Resin composition

The resin composition with sulfur-containing aromatic polymers coats metal oxide particles to prevent agglomeration, enhancing refractive index and transparency, addressing moldability issues in conventional materials.

JP7570865B2Active Publication Date: 2024-10-22NIPPON SHOKUBAI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020160171
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-24
Publication Date
2024-10-22
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Conventional molding materials with metal oxide particles suffer from poor moldability and reduced transparency due to particle agglomeration, limiting their use in applications requiring high refractive index and low light dispersion.

Method used

A resin composition containing metal oxide particles coated with a polymeric material and a binder resin, where the polymeric material or binder resin includes sulfur-containing aromatic polymers, suppressing particle agglomeration and enhancing refractive index.

Benefits of technology

The resin composition achieves high refractive index and excellent transparency, suitable for optical applications by preventing particle agglomeration and ensuring uniform compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570865000012
    Figure 0007570865000012
  • Figure 0007570865000013
    Figure 0007570865000013
  • Figure 0007570865000001
    Figure 0007570865000001
Patent Text Reader

Abstract

To provide a resin composition which has a high refractive index ratio, is excellent in suppression of aggregation of metal oxide particles, and can be formed into a new optical material.SOLUTION: A resin composition contains metal oxide particles coated with a polymer material, and a binder resin, in which the polymer material and / or the binder resin contains a divalent aromatic hydrocarbon group that may have a substituent, contains a polymer having at least one structural unit selected from the group consisting of a structural unit (A) of -S-, a structural unit (B) of -S(=O)- and a structural unit (C) of -S(=O)2-, and has an element content ratio (O / S) of an oxygen atom O bonded to a sulfur atom S in a main chain to the sulfur atom S in the main chain of 0.1-1.5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, more specifically to a resin composition that has a high refractive index and is excellent in inhibiting aggregation of metal oxide particles. [Background technology]

[0002] Polycarbonate with aromatic rings and polymeric materials with fluorene skeletons are known as high refractive index materials. Refractive index adjustment materials that improve the light extraction efficiency of LEDs and lens materials for imaging systems require materials with large Abbe numbers, i.e., small light dispersion. Materials with sulfur or halogen molecules and materials containing metal oxide nanoparticles have been developed as such materials with high refractive index and small light dispersion.

[0003] Various studies have been conducted on sulfur-containing polymeric materials that have a high refractive index and small optical dispersion. For example, Patent Document 1 describes a molding material having a polyarylene sulfide skeleton in which two hydrogen atoms in the benzene ring are substituted with methyl groups, as a molding material that has excellent moldability in a solution state and can be used as an optical component. Furthermore, for example, Patent Document 2 describes a molding material having a polyarylene sulfide skeleton in which one hydrogen atom of the benzene ring is substituted with a methyl group, as a molding material that has excellent moldability in a solution state and is capable of forming an optical component having a high refractive index exceeding 1.70. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-168790 A [Patent Document 2] JP 2017-52834 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional molding materials do not have sufficiently high refractive index or visible light transparency, and there is still room for improvement. In addition, in recent years, there has been a demand for polymer materials that can be used in a wide range of applications, such as optical applications, by having properties such as high transparency and low linear expansion coefficient as well as high refractive index. In order to achieve a high refractive index, a method of adding metal oxide particles with a high refractive index is known, but when such particles are added to conventional molding materials, there are problems such as the above particles agglomerating, which reduces the handleability of the molding material and reduces the transparency of the molded product.

[0006] In view of the above-mentioned current situation, an object of the present invention is to provide a resin composition which has a high refractive index and excellent inhibition of aggregation of metal oxide particles, and which can become a new optical material. [Means for solving the problem]

[0007] The present inventors have conducted extensive research into sulfur-containing molding materials and have found that a composition containing metal oxide particles coated with a polymeric material and a binder resin, and that at least the polymeric material or the binder resin contains a sulfur-containing aromatic polymer, has an extremely high refractive index and is excellent in suppressing the aggregation of metal oxide particles, and that the composition is useful as an optical material, thereby completing the present invention.

[0008] That is, the present invention is a resin composition comprising metal oxide particles coated with a polymeric material and a binder resin, wherein the polymeric material and / or the binder resin comprises a polymer having at least one structural unit selected from the group consisting of a structural unit (A) represented by the following general formula (1), a structural unit (B) represented by the following general formula (2), and a structural unit (C) represented by the following general formula (3).

[0009] [ka]

[0010] (In the above general formulas (1) to (3), X 1 , X 2 and X 3 are the same or different and each represents a divalent aromatic hydrocarbon group which may have a substituent.

[0011] It is preferred that the structural unit (A) is a structural unit (A-1) represented by the following general formula (1-1), the structural unit (B) is a structural unit (B-1) represented by the following general formula (2-1), and the structural unit (C) is a structural unit (C-1) represented by the following general formula (3-1).

[0012] [ka]

[0013] (In formulas (1-1), (2-1) and (3-1), R 1 , R 2 and R 3 are the same or different and each represents a halogen atom, a hydroxyl group, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. 1 represents the number of, and is an integer from 0 to 4. b is R 2 represents the number of, and is an integer from 0 to 4. c represents R 3 It represents the number of and is an integer between 0 and 4.)

[0014] In the above polymer, the elemental content ratio (O / S) of oxygen atoms O bonded to sulfur atoms S in the main chain to sulfur atoms S in the main chain is preferably 0.1 to 1.5.

[0015] The resin composition preferably further contains a compound having a (poly)styrene skeleton.

[0016] In the resin composition, the compound having a (poly)styrene skeleton and the metal oxide particles are preferably covalently bonded to each other.

[0017] The resin composition is preferably for optical use. Effect of the Invention

[0018] According to the present invention, it is possible to provide a resin composition having a high refractive index and excellent inhibition of aggregation of metal oxide particles. The resin composition of the present invention can be suitably used for optical applications such as imaging lens materials. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 shows measurement data of the transmittance of the blend film obtained in Example 1. [Diagram 2] 1 is a photograph of the blend film obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.

[0021] resin composition The resin composition of the present invention is a resin composition comprising metal oxide particles coated with a polymeric material and a binder resin, wherein the polymeric material and / or the binder resin comprises a polymer having at least one structural unit selected from the group consisting of a structural unit (A) represented by the following general formula (1), a structural unit (B) represented by the following general formula (2), and a structural unit (C) represented by the following general formula (3).

[0022] [ka] (In formulas (1) to (3), X 1 , X 2 and X 3 are the same or different and each represents a divalent aromatic hydrocarbon group which may have a substituent.

[0023] The resin composition of the present invention has a high refractive index and is excellent in suppressing aggregation of metal oxide particles. It is presumed that the resin composition of the present invention has such properties because the metal oxide particles and the polymer material are uniformly compatible with each other, thereby suppressing aggregation of the particles.

[0024] The resin composition of the present invention contains metal oxide particles coated with a polymeric material and a binder resin. In the resin composition, at least one of the polymeric material and the binder resin contains a polymer having at least one structural unit selected from the group consisting of the structural units (A), (B) and (C). The polymer will be described first.

[0025] <Polymer> In the present invention, the polymer used as the polymer material and / or binder resin includes a polymer (hereinafter also referred to as "polymer (X)") having at least one structural unit selected from the group consisting of the structural unit (A) represented by the above general formula (1), the structural unit (B) represented by the above general formula (2), and the structural unit (C) represented by the above general formula (3).

[0026] In the above general formulas (1), (2) and (3), X 1 , X 2 and X 3 are the same or different and each represents a divalent aromatic hydrocarbon group which may have a substituent. Examples of the divalent aromatic hydrocarbon group include a phenylene group, a naphthylene group, an anthrylene group, a triphenylene group, a biphenylene group, a phenanthrylene group, etc. Among these, in terms of reducing light dispersion, the divalent aromatic hydrocarbon group is preferably a phenylene group, a naphthylene group, an anthrylene group, a biphenylene group, or a triphenylene group, and more preferably a phenylene group.

[0027] The substituent (also referred to as "substituent A") of the divalent aromatic hydrocarbon group is preferably a halogen atom, a hydroxyl group, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, which may have a substituent (also referred to as "substituent B").

[0028] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a bromine atom being preferred among these.

[0029] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a hexyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a heptyl group, etc. Among these, an alkyl group having 1 to 18 carbon atoms is preferred, an alkyl group having 1 to 6 carbon atoms is more preferred, and a methyl group is even more preferred.

[0030] Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an s-butoxy group, a t-butoxy group, a pentyloxy group, a phenoxy group, a cyclohexyloxy group, a benzyloxy group, etc. Among these, an alkoxy group having 1 to 18 carbon atoms is preferred, an alkoxy group having 1 to 6 carbon atoms is more preferred, and a methoxy group is more preferred.

[0031] Examples of the aryl group include a phenyl group, a naphthyl group, an anthryl group, a biphenyl group, and a triphenyl group. Of these, a phenyl group is preferable. The number of carbon atoms in the aryl group is preferably 6 to 30, more preferably 6 to 18, and further preferably 6 to 12.

[0032] Examples of the aralkyl group include a benzyl group, a phenethyl group, a phenylpropyl group, a phenylpentyl group, a phenylhexyl group, a phenyloctyl group, etc. The aralkyl group preferably has 7 to 14 carbon atoms, and more preferably has 7 to 9 carbon atoms.

[0033] Examples of the sulfur-containing substituent include a thioalkyl group and a thioaryl group. Among them, a thioalkyl group is preferable. The number of carbon atoms of the sulfur-containing substituent is preferably 1 to 8, more preferably 1 to 6, and further preferably 1 to 4.

[0034] The above alkyl group, alkoxy group, aryl group, aralkyl group, and sulfur-containing substituent may further have a substituent (substituent B). Examples of the substituent (substituent B) include an alkyl group, a halogen atom, and a hydroxyl group. Among these, from the viewpoint of the solubility of the polymer material, an alkyl group is preferred, and from the viewpoint of the dispersibility of the metal oxide particles, a halogen atom and a hydroxyl group are preferred.

[0035] Among these, in terms of being able to further increase the refractive index of the resin composition, the substituent (substituent A) on the divalent aromatic hydrocarbon group is more preferably an alkyl group having 1 to 18 carbon atoms or a sulfur-containing substituent, further preferably a methyl group or a thioalkyl group, and particularly preferably a methyl group. In addition, from the viewpoint of improving the dispersibility of metal oxide particles, the substituent (substituent A) of the divalent aromatic hydrocarbon group is preferably a hydroxyl group or a sulfur-containing substituent, more preferably a hydroxyl group, a thioalkyl group or a thioaryl group, and particularly preferably a hydroxyl group.

[0036] The number of the substituents A in the divalent aromatic hydrocarbon group is not particularly limited, but in order to further increase the refractive index of the polymer material, a smaller number is preferable. Specifically, the number is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1.

[0037] The above structural unit (A) is preferably a structural unit (A-1) represented by the following general formula (1-1).

[0038] [ka]

[0039] (In the formula, R 1 are the same or different and each represents a halogen atom, a hydroxyl group, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. 1 It represents the number of and is an integer between 0 and 4.)

[0040] The above structural unit (B) is preferably a structural unit (B-1) represented by the following general formula (2-1).

[0041] [ka]

[0042] (In the formula, R 2 are the same or different and each represents a halogen atom, a hydroxyl group, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. 2 It represents the number of and is an integer between 0 and 4.)

[0043] The above structural unit (C) is preferably a structural unit (C-1) represented by the following general formula (3-1).

[0044] [ka]

[0045] (In the formula, R 3 are the same or different and each represents a halogen atom, a hydroxyl group, an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. 3 It represents the number of and is an integer between 0 and 4.)

[0046] Above R 1 , R 2 and R 3Examples of the alkyl group, alkoxy group, aryl group, aralkyl group, and sulfur-containing substituent, which may have a substituent, are represented by the following general formula (1): X 1 Preferred examples of the alkyl group, alkoxy group, aryl group, aralkyl group, and sulfur-containing substituent are the same as those described above. Preferred examples of the substituent that these groups may have include the same groups as the substituent B described above. Above R 1 , R 2 and R 3 When there are a plurality of each of them, they may be the same or different.

[0047] a, b, c are R 1 , R 2 , R 3 It represents the number of substituents, and is an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably an integer of 0 to 2.

[0048] The polymer (X) may be an alternating copolymer of the structural units (A), (B) and (C), or may be a block copolymer or a random copolymer. The polymeric material may have one or more of the above structural units (A), (B), or (C).

[0049] The polymer (X) may be in a form containing only one of the structural units (A), (B) and (C), or may be in a form containing two structural units, or may be in a form containing three structural units. These forms and their content ratios can be appropriately selected depending on the purpose and use of the resin composition. For example, the polymer (X) preferably contains the structural unit (A) above, and more preferably contains this as a main component, in that this can result in a higher refractive index. In addition, the polymer (X) preferably contains the structural unit (B) above, and more preferably contains this as a main component, in that this allows for both solubility and a high refractive index to be achieved. In addition, the polymer (X) preferably contains the structural unit (C) above, and more preferably contains this as a main component, in that transparency and a high refractive index can be achieved at the same time.

[0050] In view of the above, in terms of a high refractive index, the content of the structural unit (A) in the polymer (X) is preferably 1 to 100 mol %, more preferably 10 to 100 mol %, and even more preferably 50 to 100 mol %, relative to 100 mol % of all structural units of the polymer. In this case, the total content of the structural units (B) and (C) is preferably 0 to 99 mol%, more preferably 0 to 90 mol%, and even more preferably 0 to 50 mol%, relative to 100 mol% of all structural units.

[0051] In the above polymer (X), from the viewpoint of high polarity resulting from solubility, the content of the above structural unit (B) is preferably 1 to 100 mol %, more preferably 10 to 100 mol %, and even more preferably 50 to 100 mol %, relative to 100 mol % of all structural units of the polymer. In this case, the total content of the structural units (A) and (C) is preferably 0 to 99 mol%, more preferably 0 to 90 mol%, and even more preferably 0 to 50 mol%, relative to 100 mol% of all structural units.

[0052] In the above polymer (X), the content of the above structural unit (C) is preferably 1 to 100 mol %, more preferably 10 to 100 mol %, and even more preferably 50 to 100 mol %, relative to 100 mol % of all structural units of the polymer, from the viewpoint of high transparency. In this case, the total content of the structural units (A) and (B) is preferably 0 to 99 mol%, more preferably 0 to 90 mol%, and even more preferably 0 to 50 mol%, relative to 100 mol% of all structural units.

[0053] In the above polymer (X), the total content of the above structural units (A), (B) and (C) is preferably 50 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, even more preferably 95 mol% or more, and particularly preferably 100 mol%, based on 100 mol% of all structural units in the polymer (X).

[0054] The above polymer (X) may also have a structural unit (D) other than the above structural unit (A), structural unit (B) and structural unit (C). Examples of the structural unit (D) include structural units derived from the following monomers. Carboxyl group-containing (meth)acrylates such as 2-carboxyethyl (meth)acrylate, 2-carboxypropyl (meth)acrylate, 3-carboxypropyl (meth)acrylate, and 4-carboxybutyl (meth)acrylate; phosphate group-containing (meth)acrylates such as 2-(meth)acryloyloxyethyl acid phosphate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and 3,4-epoxycyclohexylmethyl (meth)acrylate; vinyl ether group-containing (meth)acrylates such as 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, and the like.

[0055] The content of the structural unit (D) is preferably 0 to 80 mol%, more preferably 0 to 50 mol%, even more preferably 0 to 20 mol%, even more preferably 0 to 10 mol%, and particularly preferably 0 to 5 mol%, relative to 100 mol% of all structural units in the polymer (X).

[0056] The polymer (X) preferably has an element ratio (O / S) of oxygen atoms O bonded to sulfur atoms S in the main chain to sulfur atoms S in the main chain of 0.1 to 1.5. When the element ratio is within the above range, the transparency and refractive index become higher. Specifically, the sulfur atom S in the main chain means, for example, the sulfur atom S of -S- in the main chain in the structural unit (A) represented by the above general formula (1), the sulfur atom S of -SO- in the main chain in the structural unit (B) represented by the above general formula (2), and the sulfur atom S of -SO2- in the main chain in the structural unit (C) represented by the above general formula (3). The oxygen atom bonded to the sulfur atom S in the main chain specifically means, for example, the oxygen atom O of -SO- in the main chain in the structural unit (B) represented by the above general formula (2), and means the oxygen atom O of -SO2- in the main chain in the structural unit (C) represented by the above general formula (3).

[0057] The element content ratio (O / S) is more preferably 0.3 or more, and even more preferably 0.7 or more, in order to further increase the transparency, and is more preferably 1.3 or less, and even more preferably 1.1 or less, in order to further increase the refractive index. The above elemental content ratios can be determined by evaluating and measuring the peak intensities of the oxygen 1s orbital (O1s), carbon 1s orbital (C1s), and sulfur 2p orbital (S2p) using an X-ray photoelectron spectrometer (XPS).

[0058] The polymer (X) preferably has a glass transition temperature (Tg) of 80 to 250° C. When the glass transition temperature is in the above range, molding can be easily performed. From the viewpoint of increasing heat resistance, the glass transition temperature is more preferably 90° C. or higher, and even more preferably 100° C. or higher, and from the viewpoint of easy molding, it is more preferably 200° C. or lower. The glass transition temperature can be determined by a method in which a differential scanning calorimeter (DSC) is used to measure a temperature rise from room temperature to 250°C (heating rate: 10°C / min) in a nitrogen gas atmosphere, and the DSC curve is obtained by evaluating the intersection point of the tangent line at the baseline and the inflection point.

[0059] The polymer (X) preferably has a SO bond energy of 163 eV to 167 eV. When the SO bond energy is within the above range, the refractive index and transparency can be further increased. The SO bond energy can be determined by evaluating the peak top position of the 2p3 / 2 orbital of a sulfur atom obtained by measurement using X-ray photoelectron spectroscopy (XPS).

[0060] The weight average molecular weight (Mw) of the polymer (X) is preferably 500 to 10,000,000. When the weight average molecular weight is within the above range, it can be suitably used as an optical material. From the viewpoint of improving mechanical properties, the weight average molecular weight is more preferably 1,000 or more, even more preferably 3,000 or more, and even more preferably 10,000 or more, and from the viewpoint of reducing melt viscosity, it is more preferably 1,000,000 or less, and even more preferably 100,000 or less.

[0061] The polymer (X) preferably has a polydispersity (weight average molecular weight / number average molecular weight) of 1 to 10. When the polydispersity is within the above range, molding becomes easy. In terms of further improving moldability, the polydispersity is more preferably 5 or less, and even more preferably 3 or less.

[0062] The weight average molecular weight and number average molecular weight can be determined by gel permeation chromatography (GPC), specifically, by the method described in the Examples below. The dispersity can be determined by dividing the weight average molecular weight by the number average molecular weight.

[0063] The refractive index of the polymer (X) is preferably 1.69 or more. When the refractive index is within the above range, the polymer can be suitably used for various applications such as optical materials (members), machine part materials, electric and electronic part materials, automobile part materials, civil engineering and construction materials, molding materials, etc., as well as paints and adhesive materials. The refractive index is more preferably 1.7 or more, and even more preferably 1.71 or more. The refractive index can be determined by forming a film having a thickness of 50 nm from the polymer as a measurement sample and measuring the film using a spectroscopic ellipsometer UVISEL (manufactured by HORIBA Scientific) with Na D line (589 nm).

[0064] The Abbe number of the polymer (X) is preferably 10 or more. When the Abbe number is within the above range, the light dispersion is small, and the optical material can be suitable for lenses. The Abbe number is more preferably 15 or more, even more preferably 18 or more, and even more preferably 20 or more. From the viewpoint of adjusting the light dispersion, the Abbe number is preferably 60 or less, and more preferably 55 or less. The Abbe number can be calculated in the same manner as the refractive index by forming a film using the polymer and measuring the refractive indices at D line (589.3 nm), F line (486.1 nm), and C line (656.3 nm) using the spectroscopic ellipsometer, and then using the following calculation formula. Abbe number (v D )=(n D -1) / (n F -n C ) In the formula, n D , n F , n C represent the refractive indices at the Fraunhofer D line (589.3 nm), F line (486.1 nm), and C line (658.3 nm), respectively.

[0065] The polymer (X) preferably has a visible light transmittance of 70% or more. When the visible light transmittance is within the above range, it can be suitably used as an optical material. The visible light transmittance is more preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more. The visible light transmittance is a parallel line transmittance, and can be determined by measuring the range of 400 nm to 700 nm in air without using an integrating sphere using a thin film of the polymer having a thickness of 0.02 mm, or by standardizing the thickness to 0.02 mm, with a spectrophotometer (for example, a JASCO V-700 series ultraviolet, visible, and infrared spectrophotometer) and evaluating the minimum transmittance.

[0066] The polymer (X) preferably has a linear expansion coefficient of 100 ppm / °C or less. When the linear expansion coefficient of the polymer is within the above range, the polymer becomes an optical material with a small temperature dependency of the refractive index, and can be suitably used for various applications such as optical materials, sealing materials, and coating materials. The linear expansion coefficient is more preferably 60 ppm / °C or less, and even more preferably 30 ppm / °C or less, in terms of further reducing the temperature dependency. The lower limit of the linear expansion coefficient is not particularly limited, but is preferably 1 ppm / °C or more, and even more preferably 3 ppm / °C or more. The linear expansion coefficient can be determined by measurement according to a method in accordance with JIS K 7197:2012.

[0067] The polymer (X) is preferably thermoplastic. When the polymer is thermoplastic, the binder resin made of the polymer is contained, so that the moldability is improved, such that a thin film can be uniformly formed and a complex shape can be formed with high accuracy, and the polymer can be easily applied to a wide range of uses.

[0068] (Method for producing polymer (X)) The method for producing the polymer (X) is not particularly limited as long as it is a method capable of producing a polymer having at least one of the above-mentioned structural units (A) to (C), and may be a known polymerization method such as polymerizing a monomer component containing a sulfur-containing monomer. In particular, in terms of being able to produce the polymer efficiently, the method for producing the polymer preferably includes a step (1) of polymerizing a monomer component containing a sulfur-containing monomer to obtain a sulfur-containing polymer, and a step (2) of oxidizing the sulfur-containing polymer using an oxidizing agent.

[0069] Process (1) In the step (1), the sulfur-containing monomer used is not particularly limited as long as it is a monomer containing a sulfur atom, but in the production method of the present invention, it is preferable to obtain a sulfur-containing polymer by oxidative polymerization of the sulfur-containing monomer. Preferred examples of the sulfur-containing monomer from which a sulfur-containing polymer can be obtained by oxidative polymerization include disulfide compounds and thiol compounds, and more specifically, for example, diaryl disulfide compounds represented by the following general formula (4) and thioaryl compounds represented by the following formula (5) are more preferred.

[0070] [ka]

[0071] In the above general formulas (4) and (5), A 1 and A 2 are the same or different and each represents a monovalent aromatic hydrocarbon group which may have a substituent. A 1 and A 2 Examples of the monovalent aromatic hydrocarbon group represented by the formula (1) include X 1 Examples of the divalent aromatic hydrocarbon group represented by the following formula (1) are monovalent groups, and include a phenyl group, a naphthyl group, an anthryl group, a triphenyl group, a biphenyl group, a phenanthryl group, etc. Among these, a phenyl group, a naphthyl group, an anthryl group, a biphenyl group, or a triphenyl group is preferable, and a phenyl group is more preferable.

[0072] A 1 and A 2 Examples of the substituent possessed by the monovalent aromatic hydrocarbon group represented by the formula (I) include a halogen atom, an alkyl group, an alkoxy group, an aryl group, an aralkyl group, a sulfur-containing substituent, etc. Examples of the halogen atom, the alkyl group, the alkoxy group, the aryl group, the aralkyl group, and the sulfur-containing substituent include the same groups as those described above.

[0073] The diaryl disulfide compound is preferably a compound represented by the following general formula (4-1). The above thioaryl compound is preferably a compound represented by the following general formula (5-1).

[0074] [ka]

[0075] (In formulas (4-1) and (5-1), R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 and R 11 are the same or different and each represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. The above halogen atom, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent which may have a substituent, is each represented by R 1 The groups are the same as those represented by the following formula: In addition, examples of the substituent that these groups may have include the same as the above-mentioned substituent B, and among these, a halogen atom and a hydroxyl group are preferable.

[0076] The disulfide compound can also be prepared by oxidation of a thiol compound. Therefore, in the polymerization step, a thiol compound can also be used as a precursor of the disulfide compound. The disulfide compound can be obtained by oxidatively bonding two molecules of a thiol compound.

[0077] The method for obtaining a disulfide compound by oxidizing a thiol compound is not particularly limited, and can be a known method such as a method of oxidation using hydrogen peroxide, iodine, or the like.

[0078] The sulfur-containing monomers may be used alone or in combination of two or more.

[0079] The polymerization is preferably oxidative polymerization. The oxidative polymerization is not particularly limited, and can be carried out by known methods such as a method using a quinone-based compound or a method using a metal compound such as a vanadium compound. Among them, the oxidative polymerization is preferably carried out using a quinone-based oxidizing agent, in terms of improving transparency. It is preferable to use a metal compound, in terms of the amount of use relative to the monomer component being small, resulting in less waste.

[0080] Examples of the quinone-based oxidizing agent include 2,3-dichloro-5,6-dicyano-parabenzoquinone (DDQ), 2,3,5,6-tetrachloroparabenzoquinone (chloranil), 2,3,5,6-tetrabromobenzoquinone (bromanil), 2,3,5,6-tetrafluoroparabenzoquinone, anthraquinone, 1,4-naphthoquinone, 2,3-dichloro-1,4-naphthoquinone, 2,3-dibromo-1,4-naphthoquinone, 2,3-dicyano-1,4-naphthoquinone, 3,4,5,6-tetrachloroorthobenzoquinone (orthochloranil), 3,4,5,6-tetrabromoorthobenzoquinone (orthobromanil), 3,4,5,6-tetrafluorobenzoquinone, etc. Among them, DDQ is preferred because of its high oxidizing power and easy availability. The quinone-based oxidizing agents may be used alone or in combination of two or more.

[0081] The amount of the quinone-based oxidizing agent added is preferably 0.1 to 3 mol, more preferably 0.8 to 1.5 mol, and even more preferably 0.9 to 1.1 mol, per mol of the sulfur-containing monomer used.

[0082] When the quinone-based oxidizing agent is used, an acid may be further added. When the quinone-based oxidizing agent acts on the quinone-based compound, the quinone-based compound becomes a dianion of hydroquinone, but when an acid is added, the dianion can be stabilized and the oxidizing power can be maintained.

[0083] The above-mentioned acid is not particularly limited, and examples thereof include sulfuric acid, acetic acid, methanesulfonic acid, benzenesulfonic acid, toluenesulfonic acid, trifluoromethanesulfonic acid, 1,1,2,2-tetrafluoroethanesulfonic acid, trifluoroacetic acid, perfluoropropionic acid, and perfluorobutyric acid. Among them, trifluoroacetic acid is preferable in terms of increasing the acidity. The above-mentioned acid may be used alone or in combination of two or more.

[0084] The amount of the acid added is preferably 10 to 1000 mol, more preferably 50 to 500 mol, and even more preferably 80 to 120 mol, relative to 100 mol of the total amount of the quinone-based oxidizing agent added.

[0085] The reaction temperature is not particularly limited as long as it is a temperature at which the polymerization proceeds, but from the viewpoint of facilitating the above-mentioned oxidative polymerization, it is preferably 0 to 200°C, more preferably 10°C or higher, and even more preferably 15°C or higher, and from the viewpoint of being able to suppress side reactions, it is more preferably 180°C or lower, and even more preferably 150°C or lower.

[0086] The reaction time is not particularly limited, but is usually 0.1 to 100 hours, preferably 1 to 80 hours, more preferably 5 to 50 hours, and further preferably 10 to 24 hours.

[0087] In the polymerization reaction, a solvent may be used. Preferred solvents include, for example, dichloromethane, chloroform, carbon tetrachloride, 1,2-dichloroethane, tetrachloroethylene, 1,1,2,2-tetrachloroethane, nitromethane, nitrobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, N-methylpyrrolidone, tetrahydrofuran, and ethyl acetate.

[0088] In the above polymerization reaction, the monomer components including the sulfur-containing monomer may be added successively during the polymerization reaction. Alternatively, the polymerization may be carried out in multiple stages, for example by oxidatively polymerizing the above-mentioned thiol compound to obtain a disulfide compound, and then oxidatively polymerizing the obtained disulfide compound.

[0089] Process (2) After the step (1), the sulfur-containing polymer is oxidized using an oxidizing agent. The oxidizing agent used is not particularly limited, and any known oxidizing agent can be used, such as a quinone compound, perbenzoic acid, metachloroperbenzoic acid, lead tetraacetate, thallium acetate, tetracyanoquinodimethane, tetracyanoethylene, cerium (IV) acetylacetonate, manganese (III) acetylacetonate, peroxide, or chloric acid.

[0090] Among them, to oxidize the sulfur atom (-S-) contained in the main chain to a sulfonyl (-SO2-), it is preferable to use a peroxide or chloric acid as an oxidizing agent, whereas to oxidize to a sulfinyl (-SO-), it is preferable to use a peroxide or chloric acid as an oxidizing agent.

[0091] Examples of the peroxide include metachloroperbenzoic acid, hydrogen peroxide, ammonium persulfate, sodium persulfate, peracetic acid, and t-butyl hydroperoxide. Among them, the oxidizing agent is preferably a peroxide, more preferably metachloroperbenzoic acid or hydrogen peroxide, in that it can be dissolved in the same solvent as the sulfur-containing polymer, and further preferably metachloroperbenzoic acid, in that water in which the polymer precipitates is not used and in that oxidation to sulfoxide by an excess of the oxidizing agent is suppressed.

[0092] The amount of the oxidizing agent to be added is not particularly limited as long as the desired oxidation reaction of sulfur atoms proceeds, but is usually preferably 0.1 to 10 mol, more preferably 0.5 to 5 mol, and even more preferably 0.8 to 1.5 mol, per 1 mol of sulfur atoms in the sulfur-containing polymer.

[0093] The reaction temperature of the oxidation reaction is not particularly limited as long as it is a temperature at which the desired oxidation reaction proceeds; however, in terms of facilitating the progression of the oxidation reaction, the reaction temperature is preferably 0 to 200°C, more preferably 10°C or higher, and even more preferably 15°C or higher; and in terms of suppressing side reactions, the reaction temperature is more preferably 180°C or lower, and even more preferably 150°C or lower.

[0094] The reaction time is not particularly limited, but is usually 0.1 to 100 hours, preferably 1 to 80 hours, more preferably 5 to 50 hours, and further preferably 10 to 24 hours.

[0095] In the oxidation reaction in the above step (2), a solvent may be used, and preferred examples of the solvent include the same solvents as those used in the polymerization step in the above step (1).

[0096] The polymer obtained in the above step (2) may contain residual acid, so it is preferable to wash it. The washing method is not particularly limited, and examples thereof include washing methods using water, acid, base, etc. In addition, in order to remove unreacted substances, the polymer may be passed through a filter or washed with a solvent. The above solvent is not particularly limited, and the same solvent as the reaction solvent can be used.

[0097] The method for producing the polymer (X) may include other steps in addition to the steps (1) and (2). Examples of the other steps include an aging step, a neutralization step, a dilution step, a drying step, a concentration step, and a purification step. These steps can be carried out by known methods.

[0098] <Metal oxide particles coated with polymeric materials> The metal oxide particles coated with the polymer material are particles in a state where a polymer material is attached to a part or all of the surface of the metal oxide particles to form a coating layer. The above-mentioned attachment refers to a state where the surface of the metal oxide particles and the polymer material are bonded by a covalent bond. Such a bonded state can be confirmed, for example, by whether or not the polymer material is separated from the metal oxide particles when extracted and washed with a solvent. From the viewpoint of preventing aggregation of the metal oxide particles, it is preferable that the entire surface of the metal oxide particles is covered with a polymer material.

[0099] The thickness of the coating layer is preferably 0.1 to 100 nm, more preferably 1 to 20 nm, and even more preferably 1 to 10 nm, from the viewpoints of high refractive index and dispersibility in resin. The thickness of the coating layer can be measured by a pyrolysis method using TGA. In addition, the thickness of the coating film can be estimated by comparing FE-SEM and TEM.

[0100] The amount of the coating layer (coating amount) is preferably 0.1 to 500 mass %, more preferably 5 to 100 mass %, and even more preferably 10 to 50 mass %, relative to 100 mass % of the metal oxide particles coated with the polymer material. The content of the coating layer can be determined by measuring with thermogravimetric differential thermal analysis (TG-DTA).

[0101] (metal oxide particles) The metal oxide particles to be coated with the polymer material include particles of a single metal oxide consisting of one metal element, a composite oxide consisting of two or more metal elements, and a solid solution oxide consisting of the single metal oxide or the composite oxide and a different element as a solid solution. The different element may be a metal element or a non-metal element other than oxygen, such as nitrogen or fluorine. Examples of the metal elements include lithium (Li), sodium (Na), potassium (K), magnesium (Mg), calcium (Ca), manganese (Mn), strontium (Sr), barium (Ba), titanium (Ti), zirconium (Zr), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), aluminum (Al), tin (Sn), silicon (Si), cerium (Se), and indium (In).

[0102] Examples of the single metal oxide include magnesium oxide, calcium oxide, strontium oxide, barium oxide, titanium oxide, zinc oxide, cerium oxide, silicon oxide, tin oxide, zirconium oxide, aluminum oxide, and indium oxide. Examples of the composite oxide include perovskite-type composite oxides such as barium titanate, barium strontium titanate, strontium titanate, barium zirconium strontium titanate, barium zirconium titanate, and lead zirconate titanate; spinel-type composite oxides such as spinel and lithium titanate; and composite oxides such as aluminum titanate. The solid solution oxide may be, for example, a solid solution oxide in which a different metal element and / or a nonmetal element other than oxygen, such as nitrogen or fluorine, is dissolved in the single metal oxide or composite oxide. These metal oxide particles may be used alone or in combination of two or more kinds.

[0103] Among them, particles of zirconium oxide, titanium oxide, or silicon dioxide are more preferable in terms of further improving transparency and reducing linear expansion of the resin composition, and particles of zirconium oxide or titanium oxide are more preferable in terms of improving the refractive index of the resin composition. Perovskite-type oxide particles are preferable in terms of having a high relative dielectric constant and being suitable for use as a ferroelectric material or piezoelectric material. Particles of boron nitride, aluminum hydroxide, and aluminum titanate are preferable in terms of having a high thermal conductivity and being suitable for use as a heat dissipation material.

[0104] Furthermore, the above-mentioned metal oxide particles are more preferably oxide particles containing Ti, Zr, Ce, Zn, In, Al, Si, or Sn as a main metal element, since they have no or little absorption in the visible light region and therefore it is easy to obtain a colorless and transparent composition in which coloring due to inorganic substances is suppressed, and further preferably particles of titanium oxide, zirconium oxide, cerium oxide, zinc oxide, indium oxide, aluminum oxide, silicon oxide, or tin oxide.

[0105] The shape of the metal oxide particles is not particularly limited, and may be, for example, any of irregular, spherical, plate-like, rod-like, polyhedral, and the like.

[0106] The average particle size of the metal oxide particles is preferably 1 nm or more and 1000 nm or less. When the average particle size of the metal oxide particles is within the above range, the transmittance of the visible light region and the infrared region can be improved. The average particle size of the metal oxide particles is more preferably 5 nm or more, and even more preferably 10 nm or more, and more preferably 100 nm or less, and even more preferably 50 nm or less. The average particle size is determined by observing the metal oxide with a SEM (magnification 1000 to 100,000 times, preferably 10,000 times), analyzing the obtained image to determine the particle size (circular area equivalent diameter) of about 10 to 1000 individual particles (primary particles), and evaluating the 50% particle size based on the particle size distribution based on the number. For the image analysis, known image analysis software (for example, Mac-View manufactured by Mountech Co., Ltd.) can be used.

[0107] The content of the metal oxide particles coated with the polymeric material can be appropriately set depending on the purpose and use of the resin composition, but is usually preferably 5 to 95% by mass relative to 100% by mass of the total solid content of the resin composition. In terms of high refractive index, the content of the metal oxide particles is more preferably 20% by mass or more, even more preferably 40% by mass or more, and even more preferably 60% by mass or more relative to 100% by mass of the total solid content of the resin composition, and from the viewpoint of transparency, it is more preferably 90% by mass or less, and even more preferably 80% by mass or less.

[0108] (Preparation of metal oxide particles coated with polymeric materials) The method for coating the metal oxide particles with the above-mentioned polymeric material is not particularly limited, and any known method can be used, such as a method using a silane coupling agent, a method of reacting a compound having a phosphate group, or a method of reacting a carboxylic acid group. Among these, the method of coating the metal oxide particles with the above-mentioned polymeric material using a silane coupling agent is preferred.

[0109] As a method using the above-mentioned silane coupling agent, for example, there can be mentioned a method in which the surface of metal oxide particles is treated with a silane coupling agent, and then the surface-treated metal oxide particles are reacted with a polymeric material.

[0110] The silane coupling agent is not particularly limited, and any known silane coupling agent can be used. Among them, silane coupling agents having a halogen atom, a vinyl group, an acrylic group, or a methacrylic group are preferred, and silane coupling agents having a halogen atom or a vinyl group are more preferred.

[0111] The above-mentioned silane coupling agent having a halogen atom can be prepared by reacting a silane compound having a group capable of reacting with an acid group with a compound having an acid group and a halogen atom. Preferred examples of the group capable of reacting with the acid group include an epoxy group. Preferred examples of the acid group include a carboxyl group, a phosphoric acid group, and a sulfo group.

[0112] In the above surface treatment, the amount of the silane coupling agent used is preferably 0.1 to 1000 parts by mass, more preferably 1 to 100 parts by mass, and even more preferably 10 to 80 parts by mass, relative to 100 parts by mass of the above metal oxide particles.

[0113] In the above surface treatment, the treatment temperature is preferably 0 to 150° C., and more preferably 10 to 100° C. The treatment time is preferably 1 to 100 hours, and more preferably 1 to 24 hours.

[0114] In the reaction between the surface-treated metal oxide particles and the polymeric material, the amount of the polymeric material used is preferably 1 to 10,000 parts by mass, and more preferably 10 to 1,000 parts by mass, per 100 parts by mass of the surface-treated metal oxide particles.

[0115] In the reaction between the surface-treated metal oxide particles and the polymeric material, the reaction temperature is preferably 0 to 150°C, and more preferably 10 to 120°C. The reaction time is not particularly limited, but is preferably 1 to 100 hours, and more preferably 1 to 48 hours.

[0116] The above surface treatment process and reaction process may be carried out in a solvent. The solvent to be used is not particularly limited, and examples thereof include one or more of alcohol-based solvents such as methanol, ethanol, propanol, butanol, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as ethyl acetate, isopropyl acetate, butyl acetate, and γ-butyrolactone; ether-based solvents such as diethyl ether, diisopropyl ether, 1,2-dimethoxyethane (DME), and tetrahydrofuran (THF); aromatic hydrocarbon-based solvents such as toluene and xylene; halogenated hydrocarbon-based solvents such as chlorobenzene, fluorobenzene, dichloromethane, chloroform, carbon tetrachloride, 1,2-dichloroethane, and benzotrifluoride; amide-based solvents such as dimethylformamide (DMF), dimethylacetamide, and N-methylpyrrolidone; dimethylsulfoxide (DMSO), nitromethane, and the like.

[0117] In the above-mentioned surface treatment step and reaction step, additives such as catalysts that are usually used in surface treatment steps and reaction steps may be further used. The types and amounts of these additives may be appropriately determined based on known techniques.

[0118] After the reaction, metal oxide particles having the surface coated with the polymer material can be obtained by optionally carrying out a washing step, a solvent removal step, etc. The washing step and the solvent removal step can be carried out by a known method.

[0119] The reaction step of the surface-treated metal oxide particles with the polymeric material may be a step of polymerizing a monomer component for forming the polymeric material in the presence of the surface-treated metal oxide particles, instead of using the polymeric material. Metal oxide particles coated with a polymeric material can also be prepared by this method.

[0120] The polymerization step may be carried out by appropriately selecting from known polymerization methods depending on the monomer components to be used, etc. In addition, in the polymerization step, known additives that are usually used, such as initiators, catalysts, and solvents, may also be appropriately used.

[0121] <Binder resin> The resin composition of the present invention further contains a binder resin. As described above, the binder resin preferably contains the polymer (X). As the binder resin, one type of the polymer (X) may be used, or two or more types of the polymer (X) may be used. Furthermore, the polymer (X) used as the binder resin may be the same as or different from the polymer (X) used as the polymer material.

[0122] The content of the binder resin can be appropriately set depending on the purpose and use of the resin composition, but is preferably 1 to 1000% by mass relative to 100% by mass of the total solid content of the resin composition. The content of the binder resin is more preferably 10% by mass or more, even more preferably 30% by mass or more, more preferably 500% by mass or less, and even more preferably 200% by mass or less, relative to 100% by mass of the total solid content of the resin composition, in terms of imparting flexibility and crack resistance.

[0123] <Compounds with a (poly)styrene skeleton> The resin composition of the present invention preferably further contains a compound having a (poly)styrene skeleton (hereinafter also referred to as "compound (Y)"). The compound having a (poly)styrene skeleton can be used as the above-mentioned polymer material or binder resin other than the above-mentioned polymer (X). For example, in the resin composition of the present invention, the polymer (X) is used as the above-mentioned polymer material, and the compound having a (poly)styrene skeleton is used as the above-mentioned binder resin, or the compound having a (poly)styrene skeleton is used as the above-mentioned polymer material, and the polymer (X) is used as the above-mentioned binder resin, or the polymer (X) is used as both the polymer material and the binder resin. Among them, the embodiment in which the polymer (X) is used as both the polymer material and the binder resin is preferred in terms of high refractive index.

[0124] The compound (Y) having a (poly)styrene skeleton is a compound having a structure represented by the following general formula (6).

[0125] [ka]

[0126] (In the formula, R 12 , R 13 and R 14 R may be the same or different and represents a hydrogen atom or a methyl group. 15 , R 16 , R 17 , R 18 and R 19 are the same or different and represent a hydrogen atom, an alkyl group, or an alkoxy group.

[0127] In the formula, R 15 , R 16 , R 17 , R 18 and R 19The alkyl group represented by the formula (I) may be linear, branched, or cyclic, but is preferably linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 18, more preferably 1 to 8, and even more preferably 1 to 3.

[0128] In the formula, R 15 , R 16 , R 17 , R 18 and R 19 The alkoxy group represented by the following formula (I) preferably has 1 to 18 carbon atoms, more preferably has 1 to 8 carbon atoms, and further preferably has 1 to 3 carbon atoms.

[0129] Specific examples of the compound (Y) include compounds such as styrene, α-methylstyrene, 4-methylstyrene, and polymers thereof. Among these, (poly)styrene is preferred because of its good compatibility with the polymer (X).

[0130] The compound (Y) preferably has a number average molecular weight of 500 to 30,000,000, more preferably 1,000 to 100,000, and even more preferably 2,000 to 10,000, in order to increase the compatibility with the polymer (X). The compound (Y) preferably has a polydispersity (Mw / Mn) of 1-10, more preferably 1-5, and even more preferably 1-2. The number average molecular weight and dispersity can be determined by the same method as the above-mentioned method for measuring the molecular weight of polymer (X).

[0131] The glass transition temperature (Tg) of the compound (Y) is preferably 80 to 250°C, more preferably 90°C or higher, more preferably 100°C or higher, more preferably 200°C or lower, and even more preferably 180°C or lower. The glass transition temperature can be determined in the same manner as for the glass transition temperature of the polymer (X).

[0132] In the case of the resin composition containing the compound (Y), the compound (Y) is preferably covalently bonded to the metal oxide particles, and in this case, the compound (Y) is used as the polymer material that coats the metal oxide particles. The covalent bond between the compound (Y) and the metal oxide particles can be confirmed by a method similar to the method for confirming the state in which the metal oxide particles are coated with the polymer material described above.

[0133] The content of the compound (Y) is preferably the content of the polymer material described above when the compound (Y) is used as the polymer material, and is preferably the content of the binder resin described above when the compound (Y) is used as the binder resin.

[0134] <Other ingredients> In addition to the above-mentioned components, the resin composition may contain, for example, resins other than those mentioned above, pigments, dyes, antioxidants, ultraviolet absorbers, reactive diluents, light stabilizers, plasticizers, non-reactive compounds, chain transfer agents, thermal polymerization initiators, anaerobic polymerization initiators, polymerization inhibitors, inorganic fillers, organic fillers, adhesion improvers such as coupling agents, heat stabilizers, antibacterial and antifungal agents, flame retardants, matting agents, defoamers, leveling agents, wetting and dispersing agents, anti-settling agents, thickeners and anti-sagging agents, color separation inhibitors, emulsifiers, slip and scratch inhibitors, anti-skinning agents, drying agents, antifouling agents, antistatic agents, conductive agents (electrostatic assistants), solvents, and other components. These components may be used alone or in combination of two or more. These components may be appropriately selected from known ones and used. The blending amounts of these components may be appropriately set.

[0135] In addition, when the resin composition is for an optical material, it may contain other components as appropriate depending on the application of the optical material. Specific examples of the other components include ultraviolet absorbers, IR cut agents, reactive diluents, pigments, detergents, antioxidants, light stabilizers, plasticizers, non-reactive compounds, and defoamers.

[0136] The resin composition preferably has a glass transition temperature (Tg) of 80 to 400° C. When the glass transition temperature is in the above-mentioned range, molding can be easily performed. From the viewpoint of increasing heat resistance, the glass transition temperature is more preferably 100° C. or higher, and even more preferably 115° C. or higher, and from the viewpoint of facilitating molding, it is more preferably 300° C. or lower, and even more preferably 200° C. or lower. The glass transition temperature can be determined by the same method as the above-mentioned method for measuring the glass transition temperature of the polymer.

[0137] The resin composition preferably has a refractive index of 1.6 or more. When the refractive index is within the above range, the resin composition can be suitably used as an optical material, etc. The refractive index is more preferably 1.65 or more, and further preferably 1.7 or more. The refractive index can be determined by the same method as the above-mentioned method for measuring the refractive index of a polymer.

[0138] The resin composition preferably has an Abbe number of 10 or more. When the Abbe number is within the above range, the light dispersion is small, and the resin composition can be an optical material suitable for lenses. The Abbe number is more preferably 15 or more, even more preferably 20 or more, and even more preferably 30 or more. From the viewpoint of adjusting the light dispersion, the Abbe number is more preferably 60 or less, and even more preferably 50 or less. The Abbe number can be determined by the same method as the above-mentioned method for measuring the Abbe number of a polymer.

[0139] The resin composition preferably has a visible light transmittance of 75% or more. If the visible light transmittance is within the above range, the resin composition can be suitably used as an optical material. The visible light transmittance is more preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more. The visible light transmittance can be determined by the same method as the above-mentioned method for measuring the visible light transmittance of a polymer.

[0140] The resin composition preferably has a linear expansion coefficient of 70 ppm / °C or less. When the linear expansion coefficient of the resin composition is within the above range, the refractive index change due to temperature is small, and the resin composition can be suitably used for various applications such as optical materials, sealing materials, and coating materials. The linear expansion coefficient is more preferably 50 ppm / °C or less, and even more preferably 20 ppm / °C or less, in terms of being able to suppress changes in optical properties due to temperature changes. The lower limit of the linear expansion coefficient is not particularly limited, but is preferably 1 ppm / °C or more, and even more preferably 3 ppm / °C or more. The linear expansion coefficient can be determined by measurement according to a method in accordance with JIS K 7197:2012.

[0141] The method for producing the resin composition is not particularly limited, and may be a method of mixing the metal oxide particles, the binder resin, and other components as necessary, using known means such as a bead mill, a roll mill, a ball mill, a jet mill, a kneader, or a blender.

[0142] <Application> INDUSTRIAL APPLICABILITY The resin composition of the present invention has a high refractive index and excellent transparency, and therefore can be suitably used in applications requiring a high refractive index or high transparency.

[0143] The resin composition of the present invention is used for various applications such as imaging lenses, optical materials (members), machine part materials, electric / electronic part materials, automobile part materials, civil engineering and construction materials, molding materials, as well as paints and adhesive materials, etc. Among these, it is particularly suitable for use as optical materials, optical device members, display device members, etc., and is more preferably used for optical purposes. Specific examples of such applications include optical applications such as eyeglass lenses, imaging lenses for cameras such as (digital) cameras, mobile phone cameras, and vehicle-mounted cameras, light beam focusing lenses, light diffusing lenses, and the like; LED sealants, optical adhesives, optical transmission bonding materials, filters, diffraction gratings, prisms, light guides, watch glass, and transparent glass and cover glass such as cover glass for display devices; optical device applications such as photosensors, photoswitches, LEDs, light-emitting elements, optical waveguides, multiplexers, branchers, disconnectors, optical splitters, and optical fiber adhesives; and display device applications such as substrates for display elements such as LCDs, organic ELs, and PDPs, substrates for color filters, substrates for touch panels, display protective films, display backlights, light guide plates, anti-reflection films, and anti-fogging films.

[0144] The resin composition is preferably thermoplastic, which allows for easy molding and excellent productivity.

[0145] The resin composition can also be suitably used as a molding material. The molding method is not particularly limited, and includes injection molding, extrusion molding, T-die method, inflation method, and other methods generally known as thermoplastic resin processing methods. It may also be molded into a desired shape by a casting method, coating method, or other method. The shape is not particularly limited, and includes various known shapes such as lenses, sheets, and films.

[0146] INDUSTRIAL APPLICABILITY As described above, the resin composition of the present invention has a high refractive index and is excellent in inhibiting aggregation of metal oxide particles, and can be suitably used for various applications such as optical applications. EXAMPLES

[0147] Examples are given below to explain the present invention in more detail, but the present invention is not limited to these examples only.

[0148] In the examples, each evaluation was conducted by the following method. <Weight-average molecular weight (Mw), number-average molecular weight (Mn), dispersity (Mw / Mn)> The weight-average molecular weight and number-average molecular weight of the polymer were determined by measuring under the following conditions by gel permeation chromatography (GPC). The dispersity was calculated by dividing the weight-average molecular weight by the number-average molecular weight. Apparatus: SHIMAZU, CBM-20A Detector: Differential refractive index detector (RI) (SHIMAZU, SPD-20MA), and ultraviolet-visible-infrared spectrophotometer (SHIMAZU, SPD-20MA) Column: TOSOH, TSKgel SuperHM-N Column temperature: 40 °C Flow rate: 0.3 mL / min Calibration curve: Polystyrene Standards Eluent: Chloroform

[0149] <Infrared spectroscopic analysis (IR)> IR measurement was performed under the following conditions. Apparatus: Fourier transform infrared spectrophotometer (FT / IR-6100) manufactured by JASCO Sample preparation: Approximately 2 mg of the sample was diluted with approximately 300 mg of dry potassium bromide (KBr). The mixture was ground with a mortar and pestle and molded.

[0150] <Thermogravimetric analysis (TGA, TG-DTA)> Measurement was performed under the following conditions. Apparatus: TG8120 manufactured by Rigaku Conditions: Measurement temperature range 20 - 200 °C (heating rate: 10.0 deg / min, hold for 30 minutes after reaching 200 °C) Sampling interval: 1.0 sec Atmosphere: N2 50 mL / min

[0151] <X-ray diffraction measurement (XRD)> The measurements were carried out under the following conditions. Equipment: Rigaku Corporation, RINT-UltimaIII X-ray source: Cu Kα ray Measurement range: 2θ=10-60° Sampling interval: 0.04° Scanning speed: 10° / min

[0152] <Glass transition temperature (Tg)> A differential scanning calorimeter (DSC) manufactured by Seiko Instruments Inc. was used, and α-alumina was used as a reference. The temperature was raised from room temperature to 250°C at a heating rate of 10°C / min. The DSC curve was obtained, and the evaluation was performed based on the intersection point of the tangent at the baseline and the inflection point.

[0153] <Transmittance of blended film> The measurements were made using a spectrophotometer (JASCO Corporation, ultraviolet, visible, and infrared spectrophotometer V-700 series). Air was used as a control sample. The visible light transmittance was evaluated at 400 nm.

[0154] <Refractive index (n D )> The phase difference and the reflection deviation ratio of the polarized light before and after incidence of the film were measured using a UVISEL spectroscopic ellipsometer manufactured by HORIBA Scientific Co., Ltd. The complex refractive index was obtained using the wavelength (450 nm) and the incident angle (75°) of the incident light, which were set in advance, and the refractive index at 190-2000 nm was calculated, and the refractive index at a wavelength of 589.3 nm was obtained. Unless otherwise specified, 30 mg of the polymer or resin composition was dissolved in 1,1,2,2-tetrachloroethane (1 ml) and passed through a membrane filter with a pore size of 0.2 μm. 0.4 ml of the solution that passed through the filter was drop-cast onto a glass substrate (2 cm × 2 cm) to obtain a film with a thickness of approximately 50 nm, which was then measured.

[0155] <Element content ratio O / S ratio> A sample was prepared by spin-coating 0.25 ml of the polymer solution on a silicon wafer, and a JEOL photoelectron spectrometer (JPS-9010TR, XPS device, light source: Mg, X-ray output: 400 W) was used to measure the peak intensity from the 2p orbital of sulfur atoms and the peak intensity from the 1s orbital of oxygen atoms, and the O / S ratio was calculated by calculating the integral ratio. If necessary, the peak intensity from the 1s orbital of carbon atoms was also measured, and the O / S ratio was calculated taking the results into consideration. The measurement method and the position of the binding energy were based on Handbook of X-ray Photoelectron Spectroscopy (published by JEOL in March 1991).

[0156] Example 1 (Synthesis of poly(2,6-dimethyldisulfide) (PMPS)) In a nitrogen atmosphere, 3,3',5,5'-tetramethyldiphenyl disulfide (5g, 18mmol) was added to a 1,1,2,2-tetrachloroethane solution (10ml) of 2,3-dichloro-5,6-dicyano-parabenzoquinone (DDQ, 2M) and trifluoromethanesulfonic acid (1M) in a 50ml three-neck flask, and oxidative polymerization was carried out by stirring at room temperature for 40 hours. After 40 hours, the 1,1,2,2-tetrachloroethane solution was dropped into hydrochloric acid-acidified methanol, and the powder was collected using a glass filter. It was then washed with an aqueous potassium hydroxide solution (0.1M) and pure water, and dried in vacuum to obtain a polymer (PMPS). The glass transition temperature of the polymer was 162°C. The O / S ratio was 0.02. The refractive index was 1.69.

[0157] (Bromo modification of titanium oxide particle surface) In a 30 mL flask, 3-glycidyloxypropyltrimethoxysilane SCA-ep (1.00 g, 4.23 mmol) and 2-bromo-2-methylpropionic acid (0.84 g, 5.00 mmol) were dissolved in 4 mL of tetrahydrofuran (THF) and reacted at 70° C. for 20 hours. After separation with water / chloroform and drying under reduced pressure, a bromo-containing silane coupling agent (SCA-Br) was obtained as a yellow viscous liquid. Next, anatase-type TiO2 fine particles (manufactured by Aldrich, particle size <25 nm, 1.0 g) were dispersed in toluene (60 mL), and the obtained SCA-Br (0.40 g) and triethanolamine (TEA) (0.1 mL) were added and reacted for 24 hours at 50°C under a N2 atmosphere. After washing with toluene and chloroform in a dialysis membrane and drying under reduced pressure, titanium oxide fine particles TiO2-Br with bromo groups on the surface were obtained as a white powder. From IR, 2900cm -1 Nearby CH stretch, 1700cm -1 Near C=O stretching, 1100 cm -1 A peak due to O-Si-O stretching was observed around the reaction site, supporting the progress of the reaction. The modification fraction was calculated to be 11 wt% (0.19 mmol of Br initiator per 1 g of TiO2-Br) by TGA.

[0158] (Polystyrene modification of titanium oxide particle surface by ATRP (Atom Transfer Radical Polymerization)) As an initiator, TiO2-Br (0.10g, Br:1eq) obtained above and 2-bromoisobutyric acid ethyl ester EBiB (3eq) were stirred in anisole, and styrene (460eq) and CuBr / PMDETA catalyst (3eq) were added as monomers, degassed, and reacted at 90℃ for 24 hours. After the reaction, the reaction solution was dissolved and dispersed in chloroform, the supernatant was collected by centrifugation, and free polystyrene was removed by precipitation purification in methanol. The precipitate obtained by centrifugation was dispersed again in chloroform, precipitated and purified in methanol, and centrifuged to obtain polystyrene-modified titanium oxide fine particles TiO2-PS as white powder. The fine particles TiO2-PS were evaluated by TG-DTA, and the weight ratio of TiO2 / PS was 78wt% / 22wt% based on the decomposition weight of polystyrene (PS), and Tg was 90℃. The molecular weight evaluation of PS showed that Mn=6100 and Mw / Mn=1.1. IR 2900 to 3050 cm -1 Aliphatic and aromatic CH stretching around 1500cm -1Aromatic ring stretching was observed around 2θ = 15°. XRD also showed a crystalline peak derived from anatase-type TiO2 and an amorphous broad peak derived from polystyrene at 2θ = 15° to 30°. These results support the progress of the reaction.

[0159] (Compatibility evaluation and optical properties of TiO2-PS / PMPS blend films) The TiO2-PS (Tg: 94°C) and PMPS (Tg: 162°C) prepared above were dissolved and dispersed in toluene at a weight ratio of 1 / 1 at 20 mg / mL to prepare a resin composition. The obtained resin composition was formed into a film on a glass substrate by the drop casting method. The blend film obtained by drop casting was visually transparent. In addition, DSC showed a single glass transition point (Tg: 120°C). This confirmed the good compatibility (uniformity) of TiO2-PS and PMPS. The transmittance of the obtained blend film was measured and it showed a high transmittance of 80% or more in the visible light range (400 to 700 nm), and 84.8% at 400 nm. 1 shows the measurement data of the transmittance of the blend membrane obtained in Example 1. FIG. 2 shows a photograph of the blend membrane obtained in Example 1. The refractive index of the resulting blend film was 1.68. From the above, it was confirmed that the resin compositions of the Examples had a high refractive index, were excellent in suppressing the aggregation of metal oxide particles, and gave blend films with high transmittance.

Claims

1. A resin composition comprising metal oxide particles coated with a polymer material and a binder resin, The polymer material and / or the binder resin includes a polymer having at least one structural unit selected from the group consisting of a structural unit (A) represented by the following general formula (1), a structural unit (B) represented by the following general formula (2), and a structural unit (C) represented by the following general formula (3): In the resin composition, the polymeric material and the binder resin contain the polymer, and the surfaces of the metal oxide particles and the polymeric material are bonded by a covalent bond, or the polymeric material contains the polymer and the binder resin contains a compound having a (poly)styrene skeleton, or the polymeric material contains the compound having a (poly)styrene skeleton and the binder resin contains the polymer, The coating amount of the polymeric material is 10 to 50% by mass based on 100% by mass of the metal oxide particles coated with the polymeric material. An optical resin composition comprising: 【Chemistry 1】 (In formulas (1) to (3), X 1 , X 2 and X 3 are the same or different and each represents a phenylene group, a naphthylene group, an anthrylene group, a biphenylene group or a triphenylene group which may have a substituent.

2. The structural unit (A) is a structural unit (A-1) represented by the following general formula (1-1): The structural unit (B) is a structural unit (B-1) represented by the following general formula (2-1):

2. The optical resin composition according to claim 1, wherein the structural unit (C) is a structural unit (C-1) represented by the following general formula (3-1): 【Chemistry 2】 (In the formulas (1-1), (2-1) and (3-1), R 1 , R 2 and R 3 are the same or different and each represents a halogen atom, a hydroxyl group, or an alkyl group, an alkoxy group, an aryl group, an aralkyl group, or a sulfur-containing substituent, each of which may have a substituent. 1 represents the number of, and is an integer from 0 to 4. 2 represents the number of, and is an integer from 0 to 4. c represents R 3 represents the number of, and is an integer from 0 to 4.

3. The optical resin composition according to claim 1 or 2, characterized in that the polymer has an elemental content ratio (O / S) of oxygen atoms O bonded to sulfur atoms S in the main chain to sulfur atoms S in the main chain of 0.02 to 1.

3.

4. 4. The optical resin composition according to claim 1, wherein the compound having a (poly)styrene skeleton and metal oxide particles are covalently bonded to each other.

Citation Information

Patent Citations

  • Resin composition for sealing semiconductor and its production, and semiconductor system using the resin composition for sealing semiconductor

    JP1999124480A

  • Polyphenylene sulfide resin composition

    JP2007302822A

  • Optical component and plastic lens

    JP2010043191A

  • Polyphenylene sulfide resin composition and molded article

    JP2014065842A

  • Molding material and optical member using the same

    JP2015168790A