Rubber particles, composite particles and their manufacturing method

The introduction of a copolymer with a polyester and polyorganosiloxane structure into silicone rubber particles enhances their degradability and dispersibility, mitigating environmental accumulation and ecological risks.

JP7570797B2Active Publication Date: 2024-10-22SHIN ETSU CHEMICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022537944
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-21
Filing Date
2021-07-13
Publication Date
2024-10-22
Estimated Expiration
2041-07-13

AI Technical Summary

Technical Problem

Silicone rubber particles used in resins and cosmetics are difficult to recover and decompose in the environment due to their small size and non-degradable crosslinked structure, posing a risk to ecosystems by accumulating in oceans and adsorbing harmful substances.

Method used

Development of rubber particles and composite particles containing a copolymer with a polyester structure and a polyorganosiloxane structure, incorporating degradable functional groups, such as aliphatic unsaturated groups, to facilitate environmental decomposition.

Benefits of technology

The particles exhibit high dispersibility, low cohesiveness, and degradability, reducing environmental impact by breaking down in the presence of moisture, thus addressing the accumulation and ecological concerns of silicone rubber particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570797000001
    Figure 0007570797000001
  • Figure 0007570797000002
    Figure 0007570797000002
  • Figure 0007570797000003
    Figure 0007570797000003
Patent Text Reader

Abstract

Provided are: rubber particles having high dispersibility and high degradability and including a polysiloxane structure; composite particles; and production methods for these particles. The rubber particles comprise a copolymer including both a polyester structure and an organopolysiloxane structure, wherein the copolymer is a product of hydrolysilation and crosslinking of both (A) a polyester having at least two aliphatic unsaturated groups in the molecule and (B) an organohydrogen polysiloxane having at least two silicon-atom-bonded hydrogen atoms in the molecule. The composite particles comprise the rubber particles, the surface of which is coated with a polyorganosilsesquioxane or silica.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to rubber particles, composite particles, and methods for producing the same. [Background technology]

[0002] Silicone rubber particles having rubber elasticity are used as stress relaxants for resins.For example, rubber particles are mixed into thermosetting resins such as epoxy resins used for packaging electronic and electrical parts, so that the package is not easily broken even when the package is stressed by the expansion caused by the heat generated by the electrical parts.In addition, silicone rubber particles are used in cosmetics to give the use feeling such as soft touch and smoothness and extensibility.

[0003] As silicone rubber particles, composite particles in which silicone rubber particles are coated with polyorganosilsesquioxane resin (Patent Document 1: JP-A-7-196815) and composite particles in which silicone rubber particles are coated with metal oxide particles such as silica (Patent Document 2: JP-A-4-348143) have also been proposed. These composite particles are characterized by low coagulation and high dispersibility.

[0004] Furthermore, as particles having good dispersibility in thermoplastic resins and the like, Patent Document 3: JP 2001-40214 A describes organic crosslinked particles obtained by crosslinking, via a hydrosilylation reaction, a liquid composition consisting of an organic compound having an aliphatic saturated bond and a silicon-containing organic compound having silicon-bonded hydrogen atoms. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-196815 [Patent Document 2] Japanese Patent Application Publication No. 4-348143 [Patent Document 3] JP 2001-40214 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, when such silicone rubber particles, which are incorporated into resins, cosmetics, etc., are discarded into the environment, their extremely small particle size makes them extremely difficult to recover, and so they are likely to end up directly flowing into land waters and into the ocean. Silicone rubber particles discarded in land waters or the ocean do not have a decomposition structure within their particle structure, so they are not decomposed in the environment and are expected to continue to remain in the environment.

[0007] In addition, marine microplastics have the property of adsorbing harmful substances and pathogens in the environment, and there are concerns that they may have a negative impact on the ecosystem, leading to the beginning of a movement to regulate microplastics. Against this background, there is a growing demand for silicone rubber particles that decompose in the environment after use and do not continue to remain as particles (solids). In order for silicone rubber particles to decompose in the environment, the crosslinked structure of the rubber particles needs to be decomposed (cut) in the environment, but since silicone rubber particles are not structurally degradable, a structure containing a degradable functional group must be introduced into the crosslinked structure.

[0008] Specifically disclosed in Patent Document 3 are particles in which polypropylene oxide containing allyl groups at both ends is crosslinked with organopolysiloxane containing silicon-bonded hydrogen atoms, and particles in which hexadiene is crosslinked with dimethylpolysiloxane-methylhydrogenpolysiloxane. These particles are poorly degradable because they do not contain degradable functional groups that are factors for decomposition in the environment. Therefore, an object of the present invention is to provide rubber particles and composite particles containing a polysiloxane structure, which have high dispersibility and high degradability, and a method for producing the same. [Means for solving the problem]

[0009] As a result of intensive research to achieve the above-mentioned object, the inventors have discovered that rubber particles and composite particles made of a copolymer containing a polyester structure and a polyorganosiloxane structure can solve the above-mentioned problems, thereby completing the present invention.

[0010] Accordingly, the present invention provides the following rubber particles, composite particles, and methods for producing the same. [1]. Rubber particles comprising a copolymer containing a polyester structure and an organopolysiloxane structure. [2]. The rubber particles according to [1], which have a spherical particle shape and a volume average particle size of 0.1 to 50 μm. [3]. The copolymer is (A) a polyester having at least two aliphatic unsaturated groups in one molecule, and (B) Organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in each molecule. wherein the rubber particles are a hydrosilylated crosslinked product of the above formula (1) or (2), except for the case where the component (A) has two aliphatic unsaturated groups in one molecule and the component (B) has two hydrogen atoms bonded to silicon atoms in one molecule. [4]. The polyester of component (A) having at least two aliphatic unsaturated groups in each molecule is The rubber particles according to [3], which are obtained by substituting an aliphatic unsaturated group for the molecular chain terminal of a polyester or polyester copolymer having a linear or branched chain structure. [5]. The rubber particles according to [4], wherein the polyester structure of the component (A) is poly-ε-caprolactone. [6]. The component (B) is represented by the following general formula (1): [ka] (R 1 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms; R 2are each independently a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms, 1≦m≦1000, 0≦n≦1000, provided that when n=0, two R 2 are both hydrogen atoms, and the two R 2 and n is 2 or more when neither of them is a hydrogen atom. [7]. The component (B) is represented by the following general formula (2): [ka] (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms, excluding a phenyl group, and 0≦a≦500, 1≦b≦1000, 1≦a+b≦1000, 0≦c≦1000, provided that when c=0, two R 2 are both hydrogen atoms, and the two R 2 and c is 2 or more when neither of them is a hydrogen atom. [8].

[0021] A composite particle comprising the rubber particle according to any one of [3] to [7], the surface of which is coated with polyorganosilsesquioxane or silica. [9]. A method for producing the rubber particles according to any one of [3] to [7], comprising the following steps (i) to (iii): (i) A process for obtaining an O / W type emulsion by adding an aqueous phase component containing a surfactant to an oil phase component composed of a polyester (A) having at least two aliphatic unsaturated groups in one molecule and an organohydrogenpolysiloxane (B) having at least two hydrogen atoms bonded to silicon atoms in one molecule, and emulsifying the aqueous phase component. (ii) A step of curing the oil phase component consisting of components (A) and (B) in the emulsion by a hydrosilylation reaction in the presence of a hydrosilylation-reactive catalyst to obtain an aqueous dispersion of rubber particles (C). (iii) A step of obtaining rubber particles by drying and removing the water, which is the continuous phase, from the aqueous dispersion (C) of rubber particles obtained in step (ii).

[10] . A method for producing the composite particle according to [8], comprising the following steps (i) to (v): (i) A process for obtaining an O / W type emulsion by adding an aqueous phase component containing a surfactant to an oil phase component composed of a polyester (A) having at least two aliphatic unsaturated groups in one molecule and an organohydrogenpolysiloxane (B) having at least two hydrogen atoms bonded to silicon atoms in one molecule, and stirring the mixture. (ii) A step of curing the oil phase component consisting of components (A) and (B) in the emulsion by a hydrosilylation reaction in the presence of a hydrosilylation-reactive catalyst to obtain an aqueous dispersion of rubber particles (C). (iii') A step of adding an alkaline substance (E) to the aqueous dispersion (C) of rubber particles obtained in the step (ii). (iv) The aqueous dispersion of rubber particles to which the alkaline substance obtained in step (iii') has been added is treated with a compound represented by the following general formula (3): [ka] (R 4 is a monovalent hydrocarbon group having 1 to 6 carbon atoms, R 5 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms or -OR 4 ) and carrying out a condensation reaction to coat the surfaces of the rubber particles with polyorganosilsesquioxane or silica, thereby obtaining an aqueous dispersion of composite particles. (v) A step of obtaining composite particles by drying and removing the water, which is the continuous phase, from the aqueous dispersion of the composite particles obtained in step (iv). Effect of the Invention

[0011] The rubber particles and composite particles of the present invention contain ester groups (polyester structures) that are degradable functional groups in the particles, and the crosslinked structures are broken in a moisture-containing environment, making them degradable. In particular, particles that have a poly-ε-caprolactone structure, which is a microorganism recognition skeleton, as the polyester structure in the particles can be expected to be environmentally degradable as rubber particles. Therefore, the rubber particles and composite particles of the present invention are particles that have low coagulation tendency, high dispersibility, and degradability, and are expected to be used as materials that reduce the environmental load. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. The rubber particles of the present invention are rubber particles made of a copolymer containing a polyester structure and an organopolysiloxane structure, and the composite particles are particles in which the surface of the rubber particles is coated with polyorganosilsesquioxane or silica.

[0013] [Rubber particles] The shape of the rubber particles of the present invention is not particularly limited, but is preferably spherical. In the present invention, "spherical" does not only refer to a particle shape that is a true sphere, but also means that it includes a deformed ellipsoid having an aspect ratio (length of the longest axis / length of the shortest axis) that is usually in the range of 1 to 4, preferably 1 to 2, more preferably 1 to 1.6, and even more preferably 1 to 1.4 on average. The shape of the particles can be confirmed by observation using, for example, an optical microscope or an electron microscope, and the aspect ratio is a value calculated by measuring the lengths of the longest axis and the shortest axis of 100 particles arbitrarily selected from a micrograph and averaging them.

[0014] The volume average particle diameter of the rubber particles is preferably 0.1 to 50 μm, more preferably 0.5 to 40 μm, and further preferably 1 to 20 μm. If the volume average particle diameter of the rubber particles is less than 0.1 μm, the particles have low fluidity and high coagulation. In addition, when the rubber particles are coated with polyorganosilsesquioxane or silica, it is difficult to coat the particles uniformly. If the volume average particle diameter is greater than 50 μm, the smoothness decreases and a rough feeling may occur. In the present invention, the particle diameter is the volume average particle diameter measured by an electrical resistance method.

[0015] The rubber, which is a component of the rubber particles, is preferably free of tack, and its rubber hardness, as measured by an Asker rubber hardness tester type C specified in the Society of Rubber Industry Standards of Japan (SRIS), is preferably 5 to 90, more preferably 20 to 85, and even more preferably 40 to 85. If the rubber hardness is less than 5, the cohesiveness increases and dispersibility decreases.

[0016] The rubber particles of the present invention are (A) a polyester having at least two aliphatic unsaturated groups in one molecule, and (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule (excluding the case where the component (A) has two aliphatic unsaturated groups in one molecule and the component (B) has two hydrogen atoms bonded to silicon atoms in one molecule). It is preferable that the liquid composition is a particle obtained by copolymerizing the liquid composition by a hydrosilylation reaction.

[0017] The polyester having at least two aliphatic unsaturated groups in one molecule of component (A) is, for example, a polyester or polyester copolymer having a linear or branched chain structure in which the molecular chain terminals are substituted with aliphatic unsaturated groups. That is, component (A) has a linear or branched chain structure, at least one polyester structure (polyester repeating unit), and has an aliphatic unsaturated group at the molecular chain terminal. This component (A) can be obtained, for example, by substituting the molecular chain terminal of a polyester, polyester copolymer, polyester polyol, etc. with an aliphatic unsaturated group. Examples of the polyester include aliphatic polyesters such as poly-ε-caprolactone, poly-β-propiolactone, γ-butyrolactone, polylactic acid, polyhydroxybutyrate, polyglycolic acid, polyethylene adipate, polyhydroxybutyric acid, polyethylene succinate, and polybutylene succinate; and aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polytrimethylene terephthalate. Of these, aliphatic polyesters, which are considered to be more degradable, are preferred.

[0018] The polyester copolymer may be a copolymer of the polyester and another polymer. The other polymer may be selected from the polyesters or may be a polymer other than polyester, such as polyether or polycarbonate. For the reasons mentioned above, the polyester copolymer is preferably a copolymer of aliphatic polyesters, such as an L-lactic acid / ε-caprolactone copolymer or an L-lactic acid / glycolic acid copolymer.

[0019] Examples of the polyester polyol include polyester polyols such as polyethylene adipateol, polytetramethylene adipate diol, and polyethylene adipate diol, and polylactone polyols such as poly-ε-caprolactone diol, poly-ε-caprolactone triol, and poly-ε-caprolactone tetraol. Of these, polylactone polyols are preferred, and poly-ε-caprolactone diol represented by the following formula (4), poly-ε-caprolactone triol represented by the following formula (5), and poly-ε-caprolactone tetraol represented by the following formula (6) are more preferred. [ka]

[0020] Examples of poly-ε-caprolactone polyols include polyaddition products of lactones with aliphatic polyhydric alcohols having 2 to 20 carbon atoms, and in the formula R 6 ~R 8 is an aliphatic polyhydric alcohol residue having 2 to 20 carbon atoms, and in the formula, k, l, m, and n are integers satisfying 1≦k+l+m+n≦100.

[0021] R in the above formula (4) 6is an aliphatic group having 2 to 20 carbon atoms, and the aliphatic group is an aliphatic hydrocarbon group having 2 to 20 carbon atoms, which may contain a heteroatom such as an oxygen atom, and specifically, is a residue derived from the following aliphatic dihydric alcohol. Examples of the aliphatic dihydric alcohols include linear alcohols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-dodecanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol; 1,2-, 1,3-, or 2,3-butanediol, 2-methyl-1,4-butanediol, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,6-hexanediol, 3-methyl-1,6-hexanediol, 2-methyl-1,7- Branched alcohols such as heptanediol, 3-methyl-1,7-heptanediol, 4-methyl-1,7-heptanediol, 2-methyl-1,8-octanediol, 3-methyl-1,8-octanediol and 4-methyloctanediol; alicyclic alcohols such as 1,4-cyclohexanediol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanediol, 1,3-cyclopentanediol, 1,4-cycloheptanediol, 2,5-bis(hydroxymethyl)-1,4-dioxane, 2,7-norbornanediol, tetrahydrofuran dimethanol, 1,4-bis(hydroxyethoxy)cyclohexane, 1,4-bis(hydroxymethyl)cyclohexane and 2,2-bis(4-hydroxycyclohexyl)propane. Commercially available poly-ε-caprolactone diols include, for example, Plaxel 205U [manufactured by Daicel Corporation].

[0022] R in the above formula (5) 7is an aliphatic group having 2 to 20 carbon atoms, the aliphatic group being an aliphatic hydrocarbon group having 2 to 20 carbon atoms, which may contain a heteroatom such as an oxygen atom, and specifically is a residue derived from the following aliphatic trihydric alcohol. Examples of the aliphatic trihydric alcohol include glycerin, trimethylolethane, and trimethylolpropane. Examples of commercially available poly-ε-caprolactone triol include Placcel 305 [manufactured by Daicel Corporation].

[0023] R in the above formula (6) 8 is an aliphatic group having 2 to 20 carbon atoms, the aliphatic group being an aliphatic hydrocarbon group having 2 to 20 carbon atoms, which may contain a heteroatom such as an oxygen atom, and specifically is a residue derived from the following aliphatic tetrahydric alcohol. An example of the aliphatic tetrahydric alcohol is pentaerythritol. An example of a commercially available product thereof is Plaxel 410 [manufactured by Daicel Corporation].

[0024] The method for producing the component (A) includes a method of introducing a molecule having an aliphatic unsaturated group at one end of the molecule into the polyester, polyester copolymer, or polyester polyol having a linear or branched structure exemplified above via an ester bond, an ether bond, a urethane bond, a urea bond, an amide bond, a sulfide bond, or the like. Specifically, for example, the above-mentioned polylactone polyol may be reacted with an acid halide, which has excellent stability and reaction rate of the polyester during reaction, as a molecule having an aliphatic unsaturated group at one end of the molecule that forms the above bond, and acid chlorides are preferred in terms of availability and cost. The aliphatic unsaturated group is preferably present at the molecular end, and examples of the aliphatic unsaturated group include alkenyl groups such as vinyl groups, allyl groups, butenyl groups, pentenyl groups, and hexenyl groups, alkynyl groups such as ethynyl groups, cyclic unsaturated groups such as norbornene groups and dicyclopentadienyl groups, and the alkenyl group is preferred. Examples of the acid chloride having an alkenyl group at the molecular end include 4-pentenoyl chloride, 6-heptenoyl chloride, 8-nonenoyl chloride, and 10-undecenoyl chloride.

[0025] Component (A) is preferably in a liquid state, and has a weight average molecular weight measured by gel permeation chromatography (GPC) of preferably 200 to 10,000, and more preferably 300 to 5,000. If the molecular weight is less than 200, decomposition may be impaired, and if it is more than 10,000, preparation of rubber particles becomes difficult.

[0026] The structure of the organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule of component (B) may be linear, cyclic, or branched. A linear structure is preferred, and a structure represented by the following formula (1) is preferred. In formula (1), R 1 R is each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms. 2 are each independently a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms. m is a number of 1≦m≦1000, and n is a number of 0≦n≦1000, preferably 1≦m≦500, 1≦n≦500. When n=0, two R 2 is a hydrogen atom, and two R 2 When neither of are hydrogen atoms, n is 2 or more. [ka]

[0027] R 1Examples of the alkyl groups include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, decyl, undecyl, dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, henicosyl, docosyl, tricosyl, tetracosyl, and triacontyl; aryl groups such as phenyl, tolyl, and naphthyl; aralkyl groups such as benzyl and phenethyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; and hydrocarbon groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with atoms such as halogen atoms (fluorine, chlorine, bromine, and iodine atoms) and / or substituents such as acryloyloxy, methacryloyloxy, epoxy, glycidoxy, and carboxyl.

[0028] In formula (1), R 2 R is a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms. 2 The unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms includes the above R 1 The same is exemplified.

[0029] Component (B) is preferably an organohydrogenpolysiloxane further containing a diphenylsiloxy unit represented by the following formula (2): 1 and R 2 is the same as in formula (1), and R 3 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms other than a phenyl group. [ka]

[0030] In formula (2), R 3Examples of the alkyl groups include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, decyl, undecyl, dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, henicosyl, docosyl, tricosyl, tetracosyl, and triacontyl groups; aryl groups other than phenyl groups such as tolyl and naphthyl groups; aralkyl groups such as benzyl and phenethyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups; and hydrocarbon groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with atoms such as halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms) and / or substituents such as acryloyloxy groups, methacryloyloxy groups, epoxy groups, glycidoxy groups, and carboxyl groups.

[0031] In formula (2), a, b, and c are in the ranges of 0≦a≦500, 1≦b≦1000, 1≦a+b≦1000, and 0≦c≦1000, and preferably 0≦a≦250, 1≦b≦500, and 1≦c≦500. However, when c=0, two R 2 are both hydrogen atoms, and the two R 2 When neither of are hydrogen atoms, c is 2 or more.

[0032] The (A) polyester having at least two aliphatic unsaturated groups per molecule and the (B) organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule are preferably such that either the aliphatic unsaturated groups of component (A) or the hydrogen atoms of component (B) are at least 3. The compounding ratio of components (A) and (B) is preferably such that the number of hydrosilyl groups of component B is 0.5 to 2.0 for each aliphatic unsaturated group of component (A).

[0033] Examples of the hydrosilylation catalyst for crosslinking the (A) component and the (B) component include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, but platinum-based catalysts are preferred. Specific examples of platinum-based catalysts include platinum (including platinum black), platinum-supported carbon or silica, chloroplatinic acid, platinum-olefin complex, platinum-alcohol complex, platinum-vinyl group-containing siloxane complex, and chloroplatinic acid-vinyl group-containing siloxane complex. The amount of platinum-based catalyst to be blended may be a catalytic amount as a hydrosilylation reaction catalyst. Specifically, the amount is about 0.1 to 500 ppm, preferably about 0.1 to 200 ppm, and more preferably about 0.5 to 100 ppm, calculated as the platinum mass in the catalyst. If the amount is less than 0.1 ppm, the curing is slow and the catalyst is easily affected by catalyst poisons. On the other hand, if the amount exceeds 500 ppm, coloring of the rubber particles is observed and it is not economically preferable.

[0034] [Method of production of component (A)] Examples of methods for producing component (A) include, but are not limited to, the following. 1 mole of the polylactone polyol or polyester polyol component shown in the above formulas (4) to (6) is mixed with an excess of 2.2 to 8.0 moles, preferably 2.5 to 6.0 moles, of a base for capturing hydrogen chloride generated, and 2.0 to 7.0 moles, preferably an excess of more than 2.2 moles but not more than 6.0 moles, of the acid chloride having an aliphatic unsaturated group at the molecular end is dropped thereto, and the reaction is carried out under heating for 30 minutes to 6 hours, preferably 1 hour to 2 hours. After the reaction, the reaction product is extracted, washed with water, and by-products are removed in an adsorption step, and the solvent is distilled off to obtain component (A).

[0035] The base is added to capture hydrogen chloride produced by the reaction, and is not reactive with the polylactone polyol or polyester polyol or the acid chloride. As such a base, a tertiary amine is preferred, and triethylamine is more preferred.

[0036] In the extraction step, a hydrophobic organic solvent may be used to adjust the viscosity of the reaction product. The hydrophobic organic solvent is not particularly limited, but toluene is preferred from the viewpoint of solubility.

[0037] Adsorption is a process for removing hydrochlorides of bases that cannot be completely removed in the washing process, and for dehydration, decolorization, and deodorization. Any known adsorbent can be used, and a combination of multiple adsorbents may be used. Preferred adsorbents include desiccants such as magnesium sulfate and sodium sulfate, activated carbon, and Kyoward series (manufactured by Kyowa Chemical Industry Co., Ltd.).

[0038] [Method of manufacturing rubber particles] The rubber particles of the present invention can be produced, for example, by a method having the following steps (i) to (iii). (i) (A) a polyester having at least two aliphatic unsaturated groups in one molecule; (B) an oil phase component composed of an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, An O / W type emulsion is prepared by adding an aqueous phase component containing a surfactant and stirring. (ii) An oil phase component consisting of components (A) and (B) in the O / W emulsion is cured in the presence of the hydrosilylation catalyst to obtain an aqueous dispersion (C) of rubber particles. (iii) The rubber particles can be obtained by drying and removing the water, which is the continuous phase of the water dispersion of the rubber particles.

[0039] Process (i) The surfactant used in step (i) is not particularly limited and may be a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. These may be used alone or in appropriate combination of two or more.

[0040] Examples of the nonionic surfactant used herein include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene hydrogenated castor oil fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene modified organopolysiloxanes, and polyoxyethylene polyoxypropylene modified organopolysiloxanes.

[0041] Examples of the anionic surfactant include alkyl sulfate salts such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfate salts, polyoxyethylene alkyl phenyl ether sulfate salts, sulfate salts of aliphatic alkylol amides, alkyl benzene sulfonates, polyoxyethylene alkyl phenyl ether sulfonates, alkyl diphenyl ether disulfonates, alkanesulfonates, N-acyltaurate salts, dialkyl sulfosuccinates, monoalkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, fatty acid salts, polyoxyethylene alkyl ether carboxylates, N-acyl amino acid salts, monoalkyl phosphate salts, dialkyl phosphate salts, polyoxyethylene alkyl ether phosphate salts, and the like.

[0042] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, polyoxyethylenealkyldimethylammonium salts, dipolyoxyethylenealkylmethylammonium salts, tripolyoxyethylenealkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, and monoalkylamidoamine salts.

[0043] Examples of the amphoteric surfactant include alkyl dimethylamine oxide, alkyl dimethyl carboxybetaine, alkyl amidopropyl dimethyl carboxybetaine, alkyl hydroxysulfobetaine, and alkyl carboxymethyl hydroxyethyl imidazolinium betaine.

[0044] As the surfactant, a nonionic surfactant is preferred, since a small amount of the surfactant is sufficient to emulsify the curable liquid silicone composition and form fine particles.

[0045] The amount of the surfactant added is preferably 0.01 to 20 parts by mass, more preferably 0.05 to 10 parts by mass, based on 100 parts by mass of the emulsion. If the amount is less than 0.01 parts by mass, problems such as failure to emulsify or failure to form fine particles occur. If the amount is more than 20 parts by mass, it becomes difficult to coat the rubber particles with polyorganosilsesquioxane or silica in the composite particle production process described below.

[0046] The content of the oil phase components in the emulsion, that is, the polyester (A) having at least two aliphatic unsaturated groups in one molecule and the organohydrogenpolysiloxane (B) having at least two hydrogen atoms bonded to silicon atoms in one molecule, is preferably 1 to 80 parts by mass, more preferably 10 to 60 parts by mass, per 100 parts by mass of the emulsion. If it is less than 1 part by mass, it is efficient, and if it is more than 80 parts by mass, it is difficult to obtain an aqueous dispersion of rubber particles.

[0047] To carry out the emulsification, a known emulsifying disperser may be used. Examples of common emulsifying dispersers include high-speed rotary shear type agitators such as a homomixer, high-speed centrifugal radiation type agitators such as a homodisper, high-pressure jet type emulsifying dispersers such as a homogenizer, colloid mills, ultrasonic emulsifiers, and the like.

[0048] Process (ii) The oil phase component in the emulsion thus prepared can be cured in the presence of the hydrosilylation catalyst to obtain a dispersion of rubber particles. The hydrosilylation catalyst may be added to the oil phase before the preparation of the emulsion, or may be added after the preparation of the emulsion. When the hydrosilylation catalyst is added after the preparation of the emulsion, the hydrosilylation catalyst may not be dispersed. In that case, the surfactant may be mixed with the hydrosilylation catalyst before the addition. The hydrosilylation may be carried out at room temperature, or may be carried out under heating at less than 100°C if the reaction is not completed. The hydrosilylation reaction time is appropriately selected. By this method, an aqueous dispersion of rubber particles having a volume average particle size of 0.1 to 50 μm can be obtained.

[0049] Process (iii) The rubber particles can be obtained by drying and removing the water, which is the continuous phase, from the obtained aqueous dispersion of rubber particles. The drying and removal of water from the aqueous dispersion of rubber particles can be carried out, for example, by heating under normal pressure or reduced pressure. Specifically, the dispersion is allowed to stand under heating to remove water, the dispersion is stirred and fluidized under heating to remove water, the dispersion is sprayed and dispersed in a hot air stream as in a spray dryer, and a fluidized heat medium is used. As a pretreatment for this operation, the dispersion may be concentrated by a method such as heat dehydration, filtration separation, or decantation, or the dispersion may be washed with water or alcohol if necessary.

[0050] [Composite particles] The shape of the polyorganosilsesquioxane or silica coated on the surface of the composite particle is not particularly limited, but in the case of the manufacturing method described below, it is granular. The particle size is preferably small, specifically 500 nm or less. The organosilsesquioxane or silica may be coated on a part or all of the surface of the rubber particle, but it is preferable that the entire surface of the rubber particle is coated with almost no gaps. The state, shape and particle size of the coating can be confirmed by observing the particle surface with an electron microscope.

[0051] The amount of polyorganosilsesquioxane or silica coating the particle surface is not particularly limited, but the ratio is preferably 0.5 to 200 parts by mass, and more preferably 1 to 50 parts by mass, per 100 parts by mass of the rubber particles.

[0052] [Method of manufacturing composite particles] The composite particles of the present invention are (C) Water dispersion of rubber particles, (D) water (optional); (E) alkaline substances, In a liquid containing (F) one selected from organotrialkoxysilanes, tetraalkoxysilanes, and hydrolysates thereof, represented by the following general formula (3): and carrying out a hydrolysis and condensation reaction to coat the surfaces of the rubber particles with polyorganosilsesquioxane or silica. [ka] In formula (3), R 4 are each independently a monovalent hydrocarbon group having 1 to 6 carbon atoms; R 5 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms or -OR 4 It is. That is, the composite particles of the present invention can be produced by a method having the following steps (i) to (v). (i) A process for obtaining an O / W type emulsion by adding an aqueous phase component containing a surfactant to an oil phase component composed of a polyester (A) having at least two aliphatic unsaturated groups in one molecule and an organohydrogenpolysiloxane (B) having at least two hydrogen atoms bonded to silicon atoms in one molecule, and stirring the mixture. (ii) A step of curing the oil phase component consisting of components (A) and (B) in the emulsion by a hydrosilylation reaction in the presence of a hydrosilylation-reactive catalyst to obtain an aqueous dispersion of rubber particles (C). (iii') A step of adding an alkaline substance (E) to the aqueous dispersion (C) of rubber particles obtained in the step (ii). (iv) A step of adding one (F) selected from organotrialkoxysilanes, tetraalkoxysilanes, and hydrolysates thereof represented by the general formula (3) to the aqueous dispersion of rubber particles to which the alkaline substance obtained in the step (iii') has been added, and carrying out a condensation reaction to coat the surfaces of the rubber particles with polyorganosilsesquioxane or silica, thereby obtaining an aqueous dispersion of composite particles. (v) A step of obtaining composite particles by drying and removing the water, which is the continuous phase, from the aqueous dispersion of the composite particles obtained in step (iv). The steps (i) and (ii) of the method for producing the composite particles are the same as the steps (i) and (ii) of the method for producing the rubber particles. In addition, in the step (iii'), water (D) may be added as an optional component.

[0053] Process (iii') (D)Water The water is not particularly limited, and purified water or the like is used, and includes the water in the water dispersion of rubber particles obtained in the above step (ii) and water added as necessary.

[0054] (E) Alkaline substances The alkaline substance may be any substance that acts as a catalyst for the hydrolysis and condensation reaction of organotrialkoxysilane or tetraalkoxysilane. Specific examples of the alkaline substance that can be used include alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, lithium hydroxide, etc.; alkaline earth metal hydroxides such as calcium hydroxide, barium hydroxide, etc.; alkali metal carbonates such as potassium carbonate, sodium carbonate, etc.; amines such as ammonia, monomethylamine, dimethylamine, etc.; and quaternary ammonium hydroxides such as tetramethylammonium hydroxide, etc. More preferred is ammonia, which has excellent water solubility and catalytic activity and is easily removed by volatilization, and for this purpose an aqueous ammonia solution that is generally available on the market can be used.

[0055] The amount of component (E) added is preferably an amount that gives a pH of 9.0 to 13.0, more preferably an amount that gives a pH of 10.0 to 12.5, at 25° C. for the liquid containing (C) to (E). If the pH is lower than 10.0, the hydrolysis and condensation reaction of the organotrialkoxysilane or tetraalkoxysilane does not proceed sufficiently, whereas if the pH is higher than 13.0, the hydrolysis rate increases and the hydrolysis and condensation reaction occurs in areas other than the surfaces of the rubber particles, resulting in poor coverage.

[0056] When the component (F) is added, one or more members selected from the group consisting of cationic surfactants and cationic water-soluble polymer compounds (G) may be added. The cationic surfactant and the cationic water-soluble polymer compound have the effect of promoting the condensation reaction of the hydrolyzed organotrialkoxysilane or tetraalkoxysilane to produce polyorganosilsesquioxane or silica, and may also cause the produced polyorganosilsesquioxane or silica to be adsorbed onto the surface of the rubber particles.

[0057] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, polyoxyethylenealkyldimethylammonium salts, dipolyoxyethylenealkylmethylammonium salts, tripolyoxyethylenealkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, monoalkylamidoamine salts, etc. Among these, alkyltrimethylammonium salts are preferred, and lauryltrimethylammonium salts and cetyltrimethylammonium salts are more preferred.

[0058] Examples of cationic water-soluble polymer compounds include polymers of dimethyldiallylammonium chloride, polymers of vinylimidazoline, polymers of methylvinylimidazolium chloride, polymers of ethyl trimethyl ammonium chloride acrylate, polymers of ethyl trimethyl ammonium chloride methacrylate, polymers of acrylamidopropyl trimethyl ammonium chloride, polymers of methacrylamidopropyl trimethyl ammonium chloride, epichlorohydrin / dimethylamine polymers, polymers of ethyleneimine, quaternary products of polymers of ethyleneimine, polymers of allylamine hydrochloride, polylysine, cationic starch, cationic cellulose, chitosan, and derivatives thereof obtained by copolymerizing monomers having nonionic groups or anionic groups with these, etc. Among these, polymers of dimethyldiallyl ammonium chloride are preferred.

[0059] The amount of component (G) added is preferably 0.001 to 2 parts by mass, more preferably 0.005 to 1 part by mass, per 100 parts by mass of water in the liquid containing components (C) to (E). If the amount added is more than 2 parts by mass, there is a risk that polyorganosilsesquioxane or silica will not be coated on the surfaces of the rubber particles.

[0060] (F) One selected from organotrialkoxysilanes, tetraalkoxysilanes, and hydrolysates thereof, represented by the above general formula (3). The polyorganosilsesquioxane or silica that coats the rubber particles is formed by adding one selected from organotrialkoxysilane, tetraalkoxysilane, and their hydrolyzates, which are represented by the above-mentioned general formula (3), to the rubber particles. In this formula, R 4 is a monovalent hydrocarbon group having 1 to 6 carbon atoms, and examples of such groups include a methyl group, an ethyl group, a propyl group, and a butyl group. 5 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms or -OR 4 Examples of unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl; aryl groups such as phenyl and tolyl; alkenyl groups such as vinyl and allyl; aralkyl groups such as β-phenylethyl and β-phenylpropyl; monovalent halogenated hydrocarbon groups such as chloromethyl and 3,3,3-trifluoropropyl; and groups in which these monovalent hydrocarbon groups are substituted with epoxy, amino, mercapto, acryloxy, methacryloxy, or the like. R 5 When R is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, the rubber particles are coated with polyorganosilsesquioxane, and R 5 -OR 4 In this case, it is silica that coats the rubber particles. Specific examples of organotrialkoxysilanes and tetraalkoxysilanes used for coating include methyltrimethoxysilane, methyltriethoxysilane, methyltripoxysilane, methyltributoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, γ-methacrylicoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3,3,4,4,5,5,6,6,6-nonafluorohexyltrimethoxysilane, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-heptadecafluorodecyltrimethoxysilane, tetramethoxysilane, and tetraethoxysilane.

[0061] The amount of component (F) added is preferably 20 parts by mass or less per 100 parts by mass of water in the liquid containing components (C) to (E). If the amount is more than 20 parts by mass, there is a risk of lumps forming.

[0062] Process (iv) (F) one selected from organotrialkoxysilane, tetraalkoxysilane and their hydrolysates is added to a liquid containing (C) to (E) and (G), and the organotrialkoxysilane and tetraalkoxysilane are hydrolyzed and condensed to coat the surface of the rubber particles with polyorganosilsesquioxane or silica. Specifically, (F) one selected from organotrialkoxysilane, tetraalkoxysilane and their hydrolysates is added to an aqueous solution in which (C) rubber particle aqueous dispersion and (D) water (optional) are dissolved with (E) an alkaline substance, (G) one or more selected from cationic surfactants and cationic water-soluble polymer compounds (optional), and hydrolysis and condensation are carried out. This condensate, i.e., polyorganosilsesquioxane or silica, coats the surface of the rubber particles, forming composite particles.

[0063] The organotrialkoxysilane, tetraalkoxysilane, and hydrolysates thereof are preferably added under stirring using a normal stirrer such as a propeller blade, flat blade, etc. The organotrialkoxysilane, tetraalkoxysilane, and hydrolysates thereof are preferably added over a period of time, and the dropwise addition time is preferably 1 minute to 6 hours, and more preferably 10 minutes to 3 hours.

[0064] The temperature in the system during the dropping is preferably in the range of 0 to 60° C., and more preferably in the range of 0 to 40° C. When the temperature is in this range, the surfaces of the rubber particles can be coated with polyorganosilsesquioxane and silica.

[0065] Process (v) After completion of the hydrolysis and condensation reaction, the composite particles can be obtained by drying and removing the water, which is the continuous phase, from the aqueous dispersion of the composite particles of the present invention obtained. The removal of water can be carried out, for example, by heating the aqueous dispersion after the reaction under normal pressure or reduced pressure. Specifically, the method of removing water by leaving the dispersion at rest under heating, the method of removing water while stirring and flowing the dispersion under heating, the method of spraying and dispersing the dispersion in a hot air current as in a spray dryer, the method of using a fluidized heat medium, etc. can be mentioned. In addition, as a pretreatment for this operation, the dispersion can be concentrated by a method such as heat dehydration, filtration separation, centrifugation, decantation, etc., and the dispersion can be washed with water or alcohol if necessary.

[0066] When the product obtained by drying and removing water from the aqueous dispersion after the reaction is aggregated, the product can be disintegrated with a grinding machine such as a jet mill, a ball mill, or a hammer mill to obtain composite particles in which the surfaces of the rubber particles are coated with polyorganosilsesquioxane and silica. EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, the kinetic viscosity is a value measured at 25°C, and "%" representing concentration and content means "mass %". The penetration of the cured rubber is a value measured in accordance with the Standards and Regulations of the Society of Rubber Industry, Japan (SRIS). The molecular weight of component (A) is a weight average molecular weight measured by GPC under the following conditions, using polystyrene as a standard substance. [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.60mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-H TSKgel SuperHM-N TSKgel SuperH2500 (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 50 μL (THF solution with a concentration of 0.5% by mass) EXAMPLES

[0068] [Synthesis of alkenyl-containing poly-ε-caprolactone 1] 200g of poly-ε-caprolactone diol (trade name: PLACCEL 205U, manufactured by Daicel Corporation, molecular weight 530, hydroxyl value 212.4mg / g), 200g of toluene and 95.8g of triethylamine were added to a 1-liter glass flask equipped with a stirrer, a dropping funnel, a thermometer and a cooling tube, and the mixture was mixed at a temperature of 55°C. 168.9g of undecenoic acid chloride (an amount to be added so that 1.1 chlorine units of the acid chloride are added per hydroxyl group of poly-ε-caprolactone diol) was added dropwise from a dropping funnel, and the mixture was aged for 2 hours after the dropping. After the aging, 200g of water and 100g of toluene were added, and the aqueous phase was transferred to a separatory funnel and extracted with 100g of toluene. After extraction, the oil phase was washed once with 450 g of water and twice with 450 g of saturated saline, and then 10 g each of magnesium sulfate, activated carbon, and Kyoward 700 (Kyowa Chemical Industry Co., Ltd.) were added and shaken for 2 hours. After shaking, magnesium sulfate, activated carbon, and Kyoward 700 were removed by pressure filtration, and the solvent was distilled off at 60°C and 10 mmHg or less to obtain alkenyl group-containing poly-ε-caprolactone 1 (the following formula (7)). [ka] (R 6 indicates an aliphatic group, 2≦m+n≦5, weight average molecular weight: 862)

[0069] [Preparation of rubber particles] The above-mentioned alkenyl group-containing poly-ε-caprolactone 1 was mixed with 171 g of a 100 g aliquot of poly-ε-caprolactone having a kinetic viscosity of 23 mm 2 83.46g of phenylhydrogenpolysiloxane of 1.0% by weight per vinyl group (amount of hydrosilyl group per vinyl group) was charged into a 1L container and dissolved by stirring at 1500 rpm using a homomixer. Next, 1.35g of polyoxyethylene lauryl ether and 31.5g of water were added, and the mixture was stirred at 5000 rpm using a homomixer, resulting in an O / W type emulsion and thickening, and stirring was continued for another 10 minutes. Next, the mixture was diluted with 258.54g of water while stirring at 1500 rpm to obtain a white emulsion. [ka]

[0070] This emulsion was transferred to a 1L glass flask equipped with an anchor-type stirring blade stirrer, and after adjusting the temperature to 15-20°C, a mixed solution of 1g of an isododecane solution of platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 0.68g of polyoxyethylene lauryl ether was added dropwise under stirring, and stirred for 30 minutes to 1 hour.The temperature was then adjusted to 40°C and stirred for 2 days to obtain an aqueous dispersion of rubber particles.

[0071] The shape of the rubber particles in the resulting aqueous dispersion was observed with an optical microscope and found to be spherical. The volume average particle size was measured using an electrical resistance particle size distribution measuring device (Multisizer 3, Beckman Coulter, Inc.) and was found to be 5 μm.

[0072] The water from the obtained aqueous dispersion of rubber particles was dried using a spray dryer set at an inlet temperature of 150° C. and an outlet temperature of 80° C., yielding white to pale yellow powder-like rubber particles.

[0073] The hardness of the rubber constituting the rubber particles was measured as follows. The alkenyl group-containing poly-ε-caprolactone 1, the phenylhydrogenpolysiloxane represented by the above formula (8), and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above ratio and poured into an aluminum petri dish to a thickness of 10 mm. After leaving it at 40°C for 2 days, a flat rubber with no stickiness (tack) was obtained. The hardness was measured with an Asker C hardness tester and was found to be 63. EXAMPLES

[0074] [Preparation of composite particles] An aqueous dispersion of rubber particles was obtained in the same manner as in Example 1. 357 g of the obtained aqueous dispersion of rubber particles was transferred to a 2 L glass flask equipped with a stirrer using an anchor-shaped stirring blade, and 602.5 g of water, 19 g of a 28% aqueous ammonia solution, and 1 g of a 40% aqueous dimethyl diallyl ammonium chloride polymer solution (product name: ME Polymer H40W, manufactured by Toho Chemical Industry Co., Ltd.) were added. The pH of the liquid at this time was 11.3. After adjusting the temperature to 5 to 10°C, 20.5 g of methyltrimethoxysilane (an amount such that polymethylsilsesquioxane after hydrolysis and condensation reaction is 6.7 parts by mass per 100 parts by mass of rubber particles) was dropped over 25 minutes, the liquid temperature during this period was kept at 5 to 10°C, and stirring was continued for another hour. Next, the mixture was heated to 55 to 60°C, and stirring was continued for 1 hour while maintaining the temperature, completing the hydrolysis and condensation reaction of methyltrimethoxysilane.

[0075] The liquid obtained by hydrolysis and condensation reaction of methyltrimethoxysilane in an aqueous dispersion of rubber particles was dehydrated to about 30% water using a pressure filter. The dehydrated product was transferred to a 2L glass flask equipped with an anchor-shaped stirring blade stirrer, 1000g of water was added, and the mixture was stirred for 30 minutes, after which it was dehydrated using a pressure filter. The dehydrated product was again transferred to a 2L glass flask equipped with an anchor-shaped stirring blade stirrer, 1000g of water was added, and the mixture was stirred for 30 minutes, after which it was dehydrated using a pressure filter. The dehydrated product was dried at 105°C in a hot air flow dryer, and the dried product was crushed using a jet mill to obtain particles with flowability.

[0076] When the obtained particles were observed under an electron microscope, it was confirmed that the rubber particles were composite particles (polyorganosilsesquioxane-coated rubber particles) in which the entire surface was coated with granular polyorganosilsesquioxane.

[0077] The obtained composite particles were dispersed in water using a surfactant and measured using an electrical resistance particle size distribution measuring device (Multisizer 3, Beckman Coulter, Inc.). The particle size distribution was found to be equivalent to that of the above-mentioned water dispersion of rubber particles, and the volume average particle size was 5 μm. EXAMPLES

[0078] An aqueous dispersion of rubber particles was obtained in the same manner as in Example 1. 265 g of the obtained aqueous dispersion of rubber particles was transferred to a 2 L glass flask equipped with an anchor-shaped stirring blade stirrer, and 651.1 g of water, 2.2 g of a 2.8% aqueous ammonia solution, and 12 g of a 30% aqueous solution of lauryl trimethyl ammonium chloride (trade name: Cation BB, manufactured by NOF Corp.) (an amount such that lauryl trimethyl ammonium chloride was 0.44 parts per 100 parts by mass of water) were added. The pH at this time was 10.4. After adjusting the temperature to 5 to 10°C, 70.7 g of tetramethoxysilane (an amount such that silica after hydrolysis and condensation reaction was 27 parts by mass per 100 parts by mass of rubber particles) was dropped over 60 minutes, and the liquid temperature during this time was kept at 5 to 10°C, and stirring was continued for another 3 hours. Next, the mixture was heated to 70 to 75°C, and stirring was continued for 1 hour while maintaining that temperature, completing the hydrolysis and condensation reaction of tetramethoxysilane.

[0079] The obtained composite particles were dispersed in water using a surfactant and measured using an electrical resistance particle size distribution analyzer (Multisizer 3, Beckman Coulter, Inc.). The particle size distribution was the same as that of the water dispersion of rubber particles, and the volume average particle size was 5 μm. When the particles were observed under an electron microscope, it was confirmed that the rubber particle surfaces were coated with granular silica to form composite particles. EXAMPLES

[0080] [Synthesis of alkenyl-containing poly-ε-caprolactone 2] In Example 1, 200 g of poly-ε-caprolactone tetraol (product name: PLACCEL 410, Daicel Corporation, molecular weight 1030, hydroxyl value 216.7 mg / g) was used instead of 200 g of poly-ε-caprolactone diol (product name: PLACCEL 205U, Daicel Corporation), and the amount of triethylamine was changed from 95.8 g to 98.4 g, and the amount of undecenoic acid chloride was changed from 168.9 g to 173.5 g (an amount of acid chloride added so that 1.1 units per hydroxyl group) in Example 1. Synthesis was performed in the same manner as in Example 1, and an alkenyl group-containing poly-ε-caprolactone 2 (weight average molecular weight: 1698) was obtained. [ka] (R 9 indicates an aliphatic group, 4≦k+l+m+n≦9, weight average molecular weight: 1698)

[0081] [Preparation of rubber particles] In Example 1, the synthesized alkenyl group-containing poly-ε-caprolactone 1 was replaced with 171 g of alkenyl group-containing poly-ε-caprolactone 2, and the kinematic viscosity of the compound represented by the above formula (8) was 23 mm 2 A water dispersion of rubber particles was obtained in the same manner as in Example 1, except that 85.32 g of phenylhydrogenpolysiloxane having a molecular weight of 1.1 / s (a compounding amount such that the number of hydrosilyl groups per vinyl group was 1.1) was used. When the shape of the rubber particles in the obtained water dispersion was observed with an optical microscope, they were found to be spherical, and when the volume average particle size was measured using an electrical resistance method particle size distribution measuring device (Multisizer 3, manufactured by Beckman Coulter, Inc.), the volume average particle size was found to be 5 μm. When the water was removed from this water dispersion using a spray dryer in the same manner as in Example 1, a white to pale yellow powder was obtained. In addition, when the hardness of the rubber constituting the rubber particles was measured in the same manner as in Example 1, the hardness of this rubber was found to be 82. EXAMPLES

[0082] Composite particles coated with polyorganosilsesquioxane were obtained from the aqueous dispersion of rubber particles obtained in Example 4 in the same manner as in Example 2. The composite particles obtained were dispersed in water using a surfactant, and the particle size distribution was measured using an electrical resistance particle size distribution measuring device (Multisizer 3, manufactured by Beckman Coulter, Inc.). The particle size distribution was the same as that of the aqueous dispersion of rubber particles, and the volume average particle size was 5 μm. EXAMPLES

[0083] Silica-coated composite particles were obtained in the same manner as in Example 3 using the aqueous dispersion of rubber particles obtained in Example 4. The composite particles obtained were dispersed in water using a surfactant, and measured using an electrical resistance particle size distribution measuring device (Multisizer 3, manufactured by Beckman Coulter, Inc.). The particle size distribution was equivalent to that of the aqueous dispersion of rubber particles, and the volume average particle size was 5 μm. When the particles were observed under an electron microscope, it was confirmed that the surfaces of the rubber particles were coated with granular silica to form composite particles.

[0084] [Comparative Example 1] [Making flat silicone rubber] The kinetic viscosity, as shown in the following formula (10), is 600 mm 2 25 g of methylvinylpolysiloxane having a viscosity of 27 mm3 / s and 2 1 g of methylhydrogenpolysiloxane of 100 mL / s (amount of compounding such that 1.1 hydrosilyl groups are mixed per vinyl group) was placed in a 100 mL container and stirred to dissolve. Next, 0.06 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) was added and stirred, poured into an aluminum petri dish to a thickness of 10 mm, and left at 40° C. for 2 days to produce a flat rubber of a rubber composition of silicone particles. The hardness of the rubber was measured in the same manner as in Example 1, and the hardness of this rubber was 60. [ka]

[0085] [Evaluation of rubber hydrolysis (measurement of flat rubber hardness over time)] The hydrolysis properties of the flat rubber (rubber hardness: 63) composed of the alkenyl group-containing poly-ε-caprolactone 1 and the phenylhydrogenpolysiloxane shown in formula (8) obtained in Example 1, the flat rubber (rubber hardness: 82) composed of the alkenyl group-containing poly-ε-caprolactone 2 and the phenylhydrogenpolysiloxane shown in formula (8) obtained in Example 4, and the flat rubber (rubber hardness: 60) composed of the methylvinylpolysiloxane shown in formula (10) and the methylhydrogenpolysiloxane shown in formula (11) obtained in Comparative Example 1 were evaluated by the following method. The three flat rubber samples were placed in a thermohygrostat (IW222 model, Yamato Scientific Co., Ltd.) at a temperature of 70° C. and a humidity of 90%, and the change in rubber hardness was measured on a daily basis. In addition, the flat rubber (rubber hardness: 63) obtained in Example 1 was left standing in a dryer (DNE601 type, manufactured by Yamato Scientific Co., Ltd.) at 70°C and in an environment of room temperature and humidity of 65% (assuming the usage environment), and the change in rubber hardness was measured on a daily basis.

[0086] [Table 1]

[0087] The flat rubber samples of Examples 1 and 4 that were left in the thermo-hygrostat had a structure crosslinked by poly-ε-caprolactone having an alkenyl group and organohydrogenpolysiloxane having a hydrogen atom bonded to a silicon atom in the presence of a hydrosilylation catalyst, and the rubber hardness decreased in a high-temperature and high-humidity environment of a temperature of 70°C and a humidity of 90%, so it is presumed to be degradable. On the other hand, the flat rubber sample of Comparative Example 1 does not use a component that has a hydrolyzable functional group such as polyester as a rubber component, and the rubber hardness is constant even in a high-temperature and high-humidity environment, so it is presumed not to be degradable. The flat rubber sample of Example 1 that was left in the 70°C dryer was confirmed to have an increase in rubber hardness, which is presumed to be due to a slight hardening due to the heat, but since there was no decrease in rubber hardness, it is presumed that decomposition does not occur unless moisture is present. The flat rubber sample of Comparative Example 1 was confirmed to have an increase in rubber hardness, which is presumed to be due to a slight hardening due to the heat, but since there was no decrease in rubber hardness, it is presumed that decomposition does not occur unless moisture is present. The flat rubber sample of Comparative Example 1 was confirmed to have an increase in rubber hardness, which is presumed to be due to a slight hardening due to the heat, and ... 5 % environment did not experience any decrease in rubber hardness over the 95-day measurement period, and therefore it is assumed that the flat rubber sample was stable in the actual usage environment during this measurement period.

Claims

1. (A) a polyester having at least two aliphatic unsaturated groups in one molecule, in which the terminal hydroxyl groups of the molecular chain of a poly-ε-caprolactone polyol are substituted with aliphatic unsaturated groups; and (B) Organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in each molecule wherein the component (A) has two aliphatic unsaturated groups per molecule and the component (B) has two hydrogen atoms bonded to silicon atoms per molecule, and the rubber particles have a spherical particle shape and a volume average particle size of 0.1 to 50 μm.

2. The component (B) is represented by the following general formula (1): 【Chemistry 1】 (R 1 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms; R 2 are each independently a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms, 1≦m≦1000, 0≦n≦1000, provided that when n=0, two R 2 are both hydrogen atoms, and the two R 2 and n is an integer of 0 to 10, and n is an integer of 0 to 10.

3. The component (B) is represented by the following general formula (2): 【Chemistry 2】 (R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms, excluding a phenyl group, and 0≦a≦500, 1≦b≦1000, 1≦a+b≦1000, and 0≦c≦1000, provided that when c=0, two R 2 are both hydrogen atoms, and the two R 2 and c is 2 or more when neither of them is a hydrogen atom.

4. A composite particle comprising the rubber particle according to any one of claims 1 to 3, the surface of which is coated with polyorganosilsesquioxane or silica.

5. A method for producing the rubber particles according to any one of claims 1 to 3, comprising the following steps (i) to (iii): (i) A step of adding a surfactant-containing aqueous phase component to an oil phase component composed of a polyester (A) having at least two aliphatic unsaturated groups in one molecule, in which the terminal hydroxyl groups of the molecular chain of a poly-ε-caprolactone polyol are substituted with aliphatic unsaturated groups, and an organohydrogenpolysiloxane (B) having at least two silicon-bonded hydrogen atoms in one molecule, and emulsifying the mixture to obtain an O / W type emulsion. (ii) A step of curing the oil phase component consisting of the components (A) and (B) in the emulsion by a hydrosilylation reaction in the presence of a hydrosilylation-reactive catalyst to obtain an aqueous dispersion of rubber particles (C). (iii) A step of obtaining rubber particles by drying and removing the water, which is the continuous phase, from the aqueous dispersion (C) of rubber particles obtained in the step (ii).

6. A method for producing the composite particle according to claim 4, comprising the following steps (i) to (v): (i) A step of adding an aqueous phase component containing a surfactant to an oil phase component composed of a polyester (A) having at least two aliphatic unsaturated groups in one molecule, in which the terminal hydroxyl groups of the molecular chain of a poly-ε-caprolactone polyol are substituted with aliphatic unsaturated groups, and an organohydrogenpolysiloxane (B) having at least two hydrogen atoms bonded to silicon atoms in one molecule, and stirring the mixture to obtain an O / W type emulsion. (ii) A step of curing the oil phase component consisting of the components (A) and (B) in the emulsion by a hydrosilylation reaction in the presence of a hydrosilylation-reactive catalyst to obtain an aqueous dispersion of rubber particles (C). (iii') A step of adding an alkaline substance (E) to the aqueous dispersion (C) of rubber particles obtained in the step (ii). (iv) The aqueous dispersion of rubber particles to which the alkaline substance obtained in the step (iii′) has been added is treated with a compound represented by the following general formula (3): 【Chemistry 3】 (R 4 is a monovalent hydrocarbon group having 1 to 6 carbon atoms, R 5 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms or -OR 4 ) and carrying out a condensation reaction to coat the surfaces of the rubber particles with polyorganosilsesquioxane or silica, thereby obtaining an aqueous dispersion of composite particles. (v) A step of obtaining composite particles by drying and removing the water, which is the continuous phase, from the aqueous dispersion of the composite particles obtained in the step (iv).

Citation Information

Patent Citations

  • Curable resin composition

    JP1991277645A

  • Silicone rubber powdery article and production thereof

    JP1992348143A

  • Fine silicone particle and its production

    JP1995196815A

  • Production of thermoplastic elastomer

    JP1996073664A

  • Powder coating material using new polyester curable composition

    JP1996209037A