Conductive film and conductive member

A conductive film made of entangled nanowires of transition metal and chalcogen elements addresses the underutilization of chalcogenides by providing a thin, flexible, and transparent conductive solution with high conductivity, suitable for diverse applications.

JP7570659B2Active Publication Date: 2024-10-22TOKYO METROPOLITAN PUBLIC UNIVERSITY CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020079285
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-28
Publication Date
2024-10-22
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

Existing technologies have not fully explored new structures and uses for chalcogenides, which possess unique properties that could be leveraged for various applications.

Method used

A conductive film composed of entangled thin wires, each made of nanowires formed by bonding transition metal and chalcogen elements, with optional alignment, supported by a substrate like silicon, quartz, or sapphire, produced through a chemical vapor deposition method.

Benefits of technology

The conductive film is thin, flexible, and transparent, with high conductivity and electrical resistivity, enabling applications such as transparent conductive films and channels in transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570659000001
    Figure 0007570659000001
  • Figure 0007570659000002
    Figure 0007570659000002
  • Figure 0007570659000003
    Figure 0007570659000003
Patent Text Reader

Abstract

To provide a thin, novel conductive film that has conductivity.SOLUTION: A conductive film includes multiple thin wires intertwined with one another. Each of the multiple thin wires includes a nanowire in which a transition metal element and a chalcogen element are bonded.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive film. and Conductive Part Material Regarding. [Background technology]

[0002] Low-dimensional materials such as fullerenes, nanotubes, graphene, and transition metal dichalcogenides have attracted attention due to their unique properties.

[0003] For example, Patent Documents 1 and 2 describe layered two-dimensional metal chalcogenides composed of chalcogens and transition metals, and their manufacturing methods, while Patent Document 3 describes nanofibers composed of Group V transition metal dichalcogenide crystals. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2019-522106 [Patent Document 2] Patent No. 3302108 Publication [Patent Document 3] International Publication No. 2004 / 108593 Summary of the Invention [Problem to be solved by the invention]

[0005] Due to their unique properties, chalcogenides are expected to be used in a variety of applications, and new structures and applications of chalcogenides are being explored.

[0006] The present invention has been made in consideration of the above problems, and provides a new thin conductive film that is conductive. [Means for solving the problem]

[0007] (1) A conductive film according to a first aspect has a plurality of entangled thin wires, each of which includes a nanowire in which a transition metal element and a chalcogen element are bonded to each other.

[0008] (2) In the conductive film according to the above aspect, each of the plurality of thin lines may be a bundle of the nanowires.

[0009] (3) In the conductive film according to the above aspect, the orientation direction of each of the plurality of fine lines may be random.

[0010] (4) In the conductive film according to the above aspect, each of the plurality of thin wires may be oriented mainly in a first direction.

[0011] (5) In the conductive film according to the above aspect, the transition metal element may be an element of Group 5 or 6 of the periodic table.

[0012] (6) A conductive member according to a second aspect includes the conductive film according to the above aspect and a substrate supporting the conductive film.

[0013] (7) The conductive member according to the above aspect may contain an alkali metal element on the surface of the substrate that supports the conductive film.

[0014] (8) The substrate may be made of silicon, quartz, or sapphire.

[0015] (9) A third aspect of the method for producing a conductive film involves heating a transition metal compound, a chalcogen precursor, an alkali metal compound, and a substrate in the same space, and growing crystals of nanowires on the substrate in which a transition metal element and a chalcogen element are bonded.

[0016] (10) In the conductive film manufacturing method according to the above aspect, a solvent containing the transition metal contained in the transition metal compound may be applied to the surface of the substrate.

[0017] (11) In the conductive film manufacturing method according to the above aspect, the substrate may be made of silicon, quartz, or sapphire.

[0018] (12) In the conductive film manufacturing method according to the above aspect, the space may be in a vacuum, an inert gas atmosphere, or a reducing atmosphere.

[0019] (13) In the conductive film manufacturing method according to the above aspect, the heating temperature may be 600° C. or higher and 1200° C. or lower. Effect of the Invention

[0020] The conductive film and conductive member according to the above aspect are thin and conductive. [Brief description of the drawings]

[0021] [Figure 1] FIG. 2 is a plan view of the conductive member according to the first embodiment. [Diagram 2] 2 is a schematic cross-sectional view of a thin wire constituting a conductive film according to the first embodiment. FIG. [Diagram 3] FIG. 2 is a schematic diagram of a nanowire constituting a thin line according to the first embodiment. [Figure 4] 2A to 2C are schematic diagrams illustrating a method for manufacturing a conductive member according to the first embodiment. [Diagram 5] FIG. 11 is a plan view of a conductive member according to a second embodiment. [Figure 6] FIG. 2 is a schematic diagram showing how to measure the electrical conductivity of a thin wire. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. They may be modified as appropriate within the scope of the effects of the present invention.

[0023] First, the directions are defined. The x and y directions are substantially parallel to one surface of a substrate, which will be described later. The x and y directions are perpendicular to each other. The z direction is perpendicular to the one surface of the substrate.

[0024] "First embodiment" FIG. 1 is a plan view of a conductive member 10 according to a first embodiment. The conductive member 10 has a substrate Sub and a plurality of thin wires 1. The white lines in FIG. 1 are the thin wires 1, and the black parts are the substrate Sub supporting the plurality of thin wires 1. The plurality of thin wires 1 spread out on the substrate Sub. The plurality of thin wires 1 form a network. The orientation direction of each of the plurality of thin wires 1 is random. The plurality of thin wires 1 are intertwined with each other. The thin wires 1 may be bonded to other thin wires 1, or may be in contact with each other so as to straddle the other thin wires.

[0025] A plurality of fine wires 1 become a conductive film by being entangled. The conductive film is composed of a plurality of entangled fine wires 1, with gaps between the fine wires. The density of the fine wires 1 when viewed in a plan view from the z direction is, for example, 3% or more and 100% or less. The conductive film is optically transparent in the z direction. For example, when the density range of the fine wires 1 is within the above range, the conductive film transmits 1% or more of light. The optical transmittance of the conductive film can be increased to 99% or more by reducing the density of the fine wires 1. The conductive film is flexible. The conductive film is peelable from the substrate Sub. There is no particular limit to the size of the conductive film in the x and y directions.

[0026] 2 is a schematic cross-sectional view of a thin wire 1 constituting the conductive film according to the first embodiment. The thin wire 1 has electrical conductivity. The electrical resistivity of the thin wire 1 is, for example, 1.0×10-5 The thin wire 1 has a resistance of, for example, 1.0×10 -6 An electrical resistivity of Ωm or less can also be achieved. The diameter of the thin wire 1 is, for example, 1 nm or more and 1000 nm or less, and may be 10 nm or more and 500 nm or less. The thin wire 1 includes, for example, a plurality of nanowires 2. The plurality of nanowires 2 are, for example, bundled together to form the thin wire 1. The thin wire 1 includes, for example, 2 to 20 nanowires 2. The length of the thin wire 1 is, for example, 10 nm or more and 10 mm or less. Atoms may be inserted between the plurality of nanowires 2. The inserted atoms are, for example, Li, Na, and K.

[0027] 3 is a schematic diagram of a nanowire 2 constituting the thin wire 1 according to the first embodiment. Each of the nanowires 2 has a transition metal element and a chalcogen element. The nanowire 2 is, for example, one in which the transition metal element and the chalcogen element are bonded and grown one-dimensionally. The nanowire 2 is a crystal in which the transition metal element and the chalcogen element are spatially regularly arranged.

[0028] The composition ratio of the transition metal element to the chalcogen element in the nanowire 2 is approximately 1:1. The nanowire 2 has a stoichiometric composition, and is expressed as, for example, MX, where M is a transition metal element and X is a chalcogen element. The nanowire 2 does not necessarily have to have a stoichiometric composition, and a slight deviation in the composition ratio is acceptable. A slight deviation in the composition ratio is, for example, a deviation in the composition ratio of within 5%.

[0029] The transition metal element M is, for example, an element of group 5 or 6 of the periodic table. The transition metal element M is, for example, one or more elements selected from the group consisting of V, Nb, Ta, Cr, Mo, and W, for example, Mo or W. The chalcogen element X is, for example, one or more elements selected from the group consisting of S, Se, Te, and Po, for example, any one of S, Se, and Te, for example, Te.

[0030] As described above, the conductive film is supported by, for example, the substrate Sub. The substrate Sub is, for example, silicon, quartz, or sapphire. When the orientation direction of the nanowires 2 is random, the substrate Sub is, for example, amorphous silicon. This is because the nanowires 2 grow under the influence of the surface condition of the substrate Sub, as will be described in detail later. The surface of the substrate Sub that supports the conductive film may contain an alkali metal element on the surface. The alkali metal element is, for example, K or Na.

[0031] Next, a method for producing a conductive member will be described. Fig. 4 is a schematic diagram for explaining the method for producing a conductive member according to the first embodiment. The conductive film can be formed on the substrate Sub by using a chemical vapor deposition method (CVD method).

[0032] First, a transition metal compound 21, a chalcogen precursor 22, an alkali metal compound 23, and a substrate Sub are placed in a heating tube 20. The transition metal compound 21, the chalcogen precursor 22, the alkali metal compound 23, and the substrate Sub are arranged in the same space Sp. The transition metal compound 21 and the chalcogen precursor 22 are arranged, for example, spaced apart. By arranging the transition metal compound 21 and the chalcogen precursor 22 at a distance, it becomes easier to control the sublimation temperatures of each.

[0033] The chalcogen precursor 22 is disposed, for example, upstream in the gas flow direction from the transition metal compound 21. By disposing the chalcogen precursor 22, which has a higher vapor pressure than the transition metal compound 21, on the upstream side, the chalcogen vapor can be efficiently supplied to the transition metal compound 21.

[0034] The transition metal compound 21 is, for example, an oxide of a transition metal. The chalcogen precursor 22 is, for example, a compound of chalcogen or an elemental chalcogen. The alkali metal compound 23 is an alkali halide, for example, KBr. The alkali metal compound 23 lowers the melting point of the transition metal compound 21 and assists the growth of the nanowire 2.

[0035] The weight ratio of the transition metal compound 21 and the chalcogen precursor 22 is set so that the supply ratio of the chalcogen element to the transition metal element in the heating tube 20 is, for example, 1:1. In the heating tube 20, the supply ratio of the chalcogen element to the supply ratio of the transition metal element is, for example, preferably 0.5 to 1.5 times, more preferably 0.7 to 1.1 times. Furthermore, when tellurium is used as the chalcogen element, nanowires tend to grow one-dimensionally.

[0036] The substrate Sub is, for example, silicon, quartz, or sapphire, and is, for example, amorphous silicon. A solvent containing a transition metal contained in a transition metal compound may be applied to the surface of the substrate Sub. The transition metal element contained in the solvent acts as a nucleus to promote the growth of the nanowires 2. The solvent in the solvent is removed when heated.

[0037] Next, the heating tube 20 is heated. During heating, the inside of the space Sp is, for example, a vacuum, an inert gas atmosphere, or a reducing atmosphere. For example, nitrogen gas and hydrogen gas are flowed into the heating tube 20. By setting the atmosphere in the space Sp as described above, oxidation of the raw material and the nanowires 2 to be generated can be prevented.

[0038] The heating temperature of the heating tube 20 is, for example, 600° C. or more and 1200° C. or less. The heating temperature of the heating tube 20 is preferably 650° C. or more and 900° C. or less, and more preferably 760° C. or more and 800° C. or less. The heating tube 20 is heated to a predetermined temperature over 10 minutes or more, for example, and then maintained at the predetermined temperature for several minutes, and then rapidly cooled to room temperature.

[0039] When the heating tube 20 is heated, the transition metal compound 21 and the chalcogen precursor 22 are gasified. The gasified transition metal element and the chalcogen element reach the substrate Sub and grow on the surface of the substrate Sub. The nanowires 2 grow under the influence of the substrate Sub. When the substrate Sub is amorphous, the influence of the substrate Sub is small, and the orientation direction of the fine wires 1 tends to be random as shown in FIG. 1.

[0040] By the above procedure, a conductive film in which thin wires 1, which are bundles of nanowires 2, are entangled can be produced on the substrate Sub.

[0041] As described above, the conductive film according to this embodiment is formed by entangling nanowires 2, which are one-dimensional crystals of transition metal elements and chalcogen elements. Since each of the nanowires 2 is conductive, the conductive film is also conductive. In addition, since the conductive film can be manufactured using a CVD method, it is easy to increase the area by using a large substrate Sub. In addition, the one-dimensional crystal is a repetition of a single structure, and can be used to explore new physical properties and applications. For example, the conductive film has spaces between the fine wires 1 and can be used as a transparent conductive film with optical transparency. In addition, the conductive film can be applied to the channel of a transistor, the conductive part of a thermoelectric element, etc.

[0042] "Second embodiment" Fig. 5 is a plan view of a conductive member 11 according to the second embodiment. The conductive member 11 has a substrate Sub and a plurality of thin wires 5. The white lines in Fig. 5 are the thin wires 5, and the black parts are the substrate Sub supporting the plurality of thin wires 5. In the conductive member 11 according to the second embodiment, a description of the same configuration as that of the conductive member 10 according to the first embodiment will be omitted.

[0043] Conductive member 11 according to the second embodiment differs from conductive member 10 according to the first embodiment in that thin wires 5 are oriented in one direction. Other structure and configuration of thin wires 5 are similar to that of thin wire 1 described above.

[0044] Each of the multiple thin wires 5 is mainly oriented in a first direction. Here, mainly means that the proportion of thin wires 5 that satisfy the condition that the main direction in which the thin wires 5 extend has an inclination angle of 20° or less with respect to the first direction is 75% or more of the total. Some of the thin wires 5 extend in a direction intersecting with the first direction. The thin wires 5 extending in a direction intersecting with the first direction connect adjacent thin wires 5. As a result, some of the thin wires 5 are entangled with each other, and the entirety forms a conductive film.

[0045] The substrate Sub is, for example, silicon, quartz, or sapphire. When the orientation direction of the fine wires 5 is uniform as shown in Fig. 5, the substrate Sub is, for example, quartz or sapphire. For example, the A-plane, C-plane, or R-plane of sapphire is exposed on the surface.

[0046] The method for manufacturing the conductive member 11 according to the second embodiment is the same as the method for manufacturing the conductive member 10 according to the first embodiment. The thin wires 5 grow under the influence of the surface state of the substrate Sub. For example, if the substrate Sub has crystallinity, the thin wires 5 grow along the crystal plane, and the orientation direction of the thin wires 5 is aligned.

[0047] The conductive member 11 according to the second embodiment has the same effects as the conductive member 10 according to the first embodiment. In addition, since the orientation direction of the thin wires 5 in the conductive member 11 is uniform, the conductive member 11 has different electrical conductivity in a first direction and a direction perpendicular to the first direction, and can be used as a conductive film having anisotropy in electrical resistivity.

[0048] The preferred embodiments of the present invention have been described above in detail. The characteristic configurations in the embodiments and modifications may be combined with each other. EXAMPLES

[0049] Example 1 In a quartz tube with a diameter of 1.5 cm and a length of 6 cm, the substrate and 100 mg of WO 3 (Sigma-Aldrich, purity 99% or more) and 10 mg of anhydrous KBr (Sigma-Aldrich, purity 99% or more) were placed in the chamber. 3 The anhydrous KBr solution was placed in a quartz boat. The substrate was a silicon substrate (SiO 2 / Si) was used.

[0050] Next, the quartz tube was inserted into a quartz chamber with a diameter of 3 cm and a length of 100 cm, and placed in the center of an electric furnace (ARF-30KC, manufactured by Asahi Rika Seisakusho). Next, 3 g of Te (manufactured by Sigma-Aldrich, purity 99.99%), which was an excess amount of reaction, was placed in an alumina boat, and placed upstream of the quartz boat.

[0051] Then, fill the reaction space with N 2 The mixture was replaced with N 2 The gas flow rate was fixed at 320 sccm. The substrate was heated to 750°C and Te to 650°C simultaneously over 15 min. When the desired temperatures were reached, H 2 Gas was flowed into the reaction space at 10 sccm and maintained for 5 minutes. 2 The gas supply was stopped and the mixture was cooled rapidly to room temperature.

[0052] As a result, the conductive film shown in Figure 1 was obtained. The sheet resistance of the conductive film was measured and found to be 500 Ω / sq. Furthermore, as shown in Figure 6, one thin wire was taken out and its electrical resistivity was measured. The thickness of the thin wire was measured using an atomic force microscope (AFM) and found to be approximately 45 nm. The electrical resistivity of the thin wire was 1.0 x 10 -6 The Raman spectrum of the thin wire was measured while changing the angle between the deflection of the incident beam and the nanowire axis. The Raman spectrum gradually decreased as the deflection angle changed, and reached a minimum when the incident beam was perpendicular to the nanowire axis. This characteristic was also confirmed in carbon nanotubes, and it was confirmed that the nanowire is a one-dimensional crystal.

[0053] Example 2 Example 2 differs from Example 1 in that a quartz substrate was used as the substrate. The other conditions were the same as those of Example 1. As a result, the conductive film shown in FIG. 5 was obtained.

[0054] Example 3 Example 3 differs from Example 1 in that a sapphire substrate was used as the substrate. The sapphire substrate was cut along the C plane, and the C plane was used as the growth surface of the conductive film. The other conditions were the same as in Example 1. As a result, a conductive film similar to that shown in FIG. 5 was obtained. Similar results were also obtained when the A plane and R plane of sapphire were used.

[0055] Example 4 Example 4 differs from Example 1 in that the following treatment was carried out before placing the substrate in the quartz tube. The other conditions were the same as those of Example 1.

[0056] First, the surface of the substrate was irradiated with ultraviolet light for 30 minutes (PL16-110, manufactured by Sen Tokushu Kogen Co., Ltd.). Then, the surface of the substrate was coated with a solution by spin coating. The solution was 5 mg / mL Na 2 O 4 W 2H 2 O (Sigma-Aldrich, purity 99.995%) was used. Spin coating was performed at 3000 rpm for 1 minute.

[0057] In the case of Example 4, as in Example 1, a conductive film similar to that shown in FIG. 1 was obtained. [Explanation of symbols]

[0058] 1, 5 thin line 2. Nanowires 10, 11 Conductive member 20 heating tube 21 Transition metal compounds 22 Chalcogen Precursors 23 Alkali metal compounds Sub board M transition metal element X Chalcogen elements

Claims

1. A plurality of intertwined thin wires are included. Each of the plurality of thin wires includes a nanowire in which tungsten and a chalcogen element are bonded in a stoichiometric composition represented as WX (X is a chalcogen element), A conductive film, wherein each of the plurality of fine lines is primarily oriented in a first direction.

2. The conductive film according to claim 1 , wherein each of the plurality of fine lines is a bundle of the nanowires.

3. The conductive film according to claim 1 or 2, A conductive member comprising: a substrate supporting the conductive film.

4. The conductive member according to claim 3 , further comprising an alkali metal element on a surface of the substrate that supports the conductive film.

5. The conductive film according to claim 1 ; A substrate supporting the conductive film, The substrate is a conductive member made of quartz or sapphire.

Citation Information

Patent Citations

  • Nanoribbon and manufacturing method therefor

    JP2018123039A

  • Manufacturing method of two-dimensional transition metal dichalcogenide thin film

    JP2018525516A

  • Chemical vapor deposition method for producing two-dimensional materials

    JP2019522106A

  • Oriented Polycrystalline Thin Films of Transition Metal Chalcogenides

    JP3302108B2

  • Method for Synthesizing Transition Metal Chalcogenide Using CVD

    KR1020170048873A