Optical fiber manufacturing method

By manufacturing a seed rod with controlled OH group concentration and optimizing the dehydration and vitrification process, the method addresses high OH group concentrations near the seed rod, reducing transmission loss and manufacturing costs in optical fibers.

JP7571607B2Active Publication Date: 2024-10-23SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021025144
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-10-23
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

The concentration of OH groups near the seed rod in the transparent glass base material is high, leading to increased transmission loss in optical fibers, necessitating the discarding of this portion and increasing manufacturing costs.

Method used

Manufacture a seed rod with an average OH group concentration of 1 ppm or less within 0.05 mm to 0.5 mm from the surface and implement a dehydration and transparent vitrification process to reduce OH group diffusion, allowing the use of the previously discarded portion for optical fiber production.

Benefits of technology

This method reduces transmission loss in optical fibers, enabling the use of the near-seed rod portion and lowering manufacturing costs by stabilizing the fiber production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571607000001
    Figure 0007571607000001
  • Figure 0007571607000002
    Figure 0007571607000002
  • Figure 0007571607000003
    Figure 0007571607000003
Patent Text Reader

Abstract

To reduce the concentration of OH group in a portion near a seed rod in a transparent glass preform to make it possible to manufacture an optical fiber having a small transmission loss derived from the OH group even when using the portion near the seed rod in the transparent glass preform.SOLUTION: A method for manufacturing an optical fiber preform comprises: a seed rod manufacturing step of manufacturing a seed rod having an average OH group concentration of 1 ppm or less in a region having a distance of 0.05 mm or more and 0.5 mm or less from the surface in a tip; a glass fine particle deposit manufacturing step of depositing glass fine particles formed by supplying a glass raw material to a burner on the rotating seed rod to manufacture a glass fine particle deposit; a dehydration step of heating and dehydrating the glass fine particle deposit by a heater in dehydration gas; and a transparent vitrification step of heating the glass fine particle deposit by the heater after the dehydration step to obtain a transparent glass preform.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing an optical fiber preform and a method for manufacturing an optical fiber. [Background technology]

[0002] Patent Document 1 discloses a method for producing a glass particle deposit by depositing glass particles on a seed rod using a vapor phase axial deposition (VAD) method. The glass particle deposit thus obtained, with the seed rod attached to one end, is turned into a transparent glass preform through a dehydration process and a transparent vitrification process by sintering. The obtained transparent glass preform is then drawn to produce an optical fiber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-178630 A Summary of the Invention [Problem to be solved by the invention]

[0004] When a transparent glass preform is manufactured from the soot glass deposit obtained by the method disclosed in Patent Document 1, the concentration of OH groups is high in the portion of the transparent glass preform close to the seed rod, even though OH groups are removed from the soot glass deposit in the dehydration process. If such a portion with a high concentration of OH groups is used to manufacture an optical fiber, the transmission loss will be large. For this reason, in the past, the portion of the transparent glass preform close to the seed rod was discarded and not used in the manufacture of an optical fiber. Discarding a portion of the transparent glass preform ultimately contributes to an increase in the manufacturing cost of the optical fiber.

[0005] The objective of the present disclosure is to reduce the concentration of OH groups in a portion of a transparent glass preform close to a seed rod, thereby enabling the production of an optical fiber with low transmission loss due to OH groups even when using the portion of a transparent glass preform close to a seed rod. [Means for solving the problem]

[0006] A method for producing an optical fiber preform according to one embodiment of the present disclosure includes the steps of: a seed rod manufacturing process for manufacturing a seed rod having an average OH group concentration of 1 ppm or less in a region at a distance of 0.05 mm or more and 0.5 mm or less from the surface at the tip; a glass soot deposit manufacturing step of manufacturing a glass soot deposit by supplying glass raw material to a burner to generate glass soot and depositing the glass soot on the rotating seed rod; a dehydration step of heating the soot glass deposit body in a dehydrating gas using a heater to dehydrate the soot glass deposit body; a transparent vitrification step of heating the soot glass deposit by the heater after the dehydration step to obtain a transparent glass base material; Equipped with.

[0007] A method for producing an optical fiber according to one aspect of the present disclosure includes the steps of: The present invention also includes manufacturing an optical fiber using a region of the optical fiber preform obtained by the manufacturing method for the optical fiber preform that is within 10 mm in the axial direction from the tip of the seed rod, and manufacturing an optical fiber having a transmission loss at a wavelength of 1380 nm that is an increase of less than 40 mdB / km compared to an optical fiber manufactured using a portion of the optical fiber preform that is located 100 mm in the axial direction from the tip of the seed rod. Effect of the Invention

[0008] According to the disclosed configuration, even if a part of a transparent glass preform close to a seed rod, which has been discarded in the past, is used, it is possible to manufacture an optical fiber with low transmission loss due to OH groups. As a result, the manufacturing cost of the optical fiber can be reduced. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing the diffusion of OH groups from a seed rod in the transparent vitrification process. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for producing an optical fiber preform according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a graph showing an example of the OH group concentration at the tip of the seed rod according to the present disclosure. [Figure 4] FIG. 4 is a graph showing the diffusion of OH groups when the seed rod according to the present disclosure is heated. [Diagram 5] FIG. 5 is an example of an infrared absorption spectrum of a seed rod. [Figure 6] FIG. 6 is a graph showing the transmission loss of optical fibers produced from the optical fiber preforms produced in each production example. [Figure 7] FIG. 7 is a graph showing the relationship between the length of the tip of the seed rod and the incidence rate of increased OH loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present inventors have conducted various studies to clarify the cause of the problem of the high concentration of OH groups in the part of the transparent glass base material close to the seed rod. First, the present inventors focused on the dehydration process and conducted experiments by changing conditions such as the temperature and time in the dehydration process and the concentration of chlorine gas introduced during dehydration, but the problem of the high concentration of OH groups was not solved. In addition, the possibility that outside air was entering from outside the furnace tube during the transparent vitrification process was also considered, but it was found that this was not related to the above problem.

[0011] As a result of various studies as described above, the present inventors have found that the above problem occurs due to the release of OH groups from a heated seed rod. FIG. 1 is a schematic diagram showing the diffusion of OH groups from a seed rod 10' in a transparent vitrification process. In the transparent vitrification process, a glass soot deposit M1 with a seed rod 10' attached to one end is placed in a furnace tube 31 and heated by a heater 32 to obtain a transparent glass base material. At this time, the OH groups contained in the seed rod 10' are diffused to the outside by heating, and diffuse into the core portion M11 and clad portion M12 of the glass soot deposit M1. Then, the OH groups remaining in the core portion M11 eventually cause transmission loss. The present disclosure has been made based on such findings.

[0012] [Description of the embodiments of the present disclosure] The embodiments of the present disclosure will be listed and described. A method for producing an optical fiber preform according to one embodiment of the present disclosure includes the steps of: a seed rod manufacturing process for manufacturing a seed rod having an average OH group concentration of 1 ppm or less in a region at a distance of 0.05 mm or more and 0.5 mm or less from the surface at the tip; a glass soot deposit manufacturing step of manufacturing a glass soot deposit by supplying glass raw material to a burner to generate glass soot and depositing the glass soot on the rotating seed rod; a dehydration step of heating the soot glass deposit body in a dehydrating gas using a heater to dehydrate the soot glass deposit body; a transparent vitrification step of heating the soot glass deposit by the heater after the dehydration step to obtain a transparent glass base material; Equipped with. According to this configuration, the concentration of OH groups in the transparent glass preform close to the seed rod is reduced, and even when the transparent glass preform close to the seed rod is used, it is possible to manufacture an optical fiber with low transmission loss due to OH groups, thereby reducing the manufacturing cost of the optical fiber.

[0013] In the method for producing an optical fiber preform, The seed rod manufacturing step is preferably a step of manufacturing a seed rod having an average OH group concentration of 3 ppm or less in a region at the tip end that is 0.05 mm or more and 2.0 mm or less away from the surface. This configuration makes it possible to further reduce the concentration of OH groups in the portion of the transparent glass preform close to the seed rod, and as a result, even when an optical fiber is manufactured using the portion of the transparent glass preform close to the seed rod, it becomes possible to stably manufacture an optical fiber with low transmission loss due to OH groups.

[0014] In the method for producing an optical fiber preform, The length of the tip portion is preferably equal to or greater than half the length of the heater. This configuration makes it possible to further reduce the concentration of OH groups in the portion of the transparent glass preform close to the seed rod, and as a result, even when an optical fiber is manufactured using the portion of the transparent glass preform close to the seed rod, it becomes possible to stably manufacture an optical fiber with low transmission loss due to OH groups.

[0015] A method for producing an optical fiber according to one aspect of the present disclosure includes the steps of: The present invention also includes manufacturing an optical fiber using a region of the optical fiber preform obtained by the manufacturing method for the optical fiber preform that is within 10 mm in the axial direction from the tip of the seed rod, and manufacturing an optical fiber having a transmission loss at a wavelength of 1380 nm that is an increase of less than 40 mdB / km compared to an optical fiber manufactured using a portion of the optical fiber preform that is located 100 mm in the axial direction from the tip of the seed rod. According to this configuration, even if the part of the transparent glass preform close to the seed rod, which was conventionally discarded, is used, it is possible to manufacture an optical fiber with low transmission loss due to OH groups, which results in a reduction in the manufacturing cost of the optical fiber.

[0016] [Details of the embodiment of the present disclosure] Hereinafter, examples of embodiments according to the present disclosure will be described with reference to the drawings. In the following description, the same or equivalent elements are denoted by the same reference numerals even in different drawings, and duplicated descriptions will be omitted as appropriate. In addition, the scale of each drawing used in the following description is appropriately changed so that each component can be recognized.

[0017] (Method of manufacturing optical fiber base material) 2 is a schematic diagram showing a method for manufacturing an optical fiber preform (hereinafter also referred to as a "transparent glass preform") M2 according to an embodiment of the present disclosure. As shown in FIG. 2, the method for manufacturing the optical fiber preform M2 according to the embodiment includes steps 1 to 4.

[0018] Step 1 is a seed rod manufacturing step for manufacturing the seed rod 10. The seed rod 10 satisfies the below-described condition 1 regarding the average OH group concentration at least in the tip portion 11 (the portion between the tip P2 and the position P1). The axial length a of the tip portion 11 is preferably, for example, half or more of the axial length b of the heater 32. This is because it is preferable that the tip P2 of the seed rod 10 descends to near the center of the heater 32 in the below-described step 4 (transparent vitrification step). In this case, the portion up to a position axially spaced a length b / 2 from the tip P2 enters the heat zone of the heater 32 in the transparent vitrification step. The portion that enters the heat zone is heated more strongly than the other portions of the seed rod 10, and therefore the OH groups are more likely to diffuse into the transparent glass base material M2. However, such diffusion can be prevented by making the length a of the tip portion 11 half or more of the length b of the heater 32.

[0019] FIG. 3 is a graph showing an example of the OH group concentration at the tip 11 of the seed rod 10. The seed rod 10 satisfies condition 1 that the average OH group concentration in the region R1 at a distance from the surface of 0.05 mm to 0.5 mm is 1 ppm or less. Conventionally, the OH groups that were the cause of transmission loss were mainly due to the OH groups present in the region R1. Therefore, by making the average OH group concentration in the region R1 1 ppm or less, it is possible to prevent the OH groups originating from the seed rod 10 from diffusing and remaining in the transparent glass base material M2. In addition to condition 1, the seed rod 10 preferably satisfies condition 2 that the average OH group concentration in the region R2 at a distance from the surface of 0.05 mm to 2.0 mm is 3 ppm or less.

[0020] In the region R3 at a distance of 0 mm or more and less than 0.05 mm from the surface, there is no condition regarding the average OH group concentration, and the average OH group concentration may reach several thousand ppm, for example. This is because the OH groups contained in the region R3 diffuse from the seed rod 10 to the soot glass deposit M1 in step 2 (dehydration step), and are further removed from the soot glass deposit M1.

[0021] Fig. 4 is a graph showing the diffusion of OH groups when the seed rod 10 is heated, and is a theoretical graph calculated from a diffusion equation. As shown in Fig. 4, the OH groups present in the region more than 0.5 mm away from the surface remain inside the seed rod 10 even after heating for 4 hours, and are unlikely to diffuse outside the seed rod 10. This shows that the average OH group concentration in the region R1, which is 0.05 mm to 0.5 mm away from the surface, is the most important.

[0022] The average OH group concentration of the seed rod 10 can be measured by a conventionally known method. For example, the average OH group concentration of the seed rod 10 can be calculated by observing the OH stretching vibration of Si-OH in an infrared absorption spectrum.

[0023] Figure 5 is an example of an infrared absorption spectrum of a seed rod. The average OH group concentration of the seed rod is at a wave number of 3670 cm, which corresponds to the OH stretching vibration shown in Figure 5. -1Using the absorption peak I at and the base I0 on the baseline, it can be calculated according to the Lambert-Beer equation of the following formula (1). C OH =α / εt (1)

[0024] In the above formula (1), the absorbance α is calculated by "α = Log10(I0 / I)". The molar absorption coefficient ε can be calculated by the value "ε = 77.5 L / mol cm" given in the paper by G. Stephenson et al. (G. Stephenson, et al., Trans. Br. Ceram. Soc., 59, 397 (1960)). The sample thickness t can be measured with a caliper or the like.

[0025] The distribution of the OH group concentration in the radial direction of the seed rod 10 can be calculated, for example, by the following method. First, the transmittance in the radial direction of the seed rod 10 is measured by the above formula (1), and the average OH group concentration in the radial direction of the seed rod 10 is obtained. Next, the surface of the seed rod 10 is etched by immersing the seed rod 10 in a hydrofluoric acid solution, for example. After that, the average OH group concentration of the seed rod 10 is obtained again by the above formula (1). From the outer diameter and the average OH group concentration of the seed rod 10 before and after etching, the OH group concentration of the etched part is calculated by the following formula (2). By sequentially repeating etching and measurement in the same procedure, the distribution of the OH group concentration in the radial direction of the seed rod 10 can be obtained. (DC-D'C') / (D-D') (2)

[0026] In the above formula (2), "D" is the outer diameter of the seed rod 10 before etching. "D'" is the outer diameter of the seed rod 10 after etching. "C" is the average OH group concentration of the seed rod 10 before etching. "C'" is the average OH group concentration of the seed rod 10 after etching.

[0027] The seed rod 10 can be manufactured by heat treating a glass rod of fused quartz glass manufactured by the electric melting method or synthetic quartz glass manufactured by the soot method in a dry atmosphere to reduce the average OH group concentration in the region R1 to 1 ppm or less. Quartz glass manufactured by the flame fusion method or direct method can also be used as the seed rod 10, but since the OH group concentration contained in the glass is high, it takes time to reduce the average OH group concentration. In addition, synthetic quartz glass sintered in a vacuum in the soot method is preferred because it is easy to obtain a low average OH group concentration in the region R1. Furthermore, synthetic quartz glass sintered by dehydration treatment in the soot method is preferred because it is possible to obtain a low average OH group concentration not only in the region R1 but also in the center (e.g., region R2).

[0028] The seed rod manufacturing process may include a step of flame polishing the surface of the seed rod 10. By carrying out flame polishing, the surface of the seed rod 10 is cleaned and smoothed, and it is possible to prevent crystallization or residual air bubbles at the interface with the deposited glass particles. Crystallization and residual air bubbles can cause cracks, so it is preferable to prevent these occurrences.

[0029] Incidentally, since flame polishing involves applying a burner flame to the surface of the seed rod 10, the OH group concentration on the surface of the seed rod 10 increases as a result of flame polishing. However, this increase in OH group concentration is within a range of 0.05 mm from the surface of the seed rod 10. As described above, within this range, the OH groups are released from the surface of the seed rod 10 by heating during the dehydration process, and the OH group concentration is reduced during the transparent vitrification process, so there is no effect on the transmission loss of the optical fiber.

[0030] Returning to FIG. 2, steps 2 to 4 will be described below. Step 2 is a glass soot deposit manufacturing step for manufacturing a glass soot deposit M1. In the glass soot deposit manufacturing step, the glass soot deposit M1 is manufactured using, for example, the VAD method. Specifically, a glass raw material gas G1 is supplied to a core burner 21, and core glass soot produced by a flame hydrolysis reaction is deposited on a rotating seed rod 10. Also, a glass raw material gas G2 is supplied to a clad burner 22, and glass soot for clad cores produced by a flame hydrolysis reaction is deposited on the core glass soot. In this manner, the glass soot deposit M1 is manufactured.

[0031] Alternatively, the glass soot deposit M1 may be manufactured using an outside vapor deposition (OVD) method. In the OVD method, a mandrel is inserted into a pipe-shaped seed rod, glass soot is deposited on the outside of the seed rod and the mandrel, and after the deposition of the glass soot is completed, the mandrel is pulled out and, with the seed rod attached to one end of it, a dehydration process and a transparent vitrification process by sintering are carried out to manufacture a transparent glass base material. Therefore, when the OVD method is used, the average OH group concentration in the region at a distance of 0.05 mm to 0.5 mm from the surface on both the inner and outer surfaces of the pipe-shaped seed rod is set to 1 ppm or less.

[0032] The glass raw material gas G1 is a gas for core, which contains, for example, silicon tetrachloride (SiCl4) or siloxane, and a dopant such as germanium tetrachloride (GeCl4). The glass raw material gas G2 is a gas for cladding, which contains, for example, silicon tetrachloride or siloxane, and does not contain a dopant. In the glass soot deposit manufacturing process, a conventionally known configuration can be appropriately adopted.

[0033] Step 3 is a dehydration step for dehydrating the soot glass deposit M1. In the dehydration step, the soot glass deposit M1 is placed in the furnace core tube 31. A dehydration gas G3 (for example, a mixed gas of an inert gas such as nitrogen and chlorine gas) is then supplied to the furnace core tube 31, and the soot glass deposit M1 is lowered in the furnace core tube 31. The soot glass deposit M1 is heated by a heater 32 arranged around the furnace core tube 31 in an atmosphere containing the dehydration gas G3, and a dehydration process is performed. The dehydration process removes OH groups contained in the soot glass deposit M1 and the like. The conditions in the dehydration step, such as temperature and time, can be appropriately set based on conventionally known conditions.

[0034] Step 4 is a transparent vitrification step in which the soot glass deposit M1 is heated by the heater 32 to obtain a transparent glass base material M2. In the transparent vitrification step, the soot glass deposit M1, which has moved downward in the furnace tube 31 in the dehydration step, is raised to the upper part of the furnace tube 31. Then, an inert gas G4 (e.g., nitrogen, helium, etc.) is supplied to the furnace tube 31, and the soot glass deposit M1 is lowered in the furnace tube 31. The soot glass deposit M1 is heated and sintered by the heater 32 in an atmosphere containing the inert gas G4, and becomes a transparent glass base material M2. In the transparent vitrification step, it is preferable to lower the tip P2 of the seed rod 10 to near the center of the heater 32. Conditions such as temperature and time in the transparent vitrification step can be appropriately set based on conventionally known conditions.

[0035] The transparent glass preform M2 manufactured through the above steps 1 to 4 has a lower OH group concentration in region M21 close to the seed rod 10 than when manufactured by the conventional manufacturing method. Therefore, region M21, which was conventionally discarded, can also be used as a preform for an optical fiber. Region M21 is a region between positions P5 and P6. Position P5 is a position corresponding to the tip P2 of the seed rod 10. Position P6 is, for example, a position 100 mm axially downward from position P5.

[0036] (Optical fiber manufacturing method) The manufacturing method of the optical fiber according to the present embodiment will be described below. The manufacturing method of the optical fiber according to the present embodiment is a manufacturing method for manufacturing an optical fiber using a region within 10 mm in the axial direction from the tip P2 of the seed rod 10 of the optical fiber preform M2 obtained by the manufacturing method of the optical fiber preform described above, and manufacturing an optical fiber in which the increase in transmission loss at a wavelength of 1380 nm is less than 40 mdB / km is based on an optical fiber manufactured using a portion of the optical fiber preform M2 located 100 mm in the axial direction from the tip P2 of the seed rod 10. Note that an increase of less than 40 mdB / km from the reference also includes a case in which the transmission loss is lower than the reference.

[0037] The optical fiber preform M2 is turned into an optical fiber through a conventionally known process for producing an optical fiber from the transparent glass preform M2, such as a drawing process. The region M21 of the optical fiber preform M2 obtained by the above-mentioned method for producing an optical fiber preform has a low average OH group concentration, and therefore the transmission loss at a wavelength of 1380 nm of the optical fiber obtained by using the region within 10 mm in the axial direction from the tip P2 of the seed rod 10 (hereinafter, the transmission loss T 10 The transmission loss of the optical fiber manufactured using the portion of the seed rod 10 located 100 mm in the axial direction from the tip P2 (hereinafter, the transmission loss T 100 This is an increase of less than 40 mdB / km compared to the T 10 -T 100 <40 mdB / km". The method for manufacturing an optical fiber according to this embodiment also includes manufacturing an optical fiber using a region within 10 to 100 mm in the axial direction from the tip P2 of the seed rod 10 or a region below region M21 shown in FIG. 2.

[0038] [Example] The present disclosure will be described in more detail below by showing examples according to the present disclosure. Note that the present disclosure is not limited to the following examples.

[0039] (Production Examples 1 to 5) Synthetic quartz glass produced by the soot method was heat-treated in a dry atmosphere to produce three low-OH seed rods, one of which was confirmed to satisfy the above-mentioned condition 1 but not condition 2. Synthetic quartz glass produced by the soot method was heat-treated in a dry atmosphere to dehydrate it to produce three low-OH seed rods, one of which was confirmed to satisfy the above-mentioned conditions 1 and 2. Two regular seed rods, which were commercially available fused quartz glass produced by the electric melting method, were also prepared. It was confirmed from one of the regular seed rods that the average OH group concentration in the area at the tip from 0.05 mm to 0.5 mm away from the surface was 130 ppm.

[0040] The above-mentioned glass particle deposit manufacturing process, dehydration process, and transparent vitrification process were carried out under the same conditions for each of the four low OH seed rods and one normal seed rod, to manufacture five transparent glass preforms M2. Next, each of the obtained transparent glass preforms M2 was drawn under the same conditions to manufacture optical fibers. The transmission loss at 1380 nm was measured for each of the obtained optical fibers. The results are shown in FIG. 6. Note that Manufacturing Examples 1 and 2 are manufacturing examples using low OH seed rods that satisfy condition 1 but do not satisfy condition 2. Manufacturing Examples 3 and 4 are manufacturing examples using low OH seed rods that satisfy condition 1 and condition 2. Manufacturing Example 5 is a manufacturing example using a normal seed rod.

[0041] Fig. 6 is a graph showing the transmission loss of optical fibers manufactured from the optical fiber preform M2 manufactured in each manufacturing example. Each plot point in the graph of Fig. 6 corresponds to the transparent glass preform M2 shown at the top of the graph. For example, the transmission loss of an optical fiber manufactured using the preform at position P6 is a value on the line showing position P6.

[0042] As can be seen from FIG. 6, when a normal seed rod not satisfying condition 1 is used, the optical fiber manufactured using region M21 exhibits a significant increase in transmission loss. On the other hand, when a low-OH seed rod satisfying condition 1 is used, even the optical fiber manufactured using region M21 does not exhibit a significant increase in transmission loss. In particular, Manufacturing Examples 3 and 4, which use low-OH seed rods satisfying conditions 1 and 2, exhibit low transmission loss values. Note that, T 10 -T100 Specifically, the values ​​are 3 mdB / km for Manufacturing Example 1, 3 mdB / km for Manufacturing Example 2, 3 mdB / km for Manufacturing Example 3, 3 mdB / km for Manufacturing Example 4, and 46 mdB / km for Manufacturing Example 5. In addition, in Manufacturing Examples 1 to 4, the transmission loss of the optical fibers manufactured using region M21 is 0.31 dB / km or less.

[0043] (Examples 6 to 10) The transparent glass preform M2 was manufactured under the same conditions except that the length a of the tip 11 of the seed rod 10 was changed to 0.1 times, 0.2 times, 0.5 times, 0.8 times, and 1 times the length b of the heater 32. In the transparent vitrification process, the tip P2 of the seed rod 10 was lowered to near the center of the heater 32.

[0044] Next, each of the obtained transparent glass preforms M2 was drawn under the same conditions to manufacture optical fibers. For each transparent glass preform M2, the optical fibers manufactured using the portion located 10 mm axially downward from position P5 were judged for the presence or absence of an increase in OH loss (transmission loss due to OH groups). The increase in OH loss was judged to have occurred when the transmission loss at 1380 nm increased by 40 mdB / km or more, based on the optical fiber manufactured using the portion located 100 mm axially downward from position P5.

[0045] The transparent glass preform M2 was manufactured multiple times under each of the above conditions for the length a of the tip portion 11, and the occurrence rate of increased OH loss under each condition (the number of transparent glass preforms M2 manufactured under the same conditions that had increased OH loss / the number of transparent glass preforms M2 manufactured under the same conditions) was calculated. The results are shown in FIG.

[0046] It can be seen from FIG. 7 that by making the length a of the tip portion 11 0.5 times or more the length b of the heater 32, the occurrence rate of increased OH loss can be reduced.

[0047] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. Furthermore, the number, position, shape, etc. of the components described above are not limited to the above embodiments, and can be changed to the number, position, shape, etc. that are suitable for implementing the present invention. [Explanation of symbols]

[0048] 10',10: Seed stick 11:Tip 21: Core burner 22: Burner for clad 31: Furnace tube 32: Heater G1, G2: Glass raw material gas G3: Dehydrated gas G4: Inert gas M1: Glass particle deposit M11: Core section M12: Clad section M2: Transparent glass base material (base material for optical fiber) M21:Area R1,R2,R3: area

Claims

1. a seed rod manufacturing process for manufacturing a seed rod having an average OH group concentration of 1 ppm or less in a region at a tip end portion that is 0.05 mm or more and 0.5 mm or less away from the surface; a glass soot deposit manufacturing step of manufacturing a glass soot deposit by supplying glass raw material to a burner to generate glass soot and depositing the glass soot on the rotating seed rod; a dehydration step of heating the soot glass deposit body in a dehydrating gas using a heater to dehydrate the soot glass deposit body; a transparent vitrification step of heating the soot glass deposit by the heater after the dehydration step to obtain a transparent glass base material; using a region of the optical fiber preform obtained by the method for producing an optical fiber preform comprising the steps of: and manufacturing an optical fiber having a transmission loss at a wavelength of 1380 nm that increases by less than 40 mdB / km based on an optical fiber manufactured using a portion of the optical fiber preform that is located 100 mm axially from the tip of the seed rod.

2. 2. The method for producing an optical fiber according to claim 1, wherein the seed rod production step is a step of producing a seed rod having an average OH group concentration of 3 ppm or less in a region at a distance of 0.05 mm or more and 2.0 mm or less from the surface at the tip portion.

3. 3. The method for producing an optical fiber according to claim 1, wherein the length of the tip portion is equal to or greater than half the length of the heater.

Citation Information

Patent Citations

  • Manufacture of optical fiber preform

    JP1986072643A

  • Method for manufacturing glass particulate deposit

    JP2005029399A

  • Method of manufacturing glass preform

    JP2005298287A

  • Method of manufacturing glass preform for optical fiber

    JP2007045643A

  • Production method of glass fine particle deposit

    JP2017178630A