How alcohol is produced
The use of a silica-supported heteropolyacid catalyst with controlled pore size and volume significantly suppresses by-product formation in ethanol production from ethylene hydration, addressing catalyst leakage and selectivity issues in existing technologies.
Patent Information
- Application Number
- JP2020195107
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-25
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Existing methods for producing ethanol through ethylene hydration using solid acid catalysts face issues such as catalyst component leakage, poor selectivity, catalyst deterioration due to coking, and the production of by-products like acetaldehyde and butene, which hinder industrial applicability.
A method utilizing a silica-supported heteropolyacid catalyst with specific pore size and volume distribution, limiting pores to 6 nm or less and total volume of 0.05 mL/g, is employed to suppress the production of by-products in the ethanol synthesis process.
This approach effectively reduces the formation of acetaldehyde and butene, enhancing the efficiency and selectivity of the ethanol production process.
Smart Images

Figure 0007571495000003 
Figure 0007571495000001 
Figure 0007571495000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for producing an alcohol by the hydration reaction of an olefin. [Background technology]
[0002] Industrial ethanol is an important industrial chemical product that is widely used as an intermediate for organic solvents, organic synthesis raw materials, disinfectants, chemical products, etc. It is known that industrial ethanol can be obtained by the hydration reaction of ethylene in the presence of a liquid acid such as sulfuric acid or sulfonic acid, a zeolite catalyst, a metal oxide catalyst such as tungsten, niobium, or tantalum, or a solid catalyst in which a heteropoly acid such as tungstophosphoric acid or tungstosilicic acid or phosphoric acid is supported on a silica carrier or a diatomaceous earth carrier.
[0003] In the case of liquid-phase ethylene hydration using a liquid acid catalyst such as sulfuric acid or sulfonic acid, the acid used in the reaction needs to be post-treated, and there are also problems such as low activity, limiting industrial use. On the other hand, the ethylene hydration using a carrier-supported solid catalyst can be carried out in a gas phase reaction, so that the reactants and the catalyst can be easily separated, and the reaction can be carried out under high temperature conditions that are favorable in terms of reaction rate, or under high pressure conditions that are favorable in terms of equilibrium.
[0004] Many proposals have been made regarding solid acid catalysts, and in particular, gas-phase reaction processes using solid acid catalysts in which phosphoric acid is supported on a carrier have already been industrially implemented. However, in industrial processes using catalysts in which phosphoric acid is supported on a carrier, phosphoric acid, which is an active component, is continuously discharged, resulting in a decrease in activity and selectivity, and a continuous supply of phosphoric acid is required. In addition, since the discharged phosphoric acid corrodes the equipment, periodic maintenance of reactors and other equipment is required, and there is a problem that the maintenance of the equipment is costly. In addition, the supported phosphoric acid catalyst is physically and chemically deteriorated by contact with water vapor. The activity decreases after long-term use, and in severe cases, the carrier particles aggregate with each other to form blocks, which may make it difficult to replace or extract the catalyst. For this reason, new carriers and supported catalysts that solve these problems in the ethylene hydration reaction are being developed.
[0005] For example, there is known a hydration reaction of ethylene using a catalyst containing titanium oxide and tungsten oxide as essential components on a titanium oxide carrier, which is free from the risk of phosphoric acid leaking out (see Patent Document 1).
[0006] Also disclosed is a method for producing ethanol by the hydration reaction of ethylene using a supported phosphoric acid catalyst in which phosphoric acid is supported on a silica carrier having an average pore volume of at least 1.23 mL / g (see Patent Document 2). The method disclosed in Patent Document 2 is said to be superior in yield and selectivity to conventional supported phosphoric acid catalysts, and to suppress a decrease in the particle strength of the carrier.
[0007] Furthermore, a heteropolyacid catalyst in which a heteropolyacid is supported on fumed silica produced by a combustion method has been disclosed as a supported catalyst for ethanol production by the hydration reaction of ethylene with improved performance (see Patent Document 3). As a method for improving the performance of heteropolyacid catalysts, a catalyst in which a heteropolyacid is supported on a clay carrier treated with a thermal acid has also been proposed (see Patent Document 4).
[0008] On the other hand, a silica carrier having a pore volume, specific surface area, and pore diameter within a specific range has been disclosed as a carrier for a supported catalyst suitable for the hydration reaction of an olefin, and the production of ethanol by the hydration reaction of ethylene using the carrier has been exemplified (see Patent Document 5).
[0009] However, Patent Documents 1 to 5 are not yet sufficient for industrial use because of problems such as outflow of catalyst-supported components, poor selectivity for ethylene hydration that leads to coking, which is one cause of catalyst deterioration, and insufficient suppression of production of by-products such as acetaldehyde and butene. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 10-298122 [Patent Document 2] Japanese Patent Application Publication No. 10-101601 [Patent Document 3] Japanese Patent Application Publication No. 8-192047 [Patent Document 4] Japanese Patent Application Publication No. 8-225473 [Patent Document 5] JP 2003-190786 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made in view of the above-mentioned background, and an object of the present invention is to provide a method for producing an alcohol by a hydration reaction of an olefin, in which the production of by-products such as acetaldehyde and butene is suppressed. [Means for solving the problem]
[0012] As a result of intensive research, the present inventors have found that by using a silica-supported heteropolyacid catalyst in which the total volume of pores of a specific size falls within a specific range, obtained by using a support material having an appropriate pore size and adjusting the amount of catalyst supported on the support material, the production of by-products can be significantly suppressed in ethanol production by ethylene hydration reaction, and have completed the present invention.
[0013] That is, the present invention relates to the following [1] to [4]. [1] A method for producing an alcohol, comprising the steps of: subjecting an olefin having 2 to 5 carbon atoms to a hydration reaction in the presence of a silica-supported heteropolyacid catalyst in which a heteropolyacid or a salt thereof is supported on a silica support to produce an alcohol, the method comprising the steps of: A method for producing an alcohol, wherein the silica-supported heteropolyacid catalyst has a total volume of pores having a pore size of 6 nm or less of 0.05 mL / g or less. [2] The method for producing an alcohol according to [1], wherein the heteropolyacid is at least one selected from the group consisting of silicotungstic acid, phosphotungstic acid, phosphomolybdic acid, silicomolybdic acid, silicovanadotungstic acid, phosphovanadotungstic acid, and phosphovanadomolybdic acid. [3] The method for producing an alcohol according to either [1] or [2], wherein the amount of the heteropolyacid or a salt thereof supported in the silica-supported heteropolyacid catalyst is 50 to 200 parts by mass per 100 parts by mass of the silica support. [4] The method for producing an alcohol according to any one of [1] to [3], wherein the olefin is ethylene and the alcohol is ethanol. Effect of the Invention
[0014] According to the present invention, by using a silica-supported heteropolyacid catalyst having pores with a pore size of 6 nm or less and a total volume of 0.05 mL / g or less in the production of an alcohol by the hydration reaction of an olefin, for example, ethylene, the production of by-products, acetaldehyde and butene, can be suppressed. [Brief description of the drawings]
[0015] [Figure 1] 1 is a graph showing the pore size distribution of silica-supported heteropolyacid catalysts prepared in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will be described below, however, the present invention is not limited to these embodiments and various applications are possible within the spirit and scope of the present invention.
[0017] <How alcohol is produced> According to one embodiment of the method for producing an alcohol, water and an olefin having 2 to 5 carbon atoms are supplied to a reactor using a solid acid catalyst (hereinafter, sometimes referred to as an "alcohol production catalyst") in which a heteropolyacid or a heteropolyacid salt is supported on a silica carrier, and an alcohol is obtained by causing a hydration reaction in a gas phase.
[0018] A specific example of an alcohol production reaction by hydration of an olefin having 2 to 5 carbon atoms is shown in the following formula (1). [ka] (In the formula, R 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; R 1 ~R 4 The total number of carbon atoms is 0 to 3.
[0019] The hydration reaction of olefins using a catalyst for alcohol production is an equilibrium reaction, and the conversion rate of olefins is at most the equilibrium conversion rate. For example, the equilibrium conversion rate in the production of ethanol by ethylene hydration is calculated to be 7.5% at a temperature of 200°C and a pressure of 2.0 MPaG. Therefore, in the process for producing alcohol by olefin hydration, the maximum conversion rate is determined by the equilibrium conversion rate, and as seen in the example of ethylene, the equilibrium conversion rate of the olefin hydration reaction tends to be small, so industrially, there is a strong demand for carrying out the olefin hydration reaction highly efficiently under mild conditions.
[0020] The olefin having 2 to 5 carbon atoms applied to the alcohol production method of one embodiment is not particularly limited. The olefin having 2 to 5 carbon atoms is, for example, ethylene, propylene, n-butene, isobutene, pentene, or a mixture of two or more of these, and is preferably ethylene.
[0021] Although there is no limitation on the ratio of the olefin to water used, since the reaction rate is highly dependent on the olefin concentration and the energy cost of the alcohol production process increases when the water concentration is high, the molar ratio of the olefin to water is preferably water:olefin=0.01 to 2.0, and more preferably water:olefin=0.1 to 1.0.
[0022] There is no limitation on the type of olefin hydration reaction using the catalyst for alcohol production, and any reaction type can be used. Preferred types include, for example, a fixed bed type, a fluidized bed type, and a suspended bed type from the viewpoint of ease of separation from the catalyst and reaction efficiency, and more preferably, a fixed bed type that requires the least energy for separation from the catalyst.
[0023] When a fixed bed system is used, the gas space velocity is not particularly limited, but from the viewpoint of energy and reaction efficiency, it is preferably 500 to 15000 / hr, more preferably 1000 to 10000 / hr. If the gas space velocity is 500 / hr or more, the amount of catalyst used can be effectively reduced, and if it is 15000 / hr or less, the amount of gas circulated can be reduced, so that within the above range, alcohol production can be performed more efficiently.
[0024] There is no restriction on the reaction pressure in the olefin hydration reaction using the catalyst for alcohol production. Since the olefin hydration reaction is a reaction in which the number of molecules is reduced, it is generally advantageous to carry out the reaction at high pressure. The reaction pressure is preferably 0.5 to 7.0 MPaG, more preferably 1.5 to 4.0 MPaG. Here, "G" means gauge pressure. If the reaction pressure is 0.5 MPaG or more, a sufficient reaction rate can be obtained, and if the reaction pressure is 7.0 MPaG or less, there is no need to install equipment for condensation measures and evaporation of olefins, or equipment for high-pressure gas safety measures, and energy costs can be further reduced.
[0025] The reaction temperature of the olefin hydration reaction using the catalyst for alcohol production is not particularly limited and can be carried out at a wide range of temperatures. The reaction temperature is preferably 100 to 550°C, more preferably 150 to 350°C, taking into consideration the thermal stability of the heteropolyacid or heteropolyacid salt and the temperature at which water, one of the raw materials, does not condense.
[0026] In the hydration reaction of olefins using a catalyst for alcohol production, the loss of olefins can be reduced by recycling unreacted olefins to the reactor. There is no limitation on the method of recycling unreacted olefins to the reactor, and olefins may be isolated from the process fluid discharged from the reactor and recycled, or may be recycled together with other inert components. Usually, industrial grade ethylene often contains a very small amount of ethane. Therefore, when using ethylene containing ethane and recycling unreacted ethylene to the reactor, it is desirable to purge a part of the recovered ethylene gas outside the system to prevent ethane from concentrating and accumulating.
[0027] In the hydration reaction of olefins using a catalyst for alcohol production, the produced alcohol may be dehydrated to produce an ether compound as a by-product. For example, when ethanol is obtained by hydration of ethylene, diethyl ether is produced as a by-product. This diethyl ether is thought to be produced by a dehydration reaction from two molecules of ethanol, and when ethanol is produced by hydration of ethylene, it significantly reduces the yield of the reaction. By recycling the by-product diethyl ether to the reactor, diethyl ether is converted to ethanol, and ethanol can be produced from ethylene with extremely high efficiency. There are no particular limitations on the method for recycling the by-product ether compound to the reactor, but examples include a method of isolating the ether compound from the component distilled from the reactor and recycling it to the reactor, and a method of recycling it to the reactor as a gas component together with unreacted olefin.
[0028] <Silica-supported heteropoly acid catalyst (catalyst for alcohol production)> In one embodiment of the alcohol production method, a silica-supported heteropolyacid catalyst is used as a catalyst for alcohol production, which is a solid acid catalyst in which a heteropolyacid or a salt thereof (also referred to as a "heteropolyacid salt" in the present disclosure) is supported on a silica support.
[0029] (Heteropolyacids, heteropolyacid salts) Heteropolyacids are acids consisting of a central element and peripheral elements bonded with oxygen. The central element is usually silicon or phosphorus, but can be any one selected from a wide variety of elements in groups 1 to 17 of the periodic table.
[0030] Examples of central elements constituting heteropolyacids include, but are not limited to, cupric ions; divalent beryllium, zinc, cobalt, or nickel ions; trivalent boron, aluminum, gallium, iron, cerium, arsenic, antimony, phosphorus, bismuth, chromium, or rhodium ions; tetravalent silicon, germanium, tin, titanium, zirconium, vanadium, sulfur, tellurium, manganese, nickel, platinum, thorium, hafnium, and cerium ions and other rare earth ions; pentavalent phosphorus, arsenic, vanadium, and antimony ions; hexavalent tellurium ions; and heptavalent iodine ions.
[0031] Examples of peripheral elements constituting the heteropolyacid include, but are not limited to, tungsten, molybdenum, vanadium, niobium, and tantalum.
[0032] Such heteropolyacids are known as "polyoxoanions", "polyoxometalates" or "metal oxide clusters". Some well-known anion structures are named after researchers in this field, such as the Keggin structure, the Wells-Dawson structure, and the Anderson-Evans-Perloff structure. For details, see "Chemistry of Polyacids" (Edited by the Chemical Society of Japan, Quarterly Chemistry Review No. 20, 1993). Heteropolyacids usually have high molecular weights, for example, in the range of 700 to 8500, and include not only monomers but also dimer complexes.
[0033] The heteropolyacid salt is a metal salt or onium salt in which some or all of the hydrogen atoms of the heteropolyacid are substituted, such as, but not limited to, metal salts of lithium, sodium, potassium, cesium, magnesium, barium, copper, gold, and gallium, and onium salts of ammonia.
[0034] Heteropolyacids have relatively high solubility in water or other polar solvents such as oxygenated solvents, especially when the heteropolyacid is in the form of a free acid or some salt. The solubility of the heteropolyacid can be controlled by selecting the appropriate counter ion.
[0035] Examples of heteropolyacids that can be supported on a silica support as a catalyst include, but are not limited to, the following: Silicotungstic acid H4[SiW 12 O 40 ]·xH2O Phosphotungstic acid H3 [PW 12 O 40 ]·xH2O Phosphomolybdic acid H3 [PMo 12 O 40 ]·xH2O Silicomolybdic acid H4 [SiMo 12 O 40 ]·xH2O Tungsten carbide H 4+n [SiV n W 12-n O 40 ]·xH2O Phosphonatotungstic acid H 3+n [PV n W 12-n O 40 ]·xH2O Phosphovanadomolybdic Acid H 3+n [PV n Mo 12-n O 40 ]·xH2O Molybdocarbamic acid H 4+n [SiV n Mo 12-n O40 ]·xH2O Silicomolybdotungstic acid H4 [SiMo n W 12-n O 40 ]·xH2O Phosphomolybdotungstic acid H3 [PMo n W 12-n O 40 ]·xH2O (In the formula, n is an integer of 1 to 11, and x is an integer of 1 or more.)
[0036] As the heteropolyacid, silicotungstic acid, phosphotungstic acid, phosphomolybdic acid, silicomolybdic acid, silicovanadotungstic acid, phosphovanadotungstic acid, or phosphovanadomolybdic acid is preferred, and silicotungstic acid, phosphotungstic acid, silicovanadotungstic acid, or phosphovanadotungstic acid is more preferred.
[0037] There is no particular limitation on the method for synthesizing such heteropolyacids, and any method may be used. For example, a heteropolyacid can be obtained by heating an acidic aqueous solution (pH 1 to 2) containing a salt of molybdic acid or tungstic acid and a simple oxygen acid of a heteroatom or its salt. The heteropolyacid compound can be isolated, for example, by crystallizing and separating it as a metal salt from the resulting heteropolyacid aqueous solution.
[0038] Specific examples of the production of heteropolyacids are described on page 1413 of "New Experimental Chemistry Lectures 8: Synthesis of Inorganic Compounds (III)" (edited by the Chemical Society of Japan, published by Maruzen Co., Ltd., August 20, 1984, 3rd edition), but are not limited thereto. The structure of the synthesized heteropolyacid can be confirmed by chemical analysis, as well as X-ray diffraction, UV, or IR measurement.
[0039] Preferred examples of the heteropolyacid salt include lithium salts, sodium salts, potassium salts, cesium salts, magnesium salts, barium salts, copper salts, gold salts, gallium salts, and ammonium salts of the above preferred heteropolyacids.
[0040] Specific examples of the heteropolyacid salt include lithium silicotungstic acid, sodium silicotungstic acid, cesium silicotungstic acid, copper silicotungstic acid, gold silicotungstic acid, and gallium silicotungstic acid; lithium phosphotungstic acid, sodium phosphotungstic acid, cesium phosphotungstic acid, copper silicotungstic acid, gold silicotungstic acid, and gallium silicotungstic acid; Lithium salt of molybdic acid, sodium salt of phosphomolybdic acid, caesium salt of phosphomolybdic acid, copper salt of phosphomolybdic acid, gold salt of phosphomolybdic acid, gallium salt of phosphomolybdic acid;Lithium salt of silicomolybdic acid, sodium salt of silicomolybdic acid, caesium salt of silicomolybdic acid, copper salt of silicomolybdic acid, gold salt of silicomolybdic acid, gallium salt of silicomolybdic acid;Lithium salt of silicomolybdic acid, sodium salt of silicomolybdic acid Thorium salts, caesium salts of phosphotungstic acid, copper salts of phosphotungstic acid, gold salts of phosphotungstic acid, gallium salts of phosphotungstic acid; lithium salts of phosphotungstic acid, sodium salts of phosphotungstic acid, caesium salts of phosphotungstic acid, copper salts of phosphotungstic acid, gold salts of phosphotungstic acid, gallium salts of phosphotungstic acid; lithium salts of phosphomolybdic acid salts, sodium salts of phosphovanadomolybdic acid, cesium salts of phosphovanadomolybdic acid, copper salts of phosphovanadomolybdic acid, gold salts of phosphovanadomolybdic acid, gallium salts of phosphovanadomolybdic acid; lithium salts of phosphovanadomolybdic acid, sodium salts of phosphovanadomolybdic acid, cesium salts of phosphovanadomolybdic acid, copper salts of phosphovanadomolybdic acid, gold salts of phosphovanadomolybdic acid, gallium salts of phosphovanadomolybdic acid, and the like.
[0041] Examples of heteropolyacid salts include lithium silicotungstic acid, sodium silicotungstic acid, cesium silicotungstic acid, copper silicotungstic acid, gold silicotungstic acid, and gallium silicotungstic acid; lithium phosphotungstic acid, sodium phosphotungstic acid, cesium phosphotungstic acid, copper phosphotungstic acid, gold silicotungstic acid, and gallium phosphotungstic acid; lithium phosphomolybdic acid, sodium phosphomolybdic acid, cesium phosphomolybdic acid, copper phosphomolybdic acid, gold silicotungstic acid, and gallium phosphomolybdic acid; lithium silicic molybdic acid, sodium silicic molybdic acid, cesium silicic molybdic acid, copper silicic molybdic acid, gold silicic molybdic acid, and gallium silicic molybdic acid; Lithium salt of silicotungstic acid, sodium salt of silicotungstic acid, caesium salt of silicotungstic acid, copper salt of silicotungstic acid, gold salt of silicotungstic acid, gallium salt of silicotungstic acid; Lithium salt of phosphorus vanadotungstic acid, sodium salt of phosphorus vanadotungstic acid, caesium salt of phosphorus vanadotungstic acid, copper salt of phosphorus vanadotungstic acid , gold salt of phosphovanadotungstic acid, gallium salt of phosphovanadotungstic acid; lithium salt of phosphovanadomolybdic acid, sodium salt of phosphovanadomolybdic acid, cesium salt of phosphovanadomolybdic acid, copper salt of phosphovanadomolybdic acid, gold salt of phosphovanadomolybdic acid, gallium salt of phosphovanadomolybdic acid; lithium salt of phosphovanadomolybdic acid, or sodium salt of phosphovanadomolybdic acid is preferred.
[0042] Examples of heteropolyacid salts include lithium silicotungstic acid, sodium silicotungstic acid, cesium silicotungstic acid, copper silicotungstic acid, gold silicotungstic acid, and gallium silicotungstic acid; lithium phosphotungstic acid, sodium phosphotungstic acid, cesium phosphotungstic acid, copper phosphotungstic acid, gold silicotungstic acid, and gallium silicotungstic acid; lithium phosphotungstic acid, sodium phosphotungstic acid, cesium phosphotungstic acid, copper phosphotungstic acid, gold silicotungstic acid, and gallium phosphotungstic acid; More preferred are phosphovanadotungstic acid, a phosphotungstic acid salt, a phosphotungstic acid sodium salt, a phosphotungstic acid cesium salt, a phosphotungstic acid copper salt, a phosphotungstic acid gold salt, and a phosphotungstic acid gallium salt; and phosphotungstic acid, a phosphotungstic acid lithium salt, a phosphotungstic acid sodium salt, a phosphotungstic acid cesium salt, a phosphotungstic acid copper salt, a phosphotungstic acid gold salt, and a phosphotungstic acid gallium salt.
[0043] As the heteropolyacid salt, a lithium salt of silicotungstic acid or a cesium salt of phosphotungstic acid is particularly suitable.
[0044] (Silica carrier) The heteropolyacid or heteropolyacid salt is used after being supported on a silica carrier.
[0045] There is no limitation on the silica that can be used as the silica carrier, and for example, natural silica or synthetic silica obtained by synthesizing various silica raw materials can be used. Generally, synthetic amorphous silica is produced by either a dry method or a wet method. The combustion method in which silicon tetrachloride is burned in a hydrogen flame in the presence of oxygen is classified as a dry method, while the gel method in which the neutralization reaction between sodium silicate and mineral acid is allowed to proceed in an acidic pH range, causing aggregation while suppressing the growth of primary particles, the sol-gel method in which alkoxysilane is hydrolyzed, and the water glass method in which sodium silicate is ion-exchanged to prepare active silicic acid, and then particles are grown in a seed particle-containing aqueous solution with a pH adjusted under heating are classified as wet methods.
[0046] In general, silica obtained by the combustion method is called fumed silica, silica obtained by the gel method is called silica gel, and silica obtained by dispersing silica particles obtained by the sol-gel method and water glass method in a medium such as water is called colloidal silica.
[0047] In one embodiment, the silica carrier can be obtained by kneading fumed silica obtained by a combustion method, silica gel obtained by a gel method, and colloidal silica obtained by a sol-gel method or a water glass method to obtain a kneaded mixture, molding the obtained kneaded mixture into a molded body, and then firing the molded body.
[0048] When fumed silica, silica gel, and colloidal silica are mixed, molded, and fired, the size of the primary particles and secondary particles of the fired silica carrier and the internal state of the porous body change depending on the mixing ratio of each component, the mixing method, the firing conditions, etc. For this reason, the higher-order structure of the silica carrier cannot be specified. The composition formula of the silica carrier is SiO2.
[0049] When using fumed silica, there is no particular limitation, and general fumed silica can be used. Examples of commercially available fumed silica include Aerosil (trademark) (manufactured by Nippon Aerosil Co., Ltd.), Reolosil (trademark) (manufactured by Tokuyama Corporation), and CAB-O-SIL (trademark) (manufactured by Cabot Corporation). Commercially available fumed silica includes hydrophilic and hydrophobic grades, and either one can be used.
[0050] Typical fumed silica has the following physical properties: primary particle size of 7 to 40 nm, specific surface area of 50 to 500 m 2 / g, is not porous, has no internal surface area, is amorphous, has a high purity as silicon oxide of 99% or more, and contains almost no metals or heavy metals.
[0051] There is no particular limitation on the silica gel, and general silica gel can be used. Examples of commercially available silica gel include NIPGEL (manufactured by Tosoh Silica Corporation), MIZUKASIL (manufactured by Mizusawa Industrial Chemical Co., Ltd.), CALiACT (manufactured by Fuji Silysia Chemical Ltd.), and Sunsphere (manufactured by AGC Si-Tech Co., Ltd.).
[0052] Generally, silica gel is produced by using sodium silicate as a raw material, which is made by dissolving sodium silicate glass (cullet) obtained by mixing and melting silica sand (SiO2) and soda ash (Na2CO3) in water, and reacting the sodium silicate with a mineral acid such as sulfuric acid under acidic conditions to cause aggregation while suppressing the growth of primary particles, thereby gelling the entire reaction liquid.
[0053] The physical properties of silica gel are not particularly limited, but silica gel is characterized by small primary particles, a high specific surface area, and hard secondary particles. Specific physical properties of silica gel include, for example, a BET specific surface area of 200 to 1000 m 2 / g, secondary particle diameter of 1 to 30 μm, and pore volume measured by nitrogen gas adsorption method (BJH method: Barrett, Joyner, Hallender method) of 0.3 to 2.5 mL / g. The higher the purity of the silica gel, the better, and the preferred purity is 95% by mass or more, and more preferably 98% by mass or more.
[0054] The colloidal silica is not particularly limited, and general colloidal silica can be used. Examples of commercially available colloidal silica include Snowtex (trademark) (manufactured by Nissan Chemical Industries, Ltd.), Silicadol (manufactured by Nippon Chemical Industry Co., Ltd.), Adelite (manufactured by ADEKA Corporation), CAB-O-SIL (trademark) TG-C colloidal silica (manufactured by Cabot Corporation), and Quartron (trademark) (manufactured by Fuso Chemical Industry Co., Ltd.).
[0055] Colloidal silica is a dispersion of silica particles in a medium such as water. There are two methods for producing colloidal silica: a water glass method and a sol-gel method using hydrolysis of alkoxysilane. Colloidal silica produced by either method can be used. Colloidal silica produced by the water glass method and colloidal silica produced by the sol-gel method may be used in combination.
[0056] Representative physical properties of colloidal silica include, for example, a particle size of 4 to 80 nm and a solid content concentration of silica dispersed in water or an organic solvent of 5 to 40 mass%. The impurity concentration in colloidal silica is preferably low because it may affect the catalytically active components carried. The silica purity in the solid content is preferably 99 mass% or more, more preferably 99.5 mass% or more.
[0057] The silica carrier can be obtained by kneading fumed silica, silica gel, and colloidal silica to obtain a kneaded mixture, molding the resulting kneaded mixture into a molded body, and then firing the molded body. Appropriate additives may be added during the kneading.
[0058] The compounding ratio of fumed silica, silica gel, and colloidal silica is preferably 5 to 50 parts by mass of fumed silica, 40 to 90 parts by mass of silica gel, and 5 to 30 parts by mass of solid content of colloidal silica, and more preferably 15 to 40 parts by mass of fumed silica, 45 to 70 parts by mass of silica gel, and 5 to 15 parts by mass of solid content of colloidal silica.
[0059] When mixing fumed silica, silica gel, and colloidal silica, water or additives can be added for the purpose of improving moldability, improving the strength of the final silica carrier, etc. The additives are not particularly limited, and additives used in the manufacture of general ceramic molded products can be used. Depending on the purpose, binders, plasticizers, dispersants, lubricants, wetting agents, antifoaming agents, etc. can be used.
[0060] Examples of the binder include wax emulsion, gum arabic, lignin, dextrin, polyvinyl alcohol, polyethylene oxide, starch, methylcellulose, Na-carboxymethylcellulose, hydroxyethylcellulose, sodium alginate, ammonium alginate, gum tragacanth, etc. Since the viscosity of the kneaded material varies greatly depending on the type and concentration of the binder, the type and amount of the binder are appropriately selected so as to obtain a viscosity suitable for the molding method to be used.
[0061] Examples of the plasticizer include glycerin, polyethylene glycol, and dibutyl phthalate. The plasticizer can increase the flexibility of the kneaded material.
[0062] Examples of dispersants for aqueous systems include carboxymethylcellulose ammonium (CMC-NH4), oligomers of acrylic acid or its ammonium salt, anionic surfactants, ammonium polycarboxylate, wax emulsion, various amines such as monoethylamine, pyridine, piperidine, tetramethylammonium hydroxide, etc. Examples of dispersants for non-aqueous systems include fatty acids, fatty acid esters, phosphate esters, synthetic surfactants, benzenesulfonic acid, etc. By adding these dispersants, it is possible to avoid the generation of aggregated particles and obtain a silica carrier having a uniform fine structure after firing.
[0063] Examples of the lubricant include hydrocarbon lubricants such as liquid paraffin, paraffin wax, chlorinated hydrocarbons, etc., and fatty acid lubricants such as stearic acid, lauric acid, and metal salts thereof, fatty acid amides, etc. Addition of a lubricant can reduce friction between powders, improve fluidity, facilitate molding, and also facilitate removal of the molded product from the mold.
[0064] In order to improve the wetting property between the silica powder and the dispersant, a wetting agent can be added. As the wetting agent, for example, in the case of an aqueous system, a nonionic surfactant, alcohol, glycol, etc., can be mentioned, and for example, in the case of a non-aqueous system, polyethylene glycol ethyl ether, polyoxyethylene ester, etc. can be mentioned. These substances are easily adsorbed at the solid-liquid interface, and by lowering the interfacial tension, they improve the wetting of the solid.
[0065] When handling a slurry-type kneaded product, a defoaming agent such as a nonionic surfactant, a polyalkylene glycol derivative, or a polyether derivative may be added.
[0066] These additives can be used alone or in combination. It is desirable that additives are effective in as small an amount as possible, are inexpensive, do not react with the powder, dissolve in water or a solvent, completely decompose in an oxidizing or non-oxidizing atmosphere at a relatively low temperature, for example, below 400°C, leave no ash, especially alkali metals and heavy metals, after decomposition and explosion, produce non-toxic and non-corrosive decomposition gases, and do not prevent the recycling of the fragments that were not used to make the product.
[0067] The shape of the silica carrier is not particularly limited. For example, it may be spherical, cylindrical, hollow cylindrical, plate-like, elliptical, sheet-like, honeycomb-like, etc. Preferably, it is spherical, cylindrical, hollow cylindrical, or elliptical, more preferably spherical or cylindrical (pellet-like), because it facilitates filling into a reactor and supporting catalytically active components.
[0068] The particle size of the silica carrier is not particularly limited. The particle size of the carrier varies depending on the reaction form, but when used in a fixed bed system, it is preferably 2 mm to 10 mm, and more preferably 3 mm to 7 mm.
[0069] The method for forming the silica carrier is not particularly limited. It is formed from a kneaded material containing fumed silica, silica gel, and colloidal silica by any convenient method such as molding, extrusion, rolling granulation, spray drying, etc.
[0070] General molding involves placing the kneaded material in a metal mold, repeatedly hitting it with a hammer or the like to pack it in tightly, and then pressing it with a piston before removing it from the mold; this process is also called stamp molding. Extrusion molding generally involves packing the kneaded material into a press, extruding it through a die (mouthpiece), cutting it to an appropriate length, and molding it into the desired shape. Rolling granulation involves dropping the kneaded material onto a rotating disk placed at an angle, and rolling the granules on the disk to grow them into spherical shapes. Spray drying generally involves spraying a thick slurry into hot air to obtain porous granules, although the granules are not very large.
[0071] The size of the silica carrier is not particularly limited. It is desirable to set the size taking into consideration the handling during the production or packing of the catalyst carrying the catalytically active component, the pressure difference after packing in the reactor, and the reaction results of the catalytic reaction, since these factors affect the size. The silica carrier shrinks during the firing of the molded body, so the size is determined by the firing conditions.
[0072] When the silica carrier is spherical, the size (after calcination) of the silica carrier is preferably 0.5 mm to 12 mm in diameter, more preferably 1 mm to 10 mm, and even more preferably 2 mm to 8 mm. When the silica carrier is not spherical, the size (after calcination) of the silica carrier is preferably 0.5 mm to 12 mm in length in the maximum dimension when the size is measured, more preferably 1 mm to 10 mm, and even more preferably 2 mm to 8 mm.
[0073] If the particle size of the silica carrier is 0.5 mm or more, it is possible to prevent a decrease in productivity during carrier production and an increase in pressure loss when used as a catalyst. If the particle size of the silica carrier is 12 mm or less, it is possible to prevent a decrease in reaction rate due to diffusion rate control within the carrier and an increase in by-products.
[0074] Before or after the calcination, if necessary, the shape of the silica carrier may be adjusted by treatment with Marmerizer (registered trademark) (manufactured by Fuji Paudal Co., Ltd.) or the like. For example, a cylindrical molded body before calcination can be molded into a spherical shape by treating it with the Marmerizer (registered trademark).
[0075] The calcination method is not particularly limited, but there is an appropriate calcination temperature range from the viewpoint of decomposing the additives and preventing the destruction of the silica structure. The calcination temperature is preferably 300°C to 1000°C, and more preferably 500°C to 900°C. When the calcination temperature is in this range, the additives are completely decomposed and there is no adverse effect on the performance of the silica carrier. In addition, the specific surface area of the silica carrier is also improved.
[0076] The calcination treatment can be carried out under either oxidizing or non-oxidizing conditions. For example, the calcination treatment can be carried out in an air atmosphere or in an inert gas atmosphere such as nitrogen gas. There is no particular restriction on the time of the calcination treatment, and it can be appropriately determined depending on the shape and size of the molded body, the type and amount of additives used, etc.
[0077] The average pore size of the mesopores in the silica carrier measured by gas adsorption method (BJH method: Barrett, Joyner, Hallender method) is preferably 5 to 16 nm. The average pore size of the mesopores in the silica carrier measured by gas adsorption method (BJH method) is more preferably 6 to 14 nm, and further preferably 7 to 12 nm. When the average pore size of the mesopores in the silica carrier measured by gas adsorption method (BJH method) is in the range of 5 to 16 nm, the specific surface area measured by the BET method is sufficient.
[0078] The specific surface area of the silica support measured by the BET method (BET specific surface area) is 200 to 500 m 2 The BET specific surface area of the silica carrier is preferably 220 to 400 m 2 / g, and more preferably 240 to 400 m 2 / g. The BET specific surface area of the silica support is 200 to 500 m 2When the amount of the hydroxyl group is in the range of 1 / g, a sufficient reaction rate can be obtained when the hydroxyl group is made into a catalyst.
[0079] The bulk density of the silica carrier is preferably 300 to 700 g / L. The bulk density of the silica carrier is more preferably 400 to 650 g / L, and further preferably 450 to 600 g / L. When the bulk density of the silica carrier is in the range of 300 to 700 g / L, the required amount of active ingredient can be supported and the strength of the carrier can be maintained.
[0080] (Method of supporting heteropolyacid on silica carrier) There is no particular limitation on the method for supporting the heteropolyacid or its salt on the silica carrier. In general, the heteropolyacid or its salt is dissolved or suspended in a solvent, the resulting solution or suspension is absorbed into the carrier, and then the solvent is evaporated.
[0081] Examples of methods for supporting a heteropolyacid salt on a carrier include, but are not limited to, a method in which a heteropolyacid is supported on a carrier and then a raw material of an element that forms a salt is supported on the carrier, a method in which a heteropolyacid and a raw material of an element that forms a salt are supported on a carrier together, a method in which a pre-prepared heteropolyacid salt is supported on a carrier, and a method in which a raw material of an element that forms a salt is supported on a carrier and then a heteropolyacid is supported, etc. In any of the above methods, the heteropolyacid, its salt, and the raw material of the element that forms the salt can be dissolved or suspended in a suitable solvent and supported on the carrier. The solvent used in this case may be any solvent that can dissolve or suspend the heteropolyacid, its salt, or the raw material of the element that forms the salt, and for example, water, an organic solvent, or a mixture thereof is used, and preferably water, alcohol, or a mixture thereof is used.
[0082] (Amount of heteropolyacid supported on silica carrier) The amount of the heteropolyacid or a salt thereof supported on the silica carrier can be adjusted, for example, by dissolving the heteropolyacid or a salt thereof in distilled water or the like in an amount equivalent to the amount of water absorbed by the carrier, and impregnating the carrier with the solution.
[0083] In another embodiment, the amount of the heteropolyacid or a salt thereof supported on the silica support can also be adjusted by immersing the silica support in a solution of an excess amount of the heteropolyacid or a salt thereof while moving the support moderately, and then filtering the solution to remove the excess heteropolyacid or a salt thereof.
[0084] The volume of the solution or suspension varies depending on the carrier used, the supporting method, etc. The carrier impregnated with the heteropolyacid or its salt is placed in a heating oven for several hours to evaporate the solvent, thereby obtaining a silica-supported heteropolyacid catalyst, which is a solid acid catalyst supported on a carrier. There is no particular limitation on the drying method, and various methods such as a static method and a belt conveyor method can be used. In addition, the amount of the heteropolyacid or its salt supported on the carrier can be accurately measured by chemical analysis such as ICP and XRF.
[0085] The amount of the heteropolyacid or a salt thereof supported on the carrier is preferably 10 to 300 parts by mass, more preferably 50 to 200 parts by mass, and even more preferably 80 to 130 parts by mass, in terms of the total mass of the heteropolyacid or a salt thereof, per 100 parts by mass of the silica carrier.
[0086] (Total volume of pores with a diameter of 6 nm or less) As the amount of heteropolyacid supported increases, the pores of the silica support become blocked. Therefore, by adjusting the amount of heteropolyacid supported, it is possible to control the pore size distribution of the silica-supported heteropolyacid catalyst.
[0087] In the silica-supported heteropolyacid catalyst, the total volume of pores having a pore size of 6 nm or less as determined by gas adsorption (BJH method: Barrett, Joyner, Hallender method) per gram of the silica-supported heteropolyacid catalyst is 0.05 mL / g or less, more preferably 0.04 mL / g or less, and even more preferably 0.02 mL / g or less.
[0088] The total volume of pores having a diameter of 6 nm or less as determined by a gas adsorption method (BJH method) can be measured by the method described in the Examples.
[0089] It is believed that pores with a pore size of 6 nm or less have poor diffusion properties for the produced ethanol and the substrate ethylene. Therefore, by reducing the number of pores with a pore size of 6 nm or less, the diffusion properties of ethanol and ethylene out of the catalyst are improved, leading to a reduction in their residence time in the catalyst, and as a result, the production of by-products such as acetaldehyde produced by the successive reaction of ethanol and butene produced by the dimerization of ethylene is suppressed. EXAMPLES
[0090] The present invention will be further described with reference to the following examples and comparative examples. However, these examples etc. show the outline of the present invention, and the present invention is not limited to these examples etc.
[0091] (Method for measuring pore size of silica-supported heteropoly acid catalyst) The pore size distribution was measured by the BJH method. Specifically, the pore size distribution of the silica-supported heteropolyacid catalyst was measured by nitrogen gas adsorption using a gas adsorption apparatus (TriStar3000, manufactured by Shimadzu Corporation).
[0092] (Analysis of the total volume of pores with a diameter of 6 nm or less) At the same time as measuring the pore distribution, the total volume of pores with a pore size of 6 nm or less per gram of catalyst was analyzed by the BJH method.
[0093] (Analysis of reaction gas) The sampled gas was analyzed using a gas chromatography device (device name: 7890, manufactured by Agilent) with a system program using multiple columns and two detectors under the following conditions. Gas Chromatography Conditions: Oven: Hold at 40°C for 3 minutes, then increase temperature to 200°C at 20°C / min. Carrier gas: Helium Split ratio: 10:1 Column used: Agilent Technologies HP-1(2m)+GasPro(30m)32m×320μm×0μm DB-624: 60m x 320μm x 1.8μm Detector: Front detector: FID (heater: 230°C, hydrogen flow rate: 40 mL / min, air flow rate: 400 L / min) Back detector: FID (heater: 230°C, hydrogen flow rate: 40 mL / min, air flow rate: 400 L / min) Auxiliary detector: TCD (heater: 230℃, reference flow rate: 45mL / min, makeup flow rate: 2mL / min)
[0094] (Analysis of reaction solution) The sampled reaction solution was analyzed using a gas chromatography device (device name: 6850, manufactured by Agilent Corporation). The water concentration in the reaction solution was analyzed using a Karl Fischer analyzer manufactured by Mitsubishi Chemical Corporation. Column used: PoraBONDQ 25m x 0.53mmID x 10μm Oven temperature: 100°C for 2 minutes, then increase to 240°C at 5°C / min. Injection temperature: 250℃ Detector temperature: 300℃
[0095] (Calculation method of reaction results) The space-time yield of ethanol, the ethanol selectivity, the acetaldehyde selectivity, and the butene selectivity were calculated by the following equations. Ethanol space-time yield (kg / h / m 3 ) = (mass of ethanol produced per hour) / (volume of catalyst used) Ethanol selectivity (%) = (moles of ethanol produced / moles of ethylene fed) x 100 Acetaldehyde selectivity (mol%)=(moles of acetaldehyde produced / moles of ethylene fed)×100 Butene selectivity (mol%)=(moles of butene produced / moles of ethylene fed)×100 The butene was determined as the total amount of 1-butene and 2-butene.
[0096] <Example 1> (Preparation of Silica Support A) 40 parts by mass of fumed silica (Aerosil (trademark) 300, manufactured by Nippon Aerosil Co., Ltd.), 60 parts by mass of silica gel (CARiACT G8, manufactured by Fuji Silysia Chemical Ltd.), and 40 parts by mass of colloidal silica (Snowtex O, manufactured by Nissan Chemical Co., Ltd.) were kneaded in a kneader, and then water and additives such as methylcellulose (SM-4000, manufactured by Shin-Etsu Chemical Co., Ltd.) and a resin-based binder (Celander (registered trademark) YB-132A, manufactured by Yuken Kogyo Co., Ltd.) were added to the kneader in appropriate amounts and further kneaded to prepare a kneaded product.
[0097] The prepared kneaded material was then put into an extrusion molding machine equipped with a die with a 3 mm diameter circular hole at the tip. The intermediate extruded from the extrusion molding machine was cut with a cutter to a length of 3 mm to obtain a cylindrical pre-fired molded body. The obtained pre-fired molded body was molded into a sphere using a Marmerizer (registered trademark), pre-dried at 70°C, and then fired at a temperature of 820°C in an air atmosphere to obtain a silica carrier A.
[0098] (Measurement of water absorption rate of silica carrier A) The water absorption rate of the obtained silica carrier A was measured by the following method. (1) Approximately 5 g of the carrier was weighed on a balance (W1(g)) and placed in a 100 mL beaker. (2) Approximately 15 mL of pure water (ion-exchanged water) was added to the beaker so as to completely cover the carrier. (3)Left it for 30 minutes. (4) The carrier and pure water were poured onto the wire mesh, the pure water was drained using the wire mesh, and the carrier was taken out. (5) Water adhering to the surface of the carrier was removed by gently pressing the surface with a paper towel until the surface no longer had any gloss. (6) The total mass of the carrier and the pure water obtained in (5) was measured (W2 (g)). (7) The water absorption rate of the carrier was calculated using the following formula. Water absorption rate (g-water / g-carrier) (%) = (W2-W1) / W1 x 100 Therefore, the water absorption amount (g) of the carrier can be calculated by "water absorption rate of the carrier (g-water / g-carrier) (%) x mass (g) of the carrier used".
[0099] (Preparation of Silica-Supported Heteropoly Acid Catalyst 1) Commercially available Keggin-type tungstosilicic acid 26-hydrate (H4SiW 12 O 40 15.0 g of silicotungstic acid (100 mL) was weighed into a 100 mL beaker, dissolved by adding a small amount of distilled water, and then transferred to a 200 mL graduated cylinder. Next, distilled water was added so that the amount of the silicotungstic acid solution in the graduated cylinder was 95% of the water absorption rate of the silica carrier A to be supported, and the mixture was stirred to make the whole mixture uniform. After stirring, the aqueous solution of silicotungstic acid was transferred to a 200 mL graduated flask, and then 30 mL (about 16 g) of silica carrier A was added to the 200 mL graduated flask, and the contents of the graduated flask were mixed so that the aqueous solution of silicotungstic acid was distributed throughout the carrier, thereby supporting silicotungstic acid on silica carrier A. The silica carrier A supporting silicotungstic acid was transferred to a magnetic dish, air-dried for 1 hour, and then dried for 5 hours in a hot air dryer adjusted to 130°C. After drying, the product was transferred into a desiccator and cooled to room temperature, thereby obtaining silica-supported heteropolyacid catalyst 1.
[0100] (Heteropolyacid supported amount) Table 1 shows the amount of heteropolyacid (silicotungstic acid) supported per 100 parts by mass of the support, assuming that the entire amount of the heteropolyacid used in the preparation is supported.
[0101] (Measurement of pore size distribution) The pore size distribution of the obtained silica-supported heteropolyacid catalyst 1 was measured by the above-mentioned method, and the results are shown in FIG.
[0102] (Analysis of the total volume of pores with a diameter of 6 nm or less) The total volume of pores having a pore size of 6 nm or less per 1 g of the obtained silica-supported heteropolyacid catalyst 1 was analyzed by the above-mentioned method. The results are shown in Table 1.
[0103] (Ethylene hydration) 30 mL of the obtained silica-supported heteropolyacid catalyst 1 was weighed out and packed into a SUS vertical gas-phase fixed-bed reactor, which was then purged with nitrogen gas and then pressurized to 2.0 MPaG. The reactor was then heated to 180°C, and when the temperature was stabilized, water vaporized by an evaporator and ethylene were fed to the reactor in amounts such that the GHSV (Gas Hourly Space Velocity) was 3000 / hr and the molar ratio to ethylene was 0.3, to carry out the hydration reaction of ethylene.
[0104] (Calculation of reaction results) After feeding water and ethylene, and once the temperature had stabilized, the temperature of the reactor was adjusted so as to achieve the target average catalyst layer temperature shown in Table 1. Two hours after the temperature had stabilized, the gas that had passed through the reactor was cooled, and the condensed liquid (reaction liquid) and the reaction gas from which the condensed liquid (reaction liquid) had been removed were each sampled for one hour. The obtained condensed liquid (reaction liquid) and reaction gas were each analyzed by the above-mentioned methods, and the reaction performance of silica-supported heteropolyacid catalyst 1 was calculated from the mass, gas flow rate, and analysis results. The results are shown in Table 1.
[0105] <Example 2> (Preparation of Silica Support B) Silica carrier B was produced in the same manner as silica carrier A, except that natural silica powder (purity 99.0%, average pore size 8 nm) was mixed with methylcellulose SM-4000 (Shin-Etsu Chemical Co., Ltd.) as an additive and a resin binder (Celander (registered trademark) YB-132A (Yuken Kogyo Co., Ltd.) and rolled into 3 mm spheres. The mixture was then calcined at 650° C. in an air atmosphere. The water absorption rate of silica carrier B was measured in the same manner as in Example 1.
[0106] (Preparation of Silica-Supported Heteropoly Acid Catalyst 2) Silica-supported heteropolyacid catalyst 2 was prepared in the same manner as silica-supported heteropolyacid catalyst 1, except that 30 mL (about 18 g) of silica support B was used.
[0107] For the obtained silica-supported heteropolyacid catalyst 2, the amount of heteropolyacid supported was calculated, the pore size distribution was measured, and the total volume of pores with a pore size of 6 nm or less was analyzed in the same manner as in Example 1. Then, ethylene hydration reaction was carried out in the same manner as in Example 1, and the reaction results were evaluated. The results are shown in Table 1.
[0108] <Example 3> (Preparation of Silica Support C) As the silica carrier C, 30 mL (about 19 g) of silica gel (CARIACT G6, manufactured by Fuji Silysia Chemical Ltd.) was used, and the water absorption rate of the silica carrier C was measured in the same manner as in Example 1.
[0109] (Preparation of Silica-Supported Heteropolyacid Catalyst 3) Silica-supported heteropolyacid catalyst 3 was prepared in the same manner as in Example 1, except that the silica support C and 22.7 g of tungstosilicic acid 26-hydrate were used.
[0110] For the obtained silica-supported heteropolyacid catalyst 3, the amount of heteropolyacid supported was calculated, the pore size distribution was measured, and the total volume of pores with a pore size of 6 nm or less was analyzed in the same manner as in Example 1. Then, ethylene hydration reaction was carried out in the same manner as in Example 1, and the reaction results were evaluated. The results are shown in Table 1.
[0111] <Comparative Example 1> (Preparation of Silica Support C) The same silica carrier C as in Example 3 was prepared.
[0112] (Preparation of Silica-Supported Heteropoly Acid Catalyst 4) Silica-supported heteropolyacid catalyst 4 was prepared in the same manner as in Example 1, except that silica support C was used.
[0113] For the obtained silica-supported heteropolyacid catalyst 4, the amount of heteropolyacid supported was calculated, the pore size distribution was measured, and the total volume of pores with a pore size of 6 nm or less was analyzed in the same manner as in Example 1. Then, ethylene hydration reaction was carried out in the same manner as in Example 1, and the reaction results were evaluated. The results are shown in Table 1.
[0114] [Table 1] [Industrial Applicability]
[0115] The present invention provides a method for producing an alcohol by the hydration reaction of an olefin using a silica-supported heteropolyacid catalyst having a total volume of pores with a pore size of 6 nm or less of 0.05 mL / g or less, thereby making it possible to reduce the production of by-products in the reaction and is industrially useful.
Claims
1. A method for producing an alcohol, comprising the steps of: producing an alcohol by a hydration reaction of an olefin having 2 to 5 carbon atoms in the presence of a silica-supported heteropolyacid catalyst in which a heteropolyacid or a salt thereof is supported on a silica support, the method comprising the steps of: The silica-supported heteropolyacid catalyst has a total volume of pores having a pore size of 6 nm or less of 0.05 mL / g or less, The method for producing an alcohol, wherein the amount of the heteropolyacid or a salt thereof supported on the silica carrier is 85 to 200 parts by mass per 100 parts by mass of the silica carrier.
2. 2. The method for producing an alcohol according to claim 1, wherein the heteropolyacid is at least one selected from the group consisting of silicotungstic acid, phosphotungstic acid, phosphomolybdic acid, silicomolybdic acid, silicovanadotungstic acid, phosphovanadotungstic acid, and phosphovanadomolybdic acid.
3. The method for producing an alcohol according to claim 1 or 2, wherein the olefin is ethylene and the alcohol is ethanol.
Citation Information
Patent Citations
Method and catalyst for hydration of olefin
JP1996192047A
Method of hydrating olefin
JP1996225473A
Production of ethanol
JP1998101601A
Production of ethanol
JP1998298122A
Silica gel for carrier of olefin hydration catalyst and catalyst for olefin hydration
JP2003190786A