Composite electrolyte, electrolyte membrane, catalyst layer, and solid polymer fuel cell

A composite electrolyte with tungsten oxide hydrate and optional second metal elements addresses radical-induced deterioration in solid polymer electrolytes, enhancing durability and performance.

JP7570784B2Active Publication Date: 2024-10-22KK TOYOTA CHUO KENKYUSHO +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021073104
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-23
Publication Date
2024-10-22
Estimated Expiration
2041-04-23

AI Technical Summary

Technical Problem

Existing electrochemical devices using solid polymer electrolytes face deterioration due to radical attack, leading to increased resistance, cross leakage, and reduced lifespan, with existing solutions like tungsten oxide addition providing limited improvement.

Method used

A composite electrolyte containing fine particles of tungsten oxide hydrate (WO3·nH2O, where n=1/3 or 2) and optionally second metal elements or compounds is used to scavenge radicals, enhancing hydrogen peroxide decomposition and radical elimination.

Benefits of technology

The composite electrolyte effectively suppresses solid polymer electrolyte deterioration by significantly improving hydrogen peroxide decomposition and radical scavenging, maintaining durability and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570784000003
    Figure 0007570784000003
  • Figure 0007570784000004
    Figure 0007570784000004
  • Figure 0007570784000001
    Figure 0007570784000001
Patent Text Reader

Abstract

To provide a composite electrolyte capable of suppressing the deterioration of a solid polymer electrolyte due to radicals, and an electrolyte membrane, a catalyst layer and a polymer electrolyte fuel cell in which the composite electrolyte is included.SOLUTION: A composite electrolyte includes a solid polymer electrolyte and a first fine particle comprising a hydrate of a tungsten oxide dispersed in the solid polymer electrolyte. The hydrate of a tungsten oxide comprises WO3 nH2O (where, n=1 / 3 and / or 2). An electrolyte membrane comprises such a composite electrolyte. A catalyst layer contains such a composite electrolyte. Further, a polymer electrolyte fuel cell includes such an electrolyte membrane and / or such a catalyst layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite electrolyte, an electrolyte membrane, a catalyst layer, and a solid polymer fuel cell, and more particularly to a composite electrolyte containing fine particles of a tungsten oxide hydrate, and an electrolyte membrane, a catalyst layer, and a solid polymer fuel cell including such a composite electrolyte. [Background technology]

[0002] In various electrochemical devices using solid polymer electrolytes, such as soda electrolysis devices, water electrolysis devices, and fuel cells, membrane electrode assemblies (MEAs) are used in the area where electrochemical reactions occur. It is said that MEAs are deteriorated by radicals generated directly by the direct reaction of oxygen and hydrogen, or by radicals generated via electrochemical reactions, or by radicals generated via hydrogen peroxide, due to the attack of the electrolyte. For example, in fuel cells, radical attack is known to increase the resistance of the electrolyte membrane, increase cross leakage, and shorten the lifespan due to thinning. Furthermore, degradation products generated by radical attack may cause catalyst poisoning, which may result in a decrease in electrolytic performance and cell performance.

[0003] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 states: (a) adding 0.25 times the molar amount of H2WO4 and 0.05 times the molar amount of Ru ions to a catalyst ink containing platinum-supported carbon and Nafion (registered trademark) relative to the molar amount of sulfonic acid groups in Nafion (registered trademark); (b) This catalyst ink is applied onto a polytetrafluoroethylene sheet and dried to produce a catalyst sheet. (c) Thermally transfer the catalyst sheet onto the sulfonated polyetherethersulfone membrane. The resulting MEA is disclosed.

[0004] The document describes that adding H2WO4 and Ru ions simultaneously to the catalyst layer improves the molecular weight retention rate of the electrolyte membrane after durability testing compared to MEAs using catalyst layers that do not contain these.

[0005] In addition, Patent Document 2 states: (a) A Nafion® 112 membrane was immersed in a 0.1 M aqueous solution of sodium tungstate (Na2WO4) at 90°C for 30 minutes; (b) The Nafion® 112 membrane is removed from the sodium tungstate aqueous solution, washed with water, and then further immersed in 0.5 M sulfuric acid. The electrolyte membrane obtained by the above process is disclosed.

[0006] The same document states: (a) When a membrane containing sodium tungstate is immersed in sulfuric acid, the sodium tungstate is hydrolyzed and a tungsten oxide hydrate is precipitated in the membrane; and (b) By using the hydrolysis method, transition metal oxides on the order of nanometers can be dispersed almost uniformly throughout the solid polymer electrolyte. is stated.

[0007] Furthermore, Non-Patent Document 1 describes that when sodium tungstate (Na2WO4) is treated under acidic conditions, tungsten oxide monohydrate (WO3·H2O or H2WO4) is obtained.

[0008] Patent Documents 1 and 2 describe that the addition of tungsten oxide alone or the addition of tungsten oxide and a certain metal ion simultaneously to a solid polymer electrolyte suppresses the deterioration of the solid polymer electrolyte. However, in order to further improve the durability of various electrochemical devices using the solid polymer electrolyte, it is desirable to further suppress the deterioration of the solid polymer electrolyte caused by radicals. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5194448 [Patent Document 2] JP 2005-019232 A [Non-patent literature]

[0010] [Non-Patent Document 1] Acta Materialia 69(2014)203-209 Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present invention is to provide a composite electrolyte capable of suppressing degradation of a solid polymer electrolyte caused by radicals. Another object of the present invention is to provide an electrolyte membrane, a catalyst layer, and a solid polymer fuel cell each including such a composite electrolyte. [Means for solving the problem]

[0012] In order to solve the above problems, the composite electrolyte according to the present invention comprises: A solid polymer electrolyte; a first microparticle made of a tungsten oxide hydrate dispersed in the solid polymer electrolyte; Equipped with The tungsten oxide hydrate is preferably WO3·nH2O (wherein n=1 / 3 and / or 2).

[0013] The electrolyte membrane according to the present invention comprises the composite electrolyte according to the present invention. The catalyst layer according to the present invention comprises the composite electrolyte according to the present invention. Furthermore, the polymer electrolyte fuel cell according to the present invention comprises the electrolyte membrane according to the present invention and / or the catalyst layer according to the present invention. Effect of the Invention

[0014] Among tungsten oxide hydrates, the 1 / 3 hydrate (WO3·(1 / 3)H2O) and dihydrate (WO3·2H2O) have a much higher hydrogen peroxide decomposition ability than the anhydrous (WO3) or monohydrate (WO3·H2O). Therefore, adding these to a solid polymer electrolyte can suppress the degradation of the solid polymer electrolyte caused by radicals. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a graph showing hydrogen peroxide decomposition rates of various additives. [Diagram 2] FIG. 1 is a graph showing the cumulative amount of fluorine discharged after 90 hours when an open circuit voltage test was performed on the electrolyte membranes obtained in Example 3 and Comparative Examples 5 and 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of the present invention will be described in detail below. [1. Composite electrolytes] The composite electrolyte according to the present invention comprises: A solid polymer electrolyte; a first microparticle made of a tungsten oxide hydrate dispersed in the solid polymer electrolyte; It is equipped with:

[0017] The composite electrolyte is (a) ions of a second metal element having a radical scavenging function, which are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte, and / or (b) second fine particles made of a second compound containing the second metal element, the second fine particles being dispersed in the solid polymer electrolyte; It may further include.

[0018] [1.1. Solid polymer electrolyte] In the present invention, the material of the solid polymer electrolyte is not particularly limited. The solid polymer electrolyte may be either a fluorine-based electrolyte or a hydrocarbon-based electrolyte. The composite electrolyte may contain one of these solid polymer electrolytes, or may contain two or more of them. The type of acid group in the solid polymer electrolyte is not particularly limited. Examples of the acid group include a sulfonic acid group, a carboxylic acid group, a phosphonic acid group, and a sulfonimide group. The solid polymer electrolyte may contain only one of these acid groups, or may contain two or more of them.

[0019] Examples of fluorine-based electrolytes include Nafion (registered trademark), Flemion (registered trademark), Aquivion (registered trademark), and Aciplex (registered trademark). The fluorine-based electrolyte may be a fully fluorine-based electrolyte that does not contain a C—H bond in the polymer structure, or may be a partially fluorine-based electrolyte that contains a C—H bond and a C—F bond in the polymer structure.

[0020] Examples of the hydrocarbon electrolyte include: (a) A wholly aromatic hydrocarbon-based electrolyte comprising polyether ether ketone, polysulfone, polyether sulfone, polyimide, polyphenylene, polyamide, polyamide imide, or a derivative thereof, into which an acid group such as a sulfonic acid group has been introduced; (b) partially aromatic hydrocarbon electrolytes having an aromatic ring in a part of the polymer chain of an aliphatic hydrocarbon electrolyte; etc.

[0021] [1.2. First fine particle] [1.2.1. Composition] The "first fine particles" refer to fine particles made of a tungsten oxide hydrate. In the present invention, first fine particles are dispersed within the solid polymer electrolyte. Here, "dispersion" means (a) A state in which first fine particles (primary particles) made of a tungsten oxide hydrate or higher-order particles such as secondary particles are surrounded by a solid polymer electrolyte, or (b) A state in which a solid polymer electrolyte is present in a portion surrounding a primary particle or a higher-order particle. This refers to. Tungsten oxide hydrate mainly acts to decompose hydrogen peroxide to render it harmless, and therefore, by adding an appropriate amount of first fine particles made of tungsten oxide hydrate to a solid polymer electrolyte, deterioration of the solid polymer electrolyte can be suppressed.

[0022] In the present invention, the tungsten oxide hydrate is composed of WO3·nH2O (where n=1 / 3 and / or 2). This is different from the conventional method. The 1 / 3 hydrate (WO3·(1 / 3)H2O) and dihydrate (WO3·2H2O) have a much higher hydrogen peroxide decomposition ability than the anhydrate (WO3) or monohydrate (WO3·H2O). Therefore, adding these to a solid polymer electrolyte can suppress the degradation of the solid polymer electrolyte caused by radicals.

[0023] [1.2.2. Content] The "content of the first fine particles" refers to the ratio of the mass of the first fine particles to the total mass of the composite electrolyte. In the present invention, the content of the first fine particles is not particularly limited, and an optimal content can be selected according to the purpose. In general, the more the content of the first fine particles, the more the degradation of the solid polymer electrolyte is suppressed. In order to obtain such an effect, the content of the first fine particles is preferably 0.5 mass% or more. The content is more preferably 1.0 mass% or more. On the other hand, if the content of the first fine particles is excessive, the conductivity of the solid polymer electrolyte may decrease. In addition, when the composite electrolyte is made into a membrane, the first fine particles may aggregate, which may reduce the degradation suppression effect due to a decrease in surface area, or may cause a decrease in the mechanical strength of the membrane. Therefore, the content of the first fine particles is preferably 10 mass% or less. The content is more preferably 3.0 mass% or less.

[0024] [1.2.3. Average particle size] The term "average particle size of the first fine particles" refers to the average value of the maximum dimension of any plurality of first fine particles, as determined by TEM observation. The average particle size of the first fine particles is not particularly limited, and an optimal average particle size can be selected depending on the purpose. In general, if the average particle size of the first fine particles is too small, the first fine particles tend to aggregate. Therefore, the average particle size of the first fine particles is preferably 8 nm or more. The average particle size is more preferably 10 nm or more. On the other hand, if the average particle size of the first fine particles is too large, the deterioration suppression effect may be reduced due to a decrease in surface area, or the mechanical strength of the film may be reduced. Therefore, the average particle size of the first fine particles is preferably 65 nm or less. The average particle size is more preferably 40 nm or less.

[0025] [1.3. Ions of second metal element or second particles] [1.3.1. Materials] The "second metal element" refers to a metal element having a function of scavenging radicals. The term "second compound" refers to a compound containing a second metallic element. The "second fine particles" refer to fine particles made of a second compound.

[0026] Compounds and ions containing certain metal elements mainly have the effect of scavenging radicals, and therefore, by adding an appropriate amount of such a compound and / or ion containing a metal element to the solid polymer electrolyte in addition to the tungsten oxide hydrate, the deterioration of the solid polymer electrolyte can be further suppressed.

[0027] Examples of the second metal element include Ce, Ag, Cs, Sn, Mn, Ti, Co, Ni, Zn, Zr, Ru, Rh, Pd, Pt, Pr, etc. The composite electrolyte may contain any one of these elements, or may contain two or more of them. Among these, the second metal element is preferably at least one element selected from the group consisting of Ce, Ag, Cs, Sn, and Mn. The second metal element is particularly preferably Ce, because these elements have a large effect of suppressing the generation of radicals or scavenging radicals.

[0028] The second compound may be a water-soluble compound or a poorly soluble compound. When a water-soluble second compound is used, the second compound dissociates in the composite electrolyte, and some of the protons of the acid groups of the solid polymer electrolyte are replaced with ions of the second metal element. On the other hand, when a poorly soluble second compound is used, the second compound is in a dispersed state in the solid polymer electrolyte. The second compound may be, for example, a nitrate, sulfate, carbonate, formate, acetate, citrate, perchlorate, phosphate, chloride, fluoride, hydroxide, or acetylacetonate compound.

[0029] [1.3.2. Content] When the composite electrolyte contains ions of a second metal element or second fine particles, the composite electrolyte preferably satisfies the following formula (1). 0.0005≦M / A≦0.15 …(1) however, M / A is the ratio of the number of moles (M) of the second metal element to the number of moles (A) of acid groups contained in the solid polymer electrolyte.

[0030] Even when only tungsten oxide hydrate is added to the solid polymer electrolyte, the deterioration of the solid polymer electrolyte can be effectively suppressed. However, when ions of a second metal element and / or second fine particles are further added in addition to the tungsten oxide hydrate, the deterioration of the solid polymer electrolyte is further suppressed due to the synergistic effect of these. In order to obtain such an effect, the M / A ratio is preferably 0.0005 or more. The M / A ratio is preferably 0.001 or more, more preferably 0.005 or more.

[0031] On the other hand, if the M / A ratio is too large, the conductivity of the solid polymer electrolyte may decrease. Therefore, the M / A ratio must be 0.15 or less. The M / A ratio is preferably 0.10 or less, more preferably 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less.

[0032] [1.3.2. Average particle size] When the second fine particles are added to the solid polymer electrolyte, the average particle size of the second fine particles is not particularly limited, and the most suitable average particle size can be selected according to the purpose. Other points regarding the average particle size of the second fine particles are the same as the average particle size of the first fine particles made of tungsten oxide hydrate, so the explanation is omitted.

[0033] [2. Electrolyte membrane, catalyst layer, and polymer electrolyte fuel cell] The electrolyte membrane according to the present invention comprises the composite electrolyte according to the present invention. The catalyst layer according to the present invention comprises the composite electrolyte according to the present invention. Furthermore, the polymer electrolyte fuel cell according to the present invention comprises the electrolyte membrane according to the present invention and / or the catalyst layer according to the present invention.

[0034] Other points regarding the electrolyte membrane, catalyst layer, and polymer electrolyte fuel cell, such as: (a) Thickness of the electrolyte membrane, (b) the composition of the catalyst layer; (c) Structure of the MEA and the gas diffusion layers and separators arranged on both sides of the MEA There are no particular limitations, and the most suitable one can be selected depending on the purpose.

[0035] Furthermore, when an electrolyte membrane is produced using the composite electrolyte of the present invention, the electrolyte membrane may be composed of only the composite electrolyte of the present invention, or may be a composite of the composite electrolyte and a reinforcing material. In this case, the type of the reinforcing material is not particularly limited. Examples of reinforcing materials include: (a) Porous membranes and nonwoven fabrics of fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (FEP), and ethylenetetrafluoroethylene copolymer (ETFE); (b) Porous membranes and nonwoven fabrics of hydrocarbon resins such as polyethylene (PE) and polypropylene (PP), etc.

[0036] [3. Manufacturing method of composite electrolyte] The composite electrolyte according to the present invention comprises: (a) preparing a solution (A) in which a solid polymer electrolyte is dissolved or dispersed in a solvent; (b) dissolving or dispersing a tungsten oxide hydrate and, if necessary, a second compound in the solution (A) to obtain a solution (B); (c) Removing the solvent from solution (B) It can be produced by the above method.

[0037] In addition, various members containing the composite electrolyte according to the present invention can be produced by various methods. For example, an electrolyte membrane made of the composite electrolyte can be produced by casting the solution (B) on a suitable substrate surface and removing the solvent.

[0038] A catalyst layer containing a composite electrolyte can be produced by further dispersing an electrode catalyst in solution (B) to obtain solution (C), casting solution (C) on a suitable substrate surface, and removing the solvent. Alternatively, the catalyst layer may be formed by applying or spraying the solution (C) onto the surface of the electrolyte membrane and then removing the solvent.

[0039] [3. Effect] Tungsten oxide anhydride (WO3) and monohydrate (WO3·H2O) are known to have the ability to decompose hydrogen peroxide. However, no additives with hydrogen peroxide decomposition capabilities greater than those of the anhydride and monohydrate were previously known.

[0040] In contrast, among tungsten oxide hydrates, the 1 / 3 hydrate (WO3·(1 / 3)H2O) and dihydrate (WO3·2H2O) have a much higher hydrogen peroxide decomposition ability than the anhydrous (WO3) or monohydrate (WO3·H2O). Therefore, adding these to a solid polymer electrolyte can suppress the degradation of the solid polymer electrolyte caused by radicals.

[0041] Furthermore, when second fine particles and / or ions of a second metal element are further added to the solid polymer electrolyte in addition to the first fine particles, high durability can be obtained even if the amount of these added is relatively small. (a) The first fine particles have the effect of decomposing hydrogen peroxide to render it harmless, and even if the amount added is small, they exhibit a high hydrogen peroxide decomposition effect. (b) The second fine particles and the ions of the second metal element have the effect of scavenging radicals, (c) When the first fine particles are coexisted with the second fine particles and / or ions of the second metal element, the hydrogen peroxide decomposition effect of the first fine particles is improved, and / or (d) Even if radicals are generated from hydrogen peroxide that is not decomposed by the first fine particles, the second fine particles and / or ions of the second metal element effectively eliminate the radicals, It is thought that. EXAMPLES

[0042] (Examples 1 to 2, Comparative Examples 1 to 4) [1. Test method] 0.067 mmol of each additive was dispersed in 10 mL of water to prepare a dispersion, to which 4.41 mmol of hydrogen peroxide was added. (a) WO 2H O (Example 1); (b) WO (1 / 3)H2O (Example 2); (c) WO2 (comparative example 1), (d) WO3 (comparative example 2), (e) WO.H2O (Comparative Example 3), or (f)Na2WO4·2H2O (Comparative Example 4) was used.

[0043] The resulting dispersion was kept at 80° C. for 1 hour, and then the concentration of hydrogen peroxide remaining in the dispersion was measured. Furthermore, the hydrogen peroxide decomposition rate was calculated from the following formula (2). Hydrogen peroxide decomposition rate (%) = (C0-C) x 100 / C0…(2) however, C0 is the concentration of hydrogen peroxide in the original dispersion, C is the concentration of hydrogen peroxide in the dispersion after holding at 80°C for 1 hour.

[0044] [2. Results] Table 1 and Figure 1 show the hydrogen peroxide decomposition rates of various additives. Table 1 also shows the compositions of various additives. Table 1 and Figure 1 also show the hydrogen peroxide decomposition rate of a blank. Table 1 and Figure 1 show that WO3·2H2O (Example 1) and WO3·(1 / 3)H2O have a significantly higher hydrogen peroxide decomposition rate than the other additives.

[0045] [Table 1]

[0046] (Example 3, Comparative Examples 5 to 6) [1. Preparation of electrolyte membrane] 1.1. Example 3 In Nafion® solution (D2020), (a) WO3·2H2O equivalent to 1 mass% of the electrolyte, (b) Ce with a sulfonic acid group substitution rate of 4.4% 3+ (added as Ce(NO3)3, equivalent to M / A = 0.015), and (c) Fe equivalent to a sulfonic acid group substitution rate of 1.0% as a radical generator 2+ (added as FeSO4) This dispersion was cast to obtain an electrolyte membrane.

[0047] [1.2. Comparative Example 5] An electrolyte membrane was prepared in the same manner as in Example 3, except that WO3·2H2O was not added. [1.3. Comparative Example 6] An electrolyte membrane was prepared in the same manner as in Example 3, except that WO3·2H2O and Ce were not added.

[0048] [2. Test Method and Results] The obtained electrolyte membrane was used to fabricate an MEA. Furthermore, an open circuit voltage test was performed on the MEA under conditions of 95°C and 30% RH. The amount of fluorine (F) contained in the generated water was measured, and the amount of fluorine eluted was totaled up to 90 hours after the start of the test.

[0049] The cumulative amount of F elution is shown in Table 2 and Figure 2. The types of additives are also shown in Table 2. Table 2 and Figure 2 show that the cumulative amount of F elution is significantly smaller in Example 3, in which WO3·2H2O and Ce were added simultaneously, than in Comparative Examples 5 and 6.

[0050] [Table 2]

[0051] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0052] The composite electrolyte according to the present invention can be used as an electrolyte membrane for a polymer electrolyte fuel cell or a polymer electrolyte water electrolysis device, a catalyst layer ionomer, or the like.

Claims

1. A composite electrolyte having the following configuration. (1) The composite electrolyte is A solid polymer electrolyte; First microparticles made of tungsten oxide hydrate dispersed in the solid polymer electrolyte; Equipped with The solid polymer electrolyte includes a fluorine-based electrolyte, The tungsten oxide hydrate is WO 3 ・nH 2 O (where n=1 / 3 and / or 2). (2) The content of the first fine particles is 0.5 mass % or more and 3.0 mass % or less. (3) The composite electrolyte is used in an electrolyte membrane and / or a catalyst layer of a polymer electrolyte fuel cell.

2. The composite electrolyte according to claim 1 , wherein the first fine particles have an average particle size of 8 nm or more and 65 nm or less.

3. (a) ions of a second metal element having a radical scavenging function, which are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte, and / or (b) second fine particles made of a second compound containing the second metal element, the second fine particles being dispersed in the solid polymer electrolyte; The composite electrolyte according to claim 1 or 2, further comprising:

4. The composite electrolyte according to claim 3 , wherein the second metal element is Ce.

5. The composite electrolyte according to claim 3 or 4, which satisfies the following formula (1): 0.0005≦M / A≦0.15 (1) however, M / A is the ratio of the number of moles (M) of the second metal element to the number of moles (A) of the acid groups contained in the solid polymer electrolyte.

6. An electrolyte membrane comprising a composite electrolyte described in any one of claims 1 to 5.

7. A catalyst layer comprising a composite electrolyte according to claim 1.

8. A solid polymer fuel cell comprising the electrolyte membrane described in claim 6 and / or the catalyst layer described in claim 7.

Citation Information

Patent Citations

  • Yosetsuyokaabudochitsupu

    JP1976094448A

  • Proton conductive material

    JP2003331869A

  • Transition metal oxide containing solid polyelectrolyte

    JP2005019232A

  • Manufacturing method for fuel cells

    JP2008034162A

  • Electrolyte membrane for fuel cell, membrane electrode assembly, and fuel cell

    JP2008091187A