which the sCO2 fraction is separated from the mesophase fraction. After this separation, the mesophase fraction can then be melt-spun or otherwise directly extruded into fibers as known in the art. Alternatively, the mesophase fraction can be sold as is or can be used for other purposes besides making fibers.
[0163] The fibers of the mesophase fraction can be further stabilized in an optional stabilization operation 810. Current stabilization practice is to extrude and draw the fibers through a series of moderate (~200°C-300°C) temperature oxidation ovens. One purpose of conventional stabilization is to oxidatively remove remaining light MW materials prior to graphitization. Because the previous operations in method 800, particularly the sCO2 / toluene extraction operation 804 and the mixing operation 808, are expected to remove many (if not most or all) of the lower molecular weight compounds, the sCO2 process described above can completely eliminate the need for stabilization operation 810, or alternatively reduce the amount of time required for adequate stabilization.
[0164] After stabilization, an optional carbonization operation 812 as known in the art may be performed. Carbonization is a process that removes all non-organic elements and produces a crystalline carbon structure in the fiber by heating the fiber in an oxygen-free environment. Due to the earlier extraction, it is possible that the mesophase fraction will be completely free of non-organic elements to eliminate the need for a carbonization operation, or it may reduce the time required for carbonization to be performed.
[0165] The mesophase fraction may then be subjected to a graphitization operation 814, as known in the art, as a final step in the manufacture of carbon fibers. Graphitization involves treating the fibers at high temperatures to improve the alignment and orientation of the crystalline regions along the fiber direction. Aligning, stacking, and orienting the crystalline regions along the fiber direction increases the overall strength of the carbon fibers.
[0166] The following numbered items define additional exemplary aspects and features of the present technology:
[0167] 1. A method comprising:
[0168] contacting a coal tar containing at least some mesophase pitch precursor with a supercritical carbon dioxide (sCO2) and toluene mixture to remove at least some toluene soluble components from the coal tar to obtain a toluene insoluble fraction;
[0169] After the contacting operation, separating the sCO2 and toluene mixture from the toluene insoluble fraction;
[0170] washing the toluene insoluble fraction with quinoline to obtain a quinoline-soluble fraction mixture of the toluene insoluble fraction;
[0171] separating the quinoline from the quinoline-soluble fraction;
[0172] The quinoline soluble fraction is mixed with sCO 2 to obtain a sCO 2 / quinoline soluble fraction mixture.
[0173] 2. The method according to item 1, wherein the contacting operation further comprises:
[0174] The sCO2 / quinoline soluble fraction mixture is passed through an extruder to separate the sCO2 from the quinoline soluble fraction to obtain fibers of mesophase pitch.
[0175] 3. The method according to item 1 or 2, further comprising:
[0176] After the separation operation, the toluene insoluble fraction is subjected to a toluene wash to remove additional soluble materials from the toluene insoluble fraction.
[0177] 4. The method according to any one of items 1 to 3, wherein separating the quinoline from the quinoline soluble fraction further comprises:
[0178] The quinoline and quinoline soluble fraction mixture is distilled.
[0179] 5. The method according to any one of items 1 to 4, wherein separating the quinoline from the quinoline soluble fraction further comprises:
[0180] The quinoline is evaporated to obtain the quinoline soluble fraction mixture.
[0181] 6. The method according to any one of items 1 to 5, further comprising:
[0182] The quinoline soluble fraction is heated to from 300°C to 400°C.
[0183] 7. The method according to any one of items 1 to 6, further comprising:
[0184] The quinoline soluble fraction is heated to from 300°C to 400°C for less than 24 hours.
[0185] 8. The method according to any one of items 1 to 7, further comprising:
[0186] The fibers of the mesophase pitch are stabilized.
[0187] 9. The method according to any one of items 1 to 8, further comprising:
[0188] The fibers of the mesophase pitch are carbonized.
[0189] 10. The method according to any one of items 1 to 9, further comprising:
[0190] The fibers of the mesophase pitch are graphitized.
[0191] 11. The method according to any one of items 1 to 10, further comprising:
[0192] passing the sCO2 and toluene mixture through a reactor vessel containing the coal tar; and
[0193] wherein the washing operation comprises washing the toluene insoluble fraction in the reactor vessel.
[0194] 12. The method according to item 11, further comprising:
[0195] The quinoline is circulated through the reactor vessel for up to 24 hours before the quinoline is separated from the quinoline soluble fraction.
[0196] 13. The method according to any one of items 1 to 12, further comprising:
[0197] The quinoline soluble fraction is heated to from 200°C to 800°C.
[0198] 14. The method according to any one of items 6 to 13, wherein the heating operation further comprises:
[0199] The quinoline soluble fraction is contacted with sCO2 heated to a temperature between 300°C and 400°C.
[0200] 15. The method according to any one of items 6 to 14, further comprising:
[0201] After the heating operation, at least some of the quinoline-insoluble material is separated from the quinoline-soluble material.
[0202] 16. A method for making carbon fiber, comprising:
[0203] contacting a coal tar containing at least some mesophase pitch precursor with a supercritical carbon dioxide (sCO2) and toluene mixture to remove at least some toluene soluble components from the coal tar to obtain a toluene insoluble fraction;
[0204] After the contacting operation, separating the sCO2 and toluene mixture from the toluene insoluble fraction;
[0205] After the separation operation, mixing the toluene insoluble fraction with sCO 2 to obtain a sCO 2 / toluene insoluble fraction mixture; and
[0206] The sCO 2 / toluene insoluble fraction mixture is passed through an extruder, thereby separating the sCO 2 from the toluene insoluble fraction to obtain fibers of the mesophase pitch.
[0207] 17. The method according to item 16, further comprising:
[0208] washing the toluene insoluble fraction with quinoline to obtain a quinoline-soluble fraction mixture of the toluene insoluble fraction and a quinoline-insoluble fraction;
[0209] separating the quinoline from the quinoline-soluble fraction of the toluene-insoluble fraction; and
[0210] The quinoline soluble fraction of the toluene-insoluble fraction is mixed with sCO 2 to obtain a sCO 2 / quinoline soluble fraction mixture.
[0211] 18. The method according to item 17, further comprising:
[0212] Prior to mixing the quinoline soluble fraction of the toluene insoluble fraction with sCO2, the quinoline soluble fraction of the toluene insoluble fraction is heated to from 300°C to 400°C for less than 24 hours.
[0213] 19. The method according to item 18, wherein the heating operation further comprises:
[0214] The quinoline soluble fraction is contacted with sCO2 heated to a temperature between 300°C and 400°C for up to 24 hours.
[0215] 20. The method according to any one of items 16-19, further comprising:
[0216] The fibers of the mesophase pitch are subjected to a stabilization operation.
[0217] 21. The method according to any one of items 16 to 20, further comprising:
[0218] The fibers of the mesophase pitch are subjected to a carbonization operation.
[0219] 22. The method according to any one of items 16 to 21, further comprising:
[0220] The fibers of the mesophase pitch are graphitized.
[0221] 23. A method for manufacturing carbon fiber, comprising:
[0222] contacting a coal tar containing at least some mesophase pitch precursor with a supercritical fluid solvent and a first co-solvent mixture to remove at least some soluble components from the coal tar to obtain an insoluble coal tar fraction;
[0223] After the contacting operation, separating the supercritical fluid solvent and the first co-solvent mixture from the insoluble coal tar fraction;
[0224] After the separation operation, mixing the insoluble coal tar fraction with sCO2 to obtain a sCO2 / insoluble fraction mixture; and
[0225] The sCO2 / insoluble fraction mixture is passed through an extruder to separate the sCO2 from the insoluble fraction to obtain fibers of the mesophase pitch.
[0226] 24. The method according to item 23, further comprising:
[0227] washing the insoluble fraction with a second co-solvent to obtain a second co-solvent and a second co-solvent soluble fraction mixture of the first insoluble fraction and a second co-solvent insoluble fraction;
[0228] separating the second co-solvent from the second co-solvent soluble fraction of the insoluble fraction; and
[0229] mixing the second co-solvent soluble fraction of the insoluble fraction with sCO2 to obtain a sCO2 / second co-solvent soluble fraction mixture;
[0230] The second co-solvent is selected from one or more of benzene, xylene, tetralin, tetrahydrofuran, pyridine and quinoline.
[0231] 25. The method according to item 24, further comprising:
[0232] The second co-solvent soluble fraction of the insoluble fraction is heated to from 300° C. to 400° C. for less than 24 hours prior to mixing the second co-solvent soluble fraction with sCO 2 .
[0233] 26. The method according to item 25, wherein the heating operation further comprises:
[0234] The second co-solvent soluble fraction is contacted with sCO2 heated to a temperature between 300°C and 400°C for up to 24 hours.
[0235] 27. The method according to any one of items 23-26, further comprising:
[0236] The fibers of the mesophase pitch are subjected to a stabilization operation.
[0237] 28. The method according to any one of items 23-27, further comprising:
[0238] The fibers of the mesophase pitch are subjected to a carbonization operation.
[0239] 29. The method according to any one of items 23-28, further comprising:
[0240] The fibers of the mesophase pitch are graphitized.
[0241] 30. A method according to any one of items 23-29, wherein the supercritical fluid solvent is selected from one or more of carbon dioxide, water, methane, nitrous oxide, ethane, propane, ethylene, propylene, methanol, ethanol and acetone.
[0242] 31. The method according to any one of items 23-30, wherein the first co-solvent is an aromatic organic solvent.
[0243] 32. The process according to any one of items 24 to 30, wherein the second co-solvent is an aromatic organic solvent.
[0244] 33. The method according to any one of items 23-32, wherein the first co-solvent is selected from one or more of benzene, xylene, tetralin, tetrahydrofuran, pyridine and quinoline.
[0245] 34. The method according to any one of items 23-33, wherein the second co-solvent is selected from one or more of benzene, xylene, tetralin, tetrahydrofuran, pyridine and quinoline.
[0246] 35. The method according to any one of items 1 to 34, wherein the coal tar is produced by:
[0247] pyrolyzing the combination of carbonaceous feedstock at a first temperature and a first pressure and for a first period of time to produce a C1-C4 gas;
[0248] raising the combination to a second temperature greater than the first temperature;
[0249] pyrolyzing the combination at the second temperature and for a second period of time to produce coal tar; and
[0250] Coal tar is extracted from the combination.
[0251] 36. The method according to item 35, wherein the first temperature is from 150°C to 350°C, and the first pressure is from 7MPa to 30MPa.
[0252] 37. The method according to item 35 or 36, wherein the second temperature is from 350°C to 550°C.
[0253] 38. A method according to any one of items 35-37, wherein the first time period is from 1 minute to 120 minutes.
[0254] 39. A method according to any one of items 35-38, wherein the first time period is determined based on the amount of at least one C1-C4 gas produced by the carbonaceous feedstock at the first temperature.
[0255] 40. A method according to any one of items 35-39, wherein the second time period is from 1 minute to 24 hours.
[0256] 41. The method according to any one of items 35-40, wherein pyrolysis of the carbonaceous feedstock at the first temperature and first pressure is carried out in a first pyrolysis reaction chamber.
[0257] 42. The method according to any one of items 35-41, wherein pyrolysis of the carbonaceous feedstock at the second temperature is carried out in a first pyrolysis reaction chamber.
[0258] 43. A method according to any one of items 35-42, wherein pyrolysis of the carbonaceous feedstock at the second temperature is carried out in a second pyrolysis reaction chamber different from the first pyrolysis reaction chamber.
[0259] 44. A method according to any one of items 35-43, wherein pyrolyzing the carbonaceous feedstock at the first temperature and first pressure is carried out in a carbon dioxide atmosphere.
[0260] 45. The method according to any one of items 35-44, further comprising:
[0261] The concentration of one or more C1-C4 gases in the pyrolysis atmosphere is monitored.
[0262] 46. The method of claim 45, wherein extracting the coal tar comprises transferring the carbon dioxide atmosphere to a separation system.
[0263] 47. A method according to item 45 or 46, wherein extracting the coal tar includes reducing at least one of the temperature or pressure of the carbon dioxide atmosphere.
[0264] Unless otherwise indicated, all numbers expressing quantities of ingredients, properties such as molecular weight, reaction conditions, etc. used in the specification and claims are to be understood as being modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the accompanying specification and claims are approximations that may vary depending upon the desired properties sought to be obtained.
[0265] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the technology are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0266] It will be apparent that the systems and methods described herein are well adapted to achieve the objects and advantages mentioned as well as those inherent therein. Those skilled in the art will recognize that the methods and systems of this specification may be implemented in many ways and therefore should not be limited by the foregoing illustrated embodiments and examples. In this regard, any number of features of the various embodiments described herein may be combined into a single embodiment, and alternative embodiments having less than or more than all of the features described herein are possible.
[0267] Although various embodiments have been described for the purposes of this disclosure, various changes and modifications may be made which are well within the contemplated scope of this disclosure. For example, in embodiments, the quinoline extraction operation 806 may be omitted and the TI fraction may be sent directly to the heat treatment operation 807. Many other changes may be made which will readily occur to those skilled in the art and which are encompassed in the spirit of this disclosure.
Claims
1. A method for manufacturing carbon fiber, comprising: contacting a coal derivative with a supercritical fluid solvent and a first co-solvent mixture to remove at least some soluble components from the coal derivative to obtain an insoluble coal derivative fraction; after contacting the coal derivative with the supercritical fluid solvent and the first co-solvent mixture, separating the supercritical fluid solvent and the first co-solvent mixture from the insoluble coal derivative fraction; After separating the supercritical fluid solvent and the first co-solvent mixture from the insoluble coal derivative fraction, mixing the insoluble coal derivative fraction with a supercritical fluid to obtain a supercritical fluid / insoluble fraction mixture; as well as After mixing the insoluble coal derivative fraction with the supercritical fluid, the supercritical fluid is separated from the insoluble fraction to obtain the carbon fiber.
2. The method of claim 1, wherein the coal derivative comprises coal tar.
3. The method according to claim 1, wherein: The coal derivative includes a mesophase pitch precursor; and The carbon fibers include fibers of mesophase pitch.
4. The method of claim 1, wherein the supercritical fluid comprises supercritical carbon dioxide.
5. The method of claim 1, wherein separating the supercritical fluid from the insoluble fraction comprises passing the supercritical fluid / insoluble fraction mixture through an extruder.
6. The method according to claim 1, further comprising: washing the insoluble coal derivative fraction with a second co-solvent to obtain a second co-solvent and a second co-solvent soluble fraction mixture of the insoluble coal derivative fraction and a second co-solvent insoluble fraction; separating the second co-solvent from the second co-solvent soluble fraction of the insoluble coal derivative fraction; as well as The second co-solvent soluble fraction of the insoluble coal derivative fraction is mixed with the supercritical fluid to obtain the supercritical fluid / insoluble fraction mixture.
7. The method of claim 6, wherein the second co-solvent comprises one or more of benzene, xylene, tetralin, tetrahydrofuran, pyridine, and quinoline.
8. The method according to claim 6, further comprising: heating the second co-solvent soluble fraction of the insoluble coal derivative fraction to a temperature in the range of 300° C. to 400° C. for less than 24 hours prior to mixing the second co-solvent soluble fraction with the supercritical fluid; as well as The second co-solvent soluble fraction is contacted with the supercritical fluid heated to a temperature between 300°C and 400°C for up to 24 hours.
9. The method according to claim 1, further comprising performing one of the following: Stabilizing the carbon fibers; Carbonizing the carbon fibers; and A graphitization operation is performed on the carbon fibers.
10. The method of claim 6, wherein at least one of the first co-solvent and the second co-solvent comprises an aromatic organic solvent.
11. The method of claim 6, wherein at least one of the first co-solvent and the second co-solvent comprises one or more of benzene, xylene, tetralin, tetrahydrofuran, pyridine, and quinoline.
12. The method of claim 1, wherein the supercritical fluid solvent comprises one or more of carbon dioxide, water, methane, nitrous oxide, ethane, propane, ethylene, propylene, methanol, ethanol, and acetone.
13. The method of claim 1, wherein the coal derivative is produced by: pyrolyzing the combination of carbonaceous feedstock at a first temperature and a first pressure and for a first period of time to produce a C1-C4 gas; raising the combination to a second temperature greater than the first temperature; pyrolyzing the combination at the second temperature and for a second period of time to produce a coal derivative; and A coal derivative is extracted from the combination.
14. The method according to claim 13, wherein: The first temperature is in the range of 150°C to 350°C; The second temperature is in the range of 350°C to 550°C; and The first pressure is in the range of 7 MPa to 30 MPa.
15. The method of claim 13, wherein the first time period is in the range of 1 minute to 120 minutes.
16. The method of claim 13, wherein the second time period is in the range of 1 minute to 24 hours.
17. The method of claim 13, wherein pyrolyzing the carbonaceous feedstock at the first temperature and first pressure is performed in a first pyrolysis reaction chamber.
18. The method of claim 13, wherein pyrolyzing the carbonaceous feedstock at the first temperature and first pressure is performed in a carbon dioxide atmosphere.
19. The method of claim 13, wherein the method is conducted in a carbon dioxide atmosphere, and wherein extracting the coal derivative comprises transferring the carbon dioxide atmosphere to a separation system.