Manufacturing method and manufacturing device for thermoplastic resin composite
By impregnating fibers with a thermoplastic resin forming composition and polymerizing at a temperature below the glass transition temperature, the method addresses the challenges of shape maintenance and efficiency in producing high-fiber content thermoplastic resin composites, enabling stable and continuous manufacturing.
Patent Information
- Application Number
- JP2020192094
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-11-18
AI Technical Summary
Existing methods for producing thermoplastic resin composites face challenges in efficiently manufacturing high-fiber content composites due to the difficulty in impregnating thermoplastic resins with fibers and maintaining the shape of the composite during polymerization, as thermoplastic resins soften and lose shape easily.
A method and apparatus that impregnate fibers with a thermoplastic resin forming composition containing an active hydrogen component and a diisocyanate component, polymerizing the resin at a temperature lower than the glass transition temperature of the resin, allowing the composite to be drawn in a glass state without cooling, maintaining its shape and enabling continuous pultrusion molding.
The method allows for efficient production of high-quality thermoplastic resin composites with maintained shape and improved manufacturing efficiency, enabling stable and continuous production without the need for cooling processes, and facilitates reprocessing and reuse.
Smart Images

Figure 0007569207000002 
Figure 0007569207000003 
Figure 0007569207000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for producing a thermoplastic resin composite containing a thermoplastic resin and fibers. [Background technology]
[0002] Fiber-reinforced plastics, which are composites containing resin and fiber, have excellent specific strength and rigidity and are used in a wide range of fields, including the automotive industry, as a substitute for metal materials to reduce weight.
[0003] As a method for producing fiber-reinforced plastics, for example, Patent Document 1 discloses a pultrusion method as a continuous production method for a thermosetting resin composite having a thermosetting resin as a matrix. Patent Document 2 discloses a method for impregnating fibers with a polyisocyanurate reaction mixture obtained by mixing a polyol component and a polyisocyanate component, and passing the polyisocyanurate reaction mixture through a heated mold to cure the polyisocyanurate reaction mixture, thereby pultrusion molding a fiber-reinforced polyisocyanurate matrix composite.
[0004] Thermosetting resins can be impregnated into fibers while still in the unpolymerized monomer stage, which is liquid at room temperature and does not have a high viscosity, so even with a high fiber content, the resin can easily be impregnated into fibers, and continuous molding can be performed with simple equipment. However, thermosetting resins have the disadvantage that they cannot be reprocessed or reused because they form a three-dimensional cross-linked structure after the polymerization reaction (hardening) and cannot be remelted after being impregnated with fibers and hardened.
[0005] On the other hand, thermoplastic resin composites, which are fiber-reinforced plastics with a thermoplastic resin matrix, can be reprocessed and reused because the base thermoplastic resin remelts and softens when heated. However, thermoplastic resins are generally supplied in the form of polymers such as pellets or films as raw materials for molding, and therefore have a much higher viscosity when melted to impregnate fibers than thermosetting resins. For this reason, it is difficult to continuously produce thermoplastic resin composites with a high fiber content and good impregnation.
[0006] In a known method for producing a thermoplastic resin composite, a fiber impregnated with a monomer is passed through a heated mold to simultaneously polymerize the monomer and mold the resulting resin to obtain a thermoplastic resin composite. However, the thermoplastic resin composite immediately after being pulled out of the mold has a problem in that it is prone to losing its shape because the thermoplastic resin matrix is soft and rubber-like. Therefore, a cooling process is required, for example, to harden the resin.
[0007] As a continuous production method for a thermoplastic resin composite, Patent Document 3 discloses a method in which fibers are impregnated with a polymerizable lactam mixture, the impregnated fibers are passed through a heated mold, the polymerization of the lactam monomer and the molding of the thermoplastic polyamide resin obtained thereby are carried out simultaneously, and the fibers are continuously pulled out of the mold by a pulling device.
[0008] Incidentally, Patent Document 4 discloses a two-component curing composition that has an active hydrogen component containing an aromatic diamine having an alkylthio group, and a diisocyanate component containing at least one diisocyanate selected from the group consisting of aliphatic diisocyanates, alicyclic diisocyanates, and modified products thereof, as a composition used to form a matrix resin of a thermoplastic resin composite. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2004-074427 A [Patent Document 2] Special Publication No. 2002-530445 [Patent Document 3] JP 2017-007266 A [Patent Document 4] Patent No. 6580774 Summary of the Invention [Problem to be solved by the invention]
[0010] It has been known that a thermoplastic resin composite can be produced by impregnating a fiber with a monomer of a thermoplastic resin, molding the resin while polymerizing, and continuously pultrusion as described above. However, it has not been known to polymerize the thermoplastic resin at a temperature lower than the glass transition temperature thereof and pultrusion mold the resin in a glassy state, making it difficult to efficiently produce a thermoplastic resin composite.
[0011] In view of the above, an object of an embodiment of the present invention is to provide a manufacturing method capable of efficiently manufacturing a thermoplastic resin composite by pultrusion molding. [Means for solving the problem]
[0012] A first embodiment of the present invention is a method for producing a thermoplastic resin composite containing a thermoplastic resin and a fiber, comprising the steps of: continuously impregnating a fiber with a thermoplastic resin forming composition containing an active hydrogen component and a diisocyanate component; passing the fiber through a hot molding section to polymerize the thermoplastic resin forming composition and mold a thermoplastic resin composite containing the thermoplastic resin obtained by the polymerization; and continuously pulling out the thermoplastic resin composite from the hot molding section, wherein the heating temperature of the hot molding section is lower than the glass transition temperature of the thermoplastic resin, and the thermoplastic resin of the thermoplastic resin composite pulled out from the hot molding section is in a glass state.
[0013] A second embodiment of the present invention is a manufacturing apparatus for a thermoplastic resin composite containing a thermoplastic resin and fibers, comprising: an impregnation section for continuously impregnating fibers with a thermoplastic resin forming composition containing an active hydrogen component and a diisocyanate component; a heat molding section for polymerizing the thermoplastic resin forming composition by passing the fibers through the composition and molding a thermoplastic resin composite containing the thermoplastic resin obtained by the polymerization; and a drawing device for continuously drawing out the thermoplastic resin composite from the heat molding section, wherein the heating temperature of the heat molding section is lower than the glass transition temperature of the thermoplastic resin, and the drawing device draws out the thermoplastic resin composite in which the thermoplastic resin is in a glassy state from the heat molding section.
[0014] In the above embodiment, the composite in which the thermoplastic resin forming composition is impregnated into the fibers may have a flexural modulus that becomes 10% or more of the flexural modulus at the time of complete curing within 5 minutes when heated at the heating temperature.
[0015] In the above embodiment, the heating temperature may be lower than the glass transition temperature of the thermoplastic resin by 30° C. or more.
[0016] In the above embodiment, the thermoplastic resin forming composition may have a pot life, which is the time it takes for the composition to reach a viscosity of 10,000 mPa·s under a temperature condition of 25° C., of 30 seconds or more.
[0017] In the above embodiment, the active hydrogen component of the thermoplastic resin forming composition may include an aromatic diamine having an alkylthio group, and the isocyanate component may include at least one diisocyanate selected from the group consisting of aliphatic diisocyanates, alicyclic diisocyanates, and modified products thereof. Effect of the Invention
[0018] According to an embodiment of the present invention, the thermoplastic resin composition impregnated into the fibers is polymerized in a heat molding section at a temperature lower than the glass transition temperature, and the thermoplastic resin composite in which the thermoplastic resin is in a glassy state is pulled out from the heat molding section. Therefore, the shape of the thermoplastic resin composite molded in the heat molding section can be maintained without a cooling step or the like, and the process can proceed to the next step such as cutting, thereby improving manufacturing efficiency. [Brief description of the drawings]
[0019] [Figure 1] Schematic diagram of a thermoplastic resin composite manufacturing apparatus according to one embodiment. [Diagram 2] Schematic diagram of a thermoplastic resin composite manufacturing apparatus according to another embodiment. [Diagram 3] Cross-sectional photograph of molded product after hot press molding in the example DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described in detail.
[0021] The manufacturing method according to the embodiment is a method for manufacturing a thermoplastic resin composite containing a thermoplastic resin and fibers. The manufacturing method includes the following steps. an impregnation step of continuously impregnating the fibers with the thermoplastic resin forming composition; A heat molding step of passing the impregnated fibers through a heat molding section to polymerize the thermoplastic resin forming composition and mold a thermoplastic resin composite containing the thermoplastic resin obtained by the polymerization; and The drawing process involves continuously drawing the thermoplastic resin composite from the heated molded section. In this manufacturing method, the heating temperature in the hot molding step (hereinafter referred to as the heating temperature T) is lower than the glass transition temperature (Tg) of the thermoplastic resin, and the thermoplastic resin of the thermoplastic resin composite that is pulled out from the hot molded part is in a glassy state.
[0022] 1 shows an example of a manufacturing apparatus 1 applicable to the manufacturing method. The manufacturing apparatus 1 includes an impregnation section 20 for continuously impregnating a fiber 10 with a thermoplastic resin forming composition, a heat molding section 30 for heating the fiber 10 impregnated with the thermoplastic resin forming composition to mold a thermoplastic resin composite 12, and a drawing device 40 for continuously drawing out the molded thermoplastic resin composite 12. More specifically, the manufacturing apparatus 1 further includes a fiber supply section 50 for supplying the fiber 10 to the impregnation section 20, and a monomer supply section 60 for supplying the thermoplastic resin forming composition to the impregnation section 20.
[0023] A thermoplastic resin composite is a fiber-reinforced thermoplastic resin that uses fibers as a reinforcing material and a thermoplastic resin as a base material (matrix).
[0024] Examples of the fibers include glass, carbon, metal, ceramic, or polymer fibers. These may be used alone or in combination of two or more. The fibers may also be provided with a glue or paint that promotes bonding of the components contained in the thermoplastic resin forming composition to the fibers. The fibers may be in the form of continuous fibers such as filaments, fibers, strand rovings, or woven fabrics, woven mats, nonwoven mats, or other forms.
[0025] The thermoplastic resin forming composition (hereinafter, sometimes referred to as a monomer mixture) is a composition used to form a thermoplastic resin, and is a mixture containing an active hydrogen component and a diisocyanate component. As the active hydrogen component, a bifunctional one is used, specifically, a diamine and / or a diol is used. The thermoplastic resin may be any of the following when the active hydrogen component contains a diol, a thermoplastic polyurethane resin when the active hydrogen component contains a diamine, and a thermoplastic polyurethane-urea resin containing both urethane bonds and urea bonds in the main chain when the active hydrogen component contains a diol and a diamine. The thermoplastic resin is preferably a thermoplastic polyurea resin or a thermoplastic polyurethane-urea resin.
[0026] It is preferable to use a monomer mixture having a pot life, which is the time it takes for the mixture to reach a viscosity of 10,000 mPa·s after mixing at a temperature of 25°C, of 30 seconds or more. By using a monomer mixture having such a long pot life, it is possible to prevent the resin from curing before it reaches the heat molded part 30. The pot life may be 100 seconds or more, or may be 200 seconds or more. There is no particular upper limit to the pot life, and it may be, for example, 1000 seconds or less.
[0027] It is preferable to use a monomer mixture liquid in which the glass transition temperature (Tg) of the thermoplastic resin after polymerization is high. In this embodiment, since the polymerization is performed at a temperature lower than the glass transition temperature, it is advantageous to have a high glass transition temperature in order to increase the polymerization temperature to shorten the polymerization time. The glass transition temperature of the thermoplastic resin is preferably, for example, 100°C or higher, more preferably 120°C or higher, and even more preferably 150°C or higher. The upper limit of the glass transition temperature is not particularly limited, and may be, for example, 220°C or lower, or 200°C or lower.
[0028] It is preferable that when the monomer mixture is impregnated into fibers and heated at a heating temperature T, the flexural modulus of the composite of the composition and fibers becomes 10% or more of the flexural modulus of the thermoplastic resin composite at the time of complete curing within 5 minutes. Since sufficient mechanical properties can be expressed within 5 minutes, the productivity in continuous pultrusion molding can be improved. Here, the flexural modulus is the longitudinal modulus measured in a bending test (the slope of the stress-strain curve when the material undergoes elastic deformation) and is measured in accordance with JIS K7074.
[0029] The monomer mixture having the above-mentioned properties is not particularly limited, but as one embodiment, the two-component curing composition described in Patent Document 4 above may be used, and it is preferable that the active hydrogen component contains an aromatic diamine (a) having an alkylthio group, and the isocyanate component contains at least one diisocyanate (b) selected from the group consisting of aliphatic diisocyanates, alicyclic diisocyanates, and modified products thereof.
[0030] As the aromatic diamine (a) having an alkylthio group, a compound having two amino groups directly bonded to the aromatic ring and an alkylthio group directly bonded to the aromatic ring is preferred. The alkylthio group is -SC n H 2n+1 (wherein n is an integer of 1 or more, preferably an integer of 1 to 5). The aromatic diamine (a) may have one alkylthio group, or two or more alkylthio groups in one molecule. It is preferable that the aromatic diamine (a) has two alkylthio groups directly bonded to the aromatic ring.
[0031] As the aromatic diamine (a), it is preferable to use, for example, a dialkylthiotoluenediamine such as dimethylthiotoluenediamine, diethylthiotoluenediamine, or dipropylthiotoluenediamine.
[0032] As the active hydrogen component, diamines such as other aromatic diamines may be used in combination with the aromatic diamine (a). Examples of other diamines include 4,4'-methylenedianiline, 4,4'-methylenebis(2-methylaniline), 4,4'-methylenebis(2-ethylaniline), 4,4'-methylenebis(2-isopropylaniline), 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(N-methylaniline), 4,4'-methylenebis(N-ethylaniline), 4,4'-methylenebis(N-sec-butylaniline), and diethyltoluenediamine. These may be used alone or in combination of two or more.
[0033] The diamine used as the active hydrogen component is preferably mainly composed of aromatic diamine (a), and preferably 50% by mass or more of the diamine is aromatic diamine (a), more preferably 70% by mass or more of the diamine is aromatic diamine (a). Also, it is preferable that 15% by mass or more of the active hydrogen component is aromatic diamine (a), more preferably 40% by mass or more of the active hydrogen component is aromatic diamine (a), and even more preferably 70% by mass or more of the active hydrogen component is aromatic diamine (a).
[0034] The active hydrogen component may contain a diol (c) together with the diamine. Examples of the diol (c) include alkylene glycols such as ethylene glycol and propylene glycol; polyalkylene glycols such as diethylene glycol, triethylene glycol, dipropylene glycol and tripropylene glycol; cyclohexanedimethanol, bisphenol A, etc. These may be used alone or in combination of two or more.
[0035] When diol (c) is contained as an active hydrogen component, the mass ratio (a / c) of aromatic diamine (a) to diol (c) is preferably 0.1 to 30. The mass ratio (a / c) is more preferably 0.5 to 20, and further preferably 1.0 to 10.
[0036] The active hydrogen component is bifunctional in order to form a thermoplastic resin, but may contain trifunctional or higher functional polyamines or polyols within the range in which a thermoplastic resin can be obtained.
[0037] Regarding the diisocyanate (b), examples of the aliphatic diisocyanate (i.e., chain aliphatic diisocyanate) include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, etc. Examples of modified aliphatic diisocyanates include isocyanate group-terminated urethane prepolymers obtained by reacting an aliphatic diisocyanate with a diol, bifunctional adduct modified products, and bifunctional allophanate modified products. Among these, it is preferable to use, as the aliphatic diisocyanate, at least one selected from the group consisting of hexamethylene diisocyanate (HDI) and its modified products.
[0038] Examples of alicyclic diisocyanates include isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate (H12MDI), 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane. Examples of modified alicyclic diisocyanates include isocyanate-terminated urethane prepolymers obtained by reacting alicyclic diisocyanates with diols, bifunctional adduct modified products, and bifunctional allophanate modified products. Among these, it is preferable to use at least one selected from the group consisting of isophorone diisocyanate (IPDI) and 4,4'-dicyclohexylmethane diisocyanate (H12MDI) as the alicyclic diisocyanate.
[0039] The diisocyanate (b) preferably has an isocyanate group content of 15 to 50 mass %. Here, the isocyanate group content is the mass ratio of reactive isocyanate groups (NCO) possessed by the bifunctional diisocyanate (b) to the diisocyanate (b). The isocyanate group content can be measured in accordance with JIS K7301-6-3.
[0040] The diisocyanate component is preferably 80% by mass or more of diisocyanate (b), more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more. As the isocyanate to be reacted with the active hydrogen component, a bifunctional isocyanate, i.e., a diisocyanate, is used to form a thermoplastic resin, but a trifunctional or higher polyisocyanate may be included within the range in which a thermoplastic resin can be obtained.
[0041] The monomer mixture is obtained by mixing Liquid A, which contains an active hydrogen component, with Liquid B, which contains a diisocyanate component. By mixing Liquid A and Liquid B together, both components can be reactively cured (i.e., polymerized), and a non-crystalline thermoplastic resin is obtained by reactive curing.
[0042] The monomer mixture may contain a catalyst for promoting the reaction between the active hydrogen component and the diisocyanate component. As the catalyst, a metal catalyst or an amine catalyst that is usually used in the production of polyurethane resins can be used. As the metal catalyst, there can be mentioned tin catalysts such as dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dioctate, lead catalysts such as lead octylate, lead octenate, and lead naphthenate, and bismuth catalysts such as bismuth octylate and bismuth neodecanoate. As the amine catalyst, there can be mentioned tertiary amine compounds such as triethylenediamine. These catalysts can be used alone or in combination.
[0043] The monomer mixture may further contain various additives, such as a plasticizer, a flame retardant, an antioxidant, a moisture absorbent, an antifungal agent, a silane coupling agent, a defoamer, a surface conditioner, and an internal mold release agent, as necessary.
[0044] In the monomer mixture, the molar ratio of isocyanate groups to active hydrogen groups (NCO / active hydrogen groups) is not particularly limited and may be 1.0 or more, 1.2 or more, or 1.5 or more. The molar ratio (NCO / active hydrogen groups) may be 2.0 or less, 1.5 or less, or 1.2 or less.
[0045] In the thermoplastic resin composite, the ratio of the fibers to the thermoplastic resin is not particularly limited. For example, the volume content of the fibers per unit volume of the thermoplastic resin composite may be 30 to 70%, or 50 to 60%.
[0046] Next, a method for producing a thermoplastic resin composite according to an embodiment will be described with reference to FIG.
[0047] In the impregnation step, in the impregnation section 20, the fibers 10 supplied from the fiber supply section 50 are impregnated with the monomer mixture supplied from the monomer supply section 60.
[0048] In this example, the fiber supplying section 50 gathers fibers unwound from a plurality of bobbins 51 into one and supplies the fibers 10 to the impregnation section 20 .
[0049] In this example, the monomer supply section 60 includes a first tank 61 storing liquid A containing an active hydrogen component, a second tank 62 storing liquid B containing a diisocyanate component, and a mixer 63 that mixes liquid A sent from the first tank 61 with liquid B sent from the second tank 62, and supplies the monomer mixture mixed in the mixer 63 to the impregnation section 20. The mixer 63 may be one that performs stirring and mixing using a stirring blade, or one that performs stirring and mixing using a mixing head arranged in a static mixer.
[0050] In this example, the impregnation section 20 is composed of multiple impregnation rollers 21, and is configured to drip the monomer mixture liquid at multiple locations onto the fibers 10 traveling via conveying rollers 22, and to impregnate the fibers 10 with the monomer mixture liquid by the multiple impregnation rollers 21.
[0051] A heating device for preheating the fiber 10 may be provided before the impregnation section 20. Preheating the fiber 10 in advance allows the fiber 10 to be quickly impregnated with the monomer mixture. Furthermore, moisture absorbed by the fiber 10 can be evaporated immediately before the fiber 10 is impregnated, and the effect of moisture during polymerization of the monomer mixture can be more suitably removed, stabilizing the polymerization reaction of the monomer mixture.
[0052] In the hot molding step, the fiber 10 impregnated in the impregnation unit 20 is passed through the hot molding unit 30 at a predetermined heating temperature T, whereby the monomer mixture is polymerized and a thermoplastic resin composite 12 containing the thermoplastic resin obtained by the polymerization is molded. That is, the fiber 10 impregnated with the monomer mixture is heated to cause a polymerization reaction while being shaped.
[0053] In this example, the hot molding section 30 includes a hot molding die 31 for molding the fiber 10 impregnated with the monomer mixture liquid to a predetermined thickness and width, and a heating device 32 for heating the thermoplastic resin composite 12 pulled out of the hot molding die 31 to promote the polymerization reaction. Note that the heating device 32 is not necessarily required.
[0054] The heating temperature T, which is the set temperature of the heat forming section 30, is the polymerization temperature for polymerizing the monomer mixture, and is not particularly limited as long as it is lower than the glass transition temperature Tg of the thermoplastic resin obtained by polymerizing the monomer mixture (T < Tg). Preferably, the heating temperature T is 30°C or more lower than the glass transition temperature Tg of the thermoplastic resin (T < Tg - 30°C). The heating temperature T may be, for example, 70 to 180°C, may be 70 to 160°C, or may be 80 to 150°C. The temperature set as the heating temperature T may be a single temperature, or may be set within a predetermined temperature range with a temperature distribution according to the part of the heat forming section 30. When the temperature set as the heating temperature T has a range, it is preferable that the highest temperature thereof is set lower than the glass transition temperature Tg and that the highest temperature is set 30°C or more lower than the glass transition temperature Tg.
[0055] In the drawing process, the thermoplastic resin composite 12 is continuously drawn from the heat forming section 30 by a drawing device 40. In this example, the drawing device 40 is composed of a pair of upper and lower rollers 41, 41 that draw the thermoplastic resin composite 12 therebetween.
[0056] In this embodiment, since the heating temperature T, which is the polymerization temperature in the heat forming section 30 as described above, is lower than the glass transition temperature Tg of the thermoplastic resin, the thermoplastic resin of the thermoplastic resin composite 12 drawn from the heat forming section 30 is in a glassy state below the glass transition temperature. That is, at the stage of coming out of the heat forming section 30, although the polymerization is not completed, it is in a state of pseudo-curing without stickiness and is in a state where its shape can be maintained. Therefore, the drawn thermoplastic resin composite 12 is difficult to have its shape collapsed and can maintain its shape.
[0057] Although not shown, a heating device for further heating the thermoplastic resin composite 12 to promote or complete the polymerization may be provided after the drawing device 40. Also, a cutting device such as a cutter may be provided after the drawing device 40 or after the additional heating device, and a plate material, a channel material, a round bar material, a strand material, etc. can be obtained.
[0058] In the example shown in Fig. 1, the impregnation section 20 is composed of a plurality of impregnation rollers 21 provided in front of the hot molding die 31, but the impregnation section may be provided inside the hot molding die 31. In this case, the impregnation section is incorporated into the front end portion of the hot molding section 30 as a part of the hot molding section 30. Fig. 2 shows one such example.
[0059] In the manufacturing apparatus 1A shown in Fig. 2, the fiber 10 unwound from a bobbin 51 of the fiber supply unit 50 is supplied into the hot molding die 31 of the hot molding unit 30 via a feed roller 52. Meanwhile, the monomer mixture supplied from the monomer supply unit 60 is directly injected into the hot molding die 31 by an injection tool 71 provided at the front end of the hot molding die 31, and the monomer mixture is impregnated into the fiber 10 in the hot molding die 31. Therefore, the front end of the hot molding die 31 also serves as the impregnation unit 70.
[0060] An impregnation tool (not shown) such as an impregnation roller may be provided inside the hot molding die 31. This allows the fibers 10 to be impregnated with the monomer mixture injected into the hot molding die 31 by the injection tool 71 in a short time. Such a device for the impregnation section 70 is highly effective in impregnating the fibers 10 with the monomer mixture in a short time while eliminating excess air, and since the air inside the fibers 10 is quickly eliminated in a short time, it is possible to reduce minute voids (cavities) inside the thermoplastic resin composite 12 after curing.
[0061] According to the embodiment described above, a thermoplastic resin composite can be efficiently produced by continuous pultrusion molding.
[0062] In detail, in general, in continuous pultrusion molding, the resin is polymerized and hardened by heating in the heat molding section, so that the temperature of the thermoplastic resin composite at the outlet of the heat molding section is almost equal to the polymerization temperature of the resin set in the heat molding section. Therefore, in continuous pultrusion molding, if the polymerization temperature is higher than the glass transition temperature of the matrix resin, the thermoplastic resin composite at the outlet of the heat molding section is in a soft rubber state, and the cross-sectional shape of the thermoplastic resin composite as a molded product cannot be maintained, making molding difficult. In contrast, for example, it is possible to cool the thermoplastic resin composite to below the glass transition temperature by providing a cooling process after heat molding, but the device becomes larger accordingly, and in addition, the drawing speed of the thermoplastic resin composite must be slowed down to cool the inside of the thermoplastic resin composite, resulting in poor manufacturing efficiency.
[0063] According to this embodiment, polymerization is performed in a heat molding section at a temperature lower than the glass transition temperature, and the thermoplastic resin composite in a glassy state is pulled out from the heat molding section. This makes it easier to maintain the shape of the thermoplastic resin composite molded in the heat molding section, thereby improving manufacturing efficiency.
[0064] In addition, in the continuous pultrusion molding of a thermoplastic resin composite having a matrix of a polyamide resin made from a polymerizable lactam mixture as disclosed in the above Patent Document 3, a decrease in strength due to moisture absorption, which is a drawback of polyamide resin, is unavoidable. In addition, the catalytic activity of the anionic catalyst of ε-caprolactam, which is a raw material of the polymerizable lactam mixture, may be deactivated by moisture in the air, and polymerization may be inhibited. In contrast, in the present embodiment, a thermoplastic resin composite can be stably and continuously produced by using a thermoplastic resin of polyurethane and / or polyurea composed of an active hydrogen component and a diisocyanate component as a matrix.
[0065] The thermoplastic resin composite obtained by the manufacturing method according to this embodiment can be used as various lightweight structural members, for example, by laminating a plurality of sheets and performing secondary processing such as hot press molding. In this case, the thermoplastic resin composite having the thermoplastic resin according to this embodiment as the base material can be expected to shorten the secondary molding time and have high productivity compared to fiber-reinforced composite materials having a thermosetting resin as the base material, and can be applied to various members as an intermediate material for metal substitutes for the purpose of reducing weight, including automotive structural members that require recyclability. EXAMPLES
[0066] A thermoplastic resin composite was produced by continuous pultrusion using a production apparatus 1 shown in Fig. 1. Carbon fibers ("T700SC-24000-60E" manufactured by Toray Industries, Inc.) were used as the fibers 10.
[0067] As the monomer mixture, a two-component curing composition ("H-6FP22" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) consisting of a liquid A containing a dialkylthiotoluenediamine and a liquid B containing a modified product of an aliphatic diisocyanate was used.
[0068] The pot life of the two-component curing composition was measured to be 300 seconds, using a BM type rotational viscometer at 25°C with a No. 4 rotor at 60 rpm to determine the time until the viscosity reached 10,000 mPa s.
[0069] The glass transition temperature of the resin after polymerization of the two-component curing composition was measured and found to be 175° C. The glass transition temperature was measured by the following method. [Glass transition temperature] Liquid A and Liquid B were adjusted to 25°C and mixed by stirring for 1 minute, and the resulting monomer mixture was applied to a sheet and treated at 120°C for 3 hours to obtain a resin sheet with a thickness of 2 mm. A test piece of 5 mm x 2 cm was cut out from the resulting resin sheet, and the glass transition temperature (Tg) was measured using Rheogel E-4000 manufactured by UBM Corporation with a chuck distance of 20 mm, a fundamental frequency of 10 Hz, and strain in automatic control mode.
[0070] In order to confirm whether the flexural modulus of the composite after impregnation becomes 10% or more of the flexural modulus of the composite when completely cured by heating within 5 minutes, the following test was performed. That is, the two-component curing composition was impregnated into fiber 10, heated at 130°C for 5 minutes, and the flexural modulus of the composite after heating was measured. In addition, the two-component curing composition was impregnated into fiber 10, heated at 130°C for 10 minutes to completely cure (i.e., polymerization was completed), and the flexural modulus of the thermoplastic resin composite when completely cured was measured. As a result, the flexural modulus of the composite after heating for 5 minutes was 20% of the flexural modulus of the composite when completely cured. Therefore, it was confirmed that the flexural modulus of the composite of the two-component curing composition becomes 10% or more of the flexural modulus of the composite when completely cured by heating within 5 minutes, and the time required for sufficient mechanical properties to be expressed is within 5 minutes. The measurement of the flexural modulus of the composite was performed in accordance with JIS K7074.
[0071] The volume fraction of the fiber 10 in the thermoplastic resin composite 12 (V f The monomer mixture was supplied by the monomer supply unit 60 so that the ratio of the monomer mixture to the total monomer mixture was 60%. In detail, the monomer mixture was prepared by sending the A liquid and the B liquid from the tanks 61 and 62 according to the compounding ratio and stirring them through a mixer 63 consisting of a static mixer. Since the monomer mixture starts to polymerize the moment it is stirred, in order to perform continuous pultrusion molding, it is necessary to continue to supply new monomer mixture and drain the stagnant monomer mixture before the pot life is reached. Therefore, the place where the monomer mixture was dropped was divided into three places to promote the flow of the stagnant monomer mixture. Then, in the impregnation unit 20 consisting of multiple impregnation rollers 21, the fibers 10 supplied from the fiber supply unit 50 were impregnated with the monomer mixture.
[0072] The heating mold 31 was made of an aluminum alloy, and in order to prevent a rapid curing reaction of the monomer mixture liquid that remained near the mold inlet where the fiber 10 was fed, a water cooling pipe was provided at the mold inlet to keep the temperature near the mold inlet at about 25°C. In addition, in order to prevent the heating mold 31 from adhering to the thermoplastic resin composite 12 during the curing reaction, a thin PTFE core mold divided into upper and lower parts was provided at the part of the aluminum alloy heating mold 31 that contacted the thermoplastic resin composite 12. Using this heating mold 31, a thermoplastic resin composite 12 with a width of 15 mm and a thickness of 0.5 mm was molded in the heating mold 31, which had a temperature distribution of 80°C to 130°C.
[0073] The thermoplastic resin composite 12 pulled out from the hot molding die 31 by the pulling device 40 was further heat-cured in the heating device 32, which is a far-infrared heater. The heating temperature by the heating device 32 was 110 to 120°C. In this example, the heating device 32 was variable in length, and the length of the heating device 32 was 1.0 m. Since the length of the hot molding die 31 was 0.5 m, the length of the hot molding section 30 including the heating device 32 was 1.5 m. The pulling speed was set to 500 mm / min so as to ensure a polymerization time of 3 minutes (i.e., so as to ensure a polymerization time of 3 minutes from the hot molding die 31 to the heating device 32).
[0074] In this example, the glass transition temperature of the resin after polymerization of the monomer mixture was 175° C., whereas the heating temperature T in the heat molding part 30 was 80 to 130° C., so that the heating temperature T was 30° C. or more lower than the glass transition temperature. Therefore, at the stage when it was pulled out from the heat molding part 30, the thermoplastic resin composite 12 was in a glassy state below the glass transition temperature, i.e., it was quasi-cured.
[0075] The thermoplastic resin composite 12 pulled out through the pulling device 40 was cut to a length of 30 cm. Thereafter, in order to further complete the polymerization reaction of the thermoplastic resin composite 12, it was heated in an oven at 120°C for 60 minutes to obtain a fully cured thermoplastic resin composite (prepreg). The obtained prepreg was used for hot pressing at a heating temperature of 200°C for 10 minutes at a pressure of 2 MPa to prepare a tensile test specimen.
[0076] The fiber volume content of the obtained tensile test piece was measured by a combustion method, and the fiber volume content was found to be 56%. The measurement of the fiber volume content by the combustion method was performed in accordance with JIS K7052.
[0077] Furthermore, when the cross section of the tensile test piece was measured with an optical microscope (OLYMPUS "GX51"), no internal air bubbles (voids) were observed, as shown in Figure 3, confirming that a very high quality thermoplastic resin composite could be molded. In Figure 3, the dark gray parts are the thermoplastic resin matrix, and the white parts are the carbon fibers.
[0078] In this way, by hot pressing the thermoplastic resin composite 12 of the embodiment at a temperature slightly higher than the glass transition temperature by about 30° C., a beautiful molded product without bubbles between the layers could be obtained. This means that the thermoplastic resin composite 12 that has been continuously pultrusion molded can be easily reprocessed into a molded product of any shape.
[0079] The tensile strength of the above tensile test specimen was measured, and the measured value was compared with the theoretical value. The measured tensile strength was 2500 MPa. The tensile test was performed in accordance with JIS K7165, and the test specimen dimensions were 240 mm in length, 15 mm in width, and 0.5 mm in thickness. Aluminum tabs were attached to both sides of the molded product at 40 mm from both ends to prevent damage due to stress concentration in the chuck. A servo pulsar (Shimadzu Corporation, EFH-EG100KN-20L) was used as the tensile tester, and the test speed was 2 mm / s.
[0080] The theoretical value was calculated based on the following composite rule, assuming that the thermoplastic resin and the carbon fiber were completely bonded to each other.
number
[0081] In the formula, σ cis the theoretical value, α is a coefficient determined by the fiber morphology (α=1.0 for unidirectional reinforcement), σ fu is the tensile breaking stress of the fiber, (σ m ) fu is the resin fracture stress relative to the fiber breakage elongation, V f is the fiber volume fraction.
[0082] As a result, the theoretical value of the tensile strength was 2750 MPa. As described above, the thermoplastic resin composite according to the embodiment exhibited a high strength of about 90% of the theoretical strength, and it is understood that very high quality molding can be performed.
[0083] In this way, the manufacturing method of the thermoplastic resin composite according to the embodiment allows stable production of high-quality thermoplastic resin composites without bubbles (voids), and since it is a continuous pultrusion molding method, the productivity is high, and it is also possible to adjust the hardening reaction speed of the thermoplastic resin composite, so that the productivity of the product can be adjusted. Furthermore, it was shown that reprocessing and secondary molding are possible by secondary pressing at a very low temperature, and it was shown that even molded products with complex shapes can be easily manufactured with high productivity.
[0084] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.
Claims
1. A method for producing a thermoplastic resin composite containing a thermoplastic resin and fibers, comprising the steps of: Continuously impregnating a fiber with a thermoplastic resin-forming composition including an active hydrogen component and a diisocyanate component; Passing the fibers through a heated molding section to polymerize the thermoplastic resin forming composition and mold a thermoplastic resin composite containing the thermoplastic resin obtained by the polymerization; and continuously drawing the thermoplastic resin composite from the heated mold portion; The heating temperature of the hot molded part is lower than the glass transition temperature of the thermoplastic resin, and the thermoplastic resin of the thermoplastic resin composite pulled out from the hot molded part is in a glass state. A method for producing a thermoplastic resin composite.
2. The method for producing a thermoplastic resin composite according to claim 1, wherein the composite in which the thermoplastic resin forming composition is impregnated into the fibers has a flexural modulus that is 10% or more of the flexural modulus at the time of complete curing within 5 minutes when heated at the heating temperature.
3. The method for producing a thermoplastic resin composite according to claim 1 or 2, wherein the heating temperature is 30° C. or more lower than the glass transition temperature of the thermoplastic resin.
4. The thermoplastic resin forming composition has a pot life of 30 seconds or more, which is the time it takes for the composition to reach a viscosity of 10,000 mPa s under a temperature condition of 25 ° C. The method for producing a thermoplastic resin composite according to any one of claims 1 to 3.
5. The active hydrogen component of the thermoplastic resin forming composition includes an aromatic diamine having an alkylthio group, and the diisocyanate component includes at least one diisocyanate selected from the group consisting of aliphatic diisocyanates, alicyclic diisocyanates, and modified products thereof. The method for producing a thermoplastic resin composite according to any one of claims 1 to 4.
6. An apparatus for producing a thermoplastic resin composite containing a thermoplastic resin and a fiber, comprising: an impregnation section for continuously impregnating the fibers with a thermoplastic resin forming composition containing an active hydrogen component and a diisocyanate component; a heating and molding section for polymerizing the thermoplastic resin forming composition and molding a thermoplastic resin composite containing the thermoplastic resin obtained by the polymerization by passing the fibers through the heating and molding section; a drawing device that continuously draws the thermoplastic resin composite from the hot molding section; a heating temperature of the hot molding part is lower than a glass transition temperature of the thermoplastic resin, and the pulling device pulls the thermoplastic resin composite in which the thermoplastic resin is in a glass state from the hot molding part. Thermoplastic resin composite manufacturing equipment.
Citation Information
Patent Citations
Fiber reinforced composite material and manufacturing method thereof
JP2002508021A
Polyisocyanurate compositions and composite materials
JP2002530445A
Continuous production method for molded object and molded object
JP2004074427A
Pultrusion manufacturing equipment of fiber-reinforced polyamide composite material, and pultrusion manufacturing method
JP2017007266A
Two-component curing composition for forming thermoplastic matrix resin, matrix resin for fiber-reinforced composite material, and fiber-reinforced composite material
JP6580774B1