Method for producing opposing surfaces and method for producing parts having complex shapes using the opposing surfaces

3D additive printing techniques are used to create opposing surfaces that compensate for material shrinkage during sintering, ensuring uniform densification and easy mold removal of complex parts, addressing non-uniformity and mold removal challenges in existing sintering methods.

JP7571977B2Active Publication Date: 2024-10-23NORIMAT SAS
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021516738
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-02
Filing Date
2019-10-01
Publication Date
2024-10-23
Estimated Expiration
2039-10-01

AI Technical Summary

Technical Problem

Existing sintering techniques face challenges in uniformly densifying parts with complex shapes, particularly due to non-uniformity and difficulty in removing molds from parts with undercuts or tapered shapes, leading to increased design and mechanical effort and potential defects.

Method used

The method involves using digitally controlled 3D additive printing to create opposing surfaces that compensate for material shrinkage during sintering by increasing size in the direction of applied pressure, allowing for precise densification and homogeneity, and dividing the opposing surfaces to facilitate mold removal.

Benefits of technology

This approach ensures high homogeneity in porosity and accuracy of geometrical features, prevents cracks, and simplifies mold removal by dividing complex shapes into manageable parts, thereby improving the manufacturing process efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571977000001
    Figure 0007571977000001
  • Figure 0007571977000002
    Figure 0007571977000002
  • Figure 0007571977000003
    Figure 0007571977000003
Patent Text Reader

Abstract

The present invention relates to a method for producing a counter surface (20) for manufacturing a part (24) having a complex shape by densification through pressure sintering. The counter surface (20) is made of successive layers produced by numerically controlled three-dimensional (3D) additive printing according to the following steps: The method includes the steps of numerically recording a three-dimensional master of the manufactured part (24) in the control unit of a three-dimensional additive printing system to obtain the final shape of the counter surface to be produced; and using 3D additive printing to produce the counter surface (20). A part having a complex shape (24d) is then produced by pressure sintering and separated from the sintered counter surface (20d). [Selected Figure] Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a counter surface for producing a part having a complex shape, and a method for producing a part having a complex shape by pressure sintering using said counter surface.

[0002] The invention relates to the field of component manufacturing, in particular the manufacture of industrial machine parts by densifying porous or powdered materials, including all techniques of densification, whether uniaxial or multiaxial, under isostatic pressure load, such as, in particular, hot isostatic pressing, high pressure discharge sintering, also known as SPS (spark plasma sintering), or selective laser sintering.

[0003] More specifically, in the SPS sintering technique, a volume of ceramic, polymer, or metal powder is consolidated in a conductive mold to rapidly obtain a dense material with an ultrafine structure. Such consolidation is achieved by simultaneously applying a load (e.g., high uniaxial pressure on the mold of about 100 MPa) and heat of 500°C to 2000°C from a high-intensity pulsed direct current (500A to 10,000A) in the mold, so that the entire sintering of the powder is completed in just a few minutes.

[0004] The main advantage of this SPS sintering technique is that the high temperature ramp rate and relatively short residence time at high temperature allows densification of the material with no or very little crystal growth. [Background technology]

[0005] Especially for parts with complex shapes and substantial thickness differences, the uniaxial pressure in SPS sintering technology has the disadvantage of causing inhomogeneous densification due to the need to remove the non-uniform material between the regions of different thicknesses within the limited space and time. ComplexRough shapes refer to shapes with various curvatures of varying or uniform thickness, shapes with large variations in thickness but varying or constant curvature, and / or shapes with geometric imperfections.

[0006] To compensate for the drawback of non-uniform densification, US Pat. No. 5,399,633 proposes adding a deformation boundary layer between the powdered (or porous) material and the opposing surface of a custom-made mold for producing the part.

[0007] However, sintering techniques also present problems when using molds or mold counter faces that are not easily removable from the mold, especially when the part has a complex shape, especially when it has undercuts that make it difficult to remove, or tapered features that make it difficult to remove from the mold without breaking the part.

[0008] The counterface may be an imprint obtained by pressing a layer of ceramic powder agglomerated with a binder onto the counterface with an inert interface, or by compacting ceramic powder onto a polymer preform. These techniques also have substantial limitations on the geometry of ease of removal due to issues with complex shapes such as undercuts and surface conditions of the counterface that must be covered by the interface.

[0009] In order to create counter faces that fit the tapered shape and can be removed from the mold, multiple counter faces were required to avoid problems during removal from the mold. This required custom tooling for each counter face, which increased the design and machining process. Also, assembling many counter faces was a source of defects (finished part shape mismatch, early cracks, material loss, etc.).

[0010] Also known from patent document 2 is the use of thin-walled containers made by additive printing, adapted to the shape of the manufactured part. The containers are molded in one piece in HIP (Hot Isostatic Pressing), a pressing technique for densifying powdered metals. In patent document 3, additive printing is used to subject several materials to a HIP press in order to give the part specific physical properties depending on the direction.

[0011] Patent document 4 also relates to HIP technology, where the container material preformed in the additive layer is the same material as the manufactured part.Others, such as patent documents 5, 6 or 7, use additive layers in the implementation of HIP technology, for example using gel layers or ceramic molds prefabricated by wax-based methods in HIP technology.

[0012] However, these methods, even with HIP technology, are far from space-saving, complicated, and time-consuming. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] French Patent Application No. 3042992 [Patent Document 2] US Patent Application Publication No. 2017 / 291221 [Patent Document 3] US Patent Application Publication No. 2017 / 368780 [Patent Document 4] European Patent Application Publication No. 2551040 [Patent Document 5] US Patent Application Publication No. 2017 / 361490 [Patent Document 6] US Patent Application Publication No. 2016 / 144432 [Patent Document 7] US Patent Application Publication No. 2016 / 030654 Summary of the Invention [Problem to be solved by the invention]

[0014] The present invention aims to solve these problems, and in particular to facilitate bonding of opposing surfaces while controlling the surface condition of the opposing surfaces without developing special tools for the production of the opposing surfaces. To this end, the present invention proposes the use of opposing surfaces produced by digitally controlled additive technology and sizing of the opposing surfaces, in particular to predict the shrinkage of the densified material along the axial direction in which pressure is applied. [Means for solving the problem]

[0015] More specifically, the subject of the invention is a method for producing a counter surface for manufacturing parts with complex shapes by densification by pressure sintering, in which the counter surface consists of successive layers deposited by digitally controlled three-dimensional (3D) additive printing, according to the following steps: A 3D master of the part to be produced is digitally created by the control unit of the 3D additive printing system so that a print of the opposing surface to be produced is formed and the remaining opposing surfaces have a shaped surface suitable for a mold for producing the part. A counter surface is produced by 3D additive printing technology. The size of the counter surface is increased by a density expansion factor that compensates for the shrinkage of the produced part (1; 24d) along the direction of pressure applied during sintering and densification of the produced part. Completing the additive printing of the opposing surfaces (20; 30a, 30b) by sintering.

[0016] In particular, the combination of the features of the counterface with the increased size and the features of conventional sintering allows adaptation in the sintering of the counterface and subsequently in the sintering of the material of the manufactured part, so that the desired degree of densification of said material can be precisely achieved, and furthermore, it is possible to obtain high homogeneity in the porosity and precision of the physicochemical properties, such as the defined porosity rate, and of the geometric features (dimensions and configuration) of the manufactured part.

[0017] The effects of the present invention include the following. 3D additive printing techniques can be selected from stereolithography, binder jetting, controlled extrusion, fused filament processing, inkjet printing, and aerosol jet printing. The porous material used to make the counter surface is selected from ceramic, silica, metal silicate and composite materials. Printing is performed against a counter surface with walls no thicker than 5 mm, which prevents any cracks from appearing during subsequent sintering of the part. The opposing surfaces are then divided into at least two sections in a subsequent process. The two sections are then joined along at least one joining surface to eliminate at least one undercut. The complex shape is divided into multiple sections, and the joining surface between the sections allows the part to be directly removed from the mold.

[0018] During 3D additive printing, a step of extracting the binder from the opposing surface can be effectively performed by performing a heat treatment at a temperature of 200°C to 600°C and a temperature increase rate of 0.1°C / min to 1°C / min according to the material of the opposing surface. In the above step, it becomes possible to extract the organic compound contained in the material during the preparation of the opposing surface.

[0019] Furthermore, following the step of removing the binder, a pre-sintering step may be performed. In the pre-sintering step, the opposing surfaces are heat-treated at a high temperature of 600°C to 1,500°C according to the material of the opposing surfaces. This starts densifying the opposing surfaces, increasing their mechanical strength and facilitating the formation of an interface.

[0020] Another object of the invention is a method for producing a part having a complex shape by pressure sintering using the counter surface produced by the above method, said method for producing a part being carried out according to the following steps: The opposing surface is placed into a densification mold where pressure sintering is performed. A powdered densifying material is introduced into at least one duct passing through the opposing surface. Densify the material to be densified by sintering under uniaxial pressure. To remove the part, the opposing surface is separated. This completes the part.

[0021] The porous or powdered material of the manufacturing part may be selected from ceramics, metal alloys, polymers, and composites. Furthermore, at least one outer wall of the facing surface may be open and filled with a ceramic powder having a sintering temperature that is the same as the sintering temperature of the ceramic of the facing surface.

[0022] Some of the preferred forms are as follows: The counterface material is selected so that it and the material of the manufactured part behave similarly during sintering. This behavior is similar to conventional sintering for the counterface material. The sintering start temperature or sintering end temperature of the ceramic on the opposing surface is equal to or higher than that of the ceramic of the manufactured product. The ceramic may be selected from powdered YSZ (yttria stabilized zirconia), ATZ (alumina toughened zirconia), ZTA (zirconia toughened alumina), and alumina exhibiting a degree of densification ranging from 40% to 80%. A duct, open at least at one end, is provided on the outside of the counter face, which allows the counter face to be filled with powdered or porous material for forming the part and for excess powder to be removed. The additive printing of the counter surface is followed by sintering of the counter surface, which can be performed simultaneously with the sintering of the production part.

[0023] According to an advantageous embodiment, it is provided for a layer of porous and / or powdery material to be arranged as an interface layer between the counter face and the material to be densified, the separation by which makes it possible to prevent any reaction between the counter face and the powder of the resulting part.

[0024] Advantageously, the interface layer is formed by at least one layer of a material chosen from graphite, yttrium oxide, boron nitride, and may be applied in a form chosen from spraying, powder lamination and a sheet of suitable shape.

[0025] Further information, features and advantages of the present invention will become apparent from the following non-limiting description, taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0026] [Figure 1a] FIG. 1a is an example of a complex shaped part that can be produced by the method according to the invention. [Figure 1b] FIG. 1b shows a digital mold of the three-dimensional master of the production part shown in FIG. 1a. [Diagram 2] FIG. 2 shows schematic cross-sectional views of the main steps 2a to 2e of a method for producing a part having a complex shape according to the invention, said method comprising sintering a counter surface produced by the method according to the invention. [Figure 3a] FIG. 3a shows two opposing surfaces created in manufacturing the parts of FIGS. 1a and 1b. [Figure 3b] FIG. 3b shows two opposing surfaces created in manufacturing the parts of FIGS. 1a and 1b. [Figure 3c] FIG. 3c shows the two opposing surfaces created in making the parts of FIGS. 1a and 1b when they are brought together in a mold and densified by SPS pressure sintering. [Figure 4] FIG. 4 is a perspective view of the manufactured part. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In the drawings, identical elements are given the same reference numerals, which are referenced at one or more points in the description of the element they represent.

[0028] With reference to Fig. 1a, an example of a part 1 having a complex shape, produced by the production method according to the invention, is shown. Plane "P" (parallel to the reference plane XOZ) is the joining plane (described below) of two previously produced opposing surfaces. This makes it easier to remove the part from the mould after production, especially if the part 1 has an undercut recess "C" which makes it difficult to remove from the mould. According to the invention, recess "C" is present over the entirety of one side of the opposing surfaces.

[0029] FIG. 1b shows a digital mold 3 of the three-dimensional original 10 of the part 1 shown in FIG. 1a. The digital mold 3 is produced in the control of a three-dimensional additive printing system (not shown), which results in the final shape of the produced counterfaces. To facilitate removal from the mold, this final shape is divided into two parts, as shown in FIG. 1a. In a subsequent step, each counterface is produced by a 3D additive printing technique, in this example by stereolithography. The two counterfaces 30a and 30b thus obtained are shown in FIG. 3.

[0030] Figure 2 shows a schematic cross-sectional view of the main steps 2a to 2e of a manufacturing method according to the invention for producing a part with a complex shape 24d by sintering under uniaxial pressure, using a counter surface 20 (step 2a) made from an agglomerated ceramic powder by a 3D additive printing technique, in this example stereolithography.

[0031] In the illustrated example, it turns out that a single counter surface is sufficient to facilitate the removal of the prismatic part 24d from the mould (see step 2e), which is assumed in a simplified example to have a complex shape. A graphite interface layer 22 of a certain thickness is then deposited on the counter surface 20 by spraying (step 2b), and a densifying material 24 is added onto this interface layer 22 (step 2c). The interface layer 22 prevents any reaction between the counter surface 20 and the powder 24 of the manufactured part.

[0032] The densified materials used in the manufacture of the components of this example are metal alloys, such as TiAl alloys (titanium aluminum alloys) and nickel-based superalloys of the Rene family.

[0033] Advantageously, the material of the counter face 20 is selected such that it and the material of the production part 24 behave similarly during sintering, both in terms of the initial and final sintering temperatures and the degree of densification.

[0034] If an alloy is used in the manufactured part, the ceramic used in the counter surface is selected to be ATZ (alumina toughened zirconia) for parts made of TiAl, or YSZ (yttria stabilized zirconia) for parts made of nickel-based superalloys selected from the Rene family. More generally, the start sintering temperature (or end sintering temperature) of the ceramic used in the counter surface is equal to or higher than the start sintering temperature (or end sintering temperature) of the metal alloy of the manufactured part.

[0035] Also, the opposing surface 20 of this example (expected shrinkage of -10% to -45%) is densified by SPS sintering under uniaxial pressure of the densifying material 24. The material 24 and the opposing surface 20 are placed in an SPS mold (not shown).

[0036] In predicting this densification, the shrinkage of the part 24 along the direction of the uniaxial SPS sintering pressure "F" (step 2d) is taken into account, and the size of each counter surface 20 is increased. The shape of the part 24 is therefore "stretched" in advance by an elongation factor "Fe" to compensate for the shrinkage in the size of the part. The factor Fe is determined by the ratio of the density of the powder before densification to the density of the powder after densification. Advantageously, when the value of the factor Fe is changed, the simplified shape of the counter surface 20 can also be changed.

[0037] Thus, in this embodiment, the uniaxial pressure "F" reduces the maximum height of the counter surface 20 by 40%, i.e. the height is reduced from value "H" (step 2c) to value "h" (step 2d). The reduced height makes it possible to produce part 24d with the desired height. The original height "H" is increased by applying the factor Fe. The agglomerated counter surface and part are designated 20d and 24d and can be easily separated (step 2e).

[0038] In the illustrated example of Figures 3a and 3b, counter faces made of ATZ ceramic are shown as parts 30a and 30b. In this example, a part 1 made of TiAl is produced, as shown in Figures 1a and 1b, and ATZ ceramic and TiAl alloys behave similarly in sintering. These counter faces 30a and 30b have connecting surfaces 40a and 40b on the joint surface "P" (see Figure 1a).

[0039] Advantageously, the binder is removed from the opposing surfaces 30a and 30b by heat treatment at a temperature between 200°C and 600°C, in this example 400°C, and at a temperature ramp rate of 0.1°C / min to 1°C / min, in this example 0.5°C / min. This step allows the removal of organic compounds that have entered the ceramic powder during the creation of the opposing surfaces by 3D printing.

[0040] Preferably, after the binder is removed, pre-sintering is performed. Pre-sintering is a process in which the opposing surfaces 30a and 30b after the binder is removed are treated at a higher temperature, for example, 600°C to 1,500°C depending on the material used, in this example, 1,200°C. The heat treatment can initiate densification of the opposing surfaces, thereby increasing their mechanical strength and facilitating the application of one or more interface layers, as described below.

[0041] The two half-imprints 41a and 41b of the production part are sprayed with graphite 42 and a layer based on yttrium oxide. This prevents a reaction between the ceramic and the material of the production part, in this example TiAl. In the case of a counter surface produced by stereolithography, the counter surface is divided into two parts, so that the paste that has not been polymerized is removed. Furthermore, the counter surface parts 30a and 30b advantageously have a maximum thickness of 5 mm. This avoids the risk of cracks occurring during sintering and heat treatment for the purpose of removing the binder when the part is removed.

[0042] With reference to Fig. 3c, the two opposing face parts 30a and 30b are joined in an SPS sintering mould 2 so that the two half impressions 41a and 41b form a single impression in the original plate, corresponding to the production part. This impression is filled with TiAl powder via three hollow ducts 4. These ducts 4 run through the face 42a opposite to the connecting face 40a of the opposing face part 30a (see Fig. 3a). The ducts 4 also allow the removal of excess TiAl powder, if necessary.

[0043] One or more of the outer walls of the counter faces 30a and 30b can advantageously be open, facilitating the creation of the counter faces by 3D printing. Such open spaces are subsequently filled with YSZ (yttria stabilized zirconia) powder, the sintering temperature of which is equal to the sintering temperature of the counter face ceramic made using ATZ.

[0044] In SPS sintering under uniaxial pressure, the ceramic and the metal alloy of the production part are sintered simultaneously, and the sintered ceramic covers the metal part. The interfacial layer 42 of graphite and yttrium oxide (see Fig. 3a and Fig. 3b) mechanically and / or chemically releases the part, so that the ceramic is easily separated from the part. Fig. 4 shows the final obtained part 1 before removing the ceramic residues 43.

[0045] The invention is not limited to what has been described and illustrated. The opposing surfaces may therefore be divided into a minimum number of sections such that the manufactured part has no undercuts.

[0046] Additionally, counter surfaces may be provided for locally weakened areas without limiting their location in order to facilitate final removal from the mold.

[0047] Additionally, the manufactured parts may be constructed from powdered metal alloys, ceramics, composites, or other suitable materials.

Claims

1. 1. A method for producing a part (24d) having a complex shape by densification through pressure sintering, comprising producing split mold parts (30a, 30b) for producing a part (24d) having a complex shape by sintering, said split mold parts (30a, 30b) being made of successive overlapping layers produced by digitally controlled three-dimensional (3D) additive printing, according to the following steps: In order to produce the divided mold parts (30a, 30b) by three-dimensional (3D) additive printing, a step of digitally modeling a three-dimensional original plate (3) of the part (24d) having a complex shape to be produced by a control unit of a three-dimensional additive printing system so that the remaining parts of the divided mold parts (30a, 30b) have a shape surface suitable for a densification mold for producing the part (24d) having the complex shape; Producing the split mold parts (30a, 30b) by 3D additive printing technology; completing the additive printing of the split mold parts (30a, 30b) by sintering; increasing the size of the divided mold parts (30a, 30b) by a density expansion factor determined by the ratio of the density of the powder before densification to the density of the powder after densification by a densification mold; Compensating for shrinkage of the complex-shaped part (24d) along the direction of uniaxial pressure (F) applied during densification of the complex-shaped part produced by pressure sintering; A method for manufacturing a part (24d) having a complex shape comprises the steps of: placing the divided mold parts (30a, 30b) together in a densification mold where sintering is performed under uniaxial pressure; - introducing a powdered material before densification or a powdered porous material into at least one duct (4) passing through one of the divided mould parts (30a); - densifying said powdered material or said powdered porous material by sintering under uniaxial pressure (F); and separating the split mold parts (30a, 30b) to remove the complex shaped part (24d) and complete production.

2. 2. The method of claim 1, wherein the 3D additive printing technique is selected from stereolithography, binder jet, extrusion, Fused Filament Fabrication (FFF), inkjet printing, and aerosol jet printing.

3. 3. The method for manufacturing a part having a complex shape according to claim 1 or 2, characterized in that the divided mold parts (30a, 30b) are made of a porous material selected from ceramic, silica, metal silicate and a composite material.

4. The method for manufacturing a part having a complex shape according to any one of claims 1 to 3, characterized in that the additive printing is performed on the divided mold parts (30a, 30b) having a thickness of 5 mm or less.

5. The method for manufacturing a part having a complex shape according to any one of claims 1 to 4, characterized in that during 3D additive printing, a step of removing the binder from the divided mold parts (30a, 30b) is carried out by carrying out a heat treatment at a temperature between 200 ° C. and 600 ° C. and at a temperature increase rate between 0.1 ° C. / min and 1 ° C. / min.

6. 6. The method for manufacturing a part having a complex shape according to claim 5, characterized in that, following the binder removal step, a pre-sintering step is carried out by heat treating the split mold parts (30a, 30b) at a temperature between 600°C and 1,500°C.

7. The divided mold parts (30a, 30b) are divided into at least two parts and the divided mold parts (30a, 30b) are joined along at least one joining surface (P) such that at least one undercut is eliminated; 7. The method for manufacturing a part having a complex shape according to any one of claims 1 to 6, characterized in that the joining surface (P) between the divided mould parts (30a, 30b) which separates the complex shape allows the complex shape to be directly removed from the mould.

8. 2. The method for producing a part with a complex shape according to claim 1, characterized in that the split mold parts (30a, 30b) are made of a porous material selected such that the material of the mold (20) or split mold parts (30a, 30b) and the material of the part with a complex shape (24d) to be produced have similar sintering behavior in terms of start and end sintering temperatures and degree of densification.

9. 2. The method for manufacturing a part having a complex shape according to claim 1, characterized in that ceramic is selected as the material for the divided mold parts (30a, 30b), and the sintering start temperature of the ceramic constituting the divided mold parts (30a, 30b) is equal to or higher than the sintering start temperature of the part having the complex shape (24d) to be manufactured, or the sintering end temperature of the ceramic constituting the divided mold parts (30a, 30b) is equal to or higher than the sintering end temperature of the part having the complex shape (24d) to be manufactured.

10. 10. The method for manufacturing a part having a complex shape according to claim 9, characterized in that the ceramic is selected from powdered yttria stabilized zirconia (YSZ), powdered alumina toughened zirconia (ATZ), powdered zirconia toughened alumina (ZTA), and alumina powder exhibiting a densification degree in the range of 40% to 80%.

11. 11. The method for manufacturing a part having a complex shape according to claim 1, characterized in that a duct (4) having at least one open end is provided on the outside of the divided mould parts (30a, 30b), said duct (4) being intended for introducing a powdered material or a powdered porous material to be moulded into the part having a complex shape (24d).

12. 12. The method for manufacturing a part with a complex shape according to any one of the preceding claims, characterized in that the powdered or powdered porous material of the part with a complex shape (24d) to be manufactured is selected from the group consisting of ceramics, metal alloys, polymers and a composite material.

13. 13. The method for manufacturing a part having a complex shape according to claim 12, characterized in that the split mold parts (30a, 30b) and part materials are selected as ceramics, and one or more outer walls of the split mold parts (30a, 30b) are open and filled with ceramic powder, the sintering temperature of the ceramic powder being the same as the sintering temperature of the ceramic of the split mold parts (30a, 30b).

14. 14. The method for manufacturing parts having complex shapes according to any one of the preceding claims, characterized in that an interface layer (22, 42) of porous or powdery material is placed between the split mould parts (30a, 30b) and the pre-densification material (24).

15. 15. The method for manufacturing a part having a complex shape according to claim 14, characterized in that the interface layer (22, 42) is formed from at least one layer of a material selected from graphite, yttrium oxide and boron nitride.

16. 16. The method for manufacturing a part having a complex shape according to claim 15, characterized in that the interface layer (22, 42) is applied in a manner selected from spraying and powder deposition.

Citation Information

Patent Citations

  • Method of manufacturing a component by hot isostatic pressing

    EP2551040A1

  • Mise en œuvre d'une interface mobile pour la fabrication de pieces complexes

    FR3042992A1

  • Transplantatiion article with as cast micro-texture surface region,and manufacture of said article

    JP1995299085A

  • Manufacturing method of casting pattern

    JP2001191146A

  • Systems and methods for uniaxial compression of articles such as 3D printed dosage forms

    JP2005507723A