Exterior glass components, housings and doors

The exterior glass member with controlled surface unevenness addresses the issue of poor finger slip by enhancing smoothness and glossiness while ensuring excellent finger slip properties and impact resistance.

JP7569017B2Active Publication Date: 2024-10-17NIPPON ELECTRIC GLASS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021529959
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-04
Filing Date
2020-06-19
Publication Date
2024-10-17
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

Exterior glass members used on household appliances and electronic devices have poor finger slip properties due to their smooth and glossy surfaces, leading to potential slipping and catching when touched.

Method used

The exterior glass member features unevenness on its surface, with specific cutoff values for high-pass and low-pass filters to maintain smoothness and glossiness while enhancing finger slip properties, and is made from tempered glass for impact resistance.

Benefits of technology

The solution provides excellent finger slip properties while maintaining the smoothness and glossiness of glass, with improved impact resistance and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569017000003
    Figure 0007569017000003
  • Figure 0007569017000004
    Figure 0007569017000004
  • Figure 0007569017000005
    Figure 0007569017000005
Patent Text Reader

Abstract

The present invention provides an exterior glass member which has excellent finger slipping properties while maintaining texture and glossiness of glass, and provides a casing, and a door. The present invention includes a glass substrate 20 that has irregularities on at least one main surface 20a, wherein in the main surface 20a having the irregularities, the maximum height range Rz of the irregularities is 3 to 1000 nm and the pitch RSm of the irregularities is 50 to 5000 μm when a cut-off value of a high pass filter λc is a value 1.6 times the pitch between adjacent irregularities of a measured profile curve and a cut-off value of a low pass filter λs is 25 μm, and the three-dimensional arithmetic average roughness Sa of the irregularities is 0.5 to 50 nm and the pitch RSm of the irregularities is 0.01 to 10 μm when the cut-off value of the high pass filter λc is 25 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to housings and doors for use in household electrical appliances and electronic devices, and to exterior glass members and housings and doors for use in furniture panels, displays, and the like. [Background technology]

[0002] Housings and doors for household electrical appliances and electronic devices, furniture panels, displays, and the like are made of materials such as resin, wood, or metal, taking into consideration various requirements such as decorativeness, scratch resistance, workability, and cost.

[0003] In recent years, household electrical appliances such as refrigerators and electronic devices have become increasingly diverse, and high-end models are required to have multiple functions, high performance, and a luxurious appearance. In response to this trend, a proposal has been made for a household electrical appliance in which a glass plate is placed on the front surface of the door body, housing, etc. as an exterior member, so that the surface of the exterior member does not feel rough and has a glossy appearance (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 3140110 Summary of the Invention [Problem to be solved by the invention]

[0005] However, when an exterior member made of a glass plate is used on the front surface of the door body as in Patent Document 1, the surface of the glass plate is generally formed smoothly with few irregularities, so that when a finger is touched and slid across the surface of the exterior member, a catch occurs, meaning that the finger slideability is very poor.

[0006] Therefore, the present invention provides an exterior glass member, as well as a housing and a door body, that have excellent finger slipperiness while retaining the smooth feel and glossiness that are characteristic of glass. [Means for solving the problem]

[0007] The exterior glass member that solves the above problems has the following features. That is, the glass member for exterior use according to the present invention comprises a glass substrate having irregularities on at least one of its main surfaces, and when the cutoff value of the high-pass filter λc on the main surface having the irregularities is set to 1.6 times the spacing between the irregularities on the measured cross-sectional curve and the cutoff value of the low-pass filter λs is set to 25 μm, the maximum height width of the irregularities is 3 nm or more and 1000 nm or less and the spacing width between the irregularities is 50 μm or more and 5000 μm or less, and when the cutoff value of the high-pass filter λc is set to 25 μm, the three-dimensional arithmetic mean roughness of the irregularities is 0.5 nm or more and 50 nm or less and the spacing width between the irregularities is 0.01 μm or more and 10 μm or less. With this configuration, the exterior glass member can have excellent finger slipperiness while retaining the smooth feel and glossiness that glass has.

[0008] In addition, when the cutoff value of the high-pass filter λc is set to 1.6 times the interval between the projections and recesses of the measured cross-sectional curve, and the cutoff value of the low-pass filter λs is set to 25 μm, it is preferable that the interval between the projections and recesses be more than 1000 μm and not more than 5000 μm. This further improves the finger sliding properties of the exterior glass member.

[0009] It is also preferable that the haze is less than 10% in the visible light wavelength range. This makes it possible to maintain the transparency of the exterior glass member.

[0010] The glass substrate is preferably made of reinforced glass. This can improve the impact resistance of the exterior glass member.

[0011] The housing further includes the exterior glass member. With this configuration, the housing can have excellent finger slipperiness while retaining the smooth feel and glossiness that glass has.

[0012] The door body is provided with the exterior glass member. With this configuration, the door body can have excellent finger sliding properties while retaining the smooth feel and glossiness that glass has. Effect of the Invention

[0013] According to the present invention, it is possible to obtain a glass having excellent finger slipperiness while retaining the smoothness and glossiness that are characteristic of glass. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic side cross-sectional view showing an example of an embodiment of an exterior glass member of the present invention. [Diagram 2] 1A and 1B are diagrams showing a measured cross-sectional curve of a main surface, irregularities with large gap widths, and irregularities with small gap widths. [Diagram 3] FIG. 13 is a diagram showing the cutoff values ​​of a high-pass filter λc and a low-pass filter λs. [Figure 4] FIG. 1 is a schematic side cross-sectional view showing an example of an embodiment of a housing or a door of the present invention. [Diagram 5] FIG. 13 is a diagram showing a state in which a fingertip touches the main surface of a glass substrate on which two types of irregularities, large and small, with different intervals between the irregularities, are formed. [Figure 6] FIG. 13 is a diagram showing a state in which a fingertip touches the main surface of a glass substrate that does not have two types of unevenness, large and small, with unevenness having different spacing widths between the unevennesses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.

[0016] 1 is a schematic side cross-sectional view showing an example of an embodiment of an exterior glass member 10 of the present invention. The exterior glass member 10 includes a glass substrate 20. Examples of the glass substrate 20 include aluminosilicate glass, borosilicate glass, alkali-free glass, soda-lime glass, tempered glass, Li 2 O?Al 2 O 3 ?SiO 2 The glass substrate 20 may be made of a glass-ceramic glass. For example, when high mechanical strength is required for the exterior glass member 10, it is preferable to make the glass substrate 20 of tempered glass. Examples of tempered glass include physically tempered glass and chemically tempered glass, and when particularly high mechanical strength is required, chemically tempered glass is preferable. For example, when excellent scratch resistance is required for the exterior glass member 10, it is preferable to make the glass substrate 20 of alkali-free glass, particularly alkali-free borosilicate glass.

[0017] The glass base material 20 has projections and recesses formed on one main surface 20a. The glass base material 20 is placed so that the main surface 20a on which the projections and recesses are formed is the surface that is touched by the fingertip 31.

[0018] As shown in Fig. 2, the unevenness is composed of two types of unevenness, large and small, with different intervals between the unevennesses. The unevenness with the large interval has a maximum height Rz of 3 nm to 1000 nm and an interval RSm of 50 µm to 5000 µm. The unevenness with the small interval has a three-dimensional arithmetic mean height Sa of 0.5 nm to 50 nm and an interval RSm of 0.01 µm to 10 µm. The maximum height width Rz is preferably larger than the three-dimensional arithmetic mean height Sa. Moreover, the maximum height width Rz is more preferably 1.1 to 500 times the three-dimensional arithmetic mean height Sa.

[0019] Here, in the case of unevenness with a large gap width, the maximum height width Rz is defined in JIS B 0633 (ISO 4288) and is the sum of the height of the highest peak and the depth of the deepest valley in the unevenness. The gap width RSm of the unevenness is defined in JIS B 0633 (ISO 4288) and is the average of each periodic length Xs of the unevenness in a specified reference length. For irregularities with small intervals, the three-dimensional arithmetic mean height Sa is defined in ISO 25178 and is the average of the absolute values ​​of the peak height Z1 and valley depth Z2 of the irregularities in a specified three-dimensional area. The interval width RSm of the irregularities is defined in JIS B 0633 (ISO 4288) and is the average of each periodic length Xs of the irregularities in a specified reference length.

[0020] As shown in Figures 2 and 3, the values ​​of the maximum height width Rz and the spacing width RSm of the asperities with the above-mentioned large spacing width are values ​​obtained when the cutoff value λc1 of the high-pass filter λc for cutting off long wavelength components from the measured cross-sectional curve of main surface 20a is set to a value 1.6 times the spacing width of the asperities of the measured cross-sectional curve, and the cutoff value λs1 of the low-pass filter λs for cutting off short wavelength components from the measured cross-sectional curve of main surface 20a is set to 25 µm.

[0021] In addition, the values ​​of the three-dimensional arithmetic mean height Sa and the spacing width RSm of the irregularities with small spacing widths described above are values ​​obtained when the cutoff value λc2 of the high-pass filter λc for blocking long wavelength components from the measured cross-sectional curve of the main surface 20a is set to 25 μm. In addition, in the measured cross-sectional curve of the main surface 20a, by applying a high-pass filter λc having a cutoff value λc2, the waviness components and large gap width unevenness components of the main surface 20a are removed, and a curve of small gap width unevenness is obtained.

[0022] By having the shape of the large gap width unevenness and the shape of the small gap width unevenness on the main surface 20a of the glass substrate 20 within such a range, the texture of glass can be maintained without feeling roughness when touching the main surface 20a on which the unevenness is formed. In addition, since scattered light due to the formed unevenness is unlikely to occur, the glossiness of glass can be maintained. In addition, when the fingertip touches the main surface 20a on which the unevenness is formed and slides, no catching occurs, and the finger slides well. Furthermore, it is preferable that no resin layer is formed on the main surface 20a of the glass substrate 20, and if the unevenness is formed directly, the scratch resistance is high and it is difficult to be scratched.

[0023] The large gap width unevenness affects the contact between the main surface 20a and the fingertip 31. The fingertip 31 comes into contact with the main surface 20a of the glass substrate 20 at the convex portions of the large gap width unevenness, but does not come into contact with the concave portions of the large gap width unevenness. This can reduce the frictional force between the fingertip 31 and the main surface 20a, and can provide excellent finger sliding properties.

[0024] The maximum height Rz of the unevenness with large gap width is 1000 nm or less, preferably 500 nm or less, and more preferably 200 nm or less. Furthermore, the maximum height Rz of the unevenness with large gap width is 3 nm or more, preferably 4 nm or more, and more preferably 5 nm or more. The gap width RSm of the large gap width irregularities is 5000 μm or less, preferably 4000 μm or less, and more preferably 3000 μm or less. Furthermore, the spacing width RSm of the unevenness with a large spacing width is 50 μm or more, preferably 100 μm or more, more preferably 530 μm or more, and even more preferably more than 1000 μm. The ratio Rz / RSm of the maximum height Rz of the large gap width unevenness to the gap width RSm of the large gap width unevenness is 5.0×10 -5 Preferably, it is less than 3.0×10 -5 It is more preferable that: In addition, the ratio Rz / RSm of the maximum height Rz of the large gap width unevenness to the gap width RSm of the large gap width unevenness is 0.1×10 -5 It is preferable that the value is 0.3×10 or more. -5 More preferably, it is equal to or greater than this.

[0025] The small-spaced unevenness contributes to reducing the frictional force between the main surface 20a of the glass substrate 20 and the fingertip 31. As a result, when the fingertip 31 is slid over the main surface 20a of the glass substrate 20, no catching occurs, and the glass substrate 20 can have excellent finger sliding properties.

[0026] The three-dimensional arithmetic mean height Sa of the small gap width irregularities is 50 nm or less, preferably 40 nm or less, and more preferably 30 nm or less. Furthermore, the three-dimensional arithmetic mean height Sa of the small gap width irregularities is 0.5 nm or more, preferably 2 nm or more, and more preferably 3 nm or more. The spacing RSm of the small spacing irregularities is 10 μm or less, preferably 7 μm or less, and more preferably 5 μm or less. Furthermore, the spacing RSm of the small-spacing irregularities is 0.01 μm or more, preferably 0.1 μm or more, and more preferably 0.5 μm or more.

[0027] Since the coating and design of the housing and door body are viewed through the glass substrate 20, the glass substrate 20 is formed so that the haze, which is an index of transparency and indicates the degree of cloudiness, is less than 10% in the wavelength range of visible light (380 nm to 780 nm). By setting the haze of the glass substrate 20 to less than 10%, the transparency of the glass substrate 20 can be maintained, and the design of the housing and door body is not impaired.

[0028] In this embodiment, the haze of the glass substrate 20 is set to less than 10%, preferably less than 7%, more preferably less than 5%, and even more preferably less than 4%.

[0029] In addition, an anti-reflection film for reducing the reflectance on the side that is in contact with a fingertip, or an anti-fouling film for preventing fingerprints from adhering and for imparting water- and oil-repellency can be formed on the main surface 20a of the glass substrate 20.

[0030] When the glass substrate 20 is used as a cover member for the exterior glass member 10, the anti-reflection film is provided at least on the main surface 20a on the front side (the side touched by the fingertip 31) of the glass substrate 20. When there is a gap between the glass substrate 20 and the housing or the door, it is preferable that the glass substrate 20 also has an anti-reflection film on the main surface 20a on the back side (the housing side or the door side). The anti-reflection film may be, for example, a low refractive index film having a refractive index lower than that of the glass substrate 20, or a dielectric multilayer film in which a low refractive index film having a relatively low refractive index and a high refractive index film having a relatively high refractive index are alternately laminated. The anti-reflection film may be formed by a sputtering method, a CVD method, or the like.

[0031] When the glass substrate 20 has an anti-reflection coating on its main surface 20a, the unevenness of the main surface 20a of the glass substrate 20 is formed so that the unevenness of the surface of the anti-reflection coating falls within the above-mentioned surface roughness range (the maximum height width Rz of the unevenness with a large gap width and the gap width RSm of the unevenness, and the three-dimensional arithmetic surface height Sa of the unevenness with a small gap width and the gap width RSm of the unevenness). Furthermore, when the main surface 20a of the glass substrate 20 has an anti-reflection coating, the irregularities are formed on the main surface 20a of the glass substrate 20 so that the haze of the glass substrate 20 having the anti-reflection coating falls within the above-mentioned range. When the interval width RSm of the irregularities and the three-dimensional arithmetic mean height Sa of the irregularities are measured after the anti-reflection coating is formed, a 10 nm Au film is formed and then these values ​​are measured.

[0032] When the glass substrate 20 is used as a cover member for the exterior glass member 10, the antifouling film is provided on the main surface 20a on the front side of the glass substrate 20 (the side that is in contact with the fingertip 31). The antifouling film preferably contains a fluorine-containing polymer containing silicon in the main chain. The fluorine-containing polymer may, for example, have a ?Si?O?Si? unit in the main chain and contain fluorine. A polymer having a water-repellent functional group in a side chain can be used. The fluorine-containing polymer can be synthesized, for example, by dehydration condensation of silanol. When the glass substrate 20 has an antireflection film and an antifouling film on the front principal surface 20a, the antireflection film is formed on the principal surface 20a of the glass substrate 20, and the antifouling film is formed on the antireflection film.

[0033] When the main surface 20a of the glass substrate 20 has an anti-fouling film, or when the main surface 20a of the glass substrate 20 has an anti-reflection film and an anti-fouling film, the unevenness of the main surface 20a of the glass substrate 20 is formed so that the unevenness of the surface of the anti-fouling film falls within the above-mentioned surface roughness range (the maximum height width Rz of the unevenness with a large interval width and the interval width RSm of the unevenness, and the three-dimensional arithmetic surface height Sa of the unevenness with a small interval width and the interval width RSm of the unevenness). Furthermore, when the main surface 20a of the glass substrate 20 has an anti-soiling film, or when the main surface 20a of the glass substrate 20 has an anti-reflection film and an anti-soiling film, the unevenness of the main surface 20a of the glass substrate 20 is formed so that the haze of the glass substrate 20 after the anti-soiling film is formed, or the haze of the glass substrate 20 after the anti-reflection film and the anti-soiling film are formed, falls within the above-mentioned range.

[0034] FIG. 4 is a schematic side cross-sectional view showing an example of an embodiment of the housing or door body 40 of the present invention. The housing or door body 40 includes, in order from the inside of the housing or door body, a frame body 41, a colored layer 42, an adhesive layer 43, and a glass substrate 20. The main surface 20a of the glass substrate 20 is disposed on the outermost surface of the housing or door body. With this configuration, the housing or door body can have excellent finger slipperiness while maintaining a smooth and glossy surface. Furthermore, by making the haze of the glass substrate 20 less than 10%, the transparency of the glass substrate 20 can be maintained, and the color tone and design of the colored layer 42 can be clearly recognized from the outside.

[0035] Next, a method for producing the exterior glass member 10 will be described. At least one of the main surfaces 20a of the glass substrate 20 constituting the exterior glass member 10 is subjected to a combination of at least one of the treatment methods such as wet blasting, chemical etching, and silica coating to form irregularities on the main surface 20a. Wet blasting is a process in which abrasive grains made of solid particles such as alumina and liquid such as water are uniformly mixed to form a slurry, which is then sprayed at high speed from a spray nozzle onto a workpiece made of glass using compressed air, forming fine irregularities on the workpiece. Furthermore, a round nozzle with a slurry spray outlet area smaller than the area of ​​the workpiece is used as the nozzle for spraying the slurry, and various surface shapes can be formed by moving this round nozzle relative to the workpiece.

[0036] In the wet blasting process, when the slurry is sprayed at high speed and collides with the workpiece, the abrasive grains in the slurry scrape, hit, and rub the surface of the workpiece, forming fine irregularities on the surface of the workpiece. In this case, the abrasive grains sprayed on the workpiece and the fragments of the workpiece scraped by the abrasive grains are washed away by the liquid sprayed on the workpiece, so that the number of particles remaining on the workpiece is reduced. In addition, by scanning the nozzle arbitrarily over the workpiece and spraying the slurry partially on the surface of the workpiece, it is possible to create irregularities with a large interval width in addition to irregularities with a small interval width. The glass substrate 20 is obtained by preparing a workpiece having two types of irregularities, large and small, with different interval widths between the irregularities on the surface by cutting it into a desired size and shape.

[0037] The surface roughness of the small gap width unevenness formed on the main surface of the workpiece by wet blasting can be adjusted mainly by the particle size distribution of the abrasive grains contained in the slurry and the injection pressure when the slurry is injected onto the workpiece. The maximum height width Rz of the large gap width unevenness and the gap width RSm of the unevenness can be adjusted by the size of the nozzle that injects the slurry, the feed pitch width, and the injection pressure.

[0038] In wet blasting, when the slurry is sprayed onto the workpiece, the liquid carries the abrasive grains to the workpiece, so that finer abrasive grains can be used than in dry blasting, and the impact when the abrasive grains collide with the workpiece is reduced, making it possible to perform precise processing. In this way, by subjecting the workpiece to wet blasting, it is easy to form two types of large and small irregularities with different spacing widths between the irregularities of appropriate size on the main surface 20a of the glass substrate 20, and it is possible to obtain excellent finger slipperiness while maintaining the smoothness and glossiness of glass without compromising the transparency of the glass substrate 20.

[0039] In the dry blasting process, friction occurs when the sprayed abrasive grains collide with the workpiece, generating processing heat in the workpiece, but in the wet blasting process, the liquid constantly cools the surface of the workpiece during the process, so the workpiece is not heated by the blasting process. In addition, although it is possible to form irregularities on the main surface 20a of the glass substrate 20 by performing the dry blasting process, the impact of the abrasive grains colliding with the main surface 20a of the glass substrate 20 in the dry blasting process is too large, so that the surface roughness of the main surface 20a on which the irregularities are formed tends to increase, making the glass substrate 20 feel rough and impairing its glossiness.

[0040] The chemical etching process is a process in which the main surface 20a of the glass substrate 20 is chemically etched with hydrogen fluoride (HF) gas, hydrofluoric acid, an aqueous sodium hydroxide solution, or an aqueous potassium hydroxide solution.

[0041] The silica coating process is a process in which a coating agent containing a matrix precursor such as a silica precursor and a liquid medium that dissolves the matrix precursor is applied to the main surface 20a of the glass substrate 20, and then heated. EXAMPLES

[0042] Next, an example of the glass base material 20 having two types of unevenness, large and small, with different intervals between the unevenness on the main surface 20a will be described, although the glass base material 20 is not limited to this.

[0043] (Sample Preparation) In this example, Samples 1 to 15 were prepared as examples of the glass substrate 20, and Samples 16 to 18 were prepared as comparative examples. As the glass substrate 20 used in Samples 1 to 18, alkali-containing aluminosilicate glass having a thickness of 1.1 mm was used.

[0044] The glass substrate 20 of the samples 1 to 12, which are examples, was subjected to wet blasting to form two types of unevenness, large and small, with different intervals between the unevenness, on one of the main surfaces 20a. Specifically, the glass substrate 20 of the samples 1 to 12 was subjected to wet blasting by uniformly stirring abrasive grains made of alumina with a grain size of #4000 to #8000 and water, placing the glass substrate 20 on a processing table, and spraying the slurry over the entire one of the main surfaces 20a of the glass substrate 20 while scanning the nozzle at a speed of 0.5 mm / s to 1.5 mm / s using air with a processing pressure of 0.1 MPa to 0.3 MPa. The round nozzle used for wet blasting is a nozzle that narrows the cross-sectional area of ​​the slurry nozzle to a small value relative to the area of ​​the main surface 20a, and partially sprays the slurry over the main surface 20a. The interval between the unevenness with a large interval was varied by changing the scanning distance of the round nozzle. The maximum height Rz of the large gap unevenness was varied by increasing the number of scans. The three-dimensional arithmetic mean height Sa of the small gap unevenness was varied by changing the alumina particle size or the processing pressure. The abrasive grains used were polygonal.

[0045] For samples 1 to 12, the interval width of the large-interval unevenness was created by varying the scanning distance of the round nozzle from 51 μm to 4900 μm. The maximum height width Rz of the large-interval unevenness was created by varying the number of round nozzle scans from 2 to 15 times that of sample 7. The three-dimensional arithmetic mean height Sa of the small-interval unevenness was created by changing the alumina particle size from #4000 to #8000 and increasing the processing pressure in the range from 0.1 MPa to 0.3 MPa.

[0046] The glass substrate 20 of Samples 13 and 14 as examples was prepared by forming two types of unevenness, large and small, with different unevenness intervals on one main surface 20a by performing the above-mentioned wet blasting treatment, and then combining it with an etching treatment. For Sample 13, the sample after the wet blasting treatment was immersed in a 2.5 mol% sodium hydroxide aqueous solution at 80°C for 24 hours to prepare the sample. For Sample 14, the sample after the wet blasting treatment was immersed in a 5 mol% hydrogen fluoride aqueous solution at 25°C to prepare the sample.

[0047] After applying a silica spray coating to the main surface 20a of the glass substrate 20 of the sample 15 as an example, forming irregularities with large intervals, the main surface 20a was subjected to a wet blasting treatment in which a slurry was uniformly sprayed onto the front surface of the main surface 20a using a wide nozzle at a treatment pressure of 0.10 MPa. The wide nozzle used for wet blasting is a nozzle that has a large width for the slurry spray port, enabling the slurry to be sprayed uniformly onto the front surface of the main surface 20a.

[0048] The main surface 20a of the glass substrate 20 of the sample 16, which is a comparative example, is not subjected to any treatment. In other words, the glass substrate 20 of the sample 16 is untreated. For the glass substrate 20 of Sample 17, which is a comparative example, wet blasting was performed on one of the main surfaces 20a by uniformly spraying a slurry over the entire main surface 20a using a wide nozzle at a processing pressure of 0.25 MPa. For the glass substrate 20 of sample 18 serving as a comparative example, one of the main surfaces 20a was spray-coated with silica.

[0049] (Surface roughness measurement) The surface roughness of the principal surface 20a of the glass substrate 20 was measured for samples 1 to 18. The surface roughness was measured on the principal surface that had been subjected to a wet blasting treatment for samples 1 to 15 and 17, on the principal surface that had been subjected to a silica spray coating for sample 18, and on one of the principal surfaces 20a for sample 16.

[0050] The measured surface roughness parameters were the maximum height Rz and the spacing RSm between the projections and recesses for irregularities with large spacing widths, and the three-dimensional arithmetic surface height Sa and the spacing RSm between the projections and recesses for irregularities with small spacing widths. The surface roughness measurements were performed using a white light interference microscope.

[0051] The white light interference microscope used was a white light interference microscope (New View 7300) manufactured by Zygo, and measurements were carried out based on JIS B0601-2013. The measurement conditions for large gap width irregularities were a 2.5x objective lens and a 1x zoom lens, with a measurement area of ​​2827 x 2120 μm, a camera pixel count of 640 x 480, and an accumulation count of 1. When measuring the maximum height width Rz of large gap width irregularities and the gap width RSm of the irregularities, the cutoff value λc1 of the high-pass filter λc was set to about 1.6 times the gap width RSm of the irregularities, and the cutoff value λs1 of the low-pass filter λs was set to 25 μm. The measurement conditions for small gap unevenness were a 50x objective lens and a 2x zoom lens, with a measurement area of ​​74 x 55 μm, camera pixel count of 640 x 480, and accumulation count of 8. When measuring the three-dimensional arithmetic mean roughness Sa of small gap unevenness and the gap width RSm of the unevenness, the cutoff value λc2 of the high-pass filter λc was set to 25 μm.

[0052] (Surface roughness measurement results) The results of the surface roughness measurements performed on Samples 1 to 18 will be described. The measurement results are shown in Tables 1 and 2.

[0053] [Table 1]

[0054] [Table 2]

[0055] As shown in Tables 1 and 2, the maximum height width Rz of the large gap width irregularities is in the range of 10 nm to 750 nm for Samples 1 to 15, which are examples. For Sample 16, which is an untreated comparative example, and Sample 17, which is a comparative example that was subjected to wet blasting treatment using a wide nozzle, large gap width irregularities were not formed. For Sample 18, which is a comparative example that was subjected to silica spray coating, the maximum height width Rz of the irregularities was 831 nm.

[0056] The spacing width RSm of the unevenness with large spacing is in the range of 51 μm to 4900 μm for Samples 1 to 15 of the embodiment. For Sample 16, which is an untreated comparative example, and Sample 17, which is a comparative example that was subjected to wet blasting treatment using a wide nozzle, unevenness with large spacing was not formed. For Sample 18, which is a comparative example that was subjected to silica spray coating, the spacing width RSm was 15 μm.

[0057] The three-dimensional arithmetic surface height Sa of the small-spaced irregularities is in the range of 0.8 nm to 21.3 nm for the embodiment samples 1 to 15. For the untreated comparative sample 16, it is 0.2 nm, which is smaller than the samples 1 to 15, and for the comparative sample 17, which is subjected to wet blasting treatment using a wide nozzle, it is 7.0 nm. For the comparative sample 18, which is subjected to silica spray coating, no small-spaced irregularities are formed.

[0058] The spacing width RSm of small-spaced irregularities is in the range of 1.6 μm to 7.2 μm for Samples 1 to 15, which are examples. For Sample 16, an untreated comparative example, and Sample 18, a comparative example that was spray-coated with silica, irregularities with large spacing were not formed. For Sample 17, a comparative example that was wet-blasted with a wide nozzle, the spacing width RSm was 2.4 μm.

[0059] (Haze measurement) The haze was measured for Samples 1 to 18. The haze was measured using an ultraviolet, visible, near-infrared analytical photometer (UV-3100PC) manufactured by Shimadzu Corporation, based on JIS K7361-1-1997.

[0060] (Haze measurement results) As shown in Tables 1 and 2, the haze of Samples 1 to 15, which are examples, is in the range of 1.0% to 9.4%. Sample 18, which is a comparative example that was spray-coated with silica, had a haze of 34%. On the other hand, there was no significant difference between Sample 16, which was untreated, and Sample 17, which was wet-blasted with a wide nozzle, and Samples 1 to 7.

[0061] (Evaluation of finger smoothness) The finger slipperiness when the fingertip 31 was slid over the surface of the glass substrate 20 was evaluated by a sensory test. The evaluation method consisted of a total of 20 men and women in their 20s to 50s evaluating the friction when the finger 31 was moved while touching the surface of the glass substrate 20, and the evaluation results of the majority were shown in Table 1. ◎: Fingers slide smoothly. ○: The finger slides smoothly, but it feels a little strange. ×: My fingers feel like they're getting caught.

[0062] (Evaluation results of finger smoothness) As shown in Tables 1 and 2, the finger sliding property was rated as ⊚ for Samples 1 to 15, which are examples. Sample 18, which is a comparative example in which irregularities were formed by silica coating, was rated as ⊚. Meanwhile, Sample 16, which is an untreated comparative example, and Sample 17, which is a comparative example in which wet blasting treatment was performed using a wide nozzle, were rated as x.

[0063] (Evaluation of glossiness) The gloss of the exterior glass member 10 was evaluated. The evaluation method consisted of shining a light from above onto the surface of the glass substrate and observing the appearance of the reflected light, and rating it according to the following three-level scale. ◎: Feels glossy and shiny, ○: It has a glossy feel, but the color looks slightly whitish. ×: The whiteness of the color is noticeable due to scattering, and the surface is matte.

[0064] (Gloss evaluation results) As shown in Tables 1 and 2, the glossiness of the examples, Samples 1 to 9, 11, 12, and 14, was rated as ⊚. Samples 10, 13, and 15 were rated as ◯. Sample 16, an untreated comparative example, and Sample 17, a comparative example that was subjected to wet blasting treatment using a wide nozzle, were rated as ⊚. On the other hand, Sample 18, a comparative example that was subjected to silica spray coating, was rated as ×.

[0065] (Evaluation of roughness) The roughness felt when touching the surface of the glass substrate 20 with a fingertip 31 was evaluated by sensory evaluation. The roughness felt when the fingertip 31 was placed on the glass substrate 20 was evaluated by a total of 20 men and women in their 20s to 50s on the three-point scale shown below, and the majority evaluation results are shown in Table 1. ◎: No roughness felt at all. ○: Feels slightly rough. ×: A strong feeling of roughness is felt.

[0066] (Evaluation results for roughness) As shown in Tables 1 and 2, the roughness of the surface of the glass substrate 20 was rated as ⊚ for Samples 1 to 9 and 10 to 14, which are examples. Samples 10 and 15 were rated as ◯. Sample 16, which is an untreated comparative example, and Sample 17, which is a comparative example that was subjected to a wet blasting treatment using a wide nozzle, were rated as ⊚. On the other hand, Sample 18, which is a comparative example in which irregularities were formed by silica coating, was rated as x.

[0067] (Overall evaluation of each sample) As shown in Tables 1 and 2 and Fig. 5, for Samples 1 to 15 as examples, two types of unevenness, large and small, with different spacing widths between the appropriate unevenness formed on the main surface 20a with which the fingertip 31 comes into contact, prevent the fingertip 31 from getting caught on the main surface 20a of the glass substrate 20. Specifically, small unevenness reduces the frictional force between the fingertip 31 and the main surface 20a, and large unevenness reduces the contact area between the fingertip 31 and the main surface 20a, thereby making it easier to slide. Due to these effects, good evaluation results were obtained, such as good finger smoothness, a glossy feel, and no roughness. On the other hand, in the case of Sample 16, which is an untreated comparative example, the unevenness of main surface 20a with which fingertip 31 comes into contact is small, so there is a lot of catching and the finger sliding property is poor. As shown in Fig. 6, sample 17, which is a comparative example that was subjected to wet blasting treatment using a wide nozzle, did not have two types of unevenness, large and small, with different spacing between the unevenness, so it was not possible to sufficiently prevent fingertips 31 from getting caught, and finger smoothness was poor. Sample 18, in which unevenness was formed by silica coating, felt very rough and the glossiness was impaired.

[0068] Examples of household electrical appliances in which the housing or door of the present invention can be used include electric refrigerators, electric washing machines, rice cookers, IH cooking heaters, vacuum cleaners, oven ranges, microwave ovens, toaster ovens, air purifiers, dishwashers and dryers, electric pots and electric kettles. Moreover, examples of electronic devices in which the housing of the present invention can be used include the following. For example, examples of electronic devices serving as communication terminals include mobile phones, smartphones, PDAs (Personal Data Assistance), and PNDs (Portable Navigation Devices, portable car navigation systems), and examples of broadcast receivers include portable radios, portable televisions, and one-segment receivers. Examples of electronic devices serving as information terminals include digital cameras, video cameras, portable music players, sound recorders, portable DVD players, portable game consoles, notebook computers, tablet PCs, electronic dictionaries, electronic organizers, e-book readers, portable printers, and portable scanners. In addition, it can also be used as a cover member for electronic devices installed inside an automobile. However, the present invention is not limited to these examples. [Industrial Applicability]

[0069] INDUSTRIAL APPLICABILITY The present invention is applicable to an exterior glass component that has excellent finger slipperiness while retaining the smooth texture and glossiness of glass, and to a housing or door body that includes the exterior glass component. [Explanation of symbols]

[0070] 10 Exterior glass components 20 Glass substrate 20a Main surface 31 Fingertips

Claims

1. A glass substrate having irregularities on at least one of its main surfaces, In the main surface having the irregularities, when the cutoff value of the high-pass filter λc is set to a value 1.6 times the interval between the projections and recesses of the measured cross-sectional curve and the cutoff value of the low-pass filter λs is set to 25 μm, the maximum height width of the projections and recesses is 3 nm or more and 1000 nm or less and the interval between the projections and recesses is more than 1000 μm and 5000 μm or less; when the cutoff value of the high-pass filter λc is set to 25 μm, the three-dimensional arithmetic average roughness of the projections and recesses is 0.5 nm or more and 50 nm or less and the interval between the projections and recesses is 0.01 μm or more and 10 μm or less; 1. An exterior glass member comprising:

2. A glass substrate having irregularities on at least one of its main surfaces, In the main surface having the irregularities, when the cutoff value of the high-pass filter λc is set to a value 1.6 times the interval between the projections and recesses of the measured cross-sectional curve and the cutoff value of the low-pass filter λs is set to 25 μm, the maximum height of the projections and recesses is 3 nm or more and 1000 nm or less and the interval between the projections and recesses is 50 μm or more and 5000 μm or less; when the cutoff value of the high-pass filter λc is set to 25 μm, the three-dimensional arithmetic average roughness of the projections and recesses is 0.5 nm or more and 50 nm or less and the interval between the projections and recesses is 0.01 μm or more and 10 μm or less; A glass member for exterior use, wherein the ratio Rz / RSm of the maximum height Rz of the irregularities with large gap widths to the gap width RSm of the irregularities with large gap widths is less than 5.0×10 −5 .

3. 3. The glass member for exterior use according to claim 1, wherein the haze is less than 10% in the wavelength range of visible light.

4. 4. The exterior glass member according to claim 1, wherein the glass substrate is made of tempered glass.

5. A housing comprising the exterior glass member according to any one of claims 1 to 4.

6. A door comprising the exterior glass member according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Door body for refrigerator

    JP1993133677A

  • Glass substrate for magnetic recording medium, and method of manufacturing glass substrate for magnetic recording medium

    JP2006228284A

  • Door body of refrigerator

    JP2013234832A

  • Light-transmissible insulation board for thin film solar battery and integration type thin film silicon solar battery

    JP2016029675A

  • Anti-glare glass plate article for display device, and method of manufacturing the same

    JP2016136232A