Non-destructive detection method for cell failure
The XRD scanning method allows for rapid identification of defects in lithium secondary batteries by analyzing LiC6 peak intensity in graphite-based negative electrodes, addressing inefficiencies in existing disassembly-based detection methods.
Patent Information
- Application Number
- JP2023552241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-02
- Filing Date
- 2022-11-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-18
AI Technical Summary
Existing methods for detecting defects in lithium secondary batteries, such as overhang and sliding, require disassembly, which is inefficient in terms of process and cost.
A non-destructive method using XRD scanning to detect cell defects by analyzing the LiC6 peak intensity in carbon-based negative electrodes, particularly graphite, during charging, without disassembling the cell.
Enables quick detection of overhang and sliding defects within 3 to 5 minutes, improving process efficiency and reducing costs by avoiding disassembly.
Smart Images

Figure 0007570767000001 
Figure 0007570767000002 
Figure 0007570767000003
Abstract
Description
[Technical field]
[0001] Cross-references to related applications (etc.) This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0171212 filed on December 2, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a non-destructive method for detecting cell failures. [Background technology]
[0003] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which exhibit high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Recently, the design of electronic devices itself has become a very important factor in consumers' product selection, and electronic devices are becoming smaller and thinner according to consumer preferences. Therefore, in order to minimize unnecessary waste of the internal space of electronic devices, lithium secondary batteries are also required to be smaller and thinner, and the shape of lithium secondary batteries needs to be diversified according to the shape of electronic devices. Recently, there has been an increasing demand for curved batteries, including flexible batteries.
[0005] Such a lithium secondary battery is manufactured by preparing a positive electrode and a negative electrode, laminating them with a separator to form an electrode assembly, and incorporating the electrode assembly together with an electrolyte into a secondary battery case.
[0006] In the secondary battery electrodes, a sliding phenomenon occurs due to the coating of electrode active material slurry during the manufacturing process, and due to different loading at different positions, a sliding failure may occur in which the ratio of the positive electrode to the negative electrode is reversed at the sliding occurrence site.
[0007] In addition, when the positive and negative electrodes are assembled, the positive electrode has a larger area than the negative electrode, which causes a reversal of the ratio between the positive and negative electrodes, resulting in overhang defects.
[0008] In the case of such defective cells, lithium deposition in the corresponding area accelerates as cycles proceed, and if the lithium deposition is severe, it may even lead to fire. Therefore, in order to improve safety, a process is required to select and remove cells that have problems with overhang or sliding defects before being sent to the field.
[0009] However, in the past, it was necessary to disassemble the cell to make such a judgment, which was extremely inefficient in terms of process and cost.
[0010] Therefore, there is a pressing need for development of a technique for detecting defective cells that can solve these problems. Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a non-destructive method for detecting cell defects, which can quickly detect overhang and sliding defects without disassembling the cell. [Means for solving the problem]
[0012] A method for non-destructively detecting a cell defect according to an embodiment of the present invention includes: (a) providing a cell including a carbon-based material as a negative electrode active material; (b) charging the cell; (c) XRD scanning the cell from the negative end inwards; The negative electrode LiC in the area after the negative electrode current collector signal in the XRD scan 6 The method is characterized in that it is confirmed whether a peak is observed or not.
[0013] Here, the cell may be charged to 4V or higher in step (b).
[0014] Moreover, the step (c) may be performed once from one end of the negative electrode toward the inside, or twice from one end toward the inside and from the other end toward the inside.
[0015] Said LiC 6 The peak observation was performed using LiC 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) may be measured.
[0016] At this time, the LiC of the negative electrode in the region after the signal of the negative electrode current collector appears in the XRD scan 6 If the peak intensity decreases from the end of the negative electrode toward the inside, it may be judged as defective.
[0017] Or, immediately after the signal of the negative electrode current collector appears in the XRD scan, LiC 6 Specifically, immediately after the signal of the negative electrode current collector is obtained in the XRD scan, the LiC 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) is 0.3 or more.
[0018] Alternatively, the charging of the cell in step (b) is performed at SOC 80% or more, and the LiC in the area after the signal of the negative electrode current collector is issued 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) is 0.8 or more.
[0019] The cell defect refers to an overhanging cell or a sliding cell. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a perspective view that illustrates a schematic diagram of an overhanging cell according to Comparative Example 1. As shown in FIG. [Diagram 2] FIG. 2 is a perspective view showing a schematic diagram of a sliding cell. [Diagram 3] FIG. 3 is a perspective view that illustrates a normal cell according to the first embodiment. [Figure 4] FIG. 4 is a graph showing the LiC6 peak intensity according to the charging SOC in the experimental example 1. [Diagram 5] FIG. 5 is a graph showing the LiC6 peak intensity and graphite d-spacing according to the charging SOC in Experimental Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The terms and words used in the present specification and claims should not be interpreted in their ordinary and dictionary sense, but should be interpreted in the sense and concept consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concept of terms to best describe their own invention. Therefore, the embodiments described in the present specification and the configurations shown in the drawings are merely preferred embodiments of the present invention, and do not fully represent the technical idea of the present invention, so there may be various equivalents and modifications that can replace them at the time of filing this application, and the scope of the present invention is not limited to the embodiments described below.
[0022] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his or her invention.
[0023] In addition, it should be understood that the embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention, and therefore there may be various equivalents and modifications that can replace them at the time of this application.
[0024] According to one embodiment, the present invention provides a method for non-destructive detection of cell failure, comprising the steps of: (a) providing a cell including a carbon-based material as a negative electrode active material; (b) charging the cell; (c) XRD scanning the cell from the negative end inwards; The negative electrode LiC in the area after the negative electrode current collector signal in the XRD scan 6 A non-destructive method for detecting cell failure is provided, which is to check whether a peak is observed.
[0025] Here, the cell defect refers to an overhanging cell or a sliding cell.
[0026] As described above, in the past, in order to determine cell defects such as an overhang cell 100 in which the positive electrode 102 facing the negative electrode 101 across the separator 103 at an end is formed to have a larger area than the negative electrode 101, resulting in a reversal of the ratio between the positive electrode and the negative electrode, as shown in FIG. 1, or a sliding cell 200 in which the end of the negative electrode 202 slides due to the characteristics of the electrodes formed by slurry coating, resulting in a lower loading of the negative electrode 202 relative to the positive electrode 201 facing the negative electrode 201 across the separator 203 in that region, it was necessary to disassemble the cell and identify the assembly defect.
[0027] However, this method of determination is inefficient in terms of process and cost because it requires a process of disassembling the cell.
[0028] Therefore, the inventors of the present application have studied a method for detecting such cell defects without disassembling the cells, and have confirmed that cell assembly defects such as overhang and sliding can be detected without disassembling the cells by using in situ XRD analysis while charging the cells at a predetermined charging temperature, thereby completing the present invention.
[0029] Specifically, when a negative electrode containing a carbon-based material, particularly graphite, is used, LiC 6 By observing the peak, defective cells can be detected.
[0030] In the case of graphite, as lithium is inserted, the crystal structure changes from stage IV, where no lithium is inserted in the graphite layers, to stage III, where lithium is inserted in every third graphite layer, to stage II, where lithium is inserted in every other graphite layer, and then, upon further charging, to stage I, where lithium is inserted in all of the graphite layers.
[0031] In the case of stage II, where lithium is inserted into every other graphite layer, XRD shows that LiC 12 In stage I, where lithium is inserted into all graphite layers, the LiC peak is observed by XRD. 6A peak is observed.
[0032] Generally, as shown in FIG. 3, in the case of a well-assembled normal cell 300 in which the area of the negative electrode 301 sandwiching the separator 303 is larger than the area of the positive electrode 302, the end of the negative electrode is hardly charged during charging. Therefore, when the end of the negative electrode is measured by XRD, the LiC observed in the middle during charging is 6 No peak is observed.
[0033] However, in the overhang cell or sliding cell shown in Fig. 1 and Fig. 2, the ratio of the negative electrode to the positive electrode is inverted in the negative electrode end region, and the loading of the negative electrode is lower than that of the positive electrode, resulting in a state of extreme overcharging at the negative electrode end during charging. As a result, when the negative electrode end is measured by XRD, it is found that LiC 6 The peak is very clearly observed.
[0034] More specifically, in overhanging cells and sliding cells, LiC is the behavior in which lithium is charged to the negative electrode at the edge of the negative electrode. 6 The peak intensity is the LiC as the behavior of lithium being charged to the negative electrode at the middle of the negative electrode. 6 It is observed to increase more rapidly than the peak intensity.
[0035] Therefore, based on such differences, the present invention can detect cell defects non-destructively and within the in situ XRD measurement time of 3 to 5 minutes, which is very efficient in terms of process and cost.
[0036] However, for this observation, the negative electrode must contain a carbon-based material, particularly graphite, as a negative electrode active material.
[0037] It can also be determined based on the cells being in a state where they have been charged to a certain extent.
[0038] Therefore, the charging of the cell in step (b) may be performed at 4V or more, and may be performed at SOC50 or more based on the SOC standard.
[0039] When charging as described above, the LiC 6 Enough lithium is intercalated at the negative electrode that a peak is observable, which is sufficient to determine cell failure.
[0040] The cell thus charged is subjected to in situ XRD measurement without a separate decomposition process.
[0041] The XRD scan was performed at room temperature of 25° C., the X-ray output conditions were 60 kv, 35 mA, and the measurement method was static mode (2 Theta: 7-14 degrees). The scan time was fixed at 4 minute intervals during the charging process.
[0042] Such XRD scanning is performed from the end of the negative electrode toward the inside, because defects such as overhanging and sliding occur at the end of the negative electrode. More specifically, the step (c) may be performed once from one end of the negative electrode toward the inside, or twice from one end toward the inside and from the other end toward the inside.
[0043] Since sliding and overhanging do not occur only at one end, accuracy can be further improved by judging both ends.
[0044] To this end, an XRD scan was performed from the edge of the negative electrode to the inside to identify the LiC 6 This is done by checking whether a peak is observed.
[0045] In this case, the signal from the negative electrode current collector can be easily identified because the peak of the metal used in the negative electrode current collector is observed by XRD.
[0046] Said LiC 6 Specifically, the observation of the peak was performed using LiC 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (ILiC6 +I LiC12 )) may be measured.
[0047] Based on this, a method for detecting defects is, for example, to detect LiC of the negative electrode in the region after the signal of the negative electrode current collector is generated in the XRD scan. 6 If the peak intensity decreases from the end of the negative electrode toward the inside, it may be judged as defective.
[0048] In other words, in the case of overhanging or sliding cells, the LiC at the negative electrode end is destroyed by overcharging. 6 In contrast, in a normal cell, no lithium is absorbed or released at the end of the negative electrode, so the LiC 6 No peak appears, and lithium insertion occurs frequently toward the inside, LiC 6 The peak intensity increases. Based on this, it is possible to detect whether or not the product is defective.
[0049] Or, immediately after the signal of the negative electrode current collector appears in the XRD scan, LiC 6 If a peak is observed, it may be judged as defective. More specifically, immediately after the signal of the negative electrode current collector appears in the XRD scan, the LiC 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 ) is 0.3 or more, more specifically, exceeds 0.3, and more specifically, is in the range of 0.3 to 0.9, the cell may be determined to be defective. On the other hand, if the value is close to 0, for example, less than 0.3, the cell is determined to be normal.
[0050] To explain again, in the case of overhanging or sliding cells, the LiC 6 In contrast, in a normal cell, no lithium absorption or desorption occurs at the negative electrode end, so there is no LiC6 Since no peak appears, the LiC at the edge 6 Simply observing the peak is sufficient to detect defective cells.
[0051] For the most accurate detection, the charging of the cell in step (b) is performed at SOC 80% or more, and the LiC in the area after the signal of the negative electrode current collector is generated is 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) is 0.8 or more.
[0052] In the case of overhanging or sliding cells, overcharging occurs at the edge of the negative electrode rather than in the normal area, i.e., the middle part of the inside of the negative electrode, and lithium accumulates to the extent that lithium is precipitated. Therefore, LiC at the edge 6 The peak intensity is very large.
[0053] In contrast, in a normal cell, lithium insertion occurs uniformly throughout the cell, so LiC 6 There is no specific region where the peak intensity is large. Therefore, the XRD scan shows that LiC 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 If an area where the difference between the ΔV and ΔV is 0.8 or more is observed, this can be determined as a defective cell.
[0054] In this manner, according to the present invention, a cell defect can be determined in a very simple manner without disassembling the cell.
[0055] The present invention will now be described in more detail with reference to the following examples.
[0056] <Comparative Example 1> A slurry for the active material layer was prepared by mixing artificial graphite as the negative electrode active material, a binder (a mixture of SBR and CMC in a weight ratio of 2:1), and carbon black as the conductive material in a weight ratio of 95:3.5:1.5, and using water as the dispersion medium, the weight ratio of the mixture to the dispersion medium was 1:2.
[0057] The active material layer slurry was coated on one side of a copper (Cu) thin film of a negative electrode current collector having a thickness of 10 μm using a slot die, and dried for 1 hour under vacuum at 130° C. The active material layer thus formed was rolled using a roll pressing method to manufacture a negative electrode having an active material layer having a thickness of 80 μm.
[0058] LiNi as the positive electrode active material 0.4 Mn 0.3 Co 0.3 O 2 Carbon black as a conductive material and PVDF as a binder were mixed in a weight ratio of 92.5:3.5:4 in N-methylpyrrolidone solvent to prepare a slurry for a positive electrode active material layer, and the slurry for the positive electrode active material layer was coated on one side of an aluminum (Al) thin film of a positive electrode current collector having a thickness of 10 μm using a slot die, and dried for 1 hour under vacuum at 130° C. to form an active material layer. The active material layer thus formed was rolled using a roll pressing method to prepare a positive electrode having an active material layer having a thickness of 80 μm.
[0059] A porous polyethylene separator was interposed between the positive electrode and the negative electrode to prepare an electrode assembly. The electrode assembly was placed inside a case, and an electrolyte was injected into the case to prepare a lithium secondary battery.
[0060] At this time, the positive electrodes were laminated such that both ends of the positive electrodes were offset from the ends of the negative electrodes, so that an overhang cell was manufactured in which the area of the positive electrode at one end was larger than the area of the negative electrode, as shown in FIG.
[0061] The electrolyte solution was prepared by dissolving 1.15M lithium hexafluorophosphate (LiPF 6 ) was dissolved to prepare the product.
[0062] <Example 1> When the lithium secondary battery was manufactured, both ends of the positive electrode were stacked inside both ends of the negative electrode to form a normal cell as shown in FIG.
[0063] <Experimental Example 1> The lithium secondary battery produced in Comparative Example 1 was subjected to XRD scanning while being charged at 25° C., constant current / constant voltage (CC / CV) conditions, and at 1C up to 4.35 V / 38 mA.
[0064] The XRD scan was performed at room temperature of 25° C., the X-ray output conditions were 60 kv, 35 mA, and the measurement method was static mode (2 Theta: 7-14 degrees). The scan time was fixed at 4 minute intervals during the charging process.
[0065] Depending on the state of charge, LiC in regions (1), (2), and (3) in Figure 1 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 ) was calculated and is shown in Figure 4.
[0066] Said LiC 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) is LiC 6 The area of the peak defined as 12The area of the peak defined as
[0067] In Fig. 4, LiC in Fig. 1(1) 6 The peak intensity is shown in red (●), and (2) LiC 6 Peak intensity is indicated in yellow (◆), (3) LiC 6 The peak intensity is indicated in blue (▲).
[0068] <Experimental Example 2> The lithium secondary battery prepared in Example 1 was subjected to XRD scanning while being charged at 25° C., constant current / constant voltage (CC / CV) conditions, and 1C up to 4.35 V / 38 mA.
[0069] The XRD scan was performed at room temperature of 25° C., the X-ray output conditions were 60 kv, 35 mA, and the measurement method was static mode (2 Theta: 7-14 degrees). The scan time was fixed at 4 minute intervals during the charging process.
[0070] At this time, depending on the state of charge, the LiC in the (4) region of Figure 3 6 Peak intensity and LiC 12 LiC for the sum of peak intensity and 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 )) and the interlayer spacing of graphite (001), i.e., the crystal lattice values, were calculated and are shown in Figure 5.
[0071] Considering Experimental Examples 1 and 2, in the case of the overhang cell, LiC increases as charging progresses in the (1) region of FIG. 1, that is, at the end of the negative electrode. 6 It can be seen that the peak intensity increases rapidly and reaches a value of 0.8 or more at SOC 80% or more. In contrast, in the case of a normal cell, even as charging progresses, the LiC 6 It can be confirmed that no peak is observed.
[0072] Therefore, through such an experiment, normal and defective cells can be detected without disassembling the cells.
[0073] Those skilled in the art will appreciate that the present invention can be applied in a variety of ways and modified within the scope of the present invention based on the above content. [Industrial Applicability]
[0074] The non-destructive detection method of cell failure according to the present invention measures a cell that has been charged to a predetermined extent by XRD and detects LiC at the end of the negative electrode where overhang or sliding may occur. 6 This is a very simple method for observing the peak, and it can rapidly detect cell defects such as overhang and sliding without disassembling the cell, making it efficient in terms of processability and cost. [Explanation of symbols]
[0075] 100 Overhanging Cell 101 Negative electrode 102 Positive electrode 103 Separation membrane 200 Sliding Cell 201 Positive electrode 202 Negative electrode 203 Separation membrane 300 normal cells 301 negative electrode 302 Positive electrode 303 Separation membrane
Claims
1. 1. A non-destructive method for detecting cell failure, comprising: (a) providing a cell including a carbon-based material as a negative electrode active material; (b) charging the cell; (c) XRD scanning the charged cell from the negative end inward; The XRD scan shows the LiC of the negative electrode in the area after the signal of the negative electrode current collector. 6 This is a non-destructive method for detecting cell failure by checking whether a peak is observed.
2. 2. The non-destructive method for detecting cell failure as claimed in claim 1, wherein the charging of the cell in step (b) is performed to 4 V or more.
3. 2. The non-destructive method for detecting cell failure according to claim 1, wherein step (c) is performed once from one end of the negative electrode toward the inside, or twice from one end to the inside and from the other end to the inside.
4. The LiC 6 The observation of the peak is 6 Peak intensity and LiC 12 LiC for the sum of the peak intensity 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 4. The non-destructive cell failure detection method according to claim 1 , wherein the cell failure is measured by the following method:
5. The XRD scan shows the LiC of the negative electrode in the area after the signal of the negative electrode current collector. 6 The non-destructive cell failure detection method according to claim 4 , wherein a cell is judged to be defective when the peak intensity decreases from the end of the negative electrode toward the inside.
6. Immediately after the signal of the negative electrode current collector appears in the XRD scan, LiC 6 The non-destructive method for detecting a cell failure according to claim 1 , wherein a peak is observed, and the cell is judged to be defective.
7. Immediately after the signal of the negative electrode current collector appears in the XRD scan, 6 Peak intensity and LiC 12 LiC for the sum of the peak intensity 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 7. The non-destructive cell detection method according to claim 6, wherein a region in which the difference between the cell density and the cell density is 0.3 or more is observed, the cell is judged to be defective.
8. The charging of the cell in step (b) is performed at an SOC of 80% or more, and the LiC in the region after the signal of the negative electrode current collector is generated 6 Peak intensity and LiC 12 LiC for the sum of the peak intensity 6 peak intensity (I LiC6 / (I LiC6 +I LiC12 2. The non-destructive cell detection method according to claim 1, wherein a region in which a difference between the cell density and the cell density is 0.8 or more is observed, the cell is judged to be defective.
9. The method for non-destructively detecting a cell failure according to claim 1 , wherein the cell failure refers to an overhanging cell or a sliding cell.
Citation Information
Patent Citations
Method and device for checking secondary battery
JP2014143164A
Battery inspection device
JP2016109654A
Inspection device for laminated type battery
JP2020085690A
Secondary battery inspection apparatus and method
US20200350637A1