Welded joints and automotive components
By optimizing the chemical composition and toe angles of weld metals in automobile parts, the welded joints achieve enhanced fatigue strength and electrodeposition coating properties, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2021000083
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-01-04
AI Technical Summary
Existing welded joints in automobile parts, particularly lap fillet joints, lack both fatigue strength and electrodeposition coating properties, with existing technologies failing to address these requirements effectively.
A welded joint composition comprising specific chemical elements in the weld metal, such as C, Si, Mn, Ti, and Zr, controlled Ceq, and optimized toe angles, along with controlled slag composition, to enhance fatigue strength and electrodeposition coating properties.
The proposed solution results in welded joints with improved fatigue characteristics and high electrodeposition coating properties, ensuring durability and coating adherence.
Smart Images

Figure 0007568920000007 
Figure 0007568920000008 
Figure 0007568920000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a welded joint and an automobile component. [Background technology]
[0002] In mechanical structural components having welded joints, the structure is usually designed so that tensile stress occurs at the weld toe, and therefore, improvements in the mechanical properties, especially fatigue strength, of the weld toe have been studied.
[0003] Patent Document 1 discloses a lap arc welded joint structure having excellent fatigue strength, characterized in that the chemical composition is: C: more than 0.005% and not more than 0.35%, Si: 2.0% or less, Mn: more than 0.10% and not more than 3.0%, P: 0.20% or less, S: 0.08% or less, Al: more than 0.01% and not more than 0.10%, and the Ceq of the steel plate - Ceq of the weld metal part is < -0.1.
[0004] Patent Document 2 describes a lap fillet arc welded joint including a first steel plate and a second steel plate overlapping each other and each having a tensile strength of 950 MPa or more, and a weld metal extending along a corner formed by the surface of the first steel plate and the end face of the second steel plate, the Vickers hardness of the weld metal being 400 HV or less, and when viewed in a cross section perpendicular to the weld line of the weld metal, the position of the fusion boundary present on the surface of the first steel plate is defined as point A, and in an X direction parallel to the surface of the first steel plate, a position 0.3 mm away from point A toward the inside of the weld metal is defined as point D, and in the X direction, a position 0.3 mm away from point A toward the inside of the weld metal is defined as point D. The present invention discloses a lap fillet arc welded joint, characterized in that, when a position 0.4 mm away toward the inside is defined as point C, an intersection point between a line passing through point D and extending in the thickness direction of the first steel plate and the surface of the weld metal is defined as point B, an angle between the line connecting point A and point B and a line connecting point A and point D is defined as a toe angle β of the weld metal, a total number of recesses present on the surface of the weld metal contained in a range between point A and point C is defined as NA, and a number of recesses that are in contact with ferrite grains having a maximum grain size of 10 μm or more is defined as NB, the weld metal simultaneously satisfies the following conditional formulas (1) and (2): 0°< β < 30° …(1) NB / NA ≦ 0.70 …(2) (However, NA is 20 or more) [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-340947 [Patent Document 2] International Publication No. 2019 / 035490 Summary of the Invention [Problem to be solved by the invention]
[0006] In the manufacture of automobile components having welded joints (e.g., lap fillet welded joints of thin plates), the welded joints are required to have electrodeposition paintability in addition to fatigue strength. Neither Patent Document 1 nor Patent Document 2 takes electrodeposition paintability into consideration, nor does it disclose any specific means for improving it. In addition, the technology of Patent Document 2 aims to lower the carbon equivalent (Ceq) of the weld metal, and in this regard, it is believed that there is room for improvement in fatigue strength.
[0007] In view of the above circumstances, an object of the present invention is to provide a welded joint and an automobile component which have excellent fatigue properties at the weld toe and high electrodeposition paintability. [Means for solving the problem]
[0008] The gist of the present invention is as follows.
[0009] (1) A welded joint according to one aspect of the present invention is a welded joint including two or more steel plates and a weld metal joining the two or more steel plates, the weld metal having a chemical composition, in unit mass%, of C: 0.01 to 0.25%, Si: 0.01 to 1.00%, Mn: 0.80 to 2.50%, P: 0.0500% or less, S: 0.0100% or less, Ti: 0.020 to 0.120%, and Zr: 0.001 to 0.050%. and the balance being iron and impurities, the Ceq of the weld metal calculated by the following formula 1 is 0.450 to 0.950 mass%, the Vickers hardness of the weld metal is 300 HV or more, at least one of the two or more steel plates has a plate thickness of 0.8 mm or more and 4.0 mm or less, the Si content of slag adhering to the weld joint is 5.0 mass% or less, and the Si content Si WM and the largest value Si among the Si contents in unit mass% of two or more of the steel plates. BM and satisfies the following formula 2. Ceq=C+Mn / 6+Si / 24: Equation 1 2.5×{(Si WM / 0.89)-0.6×Si BM}≦0.510: Formula 2 Here, the element symbols included in the formula 1 indicate the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal. (2) In the welded joint described in (1) above, the Ti content in unit mass% of the weld metal is WM and the largest Ti content in unit mass% of two or more of the steel plates. BM may satisfy the following formula 3. 0.050≦2.5×{(Ti WM / 0.54)-0.6×Ti BM}≦0.300: Formula 3 (3) In the welded joint described in (1) or (2) above, the Vickers hardness of the weld metal may be 80% or more of HM calculated by the following formula 4. HM = 884 × C × (1-0.3 × C 2 )+294:Expression 4 Here, the element symbols included in the formula 4 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal. (4) In the welded joint according to any one of the above (1) to (3), the total content of Ti and Zr in the slag may be 0.5 mass % or more. (5) In the welded joint according to any one of the above (1) to (4), a toe angle at one or more toes of the weld metal may be greater than 0° and less than 30°. (6) In the welded joint described in (5) above, the two or more steel plates may be a first steel plate and a second steel plate overlapped with each other, the weld metal may join a surface of the first steel plate and an end face of the second steel plate, and a toe angle of the weld metal at the toe of the weld metal on the side of the first steel plate may be more than 0° and less than 30°. (7) In the welded joint according to any one of (1) to (6) above, the chemical composition of the weld metal may contain, in unit mass%, one or more elements selected from the group consisting of Al: 0.12% or less, Ni: 3.00% or less, Cr: 1.20% or less, Mo: 1.00% or less, V: 0.30% or less, Nb: 0.10% or less, B: 0.0600% or less, Mg: 0.01% or less, Cu: 1.00% or less, O: 0.0500% or less, and N: 0.0300% or less, in place of a portion of the iron, and the Ceq of the weld metal may be calculated by the following formula 5. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 4: Formula 5 Here, the element symbols included in the formula 5 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal. (8) An automobile member according to another aspect of the present invention includes the welded joint according to any one of (1) to (7) above. Effect of the Invention
[0010] According to the present invention, it is possible to provide a welded joint and an automobile component having excellent fatigue properties at the weld toe and high electrodeposition paintability. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a cross-sectional schematic view of a welded joint according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating measurement points of Vickers hardness of a weld metal. [Diagram 3] FIG. 4 is a schematic diagram illustrating a welding target position. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present inventors have conducted extensive research into means for improving the fatigue properties and electrodeposition paintability of the weld toe, and as a result have discovered the following.
[0013] (1. Chemical composition, Ceq, and hardness of weld metal) First, it is necessary to properly control the chemical composition and Ceq of the weld metal and to increase the hardness of the weld metal, which will improve the fatigue strength of the weld metal.
[0014] (2. Silicon content in slag) Next, it is necessary to reduce the amount of silicon in the slag that adheres to the welded joint, which will improve the electrical conductivity of the slag and improve the electrodeposition paintability.
[0015] (3. Relationship between Si content of steel plate and Si content of weld metal) Furthermore, it is necessary to optimize the relationship between the Si content of the steel plate and the Si content of the weld metal. During arc welding, the base steel plate is also heated by heat conduction from the molten pool. As a result, oxide scale is formed on the surface of the heat-affected zone of the steel plate. In addition, welding fumes may adhere to the surface of the heat-affected zone of the steel plate. These deteriorate the electrodeposition paintability. By selecting the chemical compositions of the welding material and the steel plate so that the Si content of the steel plate and the Si content of the weld metal satisfy the formula described below, the above-mentioned phenomenon can be suppressed and the electrodeposition paintability can be further improved.
[0016] The welded joint according to the present embodiment, which was obtained based on the above findings, will be described below. Unless otherwise specified, the unit "%" regarding the chemical composition of the weld metal, the chemical composition of the steel plate, and the chemical composition of the slag means mass%.
[0017] The welded joint according to the present embodiment includes two or more steel plates and a weld metal that joins the two or more steel plates. The shape of the joint is not particularly limited, and various shapes such as a T-shaped fillet welded joint, a lap fillet welded joint, and a butt welded joint can be selected. First, the weld metal will be described.
[0018] (C: 0.01~0.25%) C is an important element that affects the strength of the weld metal. If the C content of the weld metal is less than 0.01%, the strength of the weld metal is insufficient. On the other hand, if the C content of the weld metal exceeds 0.25%, the toughness of the weld metal is impaired. Therefore, the C content of the weld metal is set to 0.01 to 0.25%. The C content of the weld metal may be 0.02% or more, 0.05% or more, or 0.10% or more. The C content of the weld metal may be 0.24% or less, 0.22% or less, or 0.20% or less.
[0019] (Si: 0.01 to 1.00%) Si has the effect of deoxidizing the weld metal. In addition, Si dissolved in the weld metal also contributes to improving the strength of the weld metal. If the Si content of the weld metal is less than 0.01%, these effects cannot be obtained. On the other hand, if the Si content of the weld metal exceeds 1.00%, the toughness of the weld metal is impaired. If the Si content of the weld metal exceeds 1.00%, the amount of insulating slag increases and the electrodeposition paintability is impaired. Therefore, the Si content of the weld metal is set to 0.01 to 1.00%. The Si content of the weld metal may be 0.02% or more, 0.05% or more, or 0.10% or more. The Si content of the weld metal may be 0.90% or less, 0.80% or less, or 0.60% or less.
[0020] (Mn: 0.80~2.50%) Mn is an important element for improving the hardenability of the weld metal. If the Mn content of the weld metal is less than 0.80%, the hardenability is insufficient, and the strength of the weld metal is insufficient. On the other hand, if the Mn content of the weld metal exceeds 2.50%, the toughness of the weld metal is impaired. Therefore, the Mn content of the weld metal is set to 0.80 to 2.50%. The Mn content of the weld metal may be 1.00% or more, 1.20% or more, or 1.50% or more. The Mn content of the weld metal may be 2.40% or less, 2.20% or less, or 2.00% or less.
[0021] (P:0.0500% or less) P is an impurity. If the P content of the weld metal exceeds 0.0500%, P segregates at the grain boundaries of the weld metal, impairing the toughness of the weld metal. Therefore, the P content of the weld metal is set to 0.0500% or less. From the viewpoint of the characteristics of the welded joint, the smaller the P content, the more preferable it is. Therefore, no lower limit value for the P content is set. The lower limit value for the P content may be set to 0%. However, in consideration of the manufacturing cost of the welded joint, it is acceptable for the weld metal to contain P within the above-mentioned range. The P content of the weld metal may be 0.0010% or more, 0.0050% or more, or 0.0100% or more. The P content of the weld metal may be 0.0400% or less, 0.0300% or less, or 0.0200% or less.
[0022] (S:0.0100% or less) S is an impurity. If the S content of the weld metal exceeds 0.0100%, S segregates at the grain boundaries of the weld metal, impairing the toughness of the weld metal. Therefore, the S content of the weld metal is set to 0.0100% or less. From the viewpoint of the characteristics of the welded joint, the smaller the S content, the more preferable. Therefore, no lower limit of the S content is set. The lower limit of the S content may be set to 0%. However, in consideration of the manufacturing cost of the welded joint, it is acceptable for the weld metal to contain S within the above-mentioned range. The S content of the weld metal may be 0.0010% or more, 0.0020% or more, or 0.0030% or more. The S content of the weld metal may be 0.0080% or less, 0.0070% or less, or 0.0050% or less.
[0023] (Ti: 0.020~0.120%) Ti has the effect of deoxidizing the weld metal and refining the structure of the weld metal. In addition, Ti forms conductive slag that does not impair the electrodeposition paintability. Therefore, by modifying the components of the slag using Ti, the electrodeposition paintability of the welded joint can be improved. If the Ti content of the weld metal is less than 0.020%, these effects cannot be obtained. On the other hand, if the Ti content of the weld metal exceeds 0.120%, coarse precipitates are generated in the weld metal, and the toughness of the weld metal is impaired. Therefore, the Ti content of the weld metal is set to 0.020 to 0.120%. The Ti content of the weld metal may be 0.030% or more, 0.040% or more, or 0.050% or more. The Ti content of the weld metal may be 0.110% or less, 0.100% or less, or 0.080% or less.
[0024] (Zr: 0.001~0.050%) Zr precipitates as fine nitrides in the weld metal and has the effect of improving the strength of the weld metal. Zr also forms conductive slag that does not impair the electrodeposition paintability. Therefore, by modifying the components of the slag using Zr, the electrodeposition paintability of the welded joint can be improved. If the Zr content of the weld metal is less than 0.001%, these effects cannot be obtained. On the other hand, if the Zr content of the weld metal exceeds 0.050%, coarse precipitates are generated in the weld metal, impairing the toughness of the weld metal. Therefore, the Zr content of the weld metal is set to 0.001 to 0.050%. The Zr content of the weld metal may be 0.002% or more, 0.010% or more, or 0.015% or more. The Zr content of the weld metal may be 0.040% or less, 0.035% or less, or 0.030% or less.
[0025] (balance: iron and impurities) The balance of the chemical composition of the weld metal includes iron and impurities. The impurities refer to components that are mixed in, for example, from raw materials such as ores or scraps, or various factors in the manufacturing process when industrially manufacturing steel materials, and are permissible within a range that does not adversely affect the welded joint according to the present embodiment. An example of an impurity other than the above-mentioned P and S is O and N. O and N are elements that are mixed into the weld metal from the atmosphere during welding. For example, by adjusting the welding environment so that the O content is 0.0500% or less and the N content is 0.0300% or less, the toughness of the weld metal is further improved.
[0026] Furthermore, the weld metal may contain, for example, one or more of the optional elements listed below in place of a portion of the remaining iron. However, even if the optional elements listed below are not contained in the weld metal, the welded joint according to this embodiment can solve the problem. Therefore, the lower limit of the content of each of the optional elements listed below is 0%.
[0027] (Al: preferably 0.12% or less) Al has the effect of deoxidizing the weld metal. Therefore, Al may be contained in the weld metal. Furthermore, by making the Al content of the weld metal 0.12% or less, it is possible to prevent an excessive amount of alumina-based oxide from precipitating in the weld metal, and the toughness of the weld metal can be further improved.
[0028] (Ni: preferably 3.00% or less) Ni has the effect of improving the low temperature toughness of the weld metal. Therefore, Ni may be contained in the weld metal. In addition, setting the Ni content of the weld metal to 3.00% or less reduces the cost of the alloy and is economically advantageous.
[0029] (Cr: preferably 1.20% or less) Cr is an element that improves the hardenability of the weld metal. Therefore, the weld metal may contain Cr. In addition, keeping the Cr content of the weld metal at 1.20% or less reduces the cost of the alloy and is economically advantageous. Furthermore, keeping the Cr content of the weld metal at 1.20% or less can further improve the toughness of the weld metal.
[0030] (Mo: preferably 1.00% or less) Mo is an element that improves the hardenability of the weld metal. Therefore, Mo may be contained in the weld metal. Furthermore, keeping the Mo content of the weld metal at 1.00% or less reduces the cost of the alloy and is economically advantageous. Furthermore, keeping the Mo content of the weld metal at 1.00% or less can further improve the toughness of the weld metal.
[0031] (V: preferably 0.30% or less) V is an element that improves the hardenability of the weld metal. Therefore, the weld metal may contain V. In addition, keeping the V content of the weld metal at 0.30% or less reduces the cost of the alloy and is economically advantageous. Furthermore, keeping the V content of the weld metal at 0.30% or less can further improve the toughness of the weld metal.
[0032] (Nb: preferably 0.10% or less) A small amount of Nb forms carbonitrides in the weld metal, which contributes to refining the structure of the weld metal and improving its strength. Therefore, Nb may be contained in the weld metal. In addition, by making the Nb content of the weld metal 0.10% or less, the toughness of the weld metal can be further improved.
[0033] (B: preferably 0.0600% or less) Even a small amount of B improves the hardenability of the weld metal. Therefore, the weld metal may contain B. Furthermore, by setting the B content of the weld metal to 0.0600% or less, the toughness of the weld metal can be further improved.
[0034] (Mg: preferably 0.01% or less) Mg has the effect of deoxidizing the weld metal, so the weld metal may contain Mg. Furthermore, if the Mg content of the weld metal is 0.01% or less, the toughness of the weld metal can be further improved.
[0035] (Cu: preferably 1.00% or less) When the surface of the welding wire, which is the material of the weld metal, is plated with Cu, the welding workability is improved. Cu also has the effect of improving the hardenability of the weld metal. Therefore, Cu may be contained in the weld metal. Furthermore, when the Cu content of the weld metal is set to 1.00% or less, the toughness of the weld metal can be further improved.
[0036] The chemical composition of the weld metal can be determined by taking a sample from the weld metal and performing a chemical analysis on it. It can also be determined by performing a QV (countback) analysis on the weld metal. In either case, it is important not to include the base steel plate in the analysis.
[0037] (Weld metal Ceq: 0.450-0.950 mass%) Ceq is called carbon equivalent and is a value obtained by converting the chemical components contained in the steel material into the amount of carbon. In the welded joint according to the present embodiment, Ceq is a value calculated by the following formula 1 or formula 5 indicated by the Japan Welding Society (WES). Ceq=C+Mn / 6+Si / 24: Equation 1 Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 4: Formula 5 Here, the element symbols included in formula 1 or formula 5 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal. When the chemical composition of the weld metal does not include the optional elements described above, Ceq is calculated using formula 1, and when the chemical composition of the weld metal includes the optional elements described above, Ceq is calculated using formula 5.
[0038] If the Ceq of the weld metal is less than 0.450%, the strength of the weld metal is insufficient. On the other hand, if the Ceq of the weld metal exceeds 0.950%, the toughness of the weld metal is impaired. Therefore, the Ceq of the weld metal is set to 0.450 to 0.950%. The Ceq of the weld metal may be 0.500% or more, 0.550% or more, or 0.600% or more. The Ceq of the weld metal may be 0.900% or less, 0.850% or less, or 0.800% or less.
[0039] (Vickers hardness of weld metal: 300HV or more) The greater the hardness of the weld metal, the higher the fatigue strength of the welded joint. According to the results of the study by the present inventors, when the Vickers hardness of the weld metal is set to 300HV or more, sufficient fatigue strength for, for example, an automobile component can be ensured. Therefore, the Vickers hardness of the weld metal is set to 300HV or more. The Vickers hardness of the weld metal may be set to 320HV or more, 350HV or more, or 380HV or more.
[0040] The Vickers hardness of the weld metal is obtained by measuring the hardness of the weld metal in a cross section perpendicular to the weld line. Vickers hardness measurements are performed on 10 or more random points inside the weld metal in the cross section perpendicular to the weld line with a load of 0.2 kN or more, and the average of the measurements is regarded as the hardness of the weld metal. The inside of the weld metal refers to the region (the region surrounded by the dashed line in Figure 2) that is 0.1 mm or more away from the outer edge of the weld metal in the cross section perpendicular to the weld line (i.e., the surface of the weld metal and the fusion boundary, which is the boundary between the weld metal and the steel plate).
[0041] (Thickness of at least one of the two or more steel plates: 0.8mm to 4.0mm) Next, the steel plates will be described. One or both of the two or more steel plates that are the base materials of the welded joint are thin plates that are suitable as materials for automobile parts, for example. Specifically, the plate thickness of one or both of the two or more steel plates is 0.8 mm or more and 4.0 mm or less. This makes it easy to apply the welded joint according to this embodiment to automobile parts.
[0042] In general, the greater the thickness of the base metal, the smaller the effect of the weld metal structure on fatigue strength. This is because the greater the thickness of the base metal, the greater the tensile residual stress introduced into the weld after welding. There is a correlation between the tensile residual stress of the weld and fatigue strength, and the greater the tensile residual stress, the lower the fatigue properties tend to be. In contrast, for steel plates in the above-mentioned thickness range, the fatigue properties can be ensured by optimizing the composition and hardness of the weld metal. In a welded joint consisting of two or more thick plates, the residual stress of the weld metal that affects the fatigue properties is dominant, and the composition of the weld metal has almost no effect on the fatigue properties. Therefore, it is not expected that the above-mentioned configuration will be adopted for the weld metal of thick plates in order to improve the fatigue properties.
[0043] As long as one of the two or more steel plates is a thin plate having a thickness of 0.8 mm or more and 4.0 mm or less, the thickness of the other is not limited. One or more of the two or more steel plates may have a thickness of 3.8 mm or less, 3.6 mm or less, or 3.2 mm. One or more of the two or more steel plates may have a thickness of 1.2 mm or more, 1.5 mm or more, or 1.6 mm or more.
[0044] (Si content of slag attached to welded joint: 5.0 mass% or less) Next, the slag attached to the welded joint will be described. The Si in the slag reduces the electrical conductivity of the slag. Slag with low electrical conductivity causes poor electrodeposition coating. Therefore, in order to further improve the electrodeposition coating properties, it is effective to reduce the Si content of the slag attached to the surface of the weld metal. Specifically, by setting the Si content of the slag attached to the welded joint to 5.0 mass% or less, the electrodeposition coating properties required for the welded joint can be ensured. The Si content of the slag attached to the welded joint may be 4.8 mass% or less, 4.5 mass% or less, or 4.0 mass% or less.
[0045] The method for measuring the Si content of the slag attached to the welded joint is as follows. At the location where the slag is attached, the welded joint is cut perpendicular to the weld line of the weld metal. Before cutting, a treatment is performed to prevent the slag from falling off, such as a treatment to cover the slag with resin. Next, the chemical composition of the slag is analyzed on the cross section using an EDS or WDS attached to a scanning electron microscope. The observation magnification is 500 to 1000 times. The analysis is performed at three locations in the slag, and the median of the obtained measurement results is regarded as the chemical composition of the slag.
[0046] In addition, when calculating the Si content of the slag, the measured value of the mass of oxygen is excluded. That is, the measured value of the Si content divided by the sum of the measured values of the contents of the components excluding oxygen is regarded as the above-mentioned Si content of the slag. For example, if the analysis results of the slag are O: 50 mass%, Fe: 40 mass%, and Si: 10 mass%, the Si content of the slag is regarded as 20 mass% (= 10 / (100-50)). This is because the measurement values of light elements such as O have a large error in X-ray analysis such as EDS. In the welded joint according to this embodiment, the Si content of the slag is the ratio of the mass of Si to the mass of the slag excluding oxygen.
[0047] (Si content in unit mass% of weld metalSi WM and the largest value of the Si content in unit mass% of two or more steel plates. BM (Relationship with: Satisfying Equation 2) Next, the relationship between the chemical components of the weld metal and the chemical components of the steel plate will be described. In the weld joint according to this embodiment, the Si content Si in the weld metal in unit mass% measured by the above-mentioned means is WM and the largest value of the Si content in unit mass% of two or more steel plates. BM satisfies the following formula 2. 2.5×{(Si WM / 0.89)-0.6×Si BM}≦0.510: Formula 2 During welding (particularly during arc welding), the base material, the steel plate, is also heated by heat conduction from the molten pool. As a result, oxide scale forms on the surface of the heat-affected zone of the steel plate. Furthermore, welding fumes generated by welding also adhere to the heat-affected zone of the steel plate. These can deteriorate the electrodeposition paintability. On the other hand, according to the findings of the present inventors, it has been found that the electrodeposition paintability of the heat-affected zone of the steel plate can be improved by selecting the components of the steel plate and welding material so as to satisfy formula 2. It should be noted that 2.5×{(Si WM / 0.89)-0.6×Si BM} may be 0.500 or less, 0.400 or less, 0.300 or less, or 0.200 or less. BM is determined by the same method as that for measuring the chemical composition of weld metal. BM The Ti content can be determined by taking a sample from the steel plate and conducting a chemical analysis of it. The chemical composition of the steel plate can also be determined by conducting a QV (countback) analysis of the steel plate. BM Also, Si BM can be found in the same way.
[0048] As long as the above-mentioned requirements are satisfied, the welded joint according to this embodiment can adopt various configurations according to its application. On the other hand, by adopting the configurations exemplified below, the properties of the welded joint according to this embodiment can be further improved.
[0049] (Toe angle β at one or more toes of the weld metal: preferably more than 0° and less than 30°) It is preferable to make the shape of one or more toes of the weld metal smooth. The toe is the point where the surface of the base metal and the surface of the weld bead intersect (JIS Z 3001-7:2018), and the toe is the toe and its surrounding area. By making the shape of the toe smooth, it is possible to alleviate the stress concentration at the toe and further improve the fatigue strength. The toe angle β is the included angle between the toe of the weld metal and the surface of the weld metal 0.3 mm away from the toe and the surface of the steel plate. The toe angle is generally 0° to 60°, but the weld metal of the welded joint according to this embodiment may have one or more toes that satisfy the following conditional expression. 0°<β<30° By satisfying the above conditional expression, the toe of the weld metal has a gentle shape, and therefore it is possible to further suppress the concentration of stress at the toe of the weld metal. The toe angle β may be 28° or less, 25° or less, or 20° or less. The toe angle β may be 12° or more, 14° or more, or 18° or more.
[0050] The method for measuring the toe angle β is as follows when the welded joint is a lap fillet welded joint. For convenience, of the two steel plates in the lap fillet welded joint, the steel plate whose surface (plate face) is joined by the weld metal is called the first steel plate 1, and the steel plate whose end face is joined by the weld metal is called the second steel plate 2. As shown in FIG. 1, if the position of the fusion boundary existing on the surface 1a of the first steel plate 1 is Point A, the weld metal 3 rises from Point A with a toe angle β. The weld metal 3 also rises from a position further from Point A toward the second steel plate 2 with a flank angle θ. The flank angle θ is generally used as a parameter representing the shape of the toe of the weld metal 3, but in this embodiment, the toe angle β is used as a parameter representing the shape of the toe of the weld metal 3. Explaining with reference to FIG. 1, the toe angle β of the weld metal is a value defined as follows when viewed in a cross section perpendicular to the weld line of the weld metal. Point A: fusion boundary present on surface 1a of first steel plate 1 Point C: A position 0.3 mm away from point A toward the inside of the weld metal 3 in the X direction parallel to the surface 1a of the first steel plate 1. Point B: an intersection point between a line passing through point C and extending in the thickness direction of the first steel plate 1 and the surface 3a of the weld metal 3. - Toe angle of weld metal β: The angle between the line connecting points A and B and the line connecting points A and C
[0051] As mentioned above, the fusion boundary means the boundary between the weld metal and the steel plate. The fusion boundary can be easily confirmed by corroding the cross section of the welded joint by a known method. By identifying points A, B, and C on the cross section where the fusion boundary is revealed, the toe angle β can be measured.
[0052] In addition, in FIG. 1, for convenience of explanation, the surface 1a of the first steel plate 1 and the end surface 2a of the second steel plate 2 included in the weld metal 3 are shown by dotted lines to indicate the position of the corner 4. However, in reality, the dotted line portion is melted into the weld metal 3. Therefore, even if a cross-sectional photograph of the weld metal 3 is obtained using an optical microscope, the dotted line portion cannot be observed. Therefore, by identifying the three points A, B, and C defined as above on the cross-sectional photograph of the weld metal 3, the toe angle β of the weld metal 3 can be easily obtained from the cross-sectional photograph of the weld metal 3. Note that the toe angle β may be measured using not only an optical microscope but also a scanning electron microscope (SEM) or a microscope, etc., as long as a photograph capable of identifying the toe angle β of the weld metal 3 can be obtained.
[0053] In a lap fillet weld joint, it is preferable that 0°<β<30° is satisfied at least at the toe on the side of the first steel plate 1. On the other hand, the toe angle β can also be specified by the above-mentioned method at the toe on the side of the second steel plate 2, and 0°<β<30° may be satisfied at either or both of the toe on the side of the first steel plate 1 and the toe on the side of the second steel plate 2.
[0054] The method for measuring the toe angle β has been described above using a lap fillet welded joint as an example, but the measurement can be performed in the same manner for other shapes of welded joints such as T-joints and butt joints. As described above, in the welded joint according to this embodiment, it is preferable to make the shape of one or more toes smooth. When the weld metal has two or more toes, it is preferable to smooth at least the toes at which fatigue cracks may occur. An example of a toe at which fatigue cracks may occur is a toe at which stress is likely to concentrate due to the structure of the member. In a lap fillet welded joint, for example, the point where the surface of the lower plate and the surface of the weld bead intersect (the toe on the lower plate side) becomes the toe where fatigue cracks may occur. In the case of a T-joint (a joint in which the end face of one plate is placed on the surface of another plate, forming a T-shape at an almost right angle), for example, the toe on the main plate side (stress transmission side) is the toe at which fatigue cracks are likely to occur. Note that in a T-joint, fatigue cracks are most likely to occur in the toe on the main plate side (stress transmission side), the toe on the side with the shorter weld leg length, and the toe on the side with the smaller throat thickness, in that order. Also, when the thicknesses of the steel base materials are different, fatigue cracks are more likely to occur at the toe on the base material side with the thinner plate thickness. In the case of a butt joint (a joint in which parts placed on the same plane face each other at an angle of 135°≦α≦180°) where the thicknesses of the steel base materials are different, fatigue cracks are likely to initiate from the toe of the thinner steel plate. Taking the above into consideration, it is possible to smooth the shape of only the toes of the welded joint where there is a risk of fatigue cracks occurring, as described above, or it is possible to smooth the shape of all the toes of the welded joint.
[0055] (Ti content in unit mass% of weld metal Ti WM and the largest Ti content in unit mass% of two or more steel plates. BM The relationship between the above and the formula (3) is preferably satisfied. In the welded joint according to this embodiment, the Ti content Ti in unit mass% of the weld metal measured by the above-mentioned means WM and the largest Ti content in unit mass% of two or more steel plates. BM and the relationship may satisfy Equation 3. 0.050≦2.5×{(Ti WM / 0.54)-0.6×Ti BM}≦0.300: Formula 3 In the weld metal, alloying elements are distributed almost evenly. However, the components of the weld metal near the toe tend to be easily influenced by the components of the base metal. The amount of Ti near the toe of the weld metal contributes to refining the structure of the weld metal. The amount of Ti near the toe of the weld metal also improves the electrical conductivity of the slag generated near the toe, improving the electrodeposition paintability of the welded joint. Since slag tends to adhere easily to the toe, modifying the slag components at the toe is particularly effective for improving the electrodeposition paintability. Ti WM and Ti BM By satisfying formula 3, the Ti content in the weld metal near the toe can be controlled favorably, and the above-mentioned effects can be obtained. WM / 0.54)-0.6×Ti BM 2.5×{(Ti WM / 0.54)-0.6×Ti BM} may be 0.080 or more, 0.100 or more, or 0.150 or more. WM is a value measured at a position sufficiently distant from the base metal (for example, at a position perpendicular to the weld line of the weld metal and distant from the fusion boundary by 0.1 mm or more).
[0056] (Vickers hardness of weld metal: preferably 80% or more of HM) In the welded joint according to this embodiment, the Vickers hardness of the weld metal measured by the above-mentioned means may be 80% or more of HM. HM is calculated by the following formula 4. HM = 884 × C × (1-0.3 × C 2 )+294:Expression 4 Here, the element symbols included in formula 4 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal.
[0057] The value HM calculated by the formula 4 is a value called 100% martensite hardness, which is an estimate of the hardness when the steel is quenched so that the entire structure becomes martensite (i.e., when the maximum quench hardening is caused). The higher the ratio of the actual hardness to HM, the greater the amount of martensite and the smaller the amount of soft structures such as ferrite that can become the starting points of fatigue cracks. Therefore, the higher the ratio of the actual hardness to HM, the fewer the starting points of fatigue cracks and the more improved the fatigue properties. For the above reasons, it is preferable that the Vickers hardness of the weld metal is 80% or more of the HM of the weld metal. The Vickers hardness of the weld metal may be 83% or more, 85% or more, or 90% or more of the HM of the weld metal. Note that the HM of the weld metal is an estimate of the hardness when the maximum quench hardening is caused in the weld metal, so the hardness of the weld metal actually measured may exceed the HM.
[0058] (Total of Ti content and Zr content of slag: preferably 0.5 mass% or more) In the welded joint according to the present embodiment, the total of the Ti and Zr contents of the slag may be 0.5% by mass or more. As described above, Ti and Zr have the function of increasing the electrical conductivity of the slag and suppressing the occurrence of electrodeposition coating defects caused by the slag. Therefore, the higher the Ti and Zr contents in the slag, the better the electrodeposition coating properties. The total of the Ti and Zr contents of the slag may be 0.6% by mass or more, 0.8% by mass or more, or 1.0% by mass or more. Here, the Ti and Zr contents of the slag are values measured by the same means as the Si content of the slag. In the welded joint according to the present embodiment, the Ti and Zr contents of the slag are the ratios of the mass of Ti and Zr to the mass of the slag excluding oxygen.
[0059] In addition to or instead of specifying the total Ti and Zr contents of the slag, the Ti and Zr contents of the slag may be specified individually. For example, the Ti content of the slag may be 0.4 mass% or more, 0.5 mass% or more, or 0.6 mass% or more. The Zr content of the slag may be 0.1 mass% or more, 0.2 mass% or more, or 0.3 mass% or more.
[0060] Next, a method for manufacturing a welded joint according to the present embodiment will be described. The method for manufacturing a welded joint according to the present embodiment includes a step of welding two or more steel plates together using a filler metal. The type of welding is not particularly limited, but it is preferable to use, for example, arc welding, particularly gas-shielded arc welding.
[0061] The chemical composition and Ceq of the weld metal, as well as the chemical composition of the slag, are determined according to the chemical composition of the steel plate to be welded, the chemical composition of the filler metal, and the transfer rate of the alloying elements. For example, elements such as Si, Ti, and Al, which tend to form oxides during welding, are partly discharged as slag out of the weld metal. On the other hand, elements that do not easily form oxides tend to remain in the weld metal. Therefore, the chemical composition of the steel plate and the chemical composition of the filler metal do not match the chemical composition of the weld metal. However, by appropriately selecting the components of the steel plate and the filler metal while taking into account the properties of each alloying element, the chemical composition and Ceq of the weld metal, as well as the chemical composition of the slag, can be set within the above-mentioned ranges.
[0062] The Vickers hardness of the weld metal is determined by the chemical composition and material structure of the weld metal. The hardenability of the weld metal depends on the Ceq of the weld metal, and the hardness of the martensitic structure depends on the C content. Therefore, by setting the Ceq of the weld metal in the appropriate range described above, the weld metal formed by welding can have a martensitic structure, and the Vickers hardness of the weld metal and the ratio of the Vickers hardness to the HM of the weld metal can be set within the above-mentioned range. By optimizing the welding conditions in this case, the toe angle at one or more toes of the weld metal can be made to be more than 0° and less than 30°.
[0063] The toe angle of the weld metal is affected by various welding conditions. For example, when the type of welding is arc welding, the higher the voltage, the wider the arc becomes, and the smaller the toe angle becomes. Also, when the welding is fillet welding, the toe angle tends to become smaller as the welding target position moves away from the corner. Here, the welding target position refers to the intersection point between the central axis of the welding torch and the surface of the lower plate. The lower plate refers to the plate whose surface is mainly welded. In the case of a lap weld joint as exemplified in Figure 1, the first steel plate 1 corresponds to the lower plate. In the case of a T-joint, the plate whose end is welded corresponds to the upper plate, and the plate against which the upper plate is butted corresponds to the lower plate.
[0064] The toe angle of the weld metal is also affected by the welding position. The molten metal drips due to gravity. Therefore, the angle of the steel plates during welding may be set so that dripping occurs that reduces the toe angle. For example, in the case of a lap weld joint as shown in FIG. 1, the toe angle of the toe on the side of the first steel plate 1 can be reduced by welding in an upright position of the first steel plate 1 and the second steel plate 2 so that the end surface 2a of the second steel plate 2 is on top.
[0065] However, if the arc is widened too much to reduce the toe angle, undercut occurs at the toe, and a sound weld joint cannot be obtained. Extreme welding positions may also have a negative effect on the overall shape of the weld metal. It is desirable to optimize the welding conditions under the above guidelines, taking into consideration the type of weld joint, the material of the steel plate, the thickness of the steel plate, and the type and material of the filler metal.
[0066] Next, an automobile component according to another aspect of the present invention will be described. The automobile component according to another aspect of the present invention has the above-mentioned welded joint according to the present embodiment. As a result, the automobile component according to the present embodiment has reduced electrodeposition coating defects and has better fatigue properties. The type of automobile component is not particularly limited, but the automobile component may be, for example, a front lower arm or a subframe. EXAMPLES
[0067] Example 1 The effects of one embodiment of the present invention will be explained more specifically with reference to an example. However, the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0068] Two steel plates having the thickness and chemical composition shown in Table 1 were overlapped and lap fillet welded. The remainder of the chemical composition of these steel plates was iron and impurities. In all examples, the two steel plates were the same type, and the specific welding conditions were as follows. In the following description, t means the thickness of one steel plate. Overlap: 10mm Welding current: DC pulse mode, 81×t(A) Welding speed: 0.8m / min Shielding gas type: Ar+20%CO 2
[0069] For various welded joints obtained by the above method, the chemical composition of the weld metal, the Vickers hardness of the weld metal, the toe angle β, the Si content of the slag, the Ti content of the slag, and the total value of the Zr content of the slag were measured. The measurement methods were as described above. The balance of the chemical composition of the weld metal was Fe and impurities. As for Mg, most of it was discharged as slag and the amount of Mg detected in the weld metal was less than 0.0003%. In addition, the toe angle β of all the welded joints was less than 30°. Furthermore, the fatigue properties and electrodeposition paintability of various welded joints obtained by the above-mentioned method were evaluated.
[0070] The fatigue property evaluation was carried out using the following procedure. Test pieces 20 mm wide were taken from the welded joint in the weld line direction. They were taken from locations where the weld bead was stable, and the start and end of the weld bead were not evaluated. Next, a plane bending fatigue test was carried out on the test pieces. The loading conditions were reverse displacement control with a stress ratio of -1. The fracture condition was the point at which the bending moment acting on the test piece fell to 1 N·m or less. Fatigue limit σW is 10 7 The stress amplitude (MPa) at the time when the specimen did not break was used. The standard stress was the maximum bending stress without considering the stress concentration at the weld toe at the center of the specimen. The maximum bending stress mentioned above, calculated from the bending moment M (N mm), specimen width h (mm), and plate thickness t (mm), was 6×M / (h×t 2 ) (MPa).
[0071] The pass / fail criteria for fatigue properties are as follows. The fatigue limit in bending load is affected by plate thickness. Therefore, taking into account the plate thickness effect, the fatigue limit σ that satisfies the relationship of the following formula A is set. W Welded joints that achieved a fatigue limit of 0.05% (MPa) were judged to have a good fatigue limit and were rated for fatigue properties as "△". Furthermore, welded joints that satisfied the relationship in formula B below were judged to have an even better fatigue limit and were rated as "O". Welded joints that did not satisfy the relationship in formula A below were judged not to have a good fatigue limit and were rated as "X". Welded joints that at least satisfied the relationship in formula A below were judged to pass with respect to fatigue properties. σ W ≧191+55.35 / t: Formula A σ W ≧200+57.99 / t: Formula B
[0072] The electrodeposition coating evaluation was carried out in the following manner. First, the welded joint was degreased and chemically treated. Next, the welded joint was electrocoated so that the film thickness was 20 μm. Then, the welded bead part after electrocoating was photographed, and the photograph was image-analyzed to measure the ratio of the area of the electrocoated defective part to the area of the welded bead, and this ratio was defined as the coating defective area rate. The length of the welded bead was 120 mm. The above-mentioned measurement was carried out for a 90 mm long area of the welded bead, excluding the weld start end (the area from the end of the welded bead on the welding start side to 15 mm) and the weld end end (the area from the end of the welded bead on the welding end side to 15 mm). A gray paint was used for the electrocoating. Since yellowish brown slag is exposed in the electrocoated defective part, the electrocoated defective part can be easily identified by electrocoating using a gray paint.
[0073] The pass / fail criteria for electrodeposition paintability were as follows: Welded joints with a paint defect area rate of 10% or less were judged to be welded joints with excellent electrodeposition paintability and were rated as "△". Welded joints with a paint defect area rate of 5% or less were judged to be welded joints with particularly excellent electrodeposition paintability and were rated as "〇". Welded joints with a paint defect area rate of more than 10% were rated as "×". Welded joints rated as "△" or "〇" were judged to pass the electrodeposition paintability.
[0074] The above-mentioned various evaluation results are shown in Table 2 and onwards. In the tables, values outside the range of the invention are underlined. In addition, for components that were not detected, the content is indicated with "-" in the tables.
[0075] [Table 1]
[0076] [Table 2]
[0077] [Table 3]
[0078] [Table 4]
[0079] [Table 5]
[0080] In addition, in the table, "H WM " indicates the Vickers hardness of the weld metal, and "base metal Si" is 2.5 × {(Si WM / 0.89)-0.6×Si BM}, and "base metal Ti" is 2.5 × {(Ti WM / 0.54)-0.6×Ti BM}, "slag Si%" indicates the Si content of the slag, and "slag Ti+Zr%" indicates the sum of the Ti content and Zr content of the slag.
[0081] The joints in which the composition of the weld metal, the Ceq of the weld metal, the Vickers hardness (molten metal HV) of the weld metal, the toe angle, the Si content of the slag, and the relationship between the Si content of the base metal and the Si content of the weld metal (molten metal Si in the base metal) were within the ranges of the invention were excellent in both fatigue properties and electrocoatability. On the other hand, the comparative examples in which one or more of these were outside the ranges of the invention were inferior in either or both of the fatigue properties and electrocoatability.
[0082] In the welded joint No. 4, the Ti content of the weld metal, the Ceq of the weld metal, and the Vickers hardness of the weld metal were insufficient. Therefore, the fatigue properties of the welded joint No. 4 were insufficient. The Ti content of the weld metal of welded joint No. 5 was insufficient. As a result, the fatigue properties of welded joint No. 5 were insufficient. In weld joint No. 10, the slag had an excessive Si content (see "Slag Si%"), and WM and Si BM did not satisfy formula 2 (see "Base metal molten silicon"). Therefore, the electrodeposition paintability of welded joint No. 10 was insufficient. The weld metal of welded joint No. 12 contained excessive Mn, which resulted in insufficient fatigue properties. The weld metal Ceq and Vickers hardness of the weld metal were insufficient in the weld joint No. 14. Therefore, the fatigue properties of the weld joint No. 14 were insufficient. The Ti content of the weld metal of welded joint No. 17 was insufficient. As a result, the fatigue properties of welded joint No. 17 were insufficient. In the welded joint No. 19, the C content, V content, and Ceq of the welded metal were excessive. Therefore, the fatigue properties of the welded joint No. 19 were insufficient. The Mn content of the weld metal of welded joint No. 20 was insufficient. As a result, the fatigue properties of welded joint No. 20 were insufficient. In weld joint No. 22, Si WMand Si BM did not satisfy formula 2 (see "Base metal molten silicon"). Therefore, the electrodeposition paintability of welded joint No. 22 was insufficient. The Zr content of the weld metal of weld joint No. 23 was insufficient. As a result, the fatigue properties of weld joint No. 23 were insufficient. In the welded joint No. 26, the Ti content of the weld metal, the Ceq of the weld metal, and the Vickers hardness of the weld metal were insufficient. Therefore, the fatigue properties of the welded joint No. 26 were insufficient.
[0083] Example 2 In order to evaluate the effect of the toe shape, the following experiment was carried out. Two steel plates A shown in Table 1 were overlapped and lap fillet welded. The welding wire, overlap, welding speed, and shielding gas type used in the lap fillet welding were the same as those for joint 1 in Table 2. Other welding conditions were as shown in Table 6. The numerical value in the "welding target position" column in Table 6 is the distance between the above-mentioned welding target position and the end face of the upper plate (second steel plate). As shown in FIG. 3, the closer the welding target position is to the upper plate (second steel plate), the larger the numerical value in the "welding target position" column in Table 6. When the welding target position is located at a position that does not overlap with the lower surface of the upper plate (second steel plate), a negative value is listed in the "welding target position" column in Table 6. For various welded joints obtained by the above procedure, the toe angle β was measured and fatigue properties were evaluated in the same manner as in Example 1, and the results are shown in Table 6. In the welded joints No. 3 to 6, fatigue cracks initiated from the weld metal surface, and the fatigue strength was further improved.
[0084] [Table 6] [Explanation of symbols]
[0085] 1 1st steel plate 1a Surface of the first steel plate 2 Second steel plate 2a End face of second steel plate 3. Weld metal 3a Surface of weld metal 4 Corners 10 Welded joints A: Melt boundary on the surface of the first steel plate The intersection point between a line passing through point BC and extending in the thickness direction of the first steel plate and the surface of the weld metal C: In the X direction parallel to the surface of the first steel plate, a position 0.3 mm away from point A toward the inside of the weld metal θ Flank angle β toe angle
Claims
1. Two or more steel plates; A weld metal that joins two or more of the steel plates; A welded joint comprising: The chemical composition of the weld metal is, in mass%, C: 0.01-0.25%, Si: 0.01-1.00%, Mn: 0.80-2.50%, P: 0.0500% or less, S: 0.0100% or less, Ti: 0.020 to 0.120%, and Zr: 0.001-0.050% and the remainder being iron and impurities, The Ceq of the weld metal calculated by the following formula 1 is 0.450 to 0.950 mass%, The Vickers hardness of the weld metal is 300 HV or more, One or more of the two or more steel plates have a plate thickness of 0.8 mm or more and 4.0 mm or less; The Si content of the slag adhered to the weld joint is 5.0 mass% or less, The Si content in the weld metal in unit mass% Si WM and the largest value Si among the Si contents in unit mass% of two or more of the steel plates. BM and satisfies the following formula 2 Welded joint. Ceq=C+Mn / 6+Si / 24: Formula 1 2.5 × { (Si WM / 0.89) - 0.6 × Si BM} ≤ 0.510: Formula 2 Here, the element symbols included in the formula 1 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal.
2. The Ti content in the weld metal in unit mass% Ti WM and the largest value Ti among the Ti contents in unit mass% of two or more of the steel plates. BM and satisfies the following formula 3. The welded joint according to claim 1 . 0.050 ≤ 2.5 × { (Ti WM / 0.54) - 0.6 × Ti BM} ≤ 0.300: Formula 3
3. The Vickers hardness of the weld metal is 80% or more of HM calculated by the following formula 4.
3. The welded joint according to claim 1 or 2. HM=884×C×(1-0.3×C 2 )+294:Formula 4 Here, the element symbols included in the formula 4 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal.
4. The total of the Ti content and the Zr content of the slag is 0.5 mass% or more. The welded joint according to any one of claims 1 to 3.
5. The toe angle at one or more toes of the weld metal is greater than 0° and less than 30°. The welded joint according to any one of claims 1 to 4.
6. The two or more steel plates are a first steel plate and a second steel plate which are overlapped with each other, The weld metal joins a surface of the first steel plate and an end surface of the second steel plate, The toe angle of the weld metal at the toe on the first steel plate side is more than 0° and less than 30°. The welded joint according to claim 5.
7. The chemical composition of the weld metal is, in mass %, Al: 0.12% or less, Ni: 3.00% or less, Cr: 1.20% or less, Mo: 1.00% or less, V: 0.30% or less, Nb: 0.10% or less, B: 0.0600% or less, Mg: 0.01% or less, Cu: 1.00% or less, O: 0.0500% or less, and N: 0.0300% or less, The Ceq of the weld metal is calculated by the following formula 5. The welded joint according to any one of claims 1 to 6. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 4: Formula 5 Here, the element symbols included in the formula 5 represent the contents, in unit mass %, of the elements corresponding to these element symbols in the chemical composition of the weld metal.
8. An automobile component comprising the welded joint according to any one of claims 1 to 7.
Citation Information
Patent Citations
Lap arc-welded joint structure excellent in fatigue strength
JP1994340947A
Metal based flux cored wire for gas-shielded arc welding
JP2003048096A
Manufacturing method of weld joint having excellent fatigue characteristic
JP2006305630A
Welded joint for fireproof construction having excellent high temperature strength and toughness
JP2007107055A
One-pass large-heat input weld joint having excellent toughness of weld metal, and method for manufacturing the same
JP2010094686A