Optical items

By incorporating specific silica particle sizes and a resin matrix with ethylenically unsaturated bonds, the optical article achieves improved hardness and adhesion, addressing the limitations of conventional optical articles.

JP7570920B2Active Publication Date: 2024-10-22JGC CATALYSTS & CHEMICALS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020219025
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-10-22
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Conventional optical articles with plastic base materials, primer layers, and hard coat layers lack sufficient hardness, particularly on the hard coat layer side, and face issues with adhesion between these layers.

Method used

The optical article comprises a plastic base material with a primer layer containing silica particles of 20 to 100 nm and a hard coat layer with silica particles of 3 to 20 nm, where the particle diameter ratio is 2.5 to 20, and uses a resin matrix with ethylenically unsaturated bonds for improved adhesion and hardness.

Benefits of technology

The solution results in an optical article with enhanced hardness, excellent adhesion, and transparency, while maintaining the appearance and adhesion between the plastic base material and the primer and hard coat layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570920000001
    Figure 0007570920000001
  • Figure 0007570920000002
    Figure 0007570920000002
  • Figure 0007570920000003
    Figure 0007570920000003
Patent Text Reader

Abstract

To provide an optical article that includes a plastic base material, primer layer and hard coating layer, and is high in rigidity.SOLUTION: An optical article comprises: a plastic base material; a primer layer; and a hard coating layer. The primer layer includes a resin matrix and a silica particle 1 in which an average particle diameter is 20 to 100nm, and the hard coating layer includes a silica-based matrix, and a silica particle 2 in which the average particle diameter is 3 to 20nm. In the optical article, the average particle diameter of the silica particle 1 / the average particle diameter of the silica particle 2 is 2.5 to 20.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical article, such as an optical lens, which comprises a plastic substrate and a primer layer containing silica particles and a hard coat layer. [Background technology]

[0002] In recent years, plastic substrates have come to be used primarily as optical lens materials, replacing inorganic glass substrates, due to the superiority of plastic substrates in impact resistance, processability, dyeability, etc.

[0003] As the plastic substrate for optical lenses, a substrate made of polycarbonate resin has been mainly used because of its high transparency, but because it is easily scratched, a hard coat layer is provided on the surface to prevent scratching. In addition, since the hard coat layer does not adhere well to the plastic substrate, a primer layer is provided between them to improve adhesion.

[0004] Such optical articles comprising a plastic substrate, a primer layer and a hard coat layer are disclosed in many documents such as Patent Documents 1 and 2. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-150309 A [Patent Document 2] International Publication No. 2007 / 026529 Summary of the Invention [Problem to be solved by the invention]

[0006] However, conventional optical articles including a plastic substrate, a primer layer, and a hard coat layer have room for further improvement in terms of hardness (hardness of the surface on the hard coat layer side). In view of the above problems, an object of the present invention is to provide an optical article having high hardness (particularly pencil hardness) comprising a primer layer and a hard coat layer on a plastic substrate. [Means for solving the problem]

[0007] The present invention relates to, for example, the following [1] to [4]. [1] An optical article comprising a plastic substrate, a primer layer provided on at least a portion of a surface of the plastic substrate, and a hard coat layer provided on a surface of the primer layer opposite to the plastic substrate, the primer layer comprises a resin matrix and silica particles 1 having an average particle diameter of 20 to 100 nm measured by a dynamic light scattering method and determined by a cumulite analysis method; the hard coat layer comprises a silica-based matrix and silica particles 2 having an average particle diameter of 3 to 20 nm measured by a dynamic light scattering method and determined by a cumulite analysis method; the ratio of the average particle size of the silica particles 1 to the average particle size of the silica particles 2 is 2.5 to 20; Optical articles.

[0008] [2] The optical article according to [1] above, wherein the resin matrix is ​​formed from a polyurethane having an ethylenically unsaturated bond-containing group.

[0009] [3] The optical article according to [1] or [2] above, wherein the resin matrix has an elongation within a range of 150 to 200% as measured in accordance with JIS K7161.

[0010] [4] The optical article according to any one of the above [1] to [3], wherein the plastic substrate is a polycarbonate resin substrate, a polyamide resin substrate or a polycellulose resin substrate. Effect of the Invention

[0011] The optical article according to the present invention has high hardness. The optical article according to the present invention is also excellent in appearance (transparency) and adhesion between the plastic substrate and the primer layer and between the plastic substrate and the hard coat layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The optical article according to the present invention will now be described in further detail. The optical article of the present invention comprises a plastic substrate, a primer layer provided on a surface of the plastic substrate, and a hard coat layer provided on the surface of the primer layer opposite the plastic substrate, and there is a predetermined relationship between the particle size of the silica particles contained in the primer layer and the particle size of the silica particles contained in the hard coat layer.

[0013] The optical article according to the present invention can be produced, for example, by forming a primer layer on the surface of the plastic substrate from a paint for forming a primer layer, and then forming a hard coat layer on the surface of the primer layer opposite the plastic substrate from a paint for forming a hard coat layer.

[0014] First, the paint for forming the primer layer and the paint for forming the hard coat layer will be described in detail. [Paint for forming primer layer] The primer layer forming paint may be, for example, a primer layer forming paint composition (hereinafter also referred to as "primer paint composition") containing (A) a resin matrix forming component, (B) silica particles 1, (C) a solvent, and optionally (D) an additive (hereinafter also referred to as component (A), component (B), component (C), and component (D), respectively). As the primer layer forming paint composition, a conventionally known one may be used.

[0015] Each component will be described in detail. (A) Resin matrix forming component Resin matrix-forming component (A) includes, for example, polyurethanes and polyesters, with polyurethanes being preferred.

[0016] The polyurethane may be used in the form of a one-component or two-component urethane paint, a water-based polyurethane dispersion, or the like, and among these, a water-based polyurethane dispersion (polyurethane particles dispersed in water) is preferred.

[0017] Among the aqueous polyurethane dispersions, self-emulsifying polyurethane emulsions are preferred. The average particle size of the emulsion particles is preferably 80 nm or less. The water-based polyurethane dispersion is preferably anionic.

[0018] The polyurethane contained in the aqueous polyurethane dispersion is preferably emulsion particles of polyurethane having an ethylenically unsaturated bond-containing group, from the viewpoint of obtaining an optical article having high hardness.

[0019] The ethylenically unsaturated bond-containing group is preferably a (meth)acryloyl group, more preferably an acryloyl group. As the resin matrix-forming component (A), a component conventionally known for forming a resin matrix of a primer layer, such as the polyurethane resin described in JP-A-6-337376 and the anionic emulsion fine particles of a polycarbonate-based polyurethane compound having a crosslinked structure described in JP-A-2011-99074, may be used.

[0020] The elongation of the film formed from the resin matrix-forming components, measured in accordance with JIS K7161, is preferably in the range of 150 to 200%. When the elongation is in the above range, an optical article with high hardness can be produced. Examples of commercially available aqueous polyurethane dispersions include NeoPac R-9699 manufactured by Kusumoto Chemical Industries, Ltd. and Superflex 110 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.

[0021] (B) Silica particle 1 The silica particles 1 are silica particles whose average particle diameter measured by dynamic light scattering and determined by cumulant analysis is in the range of 20 to 100 nm, preferably 20 to 90 nm.

[0022] By using silica particles 1 having an average particle size in the above range, it is possible to manufacture optical articles having high hardness and high transparency. On the other hand, if the average particle size is below the lower limit, the silica particles are less likely to withstand the impact or pressure on the optical article, and the hardness of the optical article is thought to decrease. Also, if the average particle size is above the upper limit, the dispersibility of the silica particles is reduced when the primer layer forming coating composition is applied to a plastic substrate, and the hardness of the optical article is thought to decrease.

[0023] The silica particles 1 may be particles made of only silica (however, unavoidable impurities may be contained), or may be particles made of an oxide of silicon and at least one metal element M selected from the group consisting of Ti, Fe, Zn, W, Sn, Ta, Zr, Sb, Nb, In, Ce, Al, Y, Pb, and Mo. The amount of this metal element M is preferably small enough not to impair the effects of the present invention, and is, for example, 1.5% by mass or less, preferably 1.4% by mass or less in terms of the oxide of metal element M in the silica particles 1.

[0024] Specific examples of commercially available spherical silica particles 1 include Cataloid (registered trademark) SI-50, SI-45P, and SI-80P (all manufactured by JGC Catalysts and Chemicals, in the form of silica sol).

[0025] Examples of the non-spherical (for example, irregular, linked, chain-like) silica particles 1 include those produced by a conventionally known method described in JP-A-2005-186435 and the like. The silica particles 1 are preferably silica particles that have not been surface-treated.

[0026] (C) Solvent The solvent (C) is water and / or an organic solvent, and preferably contains water. The organic solvent may be Alcohols such as methanol, ethanol, 1-propanol, 2-propanol, butanol, diacetone alcohol, furfuryl alcohol, tetrahydrofurfuryl alcohol, ethylene glycol, hexylene glycol, and isopropyl glycol; Esters such as methyl acetate, ethyl acetate, and butyl acetate; Ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol isopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether: Ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone etc. can be used. These may be used alone or in combination of two or more.

[0027] (D) Additives The primer layer-forming coating composition may contain an additive (D) (hereinafter also referred to as "component (D)") that may be normally contained in a primer layer-forming coating. Examples of the additive (D) include surfactants, and other examples include ultraviolet absorbers, light stabilizers, antioxidants, crosslinking agents, and colorants (dyes, pigments, etc.).

[0028] Proportion of each ingredient The ratio of each component in the primer layer-forming coating composition is appropriately adjusted so that the ratio of the silica particles 1 in the primer layer falls within the range described below.

[0029] [Hard coat layer forming paint] The coating material for forming a hard coat layer includes, for example, a coating composition for forming a hard coat layer (hereinafter also referred to as "hard coat coating composition") containing (E) a silica-based matrix forming component, (F) silica particles 2, (G) a solvent, and optionally (H) an additive (hereinafter also referred to as component (E), component (F), component (G), and component (H), respectively).

[0030] Each component will be described in detail. (E) Silica-based matrix-forming component Examples of the silica-based matrix-forming component (E) include organosilicon compounds contained in paints for forming a hard coat layer that are conventionally known as components for forming the silica-based matrix of the hard coat layer, such as the organosilicon compounds described in

[0022] to

[0030] of JP2009-197078A.

[0031] More specifically, the organosilicon compound includes at least one component selected from the group consisting of organosilicon compounds represented by the following general formula (I) (hereinafter also referred to as "organosilicon compound (e)"), their hydrolysates, and partial condensates of the hydrolysates.

[0032] R 1 R 2 a Si(OR 3 ) 3-a …(I) In formula (I), R 1 represents an organic group having a vinyl group, an epoxy group or a methacryloxy group, and preferably an organic group having an epoxy group. The number of carbon atoms in the organic group is preferably 8 or less, and more preferably 6 or less.

[0033] R 2 represents a hydrocarbon group having 1 to 4 carbon atoms. R 3 represents a hydrocarbon group having 1 to 8 carbon atoms, an alkoxyalkyl group having 8 or less carbon atoms, or an acyl group having 8 or less carbon atoms.

[0034] a represents 0 or 1. The organic silicon compound (e) is typically an alkoxysilane compound, and specific examples thereof include vinyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, α-glycidoxymethyltrimethoxysilane, α-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltriethoxysilane, and the like. Among these, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, and the like are preferred. These compounds may be used alone or in combination of two or more.

[0035] The hydrolysate of the organosilicon compound (e) and the partial condensate of the hydrolysate are respectively those obtained by partially hydrolyzing or hydrolyzing the organosilicon compound (e) in the absence of a solvent or in a polar organic solvent such as alcohol (e.g., methanol) in the presence of an acid and water (e.g., hydrochloric acid), and those obtained by further partially condensing the hydrolysate. A part or all of these organic solvents and water may be used as the solvent (G) described below when preparing the coating composition for forming a hard coat layer.

[0036] When the silica particles 2 (F) are blended as a silica sol described below in preparing the coating composition for forming a hard coat layer, the hydrolysis and / or partial condensation may be carried out in a state in which the organosilicon compound (e) is mixed with the sol of the silica particles 2 (F) or may be carried out before mixing.

[0037] (F) Silica particle 2 The silica particles 2 are silica particles having an average particle size in the range of 3 to 20 nm, preferably 4 to 15 nm, measured by dynamic light scattering and calculated by cumulant analysis.

[0038] The silica particles 2 may be particles made of only silica (however, they may contain unavoidable impurities), or may be particles made of an oxide of silicon and at least one metal element M selected from the group consisting of Ti, Fe, Zn, W, Sn, Ta, Zr, Sb, Nb, In, Ce, Al, Y, Pb, and Mo. The amount of this metal element M is preferably small enough not to impair the effects of the present invention, and is, for example, 1.5% by mass or less, preferably 1.4% by mass or less in terms of the oxide of the metal element M in the silica particles 2.

[0039] The silica particles 2 can be produced by a conventional method described in, for example, JP 2009-197078 A. Specific examples of commercially available products of the silica particles 2 include Cataloid SI-550, SI-30, and SI-40 (all manufactured by JGC Catalysts and Chemicals, in the form of silica sol). The silica particles 2 are preferably silica particles whose surfaces have been treated with a silane coupling agent or the like.

[0040] (G) Solvent Specific examples of the solvent (G) include the solvents given as specific examples of the solvent (C).

[0041] (H) Additives The coating composition for forming a hard coat layer may contain an additive (H) (hereinafter also referred to as "component (H)") that can be usually contained in a coating composition for forming a hard coat layer. Examples of the additive (H) include a curing agent, a surfactant, an ultraviolet absorber, a light stabilizer, an antioxidant, and a colorant (dye, pigment, etc.).

[0042] Examples of the curing agent include curing agents that can be contained in conventionally known coating materials for forming a hard coat layer, such as the curing agents described in

[0033] to

[0036] of JP-A-2009-197078.

[0043] Proportion of each ingredient The ratio of each component in the coating composition for forming a hard coat layer is appropriately adjusted so that the ratio of the silica particles 2 in the hard coat layer falls within the range described below.

[0044] [Optical articles] The optical article (for example, an optical lens such as a spectacle lens, or an optical film) according to the present invention comprises a plastic substrate, a primer layer, and a hard coat layer.

[0045] The primer layer is provided on at least a portion of the surface of the plastic substrate. For example, the primer layer may be provided on one surface of the plate- or film-shaped plastic substrate, or on both surfaces of the plastic substrate.

[0046] The hard coat layer is provided on the surface of the primer layer opposite to the plastic substrate. The optical article according to the present invention may further include an optional layer such as an anti-reflection film, an antistatic film, an antifouling film, etc. on the surface of the hard coat layer opposite to the primer layer, depending on the purpose of use. The optional layer may be one layer or multiple layers.

[0047] Plastic substrate: The refractive index of the plastic substrate is preferably 1.45 to 1.65. Examples of the plastic substrate include polycarbonate resins, polyamide resins, and polycellulose resins (such as triacetyl cellulose).

[0048] Primer and hard coat layers: The primer layer contains a resin matrix and the silica particles 1. The silica particles 1 are dispersed in the resin matrix.

[0049] The content of the silica particles 1 in the primer layer is preferably 10 to 70% by mass, and more preferably 15 to 60% by mass. The thickness of the primer layer is preferably in the range of 0.5 to 5.0 μm, more preferably 0.5 to 4.0 μm.

[0050] The primer layer can be formed, for example, by applying the primer layer-forming paint to the surface of the plastic substrate and curing the paint, which forms the resin matrix from the resin matrix-forming components.

[0051] The resin matrix is ​​preferably formed from a polyurethane having an ethylenically unsaturated bond-containing group. The ethylenically unsaturated bond-containing group is preferably a (meth)acryloyl group, more preferably an acryloyl group.

[0052] The hard coat layer contains a silica-based matrix and the silica particles 2. The silica particles 2 are dispersed in the silica-based matrix. The content of the silica particles 2 in the hard coat layer is preferably 10 to 70% by mass, and more preferably 15 to 60% by mass. The thickness of the hard coat layer is preferably in the range of 3.0 to 10.0 μm, and more preferably 3.0 to 8.0 μm.

[0053] The hard coat layer can be formed, for example, by applying the coating material for forming the hard coat layer onto the surface of the primer layer and curing the coating material, which forms the silica matrix from the silica matrix-forming components.

[0054] When curing each coating material, for example, the coating material for forming a primer layer may be applied to the surface of the plastic substrate and pre-cured by heating at 60 to 120°C for 3 to 30 minutes, and the coating material for forming a hard coat layer may be applied to the surface of the pre-cured coating film and pre-cured by heating at 80 to 130°C for 0.5 to 5 hours.

[0055] Silica particle size: As described above, the silica particles 1 contained in the primer layer are preferably silica particles having a large area for receiving impacts and pressures from above (toward the hard coat layer), and taking into consideration the transparency of the primer layer, the average particle size of the silica particles 1 is 20 to 100 nm, and preferably 20 to 90 nm.

[0056] As described above, the silica particles 2 contained in the hard coat layer are preferably silica particles having a large surface area, which is easily densified, and a small particle size. Therefore, the average particle size of the silica particles 2 is 3 to 20 nm, and preferably 4 to 15 nm.

[0057] In the optical article according to the present invention, the relationship between the average particle size of the silica particles 1 contained in the primer layer and the average particle size of the silica particles 2 contained in the hard coat layer is important, and the value of the average particle size of the silica particles 1 / the average particle size of the silica particles 2 (hereinafter also referred to as the "particle size ratio") is 2.5 to 20, and preferably 2.5 to 18. When the particle size ratio is within this range, for the above-mentioned reasons, the optical article of the present invention has high hardness on the surface of the hard coat layer. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0059] [Measurement and evaluation test methods] The measurement methods and evaluation test methods employed in the examples and other sections are as follows. (1) Average particle size of silica particles: A sample with a solid content of 0.15%, prepared by mixing a water-dispersed sol of silica particles with pure water, was placed in a quartz cell measuring 1 cm in length, 1 cm in width, and 5 cm in height, and the particle size distribution of the particle group was measured using an ultrafine particle size analyzer (manufactured by Otsuka Electronics Co., Ltd., model ELS-Z2) using the dynamic light scattering method. From the measurement results, the average particle size was calculated by the cumulant method.

[0060] (2) Adhesion between primer layer and hard coat layer: On the hard coat layer side surface of a plastic lens substrate with a primer layer and a hard coat layer produced in an Example or Comparative Example, 100 1 mm square grids were formed by cutting with a knife at 1 mm intervals down to the substrate. Cellophane adhesive tape (product name "NICHIBAN") was pressed against the grids and then pulled in a direction at 90 degrees to the in-plane direction of the lens substrate. This operation was repeated a total of 10 times and the number of grids that did not peel off was counted.

[0061] (3) Appearance of coating film (cloudy): The haze of the plastic lens substrate with the primer layer and hard coat layer produced in the Examples and Comparative Examples was measured using a color / turbidity simultaneous measuring instrument COH 400 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0062] (4) Pencil hardness of optical article: The hardness of the surface on the hard coat layer side of the plastic lens substrate with a primer layer and a hard coat layer produced in the Examples or Comparative Examples was measured using a pencil hardness tester in accordance with JIS K5600.

[0063] [Manufacturing of optical articles] (Preparation of primer coating composition) [Manufacturing example P1] While stirring 124.5 g of urethane acrylic copolymer dispersion (Kusumoto Chemicals, NeoPac R-9699, elongation: 160%, average particle size: 77 nm, solid content: 40% by mass), 252.1 g of pure water (Takasugi Pharmaceutical Co., Ltd.), 496.4 g of methanol (Hayashi Pure Chemical Industries, Ltd.), 123.0 g of silica particles (JGC Catalysts and Chemicals, Cataloid SI-45P, average particle size: 45 nm, solid content: 40.5% by mass), and 4.0 g of leveling agent (L-7604 (Dow Corning Toray Co., Ltd.) diluted with 10% methanol) were added, and the mixture was stirred at room temperature for one day and night to prepare a primer coating composition (P1). Table 1 shows the amount of each component in the primer coating composition (P1) (expressed as a relative amount with the total amount of each component being 100 parts by mass).

[0064] [Manufacturing examples P2~P3, C1~C4] Primer coating compositions (P2), (P3), (C1) to (C4) were prepared in the same manner as in Production Example P1, except that the type and amount of each component was changed as shown in Table 1. The amount of each component in these coating compositions is shown in Table 1.

[0065] [Table 1]

[0066] (Preparation of hard coat coating composition) [Manufacturing example H1] 131.9 g of γ-glycidoxypropyltrimethoxysilane (A-187, Momentive Performance Materials Japan, LLC, solid content concentration: 98.5% by mass or more) was mixed with 17.3 g of methanol (Hayashi Pure Chemical Industries, Ltd.), and 38.9 g of 0.01 N hydrochloric acid solution was added dropwise to the solution while stirring. Furthermore, the solution was stirred at room temperature for a whole day and night to hydrolyze the silane compound.

[0067] Next, to this hydrolysis liquid, 3.08 g of methanol, 643.5 g of silica particles (Cataloid SI-550 manufactured by JGC Catalysts and Chemicals Co., Ltd., average particle size: 5 nm, solid content concentration: 20.5 mass%, dispersion medium: water), 134.5 g of propylene glycol monomethyl ether (manufactured by Dow Chemical Japan Co., Ltd.), 11.3 g of 1,2,3,4-butanetetracarboxylic acid (manufactured by Kanto Chemical Co., Ltd., purity: 98 mass% or more), 8.1 g of dicyandiamide (manufactured by Kishida Chemical Co., Ltd., purity: 98 mass% or more), and a leveling agent (DOWSIL TM L-7001 Fluid (Dow Toray Co., Ltd.) 10% methanol dilution) 7.6 g, and leveling agent (DOWSIL TM 3.8 g of SH 28 Paint Additive (a 10% dilution of propylene glycol monomethyl ether from Dow Toray Industries, Inc.) was added and stirred overnight at room temperature to prepare a coating composition (H1). Table 1 shows the amounts of each component in the hard coat coating composition (H1) (expressed as relative amounts with the total amount of each component taken as 100 parts by mass) and the evaluation results.

[0068] [Manufacturing examples H2, H3, C5] Hard coat coating compositions (H2), (H3), and (C5) were prepared in the same manner as in Production Example H1, except that the type and amount of each component was changed as shown in Table 2. The amount of each component in these coating compositions is shown in Table 2.

[0069] [Table 2]

[0070] (Manufacturing of optical articles) [Example 1] (Formation of primer layer) Etching was performed by immersing a plastic lens (made of polycarbonate resin) in a 5% aqueous NaOH solution heated to 40° C. for 3 minutes, after which the sodium hydroxide adhering to the lens was thoroughly washed away with water and dried with hot air at 50° C. The primer coating composition (P1) produced in Production Example P1 was applied by dipping to the surface of the plastic lens (made of polycarbonate resin) substrate thus pretreated to form a coating film.

[0071] Next, the coating film (primer layer) was cured by heat treatment at 80° C. for 10 minutes. The primer layer thus formed had a film thickness of 0.9 μm after curing.

[0072] (Formation of hard coat layer) The hard coat paint composition (H1) was applied by dipping onto the surface of the primer layer formed on the plastic lens substrate to form a coating film.

[0073] Next, the coating film was dried at 100° C. for 10 minutes, and then heat-treated at 120° C. for 1 hour to cure the coating film (hard coat layer), thereby obtaining a lens substrate with a coating film (hereinafter also referred to as an "optical article"). The thickness of the hard coat layer thus formed after curing was 5.2 μm.

[0074] [Examples 2 to 6, Comparative Examples 1 to 5] Optical articles were produced in the same manner as in Example 1, except that the primer coating composition and hard coat coating composition shown in Table 3 were used. In Example 4, the thickness of the primer layer was adjusted by increasing the lifting speed in the dipping method. The evaluation results of the optical articles are shown in Table 3.

[0075] [Table 3]

Claims

1. An optical article comprising a plastic substrate, a primer layer provided on at least a portion of a surface of the plastic substrate, and a hard coat layer provided on a surface of the primer layer opposite to the plastic substrate, the primer layer comprises a resin matrix and silica particles 1 having an average particle diameter of 20 to 100 nm measured by a dynamic light scattering method and determined by a cumlite analysis method; The silica particles 1 are particles consisting of silica only (however, unavoidable impurities may be contained), or particles consisting of an oxide of silicon and at least one metal element M selected from the group consisting of Ti, Fe, Zn, W, Sn, Ta, Zr, Sb, Nb, In, Ce, Al, Y, Pb and Mo, in which the amount of the metal element M is 1.5 mass% or less in terms of the oxide of the metal element M, the hard coat layer comprises a silica-based matrix and silica particles 2 having an average particle diameter of 3 to 20 nm measured by a dynamic light scattering method and determined by a cumulite analysis method; the ratio of the average particle size of the silica particles 1 to the average particle size of the silica particles 2 is 2.5 to 20; Optical articles.

2. 2. The optical article according to claim 1, wherein the resin matrix is ​​formed from a polyurethane having an ethylenically unsaturated bond-containing group.

3. 3. The optical article according to claim 1, wherein the resin matrix has an elongation in the range of 150 to 200% as measured in accordance with JIS K7161.

4. The optical article according to any one of claims 1 to 3, wherein the plastic substrate is a polycarbonate resin substrate, a polyamide resin substrate, or a polycellulose resin substrate.

Citation Information

Patent Citations

  • Photo-setting composition

    JP1989266155A

  • Coating composition for forming hardcoat layer, and optical article

    JP2009197078A

  • Optical article and process for producing optical article

    JP2010091995A

  • Water-based primer composition, and plastic article using the same

    JP2010150309A