CURABLE COMPOSITION AND OPTICAL MEMBER COMPRISING THE SAME
A curable composition with episulfide and sulfur-containing polymer compounds addresses the limitations of high refractive index polymers by enhancing strength, hardness, and optical properties, achieving a high refractive index and low deformation for optical members.
Patent Information
- Application Number
- JP2023541119
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-02
- Filing Date
- 2022-03-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-08
AI Technical Summary
Existing high refractive index polymers face challenges with low Abbe number, chromatic aberration, and deformation due to low glass transition temperature, making them unsuitable for long-term use in devices.
A curable composition comprising an episulfide compound and a sulfur-containing polymer compound is used to form a high refractive index optical member, which includes specific repeating units and molecular weights to enhance strength, hardness, and optical properties.
The composition achieves a high refractive index of 1.710 or more, low haze and yellowness, and a glass transition temperature of 65°C or higher, making it suitable for replacing glass lenses in devices with improved durability and optical performance.
Smart Images

Figure 0007570763000001 
Figure 0007570763000002 
Figure 0007570763000003
Abstract
Description
[Technical field]
[0001] Cross-references to related applications (etc.) This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0031499 filed on March 10, 2021 and Korean Patent Application No. 10-2022-0026941 filed on March 2, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a curable composition for forming a high refractive index optical member and an optical member containing the same. [Background technology]
[0003] High Refractive Index Polymer (HRIP) is generally defined as a polymer material with a refractive index of 1.50 or more, and is used as a coating / sealing material to increase the light extraction efficiency of light-emitting diodes (LEDs) and as a microlens material for image sensors.
[0004] Ordinary glass lenses can cause fatal damage to the user's eyeball when broken, and are inconvenient to wear for long periods of time because they are highly dense and heavy. However, lenses made of high refractive index polymers are lighter than glass lenses and easier to wear, less likely to break and even if they do break, they are relatively safer than glass lenses, and can be made in a variety of colors.
[0005] However, in highly refractive polymers, there is generally a trade-off between the refractive index and chromatic aberration (Abbe number), so lenses using such highly refractive polymers have the problem of having a relatively low Abbe number and a low glass transition temperature, which causes deformation due to heat generation when the lenses are used in devices and the like. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a curable composition for forming a high refractive index optical member, which is lighter than glass or reinforced glass used in existing lenses, has excellent strength and hardness, can realize various colors, can realize a high refractive index, has a low yellow index value, and has excellent optical properties, has a high glass transition temperature and is less deformed, and an optical member including the same. [Means for solving the problem]
[0007] The present specification provides a curable composition for forming a high refractive index optical member, which contains an episulfide compound and a sulfur-containing polymer compound.
[0008] The present specification also provides an optical member comprising the episulfide compound and the sulfur-containing polymer compound.
[0009] Hereinafter, the curable composition according to the specific embodiment of the present invention and the optical member including the same will be described in more detail.
[0010] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise.
[0011] As used herein, the meaning of "comprising" is to embody certain properties, regions, integers, steps, operations, elements, components and / or ingredients, and does not exclude the presence or addition of other certain properties, regions, integers, steps, operations, elements, components and / or groups.
[0012] As used herein, the term "episulfide compound" is defined as a compound containing one or more episulfides, where an episulfide refers to a compound in which an oxygen (O) atom of an epoxide is replaced with a sulfur (S) atom.
[0013] The definition of "sulfur-containing polymeric compound" as used herein means a polymer that essentially contains a sulfur atom.
[0014] As used herein, "curing" refers to both heat curing and photocuring, and a "curable composition" refers to a composition that can be heat cured and / or photocured.
[0015] As used herein, high refractive index means greater than about 1.600 in the wavelength region of 350 to 800 nm or at 632.8 nm wavelength.
[0016] The term "substituted or unsubstituted" as used herein means that the group is substituted or unsubstituted with one or more substituents selected from the group consisting of deuterium, halogen, nitrile, nitro, hydroxy, carbonyl, ester, imide, amino, phosphine oxide, alkoxy, aryloxy, alkylthio, arylthio, alkylsulfoxy, arylsulfoxy, silyl, boron, alkyl, cycloalkyl, alkenyl, aryl, aralkyl, aralkenyl, alkylaryl, alkylamine, aralkylamine, heteroarylamine, arylamine, arylphosphine, or heterocyclic group containing one or more of N, O, and S atoms, or is substituted or unsubstituted with a substituent in which two or more of the above-listed substituents are linked. For example, the "substituent in which two or more substituents are linked" may be a biphenyl group. In other words, the biphenyl group may be an aryl group, and may be interpreted as a substituent in which two phenyl groups are linked.
[0017] According to one embodiment of the present invention, the sulfur-containing polymer compound includes an episulfide compound and a sulfur-containing polymer compound, and the sulfur-containing polymer compound is S n+1 (n is an integer of 1 to 20), and one or more repeating units selected from the group consisting of repeating units containing selenium and sulfur.
[0018] The present inventors have discovered that a composition containing an episulfide compound and a sulfur-containing polymer compound and an optical member containing the same are lighter than glass or reinforced glass used in existing lenses, have excellent physical properties such as strength and hardness, and have excellent optical properties due to high transmittance and low yellow index (YI), have a high glass transition temperature and are less deformed by heat, and can provide an optical material that can replace previously used glass and plastic materials, which has led to the present invention.
[0019] As a result, the curable composition and an optical member including the same can be used as a substitute for existing glass or optical glass in products and commercial fields, such as display substrates, protective films for displays, lenses for image sensors in touch panels and wearable devices, and coating / sealing materials for increasing the light extraction efficiency of light-emitting diodes (LEDs), etc.
[0020] The sulfur-containing polymer compound contained in the curable composition is S n+1 (n is an integer from 1 to 20) and one or more repeating units selected from the group consisting of repeating units containing selenium and sulfur.
[0021] The sulfur-containing polymer compound can be used as a curing agent for curing a curable composition containing an episulfide compound, and thereby, while improving the optical properties related to transmittance, haze, and yellowness of an optical member that is a cured product of the curable composition, the glass transition temperature can be increased to 65° C. or higher, and the optical member can exhibit a high refractive index of 1.710 or higher.
[0022] For example, the sulfur-containing polymer compound may include a repeating unit represented by the following formula 1 or 2: [ka] In the above Chemical Formula 1, R1 is a substituted or unsubstituted alkylene having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms; a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a substituted or unsubstituted heteroarylene having 2 to 30 carbon atoms containing one or more of oxygen (O), nitrogen (N) and sulfur (S) atoms; -R a OR b -;-R c COOR d -;-R e SO2R f -or-R g SOR h - and R a Or R h each independently represents a single bond, a substituted or unsubstituted alkylene having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms, or a substituted or unsubstituted arylene having 5 to 30 carbon atoms; n is an integer from 1 to 20, [ka] In the above Chemical Formula 2, R2 is a substituted or unsubstituted alkylene having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms; a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a substituted or unsubstituted heteroarylene having 2 to 30 carbon atoms containing one or more of oxygen (O), nitrogen (N) and sulfur (S) atoms; -R a OR b -;-R c COOR d -;-R e SO2R f -or-R g SOR h - and R a Or R h each independently represents a single bond, a substituted or unsubstituted alkylene having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms, or a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a and b are each independently an integer of 0 to 10, a+b is an integer between 1 and 20.
[0023] For example, a and b may each independently be 0 to 7, 0 to 5, or 1 to 3; and a+b may be 1 to 10, 2 to 7, or 3 to 5.
[0024] In the above Chemical Formula 1, n may be 1 to 20, 1 to 18, 5 to 15, or 8 to 13. For example, the following Chemical Formula 1 may be a repeating unit represented by the following Chemical Formula 1-1 or 1-2. [ka] [ka] In the above chemical formulas 1-1 and 1-2, R1 is the same as defined above.
[0025] In addition, the repeating units represented by Chemical Formula 2 may be one selected from the repeating units represented by Chemical Formulas 2-1 to 2-4 below. [ka] [ka] [ka] [ka] In the above formulas 2-1 to 2-4, R2 is the same as defined above.
[0026] In the definitions of R1 and R2, the substituted or unsubstituted alkylene having 1 to 20 carbon atoms may be methylene, ethylene, propylene, isopropylene, butylene, isobutylene, tert-butylene, pentylene, isopentylene, neopentylene, tert-pentylene, hexylene, 2-methylpentylene, heptylene, 1-ethylpentylene, octylene, 2-ethylhexylene, isooctylene, nonylene, isononylene, decylene, isodecylene, undecylene, or dodecylene.
[0027] Furthermore, the alkylene having 1 to 20 carbon atoms may be substituted with a halogen group. For example, the halogen group may be a fluoro group, a bromo group, or a chloro group.
[0028] In the definitions of R1 and R2, the substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms includes 1,3-cyclopentylene, 1,3-(2-methyl)cyclopentylene, 1,4-(2-methyl)cyclopentylene, 1,5-(2-methyl)cyclopentylene, 1,3-(2-ethyl)cyclopentylene, 1,4-(2-ethyl)cyclopentylene, and 1,5-(2-ethyl)cyclopentylene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, 1,3-(2-methyl)cyclohexylene, 1,4-(2-methyl)cyclohexylene, and 1,5-(2-methyl)cyclohexylene and 1,6-(2-methyl)cyclohexylene, 1,3-(2-ethyl)cyclohexylene, 1,4-(2-ethyl)cyclohexylene, 1,5-(2-ethyl)cyclohexylene, 1,6-(2-ethyl)cyclohexylene, 1,3-(2-propyl)cyclohexylene, 1,4-(2-propyl)cyclohexylene, 1,5-(2-propyl)cyclohexylene, 1,6-(2-propyl)cyclohexylene, 1,3-(2-isopropyl)cyclohexylene, 1,4-(2-isopropyl)cyclohexylene, 1,5-(2-isopropyl)cyclohexylene, 1,6-(2-isopropyl)cyclohexylene, 1,3-(2-butyl)cyclohexylene, 1,4-(2-butyl)cyclohexylene, 1,5-(2-butyl)cyclohexylene and 1,6-(2-butyl)cyclohexylene, 1,3-(2-sec-butyl)cyclohexylene, 1,4-(2-sec-butyl)cyclohexylene, 1,5-(2-sec-butyl)cyclohexylene, 1,6-(2-sec-butyl)cyclohexylene, 1,3-(2-tert- butyl)cyclohexylene, 1,4-(2-tert-butyl)cyclohexylene, 1,5-(2-tert-butyl)cyclohexylene, 1,6-(2-tert-butyl)cyclohexylene, 1,2-cycloheptylene, 1,3-cycloheptylene, 1,4-cycloheptylene, 1,3-(2-methyl)cycloheptylene, 1,4-(2-methyl)cycloheptylene, 1,5-(2-methyl)cycloheptylene, 1,6-(2-methyl)cycloheptylene and 1,7-(2-methyl)cycloheptylene, 1,3-(2-ethyl)cycloheptylene, 1,4-(2-ethyl)cycloheptylene, 1,5-(2-ethyl)cycloheptylene, 1,6-(2-ethyl)cycloheptylene and 1,7-(2-ethyl)cycloheptylene, 1,3-(2-propyl)cycloheptylene, 1,4-(2-propyl)cycloheptylene, 1,5-(2-propyl)cycloheptylene, 1,6-(2-propyl)cycloheptylene, 1,7-(2-propyl)cycloheptylene, 1,3-(2-isopropyl)cycloheptylene, 1,4-(2-isopropyl)cycloheptylene, 1,5-(2-isopropyl)cycloheptylene Cycloheptylene, 1,6-(2-isopropyl)cycloheptylene, 1,7-(2-isopropyl)cycloheptylene, 1,3-(2-butyl)cycloheptylene, 1,4-(2-butyl)cycloheptylene, 1,5-(2-butyl)cycloheptylene, 1,6-(2-butyl)cycloheptylene and 1,7-(2-butyl)cycloheptylene, 1,3-(2-sec-butyl)cycloheptylene, 1,4-(2-sec-butyl)cycloheptylene, 1,5-(2-sec-butyl)cycloheptylene, 1,6-(2-sec-butyl)cycloheptylene Heptylene, 1,7-(2-sec-butyl)cycloheptylene, 1,3-(2-tert-butyl)cycloheptylene, 1,4-(2-tert-butyl)cycloheptylene, 1,5-(2-tert-butyl)cycloheptylene, 1,6-(2-tert-butyl)cycloheptylene, 1,7-(2-tert-butyl)cycloheptylene, 1,2-cyclooctylene, 1,3-cyclooctylene, 1,4-cyclooctylene and 1,5-cyclooctylene, 1,3-(2-methyl)cyclooctylene, 1,4-(2-methyl)cyclooctylene. cyclooctylene, 1,5-(2-methyl)cyclooctylene, 1,6-(2-methyl)cyclooctylene, 1,7-(2-methyl)cyclooctylene, 1,8-(2-methyl)cyclooctylene, 1,3-(2-ethyl)cyclooctylene, 1,4-(2-ethyl)cyclooctylene, 1,5-(2-ethyl)cyclooctylene, 1,6-(2-ethyl)cyclooctylene, 1,7-(2-ethyl)cyclooctylene, 1,8-(2-ethyl)cyclooctylene, 1,3-(2-propyl)cyclooctylene, 1,4-(2-propyl)cyclooctylene, 1,5-(2-propyl)cyclooctylene, 1,6-(2-propyl)cyclooctylene, 1,7-(2-propyl)cyclooctylene, 1,8-(2-propyl)cyclooctylene, 2,3-(1,4-dioxanylene), 2,5-(1,4-dioxanylene) and 2,6-(1,4-dioxanylene), 2,4-morpholinylene, 3,4-morpholinylene, 2,5-tetrahydrofurylene, 3,4-tetrahydrofurylene, 1,2-pyrrolidinylene, 1,3-pyrrolidinylene, 2,5-pyrrolidinylene and 3,4-pyrrolidinylene, and also 1,2-piperidylene, 1,3-piperidylene, 1,4-piperidylene, 2,3-piperidylene or 2,6-piperidylene.
[0029] In the definitions of R1 and R2, the substituted or unsubstituted arylene having 5 to 30 carbon atoms includes 1,2-phenylene, 1,3-phenylene, 1,4-phenylene, 1,2-naptylene, 2,3-naptylene, 1,4-naptylene, 1,5-naptylene, 2,6-naptylene, 1,8-naptylene, 2,5-pyrylene, 3,4-pyrylene, 2,3-pyridylene, 2,4-pyridylene, 2,5-pyridylene, 2,6-pyridylene, 3,5-pyridylene, 2,4-pyrimidylene, 2,5-pyrimidylene, 2,3-pyrazylene, 2,5-pyrazylene, and and 2,6-pyrazylene, 3,5-pyrazolylene, 1,2-imidazolylene, 1,4-imidazolylene, 1,5-imidazolylene, 2,4-imidazolylene, 2,5-imidazolylene, 2,4-diazolylene and 2,5-diazolylene, 3,5-(1,2,4-triazylene), 3,6-(1,2,4-triazylene), 2,4-(1,3,5-triazylene), 3,5-quinalzylene, 3,6-quinalzylene, 3,8-quinalzylene, 5,8-quinalzylene, 3,5-quinolinylene, 3,6-quinolinylene, 3,8-quinolinylene, 5,8-quinolinylene. 1,3-isoquinolylene, 1,4-isoquinolylene, 1,5-isoquinolylene, 1,6-isoquinolylene, 2-methyl-1,3-phenylene, 2-methyl-1,4-phenylene, 2-methyl-1,5-phenylene, 2-methyl-1,6-phenylene, 2,3-dimethyl-1,4-phenylene, 2,3-dimethyl-1,5-phenylene, 2,3-dimethyl-1,6-phenylene, 2,4-dimethyl-1,3-phenylene, 2,4-dimethyl-1,5-phenyl, 2,4-dimethyl-1,5-phenyl, 2,4-dimethyl- 1,6-phenylene, 2,5-dimethyl-1,3-phenylene, 2,5-dimethyl-1,4-phenylene, 2,5-dimethyl-1,6-phenylene, 2,4,5-trimethyl-1,3-phenylene, 2,4,5-trimethyl-1,6-phenylene, 2,4,6-trimethyl-1,3-phenylene, 2-ethyl-1,3-phenylene, 2-ethyl-1,4-phenylene, 2-ethyl-1,5-phenylene, 2-ethyl-1,6-phenylene, 2,3-diethyl-1,4-phenylene, 2,3-diethyl-1,5-phenylene, 2,3-diethyl-1,6-phenylene, 2,4-diethyl-1,3-phenylene, 2,4-diethyl-1,5-phenylene, 2,4-diethyl-1,6-phenylene, 2,5-diethyl-1,3-phenylene, 2,5-diethyl-1,4-phenylene, 2-methoxy-1,3-phenylene, 2-methoxy-1,4-phenylene, 2-methoxy-1,5-phenylene, 2-methoxy-1,6-phenylene, 2,3-dimethoxy-1,4-phenylene, 2,3-dimethoxy-1,5-phenylene, 2,3-dimethoxy-1,6-phenylene, 2,4-dimethoxy-1 ,3-phenylene, 2,4-dimethoxy-1,5-phenylene, 2,4-dimethoxy-1,6-phenylene, 2,5-dimethoxy-1,3-phenylene, 2,5-dimethoxy-1,4-phenylene, 2,5-dimethoxy-1,6-phenylene, 2,4,5-trimethoxy-1,3-phenylene, 2,4,5-trimethoxy-1,6-phenylene, 2,4,6-trimethoxy-1,3-phenylene, 2-ethoxy-1,3-phenylene, 2-ethoxy-1,4-phenylene, 2-ethoxy-1,5-phenylene, 2-ethoxy-1,6-phenylene 2,3-diethoxy-1,4-phenylene, 2,3-diethoxy-1,5-phenylene, 2,3-diethoxy-1,6-phenylene, 2,4-diethoxy-1,3-phenylene, 2,4-diethoxy-1,5-phenylene, 2,4-diethoxy-1,6-phenylene, 2-chloro-1,3-phenylene, 2-chloro-1,4-phenylene, 2-chloro-1,5-phenylene, 2-chloro-1,6-phenylene, 2,3-dichloro-1,4-phenylene, 2,3-dichloro-1,5-phenylene, 2,3-dichloro-1,6-phenylene , 2,4-dichloro-1,3-phenylene, 2,4-dichloro-1,5-phenylene, 2-hydroxy-1,3-phenylene, 2-hydroxy-1,4-phenylene, 2-hydroxy-1,5-phenylene, 2-hydroxy-1,6-phenylene, 2,3-dihydroxy-1,4-phenylene, 2-cyano-1,3-phenylene, 2-cyano-1,4-phenylene, 2-cyano-1,5-phenylene, 2-cyano-1,6-phenylene, 2,3-dicyano-1,4-phenylene or 2,3-dicyano-1,5-phenylene.
[0030] For example, R1 and R2 may each independently be methylene, ethylene, propylene, isopropylene, cyclohexylene, cycloheptylene, phenylene, methylphenylene, ethylphenylene, methoxyphenylene, or ethoxyphenylene.
[0031] The sulfur-containing polymer compound may include any one selected from the group consisting of the following repeating units: [ka]
[0032] The sulfur-containing polymer compound contains the repeating unit described above, and therefore does not suffer from problems such as a decrease in refractive index even when stored at room temperature for a long period of time. However, in the case of a sulfur-containing polymer compound not containing the repeating unit described above, a problem of a decrease in refractive index may occur when the compound is stored at room temperature for a long period of time, for example, for more than 200 hours, more than 240 hours, or more than 300 hours.
[0033] The sulfur-containing polymer may include 1 to 1000, 2 to 800, 5 to 500, or 10 to 200 repeating units of Formula 1 or Formula 2.
[0034] In addition, the weight average molecular weight of the sulfur-containing polymer may be 250 to 50,000, 500 to 40,000, or 1,000 to 30,000. If the weight average molecular weight of the sulfur-containing polymer is too high, the solubility in the episulfide compound is low, and it is difficult to obtain uniform physical properties such as uniform refractive index deviation and transparency deviation during the manufacture of optical members. If the weight average molecular weight is too low, the refractive index of the optical member formed after curing may be low.
[0035] The weight average molecular weight (Mw) means a molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC). In the process of measuring the weight average molecular weight in terms of polystyrene measured by the GPC method, a commonly known analyzer, a detector such as a refractive index detector, and an analytical column can be used, and commonly applied temperature conditions, solvents, and flow rates can be applied. Specific examples of the measurement conditions include a temperature of 30°C, a chloroform solvent, and a flow rate of 1mL / min. Specific examples of the measurement conditions include a Polymer Laboratories PLgel MIX-B 300mm long column, a Waters PL-GPC220 instrument, an evaluation temperature of 160°C, 1,2,4-trichlorobenzene as a solvent, a flow rate of 1mL / min, a sample prepared to a concentration of 10mg / 10mL, and then supplied in an amount of 200μL, and the Mw value can be obtained using a calibration curve formed using a polystyrene standard. Nine types of polystyrene standards with molecular weights of 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000 were used.
[0036] Meanwhile, the content of the sulfur-containing polymer compound may be 1 to 30 wt%, 2 to 25 wt%, or 5 to 20 wt%, based on 100 wt% of the total curable composition. If the content of the sulfur-containing polymer compound is too high, the haze and yellowness of the optical member formed after curing may be high, and if the content of the sulfur-containing polymer compound is too low, the refractive index of the optical member formed after curing may be low.
[0037] The sulfur-containing polymer compound may be prepared through the following Reaction Scheme 1 or Reaction Scheme 2, but is not limited thereto. [ka]
[0038] The sulfur-containing polymer compound can be prepared by dissolving sulfur (nS) or selenium disulfide (SeS2) in an aqueous Na2S solution, followed by polymerization with a bifunctional organic halogen compound. In this case, in the above-mentioned reaction formulas 1 and 2, the definitions of R1, R2 and n are the same as those described above, the Na2S aqueous solution can be an aqueous L2S solution or an aqueous K2S solution, and the bifunctional organic halogen compound can be a polyfunctional organic halogen compound having three or more functional groups, a bifunctional or polyfunctional organic tosylate compound, a bifunctional or polyfunctional organic mesylate compound, etc.
[0039] The reaction formed in Reaction Scheme 2 [ka] is just an example. [ka] may be, but is not limited thereto.
[0040] Conventionally, a thiol compound containing a thiol group (-SH) has been included in a curable composition for forming a high refractive index optical member. However, in the case of a composition using a thiol compound, a curing reaction proceeds immediately after mixing, causing a rapid increase in viscosity, and a striae phenomenon occurs due to the rapid curing. Therefore, an optical member formed from such a composition has problems such as poor optical properties and physical properties.
[0041] However, since the curable composition for forming a high refractive index optical member according to the embodiment includes the sulfur-containing polymer compound, a rapid curing reaction does not occur immediately after mixing, so that the composition can be stored for a long period of time, and striae development due to rapid curing may not occur.
[0042] The episulfide compound contained in the curable composition is represented by the following chemical formula 3. [ka] In the above Chemical Formula 3, R3 and R4 are each independently hydrogen or alkyl having 1 to 10 carbon atoms; R5 and R6 are each independently a single bond or an alkylene having 1 to 10 carbon atoms; a is an integer from 0 to 4, b is an integer from 0 to 6.
[0043] The episulfide compound may contain a high content of sulfur (S) atoms having a large atomic refraction in the molecule due to the specific chemical structure described above, and such a high content of sulfur atoms can increase the refractive index of the cured product.
[0044] In addition, the episulfide compound can be cured by ring-opening polymerization, and the alkylene sulfide group formed by ring-opening polymerization of the episulfide group can further increase the high refractive index of the cured product.
[0045] Meanwhile, in the above Chemical Formula 3, R3 and R4 may each independently be a hydrogen atom or a methyl group, but are not limited thereto.
[0046] Additionally, R5 and R6 may each independently be a single bond, methylene, ethylene, propylene, isopropylene, butylene, or isobutylene, but are not limited thereto.
[0047] Furthermore, a and b may each independently be 0 or 1.
[0048] In Chemical Formula 3, a refers to the number of carbon atoms in the alkylene group contained in the thioether repeat unit. If a is too large, the length of the carbon chain in the molecule becomes long, and the glass transition temperature of the cured product becomes low upon curing. This may result in a problem of reduced heat resistance of the cured product. In addition, the relative sulfur content becomes low, and thus the refractive index of the cured product becomes low.
[0049] In Chemical Formula 3, b is the repeat number of thioether repeat units in which alkylene groups are linked by sulfur (S) atoms. If b is too large, the molecular chain length becomes long, lowering the glass transition temperature of the cured product during curing, which can cause problems such as reduced heat resistance of the cured product.
[0050] The compound represented by the formula 3 may be used alone or in combination of two or more kinds.
[0051] The episulfide compound may include, for example, at least one selected from the group consisting of bis(β-epithiopropyl)sulfide, bis(β-epithiopropyl)disulfide, bis(β-epithiopropylthio)methane, 1,2-bis(β-epithiopropylthio)ethane, 1,3-bis(β-epithiopropylthio)propane, and 1,4-bis(β-epithiopropylthio)butane, but is not necessarily limited thereto.
[0052] The content of the episulfide compound may be 50 to 99 wt%, 60 to 95 wt%, or 65 to 85 wt%, based on 100 wt% of the total curable composition. If the content of the episulfide compound is too high, the refractive index may be low or the physical and optical properties of the final optical member may be deteriorated, and if the content of the episulfide compound is too low, the yellowness of the final optical member may be increased.
[0053] In addition, the weight ratio of the sulfur-containing polymer compound and the episulfide compound may be 1:2 to 1:30, 1:3 to 1:25, 1:4 to 1:20, 1:4 to 1:15, or 1:4 to 1:13. If the content of the episulfide compound is too low compared to the sulfur-containing polymer compound, yellowness may increase and the polymer compound may not be completely dissolved. If the content of the episulfide compound is too high compared to the sulfur-containing polymer compound, the refractive index of the formed optical member may be low or the physical or optical properties may be deteriorated.
[0054] The curable composition for forming a high refractive index optical member may include sulfur (S8) particles, selenium disulfide (SeS2) particles, or a mixture thereof. The curable composition may include sulfur particles and / or selenium disulfide particles to further improve the refractive index and reduce the haze and yellow index.
[0055] The sulfur (S8) particles may have a particle size of 1 to 200 μm, 2 to 180 μm, or 3 to 170 μm. If the particle size of the sulfur particles is too small, the particle shape may not be maintained, and if the particle size is too large, the transmittance of the high refractive index plastic substrate may be reduced and haze may be increased.
[0056] In addition, the selenium disulfide (SeS2) particles may have a particle size of 1 to 200 μm, 5 to 180 μm, or 10 to 170 μm. If the particle size of the selenium disulfide particles is too small, the particle shape may not be maintained, and if the particle size is too large, the transmittance of the high refractive index plastic substrate may be reduced and haze may be increased.
[0057] The particle size can be measured by, for example, dynamic light scattering, laser diffraction, centrifugal sedimentation, FFF (Field Flow Fractionation), pore electrical resistance, scanning electron microscopy (SEM) analysis, transmission electron microscopy (TEM) analysis, etc.
[0058] When the curable composition further comprises sulfur particles and / or selenium disulfide particles, the content of the sulfur particles relative to 100 wt% of the curable composition may be 0.1 to 30 wt%, 1 to 20 wt%, 2 to 15 wt%, or 3 to 10 wt%, and the content of the selenium disulfide particles relative to 100 wt% of the curable composition may be 0.1 to 30 wt%, 0.5 to 20 wt%, or 0.8 to 15 wt%,.
[0059] The curable composition may include a catalyst. The catalyst is not particularly limited as long as it is a catalyst used in a general curable composition for forming a high refractive index optical member, and may be, for example, a nucleophilic catalyst including an amine or a phosphine.
[0060] Examples of the catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, 4-methyl-N,N-dimethylbenzylamine, N,N-dicyclohexylmethylamine, N-ethyl-N-isopropylpropan-2-amine, and N,N-dimethylcyclohexanamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; phosphorus compounds such as triphenylphosphine; and pyridine compounds such as 2-bromopyridine. Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all of which are trade names for imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT3503N and UCAT3502T (all of which are trade names for dimethylamine blocked isocyanate compounds), DBU, DBN, U-CATSA102, and U-CAT5002 (all of which are bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.
[0061] The content of the catalyst may be 0.001 to 10 wt%, 0.01 to 5 wt%, or 0.1 to 1 wt%, based on 100 wt% of the total curable composition. If the content of the catalyst is too high, the curing speed increases, resulting in a problem of reduced storage stability of the composition, whereas if the content is too low, the curing speed decreases, resulting in a problem of a longer thermal curing process.
[0062] In addition, the curable composition may further include other additives used to impart specific functions to display substrates in the technical field to which the present invention belongs, such as an ultraviolet absorber, a bluing agent, a pigment, etc.
[0063] According to another embodiment of the present invention, there is provided an optical member comprising the episulfide compound and the sulfur-containing polymer compound.
[0064] In addition, the episulfide compound, the sulfur-containing polymer compound, and the sulfur particles, selenium disulfide, catalyst, and other additives contained in the optical member are replaced with those described in the photocurable composition described above.
[0065] Such an optical member can be manufactured by a method of curing the above-mentioned curable composition. Specifically, the above-mentioned curable composition or a homogeneous composition containing various additives in the curable composition can be manufactured, and the composition can be injected into a mold formed by combining a mold made of components such as glass, metal, or polymer resin with a resin gasket, and cured by heating. In this case, in order to facilitate removal of the final resin after molding, the mold can be subjected to a release treatment in advance, or a release agent can be further added to the above-mentioned composition.
[0066] The temperature of the curing reaction may vary depending on the type and content of the compound used, but generally, the reaction may proceed at about 50 to about 120° C., or about 60 to about 100° C., and the curing time may be about 0.1 to about 72 hours, or about 0.5 to about 24 hours.
[0067] The curing reaction may be carried out by combining a process of maintaining the predetermined polymerization temperature for a certain period of time, a temperature increase process, and a temperature decrease process. After the reaction is completed, the resin may be post-treated at a temperature of about 50 to about 150° C. or about 80 to about 120° C. for about 10 minutes to about 3 hours to prevent deformation.
[0068] The optical member released from the mold after polymerization can be provided with various functions through subsequent processes such as dyeing and coding.
[0069] The optical member according to the other embodiment may have a refractive index of 1.710 or more, 1.715 to 1.850, or 1.720 to 1.800, measured at a wavelength of 500 nm to 750 nm, 550 nm to 700 nm, 600 nm to 650 nm, or 632.8 nm.
[0070] In addition, the optical component may have a very high transmittance, specifically, a transmittance value of 75% or more, 77% or more, 80 to 99%, or 85 to 99% when the optical component has a thickness of 1 mm, as measured according to JIS K 7361.
[0071] In addition, the optical member may have a very low haze value, specifically, a haze value of 35% or less, 33% or less, 31% or less, 25% or less, 20% or less, or 10 to 1% when the optical member has a thickness of 1 mm, as measured according to JIS K 7136.
[0072] The optical member may have a glass transition temperature of 65°C or higher, 67°C or higher, 68°C or higher, 70°C to 99°C, or 72°C to 99°C.
[0073] The optical member may have a yellow index (YI) of 0.1 to 50, 1 to 40, or 1 to 35, 1 to 20, 1 to 15, or 1 to 10.
[0074] The optical member according to the other embodiment may be included in a wearable device, and specifically, may be used to replace glass or tempered glass for the lens of the wearable device.
[0075] In other words, the optical member has high refractive index properties comparable to those of glass, but is lighter than glass or reinforced glass, and in addition to mechanical properties such as strength and hardness, it also has excellent optical properties as described above, and can also be used for lenses of wearable devices such as augmented reality devices or virtual reality devices, which have a high glass transition temperature and may generate heat. Effect of the Invention
[0076] According to the present invention, it is possible to provide a curable composition for forming a high refractive index optical member, which is lighter than glass or reinforced glass used in existing lenses, has excellent strength and hardness, can realize various colors, can realize a high refractive index, has low haze and yellow index values, and has excellent optical properties, has a high glass transition temperature and little deformation, and an optical member including the cured product thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0077] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention. However, these examples are presented only as examples of the present invention and do not define the scope of the invention.
[0078] Example 1 60mg of sulfur-containing polymer compound 50A (n is 10, weight average molecular weight: 2,500), 948mg of episulfide compound (70A) (below), 48mg of selenium sulfide particles (SeS2, particle size: 50μm), 144mg of sulfur particles (S8, particle size: 50μm), and 4mg of catalyst (C1) (below) were mixed and filtered using a glass filter with a pore size of 0.45μm. Then, 1mm thick glass slides were placed on both sides of an LCD glass measuring 10cm in width and height, about 1g of the above mixture was applied to the center of the LCD glass, and then another LCD glass was placed on top to prepare a mold. This was placed in an oven and a curing reaction was carried out at about 60℃ for about 12 hours. After removing from the oven, the LCD glass was removed to obtain a plastic specimen that is a flat optical member. The thickness of the plastic specimen was about 1 mm, and this thickness was measured using a Mitutoyo thickness gauge (Model: ID-C112XBS). [ka]
[0079] Examples 2 to 7 The curable composition and the optical component of the cured product thereof were prepared in the same manner as in Example 1, except that the sulfur-containing compound, the episulfide compound, the selenium sulfide particles, the sulfur particles, and the catalyst were used in the compound contents shown in Table 1 below.
[0080] Comparative Example 1 1,000mg of sulfur particles were added to a 5ml vial and stirred at 130℃ until completely dissolved. After the sulfur was completely dissolved, 538mg of divinylbenzene (DVB) was added and stirred at 130℃ for 150 minutes. The mixture was then poured into a simple mold and hardened at 130℃ for 12 hours, then cooled at room temperature for 1 hour to produce a plastic specimen with a thickness of approximately 1mm.
[0081] Comparative Examples 2 to 4 Curable compositions and optical components made of the cured compositions were prepared in the same manner as in Example 1, except that the episulfide compound, selenium sulfide particles, sulfur particles, and catalyst were used in the amounts of compounds shown in Table 1 below. Meanwhile, 70B used in Comparative Examples 2 to 4 is as follows. [ka]
[0082] [Table 1]
[0083] Physical property evaluation 1.Transmittance, haze and yellowness evaluation For the optical components of the Examples and Comparative Examples, the transmittance (JIS K 7361) and haze (JIS K 7136) were measured in the thickness direction of the cured products cured to a reference thickness of 1 mm using an NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd., and the results are shown in Table 2 below.
[0084] In addition, the yellow index of the test specimens was measured using a colorimeter, and the results are shown in Table 2 below.
[0085] 2. Glass transition temperature (Tg) measurement The glass transition temperatures of the optical members of the Examples and Comparative Examples were measured using a differential scanning calorimeter (DSC) manufactured by TA Instruments, and the results are shown in Table 2 below.
[0086] 3. Refractive Index Measurement The refractive index values of the optical members of the examples and comparative examples were measured at a wavelength of 632.8 nm using a SPA-4000 prism coupler manufactured by Sairon Technology Co., Ltd., and the results are shown in Table 2 below.
[0087] [Table 2]
[0088] Referring to Table 2, it was confirmed that the specimens including the compositions according to the embodiments of the present invention have high characteristics such as a high glass transition temperature (Tg) and a refractive index of 1.7261 or more, a high transmittance of 79.2% or more, a low haze of 30.7% or less, and a low yellow index of 14.5 or less.
[0089] On the other hand, it was confirmed that Comparative Example 1, which does not use the sulfur-containing polymer compound of the present invention, has a significantly lower transmittance and a significantly higher yellow index and haze than the Examples, and thus has inferior optical properties.
[0090] In addition, it was confirmed that Comparative Examples 2 to 4, which use a compound (70B) containing a thiol group instead of the sulfur-containing polymer compound of the present invention, have a lower refractive index and a significantly lower glass transition temperature than the Examples.
[0091] 4. Evaluation of refractive index change The precise refractive index of the optical members of Examples 4 and 8 and Comparative Example 1 was measured using a prism coupler.
[0092] Specifically, the refractive index of the optical member was measured over time under room temperature conditions, and the results are shown in Table 3 below. The difference between the maximum and minimum refractive indexes is indicated as ΔRI, and the average refractive index is indicated as RI ave As shown in.
[0093] [Table 3]
[0094] According to Table 3, it was confirmed that the average refractive index was high, 1.7309 or more, and the refractive index hardly changed with time in Examples 4 and 8. In contrast, it was confirmed that the refractive index of Comparative Example 1 changed significantly with time.
Claims
1. Contains episulfide compounds and sulfur-containing polymer compounds, The sulfur-containing polymer compound is S n+1 (n is an integer of 1 to 20), and one or more repeating units selected from the group consisting of repeating units containing selenium and sulfur, The curable composition for forming a high refractive index optical member further comprises sulfur (S 8 ) particles, selenium disulfide (SeS 2 ) particles, or a mixture thereof.
2. The curable composition for forming a high refractive index optical member according to claim 1, wherein the sulfur-containing polymer compound comprises a repeating unit represented by the following chemical formula 1 or 2: 【Chemistry 1】 In the above Chemical Formula 1, R 1 is a substituted or unsubstituted alkylene having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms; a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a substituted or unsubstituted heteroarylene having 2 to 30 carbon atoms containing one or more of oxygen (O), nitrogen (N) and sulfur (S) atoms; a OR b -;-R c COOR d -;-R e SO 2 R f -or-R g SOR h - and R a Or R h each independently represents a single bond, a substituted or unsubstituted alkylene having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms, or a substituted or unsubstituted arylene having 5 to 30 carbon atoms; n is an integer from 1 to 20, 【Chemistry 2】 In the above Chemical Formula 2, R 2 is a substituted or unsubstituted alkylene having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms; a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a substituted or unsubstituted heteroarylene having 2 to 30 carbon atoms containing one or more of oxygen (O), nitrogen (N) and sulfur (S) atoms; a OR b -;-R c COOR d -;-R e SO 2 R f -or-R g SOR h - and R a Or R h each independently represents a single bond, a substituted or unsubstituted alkylene having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene having 3 to 40 carbon atoms, or a substituted or unsubstituted arylene having 5 to 30 carbon atoms; a and b are each independently an integer of 0 to 10, a+b is an integer between 1 and 20.
3. R 1 and R 2 The curable composition for forming a high refractive index optical member according to claim 2, wherein each of the radicals independently represents methylene, ethylene, propylene, isopropylene, cyclohexylene, cycloheptylene, phenylene, methylphenylene, ethylphenylene, methoxyphenylene, or ethoxyphenylene.
4. The curable composition for forming a high refractive index optical member according to any one of claims 1 to 3, wherein the sulfur-containing polymer compound includes any one selected from the group consisting of the following repeating units: 【Chemistry 3】 。
5. The curable composition for forming a high refractive index optical member according to claim 1 , wherein the sulfur-containing polymer compound and the episulfide compound have a weight ratio of 1:2 to 1:
30.
6. The sulfur (S 8 ) the particles have a particle size of 1 to 200 μm; The selenium disulfide (SeS 2 2. The curable composition for forming a high refractive index optical member according to claim 1, wherein the particles have a particle size of 1 to 200 μm.
7. The episulfide compound is represented by the following chemical formula 3: 【Chemistry 4】 In the above Chemical Formula 3, R 3 and R 4 are each independently hydrogen or alkyl having 1 to 10 carbon atoms; R 5 and R 6 each independently represents a single bond or an alkylene having 1 to 10 carbon atoms; a is an integer from 0 to 4; b is an integer from 0 to 6.
8. The curable composition for forming a high refractive index optical member according to claim 7, wherein the episulfide compound includes at least one selected from the group consisting of bis(β-epithiopropyl)sulfide, bis(β-epithiopropyl)disulfide, bis(β-epithiopropylthio)methane, 1,2-bis(β-epithiopropylthio)ethane, 1,3-bis(β-epithiopropylthio)propane, and 1,4-bis(β-epithiopropylthio)butane.
9. Contains episulfide compounds and sulfur-containing polymer compounds, The sulfur-containing polymer compound is S n+1 (n is an integer from 1 to 20) and one or more repeating units selected from the group consisting of repeating units containing selenium and sulfur, The optical member further comprises sulfur (S 8 ) particles, selenium disulfide (SeS 2 ) particles, or a mixture thereof.
10. The optical member according to claim 9, which has a glass transition temperature of 65° C. or higher.
11. 11. The optical member according to claim 9, having a refractive index of 1.710 or more measured at a wavelength of 500 nm or more and 750 nm or less.
12. 12. The optical member according to claim 9, having a yellow index (YI) of 0.1 to 50.
Citation Information
Patent Citations
Method for producing optical material
JP2004339329A
Composition for optical material
JP2005182084A
High impact poly(urethane urea) polysulfide
JP2008540817A
Method of preparing a polymerizate
US20010047043A1
Curable composition, and optical member including cured product thereof
WO2020235913A1