Block copolymer, dispersant and coloring composition
A block copolymer with tailored structural units addresses the dispersion and agglomeration issues of carbon particles in water-based paints, enhancing the jet blackness of the coating film by improving dispersibility and preventing particle aggregation.
Patent Information
- Application Number
- JP2020157366
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-04
- Filing Date
- 2020-09-18
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-09-18
AI Technical Summary
Water-based paints face challenges in uniformly dispersing carbon particles like carbon black due to their small particle size and strong cohesive forces, leading to agglomeration, which affects the jet blackness of the coating film.
A block copolymer with specific structural units, including an A block that adsorbs to the colorant and a B block with high affinity for the aqueous medium, enhancing dispersion performance and suppressing agglomeration.
The block copolymer effectively disperses carbon particles in water-based paints, improving jet blackness of the coating film by preventing agglomeration and ensuring uniform distribution.
Smart Images

Figure 0007569187000001 
Figure 0007569187000002 
Figure 0007569187000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a block copolymer, a dispersant containing the block copolymer, and a colored composition containing the dispersant. [Background technology]
[0002] In recent years, there has been a demand to reduce emissions of volatile organic compounds (VOCs) from factories and offices in order to prevent air pollution. As a result, there has been discussion about switching to water-based paints for painting automobiles, etc.
[0003] Here, the coloring agent used in paint generally has a hydrophobic surface. Therefore, in water-based paint, the dispersibility of the coloring agent becomes a problem. In particular, carbon particles such as carbon black used as a black coloring agent have a small primary particle diameter and an extremely large specific surface area, and therefore have a very strong cohesive force. Therefore, it is difficult to disperse the carbon particles uniformly in the water-based dispersion medium, and even if they are dispersed, they tend to aggregate.
[0004] Therefore, in paints that use carbon black as a black colorant, a technique for improving the dispersibility of carbon black has been proposed. For example, Patent Document 1 describes a paint with a DBP oil supply of 150 ml / 100 g or less, an average primary particle size of 15 nm or less, and a specific surface area of 500 m 2 / g or less and having a pH in the acidic to neutral range, is dispersed in an aqueous medium by a pigment dispersant to form a highly jet-black carbon black dispersion. In this patent document 1, the dispersibility of carbon black is improved by controlling the physical properties of the carbon black (see cited document 1 (claim 1, paragraphs 0019, 0021, 0024)).
[0005] Furthermore, Patent Document 2 describes an aqueous coating composition containing (A) (a) a polymerizable unsaturated monomer having a specific cationic functional group, (b) a polymerizable unsaturated monomer having a polyoxyalkylene chain, and (c) a copolymer of other polymerizable unsaturated monomers, (B) a pigment, and (C) an acid group- and hydroxyl group-containing acrylic resin (see Patent Document 2 (Claim 1, paragraph 0014)). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-285632 A [Patent Document 2] JP 2014-5399 A Summary of the Invention [Problem to be solved by the invention]
[0007] In water-based paints using carbon particles as a black coloring material, paints with improved dispersibility of the carbon particles have been proposed, but there is room for improvement in preventing the aggregation of the carbon particles. The present invention has been made in consideration of the above circumstances, and has an object to provide a block copolymer that can be used as a dispersant for water-based paints, which has high dispersibility of coloring materials (especially carbon particles) and can suppress aggregation. Another object of the present invention is to provide a block copolymer that can improve the jet blackness of a coating film when used as a dispersant for a coloring composition containing carbon particles. [Means for solving the problem]
[0008] The present invention has an A block and a B block that can solve the above-mentioned problems, and is characterized in that the A block contains a structural unit represented by formula (1) and a structural unit represented by formula (2), and the B block contains a structural unit represented by formula (3).
[0009] [ka] [In formula (1), R 11 and R 12 R each independently represents a chain or cyclic hydrocarbon group which may have a substituent. 11 and R 12 may be bonded to each other to form a ring structure. 13 represents a divalent hydrocarbon group. 1 represents O or NH. 14 represents a hydrogen atom or a methyl group. In formula (2), Z 2 R represents a single bond, an ester group, or an amide group. 21 R represents an aromatic group which may have a substituent. 22 represents a hydrogen atom or a methyl group.
[0010] [ka] [In formula (3), n3 represents an integer of 2 to 30. 31 R represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 32 R represents an alkylene group having 1 to 3 carbon atoms. 33 represents a hydrogen atom or a methyl group. 32 may be the same or different.
[0011] In the block copolymer, the A block contains a structural unit represented by formula (1) and a structural unit represented by formula (2). The A block has a structural unit represented by formula (1) having a portion that adsorbs to a colorant, and by introducing a structural unit represented by formula (2), i.e., an aromatic group, into the A block, the dispersion performance of the colorant (particularly carbon particles) is improved and aggregation can be suppressed. Furthermore, by using the block copolymer as a dispersant for a coloring composition that further contains carbon particles, a coating film with excellent jet blackness can be formed. Effect of the Invention
[0012] The block copolymer of the present invention can be used as a dispersant for water-based paints, has high dispersibility for carbon particles, and can suppress aggregation. In addition, by using the block copolymer of the present invention as a dispersant for a coloring composition containing carbon particles, the jet blackness of the coating film can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Block copolymer> The block copolymer of the present invention is characterized in that it has an A block and a B block, the A block contains a structural unit represented by formula (1) and a structural unit represented by formula (2), and the B block contains a structural unit represented by formula (3).
[0014] In the block copolymer, the A block contains a structural unit represented by formula (1) and a structural unit represented by formula (2). The A block has a structural unit represented by formula (1) having a portion that adsorbs to a colorant, and a structural unit represented by formula (2), i.e., an aromatic group, is introduced into the A block. The B block contains a structural unit represented by formula (3) that has high affinity with an aqueous dispersion medium. With this configuration, the block copolymer has high dispersibility of a colorant (especially carbon particles) and can suppress aggregation. In addition, by using the block copolymer as a dispersant for a coloring composition containing carbon particles, a coating film with excellent jet blackness can be formed.
[0015] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.
[0016] In the present invention, the "A block" can be rephrased as the "A segment", and the "B block" can be rephrased as the "B segment". In the present invention, the "vinyl monomer" refers to a monomer having a radically polymerizable carbon-carbon double bond in the molecule. The "structural unit derived from a vinyl monomer" refers to a structural unit in which the radically polymerizable carbon-carbon double bond of a vinyl monomer is polymerized to become a carbon-carbon single bond. "(Meth)acrylic" refers to "at least one of acrylic and methacrylic". "(Meth)acrylate" refers to "at least one of acrylate and methacrylate". "(Meth)acryloyl" refers to "at least one of acryloyl and methacryloyl".
[0017] (A Block) The A block is a block containing a structural unit represented by formula (1) and a structural unit represented by formula (2). By containing the structural unit represented by formula (1) and the structural unit represented by formula (2), the dispersion performance of the colorant (particularly carbon particles) is high, and aggregation can be suppressed.
[0018] (Structural unit represented by formula (1)) The structural unit represented by formula (1) in the A block may be of one type or of two or more types. The structural unit represented by formula (1) adsorbs a colorant.
[0019] [ka] [In formula (1), R 11 and R 12 R each independently represents a chain or cyclic hydrocarbon group which may have a substituent. 11 and R 12 may be bonded to each other to form a ring structure. 13 represents a divalent hydrocarbon group. 1 represents O or NH. 14 represents a hydrogen atom or a methyl group.
[0020] R11 and R 12 Examples of the chain-like hydrocarbon group represented by the formula (I) include linear alkyl groups and branched alkyl groups. The linear alkyl group preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 5 carbon atoms. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-octyl, n-nonyl, n-decyl, and n-lauryl. The branched alkyl group preferably has 3 to 20 carbon atoms, more preferably 3 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, 2-ethylhexyl, neopentyl, and isooctyl.
[0021] R 11 and R 12 Examples of the substituent that the chain hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a benzoyl group (-COC6H5), and a hydroxy group.
[0022] R 11 and R 12 Examples of the cyclic hydrocarbon group represented by the formula (I) include a cyclic alkyl group and an aromatic group, and the cyclic alkyl group and the aromatic group may have a chain portion. The number of carbon atoms of the cyclic alkyl group is preferably 4 to 18, more preferably 6 to 12, and even more preferably 6 to 10. Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. The number of carbon atoms of the aromatic group is preferably 6 to 18, more preferably 6 to 12, and even more preferably 6 to 8. Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a mesityl group. Examples of the cyclic alkyl group having a chain portion and the chain portion of the aromatic group having a chain portion include an alkylene group having 1 to 12 carbon atoms, preferably an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.
[0023] R 11 and R 12 Examples of the substituent that the cyclic hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a chain alkyl group, and a hydroxy group.
[0024] R 11 or R 12 Examples of the cyclic structure formed by bonding with each other include a 5- to 7-membered nitrogen-containing heterocycle or a condensed ring formed by condensing two of these. The nitrogen-containing heterocycle is preferably one that does not have aromaticity, and more preferably a saturated ring. Specific examples include structures represented by the following formulas (1-1), (1-2), and (1-3).
[0025] [ka] [In formulas (1-1), (1-2), and (1-3), R 15 represents an alkyl group having 1 to 6 carbon atoms. l represents an integer of 0 to 5. m represents an integer of 0 to 4. n represents an integer of 0 to 4. * represents a bond. When l is 2 to 5, m is 2 to 4, and n is 2 to 4, multiple R 15 may be the same or different.
[0026] R 13 Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 10 carbon atoms, an alkenylene group having 1 to 10 carbon atoms, and an arenediyl group having 6 to 10 carbon atoms. Among these, an alkylene group having 1 to 10 carbon atoms is preferred. The alkylene group may be either linear or branched, but linear is preferred. The number of carbon atoms in the alkylene group is more preferably 1 to 4. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.
[0027] Specific examples of vinyl monomers forming the structural unit represented by the formula (1) include dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dimethylaminobutyl (meth)acrylate, diethylaminoethyl (meth)acrylate, diethylaminopropyl (meth)acrylate, diethylaminobutyl (meth)acrylate, ethylaminoethyl (meth)acrylate, ethylaminopropyl (meth)acrylate, ethylaminobutyl (meth)acrylate, propylaminoethyl (meth)acrylate, propylaminopropyl (meth)acrylate, propylaminobutyl (meth)acrylate, and dimethylaminopropyl (meth)acrylamide.
[0028] The content of the structural unit represented by the formula (1) is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, in 100% by mass of the A block. If the content of the structural unit represented by the formula (1) is 20% by mass or more, the dispersibility of the coloring material is further improved, and if it is 80% by mass or less, discoloration of the coloring composition due to long-term storage can be suppressed.
[0029] (Structural unit represented by formula (2)) The structural unit represented by formula (2) in the A block may be of one type or of two or more types. The structural unit represented by formula (2) adsorbs a colorant.
[0030] [ka] [In formula (2), Z 2 R represents a single bond, an ester group, or an amide group. 21 R represents an aromatic group which may have a substituent. 22 represents a hydrogen atom or a methyl group.
[0031] Said Z 2represents a single bond, an ester group (-CO-O-) or an amide group (-CO-NH-). The bonding direction of the ester group and the amide group is not particularly limited. The bonding mode of the ester group is C-CO-OR 21 , or CO-CO-R 21 The bonding form of the amide group is C-CO-NH-R 21 , or C-NH-CO-R 21 The Z 2 is preferably a single bond or an ester group.
[0032] R 21 Examples of the aromatic group represented by the formula (I) include an aryl group, and may also have a chain portion such as an alkylaryl group, an aryloxyalkyl group, etc. The aromatic group preferably has 6 to 12 carbon atoms, more preferably 6 to 8 carbon atoms. Specific examples of the aromatic group include a phenyl group, a naphthyl group, a benzyl group, and a phenoxyethyl group. R 21 Examples of the substituent that the aromatic group represented by the formula (I) has include a halogen group, an alkyl group, an alkoxy group, and a hydroxy group.
[0033] Specific examples of vinyl monomers forming the structural unit represented by the formula (2) include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-methoxystyrene, 2-hydroxymethylstyrene, 1-vinylnaphthalene, benzyl(meth)acrylate, phenyl(meth)acrylate, 2-phenylethyl(meth)acrylate, phenoxyethyl(meth)acrylate, N-phenyl(meth)acrylamide, N-benzyl(meth)acrylamide, and N-(2-phenoxyethyl)(meth)acrylamide.
[0034] The content of the structural unit represented by the formula (2) is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, in 100% by mass of the A block. If the content of the structural unit represented by the formula (2) is 20% by mass or more, the dispersibility of the coloring material is further improved, and if it is 80% by mass or less, an increase in the viscosity of the coloring composition can be suppressed.
[0035] In the A block, the mass ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) (formula (1) / formula (2)) is preferably 0.25 or more, more preferably 0.60 or more, even more preferably 1.0 or more, and is preferably 4.0 or less, more preferably 2.0 or less, even more preferably 1.6 or less, and particularly preferably 1.5 or less. When the mass ratio (formula (1) / formula (2)) is 0.25 or more, the viscosity increase of the coloring composition can be suppressed and the influence on other properties can be reduced, and when it is 4.0 or less, discoloration due to long-term storage of the coloring composition can be suppressed and the influence on other properties can be reduced.
[0036] The total content of the structural unit represented by the formula (1) and the structural unit represented by the formula (2) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, in 100% by mass of the A block. If the total content is 70% by mass or more, aggregation of the coloring material is suppressed, and when a black coloring material (particularly carbon particles) is used as the coloring material, a coating film with excellent jet blackness can be formed. The A block may be composed only of the structural unit represented by the formula (1) and the structural unit represented by the formula (2).
[0037] The A block may have a structural unit represented by formula (5). The A block may have only one type of structural unit represented by formula (5), or may have two or more types. If the A block has a structural unit represented by formula (5), strong adsorptivity to the colorant surface can be maintained for a long period of time, and storage stability can be further improved.
[0038] [ka] [In formula (5), R 51 , R 52 and R 53 R each independently represents a chain or cyclic hydrocarbon group which may have a substituent. 51 , R 52 and R 53 Two or more of R may be bonded to each other to form a cyclic structure. 54 represents a divalent hydrocarbon group. 5 represents O or NH. 55 represents a hydrogen atom or a methyl group. - indicates a counter ion.]
[0039] R 51 ~R 53 Examples of the chain-like hydrocarbon group represented by the formula (I) include linear alkyl groups and branched alkyl groups. The linear alkyl group preferably has 1 to 20 carbon atoms, more preferably 2 to 20 carbon atoms, even more preferably 2 to 10 carbon atoms, and particularly preferably 2 to 5 carbon atoms. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-octyl, n-nonyl, n-decyl, and n-lauryl. The branched alkyl group preferably has 3 to 20 carbon atoms, more preferably 3 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, 2-ethylhexyl, neopentyl, and isooctyl.
[0040] R 51 ~R 53 Examples of the substituent that the chain hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a benzoyl group (-COC6H5), and a hydroxy group.
[0041] R 51 ~R 53Examples of the cyclic hydrocarbon group represented by the formula (I) include a cyclic alkyl group and an aromatic group, and the cyclic alkyl group and the aromatic group may have a chain portion. The number of carbon atoms of the cyclic alkyl group is preferably 4 to 18, more preferably 6 to 12, and even more preferably 6 to 10. Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. The number of carbon atoms of the aromatic group is preferably 6 to 18, more preferably 6 to 12, and even more preferably 6 to 8. Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a mesityl group. Examples of the cyclic alkyl group having a chain portion and the chain portion of the aromatic group having a chain portion include an alkylene group having 1 to 12 carbon atoms, preferably an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.
[0042] R 51 ~R 53 Examples of the substituent that the cyclic hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a chain alkyl group, and a hydroxy group.
[0043] R 52 and R 53 Examples of the cyclic structure formed by bonding with each other include 5- to 7-membered nitrogen-containing heterocycles and condensed rings formed by condensing two of these. The nitrogen-containing heterocycle is preferably one that does not have aromaticity, and more preferably a saturated ring. Specific examples include structures represented by the following formulas (5-1), (5-2), and (5-3).
[0044] [ka] [In formulas (5-1), (5-2), and (5-3), R 56 is R 51 R 57 represents an alkyl group having 1 to 6 carbon atoms. l represents an integer of 0 to 5. m represents an integer of 0 to 4. n represents an integer of 0 to 4. * represents a bond. When l is 2 to 5, m is 2 to 4, and n is 2 to 4, multiple R57 may be the same or different.
[0045] R 54 Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 10 carbon atoms, an alkenylene group having 1 to 10 carbon atoms, and an arenediyl group having 6 to 10 carbon atoms. Among these, an alkylene group having 1 to 10 carbon atoms is preferred. The alkylene group may be either linear or branched, but linear is preferred. The number of carbon atoms in the alkylene group is more preferably 1 to 4. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.
[0046] Y - Examples of the anion include a halogen anion, a carboxylate anion, a sulfate anion, a sulfonate anion, a phosphate anion, and a nitroxide anion. Examples of the halogen anion include a fluoro anion, a chloro anion, a bromo anion, and an iodo anion. Examples of the carboxylate anion include alkyl carboxylate anions such as acetate anion and propionate anion; and aromatic carboxylate anions such as benzoate anion. Examples of the sulfate anion include alkyl sulfate anions such as methyl sulfate anion and ethyl sulfate anion; and aromatic sulfate anions such as phenyl sulfate anion and benzyl sulfate anion. Examples of the sulfonate anion include alkylsulfonate anions such as methanesulfonate anion and ethanesulfonate anion; and aromatic sulfonate anions such as benzenesulfonate anion and toluenesulfonate anion. Examples of the phosphate anion include alkyl phosphate anions such as methylphosphonate anion and ethylphosphonate anion; and aromatic phosphate anions such as phenylphosphonate anion and benzylphosphonate anion.
[0047] Specific examples of vinyl monomers forming the structural unit represented by the formula (5) include (meth)acryloyloxyethyl benzyl diethyl ammonium chloride, (meth)acryloyloxypropyl benzyl diethyl ammonium chloride, (meth)acryloyloxybutyl benzyl diethyl ammonium chloride, (meth)acryloyloxyethyl benzyl diethyl ammonium bromide, (meth)acryloyloxypropyl benzyl diethyl ammonium bromide, (meth)acryloyloxybutyl benzyl diethyl ammonium bromide, (meth)acryloyloxyethyl benzyl diethyl ammonium iodide, (meth)acryloyloxypropyl benzyl diethyl ammonium iodide, (meth)acryloyloxybutyl benzyl diethyl ammonium iodide, (meth)acryloyloxyethyl benzyl diethyl ammonium fluoride, (meth)acryloyloxypropyl benzyl diethyl ammonium fluoride, (meth)acryloyloxybutyl benzyl diethyl ammonium fluoride, and the like.
[0048] The A block may have other structural units other than the structural unit represented by formula (1) and the structural unit represented by formula (2). The other structural units that may be included in the A block are not particularly limited as long as they are formed by vinyl monomers that can copolymerize with all of the vinyl monomers that form the structural unit represented by formula (1), the vinyl monomers that form the structural unit represented by formula (2), and the vinyl monomers that form the B block described below. The vinyl monomers that can form the other structural units of the A block may be used alone or in combination of two or more kinds.
[0049] Specific examples of vinyl monomers that can form other structural units of the A block include α-olefins, vinyl monomers containing a heterocycle, vinylamides, vinyl carboxylates, dienes, (meth)acrylic monomers, etc. These vinyl monomers may have a hydroxy group or an epoxy group.
[0050] Examples of the α-olefin include 1-hexene, 1-octene, and 1-decene. Examples of vinyl monomers containing a heterocycle include 2-vinylthiophene, N-methyl-2-vinylpyrrole, 1-vinyl-2-pyrrolidone, 2-vinylpyridine, 4-vinylpyridine, N-phenylmaleimide, N-benzylmaleimide, and N-cyclohexylmaleimide. Examples of the vinyl amide include N-vinylformamide, N-vinylacetamide, and N-vinyl-ε-caprolactam. Examples of the vinyl carboxylate include vinyl acetate, vinyl pivalate, and vinyl benzoate. Examples of dienes include butadiene, isoprene, 4-methyl-1,4-hexadiene, and 7-methyl-1,6-octadiene.
[0051] Examples of the (meth)acrylic monomer include (meth)acrylates having a chain alkyl group (straight-chain alkyl group or branched-chain alkyl group), (meth)acrylates having a cyclic alkyl group, and (meth)acrylates having a polycyclic structure.
[0052] The (meth)acrylate having a linear alkyl group is preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 20, and more preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 10. Examples of the (meth)acrylate having a linear alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate.
[0053] The (meth)acrylate having a branched alkyl group is preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 20, and more preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 10. Examples of the (meth)acrylate having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate.
[0054] The (meth)acrylate having a cyclic alkyl group is preferably a (meth)acrylate having a cyclic alkyl group with a carbon number of 6 to 12. Examples of the cyclic alkyl group include a cyclic alkyl group having a monocyclic structure (e.g., a cycloalkyl group). Specific examples of the (meth)acrylate having a cyclic alkyl group with a monocyclic structure include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, and cyclododecyl (meth)acrylate.
[0055] The (meth)acrylate having a polycyclic structure is preferably a (meth)acrylate having a polycyclic structure with 6 to 12 carbon atoms. Examples of the polycyclic structure include cyclic alkyl groups having a bridged ring structure (e.g., adamantyl group, norbornyl group, isobornyl group). Specific examples of the (meth)acrylate having a polycyclic structure include isobornyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, etc.
[0056] From the viewpoint of maintaining affinity with the colorant, the total content of the structural unit represented by formula (1) and the structural unit represented by formula (5) in the A block is preferably 20 mass% or more, more preferably 30 mass% or more, and even more preferably 40 mass% or more, based on 100 mass% of the A block, and is preferably 80 mass% or less, more preferably 70 mass% or less, and even more preferably 60 mass% or less.
[0057] In addition, it is preferable that the A block does not substantially contain a structural unit derived from a vinyl monomer having an acidic group, i.e., the content of the structural unit derived from a vinyl monomer having an acidic group is preferably 5% by mass or less, and more preferably 2% by mass or less, in 100% by mass of the A block.
[0058] The A block has a content of the structural unit represented by formula (3) described below of less than 10% by mass, preferably less than 3% by mass, more preferably 2% by mass or less, even more preferably 1% by mass or less, particularly preferably 0.1% by mass or less, and most preferably does not contain the structural unit represented by formula (3). The lower the content of the structural unit represented by formula (3) in the A block, the more likely it is that a coating film with excellent jet blackness can be formed when a black colorant (particularly carbon particles) is used as the colorant.
[0059] When two or more types of structural units are contained in the A block, the various structural units contained in the A block may be contained in the A block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the A block in the form of random copolymerization. For example, the A block may be formed of a copolymer of structural units consisting of the a1 block and structural units consisting of the a2 block.
[0060] (Block B) The B block is a block containing a structural unit represented by formula (3). The B block may contain only one type of structural unit represented by formula (3), or may contain two or more types. By containing the structural unit represented by formula (3), high affinity with an aqueous dispersion medium (solvent) can be maintained.
[0061] [ka] [In formula (3), n3 represents an integer of 2 to 30. 31 R represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 32 R represents an alkylene group having 1 to 3 carbon atoms. 33 represents a hydrogen atom or a methyl group. 32 may be the same or different.
[0062] In the formula (1), n3 is 2 or more, preferably 5 or more, and 30 or less, preferably 20 or less, and more preferably 15 or less. R 31 The alkyl group having 1 to 3 carbon atoms represented by the formula (I) may be either linear or branched, but is preferably linear. 31 Specific examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. R 32 The alkylene group having 1 to 3 carbon atoms represented by may be either linear or branched, but is preferably linear. 32 Specific examples of the alkylene group having 1 to 3 carbon atoms represented by the formula (I) include a methylene group, an ethylene group, a trimethylene group, and a propane-1,2-diyl group. 32 is preferably an ethylene group or a trimethylene group.
[0063] The monomer constituting the structural unit represented by the formula (3) includes (meth)acrylates having a polyalkylene glycol structure. The polyalkylene glycol portion may be, for example, a mixture of ethylene oxide and propylene oxide. The (meth)acrylates having a polyalkylene glycol structure include (meth)acrylates having a polyethylene glycol structure such as polyethylene glycol (degree of polymerization = 2-30) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization = 2-30) ethyl ether (meth)acrylate, and polyethylene glycol (degree of polymerization = 2-30) propyl ether (meth)acrylate; and (meth)acrylates having a polypropylene glycol structural unit such as polypropylene glycol (degree of polymerization = 2-30) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization = 2-30) ethyl ether (meth)acrylate, and polypropylene glycol (degree of polymerization = 2-30) propyl ether (meth)acrylate.
[0064] The content of the structural unit represented by the formula (3) is preferably 20% by mass or more, more preferably 35% by mass or more, even more preferably 50% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, in 100% by mass of the B block. If the content of the structural unit represented by the formula (3) is 20% by mass or more, the affinity with the aqueous dispersion medium can be improved, and if it is 80% by mass or less, the affinity with the coating film-forming resin is good.
[0065] The B block preferably further contains a structural unit represented by formula (4). The B block may contain only one type of structural unit represented by formula (4), or may contain two or more types. By containing the structural unit represented by formula (4), affinity with the coating film-forming resin can be improved.
[0066] [ka] [In formula (4), R41 R represents a chain or cyclic hydrocarbon group which may have a substituent. 42 represents a hydrogen atom or a methyl group.
[0067] R 41 Examples of the chain-like hydrocarbon group represented by the formula (I) include linear alkyl groups and branched alkyl groups. The linear alkyl group preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 5 carbon atoms. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-octyl, n-nonyl, n-decyl, and n-lauryl. The branched alkyl group preferably has 3 to 20 carbon atoms, more preferably 3 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, 2-ethylhexyl, neopentyl, and isooctyl.
[0068] R 41 Examples of the substituent that the chain hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a benzoyl group (-COC6H5), and a hydroxy group.
[0069] R 41Examples of the cyclic hydrocarbon group represented by the formula (I) include a cyclic alkyl group and an aromatic group, and the cyclic alkyl group and the aromatic group may have a chain portion. The number of carbon atoms of the cyclic alkyl group is preferably 4 to 18, more preferably 6 to 12, and even more preferably 6 to 10. Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. The number of carbon atoms of the aromatic group is preferably 6 to 18, more preferably 6 to 12, and even more preferably 6 to 8. Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a mesityl group. Examples of the cyclic alkyl group having a chain portion and the chain portion of the aromatic group having a chain portion include an alkylene group having 1 to 12 carbon atoms, preferably an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.
[0070] R 41 Examples of the substituent that the cyclic hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a chain alkyl group, and a hydroxy group.
[0071] Examples of the vinyl monomer that forms the structural unit represented by the formula (4) include (meth)acrylates having a chain alkyl group (straight-chain alkyl group or branched-chain alkyl group), (meth)acrylates having a cyclic alkyl group, (meth)acrylates having an aromatic group, etc. Among these, (meth)acrylates having a chain alkyl group (straight-chain alkyl group or branched-chain alkyl group) and (meth)acrylates having a cyclic alkyl group are preferred.
[0072] When the structural unit represented by formula (4) is contained, its content is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and preferably 80% by mass or less, more preferably 65% by mass or less, and even more preferably 50% by mass or less, in 100% by mass of the B block. If the content of the structural unit represented by formula (4) is 20% by mass or more, the affinity with the coating film-forming resin is further improved, and if it is 80% by mass or less, the affinity with the aqueous dispersion medium is good.
[0073] The B block may be composed of only the structural unit represented by formula (3), or may be composed of only the structural unit represented by formula (3) and the structural unit represented by formula (4), or may contain other structural units. Examples of other structural units include the structural units constituting the A block. Specific examples of vinyl monomers capable of forming other structural units of the B block include those exemplified as specific examples of vinyl monomers capable of forming other structural units of the A block, (meth)acrylates having a hydroxy group, (meth)acrylates having a lactone-modified hydroxy group, (meth)acrylates having an alkoxy group, (meth)acrylates having an oxygen-containing heterocyclic group, (meth)acrylates having an acidic group, (meth)acrylic acid, etc.
[0074] Examples of the (meth)acrylate having a hydroxy group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, etc. Among these, (meth)acrylates having a hydroxyalkyl group having 1 to 5 carbon atoms are more preferred.
[0075] The (meth)acrylate having a lactone-modified hydroxy group includes a (meth)acrylate having a hydroxy group to which a lactone has been added, and preferably a (meth)acrylate having a caprolactone added. The amount of caprolactone added is preferably 1 mol to 10 mol, more preferably 1 mol to 5 mol. The (meth)acrylate having a lactone-modified hydroxy group is preferably a 1 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, a 2 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, a 3 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, a 4 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, a 5 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, a 10 mol adduct of 2-hydroxyethyl (meth)acrylate with caprolactone, and the like.
[0076] Examples of the (meth)acrylate having an alkoxy group include methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate.
[0077] The (meth)acrylate having an oxygen-containing heterocyclic group is preferably a (meth)acrylate having a 4- to 6-membered oxygen-containing heterocyclic group.Specific examples of the (meth)acrylate having an oxygen-containing heterocyclic group include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropaneformal (meth)acrylate, 2-[(2-tetrahydropyranyl)oxy]ethyl (meth)acrylate, and 1,3-dioxane-(meth)acrylate.
[0078] Examples of the acidic group include a carboxy group (-COOH), a sulfonic acid group (-SO3H), a phosphoric acid group (-OPO3H2), a phosphonic acid group (-PO3H2), and a phosphinic acid group (-PO2H2). Examples of the (meth)acrylate having an acidic group include a (meth)acrylate having a carboxy group, a (meth)acrylate having a phosphoric acid group, and a (meth)acrylate having a sulfonic acid group.
[0079] Examples of the (meth)acrylate having a carboxy group include monomers obtained by reacting (meth)acrylates having a hydroxy group such as carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, and 2-(meth)acryloyloxyethyl phthalate with acid anhydrides such as maleic anhydride, succinic anhydride, and phthalic anhydride. Examples of the (meth)acrylate having a sulfonic acid group include ethyl sulfonate (meth)acrylate. Examples of the (meth)acrylate having a phosphoric acid group include 2-(phosphonooxy)ethyl (meth)acrylate.
[0080] The B block has a total content of the structural units represented by formula (1) and (5) of less than 10% by mass, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.1% by mass or less. The lower the total content of the structural units represented by formula (1) and (5) in the B block, the more improved the dispersion performance of the colorant.
[0081] It is preferable that the B block does not have an amino group. In other words, it is preferable that the vinyl monomer constituting the B block does not contain a vinyl monomer having an amino group. If a large amount of amino groups are present in the B block, when the B block is used as a dispersant, the colorant is adsorbed to both the A block and the B block, and the dispersing performance of the colorant is reduced. The content of structural units derived from vinyl monomers having amino groups (including those in which the amino groups are quaternized) in the B block is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less.
[0082] When two or more types of structural units are contained in the B block, the various structural units contained in the B block may be contained in the B block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the B block in the form of random copolymerization. For example, the B block may be formed of a copolymer of structural units consisting of the b1 block and structural units consisting of the b2 block.
[0083] (Block Copolymer) The structure of the block copolymer is preferably a linear block copolymer. The linear block copolymer may have any structure (arrangement), but from the viewpoint of the physical properties of the linear block copolymer or the physical properties of the composition, when the A block is represented as A and the B block is represented as B, the structure (arrangement) of the linear block copolymer is preferably (AB) m Type, (AB) m - Type A, (BA) mIt is preferable that the copolymer has at least one structure selected from the group consisting of -B type (m is an integer of 1 or more, for example, an integer of 1 to 3). Among these, it is preferable that the copolymer is an AB type diblock copolymer from the viewpoint of handling during processing and physical properties of the composition. It is considered that by forming an AB type diblock copolymer, the structural unit represented by formula (1) and the structural unit represented by formula (2) in the A block and the structural unit represented by formula (3) in the B block are localized, and they can efficiently and suitably interact with the colorant and the dispersion medium (solvent). The block copolymer may have other blocks other than the A block and the B block.
[0084] The content of the A block is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the entire block copolymer. The content of the B block is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on 100% by mass of the entire block copolymer. By adjusting the contents of the A block and the B block within the above ranges, the dispersing performance when used as a dispersant is further improved.
[0085] The mass ratio of the A block to the B block in the block copolymer (A block / B block) is preferably 5 / 95 or more, more preferably 10 / 90 or more, even more preferably 20 / 80 or more, and is preferably 60 / 40 or less, more preferably 55 / 45 or less, even more preferably 50 / 50 or less, and particularly preferably 40 / 60 or less. If the mass ratio of the A block to the B block is within the above range, the dispersing performance when used as a dispersant is further improved.
[0086] The total content of the structural unit represented by formula (1) and the structural unit represented by formula (5) in the block copolymer is preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and is preferably 50 mass% or less, more preferably 45 mass% or less, even more preferably 40 mass% or less, and particularly preferably 30 mass% or less.
[0087] The content of the structural unit represented by formula (3) in the block copolymer is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less.
[0088] The molecular weight of the block copolymer is measured by gel permeation chromatography (hereinafter referred to as "GPC"). The weight average molecular weight (Mw) of the block copolymer is preferably 3,000 or more, more preferably 4,000 or more, even more preferably 5,000 or more, particularly preferably 10,000 or more, most preferably 11,000 or more, and is preferably 40,000 or less, more preferably 30,000 or less, even more preferably 25,000 or less, and particularly preferably 20,000 or less. If the weight average molecular weight is within the above range, the dispersion performance when used as a dispersant will be better.
[0089] The molecular weight distribution (PDI) of the block copolymer is preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.6 or less. In the present invention, the molecular weight distribution (PDI) is calculated by (weight average molecular weight (Mw) of the block copolymer) / (number average molecular weight (Mn) of the block copolymer). The smaller the PDI, the narrower the molecular weight distribution width, and the copolymer has a uniform molecular weight, and when the PDI value is 1.0, the molecular weight distribution width is the narrowest. In other words, the lower limit of the PDI is 1.0. When the molecular weight distribution (PDI) of the block copolymer exceeds 2.5, it includes those with low molecular weight and those with high molecular weight.
[0090] From the viewpoint of adsorption to a colorant and dispersibility of a colorant, the amine value of the block copolymer is preferably 10 mgKOH / g or more, more preferably 20 mgKOH / g or more, even more preferably 30 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, even more preferably 120 mgKOH / g or less, and particularly preferably 60 mgKOH / g or less.
[0091] (Method of Producing Block Copolymer) Examples of methods for producing the block copolymer include a method in which an A block is first produced by a polymerization reaction of a vinyl monomer, and then a monomer for a B block is polymerized onto the A block; a method in which a B block is first produced, and then a monomer for an A block is polymerized onto the B block; and a method in which the A block and the B block are produced separately, and then the A block and the B block are coupled together.
[0092] The polymerization method is not particularly limited, but living radical polymerization is preferred. That is, the block copolymer is preferably one polymerized by living radical polymerization. The living radical polymerization method is preferred in that it maintains the simplicity and versatility of conventional radical polymerization methods, while being less susceptible to termination reactions and chain transfer, and grows without being hindered by side reactions that deactivate the growing end, making it easy to precisely control the molecular weight distribution and produce a polymer with a uniform composition.
[0093] Living radical polymerization methods include, depending on the method of stabilizing the polymer growing end, a method using a transition metal catalyst (ATRP method), a method using a sulfur-based reversible chain transfer agent (RAFT method), a method using an organic tellurium compound (TERP method), etc. Among these methods, the TERP method is preferred from the viewpoints of the variety of monomers that can be used, molecular weight control in the polymer region, uniform composition, and coloring.
[0094] The TERP method is a method in which an organic tellurium compound is used as a chain transfer agent to polymerize a radically polymerizable compound (vinyl monomer), and is a method described, for example, in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870.
[0095] Specific polymerization methods of the TERP method include the following (a) to (d). (a) A method of polymerizing a vinyl monomer using an organotellurium compound represented by formula (6): (b) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (6) and an azo-based polymerization initiator. (c) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (6) and an organoditelluride compound represented by formula (7). (d) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (6), an azo-based polymerization initiator, and an organoditelluride compound represented by formula (7).
[0096] [ka] [In the general formula (6), R 61 R represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group. 62 and R 63 R each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 64 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group. In the general formula (7), R 61 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group.]
[0097] Specific examples of the organic tellurium compound represented by the general formula (3) include ethyl-2-methyl-2-n-butyltellanyl-propionate, ethyl-2-n-butyltellanyl-propionate, (2-hydroxyethyl)-2-methyl-methyltellanyl-propionate, and the organic tellurium compounds described in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870. Specific examples of the organic ditelluride compound represented by the general formula (4) include dimethyl ditelluride, dibutyl ditelluride, and the like. The azo polymerization initiator can be any azo polymerization initiator used in normal radical polymerization without any particular limitation. Examples of the azo polymerization initiator include 2,2'-azobis(isobutyronitrile) (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1'-azobis(1-cyclohexanecarbonitrile) (ACHN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70), and the like.
[0098] In the polymerization step, a vinyl monomer and an organic tellurium compound of general formula (6) are mixed in a vessel purged with an inert gas, and for the purpose of promoting the reaction and controlling the molecular weight and molecular weight distribution depending on the type of vinyl monomer, an azo polymerization initiator and / or an organic ditelluride compound of general formula (7) are further mixed. Examples of the inert gas include nitrogen, argon, and helium. Argon and nitrogen are preferable. The amount of the vinyl monomer used in the above (a), (b), (c), and (d) may be appropriately adjusted depending on the physical properties of the desired copolymer.
[0099] The polymerization reaction can be carried out without a solvent, but may be carried out by stirring the mixture using an aprotic solvent or a protic solvent generally used in radical polymerization. Examples of aprotic solvents that can be used include anisole, benzene, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, and tetrahydrofuran (THF). Examples of protic solvents include water, methanol, and 1-methoxy-2-propanol. The solvent may be used alone or in combination of two or more. The amount of the solvent used may be appropriately adjusted, and is preferably 0.01 ml to 50 ml per 1 g of vinyl monomer. The reaction temperature and reaction time may be appropriately adjusted depending on the molecular weight or molecular weight distribution of the resulting copolymer, but the mixture is usually stirred at 0°C to 150°C for 1 minute to 100 hours. After the polymerization reaction is completed, the solvent used and the remaining vinyl monomer are removed from the resulting reaction mixture by a conventional separation and purification means, and the target copolymer can be separated.
[0100] The growing end of the copolymer obtained by the polymerization reaction is -TeR derived from the tellurium compound. 61 (In the formula, R 61 is the same as above), and is deactivated by handling in air after the polymerization reaction is completed, but tellurium atoms may remain. Since copolymers with tellurium atoms remaining at the terminals are colored and have poor thermal stability, it is preferable to remove the tellurium atoms. Methods for removing tellurium atoms include radical reduction methods, adsorption methods using activated carbon, and adsorption of metals using ion exchange resins, and these methods can also be used in combination. The other end of the copolymer obtained by the polymerization reaction (the end opposite to the growing end) is formed of -CR derived from the tellurium compound. 62 R 63 R 64 (In the formula, R 62 , R 63 and R 64 is R in Eq. (6). 62 , R 63 and R 64 (same as above.)
[0101] When the tertiary amine group of the structural unit represented by formula (1) is quaternized, examples of the quaternizing agent include alkyl halides such as methyl chloride; aralkyl halides such as benzyl chloride; and dialkyl sulfates such as dimethyl sulfate. As a method for quaternizing a part of the tertiary amine structure of the structural unit represented by formula (1) in the polymer, a method of contacting the polymer with a quaternizing agent can be mentioned. Specifically, a method of polymerizing a monomer composition containing a vinyl monomer capable of forming the structural unit represented by formula (1), adding a quaternizing agent to this reaction liquid, and stirring the mixture can be mentioned. The temperature of the reaction liquid to which the quaternizing agent is added is preferably 55°C to 65°C, and the stirring time is preferably 5 hours to 20 hours.
[0102] <Dispersant> The dispersant of the present invention contains the block copolymer. The dispersant contains the block copolymer as a main component (50% by mass or more), preferably contains the block copolymer in an amount of 75% by mass or more, and more preferably is composed only of the block copolymer. The block copolymer, for example, is considered to exert an effect of enhancing the dispersibility of the colorant by a tertiary amino group in its structure (A block) being strongly bonded to an acidic colorant or an acidic group of a colorant treated with an acidic group-containing dye derivative, and the B block being adsorbed to the colorant. That is, the dispersant of the present invention is a component that disperses the colorant well by this action, so that the type of colorant to be dispersed is not particularly limited.
[0103] The block copolymer has an aromatic group in addition to a tertiary amino group in the A block. Therefore, the dispersant has particularly high dispersing performance for carbon black, which is a black coloring material, and can suppress aggregation. The dispersant also exhibits excellent dispersing performance for carbon particles such as carbon nanotubes and graphene, as well as carbon black. Therefore, the dispersant of the present invention can be suitably used as a dispersant for carbon particles.
[0104] <Coloring composition> The colored composition of the present invention contains a dispersant (block copolymer), a colorant, and an aqueous dispersion medium.
[0105] (Coloring material) The coloring material is not particularly limited, and pigments and dyes that have been used as coloring materials for conventional paints can be used, but pigments are preferred from the viewpoint of light resistance and heat resistance. Examples of pigments include red pigments, yellow pigments, orange pigments, blue pigments, green pigments, purple pigments, black pigments, and other pigments of various colors. The structure of the pigment includes organic pigments such as azo pigments such as monoazo pigments, diazo pigments, and condensed diazo pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, isoindolinone pigments, isoindoline pigments, quinacridone pigments, indigo pigments, thioindigo pigments, quinophthalone pigments, dioxazine pigments, anthraquinone pigments, perylene pigments, and polycyclic pigments such as perinone pigments; carbon black, graphite, titanium black, and inorganic pigments such as metal oxides, composite oxides, metal sulfides, metal sulfates, and metal carbonates of copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, and silver. The coloring composition may contain only one type of pigment, or may contain multiple types of pigments.
[0106] The block copolymer exhibits excellent dispersibility, particularly with respect to carbon particles, and therefore carbon particles are preferred as the colorant, and the coloring composition preferably contains a dispersant (block copolymer), carbon particles, and an aqueous dispersion medium.
[0107] Examples of the carbon particles include carbon black such as furnace black, channel black, acetylene black, thermal black, lamp black, and bone black; carbon nanotubes; carbon nanofibers; fullerene; natural graphite; and graphite, with carbon black being preferred. The primary particle size of the carbon particles is not particularly limited, but is preferably 5 nm to 100 nm.
[0108] The specific surface area of the carbon particles is 300 m 2 / g~1300m 2 / g is preferred, and 400m 2 / g~800m 2 The specific surface area is measured in accordance with JIS K 6217-3 (2001).
[0109] The DBP (dibutyl phthalate) oil absorption of the carbon particles is preferably 50 ml / 100 g to 150 ml / 100 g, and more preferably 80 ml / 100 g to 120 ml / 100 g. The DBP oil absorption is measured according to JIS K 6217-4 (2017).
[0110] The carbon particles may be subjected to an oxidation treatment on the surface. By performing the oxidation treatment, a carboxy group or a phenolic hydroxy group can be imparted to the surface of the carbon particles. The oxidation treatment can be performed by treating the surface of the carbon particles with ozone, nitric acid, or the like. The carbon particles having a carboxy group or a phenolic hydroxy group imparted to the surface have an acidic pH.
[0111] The carbon particles preferably have a pH of 3 to 9, and more preferably 5 to 9, when 1 g of the carbon particles is dispersed in 100 ml of water (25° C.).
[0112] The upper limit of the content of the coloring material in the coloring composition is usually 80% by mass, preferably 65% by mass, and more preferably 50% by mass, based on the total solid content of the coloring composition. The lower limit of the content of the coloring material in the coloring composition is usually 5% by mass, preferably 20% by mass, and more preferably 30% by mass, based on the total solid content of the coloring composition. Here, the solid content refers to components other than the dispersion medium described below.
[0113] The content of the dispersant component (block copolymer) relative to the colorant in the coloring composition is preferably 5 parts by mass to 200 parts by mass, more preferably 10 parts by mass to 100 parts by mass, and further preferably 10 parts by mass to 80 parts by mass, relative to 100 parts by mass of the colorant.
[0114] (aqueous dispersion medium) The aqueous dispersion medium may be water or an aqueous solvent (a solvent miscible with water). The aqueous solvent may be alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, etc.; polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, triethylene glycol, diethylene glycol, polyethylene glycol, polypropylene glycol, glycerin, etc.; ethers such as tetrahydrofuran, dioxane, ethylene glycol methyl ether, ethylene glycol ethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, triethylene glycol, monomethyl ether, monoethyl ether, etc.; ketones such as acetone, methyl ethyl ketone, isobutyl ketone, etc.; amides such as dimethylformaldehyde, dimethylacetamide, etc. Among these, alcohols and glycols are preferred. The aqueous solvent may be used alone or in combination of two or more.
[0115] The content of the aqueous dispersion medium in the coloring composition is not particularly limited and can be adjusted appropriately.The upper limit of the content of the aqueous dispersion medium in the coloring composition is usually 99% by mass.In addition, the lower limit of the content of the aqueous dispersion medium in the coloring composition is usually 60% by mass, preferably 80% by mass, in consideration of the viscosity suitable for application of the coloring composition.
[0116] The coloring composition may further contain additives such as a resin for forming a coating film, a surfactant, a leveling agent, a filler, an ultraviolet absorber, an antioxidant, a preservative, an antifungal agent, a viscosity adjuster, a pH adjuster, an antifoaming agent, and a crosslinking agent, depending on the application. In addition, when conductive carbon particles are used in the coloring composition, it can be used for an electrode. In this case, the coloring composition may contain additives such as a resin for forming an electrode, an electrode active material, a surfactant, a film-forming assistant, a leveling agent, a preservative, an antifungal agent, a viscosity adjuster, a pH adjuster, an antifoaming agent, and a crosslinking agent.
[0117] (Resin for coating film formation) The coating film-forming resin is a component that becomes the main body of the film when a coating film is formed using the coloring composition. The coating film-forming resin is not particularly limited, and any resin that has been used in conventional paints can be used. Examples of the coating film-forming resin include thermosetting resins, thermoplastic resins, and polymerizable compounds (polymerizable resins, monomers having one polymerizable unsaturated bond in the molecule, monomers having two or more polymerizable unsaturated bonds in the molecule, oligomers, etc.). The coating film-forming resins can be used alone or in combination of two or more kinds. When the coating film-forming resin is blended in the coloring composition, the content of the coating film-forming resin is preferably 60% by mass to 95% by mass of the total solid content of the coloring composition.
[0118] (thermosetting resin, thermoplastic resin) Examples of the thermosetting resin and thermoplastic resin include butyral resin, styrene-maleic acid copolymer, chlorinated polyethylene resin, chlorinated polypropylene resin, vinyl chloride resin, vinyl chloride-vinyl acetate copolymer, vinyl acetate resin, urethane resin, phenol resin, polyester resin, acrylic resin, alkyd resin, styrene resin, styrene acrylic resin, polyamide resin, rubber resin, cyclized rubber, epoxy resin, cellulose, polybutadiene, polyimide resin, benzoguanamine resin, melamine resin, urea resin, silicone resin, and fluororesin.
[0119] (polymerizable compound) As the polymerizable resin as the polymerizable compound, a resin in which a crosslinkable group such as a (meth)acrylic compound or cinnamic acid is introduced into a linear polymer having a reactive substituent such as a hydroxy group, a carboxy group, an amino group, etc., via an isocyanate group, an aldehyde group, an epoxy group, etc. is used. Polymers in which a linear polymer containing an acid anhydride such as a styrene-maleic anhydride copolymer or an α-olefin-maleic anhydride copolymer is half-esterified with a (meth)acrylic compound having a hydroxy group such as a hydroxyalkyl (meth)acrylate are also used.
[0120] (Surfactant) The surfactant may, for example, be a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. Examples of the nonionic surfactant include a fluorine-based surfactant, a silicone-based surfactant, and a polyoxyethylene-based surfactant. Examples of anionic surfactants include alkyl sulfonates, alkyl benzene sulfonates, alkyl naphthalene sulfonates, polyoxyethylene alkyl ether sulfonates, alkyl sulfates, alkyl sulfate ester salts, higher alcohol sulfate ester salts, aliphatic alcohol sulfate ester salts, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkyl phenyl ether sulfates, alkyl phosphate ester salts, polyoxyethylene alkyl ether phosphates, polyoxyethylene alkyl phenyl ether phosphates, and special polymer surfactants. Examples of the cationic surfactant include quaternary ammonium salts, imidazoline derivatives, and alkylamine salts. Examples of the amphoteric surfactant include betaine-type compounds, imidazolium salts, imidazolines, and amino acids.
[0121] (Leveling agent) Examples of the leveling agent include silicone-based agents and fluorine-based agents. Examples of silicone-based agents include dimethyl silicone oil, methylphenyl silicone oil, alkyl-modified silicone, alkoxy-modified silicone, oxyalkyl-modified silicone, glycol-modified silicone, polyether-modified silicone, polyether-modified silicone, and fatty acid ester-modified silicone. Examples of fluorine-based agents include fluorocarbon compounds and fluorine silicone. These agents can be used alone or in combination of two or more. (filling material) Examples of the filler include silicon dioxide, alumina, zinc oxide, potassium titanate fiber, aluminum flakes, stainless steel powder, tin powder, gold powder, metal-plated glass powder, titanic mica, calcium carbonate, barium sulfate, barium carbonate, kaolin, baryta, clay, other metal oxides, and composite metal oxides. These can be used alone or in combination of two or more kinds to prevent a decrease in viscosity or poor gloss.
[0122] (Resin for electrode formation) The electrode-forming resin is used to bond particles of active materials or conductive carbon materials, or to bond conductive carbon particles to a current collector. Examples of the electrode-forming resin include acrylic resins, polyurethane resins, polyester resins, phenolic resins, epoxy resins, phenoxy resins, urea resins, melamine resins, alkyd resins, formaldehyde resins, silicone resins, fluororesins, cellulose resins such as carboxymethylcellulose, synthetic rubbers such as styrene butadiene rubber and fluororubber, conductive resins such as polyaniline and polyacetylene, and polymer compounds containing fluorine atoms such as polyvinylidene fluoride, polyvinyl fluoride, and tetrafluoroethylene. Modified products, mixtures, or copolymers of these resins can also be used. These resins can be used alone or in combination.
[0123] <Method of producing colored composition> The coloring composition can be prepared by mixing a coloring material, a dispersant (block copolymer), an aqueous dispersion medium, and, if necessary, a resin for forming a coating film and other compounding agents. For mixing, a mixer / disperser such as a paint shaker, a bead mill, a ball mill, a dissolver, or a kneader can be used. The coloring composition is preferably filtered after mixing. The coloring composition can be an automobile coating composition.
[0124] The coloring composition can be applied (coated) to a substrate such as a stainless steel plate or an aluminum plate by, for example, roll coating, spin coating, flow coating, slot die coating, spray coating, dip coating, electrostatic coating, brush coating, powder coating, or the like. Thereafter, the coating is heated as necessary to evaporate the solvent, and the coating is dried and cured. At this time, heating or irradiation with ultraviolet rays or the like may be performed. The coating obtained by applying the coloring composition may be further coated with one or more layers of a top clear coating to form a top clear coating. The top clear coating is a liquid coating that forms a colorless or colored transparent coating film, which is mainly composed of a resin component and a solvent, and further contains other coating additives as necessary. EXAMPLES
[0125] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention. The polymerization rate, weight average molecular weight (Mw), molecular weight distribution (PDI) and amine value of the block copolymer, and the L value and appearance of the coating film prepared using the coloring composition (black paint) were evaluated according to the following method.
[0126] The meanings of the abbreviations are as follows: St: styrene BzA: benzyl acrylate PhEA: 2-phenylethyl acrylate DMAEMA: Dimethylaminoethyl methacrylate BA: Butyl acrylate M9EGA: methoxypolyethylene glycol monoacrylate (number of moles of ethylene oxide added: 9) (NOF Corporation, Blenmer (registered trademark) AME-400) BTEE: Ethyl 2-methyl-2-n-butyltellanyl-propionate AIBN: 2,2'-azobis(isobutyronitrile) MP: 1-methoxy-2-propanol
[0127] (Polymerization rate) Using a nuclear magnetic resonance (NMR) measuring device (Bruker Biospin, model: AVANCE500 (frequency 500 MHz)), 1 H-NMR was measured (solvent: CDCl3, internal standard: TMS). For the obtained NMR spectrum, the integral ratio of the peaks of the vinyl group derived from the monomer and the ester side chain derived from the polymer was obtained, and the polymerization rate of the monomer was calculated.
[0128] (Weight average molecular weight (Mw) and molecular weight distribution (PDI)) The molecular weight was determined by gel permeation chromatography (GPC) using a high performance liquid chromatograph (Tosoh, model HLC-8320). A column of SHODEX KF-603 (φ6mm×150mm) (SHODEX) was used, and a 10mmol / L lithium bromide / 10mmol / L acetic acid / N-methyl-2-pyrrolidone solution was used as the mobile phase, and a differential refractometer was used as the detector. The measurement conditions were: column temperature 40°C, sample concentration 20mg / mL, sample injection volume 10μm, and flow rate 0.2mL / min. A calibration curve was created using polystyrene (molecular weight 70,500, 37,900, 19,920, 10,200, 4,290, 2,630, 1,150) as the standard substance, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured. From this measurement, the molecular weight distribution (PDI=Mw / Mn) was calculated.
[0129] (amine value) The amine value represents the mass of potassium hydroxide (KOH) equivalent to the basic component per 1 g of solid content. The measurement sample was dissolved in tetrahydrofuran, and the resulting solution was neutralized with a 0.1 mol / L hydrochloric acid / 2-propanol solution using a potentiometric titrator (product name: GT-06, manufactured by Mitsubishi Chemical Corporation). The inflection point of the titration pH curve was used as the titration end point, and the amine value (B) was calculated using the following formula. B=56.11×Vs×0.1×f / w B: Amine value (mgKOH / g) Vs: Amount of 0.1 mol / L hydrochloric acid / 2-propanol solution required for titration (mL) f: Potency of 0.1 mol / L hydrochloric acid (2-propanol) w: Mass of the measurement sample (g) (solid content equivalent)
[0130] (viscosity) The viscosity was measured using an E-type viscometer (product name: TVE-25L, manufactured by Toki Sangyo Co., Ltd.) with a rotor of 01 or 06 at 23° C. and a rotor rotation speed of 60 rpm.
[0131] (Coating film evaluation) The black paint was applied to a stainless steel plate using a bar coater (#20) and dried at 60°C for 10 minutes to form a coating, and a test specimen was prepared. The L value of the coating surface of the obtained test piece was measured by removing regular reflected light using an L value measuring device (Model CM-2600d, manufactured by Konica Minolta Japan, Inc.) The coating was also visually observed and evaluated according to the following criteria. ◯: The coating is a vivid jet black. △: The coating is slightly cloudy. ×: The coating is cloudy and lacks brightness.
[0132] <Production of block copolymer> (Block Copolymer No. 1) Block copolymer No. 1 was produced by first producing the A block and then polymerizing the B block monomer onto the A block. A reaction vessel equipped with a nitrogen inlet tube and a stirrer was replaced with nitrogen in advance, and 7.5 g of MP, 0.45 g of BTEE, 0.14 g of AIBN, 3.8 g of St, and 4.2 g of DMAEMA were charged into the reaction vessel and reacted at 59° C. for 26 hours. The polymerization rate was 98%.
[0133] To this reaction solution, 20.0 g of MP, 0.12 g of AIBN, 9.0 g of BA, and 18.0 g of M9EGA, which had been previously replaced with nitrogen, were added and reacted at 59°C for 24 hours. The polymerization rate was 96%. The monomers of the first polymerization stage remaining in the reaction solution were also polymerized, and the polymerization rate of the monomers of the first polymerization stage remaining in these reaction solutions was 100%.
[0134] After the reaction was completed, the reaction solution was poured into stirred n-heptane. The precipitated polymer was filtered by suction and dried to obtain block copolymer No. 1. The obtained block copolymer No. 1 had an Mw of 18,358, a PDI of 1.48, and an amine value of 44 mgKOH / g. The composition of block copolymer No. 1 is shown in Table 2. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0135] (Block Copolymer No. 2) Block copolymer No. 2 was produced by first producing the B block and then polymerizing the monomers for the A block onto the B block. A reaction vessel equipped with a nitrogen inlet tube and a stirrer was replaced with nitrogen in advance, and 6.7 g of PMA, 0.45 g of BTEE, 0.03 g of AIBN, 9.0 g of BA, and 18.0 g of M9EGA were charged into the reaction vessel and reacted at 60° C. for 25 hours. The polymerization rate was 95.2%.
[0136] To this reaction solution, 3.1g of PMA, 0.05g of AIBN, 5.3g of BzA, and 7.1g of DMAEMA, which had been previously replaced with nitrogen, were added and reacted at 60°C for 85 hours. The polymerization rate was 88.6%. The monomers of the first polymerization step remaining in the reaction solution were also polymerized, and the polymerization rate of the monomers of the first polymerization step remaining in these reaction solutions was 100%.
[0137] After the reaction was completed, the reaction solution was poured into stirred n-heptane. The precipitated polymer was filtered by suction and dried to obtain block copolymer No. 2. The obtained block copolymer No. 2 had an Mw of 28,822, a PDI of 1.28, and an amine value of 72 mgKOH / g. Table 2 shows the composition of block copolymer No. 2. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0138] (Block copolymers No. 3-5) Block copolymer No. 3 was prepared in the same manner as block copolymer No. 2. Block copolymers No. 4 and No. 5 were prepared in the same manner as block copolymer No. 1. Table 1 shows the monomers, organotellurium compounds, azo-based polymerization initiators, solvents, reaction conditions, and polymerization rates used. Table 2 shows the composition, Mw, PDI, and amine value of each block copolymer. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.
[0139] [Table 1]
[0140] [Table 2]
[0141] <Production of Carbon Particle Dispersion> (Carbon particle dispersion No. 1-6) Carbon particle dispersions were prepared using the block copolymers Nos. 1, 4, and 5 obtained above as dispersants. Specifically, each component was placed in a 50 mL mayonnaise bottle so as to obtain the composition shown in Table 3, and 66 g of zirconia beads (φ0.3 mm) was further added, followed by stirring for 10 hours using a disperser (manufactured by O-Well, SKANDEX DISPERSER BA-S20). After stirring was completed, the beads were filtered off to prepare carbon particle dispersions No. 1 to 6. It was visually confirmed that the carbon particles in the obtained carbon particle dispersions No. 1 to 6 had good dispersibility.
[0142] (Carbon particle dispersion No. 7-9) Carbon particle dispersions were prepared using the block copolymers Nos. 1 to 3 obtained above as dispersants. Specifically, each component was added to a 50 mL mayonnaise bottle so as to obtain the composition shown in Table 3, and 66 g of zirconia beads (φ0.3 mm) was added and stirred for 10 hours using a disperser (Paint Shaker PC-1972, manufactured by Asada Iron Works). After stirring was completed, the beads were filtered off to prepare carbon particle dispersions No. 7 to 9. It was visually confirmed that the carbon particles in the obtained carbon particle dispersions No. 7 to 9 had good dispersibility. The viscosity measurement results of the obtained carbon particle dispersions No. 7 to 9 are also shown in Table 3.
[0143] [Table 3] EMPEROR® 2000: manufactured by Cabot Corporation (carbon black, pH 6 to 9) Raven5000: BIRLA CARBON (carbon black, pH 5-9)
[0144] <Production of black paint> (Black Paint No. 1-9) A black paint was prepared by mixing the carbon particle dispersion obtained above, acrylic resin, melamine resin, and solvent according to the composition shown in Table 4. Specifically, the carbon particle dispersion, acrylic resin dispersion, and melamine resin solution were charged into a container to obtain a black paint. A coating film was formed using the obtained black paint, and was evaluated.
[0145] [Table 4] Acrylic resin dispersion: Watersol (registered trademark) ACD-2001 (non-volatile content: 40% by mass, solvent: water, propylene glycol-n-butyl ether), manufactured by DIC Corporation Melamine resin solution: Watersol S-695 (non-volatile content: 66% by mass, solvent: water, methanol) manufactured by DIC Corporation
[0146] Black paint Nos. 1, 2 and 7 to 9 contain a block copolymer having an A block containing a structural unit represented by formula (1) and a structural unit represented by formula (2) and a B block containing a structural unit represented by formula (3) as a dispersant. These black paints Nos. 1, 2 and 7 to 9 had a good dispersion state of carbon particles. Furthermore, the coating films prepared using these black paints Nos. 1, 2 and 7 to 9 had a low L value and good appearance.
[0147] Black paint No. 3 and 4 contain block copolymer No. 4 as a dispersant. Aggregation of carbon particles was observed in black paint No. 3. The coating film made using this black paint No. 3 was cloudy and lacked brightness. Since aggregation of carbon particles was observed in black paint No. 3, the L value of the coating film was not measured. Although the carbon particles in black paint No. 4 were well dispersed, the coating film made using this paint was cloudy and had a high L value. This is thought to be due to differences in the association state of the carbon particles.
[0148] Black paint No. 5 and 6 contain block copolymer No. 5 as a dispersant. Although the dispersion state of carbon particles in black paint No. 5 and 6 is good, the coating film made using these black paints No. 5 and 6 was cloudy and had a high L value. This is thought to be due to the difference in the association state of the carbon particles. [Industrial Applicability]
[0149] The block copolymer of the present invention can be used as a dispersant for a coloring composition containing a colorant and an aqueous dispersion medium, and is particularly useful as a dispersant for carbon particles. The coloring composition of the present invention is useful for automobile paints, etc., because the coating film formed has high jet blackness.
Claims
1. Having A block and B block, The A block contains a structural unit represented by formula (1) and a structural unit represented by formula (2), and the B block contains a structural unit represented by formula (3), a mass ratio of the A block to the B block (A block / B block) in the block copolymer is 5 / 95 to 60 / 40; the content of the structural unit represented by the formula (1) is 20% by mass to 60% by mass in 100% by mass of the A block, the content of the structural unit represented by the formula (2) is 20% by mass to 80% by mass in 100% by mass of the A block, the content of the structural unit represented by the formula (3) is 20% by mass to 80% by mass in 100% by mass of the B block, the total content of the structural unit represented by the formula (1) and the structural unit represented by the formula (2) is 80% by mass or more in 100% by mass of the A block, A block copolymer, characterized in that the total content of the structural unit represented by the formula (1) and the structural unit represented by the formula (5) is 20% by mass to 60% by mass in 100% by mass of the A block. 【Chemistry 1】 [In formula (1), R 11 and R 12 R each independently represents a chain or cyclic hydrocarbon group which may have a substituent. 11 and R 12 may be bonded to each other to form a cyclic structure. 13 represents a divalent hydrocarbon group. 1 represents O or NH. 14 represents a hydrogen atom or a methyl group. In formula (2), Z 2 represents a single bond, an ester group, or an amide group. 21 R represents an aromatic group which may have a halogen group. 22 represents a hydrogen atom or a methyl group. 【Chemistry 2】 [In formula (3), n3 represents an integer of 2 to 30. 31 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 32 represents an alkylene group having 1 to 3 carbon atoms. 33 represents a hydrogen atom or a methyl group. 32 may be the same or different. 【Chemistry 3】 [In formula (5), R 51 , R 52 and R 53 each independently represent a chain or cyclic hydrocarbon group which may have a substituent. Two or more of R 51 , R 52 and R 53 may be bonded to each other to form a cyclic structure. R 54 represents a divalent hydrocarbon group. Z 5 represents O or NH. R 55 represents a hydrogen atom or a methyl group. Y - represents a counter ion.]
2. The block copolymer according to claim 1, wherein in the A block, a mass ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) (formula (1) / formula (2)) is 0.25 to 4.
0.
3. The block copolymer according to claim 1, wherein the content of the structural unit represented by the formula (3) is less than 10% by mass in 100% by mass of the A block.
4. The block copolymer according to any one of claims 1 to 3, wherein the total content of the structural unit represented by the formula (1) and the structural unit represented by the formula (5) is less than 10 mass% in 100 mass% of the B block.
5. The block copolymer according to any one of claims 1 to 4, having an amine value of 10 mg KOH / g to 200 mg KOH / g.
6. The block copolymer according to any one of claims 1 to 5, wherein the B block further contains a structural unit represented by formula (4). 【Chemistry 4】 [In formula (4), R 41 R represents a chain or cyclic hydrocarbon group which may have a substituent. 42 represents a hydrogen atom or a methyl group.
7. The block copolymer according to any one of claims 1 to 6, wherein the molecular weight distribution (PDI) of the block copolymer is 2.5 or less.
8. The block copolymer according to any one of claims 1 to 7, wherein the weight average molecular weight (Mw) of the block copolymer is 3,000 to 40,000.
9. A dispersant comprising the block copolymer according to any one of claims 1 to 8.
10. A coloring composition comprising the dispersant according to claim 9, carbon particles, and an aqueous dispersion medium.
11. 11. The coloring composition according to claim 10, wherein the carbon particles are carbon black.
12. The colored composition according to claim 10 or 11, further comprising a coating film-forming resin.
13. The colored composition according to any one of claims 10 to 12, which is an automotive coating composition.
Citation Information
Patent Citations
High jetness carbon black dispersion, process for producing the same, and coating material composition using the high jetness carbon black dispersion
JP2008285632A
Pigment coloring agent composition, coloring agent for color filter, polymer dispersant and production method of the polymer dispersant
JP2013203887A
Pigment dispersing resin
JP2013221131A
Water paint composition
JP2014005399A
Colorant dispersion
JP2014058672A