Toner composition for developing electrostatic images

A toner composition using silica particles treated with aluminum hydroxide and an organic substance addresses the carcinogenic concerns of titanium oxide, enhancing image density and charge stability while maintaining fluidity and charging properties.

JP7569725B2Active Publication Date: 2024-10-18SAKATA INX
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021047443
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-10-18
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

The use of titanium oxide in toner compositions for electrostatic image development is concerning due to potential carcinogenic risks, leading to excessive charge amounts and issues like decreased cleaning properties and developability.

Method used

A toner composition using silica particles with a particle size of 10 to 30 nm, surface-treated with aluminum hydroxide and an organic substance, replaces titanium oxide to achieve excellent image density, charge amount, and charge stability.

Benefits of technology

The toner composition exhibits improved image density, charge amount, and charge stability without titanium oxide, ensuring good fluidity, charging properties, and environmental stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569725000001
    Figure 0007569725000001
Patent Text Reader

Abstract

To provide an electrostatic image developing toner composition which does not contain titanium oxide and offers superior image density, charge amount, and charging stability.SOLUTION: An electrostatic image developing toner composition is provided, comprising toner particles and an external additive containing silica particles with diameters of 10-30 nm, surface-treated with aluminum hydroxide and an organic substance.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner composition for developing electrostatic images, and more particularly to a toner composition for developing electrostatic images that does not contain titanium oxide and exhibits excellent image density, charge amount and charge stability. [Background technology]

[0002] Conventionally, in electrostatic image developers containing toner compositions, external additives such as titanium oxide have been blended in order to output stable images over a long period of time (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-122046 A Summary of the Invention [Problem to be solved by the invention]

[0004] Titanium oxide is a carcinogenic substance, but if titanium oxide is not used, the charge amount of the toner composition in the developer increases excessively, which can lead to problems such as a decrease in the cleaning property of the toner composition, and a decrease in the developability and transferability.

[0005] The present invention has been made in consideration of such conventional problems, and has an object to provide a toner composition for developing electrostatic images that does not contain titanium oxide and exhibits excellent image density, charge amount and charge stability. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved when toner particles contain, as an external additive, silica particles with a particle size of 10 to 30 nm that have been surface-treated with aluminum hydroxide and an organic substance, and have thus completed the present invention. The present invention that solves the above problems mainly comprises the following configurations.

[0007] (1) A toner composition for developing electrostatic images, comprising toner particles and an external additive, the external additive comprising silica particles having a particle size of 10 to 30 nm and surface-treated with aluminum hydroxide and an organic substance.

[0008] According to this constitution, the toner composition for developing electrostatic images exhibits excellent image density, charge amount and charge stability even without containing titanium oxide.

[0009] (2) The toner composition for developing electrostatic images according to (1), wherein the organic substance contains at least one of an alkylsilane having 8 to 12 carbon atoms and a saturated fatty acid having 16 to 20 carbon atoms.

[0010] According to such a constitution, the toner composition for developing electrostatic images has good fluidity, chargeability, cleaning properties, and the like.

[0011] (3) The toner composition for developing electrostatic images according to (1) or (2), wherein the organic substance contains at least one of decylsilane and stearic acid.

[0012] According to such a constitution, the toner composition for developing electrostatic images has good charge stability and environmental stability. Effect of the Invention

[0013] According to the present invention, it is possible to provide a toner composition for developing electrostatic images that does not contain titanium oxide and exhibits excellent image density, charge amount and charge stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <Toner composition for developing electrostatic images> The toner composition for developing electrostatic images (hereinafter also referred to as toner composition) according to one embodiment of the present invention contains toner particles and an external additive. The external additive contains silica particles having a particle size of 10 to 30 nm and surface-treated with aluminum hydroxide and an organic substance. Each of these will be described below.

[0015] (Toner particles) The toner particles are not particularly limited. For example, the toner particles include a binder resin, a colorant, and a release agent.

[0016] Binder resin The binder resin is blended to disperse the colorant contained in the toner composition and to fix the colorant to the surface of the recording medium by melting it on the surface of the recording medium due to the heat of the fixing roller during the fixing process during printing and then solidifying it.

[0017] The binder resin is not particularly limited. For example, the binder resin is a resin material such as polystyrene, a styrene-based copolymer such as a styrene-methyl acrylate copolymer or a styrene-acrylonitrile copolymer, polyester, or an epoxy resin. The binder resin may be used in combination. Among these, the binder resin is preferably polyester, since it is easy to color and a toner with a vivid color can be obtained.

[0018] The polyester is obtained by polymerizing a monomer composition consisting of a dihydric or higher polyhydric alcohol and a polybasic acid. The dihydric alcohol used in the polymerization of the polyester is not particularly limited. For example, the dihydric alcohol is a diol such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, or 1,6-hexanediol, or an alkylene oxide adduct of bisphenol A such as bisphenol A, hydrogenated bisphenol A, polyoxyethylenated bisphenol A, or polyoxypropylenated bisphenol A.

[0019] The trihydric or higher polyhydric alcohol is not particularly limited. For example, the trihydric or higher polyhydric alcohol may be sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, sucrose, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, etc.

[0020] The dibasic acid is not particularly limited. Examples of the dibasic acid include maleic acid, fumaric acid, citraconic acid, itaconic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, and anhydrides of these acids.

[0021] The trivalent or higher polybasic acid is not particularly limited. For example, the trivalent or higher polybasic acid is 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, anhydrides of these acids, etc.

[0022] The content of the binder resin is not particularly limited. The content of the binder resin may be appropriately adjusted in consideration of the performance required for the toner. For example, the content of the binder resin is preferably 50 to 95 parts by mass in 100 parts by mass of the toner particles.

[0023] Coloring agents Colorants are included to impart color strength to the toner composition.

[0024] The colorant is not particularly limited. For example, the colorant may be a magnetic powder colorant that exhibits a black color such as carbon black, a cyan colorant such as copper phthalocyanine, methylene blue, or Victoria blue, a magenta colorant such as rhodamine dye, dimethylquinacridone, dichloroquinacridone, or carmine red, or a yellow colorant such as benzidine yellow, chrome yellow, naphthol yellow, or disazo yellow. The colorants may be used in combination.

[0025] The content of the colorant is not particularly limited. For example, the content of the colorant is preferably 0.1 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the binder resin in the toner composition. Note that various masterbatches in which a high concentration of pigment is pre-dispersed in a resin are commercially available, and may be purchased and used as the colorant. In this case, the amount of the colorant used may be determined in consideration of the concentration of the pigment contained in the masterbatch so that the concentration of the pigment contained in the toner composition falls within the above range.

[0026] Release agent The release agent is not particularly limited, and various known waxes can be used. Examples include polyolefin waxes such as polyethylene wax and polypropylene wax, branched chain hydrocarbon waxes such as microcrystalline wax, long chain hydrocarbon waxes such as paraffin wax and sazol wax, dialkyl ketone waxes such as distearyl ketone, carnauba wax, montan wax, behenic acid behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, trimellitic acid tristearyl, distearyl maleate, and other ester waxes, ethylenediamine behenylamide, trimellitic acid tristearylamide, and other amide waxes. The release agents may be used in combination. Among these, ester waxes and hydrocarbon waxes are preferred as the release agent.

[0027] The content of the release agent is not particularly limited. For example, the content of the release agent can be usually within the range of 1 to 30 parts by mass, preferably within the range of 5 to 20 parts by mass, relative to 100 parts by mass of the binder resin. The content of the release agent in the toner particles is preferably within the range of 3 to 15% by mass. By having the content of the release agent within the above range, the toner composition obtained can obtain good releasability between the fixing roller and the printing surface during the fixing process during printing. In addition, the toner composition is less likely to exude the release agent, and is less likely to cause poor charging, filming, etc.

[0028] Other Ingredients In addition to the above, the toner particles may contain, for example, a charge control agent, etc. The charge control agent is suitably blended in order to adjust the charge amount of the toner composition.

[0029] The charge control agent is not particularly limited. For example, the charge control agent may be a metal complex of nigrosine, a basic dye, a monoazo dye, or the like, a salt or complex of a carboxylic acid such as salicylic acid or a dicarboxylic acid with a metal such as chromium, zirconium, or aluminum, an organic dye, a metal salt of naphthenic acid or a higher fatty acid, an alkoxylated amine, a quaternary ammonium salt compound, or a resin-type charge control agent such as an aromatic polycondensate. The charge control agents may be used in combination. Among these, it is preferable that the toner composition contains a resin-type charge control agent from the viewpoint of the stability of charging.

[0030] The content of the charge control agent is not particularly limited. As an example, the content of the charge control agent in the toner particles may not be contained, but is preferably 0.5% by mass or more. The content of the charge control agent in the toner particles is preferably 8% by mass or less. By containing the charge control agent in the above range, the toner composition obtained has better charging properties.

[0031] (External additives) External additives are blended to adhere to the surfaces of toner particles to improve the charging characteristics of the toner particles, or to exist separately from the toner particles to improve the fluidity of the toner composition or improve printability.

[0032] The external additive of this embodiment contains aluminum hydroxide and silica particles having a particle size of 10 to 30 nm that have been surface-treated with an organic substance.

[0033] The organic substance is not particularly limited. The organic substance preferably contains at least one of an alkylsilane having 8 to 12 carbon atoms and a saturated fatty acid having 16 to 20 carbon atoms. This improves the flowability, chargeability, cleaning properties, etc. of the toner composition.

[0034] Among these, it is more preferable that the organic substance contains at least one of decylsilane and stearic acid, which provides the toner composition with good charge stability and environmental stability.

[0035] The particle size (average primary particle size) of the silica particles may be 10 nm or more, and more preferably 12 nm or more. The particle size (average primary particle size) of the silica particles may be 30 nm or less, and more preferably 20 nm or less. If the particle size of the silica particles is less than 10 nm, the toner composition may have poor charging stability and may cause a decrease in charging. On the other hand, if the particle size of the silica particles exceeds 30 nm, there is a risk of causing contamination of components due to detachment of the silica particles. In this embodiment, the particle size (average primary particle size) of the silica particles was determined by taking a transmission electron microscope photograph and processing the image of the particles to determine the length (nm) of the major axis and the length (nm) of the minor axis of each particle.

[0036] The content of silica particles is not particularly limited. For example, the content of silica particles is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, relative to 100 parts by mass of toner particles. The content of silica particles is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, relative to 100 parts by mass of toner particles. By having the content of silica particles within the above range, the toner composition has good fluidity, charging property, cleaning property, etc.

[0037] The method of surface-treating silica particles with aluminum hydroxide and an organic substance is not particularly limited. For example, silica is subjected to an inorganic treatment with aluminum hydroxide and an organic treatment with the organic substance. For example, the inorganic treatment method includes a method of adding a salt such as aluminum chloride, hydrolyzing the salt, and precipitating aluminum hydroxide on the silica particle surface. For example, the organic treatment method includes a method of adding an alkali metal fatty acid salt, and then adding a strong acid such as sulfuric acid to precipitate the liberated fatty acid on the silica particle surface.

[0038] In the present embodiment, the silica is inorganically treated with aluminum hydroxide to adjust the resistance of the silica, and is organically treated with an organic substance to impart hydrophobicity to the silica, so that the resulting toner composition has excellent chargeability and environmental stability.

[0039] The external additive may appropriately contain other external additives in addition to aluminum hydroxide and silica particles with a particle size of 10 to 30 nm that have been surface-treated with an organic substance. The other external additives are not particularly limited. For example, the other external additives may be negatively charged lubricant particles, positively charged lubricant particles, inorganic oxide particles (excluding the above-mentioned silica particles), etc. These may be used in combination.

[0040] The positively charged lubricant particles are lubricant particles that are positively charged by frictional charging between the carrier or the charging blade. Such lubricant particles are known, and a preferred example is a metal salt particle of fatty acid. Preferred examples of such metal salts of fatty acid include zinc stearate, aluminum stearate, calcium stearate, magnesium stearate, zinc laurate, zinc myristate, zinc palmitate, zinc oleate, etc., and more preferred among them are zinc stearate and magnesium stearate. The positively charged lubricant particles may be a single type or a combination of two or more types.

[0041] Negatively charged lubricant particles are lubricant particles that are negatively charged by frictional charging between the carrier or the charging blade. Such lubricant particles are known, and preferred examples thereof include polytetrafluoroethylene (PTFE), silicone, boron nitride, polymethylmethacrylate (PMMA), and polyvinylidene fluoride, and more preferred examples thereof include boron nitride and polytetrafluoroethylene (PTFE). The negatively charged lubricant particles may be a single type or a combination of two or more types.

[0042] The inorganic oxide particles are not particularly limited. Examples of the inorganic oxide particles include alumina, zirconia, zinc oxide, chromium oxide, cerium oxide, antimony oxide, tungsten oxide, tin oxide, tellurium oxide, manganese oxide, boron oxide, etc. The inorganic oxide particles may be used in combination.

[0043] The inorganic oxide particles are preferably surface-treated for hydrophobization. The method of hydrophobization is not particularly limited. For example, the method of hydrophobization is a method in which a conventionally known hydrophobization agent is brought into contact with the surface of the inorganic oxide particles before hydrophobization, and a hydrophobic functional group or component is chemically bonded or attached to the surface of the inorganic oxide particles. The hydrophobization agent for hydrophobizing the inorganic oxide particles is not particularly limited. For example, the hydrophobization agent is octyltriethoxysilane, polydimethylsiloxane, dimethyldichlorosilane, hexamethyldisilazane, etc. The hydrophobization agents may be used in combination.

[0044] The content of the external additive in this embodiment is not particularly limited. As an example, the content of the external additive is preferably 1 part by mass or more, more preferably 2 parts by mass or more, relative to 100 parts by mass of the toner particles. The content of the external additive is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, relative to 100 parts by mass of the toner particles. When the content of the external additive is within the above range, the obtained toner composition has good fluidity, charging property, cleaning property, etc.

[0045] As described above, the toner composition of the present embodiment exhibits excellent image density, charge amount and charge stability even without containing titanium oxide.

[0046] <Method of manufacturing a toner composition for developing electrostatic images> The method for producing a toner composition for developing electrostatic images (hereinafter also referred to as a method for producing a toner composition) according to one embodiment of the present invention is a method for producing the above-mentioned toner composition for developing electrostatic images. The method for producing a toner composition is not particularly limited. As an example, the method for producing a toner composition includes the steps of kneading, cooling and solidifying the mixture, pulverizing, classifying, and adding an external additive. Note that each of these steps is a step that is adopted in a conventionally known method for producing a toner composition. That is, the method for producing a toner composition according to this embodiment can produce a toner composition by a conventionally known method using a conventionally known production device.

[0047] More specifically, first, in the kneading step, the components of the toner particles are melted and kneaded to prepare a kneaded product. The components can be mixed using various conventionally known mixing devices (for example, a double con mixer, a V-type mixer, a drum mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke and Engineering Co., Ltd.), etc.). For melt kneading, a batch type kneader such as a pressure kneader or a Banbury mixer, or a continuous type kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of being capable of continuous production. For example, a KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-Kneader (manufactured by Buss Co., Ltd.), and a Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. As the toner material, a master batch containing the above-mentioned binder resin and colorant may be used.

[0048] Thereafter, the kneaded product is cooled, and then the cooled kneaded product is pulverized (for example, after coarsely pulverizing with a pulverizer such as a crusher, hammer mill, or feather mill, it is further pulverized with a fine pulverizer using, for example, a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), a Super Rotor (manufactured by Nisshin Engineering Co., Ltd.), a Turbo Mill (manufactured by Freund Turbo Co., Ltd.), or an air jet type). The powder (pulverized product) obtained in the pulverization step is classified (for example, using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Co., Ltd.), a TSP Separator (manufactured by Hosokawa Micron Co., Ltd.), or a Faculty (manufactured by Hosokawa Micron Co., Ltd.)). The volume median particle size (D50) of the toner particles after pulverization and classification is preferably 4 to 10 μm. In this embodiment, the volume median particle diameter (D50) is also called the volume-based median diameter, and indicates a value where the total volume of particles with diameters smaller than this value and the total volume of particles with diameters larger than this value are 50% of the total volume. The volume median particle diameter (D50) can be calculated by measuring particle size distribution. An example of a particle size distribution measuring device is "Multisizer 3" manufactured by Beckman Coulter. Next, an external additive is added to the toner particles, and the mixture is stirred and mixed in various conventionally known mixing devices (for example, a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), etc.) to obtain a toner composition.

[0049] As described above, the method for producing a toner composition according to the present embodiment does not require special equipment, and the toner composition can be produced using equipment similar to existing equipment. Furthermore, the toner composition obtained exhibits excellent image density, charge amount, and charge stability, even without containing titanium oxide, as described above. EXAMPLES

[0050] The present invention will be described in more detail below with reference to the following examples. The present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass".

[0051] The raw materials and preparation methods used are shown below. <Preparation of toner base particles> 58.8 parts of a commercially available polyester resin (product name: FC1494, manufactured by Mitsubishi Chemical Corporation) as a binder resin, 25.0 parts of a commercially available polyester resin (product name: ER561, manufactured by Mitsubishi Chemical Corporation) as a binder resin, 11.2 parts of a yellow colorant (Pigment Yellow 180-based colorant) as a colorant, and 5 parts of a fatty acid ester wax (product name: WE-10, manufactured by NOF Corporation) as a release agent were mixed in a Henschel mixer, and then melt-kneaded using a twin-screw extruder. The resulting kneaded product was melted and solidified, coarsely pulverized using a Rotoplex, finely pulverized using a jet mill, and classified using an air classifier to obtain negatively charged toner base particles with a volume median particle size of 6.5 μm. <Silica particles> Wacker, H05TD, surface treatment: PDMS treatment, particle size 50 nm <Titanium oxide particles> Titan Kogyo Co., Ltd., STT-30S, treated with silane coupling agent, particle size 20-25 nm <Silica> Silica 1: Prototype, manufactured by Sakata Inx Corporation, inorganic treatment: aluminum hydroxide, organic treatment: silica particles surface-treated with decylsilane, particle size 15 nm Silica 2: Prototype, manufactured by Sakata Inx Corporation, inorganic treatment: aluminum hydroxide, organic treatment: silica particles surface-treated with stearic acid, particle size 15 nm <Alumina> Alumina 1: VP Alu C RK, manufactured by Aerosil Co., Ltd. Surface treatment: alkylsilane treatment Alumina 2: Prototype, manufactured by Cabot Corporation, Surface treatment: PDMS treatment <Other> Tin oxide: Prototype, manufactured by Sukgyung Co., Ltd., Surface treatment: HMDS treatment

[0052] <Examples 1 to 4, Comparative Examples 1 to 6, Reference Examples> (Preparation of Toner Composition) Each component was added to 100 parts by mass of the toner base particles according to the blending ratio (parts by mass) shown in Table 1 below, and stirred for 10 minutes with a Henschel mixer to obtain toner compositions of the Examples, Reference Examples and Comparative Examples.

[0053] [Table 1]

[0054] For the toner compositions of the Examples, Reference Examples, and Comparative Examples obtained above, printed matter was produced under the following conditions, and image density, toner charge amount, charge stability, and environmental stability were evaluated. The results are shown in Table 1.

[0055] <Image density> Using a non-magnetic two-component negatively charged copying machine for evaluation, 10,000 sheets of ISO chart ISO-IEC24712 were printed in an environment of 25°C temperature and 50% humidity (NN environment), and then a solid image was printed and the image density was evaluated using a reflection densitometer RD-914 (manufactured by Macbeth).

[0056] <Toner charge amount> The toner charge amount when printing 10,000 sheets of ISO chart ISO-IEC24712 in an environment of 25°C and 50% humidity (NN environment) using a non-magnetic two-component negatively charged copier for evaluation was evaluated using a Q / M meter MODEL210HS-2A (manufactured by TREK Corporation).

[0057] <Charge stability> Using a non-magnetic two-component negatively charged copying machine for evaluation, 10,000 sheets of ISO chart ISO-IEC24712 were printed in an environment of 25°C temperature and 50% humidity (NN environment), and the toner charge amount was measured with a Q / M meter initially and after 10,000 sheets were printed, and the difference was evaluated according to the following evaluation criteria. (Evaluation Criteria) ○: The difference was less than -10 μC / g. △: The difference was -10 μC / g or more and less than -20 μC / g. ×: The difference was −20 μC / g or more.

[0058] <Environmental stability> Using a non-magnetic two-component negatively charged copying machine for evaluation, the toner charge amount when 5,000 sheets of ISO chart ISO-IEC24712 were printed in an environment of 25°C temperature and 50% humidity (NN environment), and the toner charge amount when 5,000 sheets of ISO chart ISO-IEC24712 were printed in an environment of 10°C temperature and 20% humidity (LL environment) were measured with a Q / M meter, and the difference was evaluated according to the following evaluation criteria. (Evaluation Criteria) ○: The difference was less than -10 μC / g. △: The difference was -10 μC / g or more and less than -20 μC / g. ×: The difference was −20 μC / g or more.

[0059] As shown in Table 1, the toner compositions of Examples 1 to 4 exhibited image density, charge amount and charge stability that were comparable to or superior to the toner composition of the Reference Example using titanium oxide.

Claims

1. The toner particles include an external additive, The external additive contains silica particles having a particle size of 10 to 30 nm and surface-treated with aluminum hydroxide and an organic substance, The toner composition for developing electrostatic images, wherein the organic material contains an alkylsilane having 8 to 12 carbon atoms.

2. 2. The toner composition for developing electrostatic images according to claim 1, wherein said organic material comprises decylsilane.

Citation Information

Patent Citations

  • Toner

    JP2003122046A

  • Multi-color toner, image formation device, and image formation method

    JP2017003659A

  • Toner external additive for electrostatic latent image development

    JP2019109297A

  • Toner, toner storage unit, developer, image forming apparatus, and image forming method

    JP2021128218A

  • Toner and method for manufacturing the same, and developer including the same

    JP2021128245A