How to shave steel
By controlling cutting speed and adjusting oxygen parameters, the method ensures stable and uniform cutting of steel surfaces, addressing productivity and irregularity issues in melt cutting.
Patent Information
- Application Number
- JP2021072509
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-22
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-04-22
AI Technical Summary
Existing melt cutting methods for steel materials face challenges in achieving stable and uniform cutting depth with increased productivity, as higher conveyance speeds lead to unstable oxygen supply and irregular cutting surfaces.
A method involving a preheating gas and cutting oxygen ejection system, where the cutting speed is controlled to be at least 0.8 times the calculated limit cutting speed, and oxygen pressure and jet distance are adjusted to maintain stable oxygen supply, ensuring shallow and uniform cutting.
Stable and uniform cutting of steel surfaces is achieved with controlled cutting speed, oxygen pressure, and jet distance, resulting in improved productivity and reduced surface irregularities.
Smart Images

Figure 0007568935000002 
Figure 0007568935000003 
Figure 0007568935000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for laser cutting a steel material by laser cutting the surface of the steel material. [Background technology]
[0002] For example, surface defects such as inclusions and surface scratches may occur on the surface of a steel material such as a slab produced by continuous casting. When removing such surface defects of steel materials, for example, scarifying devices (scarfer equipment) disclosed in Patent Documents 1 to 4 are used. These scarifying devices (scarfer equipment) locally heat and melt the surface of the slab (steel material) to remove surface defects. In the above-mentioned scarifying device (scarfer equipment), a scarfer unit is disposed so as to face the surface of the steel material.
[0003] In a scarifying device (scarfer equipment) configured as described above, first, combustible gas and preheating oxygen are sprayed onto the surface of the steel material to combust the combustible gas, and the heat of combustion melts the surface of the steel material locally to form a pool portion (preheating step). Next, oxygen for slag cutting is supplied to the surface of the steel material while the steel material is being transported, and the slag cutting oxygen and iron are oxidized using the above-mentioned basin as a heat source, and the heat from this oxidation reaction melts the surface of the steel material and removes surface defects (slag cutting step). The area where the oxygen for slag cutting is supplied and where the oxidation reaction with the iron of the steel material occurs is called the hot spot.
[0004] When the above-mentioned cutting device is used to cut steel, the cutting depth of the steel is determined by the oxygen supply rate. To increase the cutting depth, the oxygen supply pressure is increased or the feed speed of the steel is slowed down to increase the amount of oxygen supplied per unit time. In order to improve the productivity of swarf cutting, it is common to increase the feed speed of the steel material. However, as the feed speed is increased, the swarf cutting depth gradually becomes shallower, resulting in localized unswarfed areas.
[0005] To address such problems, for example, Patent Documents 1 and 2 disclose a method of uniformizing the raw-cutting oxygen in the width direction by inserting an orifice or a straightening plate into the oxygen flow path. Moreover, Patent Document 3 discloses a method of setting an angle between the discharge direction of the nozzle and the direction of machining. Furthermore, Patent Document 4 discloses a method of alternately switching the supply oxygen pressure between high and low pressures. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Utility Model Application Publication No. 03-070856 [Patent Document 2] Japanese Patent Application Publication No. 10-272561 [Patent Document 3] Japanese Patent Application Publication No. 07-214302 [Patent Document 4] JP 2010-029911 A Summary of the Invention [Problem to be solved by the invention]
[0007] Recently, in order to improve the productivity of the cutting and the yield rate during the cutting, it is required to perform the cutting with a shallow and uniform depth. However, when the conveying speed of the steel material (screw cutting speed) is increased in order to make the cutting depth shallow, the supply of oxygen to the hot point becomes unstable, making it impossible to perform stable scarification, resulting in fluctuations in the scarification depth in the width direction and the formation of large irregularities on the surface of the steel material after scarification.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a method for laser cutting steel material, which can stably laser cut the surface of the steel material and can perform laser cutting to a shallow and uniform depth. [Means for solving the problem]
[0009] In order to solve the above problems, a method for laser-cutting a steel material according to the present invention is a method for laser-cutting a surface of a steel material using a laser-cutting device for steel material having a preheating gas jetting part for jetting combustible gas and preheating oxygen, and a laser-cutting oxygen jetting part for jetting laser-cutting oxygen, the method comprising: a preheating step of spraying combustible gas and preheating oxygen from the preheating gas jetting part onto the surface of the steel material to combust and form a basin part on the surface of the steel material; and a laser-cutting step of spraying laser-cutting oxygen from the laser-cutting oxygen jetting part onto the surface of the steel material while transporting the steel material, and laser-cutting the surface of the transported steel material by heat of oxidation reaction between the laser-cutting oxygen and iron, and a critical laser-cutting speed V at which the temperature of the steel material at a front part in the laser-cutting proceeding direction of a hot spot formed by an oxidation reaction between the laser-cutting oxygen and the steel material is equal to or higher than a liquid phase generation temperature of the steel material, C is calculated based on the following formula (1), and the cutting speed is 0.8 × V C More than V C It is characterized by performing the shaving within the following ranges: (1) Formula: V C =(-0.0516×T L +92.0)×exp(0.00146×T 0 ) T L : Liquidus temperature of steel (℃) T 0 : Initial temperature of steel material (℃).
[0010] According to the method for cutting steel material having this configuration, in the cutting step, a critical cutting speed V at which the temperature of the steel material in the forward portion of the cutting advance direction of the hot spot formed by the oxidation reaction of the cutting oxygen with the steel material is equal to or higher than the liquid phase generation temperature of the steel material is set. C The cutting speed is then set to the limit cutting speed V C Since the cutting speed is set to the limit of V, the steel can be cut stably. C Since the cutting speed is set to 0.8 times or more, the cutting speed can be secured and the cutting depth can be made shallow and uniform.
[0011] Here, in the method for cutting steel material of the present invention, in the cutting step, the cutting speed is V0 When changing from V to V, the oxygen pressure of the above-mentioned oxygen for cutting is set to P so as to satisfy the following formula (2). 0 It is preferable to change from (2) Formula: V≧V 0 ×(P / P 0 ) 0.5
[0012] In this case, when the cutting speed is changed, the oxygen pressure of the oxygen for cutting is changed so as to satisfy equation (2). Therefore, even if the cutting speed is increased, sufficient oxygen for cutting can be supplied to the vicinity of the hot point, making it possible to perform the cutting stably.
[0013] In the method for cutting steel material according to the present invention, the cutting speed is set to V 0 When V is set to V, the distance from the tip of the oxygen jet for scavenging to the surface of the steel material is set to L so as to satisfy the following formula (3). 0 It is preferable to change from (3) Formula: V≧V 0 ×(L 0 / L) 0.858
[0014] In this case, when the cutting speed is changed, the distance from the tip position of the oxygen jetting part for laser cutting to the surface of the steel is changed so as to satisfy equation (3). Therefore, when the laser cutting speed is increased, the distance from the tip position of the oxygen jetting part for laser cutting to the surface of the steel becomes shorter, which prevents impurities from being mixed into the oxygen for laser cutting from the atmosphere. This enables the oxygen for laser cutting to be supplied to the fire point with a high purity, and enables stable laser cutting. Effect of the Invention
[0015] As described above, according to the present invention, it is possible to provide a method for thermally cutting a steel material, which can stably thermally cut the surface of the steel material, and can perform thermal cutting to a shallow and uniform depth. [Brief description of the drawings]
[0016] [Figure 1]1 is a schematic explanatory diagram of a method for hot cutting a steel material according to an embodiment of the present invention, in which (a) shows a preheating step and (b) shows a hot cutting step. [Diagram 2] 1 is an enlarged explanatory view of a steel material laser cutting device used in a steel material laser cutting method according to an embodiment of the present invention; [Diagram 3] 1 is a graph showing the relationship between the initial temperature of steel and the cutting speed. [Figure 4] 1 is a graph showing the relationship between oxygen concentration and the amount of machining. [Diagram 5] 1 is a graph showing the relationship between the distance from the tip position of the oxygen jetting part for thermal cutting to the surface of the steel material and the amount of thermal cutting. [Figure 6] 1 is a graph showing the results of an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, a method for scarifying a steel material according to an embodiment of the present invention will be described with reference to the accompanying drawings. Note that the present invention is not limited to the following embodiment.
[0018] The steel material laser cutting apparatus 10 used in the steel material laser cutting method of this embodiment has, as shown in Figure 1, a scarfer unit 20 arranged to face the surface of the steel material 1, and a conveying table (not shown) for conveying the steel material 1. 1 and 2, the scarfer unit 20 is provided with a preheating gas ejection section 21 that ejects preheating oxygen 22 and combustible gas 23, and a laser cutting oxygen ejection section 26 that ejects laser cutting oxygen 27. The laser cutting oxygen ejection section 26 is configured to eject shielding gas 28 consisting of combustible gas together with the laser cutting oxygen 27. The steel material 1 is placed on a conveying table and is configured to be conveyed in the direction of arrow X in FIG. As shown in Figures 1(a) and 1(b), the jet of oxygen for melt cutting 27 jetted out from the oxygen for melt cutting jetting section 26 is positioned so as to collide forward in the conveying direction X of the steel material 1 relative to the jets of preheating oxygen 22 and combustible gas 23 jetted out from the preheating gas jetting section 21.
[0019] In the steel material melt-cutting apparatus 10 having the above-mentioned configuration, first, as shown in Fig. 1(a), preheating oxygen 22 and combustible gas 23 are ejected from the preheating gas ejection part 21 of the scarfer unit 20 toward the surface of the steel material 1, and the combustible gas 23 is burned. Then, a part of the surface of the steel material 1 is melted by the heat of the burning combustible gas 23 to form a basin part 3 (preheating process). The length of the well portion 3 formed on the surface of the steel material 1 along the conveying direction X is set to, for example, within a range of about 20 mm to 30 mm.
[0020] Next, the oxygen for cutting 27 is ejected from the oxygen for cutting ejection portion 26 of the scarfer unit 20 toward the surface of the steel material 1, and the steel material 1 on which the basin portion 3 has been formed is transported in the transport direction X. At this time, the shielding gas 28 is ejected together with the oxygen for cutting 27, and the oxygen for cutting 27 is protected by the shielding gas 28. Then, the jet of oxygen for cutting 27 jetted out from the oxygen for cutting jetting section 26 passes through the pool section 3 of the steel material 1 being transported, and using this pool section 3 as a heat source, an oxidation reaction occurs between the oxygen for cutting 27 and the iron, and the heat of this oxidation reaction melts the surface of the steel material 1, thereby laser-cutting the surface of the steel material 1 (screw-cutting process). 1(b) and 2, the rear side of the well 3 in the transport direction X is smelted by the heat of oxidation reaction. The area where oxygen 27 for smelting is supplied and the oxidation reaction with the iron of the steel material 1 occurs becomes a hot spot.
[0021] Here, if the conveying speed of the steel material 1 in the cutting process, i.e., the cutting speed, is increased, the supply of oxygen to the hot point becomes unstable, making it impossible to carry out the cutting stably, and there is a risk that the cutting depth will become uneven in the width direction of the steel material 1. In other words, in the slag cutting process, the limit slag cutting speed V at which oxygen can be stably supplied to the hot point and slag cutting of steel 1 can be stably performed is C There will be a
[0022] In this embodiment, a critical cutting speed V at which the steel temperature in the forward portion of the hot spot in the cutting advance direction becomes equal to or higher than the liquid phase generation temperature of the steel is set in advance. C is calculated based on the following formula (1). (1) Formula: V C =(-0.0516×T L +92.0)×exp(0.00146×T 0 ) Here, T L is the liquidus temperature of steel 1 (℃), and T 0 is the initial temperature (° C.) of the steel material 1. Note that the initial temperature of the steel material 1 is the temperature of the steel material 1 before the preheating process.
[0023] Figure 3 shows the limiting cutting speed V C An example of the calculated liquid phase temperature T L The temperature at which the liquid phase occurs in steel material 1 is 1435℃. L The temperature at which the liquid phase occurs in steel material 1 is 1485℃. L The C line is when the cutting speed is 1535℃. In other words, depending on the type of steel 1 to be cut, the respective limit cutting speed V C is calculated.
[0024] In this embodiment, the cutting speed in the cutting process is 0.8 × V C More than V C The following range is subjected to the laser cutting. The cutting speed in the cutting process is the limit cutting speed V C By setting the cutting speed at 0.8 times or more, the cutting speed can be made sufficiently fast, and the cutting depth can be made shallow and uniform. On the other hand, the cutting speed in the cutting process is set to the limit cutting speed V C By satisfying the following conditions, oxygen can be stably supplied to the hot point, and the steel material can be stably spalled. The cutting speed in the cutting process is the limit cutting speed V C It is more preferable that the cutting speed in the cutting process is 0.85 times or more. C It is more preferable that the amount of the ion exchange resin is 0.95 times or less.
[0025] In this embodiment, the cutting speed is V 0 From V 1 When setting the oxygen pressure for the cutting oxygen, P is set to satisfy the following formula (2). 0 From P 1 It is preferable to change it to (2) Formula: V 1 ≧V 0 ×(P 1 / P 0 ) 0.5
[0026] As shown in Figure 4, the amount of swarf cutting increases as the oxygen concentration at the hot point increases due to the oxygen pressure of the swarf cutting oxygen. Also, the amount of swarf cutting decreases by increasing the swarf cutting speed. Therefore, by controlling the oxygen pressure of the swarf cutting oxygen according to the swarf cutting speed, it is possible to obtain an appropriate amount of swarf cutting and perform swarf cutting stably.
[0027] In this embodiment, the cutting speed is V 0 From V 1 When setting the distance from the tip of the oxygen jetting portion 26 for cutting to the surface of the steel material 1 is set to L so as to satisfy the following formula (3). 0 From L 1 It is preferable to change it to (3) Formula: V 1 ≧V 0 ×(L 0 / L 1 ) 0.858
[0028] As shown in Fig. 5, the amount of erosion increases as the oxygen concentration at the hot point increases depending on the distance from the tip of oxygen jetting part for erosion cutting 26 to the surface of steel material 1. Also, the amount of erosion decreases by increasing the erosion speed. Therefore, by controlling the distance from the tip of oxygen jetting part for erosion cutting 26 to the surface of steel material 1 according to the erosion speed, an appropriate amount of erosion can be achieved, making it possible to perform erosion stably.
[0029] According to the method for cutting steel material of the present embodiment configured as described above, in the cutting process, a critical cutting speed V C The cutting speed is then set to the limit cutting speed V C Since the cutting speed is set to the limit of V, the steel can be cut stably. C Since the cutting speed is set to 0.8 times or more, the cutting speed can be secured and the cutting depth can be made shallow and uniform.
[0030] In this embodiment, the cutting speed is V 0 From V 1 When V1 ≥ V 0 ×(P1 / P 0 ) 0.5 The oxygen pressure of the oxygen for scrubbing is set to P 0 From P 1 When the flow rate is changed to 1000 rpm, even if the cutting speed is increased, sufficient oxygen for cutting can be supplied to the vicinity of the hot point, and the cutting can be performed stably.
[0031] In this embodiment, the cutting speed is V 0 From V 1 When doing so, V 1 ≧V 0 ×(L 0 / L 1 ) 0.858 The distance from the tip of the oxygen jet for scavenging to the surface of the steel material is set to L 0 From L 1When the cutting speed is changed to 100 / s, when the cutting speed is increased, the distance from the tip of the oxygen jetting portion for cutting to the surface of the steel material becomes shorter, which prevents impurities from being mixed into the oxygen for cutting from the atmosphere. This enables the oxygen for cutting to be supplied to the fire point with a high purity, and makes it possible to perform cutting stably.
[0032] The above describes the method for hot cutting steel, which is an embodiment of the present invention. However, the present invention is not limited to this embodiment and can be modified as appropriate without departing from the technical concept of the invention. In this embodiment, the steel material laser cutting device has been described as having the configuration shown in Figure 1, but is not limited to this, and there are no particular limitations on other structures as long as it has a preheating gas ejection section that ejects combustible gas and preheating oxygen, and a laser cutting oxygen ejection section that ejects laser cutting oxygen. EXAMPLES
[0033] The results of experiments carried out to confirm the effects of the present invention will be described below.
[0034] Using the steel material thermal cutting device described in this embodiment, steel material was thermally cut under the conditions shown in Table 1. The average shaving thickness and the standard deviation σ of the unevenness of the shaving surface were evaluated. The evaluation results are shown in Table 1 and Figure 6.
[0035] [Table 1]
[0036] The melting speed V is 0.7 x V C In the comparative example, the average shave thickness was 2.0 mm, and the standard deviation σ of the unevenness of the shave surface was 0.3 mm. In contrast, the melting speed V is 0.8 × V C In the above-described examples of the present invention, the average shave thickness was shallower and the standard deviation σ of the unevenness of the shave surface was smaller than in the comparative examples.
[0037] From the above, it was confirmed that according to the present invention, the surface of the steel material can be stably cut, and the cutting depth can be made shallow and uniform. [Explanation of symbols]
[0038] 1 Steel material 3. Bathtub 10. Steel cutting equipment 20 Scarfer Unit 21 Preheating gas outlet 26 Oxygen outlet for cutting
Claims
1. A method for laser cutting a steel material, comprising: a laser cutting device for laser cutting a surface of the steel material, the laser cutting device having a preheating gas ejection section for ejecting a combustible gas and preheating oxygen; and an oxygen ejection section for ejecting oxygen for laser cutting, the method comprising the steps of: a preheating step of blowing combustible gas and preheating oxygen from the preheating gas jetting portion onto a surface of the steel material to combust them and form a basin portion on the surface of the steel material; a cutting process in which oxygen for cutting is blown onto a surface of the steel material from the oxygen for cutting jetting portion while the steel material is being transported, and the surface of the transported steel material is cut by heat of oxidation reaction between the oxygen for cutting and iron; having In the above-mentioned slag cutting process, a critical slag cutting speed V is set in advance at which the temperature of the steel material at the front part of the slag cutting direction of the hot spot formed by the slag cutting oxygen reacting with the steel material becomes equal to or higher than the liquid phase generation temperature of the steel material. C is calculated based on the following formula (1), and the cutting speed is set to 0.8 × V C More than V C A method for laser cutting a steel material, characterized in that laser cutting is performed within the following range. (1) Formula: V C =(-0.0516×T L +92.0)×exp(0.00146×T 0 ) T L :Liquidus temperature of steel (℃) T 0 :Steel initial temperature (℃)
2. In the above-mentioned cutting process, the cutting speed is V 0 From V 1 In this case, the oxygen pressure of the oxygen for cutting is set to P so as to satisfy the following formula (2). 0 From P 1 2. The method for laser cutting steel material according to claim 1, further comprising changing the temperature of the material to a temperature of 100.degree. (2) Formula: V 1 ≧V 0 ×(P 1 / P 0 ) 0.5
3. In the above-mentioned cutting process, the cutting speed is V 0 From V 1 When the above formula (3) is satisfied, the distance from the tip of the oxygen jetting portion for laser cutting to the surface of the steel material is set to L 0 From L 1 3. The method for laser cutting steel material according to claim 1, further comprising changing the temperature of the material into a temperature range of 100° C. (3) Formula: V 1 ≧V 0 ×(L 0 / L 1 ) 0.858
Citation Information
Patent Citations
JP1991070856U
Method for scarfing metallic slab
JP1995214302A
Nozzle unit for hot-scarfing steel and steel hot-scarfing method
JP1998272561A
Flame scarfing device