Thermosetting sheet, dicing die bond film, and semiconductor device

A thermosetting sheet with specific resin and particle compositions and roughness characteristics addresses adhesion and thermal conductivity issues, enhancing semiconductor device performance by reducing gaps and promoting heat conduction.

JP7570885B2Active Publication Date: 2024-10-22NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020178947
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-26
Publication Date
2024-10-22
Estimated Expiration
2040-10-26

AI Technical Summary

Technical Problem

Existing thermosetting sheets used in semiconductor manufacturing often fail to achieve sufficient adhesion to substrates due to gaps forming between the sheet and the substrate, leading to increased thermal and electrical resistance, particularly when used with power semiconductor elements that generate significant heat.

Method used

A thermosetting sheet containing a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles is developed, with an arithmetic mean roughness Ra of 0.1 μm to 1.2 μm, which enhances adhesion and thermal conductivity by reducing void formation and promoting heat conduction paths.

Benefits of technology

The solution improves adhesion to substrates and achieves relatively high thermal conductivity, ensuring effective heat dissipation and electrical conduction in semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570885000007
    Figure 0007570885000007
  • Figure 0007570885000008
    Figure 0007570885000008
  • Figure 0007570885000001
    Figure 0007570885000001
Patent Text Reader

Abstract

To provide a thermosetting sheet with relatively high thermal conductivity after curing, capable of improving the adhesion with a substrate including a region where a semiconductor element is mounted, a dicing die bond film, and a semiconductor device.SOLUTION: In a dicing die bond film 20, a thermosetting sheet 3 includes thermosetting resin, thermoplastic resin, a volatile component, and a conductive particle. An arithmetic average roughness Ra measured before the curing is 0.1 μm or more and 1.2 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermosetting sheet, a dicing die bond film, and a semiconductor device. [Background technology]

[0002] 2. Description of the Related Art In the manufacture of semiconductor devices, it has been known to use a thermosetting sheet as a method for bonding a semiconductor element to a substrate having a mounting area for the semiconductor element (die bonding method) (see, for example, Patent Document 1). Patent Document 1 discloses a thermosetting sheet that contains conductive particles and a thermosetting resin.

[0003] In such a method, for example, a thermosetting sheet is attached to one side of a semiconductor wafer (the side opposite to the circuit-forming surface), and the semiconductor wafer and the thermosetting sheet are diced to obtain a plurality of thermosetting sheets each having a semiconductor element attached to one side. The thermosetting sheet with the semiconductor element attached on one side has the other side temporarily attached to the region of the substrate where the semiconductor element is to be attached at a predetermined temperature (e.g., 70° C.), and then is thermally cured at a higher temperature (e.g., 200° C.) to be bonded to the substrate. In other words, the semiconductor element is bonded to the substrate with the thermosetting sheet interposed therebetween. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-21813 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the other side of the thermosetting sheet is temporarily attached to the substrate, the other side of the thermosetting sheet may not be sufficiently adhered to the substrate, resulting in a gap being formed between the other side of the thermosetting sheet and the substrate. Furthermore, any gap that occurs between the other side of the thermosetting sheet and the substrate in the temporary adhesion state will remain when the thermosetting sheet is thermally cured and adhered to the substrate (the gap that occurred in the temporary adhesion state will be carried over even in the adhered state). If such a gap occurs between the thermosetting sheet and the substrate, the thermal resistance and electrical resistance at the interface will increase, resulting in insufficient electrical and thermal conduction, which is undesirable. However, it cannot be said that sufficient research has been done yet on improving the adhesion between the thermosetting sheet and the substrate in a temporarily attached state.

[0006] Furthermore, when a power semiconductor element is used in a semiconductor device, the power semiconductor element generates a large amount of heat because it is used with a large amount of electric power. Therefore, when the above-mentioned thermosetting sheet is used for a power semiconductor element, it is preferable that the thermosetting sheet after being adhered to the substrate, that is, the thermosetting sheet after being cured, has high thermal conductivity.

[0007] Although the above-mentioned heat generation problem also occurs when semiconductor elements other than power semiconductor elements are used, it cannot be said that sufficient research has yet been conducted into improving the thermal conductivity of the cured thermosetting sheet.

[0008] Therefore, the present invention aims to provide a thermosetting sheet that can improve adhesion to a substrate having a mounting area for a semiconductor element in a temporarily attached state and has relatively high thermal conductivity after curing, as well as a dicing die bond film and a semiconductor device that include the thermosetting sheet. [Means for solving the problem]

[0009] After extensive research, the inventors discovered that by making the thermosetting sheet contain a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles, and by making the arithmetic mean roughness Ra measured in the pre-cured state 0.1 μm or more and 1.2 μm or less, the adhesion to the substrate can be improved when the thermosetting sheet is temporarily attached to the mounting area of ​​the semiconductor element of the substrate, and the thermal conductivity after curing becomes relatively high, which led to the invention.

[0010] That is, the thermosetting sheet according to the present invention is The composition includes a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles, The arithmetic mean roughness Ra measured before curing is 0.1 μm or more and 1.2 μm or less.

[0011] According to this configuration, the arithmetic mean roughness Ra of the thermosetting sheet measured in the pre-cured state is 0.1 μm or more and 1.2 μm or less, so that in the temporarily attached state, it is possible to relatively suppress the occurrence of gaps between the substrate having the mounting area for the semiconductor element and the thermosetting sheet. This can improve the adhesion between the thermosetting sheet and the substrate. Furthermore, since the thermosetting sheet contains the volatile component, the volume of the thermosetting sheet can be reduced by volatilizing the volatile component during thermal curing of the thermosetting sheet. Furthermore, since the volume of the thermosetting sheet is reduced, the conductive particles are positioned closer to each other in the thermosetting sheet, making it easier for the conductive particles to form thermal conduction paths within the thermosetting sheet. This allows the thermal conductivity after curing to be relatively high. Furthermore, since the thermosetting sheet contains the thermoplastic resin, the thermosetting sheet can have a relatively low elasticity even after being thermally cured. This makes it possible to more sufficiently maintain the adhesion between the thermosetting sheet and the substrate even after thermal curing, thereby more sufficiently increasing the thermal conductivity. As a result, the thermosetting sheet of the present invention, in a temporarily attached state, has improved adhesion to a substrate having a mounting area for a semiconductor element, and also has relatively high thermal conductivity after curing.

[0012] In the thermosetting sheet, The maximum height roughness Rz measured before curing is preferably 1 μm or more and 12 μm or less.

[0013] With this configuration, the adhesion between the thermosetting sheet and the substrate can be further improved.

[0014] In the thermosetting sheet, It is preferable that the particle filling rate P of the conductive particles in the thermosetting sheet after curing is 30 volume % or more.

[0015] With this configuration, the thermal conductivity of the thermally conductive sheet after curing can be further increased.

[0016] In the thermosetting sheet, It is preferable that the thermal conductivity after curing is 3 W / m·K or more.

[0017] With this configuration, the thermal conductivity of the thermosetting sheet after curing can be further increased.

[0018] The dicing die bond film according to the present invention is A base layer; a dicing tape having a pressure-sensitive adhesive layer laminated on the base layer; a thermosetting sheet laminated on the pressure-sensitive adhesive layer of the dicing tape; The thermosetting sheet is any one of the thermosetting sheets described above.

[0019] According to this configuration, the dicing die bond film has improved adhesion to a substrate having an area for mounting a semiconductor element in a temporarily attached state, and also has relatively high thermal conductivity after curing.

[0020] The semiconductor device according to the present invention comprises: a substrate having a mounting area for a semiconductor element; a semiconductor element mounted in the semiconductor element mounting area; the semiconductor element is mounted on a mounting area of ​​the substrate for the semiconductor element via a thermosetting sheet, the thermosetting sheet is cured, The bonding rate of the thermosetting sheet to the substrate is 70% or more; The thermosetting sheet is any one of the thermosetting sheets described above.

[0021] According to this configuration, the bonding rate of the thermosetting sheet to the substrate is 70% or more, so that the semiconductor device has the thermosetting sheet sufficiently bonded to the mounting area of ​​the semiconductor element of the substrate. This provides the semiconductor device with relatively high thermal conductivity after curing. Effect of the Invention

[0022] According to the present invention, it is an object of the present invention to provide a thermosetting sheet that can improve adhesion to a substrate having a mounting area for a semiconductor element in a temporarily attached state and has relatively high thermal conductivity after curing, as well as a dicing die bond film and a semiconductor device that include the thermosetting sheet. [Brief description of the drawings]

[0023] [Figure 1] 1 is a cross-sectional view showing a configuration of a dicing die bond film according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a configuration of a semiconductor device according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, one embodiment of the present invention will be described.

[0025] [Thermosetting sheet] The thermosetting sheet according to this embodiment contains a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles. In this specification, the conductive particles refer to particles having an electrical conductivity of 100 μS / cm or less as measured in accordance with JIS K 0130 (2008). As described above, the thermosetting sheet according to this embodiment contains a volatile component. Therefore, the volume of the thermosetting sheet can be reduced by volatilizing the volatile component during thermal curing of the thermosetting sheet. Furthermore, since the volume of the thermosetting sheet is reduced, the conductive particles are positioned closer to each other in the thermosetting sheet, making it easier for the conductive particles to form thermal conduction paths within the thermosetting sheet. This allows the thermosetting sheet to have relatively high thermal conductivity after being thermally cured.

[0026] The thermosetting sheet according to this embodiment has an arithmetic mean roughness Ra measured before curing of 0.1 μm or more and 1.2 μm or less. By having the arithmetic mean roughness Ra measured in the pre-cured state be 0.1 μm or more and 1.2 μm or less, when the thermosetting sheet is temporarily attached to a substrate having an area for mounting a semiconductor element, the occurrence of gaps between the substrate and the thermosetting sheet can be relatively suppressed. As a result, the thermosetting sheet according to this embodiment has improved adhesion to the substrate having the area for mounting the semiconductor element in a temporarily attached state.

[0027] The thermosetting sheet according to this embodiment may have two adhesive surfaces (the front and back surfaces of the sheet) such that the arithmetic mean roughness Ra of at least one of the surfaces falls within the above-mentioned numerical range, but it is preferable that the arithmetic mean roughness Ra of both surfaces falls within the above-mentioned numerical range.

[0028] The arithmetic mean roughness Ra of a thermosetting sheet before curing can be measured by a non-contact roughness measurement method with a cutoff value of 0.08 mm using a Lasertec 3CCD color confocal microscope (model OPTELICS H3000) and control software LM eye for the roughness curve of the surface of the thermosetting sheet before curing. In the non-contact roughness measurement method, the microscope is operated under conditions in which the observation magnification is set to 500 times and the resolution is set to 0.05 μm. The arithmetic mean roughness Ra is defined in JIS B0601:2013.

[0029] The thermosetting sheet according to this embodiment can be obtained, for example, by applying a varnish containing a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles to a release film, drying the varnish, and then pressing the resulting single layer or multiple layers in a laminated state under vacuum (for example, under a pressure of 3.3 kPa or less). Therefore, when obtaining the varnish, the arithmetic mean roughness Ra of the thermosetting sheet can be adjusted to the above-mentioned numerical range by improving the dispersibility of the conductive particles in the resin components (thermosetting resin and thermoplastic resin). For example, by stirring and mixing a primary mixture containing the resin component (primary stirring), and then adding the conductive particles and the volatile component to the primary mixture, and stirring and mixing the resulting secondary mixture (secondary stirring), the dispersibility of the conductive particles in the resin component can be improved, and the arithmetic mean roughness Ra of the thermosetting sheet can be adjusted to the above-mentioned numerical range. When spherical conductive particles, which will be described later, are used as the conductive particles, the dispersibility of the conductive particles in the resin component can be more easily improved. In addition, as described above, the thermosetting sheet according to this embodiment contains, in addition to the thermosetting resin, a thermoplastic resin and a volatile component, and it is believed that these components are one of the factors that affect the smoothness of the surface when pressed under vacuum.

[0030] The mass % of the thermosetting resin in 100 mass % (mass parts) of the thermosetting sheet is preferably 1 mass % or more and 30 mass % or less, and more preferably 3 mass % or more and 15 mass % or less. The mass % of the thermoplastic resin in 100 mass % of the thermosetting sheet is preferably 0.5 mass % or more and 10 mass % or less, and more preferably 1 mass % or more and 7 mass % or less. The mass % of the conductive particles in 100 mass % of the thermosetting sheet is preferably 60 mass % or more and 95 mass % or less, and more preferably 80 mass % or more and 93 mass % or less. The mass proportion of the thermosetting resin in 100 mass% of resins (thermosetting resin and thermoplastic resin) is preferably 30 mass% or more and 90 mass% or less, and more preferably 50 mass% or more and 80 mass% or less.

[0031] Examples of the thermosetting resin include epoxy resin, phenol resin, amino resin, unsaturated polyester resin, polyurethane resin, silicone resin, and thermosetting polyimide resin, etc. Among these, it is preferable to use epoxy resin.

[0032] Examples of epoxy resins include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, cresol novolac type, orthocresol novolac type, trishydroxyphenylmethane type, tetraphenylolethane type, hydantoin type, trisglycidyl isocyanurate type, and glycidylamine type epoxy resins. Among these, it is preferable to use at least one of bisphenol A type epoxy resin and cresol novolac type epoxy resin, and it is more preferable to use a combination of bisphenol A type epoxy resin and cresol novolac type epoxy resin. The bisphenol A type epoxy resin includes an aliphatic modified bisphenol A type epoxy resin.

[0033] Examples of phenolic resins as a curing agent for epoxy resins include novolac-type phenolic resins, resol-type phenolic resins, biphenyl-type phenolic resins, and polyoxystyrenes such as polyparaoxystyrene. Among the above phenolic resins, it is preferable to use biphenyl-type phenolic resins.

[0034] In addition, as the thermosetting resin, a thermoplastic resin having a thermosetting functional group can also be used. As the thermoplastic resin having a thermosetting functional group, for example, a thermosetting functional group-containing acrylic resin can be mentioned. As the acrylic resin in the thermosetting functional group-containing acrylic resin, a monomer unit derived from a (meth)acrylic acid ester can be mentioned. In the case of a thermoplastic resin having a thermosetting functional group, a curing agent is selected depending on the type of the thermosetting functional group.

[0035] The thermoplastic resin functions as a binder. Since the thermosetting sheet according to this embodiment contains a thermoplastic resin as a binder, the thermosetting sheet according to this embodiment can have a relatively low elasticity even after being thermally cured. Examples of the thermoplastic resin include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resin such as polyamide 6 and polyamide 6,6, phenoxy resin, acrylic resin, saturated polyester resin such as PET and PBT, polyamideimide resin, fluororesin, etc. Only one type of the thermoplastic resin may be used, or two or more types may be used in combination. As the thermoplastic resin, acrylic resin is preferable from the viewpoint that it has a small amount of ionic impurities and has high heat resistance, so that it is easy to ensure the connection reliability by the thermosetting sheet.

[0036] The acrylic resin is preferably a polymer containing a monomer unit derived from a (meth)acrylic acid ester as the monomer unit having the largest mass ratio. Examples of the (meth)acrylic acid ester include an alkyl (meth)acrylic acid ester, a cycloalkyl (meth)acrylic acid ester, and an aryl (meth)acrylic acid ester. The acrylic resin may contain a monomer unit derived from another component copolymerizable with the (meth)acrylic acid ester. Examples of the other component include a functional group-containing monomer such as a carboxyl group-containing monomer, an acid anhydride monomer, a hydroxyl group-containing monomer, a glycidyl group-containing monomer, a sulfonic acid group-containing monomer, a phosphoric acid group-containing monomer, an acrylamide, and an acrylonitrile, and various polyfunctional monomers. The acrylic resin is preferably a carboxyl-containing acrylic rubber.

[0037] The conductive particles preferably include silver particles. The silver particles may be in the form of, for example, flakes, needles, filaments, spheres, or flat (including scales). Of these, it is preferable to use spherical particles. By using spherical silver particles, the dispersibility of the silver particles in the thermosetting sheet can be improved. In this specification, the silver particles being spherical means that the silver particles have a circularity of 0.7 or more in a cross section obtained by cutting the thermosetting sheet in the thickness direction. Circularity is an index that measures the complexity of a sphere based on the area and perimeter values. If the area is S and the perimeter is L, the circularity is 4πS / L. 2 A circularity of 1 results in a perfect circle, and a circularity value less than 1 results in a shape that is less circular. The circularity can be obtained by cutting the thermosetting sheet in the thickness direction, taking an SEM image of the cut surface, and analyzing the SEM image using a powder image analyzer (PITA-3, manufactured by Seishin Enterprise Co., Ltd.) (specifically, by analyzing it with image analysis software such as "Image J"). Analysis using the powder image analyzer is performed on 10 randomly selected silver particles in the SEM image, and the circularity can be calculated by taking the arithmetic average of the circularity values ​​obtained for the 10 silver particles. In addition, when the thermosetting sheet contains conductive particles other than silver particles, the silver particles can be distinguished from the conductive particles other than silver particles by observing the reflected electron images so that light and dark appear due to differences in composition.

[0038] The silver particles have a volume average particle diameter D 50 However, it is preferably 0.01 μm or more, more preferably 0.1 μm or more, and particularly preferably 0.5 μm or more. The volume average particle diameter D of the silver particles 50When the specific surface area of ​​the silver particles is 0.01 μm or more, the silver particles can be dispersed relatively easily in the thermosetting sheet. In addition, the specific surface area of ​​the silver particles can be prevented from becoming excessively large, which would otherwise make the surfaces of the silver particles more susceptible to oxidation, thereby ensuring sufficient electrical conductivity for the silver particles. The volume average particle diameter D of the silver particles 50 When the particle size is 0.1 μm or more, the silver particles can be more easily dispersed in the thermosetting sheet, and the electrical conductivity of the silver particles can be more securely ensured. The volume average particle diameter D of the silver particles 50 When the particle size is 0.5 μm or more, the silver particles are more easily dispersed in the thermosetting sheet, and the electrical conductivity of the silver particles can be more securely ensured. The silver particles have a volume average particle diameter D 50 However, it is preferably 10 μm or less, more preferably 5 μm or less, and particularly preferably 1 μm or less. The volume average particle diameter D of the silver particles 50 By making the diameter of the silver particles 10 μm or less, the outer surfaces of the silver particles can be melted to a degree that enables sintering at a temperature (for example, 200° C.) sufficient to cure the thermosetting resin. The volume average particle diameter D of the silver particles 50 By making the diameter of the silver particles 5 μm or less, the outer surfaces of the silver particles can be more easily melted to a degree that enables sintering at a temperature that cures the thermosetting resin. The volume average particle diameter D of the silver particles 50 By making the diameter of the silver particles 1 μm or less, the outer surfaces of the silver particles can be more easily melted to a degree that enables sintering at a temperature that cures the thermosetting resin. Furthermore, the conductive particles have a volume average particle diameter D 50 However, the thickness is preferably 0.01 μm or more and 10 μm or less, more preferably 0.1 μm or more and 5 μm or less, and particularly preferably 0.5 μm or more and 1 μm or less.

[0039] The silver particles have a volume average particle diameter D 90However, it is preferably 0.05 μm or more, more preferably 0.5 μm or more, and particularly preferably 1 μm or more. The silver particles have a volume average particle diameter D 90 However, it is preferably 10 μm or less, more preferably 5 μm or less, and particularly preferably 2 μm or less. Furthermore, the silver particles have a volume average particle diameter D 90 However, the thickness is preferably 0.05 μm or more and 10 μm or less, more preferably 0.5 μm or more and 5 μm or less, and particularly preferably 1 μm or more and 2 μm or less.

[0040] The volume average particle diameter D of the silver particles 50 and D. 90 can be measured on a volume basis using, for example, a laser diffraction / scattering type flow particle size measuring device (Microtrac MT3000II series, manufactured by Microtrac Bell).

[0041] The silver particles may be silver particles composed of silver element and other elements (metal elements, etc.) contained as unavoidable impurity elements, or may be silver particles that have been subjected to a surface treatment (for example, silane coupling treatment). Examples of surface treatment agents for silver particles include fatty acid-based, amine-based, and epoxy-based coating agents. Examples of commercially available silver particles that have been surface-treated with a fatty acid-based coating agent include AG-2-8F manufactured by DOWA Electronics Co., Ltd., and examples of commercially available silver particles that have been surface-treated with an epoxy-based coating agent include HP02-B manufactured by Mitsui Mining & Smelting Co., Ltd. In the following, silver particles that have been surface-treated with a coating agent such as a fatty acid-based, amine-based, or epoxy-based coating agent may be referred to as coating agent-treated silver particles. In the thermosetting sheet according to the present embodiment, it is preferable to use coated silver particles as the silver particles. By using coated silver particles as the silver particles, it is possible to increase the affinity with the resin components (thermosetting resin and thermoplastic resin) contained in the thermosetting sheet, so that the silver particles are easily dispersed in the thermosetting sheet.

[0042] The conductive particles may include, in addition to silver particles, nickel particles, copper particles, aluminum particles, carbon black, carbon nanotubes, particles in which the surface of a metal particle serving as a core (nucleus) is plated with a metal such as gold or silver (hereinafter also referred to as plated metal particles), and particles in which the surface of a resin particle serving as a core (nucleus) is coated with a metal (hereinafter also referred to as metal-coated resin particles), etc. Only one of these conductive particles may be used, or two or more types may be used in combination.

[0043] As the plated metal particles, for example, particles having a nickel particle or copper particle as a core, the surface of which is plated with a noble metal such as gold or silver, can be used. As the metal-coated resin particles, for example, particles having a resin particle as a core, the surface of which is coated with a metal such as nickel or gold, can be used. When the thermosetting sheet according to the present embodiment contains conductive particles other than silver particles, it is preferable to use plated metal particles as the conductive particles, and it is preferable to use particles (silver-coated copper particles) in which copper particles are used as the core and the surface of the core is plated with silver as the plated metal particles. Commercially available silver-coated copper particles include 1200YP (copper particles) manufactured by Mitsui Mining & Smelting Co., Ltd., 20% by mass of silver particles coated on the product name, MA-C03K (copper particles) manufactured by Mitsui Mining & Smelting Co., Ltd., 20% by mass of silver particles coated on the product name, and AOP-TCY-2 (EN) manufactured by DOWA Electronics Co., Ltd. When the thermosetting sheet according to this embodiment contains conductive particles other than silver particles, the mass percentage of silver particles in 100 mass% of the conductive particles is preferably 10 mass% or more and 95 mass% or less, and more preferably 20 mass% or more and 90 mass% or less.

[0044] The conductive particles other than silver particles may be, for example, flake-shaped, needle-shaped, filament-shaped, spherical, or flat (including scale-shaped) particles, with spherical particles being preferred among these. By using spherical conductive particles other than silver particles, the dispersibility of the conductive particles other than silver particles in the thermosetting sheet can be improved. Here, since spherical particles have a smaller specific surface area than flat particles, if spherical particles are used as conductive particles other than silver particles, the contact area between the conductive particles other than silver particles and the silver particles will be small, which is thought to be disadvantageous in terms of electrical conductivity and thermal conductivity. However, since the thermosetting sheet according to this embodiment contains a volatile component, the volatile component evaporates during the thermal curing of the thermosetting sheet, thereby reducing the volume of the thermosetting sheet after curing (the thermosetting sheet shrinks), and the conductive particles other than the silver particles are positioned close to the silver particles. Therefore, even when spherical particles are used as conductive particles other than silver particles, a sufficient contact area between the conductive particles other than silver particles and the silver particles can be ensured, thereby ensuring sufficient electrical conductivity and thermal conductivity. In addition, the above-mentioned 1200YP (trade name) manufactured by Mitsui Metals and Smelting Co., Ltd., coated with 20% by mass of silver particles, MA-C03K (trade name) manufactured by Mitsui Metals and Smelting Co., Ltd., coated with 20% by mass of silver particles, and AOP-TCY-2(EN) (trade name) manufactured by Dowa Electronics Co., Ltd. are all classified as spherical.

[0045] Conductive particles other than silver particles have a volume average particle diameter D 50 However, it is preferably 0.01 μm or more, more preferably 0.5 μm or more, and particularly preferably 1.5 μm or more. In addition, conductive particles other than silver particles have a volume average particle diameter D 50 However, it is preferably 20 μm or less, more preferably 10 μm or less, and particularly preferably 5 μm or less. Furthermore, the conductive particles other than silver particles have a volume average particle diameter D 50 However, the thickness is preferably 0.01 μm or more and 20 μm or less, more preferably 0.5 μm or more and 10 μm or less, and particularly preferably 1.5 μm or more and 5 μm or less. Volume average particle diameter D of conductive particles other than silver particles 50 The volume average particle diameter D of the silver particles described above is 50It can be measured in the same manner as above.

[0046] Conductive particles other than silver particles have a volume average particle diameter D 90 However, it is preferably 0.1 μm or more, more preferably 1 μm or more, and particularly preferably 3 μm or more. In addition, conductive particles other than silver particles have a volume average particle diameter D 90 However, it is preferably 30 μm or less, more preferably 15 μm or less, and particularly preferably 10 μm or less. Furthermore, the conductive particles other than silver particles have a volume average particle diameter D 90 However, the thickness is preferably 0.1 μm or more and 30 μm or less, more preferably 1 μm or more and 15 μm or less, and particularly preferably 3 μm or more and 10 μm or less.

[0047] When the thermosetting sheet according to the present embodiment contains silver particles and conductive particles other than silver particles as the conductive particles, the D 50 is the D of silver particles 50 It is preferable that the D of conductive particles other than silver particles is larger than 90 is the D of silver particles 90 It is preferable that it is greater than . This allows the silver particles to be in more sufficient contact with the conductive particles other than silver particles in the thermosetting sheet, thereby providing the thermosetting sheet with superior thermal conductivity. In addition, the D of silver particles 50 D of conductive particles other than silver particles 50 Ratio of conductive particles other than silver particles to 50 / Silver particle D 50 ) is preferably 1.5 or more, and more preferably 2.5 or more. In addition, the D of silver particles 50 D of conductive particles other than silver particles 50 The ratio is preferably 10 or less, and more preferably 6 or less. In addition, the D of silver particles 50 D of conductive particles other than silver particles 50The ratio is preferably 1.5 or more and 10 or less, and more preferably 2.5 or more and 6 or less. In addition, the D of silver particles 90 D of conductive particles other than silver particles 90 Ratio of conductive particles other than silver particles to 90 / Silver particle D 90 ) is preferably 1.5 or more, and more preferably 2 or more. In addition, the D of silver particles 90 D of conductive particles other than silver particles 90 The ratio is preferably 10 or less, and more preferably 5 or less. In addition, the D of silver particles 90 D of conductive particles other than silver particles 90 The ratio is preferably 1.5 or more and 10 or less, and more preferably 2 or more and 5 or less.

[0048] The thermosetting sheet according to the present embodiment may contain a thermosetting catalyst in order to sufficiently advance the curing reaction of the resin component and to increase the curing reaction rate. Examples of the thermosetting catalyst include imidazole-based compounds, triphenylphosphine-based compounds, amine-based compounds, and trihalogen borane-based compounds.

[0049] The thermosetting sheet according to this embodiment preferably has a maximum height roughness Rz measured before curing of 1 μm or more and 12 μm or less. By having the maximum height roughness Rz measured in the pre-cured state be 1 μm or more and 12 μm or less, it is possible to further prevent gaps from occurring between the substrate and the thermosetting sheet when the thermosetting sheet is temporarily attached to a substrate having an area for mounting a semiconductor element. This allows the thermosetting sheet according to this embodiment to have even greater adhesion to the substrate having the area for mounting the semiconductor element in a temporarily attached state.

[0050] The maximum height roughness Rz of the thermosetting sheet before curing can be measured by a non-contact roughness measurement method with a cutoff value of 0.08 mm using a Lasertec 3CCD color confocal microscope (model OPTELICS H3000) and control software LM eye to measure the roughness curve of the surface of the thermosetting sheet before curing. In the non-contact roughness measurement method, the microscope is operated under conditions in which the observation magnification is set to 500 times and the resolution is set to 0.05 μm. The maximum height roughness Rz is defined in JIS B0601:2013.

[0051] The thermosetting sheet according to this embodiment may contain a volatile component. The thermosetting sheet according to this embodiment preferably contains 5% by mass or more and 50% by mass or less of the volatile components relative to the total mass of the organic components (thermosetting resin, thermoplastic resin, volatile components) contained in the thermosetting sheet, and more preferably contains 10% by mass or more and 40% by mass or less of the volatile components. The volatile component may be an organic compound having one or more hydroxyl groups and a boiling point of 250°C or higher. The boiling point of the organic compound is preferably 350°C or lower. Such an organic compound may be a terpene compound. Among terpene compounds, the volatile component is preferably isobornylcyclohexanol represented by the following formula (1). Isobornylcyclohexanol is an organic compound having a boiling point of 308 to 318°C. When heated from room temperature (23±2°C) to 600°C under a nitrogen gas flow of 200mL / min and at a temperature increase rate of 10°C / min, it has the property of undergoing a large weight loss from 100°C or higher and volatilizing and disappearing at 245°C (no further weight loss is observed). It also has the property of exhibiting an extremely high viscosity of 1,000,000 mPa·s at 25°C, but a relatively low viscosity of 1,000 mPa·s or lower at 60°C. The weight loss is a value when the weight loss rate at the measurement start temperature (room temperature) is set to 0%. Thus, isobornylcyclohexanol exhibits extremely high viscosity at 25° C. as described above, and is therefore capable of maintaining a sheet shape at room temperature, but exhibits relatively low viscosity at 60° C. as described above, and thus becomes tacky. In other words, a thermosetting sheet containing isobornylcyclohexanol exhibits excellent sheet shape retention at room temperature, and becomes tacky at temperatures of 60° C. or higher. Here, when mounting a semiconductor element attached to one side of a thermosetting sheet on a metal lead frame or the like, the semiconductor element is usually temporarily attached (temporarily fixed) to an adherend such as a metal lead frame via the thermosetting sheet at a temperature of 60 to 80° C., but since isobornylcyclohexanol has tackiness at 60° C. or higher as described above, when the thermosetting sheet according to this embodiment contains isobornylcyclohexanol as a volatile component, the thermosetting sheet has improved temporary adhesion to an adherend such as a metal lead frame. In other words, in the temporarily attached state, the mounting position of the semiconductor element is not shifted and the thermosetting sheet is prevented from lifting off the adherend. Therefore, when the thermosetting sheet is thermally cured to bond the semiconductor element to the adherend, the semiconductor element can be bonded to the adherend with high reliability.

[0052] [ka]

[0053] In the thermosetting sheet according to this embodiment, the particle filling rate P of the conductive particles in the thermosetting sheet before curing is preferably 30% by volume or more, more preferably 40% by volume or more, and even more preferably 50% by volume or more. The particle packing ratio P is preferably 70% by volume or less, and more preferably 60% by volume or less. When the particle filling rate P falls within the above range, the heat dissipation properties of the cured thermosetting sheet can be further improved. The particle filling rate refers to the proportion of conductive particles per unit volume, and can be determined by, as described below, mechanically polishing a thermosetting sheet to expose a cross section, taking an SEM image of an arbitrary cross-sectional region using a field emission electron microscope to obtain a reflected electron image as image data, and then performing image analysis on the image data.

[0054] The particle packing ratio P can be determined according to the following procedure. (1) The cured thermosetting sheet is mechanically polished to expose a cross section, and the exposed cross section is subjected to ion polishing using an ion polishing device (for example, product name: Cross Section Polisher SM-09010, manufactured by JEOL Ltd.). (2) An SEM image (scanning electron microscope image) of an arbitrary cross-sectional area of ​​the exposed cross-section that has been ion-polished is taken using a field emission scanning electron microscope (e.g., Hitachi High-Technologies Corporation, product name SU8020), and a backscattered electron image is obtained as image data. The imaging conditions can be an acceleration voltage of 5 kV and a magnification of 5000 times. (3) The obtained image data is subjected to an automatic binarization process using image analysis software (e.g., ImageJ) to binarize the metal parts and the resin parts. (4) The total area of ​​the conductive particle parts and the total area (conductive particle parts + resin part) are calculated from the binarized image, and the total area of ​​the conductive particle parts is divided by the total area to calculate the particle filling rate P of the conductive particles for the cured thermosetting sheet. The particle packing ratio P of the conductive particles is preferably determined by arithmetically averaging the packing ratios determined for five cross-sectional regions on the exposed cross-section subjected to ion polishing.

[0055] The thickness of the thermosetting sheet according to this embodiment is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. When the thickness of the thermosetting sheet is 150 μm or less, the thermal conductivity can be further improved. The thickness of the thermosetting sheet can be determined, for example, by measuring the thickness at five randomly selected points using a dial gauge (manufactured by PEACOCK, model R-205) and calculating the arithmetic average of these thicknesses.

[0056] The thermosetting sheet according to this embodiment preferably has a thermal conductivity of 3 W / m·K or more, and more preferably 10 W / m·K or more, after curing. When the thermal conductivity after curing is within the above range, the electrical conductivity of the thermosetting sheet after curing can be further increased. In the thermosetting sheet according to this embodiment, the upper limit of the thermal conductivity after curing is usually 100 W / m·K. The thermal conductivity after curing can be calculated by subjecting the thermosetting sheet according to this embodiment to heat curing at 200°C for 1 hour in a pressure cooker while applying a pressure of 0.5 MPa, and using the following formula for the heat-cured thermosetting sheet.

[0057]

number

[0058] In the above formula, thermal diffusivity (m 2 / s) can be measured by a TWA method (temperature wave thermal analysis, measuring device: iPhase Mobile, manufactured by iPhase Corporation). The specific heat (J / g°C) in the above formula can be measured by the DSC method. Specific heat measurement is performed using a DSC6220 manufactured by SII Nanotechnology, Inc., at a heating rate of 10°C / min and in the temperature range of 20 to 300°C. Based on the obtained data, the specific heat can be calculated using the method described in the JIS Handbook (specific heat capacity measurement method K-7123). Furthermore, the specific gravity in the above formula can be measured by Archimedes' method.

[0059] The thermosetting sheet according to the present embodiment may contain one or more other components as required, such as a filler dispersant, a flame retardant, a silane coupling agent, and an ion trapping agent.

[0060] [Dicing die bond film] Next, the dicing die bond film 20 will be described with reference to Fig. 1. In the following description, the description of the parts that overlap with the thermosetting sheet will not be repeated.

[0061] As shown in FIG. 1, the dicing die bond film 20 of this embodiment comprises a base layer 1, a dicing tape 10 having an adhesive layer 2 laminated on the base layer 1, and a thermosetting sheet 3 laminated on the adhesive layer 2 of the dicing tape 10. In the dicing die bond film 20, a semiconductor element is attached onto a thermosetting sheet 3. The semiconductor element may be a bare wafer. The bare wafer attached to the dicing die bond film 20 according to this embodiment is cleaved into a plurality of bare chips by blade dicing, DBG (Dicing Before Grinding), SDBG (Stealth Dicing Before Grinding), or the like. During the cleaving process, the thermosetting sheet 3 is also cleaved together with the bare wafer. The thermosetting sheet 3 is cleaved into pieces of a size corresponding to the size of the individual bare chips. This allows a plurality of bare chips with the thermosetting sheet 3 to be obtained.

[0062] As described above, the thermosetting sheet 3 of the dicing die bond film 20 is a thermosetting sheet containing a thermosetting resin, a thermoplastic resin, and conductive particles, and has an arithmetic mean roughness Ra measured in the pre-cured state of 0.1 μm or more and 1.2 μm or less.

[0063] The base layer 1 supports the adhesive layer 2 and the thermosetting sheet 3 laminated on the adhesive layer 2. The base layer 1 contains a resin. Examples of the resin include olefin-based resins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers; copolymers containing ethylene as a monomer component, such as ethylene-vinyl acetate copolymers (EVA), ionomer resins, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester (random, alternating) copolymers; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); acrylic resins; polyvinyl chloride (PVC); polyurethane; polycarbonate; polyphenylene sulfide (PPS); amide-based resins such as polyamide and fully aromatic polyamide (aramid); polyether ether ketone (PEEK); polyimide; polyetherimide; polyvinylidene chloride; ABS (acrylonitrile-butadiene-styrene copolymer); cellulose-based resins; silicone resins; and fluororesins. Among these, it is preferable to use polyethylene terephthalate.

[0064] The substrate layer 1 may contain one type of the above-mentioned resin, or may contain two or more types of the above-mentioned resin.

[0065] Materials for the base layer 1 include polymers such as crosslinked bodies of the resins (e.g., plastic films). The plastic films may be used without stretching, or may be uniaxially or biaxially stretched as necessary. When a resin sheet is provided with heat shrinkability by stretching or the like, the base layer 1 is heat-shrunk after dicing to reduce the adhesion area between the pressure-sensitive adhesive layer 2 and the thermosetting sheet 3, facilitating the recovery of the semiconductor chips (semiconductor elements).

[0066] The surface of the base layer 1 may be subjected to a general surface treatment in order to improve adhesion to adjacent layers, retention, etc. Examples of such surface treatments include chemical or physical treatments such as chromate treatment, ozone exposure, flame exposure, high-voltage shock exposure, and ionizing radiation treatment, as well as coating treatment with a primer.

[0067] The thickness of the base layer 1 is preferably from 1 μm to 1000 μm, more preferably from 10 μm to 500 μm, further preferably from 20 μm to 300 μm, and particularly preferably from 30 μm to 200 μm. The thickness of the base layer 1 can be determined using a dial gauge (Model R-205, manufactured by PEACOCK) in the same manner as the thickness of the thermosetting sheet 3 described above.

[0068] The base layer 1 may contain various additives, such as colorants, fillers, plasticizers, antioxidants, antioxidants, surfactants, and flame retardants.

[0069] The adhesive used to form the adhesive layer 2 is not particularly limited, and may be, for example, a general pressure-sensitive adhesive such as an acrylic adhesive or a rubber-based adhesive. As the pressure-sensitive adhesive, an acrylic adhesive having an acrylic polymer as a base polymer is preferred from the viewpoint of cleaning and washing properties with ultrapure water or organic solvents such as alcohol for electronic components that are sensitive to contamination, such as semiconductor wafers and glass.

[0070] Examples of the acrylic polymer include acrylic polymers using one or more of (meth)acrylic acid alkyl esters and (meth)acrylic acid cycloalkyl esters as monomer components. Examples of the (meth)acrylic acid alkyl esters include methyl esters, ethyl esters, propyl esters, isopropyl esters, butyl esters, isobutyl esters, s-butyl esters, t-butyl esters, pentyl esters, isopentyl esters, hexyl esters, heptyl esters, octyl esters, 2-ethylhexyl esters, isooctyl esters, nonyl esters, decyl esters, isodecyl esters, undecyl esters, dodecyl esters, tridecyl esters, tetradecyl esters, hexadecyl esters, octadecyl esters, eicosyl esters, and other linear or branched alkyl esters having 1 to 30 carbon atoms, particularly 4 to 18 carbon atoms, of the alkyl group. Examples of the (meth)acrylic acid cycloalkyl esters include cyclopentyl esters and cyclohexyl esters. The (meth)acrylic acid ester means at least one of an acrylic acid ester and a methacrylic acid ester, and all (meth) in the present invention have the same meanings as those described above.

[0071] The acrylic polymer may contain units corresponding to other monomer components copolymerizable with the (meth)acrylic acid alkyl ester or (meth)acrylic acid cycloalkyl ester, if necessary, for the purpose of modifying the cohesive strength, heat resistance, etc. Examples of such monomer components include carboxyl-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and 10-hydroxydecyl (meth)acrylate. Examples of the copolymerizable monomers include hydroxyl group-containing monomers such as 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, etc.; styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acryloyloxynaphthalenesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, etc.; phosphoric acid group-containing monomers such as 2-hydroxyethylacryloylphosphate, etc.; acrylamide, acrylonitrile, etc. These copolymerizable monomer components can be used alone or in combination. The amount of these copolymerizable monomers used is preferably 40% by mass or less of the total monomer components.

[0072] Furthermore, the acrylic polymer may contain a polyfunctional monomer as a copolymerization monomer component for crosslinking, if necessary. Examples of such polyfunctional monomers include hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy(meth)acrylate, polyester(meth)acrylate, and urethane(meth)acrylate. These polyfunctional monomers may be used alone or in combination. The amount of the polyfunctional monomer used is preferably 30% by mass or less of the total monomer components in terms of adhesion properties, etc.

[0073] The acrylic polymer can be obtained by polymerizing a single monomer or a mixture of two or more monomers. The polymerization may be carried out by any method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, etc. From the viewpoint of preventing contamination of clean adherends, it is preferable that the content of low molecular weight substances is small. From this viewpoint, the number average molecular weight of the acrylic polymer is preferably 300,000 or more, and more preferably about 400,000 to 3,000,000.

[0074] In addition, an external crosslinking agent can be appropriately added to the adhesive in order to increase the number average molecular weight of the base polymer, such as an acrylic polymer. Specific means for the external crosslinking method include a method of adding a crosslinking agent such as a polyisocyanate compound, an epoxy compound, an aziridine compound, or a melamine crosslinking agent and reacting it. When using an external crosslinking agent, the amount of the agent is appropriately determined in consideration of the balance with the base polymer to be crosslinked and the intended use as an adhesive. In general, the external crosslinking agent is preferably blended in an amount of about 5 parts by mass or less, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the base polymer.

[0075] In addition to the above components, the pressure-sensitive adhesive may contain various known additives such as a tackifier and an antiaging agent, if necessary.

[0076] The adhesive layer 2 can be formed from a radiation-curable adhesive. The degree of crosslinking of a radiation-curable adhesive can be increased by irradiation with radiation such as ultraviolet light, and the adhesive strength can be easily reduced. That is, by forming the adhesive layer 2 from a radiation-curable adhesive, the adhesive layer 2 can be sufficiently adhered to the thermosetting sheet 3 without being irradiated with radiation before dicing, and after dicing, the adhesive layer 2 can be irradiated with radiation to reduce the adhesive strength of the adhesive layer 2, allowing the semiconductor chip (semiconductor element) to be easily picked up (recovered).

[0077] The radiation curable adhesive can be used without any particular limitation as long as it has a radiation curable functional group such as a carbon-carbon double bond and exhibits adhesive properties. Examples of the radiation curable adhesive include additive-type radiation curable adhesives in which a radiation curable monomer component or oligomer component is blended with a general pressure-sensitive adhesive such as an acrylic adhesive or a rubber adhesive.

[0078] Examples of the radiation-curable monomer component include urethane (meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 1,4-butanediol di(meth)acrylate. Examples of the radiation-curable oligomer component include various oligomers such as urethane-based, polyether-based, polyester-based, polycarbonate-based, and polybutadiene-based oligomers, and those having a molecular weight in the range of about 100 to 30,000 are preferred. The amount of the radiation-curable monomer component or the radiation-curable oligomer component is preferably an amount that can suitably reduce the adhesive strength of the adhesive layer 2 after radiation irradiation. In general, the amount of the radiation-curable monomer component or the radiation-curable oligomer component is, for example, preferably 5 to 500 parts by mass, and more preferably 40 to 150 parts by mass, per 100 parts by mass of the base polymer, such as an acrylic polymer, that constitutes the pressure-sensitive adhesive.

[0079] In addition to the above-mentioned additive-type radiation-curable adhesives, examples of the radiation-curable adhesive include internal-type radiation-curable adhesives using a base polymer having a carbon-carbon double bond in the polymer side chain, in the main chain, or at the end of the main chain. The internal-type radiation-curable adhesive does not need to contain low molecular weight oligomer components or the like, or the content of the oligomer components or the like is relatively small. Therefore, when the internal-type radiation-curable adhesive is used, the oligomer components or the like are prevented from moving over time in the adhesive layer 2. As a result, the adhesive layer 2 can have a relatively stable layer structure.

[0080] The base polymer having a carbon-carbon double bond can be used without any particular limitation as long as it has a carbon-carbon double bond and has adhesiveness. As such a base polymer, it is preferable that the base polymer has an acrylic polymer as a basic skeleton. As the basic skeleton of the acrylic polymer, the above-mentioned acrylic polymer can be mentioned.

[0081] The method of introducing a carbon-carbon double bond into the acrylic polymer is not particularly limited, and various methods can be adopted, but the adoption of a method of introducing a carbon-carbon double bond into a polymer side chain makes molecular design easier. For example, a method of copolymerizing a monomer having a functional group with an acrylic polymer in advance, and then carrying out a condensation reaction or addition reaction with a compound having a functional group and a carbon-carbon double bond that can react with the functional group while maintaining the radiation curability of the carbon-carbon double bond can be mentioned.

[0082] Examples of combinations of these functional groups include a carboxylic acid group and an epoxy group, a carboxylic acid group and an aziridyl group, and a hydroxyl group and an isocyanate group. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferred from the viewpoint of ease of reaction tracking. In addition, as long as the combination of these functional groups produces an acrylic polymer having a carbon-carbon double bond, either of the functional groups may be on the acrylic polymer side or on the compound having a carbon-carbon double bond side. In the case of the above preferred combination, it is preferred that the acrylic polymer has a hydroxyl group and the compound having a carbon-carbon double bond has an isocyanate group. In this case, examples of the isocyanate compound having a carbon-carbon bond include methacryloyl isocyanate, 2-methacryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, and the like. As the acrylic polymer, a copolymer of the above-mentioned hydroxyl group-containing monomers or ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether can be used.

[0083] The inherent type radiation-curable adhesive can use the base polymer having a carbon-carbon double bond (particularly, an acrylic polymer) alone, but can also contain the radiation-curable monomer component or the radiation-curable oligomer component to the extent that the properties are not deteriorated. The radiation-curable oligomer component is usually contained in an amount of 30 parts by mass or less, and preferably 1 to 10 parts by mass or less, per 100 parts by mass of the base polymer.

[0084] The radiation-curable adhesive contains a photopolymerization initiator when curing with ultraviolet light or the like. Examples of the photopolymerization initiator include α-ketol-based compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-hydroxypropiophenone, and 1-hydroxycyclohexylphenylketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether-based compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; and ketal-based compounds such as benzyl dimethyl ketal. Examples of the photopolymerization initiator include aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates. The amount of the photopolymerization initiator is, for example, 0.05 to 20 parts by mass relative to 100 parts by mass of the base polymer such as an acrylic polymer constituting the adhesive.

[0085] Examples of radiation-curable adhesives include rubber-based adhesives and acrylic-based adhesives that contain a photopolymerizable compound, such as an addition-polymerizable compound having two or more unsaturated bonds or an alkoxysilane having an epoxy group, and a photopolymerization initiator, such as a carbonyl compound, an organic sulfur compound, a peroxide, an amine, or an onium salt compound, as disclosed in JP-A-60-196956.

[0086] In cases where curing is inhibited by oxygen during radiation irradiation, it is desirable to use some method to block oxygen (air) from the surface of the radiation-curable pressure-sensitive adhesive layer 2. Examples of such methods include a method of covering the surface of the pressure-sensitive adhesive layer 2 with a separator, and a method of irradiating the pressure-sensitive adhesive layer 2 with radiation such as ultraviolet light in a nitrogen gas atmosphere.

[0087] The thickness of the adhesive layer 2 is not particularly limited, but from the viewpoint of preventing chipping of the cut surface of the chip and at the same time maintaining the fixing and retention of the thermosetting sheet 3, it is preferably 1 to 50 μm, more preferably 2 to 30 μm, and even more preferably 5 to 25 μm.

[0088] [Semiconductor Devices] The semiconductor device of this embodiment comprises a substrate having a mounting area for a semiconductor element, and a semiconductor element mounted in the mounting area for the semiconductor element, the semiconductor element being mounted in the mounting area for the semiconductor element of the substrate via a thermosetting sheet, the thermosetting sheet being hardened, and the bonding rate of the thermosetting sheet to the substrate being 70% or more. In this specification, the bonding rate of a thermosetting sheet to a substrate means the ratio of the area of ​​the thermosetting sheet actually attached to the mounting area of ​​the semiconductor element to the total area of ​​the thermosetting sheet that will be attached to the mounting area of ​​the semiconductor element.

[0089] An example of the semiconductor device according to this embodiment is configured as shown in FIG. As shown in FIG. 2, the semiconductor device 30 includes a lead frame substrate 31 having a die pad 31a which is partitioned into an approximately rectangular shape when viewed from above, and a pair of lead portions 31b, 31b extending from both ends of the die pad 31a, a semiconductor element 32 which is attached to the die pad 31a of the lead frame substrate 31 while being laminated on a thermosetting sheet 3, a pair of wires 33, 33 which electrically connect the semiconductor element 32 to the pair of lead portions 31b, 31b, and a hollow package 34 which accommodates inside the entire die pad 31a, part of the pair of lead portions 31b, 31b, the entire semiconductor element 32 laminated on the thermosetting sheet 3, and the entire pair of wires 33, 33, and the gap between the semiconductor element 32 etc. and the package 34 is filled with molded resin 35. That is, in the semiconductor device 30 shown in FIG. 2, the lead frame substrate 31 is a substrate having a mounting area for a semiconductor element, and the die pad 31a is the mounting area for the semiconductor element.

[0090] In addition, in the semiconductor device 30, one end of a pair of lead portions 31b, 31b is arranged on the upper surface side of both ends of the die pad 31a, extends in a direction parallel to the upper surface of the die pad 31a (hereinafter also referred to as the horizontal direction), and then extends downward in a direction perpendicular to the upper surface of the die pad 31a (hereinafter also referred to simply as the vertical downward direction), and the horizontally extending portions of the pair of lead portions 31b, 31b penetrate the package 34. That is, in the semiconductor device 30, a portion of the horizontally extending portion of a pair of lead portions 31b, 31b is accommodated inside the package 34, and the remainder of the horizontally extending portion and the entire portion extending vertically downward are exposed to the outside of the package 34.

[0091] As shown in FIG. 2, the semiconductor device 30 is mounted on a wiring board 40 having a pair of electrodes 41, 41 spaced apart from each other on its surface. More specifically, the semiconductor device 30 is attached to a wiring board 40 by joining a portion of the vertically downward extending portions of a pair of lead portions 31b, 31b to a pair of electrodes 41, 41, respectively, using solder or the like.

[0092] In the semiconductor device according to this embodiment, the bonding rate of the thermosetting sheet to the substrate is preferably 80% or more, and more preferably 90% or more. Furthermore, in the semiconductor device according to this embodiment, the bonding rate of the thermosetting sheet to the substrate before curing is preferably 70% or more, more preferably 80% or more, and particularly preferably 90% or more. Furthermore, in the semiconductor device according to this embodiment, the bonding rate of the thermosetting sheet to the lead frame substrate having the die pad is preferably 70% or more, more preferably 80% or more, and particularly preferably 90% or more. Furthermore, in the semiconductor device of this embodiment, the bonding rate of the thermosetting sheet before curing to the lead frame substrate having the die pad is preferably 70% or more, more preferably 80% or more, and particularly preferably 90% or more.

[0093] In the semiconductor device according to this embodiment, as described above, the thermosetting sheet is a thermosetting sheet containing a thermosetting resin, a thermoplastic resin, and conductive particles, and has an arithmetic mean roughness Ra measured in an uncured state of 0.1 μm or more and 1.2 μm or less.

[0094] The bonding ratio of the thermosetting sheet to the substrate can be determined according to the following procedure. (1) A test specimen for evaluating the bonding rate is obtained by attaching one surface of a thermosetting sheet (or a laminate of multiple thermosetting sheets) having a silicon chip (bare chip) attached to the other surface of the sheet to a semiconductor element mounting area of ​​a substrate having the semiconductor element mounting area. (2) Using an ultrasonic imaging device (manufactured by Hitachi Construction Machinery Finetech Co., Ltd., model: FineSAT FS200II, hereinafter also referred to as SAT), the specimen for evaluation of the bonding rate is imaged by a reflection method to obtain an SAT image. The imaging is performed by adjusting the gate so as to match the echo of the bonding portion between the substrate and the thermosetting sheet displayed on the waveform monitor of the ultrasonic imaging device, setting the pixel to 1, the gain to 25 dB, and the Z-axis height to 11.34 mm. (3) Using the image analysis software ImageJ, the obtained SAT image is subjected to an automatic binarization process to binarize the bonded portion between the substrate and the thermosetting sheet (hereinafter also referred to as the bonded portion) and the non-bonded portion between the substrate and the thermosetting sheet (hereinafter also referred to as the non-bonded portion). The threshold value is set to 82. (4) From the binarized image, the area of ​​the bonded parts and the area of ​​the non-bonded parts are calculated, the value of the area of ​​the bonded parts is divided by the sum of the area of ​​the bonded parts and the area of ​​the non-bonded parts, and then multiplied by the number 100 to calculate the bonding rate of the thermosetting sheet to the substrate. In the binarized image, the joints are shown in black, and the non-joints are shown in white.

[0095] The thermosetting sheet, dicing die bond film, and semiconductor device according to the present invention are not limited to the above-mentioned embodiment. The thermosetting sheet, dicing die bond film, and semiconductor device according to the present invention are not limited by the above-mentioned action and effect. The thermosetting sheet, dicing die bond film, and semiconductor device according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES

[0096] The present invention will now be described in more detail with reference to examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.

[0097] [Example 1] A mixture containing each material in the mass ratio shown in the Example 1 section of Table 1 below was stirred and mixed in "stirring mode" using a hybrid mixer (manufactured by Keyence Corporation, product name: HM-500) to prepare a varnish. The stirring and mixing using the hybrid mixer was performed in three stages. Specifically, first, a primary mixture containing a thermosetting resin and a thermoplastic resin was stirred and mixed for 3 minutes (primary stirring), then, a secondary mixture obtained by adding conductive particles and a volatile material to the primary mixture was stirred and mixed for 6 minutes (secondary stirring), and further, a tertiary mixture obtained by adding a catalyst and a solvent to the secondary mixture was stirred and mixed for 3 minutes (tertiary stirring). This varnish was applied to one side of a release-treated film (manufactured by Mitsubishi Chemical Corporation, product name: MRA38, thickness 38 μm) and then dried at a temperature of 100° C. for 2 minutes to obtain a thermosetting sheet with a thickness of 30 μm. The materials used in the following Table 1 are as follows: Phenolic resin MEHC-7851S (biphenyl-type phenolic resin, phenol equivalent: 209 g / eq) manufactured by Meiwa Kasei Co., Ltd. Solid epoxy resin Nippon Steel & Sumikin Chemical's KI-3000-4 (cresol novolac type multifunctional epoxy resin, epoxy equivalent 200g / eq) Liquid epoxy resin DIC EXA-4816 (aliphatic modified bisphenol A type epoxy resin (bifunctional type), epoxy equivalent 403g / eq) ·Silver (Ag) coated copper (Cu) particles DOWA Electronics' product name: AOP-TCY-2(EN) (Spherical copper particles coated with 20% by mass of silver particles. The particle shape is spherical.) ·Silver (Ag) particles AG-2-8F manufactured by DOWA Electronics (silver particles surface-treated with a fatty acid-based coating agent. The particles are spherical.) · Volatile material (isobornylcyclohexanol (MTPH)) MTPH manufactured by Nippon Terpene Chemical Acrylic resin solution Nagase Chemitec's Teisan Resin SG-70L (contains MEK and toluene as solvents, solids content 12.5%, glass transition temperature -13°C, mass average molecular weight 900,000, acid value 5mg / KOH, carboxyl group-containing acrylic copolymer) Coupling Agent Shin-Etsu Chemical Co., Ltd.'s KBE-846 (bis(triethoxysilylpropyl)tetrasulfide) ·catalyst TPP-K (Tetraphenylphosphonium tetraphenylborate) manufactured by Hokko Chemical Industry Co., Ltd. ·solvent Methyl ethyl ketone (MEK) The mass ratio of silver-coated copper particles and silver particles in 100 parts by mass of the conductive particles (silver-coated copper particles and silver particles) is shown in Table 3 below. % Mass of epoxy resin (solid and liquid) % , 100 mass of thermosetting sheet % Mass of phenolic resin in % , The mass% of thermosetting resin (epoxy resin (solid and liquid), phenolic resin) in 100% by mass of the thermosetting sheet, 100 mass of thermosetting sheet % Mass of acrylic resin in % , and 100 mass of organic components (phenolic resin, epoxy resin (solid and liquid), acrylic resin solution, isobornylcyclohexanol) % Mass of isobornylcyclohexanol in % The details are shown in Table 2 below. In addition, since the circularity of the silver-coated copper particles (AOP-TCY-2(EN)) and the silver particles (AG-2-8F) measured by the above-mentioned method was 70% or more, the particle shapes of the silver-coated copper particles and the silver particles are described as "spherical."

[0098] [Example 2] A thermosetting sheet according to Example 2 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 2 in Table 1 below was obtained.

[0099] [Example 3] A thermosetting sheet according to Example 3 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 3 in Table 1 below was obtained.

[0100] [Example 4] A thermosetting sheet according to Example 4 was obtained in the same manner as in Example 1, except that silver particles were HP02-B (silver particles surface-treated with an epoxy-based coating agent, spherical particle shape) manufactured by Mitsui Smelting Co., Ltd., and a mixture containing each material was obtained in the mass ratio shown in the section on Example 4 in Table 1 below. In addition, since the circularity of HP02-B measured by the above-mentioned method was 70% or more, the particle shape is described as spherical.

[0101] [Example 5] A thermosetting sheet of Example 5 was obtained in the same manner as in Example 1, except that the silver particles were HP02-B manufactured by Mitsui Mining & Smelting Co., Ltd., and a mixture containing each material was obtained in the mass ratio shown in the Example 5 section of Table 1 below.

[0102] [Example 6] The silver-coated copper particles were prepared by coating 20% ​​by mass of silver particles on 1200Y manufactured by Mitsui Mining & Smelting Co., Ltd. (surface-treated with a fatty acid-based coating agent; spherical particle shape; hereinafter also referred to as 20% Ag / 1200Y). A thermosetting sheet according to Example 6 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 6 in Table 1 below was obtained. In addition, since the circularity of 20% Ag / 1200Y measured by the above-mentioned method was 70% or more, the particle shape is described as spherical.

[0103] [Example 7] The silver-coated copper particles were prepared by coating 20% ​​by mass of silver particles on MA-C03K manufactured by Mitsui Mining & Smelting Co., Ltd. (surface-treated with a fatty acid-based coating agent; spherical particle shape; hereinafter also referred to as 20% Ag / 03K). A thermosetting sheet of Example 7 was obtained in the same manner as in Example 1, except that a mixture containing each material was obtained in the mass ratio shown in the section of Example 7 in Table 1 below. In addition, since the circularity of 20% Ag / 03K measured by the above-mentioned method was 70% or more, the particle shape is described as spherical.

[0104] [Comparative Example 1] The silver-coated copper particles were 1200YP manufactured by Mitsui Mining & Smelting Co., Ltd., coated with 10% silver by mass (surface-treated with an epoxy-based coating agent; flat particle shape; hereinafter also referred to as 10% Ag / 1200YP-B), the silver particles were HP02A manufactured by Mitsui Mining & Smelting Co., Ltd. (surface-treated with a fatty acid-based coating agent; spherical particle shape), and a mixture containing each material in the mass ratio shown in the section for Comparative Example 1 in Table 1 below was obtained in the same manner as in Example 1, to obtain a thermosetting sheet of Comparative Example 1. In addition, since the circularity of HP02A measured by the above-mentioned method was 70% or more, the particle shape is described as spherical.

[0105] [Comparative Example 2] A thermosetting sheet according to Comparative Example 2 was obtained in the same manner as in Example 1, except that the silver-coated copper particles were 1200YP manufactured by Mitsui Mining & Smelting Co., Ltd., which was coated with 10% silver particles (10% Ag / 1200YP-B), the silver particles were HP02A-B manufactured by Mitsui Mining & Smelting Co., Ltd. (surface-treated with an epoxy-based coating agent; spherical particle shape), and a mixture containing each material in the mass ratio shown in the section for Comparative Example 2 in Table 1 below was obtained. In addition, since the circularity of HP02A-B measured by the above-mentioned method was 70% or more, the particle shape is described as spherical.

[0106] [Comparative Example 3] A thermosetting sheet according to Comparative Example 3 was obtained in the same manner as in Example 1, except that the silver-coated copper particles were 1200YP manufactured by Mitsui Mining & Smelting Co., Ltd., which was coated with 10% silver particles (10% Ag / 1200YP-B), the silver particles were HP02A-B manufactured by Mitsui Mining & Smelting Co., Ltd. (surface-treated with an epoxy-based coating agent; spherical particle shape), and a mixture containing each material in the mass ratio shown in the section for Comparative Example 2 in Table 1 below was obtained.

[0107] [Table 1]

[0108] [Table 2]

[0109] <Volume average particle size D of silver particles and silver-coated copper particles 50 and D. 90 > Before blending, the particle size distribution was measured using a laser diffraction / scattering particle size distribution measuring device (Microtrac-Bell, Microtrac MT3000II series). The volume average particle diameter D of the silver particles and silver-coated copper particles contained in the heat-cured sheets according to each example 50 and D. 90 The results of the measurements are shown in Table 3 below.

[0110] <Conductive particle filling rate> The particle packing ratio P was determined for the thermosetting sheet according to each example according to the following procedure. (1) The cured thermosetting sheet is mechanically polished to expose a cross section, and the exposed cross section is subjected to ion polishing using an ion polishing device (manufactured by JEOL Ltd., product name: Cross Section Polisher SM-09010). (2) An SEM image (image taken by a scanning electron microscope) of an arbitrary cross-sectional area of ​​the exposed cross-section that has been ion-polished is taken using a field emission scanning electron microscope SU8020 (manufactured by Hitachi High-Technologies Corporation), and a backscattered electron image is obtained as image data. The imaging conditions are an acceleration voltage of 5 kV and a magnification of 5000 times. (3) The obtained image data is subjected to automatic binarization processing using the image analysis software ImageJ to binarize the metal parts and the resin parts. (4) The total area of ​​the metal parts and the total area (metal parts + resin parts) are calculated from the binarized image, and the total area of ​​the metal parts is divided by the total area to calculate the particle filling rate P of the conductive particles for the cured thermosetting sheet. The particle packing ratio P of the conductive particles was determined by arithmetically averaging the particle packing ratios determined for five cross-sectional regions on the exposed cross-section that had been ion-polished. The particle filling rate P of the conductive particles was determined for each of the thermosetting sheets according to the examples, and the results are shown in Table 3 below.

[0111] <Thermal conductivity of thermosetting sheets> The thermosetting sheet according to each example was heat-cured in a pressure cooker at 200° C. for 1 hour while applying a pressure of 0.5 MPa. The thermal conductivity of the heat-cured thermosetting sheet according to each example was calculated according to the following formula.

[0112]

number

[0113] Thermal diffusivity α(m 2 / s) was measured by the TWA method (temperature wave thermal analysis, measuring device: iPhase Mobile, manufactured by iPhase Corporation). Specific heat C p The specific heat capacity (J / g·°C) was measured by the DSC method. Specific heat measurements were performed using a DSC6220 manufactured by SII Nanotechnology, Inc., at a heating rate of 10°C / min and in the temperature range of 20 to 300°C. Based on the data obtained, the specific heat was calculated using the method described in the JIS Handbook (specific heat capacity measurement method K-7123). The specific gravity was measured by the Archimedes method. The thermal conductivity of the cured thermosetting sheets of each example was calculated and the results are shown in Table 3 below.

[0114] <Arithmetic mean roughness Ra and maximum height roughness Rz> For the thermosetting sheet according to each example, the arithmetic mean roughness Ra and maximum height roughness Rz were measured before curing. Specifically, before curing, the roughness curve of the surface of the thermosetting sheet of each example was measured using a Lasertec 3CDD color confocal microscope (model OPTELICS H3000) and control software LM eye using a non-contact roughness measurement method with a cutoff value of 0.08 mm. In the non-contact roughness measurement method, the microscope was operated under conditions where the observation magnification was set to 500 times and the resolution was set to 0.05 μm. The arithmetic mean roughness Ra and maximum height roughness Rz are both defined in JIS B0601:2013.

[0115] <Joining rate> For each of the thermosetting sheets according to the examples, the bonding rate to the substrate was measured. When measuring the bonding rate, the thermosetting sheet of each example was cut into a 5 cm square, 10 of the 5 cm square thermosetting sheets were stacked together, and then pressed under vacuum (pressure of 3.3 kPa) to obtain a sheet laminate with a thickness of 300 μm. A bare chip diced into a 5 cm square was attached to one side of the sheet laminate to produce a sheet laminate with bare chips. The bonding rate to the substrate was measured according to the following procedure. (1) A sheet laminate having a bare chip attached to one surface thereof is attached to the other surface thereof on a die pad of a lead frame substrate (Cu lead frame substrate) to obtain a test specimen for evaluating a bonding rate. (2) Using an ultrasonic imaging device (manufactured by Hitachi Construction Machinery Finetech Co., Ltd., model: FineSAT FS200II, hereinafter also referred to as SAT), the test specimen for evaluating the bonding rate is imaged by a reflection method to obtain an SAT image. The imaging is performed by adjusting the gate so as to match the echo of the bonding portion between the thermosetting sheet and the test specimen displayed on the waveform monitor of the ultrasonic imaging device, setting the pixel to 1, the gain to 25 dB, and the Z-axis height to 11.34 mm. (3) Using image analysis software ImageJ, the obtained SAT image is subjected to automatic binarization processing to binarize the joint portion between the lead frame substrate and the sheet laminate (hereinafter also simply referred to as the joint portion) and the non-joint portion between the lead frame substrate and the sheet laminate (hereinafter also simply referred to as the non-joint portion). The threshold value is set to 82. (4) From the binarized image, the area of ​​the bonded portions and the area of ​​the non-bonded portions are calculated, and the area of ​​the bonded portions is divided by the sum of the area of ​​the bonded portions and the area of ​​the non-bonded portions. Then, the resulting area is multiplied by the number 100 to calculate the bonding rate of the sheet laminate (the thermosetting sheet abutting against the lead frame substrate) to the lead frame substrate. In the binarized image, the joints are shown in black, and the non-joints are shown in white.

[0116] The bonding rate of the thermosetting sheet according to each example to the substrate (lead frame substrate) was measured, and the results are shown in Table 3 below.

[0117] [Table 3]

[0118] It can be seen from Table 3 that the thermosetting sheets according to each Example all had an arithmetic mean roughness Ra measured before curing in the range of 0.1 μm or more and 1.2 μm or less. After curing, the thermosetting sheets of each Example all exhibited a relatively high thermal conductivity of 3 W / m K or more, and before curing, the bonding rate to the lead frame substrate was 70% or more. In addition, the maximum height roughness Rz of the thermosetting sheets according to each Example, measured before curing, was in the range of 1 μm or more and 12 μm or less.

[0119] In contrast, it was found that the arithmetic mean roughness Ra measured before curing for each of the thermosetting sheets according to the comparative examples was not within the range of 0.1 μm or more and 1.2 μm or less. After curing, the thermosetting sheets according to each of the comparative examples all had a relatively high thermal conductivity of 3 W / m K or more, but these values ​​were lower than those of the thermosetting sheets according to each of the examples. Moreover, the thermosetting sheets according to the respective comparative examples all had a bonding rate to the lead frame substrate of less than 70% before curing. In addition, in each of the thermosetting sheets according to the comparative examples, the maximum height roughness Rz measured before curing was not within the range of 1 μm or more and 12 μm or less.

[0120] These results show that by making the thermosetting sheet contain a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles, and further making the arithmetic mean roughness Ra measured in the pre-cured state fall within the range of 0.1 μm or more and 1.2 μm or less, it is possible to improve the adhesion to the substrate having the mounting area for the semiconductor element in the temporarily attached state, and to make the thermal conductivity after curing relatively high. [Explanation of symbols]

[0121] 1 Base material layer 2 Adhesive layer 3 Thermosetting Sheet 10 Dicing tape 20 Dicing die bond film 30 Semiconductor Devices 31 Lead frame substrate 32 Semiconductor elements 33 Wire 34 Packages 35 Molding resin 40 Wiring board 41 electrode 31a Die pad 31b Lead section.

Claims

1. The composition includes a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles, The content of the thermosetting resin is 1% by mass or more and 30% by mass or less, The content of the thermoplastic resin is 0.5% by mass or more and 10% by mass or less, The content of the volatile component is 5% by mass or more and 50% by mass or less with respect to the total mass of the thermosetting resin, the thermoplastic resin, and the volatile component, The arithmetic mean roughness Ra measured before curing is 0.1 μm or more and 1.2 μm or less. Thermosetting sheet.

2. The content of the thermosetting resin is 1.48 mass% or more and 4.07 mass% or less. The thermosetting sheet according to claim 1 .

3. The conductive particles include silver particles, The silver particles have a volume average particle diameter D 90 of 0.5 μm or more and 5 μm or less. The thermosetting sheet according to claim 1 or 2.

4. A composition comprising a thermosetting resin, a thermoplastic resin, a volatile component, and conductive particles, the conductive particles include silver particles; The silver particles have a volume average particle diameter D 90 of 0.5 μm or more and 5 μm or less, The arithmetic mean roughness Ra measured before curing is 0.1 μm or more and 1.2 μm or less. Thermosetting sheet.

5. The maximum height roughness Rz measured before curing is 1 μm or more and 12 μm or less. The thermosetting sheet according to claim 1 .

6. The particle filling rate P of the conductive particles in the thermosetting sheet after curing is 30 volume % or more. The thermosetting sheet according to claim 1 .

7. Thermal conductivity after curing is 3W / mK or more The thermosetting sheet according to any one of claims 1 to 6.

8. A base layer; a dicing tape having a pressure-sensitive adhesive layer laminated on the base layer; a thermosetting sheet laminated on the pressure-sensitive adhesive layer of the dicing tape; The thermosetting sheet is the thermosetting sheet according to any one of claims 1 to 7. Dicing die bond film.

9. a substrate having a mounting area for a semiconductor element; a semiconductor element mounted in the semiconductor element mounting area; the semiconductor element is mounted on a mounting area of ​​the substrate for the semiconductor element via a thermosetting sheet, the thermosetting sheet is cured, The bonding rate of the thermosetting sheet to the substrate is 70% or more; The thermosetting sheet is the thermosetting sheet according to any one of claims 1 to 7. Semiconductor device.

Citation Information

Patent Citations

  • Semiconductor device manufacturing method, bonding sheet used therein, and semiconductor device attained therewith

    JP2006114586A

  • Thermosetting die bond film, die bond film with dicing sheet method for manufacturing thermosetting die bond film and method for manufacturing semiconductor device

    JP2015103580A

  • Dicing / die-bonding film and film-like adhesive for thermosetting die-bonding film

    JP2019021813A

  • Semiconductor device manufacturing method

    JP2020107711A