High-performance ceramics
A glaze layer with spherical silica particles and MgO, treated with an alkaline solution, enhances ceramic surfaces' oil repellency and durability, addressing peeling issues and improving oil stain removal efficiency in dishwashers.
Patent Information
- Application Number
- JP2020120832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-14
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-07-14
AI Technical Summary
Conventional methods for improving the oil repellency and durability of ceramic surfaces are inadequate, leading to peeling or dissolution of coatings in hot water, high manufacturing costs due to expensive raw materials and additional heating steps, and insufficient oil stain removal efficiency, especially in dishwashers.
A glaze layer on ceramic surfaces containing spherical silica particles and MgO with specific dimensions and grooves, treated with an alkaline solution to enhance oil repellency and durability, allowing easy oil stain removal with running water.
The glaze layer achieves improved oil repellency and durability, enabling effective oil stain removal in dishwashers and reducing water and detergent usage, while maintaining functionality over time.
Smart Images

Figure 0007571948000001 
Figure 0007571948000002 
Figure 0007571948000003
Abstract
Description
[Technical field]
[0001] The present invention relates to high-performance ceramics that improve the oil stain removal performance by improving the oil repellency of the surface for ceramic tableware, kitchen interior tiles, etc. used in ordinary households, businesses, school lunches, etc., and that can maintain this function for a long period of time. [Background technology]
[0002] Many methods have been reported for imparting hydrophilicity to ceramic tableware or tiles by applying various alkoxide or sol silica raw materials, or silica microparticles and a siliceous binder, to the surface of the tableware or tiles, and then heating the surface to approximately 150°C to 700°C to form a silica film, and creating nano-sized irregularities on the surface of the silica film (see, for example, Patent Documents 1, 2, and 3). In addition, there has been a report on sanitary ware in which mill-ground fused silica, silica sand, and feldspar are added to a glaze, the glaze is applied to the surface of a base material, and the glaze is fired at 800°C to 1300°C, thereby reducing surface irregularities and making it easier to remove dirt (see, for example, Patent Documents 4, 5, and 6). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-302637 A [Patent Document 2] JP 2002-080830 A [Patent Document 3] JP 2004-99912 A [Patent Document 4] JP 2001-220270 A [Patent Document 5] JP 2001-48681 A [Patent Document 6] JP 2001-48680 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above conventional techniques have problems in terms of durability, oil repellency, and cost. First, the methods of Patent Documents 1, 2, and 3 have the advantage that the surface is hydrophilized by generating fine irregularities, and the oil adhering to the tableware is easily removed by washing with water. However, since the heat treatment is performed at a relatively low temperature of 700°C or less and silica is simply attached to the substrate, washing with water at room temperature has little effect on durability, but in hand washing using warm water of about 40°C in an ordinary household, or in dishwashing machines using hot water of about 80°C, the coating itself is easily peeled off or dissolved away because alkaline detergent is dissolved in these warm or hot water. Furthermore, detergents for dishwashing machines also contain abrasives such as silicates to remove stuck dirt, and coating materials with thin film thickness and low adhesive strength are easily peeled off. Therefore, even conventional ceramic overpainted products, which have glass frit baked at about 800°C, are classified as unusable in the dishwashing machine instruction manual. In terms of raw material and manufacturing costs, the use of alkoxides and sols, which are more expensive than ceramic raw materials, increases raw material costs, and the manufacturing process also requires a coating process to be applied to a product that has been fired at 1000°C or higher, and then another heating process, which adds an additional heating step, thereby increasing manufacturing costs.
[0005] In Patent Documents 4, 5, and 6, the glaze layer is thick due to the adhesion between the glazes, and thus the durability is sufficient, but the surface of the glaze layer is stabilized and the oil repellency is reduced because it is fired at a high temperature of 1000°C or more. In addition, if the surface is simply smoothed, there are no grooves or depressions on the surface, so the water pressure caused by running water is dispersed, and running water is less likely to enter the gap between the oil stains and the surface of the glaze layer, making it difficult for the oil stains to peel off. Therefore, it is effective for sanitary ware that does not require the removal of oil, but is insufficient for items such as tableware that require the removal of oil on a daily basis. Furthermore, if too much silica fine particles are simply added to the glaze during the manufacturing process, cristobalite is generated during firing, causing cracks, so it was necessary to reduce the amount of silica added to the glaze. [Means for solving the problem]
[0006] As a result of intensive research into solving the above-mentioned problems, the inventors have found that by immersing ceramic ware having a glaze layer on its surface, in which the glaze constituting the glaze layer contains a predetermined amount of spherical silica particles of a predetermined average particle size and a predetermined amount of MgO, relative to 100% by mass of the total solids content, and in which the surface of the glaze layer has one or more grooves of predetermined dimensions, the total opening areas of the grooves occupying a predetermined proportion of the total surface area of the glaze layer, in an alkaline solution, the contact angle of an oil droplet with the surface of the glaze layer reaches a predetermined value as measured by the width-height method, and the oil repellency of the surface can be improved, thereby completing the present invention. That is, the present invention is as follows. [1] A ceramic ware having a glaze layer on its surface, the glaze constituting the glaze layer contains 20 to 50 mass% of spherical silica particles having an average particle size of 10 to 500 nm and 0.5 to 3.0 mass% of MgO relative to 100 mass% of the total solid content; The contact angle of an oil droplet with respect to the surface of the glaze layer is 25 to 50° as measured by a width-height method; The surface of the glaze layer has one or more grooves having a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer. Ceramics. [2] The ceramic according to [1], wherein the spherical silica particles have an average particle size of 50 to 300 nm. [3] The ceramic according to [1] or [2], wherein the contact angle of an oil droplet with the surface of the glaze layer is 30 to 40° as measured by the width-height method. [4] A method for manufacturing ceramic ware having a glaze layer on its surface, comprising the steps of: The method includes the step of immersing the ceramic in an alkaline solution, the glaze constituting the glaze layer contains 20 to 50 mass% of spherical silica particles having an average particle size of 10 to 500 nm and 0.5 to 3.0 mass% of MgO relative to 100 mass% of the total solid content; The surface of the glaze layer has one or more grooves having a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer. Manufacturing method. [5] The manufacturing method according to [4], which includes a step of immersing the ceramic in an alkaline solution having a pH of 9 to 14 and a temperature of 10 to 90°C for 10 minutes to 24 hours. [6] The method according to [4] or [5], wherein the alkaline solution contains at least one selected from the group consisting of sodium hydroxide, potassium hydroxide and barium hydroxide. Effect of the Invention
[0007] The ceramics of the present invention have improved oil repellency on the surface of the glaze layer, as shown by the contact angle of an oil droplet with the surface of the glaze layer being 25 to 50° as measured by the width-height method. In addition, the surface of the glaze layer has one or more grooves of specified dimensions, the total opening area of which occupies a specified proportion of the total surface area of the glaze layer. Therefore, oil stains can be easily removed with a small amount of running water, and the function can be maintained for a long period of time even under the harsh conditions of a dishwasher. This reduces the amount of water and detergent used during washing, making it environmentally friendly. The method for producing ceramics of the present invention includes a step of immersing ceramics having a glaze layer on its surface composed of a glaze having a prescribed composition, the surface of the glaze layer having grooves of prescribed dimensions, the total opening area of the grooves occupying a prescribed proportion of the total surface area of the glaze layer, in an alkaline solution; this step makes it possible to improve the contact angle of an oil droplet with the surface of the glaze layer, as measured by the width-height method, of 25 to 50°, thereby improving the oil repellency of the surface and enhancing the oil stain removal performance. [Brief description of the drawings]
[0008] [Figure 1] 1 shows an electron microscope photograph of the surface of the glaze layer of a ceramic test sample obtained in Example 1. [Diagram 2] 1 shows the results of X-ray diffraction measurement of the surface of a glaze layer in Reference Example 1 that is made of a glaze with an MgO content of 1.5 mass %. [Diagram 3] 1 shows the results of X-ray diffraction measurement of the surface of a glaze layer in Comparative Reference Example 1, which is made of a glaze with an MgO content of 0.3 mass %. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The ceramic of the present invention will now be described. The ceramic of the present invention has a glaze layer on its surface, the glaze constituting the glaze layer contains 20 to 50 mass% of spherical silica particles having an average particle size of 10 to 500 nm and 0.5 to 3.0 mass% of MgO relative to 100 mass% of the total solid content; The contact angle of an oil droplet with respect to the surface of the glaze layer is 25 to 50° as measured by a width-height method; The surface of the glaze layer has one or more grooves having a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer.
[0010] The average particle size of the spherical silica particles is 10 to 500 nm, preferably 50 to 300 nm, and more preferably 70 to 250 nm. If the average particle size is less than 10 nm, the unevenness of sufficient size is not formed on the surface of the glaze layer, and the effect of the present invention cannot be obtained. On the other hand, if the average particle size exceeds 500 nm, the unevenness formed on the surface of the glaze layer becomes too large, and dirt and the like easily adheres to the surface. The content of spherical silica particles in the glaze constituting the glaze layer is 20-50% by mass, preferably 25-45% by mass, and more preferably 30-40% by mass, based on 100% by mass of the total solid content. If the content is less than 20% by mass, the oil repellency is low, and the effect of removing oil stains by using the force of running water during washing is reduced. On the other hand, if the content exceeds 50% by mass, the amount of cristobalite generated during firing increases, and cracks are likely to occur in the glaze layer.
[0011] The average particle size of the spherical silica particles in the present invention is measured by a dynamic light scattering method using an electrophoretic light scattering photometer.
[0012] The content of MgO in the glaze constituting the glaze layer is 0.5 to 3.0% by mass, preferably 1.0 to 2.5% by mass, based on 100% by mass of the total solid content. If the content is less than 0.5% by mass, the amount of cristobalite generated by spherical silica particles that are partially precipitated during firing increases, and cracks tend to occur in the glaze layer. On the other hand, if the content exceeds 3.0% by mass, the glaze melts too much during firing and tends to flow.
[0013] The glaze constituting the glaze layer may contain, in addition to spherical silica particles and MgO, glaze components generally used for commercially available ceramic ware, such as quartz, feldspar, kaolin, dolomite, talc, and magnesite.
[0014] The contact angle of an oil drop to the surface of the glaze layer is an index for evaluating the oil repellency of the surface, and is 25 to 50°, preferably 30 to 40°, measured by the width-height method. If the contact angle is less than 25°, running water is unlikely to penetrate between the oil and the surface of the glaze layer, and as a result, oil stains are difficult to remove. On the other hand, if the contact angle exceeds 50°, for example, when used as tableware, when food is served on it, the oil is too easily repelled, resulting in a poor appearance of the food. The width-height method is also called the θ / 2 method, and is a common measurement method that has long been used to evaluate wettability.
[0015] The surface of the glaze layer has one or more grooves, preferably a plurality of grooves, depending on the area. The groove has a total length of 1 to 800 mm, preferably 10 to 300 mm, a width of 100 to 1000 μm, preferably 150 to 800 μm, more preferably 200 to 600 μm, and a depth of 100 to 1000 μm, preferably 150 to 800 μm, more preferably 200 to 600 μm. If the dimensions of the groove are outside the above range, for example, when used as tableware, there is a problem that the effect of removing oil stains by utilizing the force of running water during washing with water is reduced. The cross-sectional shape of the groove is not particularly limited as long as the effects of the present invention are exerted, and is generally a roughly U-shaped shape such as a U-shaped, V-shaped, or arc-shaped shape. The shape of the groove may be roughly linear, roughly curved, roughly elliptical, roughly circular, roughly polygonal, roughly U-shaped, or spiral, and is preferably linear or circular. When there are multiple grooves, the shapes and dimensions of each groove may be the same or different, preferably the same shape and dimensions.
[0016] The total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer, preferably 40 to 80%, and more preferably 50 to 70%. If it occupies less than 30%, there is a problem that the running water will spread during washing and sufficient washing power cannot be obtained. On the other hand, if it occupies more than 90%, there is a problem that the strength of the surface is weakened and cracks or chips are likely to occur even with a slight impact.
[0017] Next, the method for producing the ceramic ware of the present invention will be described. The method for producing ceramic of the present invention includes a step of immersing ceramic having a glaze layer on its surface, the glaze constituting the glaze layer containing 20-50% by mass of spherical silica particles having an average particle size of 10-500 nm and 0.5-3.0% by mass of MgO relative to 100% by mass of total solids, the surface of the glaze layer having one or more grooves each having a total length of 1-800 mm, a width of 100-1000 μm and a depth of 100-1000 μm, the total opening area of the grooves occupying 30-90% of the total surface area of the glaze layer, in an alkaline solution.
[0018] The above-mentioned "step of immersing in an alkaline solution" dissolves the glaze on the very surface of the glaze layer, leaving only spherical silica particles with excellent alkali resistance on the surface, and nano-sized fine irregularities are formed on the surface. As a result, the contact angle of an oil drop with the surface of the glaze layer is 25 to 50° as measured by the width-height method (hereinafter, sometimes simply referred to as "contact angle of 25 to 50°"), improving the oil repellency of the surface.
[0019] The pH and temperature of the alkaline solution, as well as the immersion time, are not particularly limited as long as the contact angle is within a range of 25 to 50°. The pH is preferably 9 to 14, more preferably 10 to 13. If the pH is less than 9, the amount of glaze eluted from the very surface of the glaze layer is small, and sufficient oil repellency cannot be obtained. On the other hand, if the pH exceeds 14, the rate of elution of the glaze from the very surface of the glaze layer is too fast, and it is difficult to control the amount of elution. The temperature is preferably 10 to 90°C, more preferably 20 to 70°C. If the temperature is less than 10°C, the rate of elution of the glaze from the very surface of the glaze layer is slow, and it takes a long time, resulting in low productivity. On the other hand, if the temperature exceeds 90°C, the rate of elution of the glaze from the very surface of the glaze layer is too fast, and it is difficult to control the amount of elution. The immersion time is preferably 10 minutes to 24 hours, more preferably 20 minutes to 16 hours. If the immersion time is less than 10 minutes, the temperature must be increased, which makes it difficult to control the amount of eluted glaze from the very surface of the glaze layer, whereas if the immersion time is more than 24 hours, the temperature can be lowered and it becomes easier to control the amount of eluted glaze from the very surface of the glaze layer, but the long immersion time reduces productivity.
[0020] The alkaline solution is not particularly limited, but from the viewpoints of ease of handling and cost, it preferably contains at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, and barium hydroxide, and more preferably contains sodium hydroxide. Moreover, from the viewpoints of ease of handling, cost, effect, etc., the alkaline solution is preferably an aqueous solution.
[0021] The method for producing ceramics of the present invention, which includes the above-mentioned "step of immersing in an alkaline solution", is, for example, as follows.
[0022] (1) As with regular ceramics, clay is shaped into dish shapes to form the base material. (2) On the surface of the base material formed in (1) above (for example, the inner surface that comes into contact with food when the product is ultimately used as tableware), one or more grooves are formed so that the surface of the glaze layer of the resulting ceramic ware has a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer. (3) The base material having the grooves formed therein obtained in (2) above is thoroughly dried and bisque fired at 800 to 950°C. (4) A glaze is prepared containing 20-50% by mass of spherical silica particles having an average particle size of 10-500 nm and 0.5-3.0% by mass of MgO relative to 100% by mass of the total solids (for example, spherical silica particles are dispersed in water, allowed to stand for a certain period of time, and the supernatant is collected to perform elutriation to extract only fine particles, thereby obtaining spherical silica particles having an average particle size of 10-500 nm that do not contain coarse particles of 1 μm or more. These spherical silica particles are added to a commercially available glaze, and the composition is adjusted so that the glaze contains 20-50% by mass of spherical silica particles and 0.5-3.0% by mass of MgO relative to 100% by mass of the total solids). (5) The glaze prepared in (4) above is applied to the surface of the bisque-fired base obtained in (3) above, and fired at 1200-1350°C. (The thickness of the glaze layer is appropriately adjusted depending on the moisture content in the glaze, etc., so that the surface of the glaze layer of the finally obtained ceramic ware has a total length of 1-800 mm, one or more grooves each having a width of 100-1000 μm and a depth of 100-1000 μm, and the total opening area of the grooves occupies 30-90% of the total surface area of the glaze layer.) (6) The sintered body obtained in (5) above is cooled to room temperature. (7) The sintered body cooled in (6) above is subjected to the "step of immersing in an alkaline solution". (8) The sintered body immersed in the alkaline solution in (7) above is thoroughly washed with water and then dried.
[0023] The ceramic of the present invention can be manufactured by the method for manufacturing ceramic of the present invention, which includes the "step of immersing in an alkaline solution" described above. EXAMPLES
[0024] The present invention will be further explained in detail by the following examples and comparative examples, as well as reference examples and comparative reference examples, but these are not intended to limit the present invention and may be modified without departing from the scope of the present invention.
[0025] Example 1 The basic glaze with a solid content of 60% (SiO2: 40% by mass, Al2O3: 10% by mass, MgO: 1.0% by mass, CaO: 3.0% by mass, Na2O: 1.5% by mass, K2O: 4.5% by mass) and spherical silica particles with an average particle size of 180 nm were mixed thoroughly in a ball mill to adjust the final content of spherical silica particles to 40% by mass and MgO to 1.0% by mass. On the other hand, for the base, a ceramic plate with a size of 100 mm x 100 mm and a thickness of 5 mm was made by pressure casting using china clay, and 50 linear grooves with a total length of 100 mm, width of 800 μm and depth of 200 μm were cut on the surface with a brush, dried, and bisque fired at 900°C. The prepared glaze was applied to the grooved surface of the bisque fired ceramic plate, and reduction firing was performed at 1300°C. After cooling, the obtained sintered body was immersed in a sodium hydroxide solution of pH 13 at 20°C and left to stand at room temperature for 16 hours. The sintered body was then thoroughly washed with water and dried to obtain a ceramic test sample (contact angle 34°; the surface of the glaze layer had 50 linear grooves with a total length of 90 mm, a width of 720 μm, and a depth of 180 μm, and the total opening area of the grooves occupies 40% of the total surface area of the glaze layer). The obtained sample was leaned against a wall at an angle of 45 degrees. 10 drops of edible oil were dropped on the surface of the leaned sample, and after 30 minutes, water was sprayed from a washing bottle and the ease of oil removal was visually observed. As a result, it was confirmed that the oil easily flowed down from the surface of the glaze layer as if peeling off with 100 ml of running water. FIG. 1 shows an electron microscope photograph of the surface of the glaze layer of the obtained ceramic test sample.
[0026] Comparative Example 1 The sintered body was subjected to reduction firing at 1300°C in the same manner as in Example 1, and after cooling, it was washed with water and dried without being immersed in an alkaline solution to obtain a ceramic test sample (contact angle 24°; the surface of the glaze layer has 50 linear grooves with a total length of 90 mm, a width of 720 μm, and a depth of 180 μm, and the total opening area of the grooves occupies 40% of the total surface area of the glaze layer). The obtained sample was leaned against a wall at an angle of 45 degrees. Then, 10 drops of edible oil were dropped on the surface of the leaned sample, and after 30 minutes, water was sprayed from a washing bottle and the ease of removing the oil was visually observed. As a result, it was not possible to remove all the oil from the surface of the glaze layer even with 200 ml of running water. This revealed that immersion in an alkaline solution after firing affects the ease of removing the oil.
[0027] (Reference example 1) The basic glaze with a solid content of 65% (SiO2: 42% by mass, Al2O3: 13% by mass, MgO: 1.5% by mass, CaO: 3.1% by mass, Na2O: 1.1% by mass, K2O: 4.3% by mass) and spherical silica particles with an average particle size of 220 nm with a solid content of 35% by mass were thoroughly wet mixed in a ball mill. Chemical analysis of the mixed glaze showed that the MgO content was 1.5% by mass. This glaze was applied to a clay plate and reduced and fired at 1300°C. The obtained sintered body was visually observed for the presence or absence of cracks, and the crystal phase of the glaze layer was identified using an X-ray diffraction device. As a result, no cracks were observed visually, and it was confirmed that the amount of cristobalite that causes cracks was small compared to the amount of quartz, as shown in Figure 2.
[0028] (Comparative Reference Example 1) The basic glaze with a solid content of 65% (SiO2: 42% by mass, Al2O3: 12.5% by mass, MgO: 0.3% by mass, CaO: 3.8% by mass, Na2O: 1.5% by mass, K2O: 4.9% by mass) and spherical silica particles with an average particle size of 220 nm with a solid content of 35% by mass were thoroughly wet mixed in a ball mill. Chemical analysis of the mixed glaze showed that the MgO content was 0.3% by mass. This glaze was applied to a porcelain clay plate and reduced and fired at 1300°C. The obtained sintered body was visually observed for the presence or absence of cracks, and the crystalline phase of the glaze layer was identified using an X-ray diffraction device. As a result, many fine cracks were visually observed, and it was confirmed that the amount of cristobalite was much greater than the amount of quartz in the crystalline phase, as shown in Figure 3. This revealed that the composition of the glaze affects the formation of cristobalite.
[0029] Example 2 The basic glaze, 55% by mass (SiO2: 37.9%, Al2O3: 9.0%, MgO: 0.7%, CaO: 2.1%, Na2O: 1.2%, K2O: 4.1%), and 45% by mass of spherical silica particles with an average particle size of 240 nm were thoroughly wet-mixed in a ball mill to adjust the final content of spherical silica particles to 45% by mass and MgO to 0.7% by mass. On the other hand, for the base, a ceramic plate 100 mm x 100 mm in size and 5 mm in thickness was made by pressure casting using china clay, and 300 linear grooves, each 100 mm long, 200 μm wide, and 100 μm deep, were scraped on the surface with a brush, dried, and bisque-fired at 900°C. The prepared glaze was applied to the grooved surface of the bisque-fired ceramic plate, and reduction firing was performed at 1300°C. After cooling the obtained sintered body, it was immersed in a sodium hydroxide solution of pH 10 at 70°C for 30 minutes. Thereafter, the sintered body was thoroughly washed with water and dried to obtain a ceramic test sample (contact angle 38°; the surface of the glaze layer has 300 linear grooves with a total length of 90 mm, a width of 180 μm, and a depth of 90 μm, and the total opening area of the grooves occupies 60% of the total surface area of the glaze layer). The obtained sample was leaned against a wall at an angle of 45 degrees. After dropping 10 drops of edible oil on the surface of the leaned sample, water was sprayed from a washing bottle, and the ease of oil removal was visually observed. As a result, it was confirmed that even with 100 ml of running water, the oil easily flowed down as if peeling off from the surface of the glaze layer.
[0030] Comparative Example 2 The base material, which was pressure-cast in the same manner as in Example 2, was dried in a smooth state without grooves on the surface, and then bisque-fired at 900°C. After that, as in Example 2, the obtained sintered body was cooled and immersed in a sodium hydroxide solution of pH 10 at 70°C for 30 minutes. The sintered body was then thoroughly washed with water and dried to obtain a ceramic test sample (contact angle 31°). The obtained sample was leaned against a wall at an angle of 45 degrees. After dropping 10 drops of edible oil on the surface of the leaned sample, water was sprayed from a washing bottle and the ease of removing the oil was visually observed. As a result, it was not possible to remove all the oil from the surface of the glaze layer with a water flow of 100 ml. From this, it was confirmed that using the force of running water is very effective in removing oil, and that the influence of the surface shape is large. [Industrial Applicability]
[0031] According to the present invention, it is possible to provide environmentally friendly ceramics which can easily remove oily stains with a small amount of running water and which maintain their functionality for a long period of time even under the harsh conditions of a dishwasher, thereby reducing the amount of water and detergent used for washing, and a method for producing the same.
Claims
1. A ceramic ware having a glaze layer on its surface, the glaze constituting the glaze layer contains 20 to 50 mass% of spherical silica particles having an average particle size of 10 to 500 nm and 0.5 to 3.0 mass% of MgO relative to 100 mass% of the total solid content; the contact angle of an oil droplet of edible oil with the surface of the glaze layer is 25 to 50° as measured by a width-height method; The surface of the glaze layer has one or more grooves having a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer. Ceramics.
2. The ceramic according to claim 1, wherein the spherical silica particles have an average particle size of 50 to 300 nm.
3. 3. The ceramic ware according to claim 1, wherein the contact angle of an oil drop of edible oil with the surface of the glaze layer is 30 to 40° as measured by the width-height method.
4. A method for manufacturing ceramic ware having a glaze layer on its surface, comprising the steps of: The method includes the step of immersing the ceramic in an alkaline solution, the glaze constituting the glaze layer contains 20 to 50 mass% of spherical silica particles having an average particle size of 10 to 500 nm and 0.5 to 3.0 mass% of MgO relative to 100 mass% of the total solid content; The surface of the glaze layer has one or more grooves having a total length of 1 to 800 mm, a width of 100 to 1000 μm, and a depth of 100 to 1000 μm, and the total opening area of the grooves occupies 30 to 90% of the total surface area of the glaze layer. Manufacturing method.
5. The method of claim 4, comprising the step of immersing the ceramic in an alkaline solution having a pH of 9 to 14 and a temperature of 10 to 90° C. for 10 minutes to 24 hours.
6. The method according to claim 4 or 5, wherein the alkaline solution contains at least one selected from the group consisting of sodium hydroxide, potassium hydroxide and barium hydroxide.
Citation Information
Patent Citations
Nano TiO2 self-cleaning functional ceramic as well as preparation method and application thereof
CN111233325A
Antifouling glazed product
JP2000302581A
Sanitary pottery
JP2001048680A
Sanitary chinaware
JP2001048681A
Sanitary earthenware and production thereof
JP2001058865A