Optical film and image display device
The foldable optical film with reinforced resin base material and controlled refractive index layers addresses the challenge of maintaining impact resistance and foldability, ensuring durability and protection for display devices.
Patent Information
- Application Number
- JP2019068028
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-03-29
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2039-03-29
AI Technical Summary
Foldable image display devices face challenges in achieving both good foldability and excellent impact resistance, as existing optical films risk cracking or breaking when folded, and impacts can cause dents that damage internal components like display panels.
A foldable optical film with a resin base material and reinforcing parts, each with a thickness of 150 μm or more and a Martens hardness of 30 MPa or more, is designed to maintain impact resistance and flexibility, featuring a resin layer and hard coat layers with controlled refractive index differences to enhance durability.
The optical film can withstand repeated 180° folds up to 100,000 times without cracking, providing excellent impact resistance and maintaining functionality, protecting internal display components from damage.
Smart Images

Figure 0007572143000031 
Figure 0007572143000032 
Figure 0007572143000033
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film and an image display device. [Background technology]
[0002] Image display devices such as smartphones and tablet terminals have been known for some time, and currently, foldable image display devices are being developed. The surface of an image display device may be made of a cover glass. When the cover glass is used for an image display device, although it has excellent hardness, it is difficult to bend, and there is a high possibility that the image display device will break when folded. For this reason, instead of the cover glass, the use of an optical film having a foldable resin substrate and a hard coat layer, which is foldable, has been considered for a foldable image display device (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-125063 A Summary of the Invention [Problem to be solved by the invention]
[0004] Optical films used in such foldable image display devices are required to have impact resistance because an impact may be applied to the surface of the optical film. When an impact is applied to the surface of the optical film, the surface of the optical film may be dented, and components such as a display panel (e.g., an organic light-emitting diode panel) that are located inside the optical film in the image display device may be damaged.
[0005] Regarding the dents on the surface of the optical film, there are dents caused by the optical film itself and dents caused by a soft layer such as an adhesive layer arranged inside the image display device rather than the optical film. The "dents caused by the optical film itself" refers to dents caused by the optical film itself being deformed by an impact applied to the surface of the optical film, and the "dents caused by a soft layer" refers to dents caused by the soft layer, which is arranged inside the image display device rather than the optical film, undergoing plastic deformation when an impact is applied to the surface of the optical film because the layer is soft, and the optical film following the plastic deformation of this soft layer.
[0006] For this reason, optical films are required to have excellent impact resistance such that when an impact is applied to the surface of the optical film, dents caused by the optical film itself and dents caused by the soft layer are suppressed, and components present inside the image display device are not damaged as much as the optical film.
[0007] For this reason, in order to obtain excellent impact resistance, it is conceivable to provide a layer harder than the hard coat layer on one side of the resin substrate, but if a layer hard enough to obtain excellent impact resistance is provided, there is a risk of the film cracking when folded. Therefore, at present, an optical film having excellent impact resistance while maintaining good foldability has not yet been obtained.
[0008] The present invention has been made to solve the above problems, and aims to provide an optical film having excellent impact resistance while maintaining good foldability, and an image display device including the optical film. [Means for solving the problem]
[0009] The present invention includes the following inventions. [1] A foldable optical film comprising a resin substrate and a plurality of reinforced portions arranged in a plane on a first surface side of the resin substrate, each of the reinforced portions having a thickness of 150 μm or more and a Martens hardness of 30 MPa or more.
[0010] [2] The optical film according to [1] above, further comprising a resin layer provided on the first surface side of the resin substrate, wherein at least a portion of each of the reinforced portions is covered with the resin layer.
[0011] [3] The optical film according to the above [2], wherein the absolute value of the refractive index difference between the resin layer and the reinforced portion is 0.02 or less.
[0012] [4] The optical film according to any one of [1] to [3] above, which does not crack or break when a test in which the optical film is folded 180° so that the distance between opposing sides of the optical film is 30 mm is repeated 100,000 times.
[0013] [5] The optical film according to any one of the above [1] to [4], wherein the resin substrate is a substrate made of a polyimide resin, a polyamide resin, or a mixture thereof.
[0014] [6] A foldable image display device comprising: a display panel; and the optical film according to any one of [1] to [5] above, which is disposed on a viewer's side relative to the display panel.
[0015] [7] The image display device according to [6] above, wherein the display panel is an organic light-emitting diode panel. Effect of the Invention
[0016] According to the present invention, it is possible to provide an optical film having excellent impact resistance while maintaining good foldability, and an image display device including such an optical film. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic diagram of an optical film according to an embodiment. [Diagram 2] FIG. 2 is a plan view of the optical film in FIG. 1, seen from the hard coat layer side. [Diagram 3] FIG. 1 is a schematic diagram showing a continuous folding test. [Figure 4] FIG. 1 is a schematic diagram showing a folding static test. [Diagram 5] FIG. 1 is a schematic diagram of a solid shearing jig used for measuring the shear storage modulus G' and the shear loss modulus G''. [Figure 6] 1 is a schematic configuration diagram of an image display device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an optical film and an image display device according to an embodiment of the present invention will be described with reference to the drawings. In this specification, the terms "film" and "sheet" are not distinguished from each other based only on the difference in name. Therefore, for example, "film" is used to mean a member also called a sheet. FIG. 1 is a schematic diagram of the optical film according to this embodiment, and FIG. 2 is a plan view of the optical film in FIG. 1 from the hard coat layer side. FIG. 3 is a schematic diagram showing the state of a continuous folding test, FIG. 4 is a schematic diagram showing the state of a folding static test, and FIG. 5 is a schematic diagram of a solid shearing jig used when measuring the shear storage modulus G' and the shear loss modulus G".
[0019] <<<Optical films>>> The optical film 10 shown in Fig. 1 is a foldable film having optical transparency. In this specification, "optical transparency" means a property of transmitting light, and includes, for example, a total light transmittance of 50% or more, preferably 70% or more, more preferably 80% or more, and particularly preferably 90% or more. Optical transparency does not necessarily mean transparency, and may be translucent.
[0020] 1, the optical film 10 includes a resin substrate 11, a plurality of reinforced portions 12 arranged in a plane on a first surface 11A side of the resin substrate 11, a resin layer 13 provided on the first surface 11A side of the resin substrate 11, and a hard coat layer 14 provided on a second surface 11B side of the resin substrate 11 opposite to the first surface 11A. The optical film 10 includes the resin layer 13 and the hard coat layer 14, but does not necessarily include the resin layer 13 and the hard coat layer 14. The reinforced portions 12 are attached to the resin substrate 11 via an adhesive layer 17.
[0021] In Fig. 1, the surface 10A of the optical film 10 is the surface 14A of the hard coat layer 14. In this specification, the surface of the optical film is used to mean one surface of the optical film, and the surface opposite to the surface of the optical film is referred to as the back surface to distinguish it from the front surface of the optical film. The back surface 10B of the optical film 10 is the surface 13A of the resin layer 13.
[0022] The optical film 10 is foldable as described above. The optical film 10 includes a bent region 10C that is a foldable region, and a non-bent region 10D that exists on both sides of the bent region 10C. Since the optical film 10 can be folded at the bent region 10C, the optical film 10 is folded at the bent region 10C. The bent region 10C is a region that corresponds to the gap 12A between the reinforced portions 12, and the non-bent region 10D is a region that corresponds to the reinforced portion 12. In FIG. 1, since the gap 12A exists between the reinforced portions 12, the bent region 10C is the gap 12A, but when there is no gap between the reinforced portions, that is, when the reinforced portions are in contact with each other, the bent region is a boundary region between the reinforced portions.
[0023] In the optical film 10, two reinforced portions 12 are arranged in a plane as shown in Fig. 2, but the number of reinforced portions is not limited to two, and three or more may be arranged. Also, four or more reinforced portions may be arranged in a plane in multiple rows and columns. By arranging four or more reinforced portions in this manner, the optical film can be folded along two directions, such as the vertical direction and the horizontal direction.
[0024] Since the optical film 10 is foldable, it is preferable that the optical film 10 does not crack or break even when the folding test (continuous folding test) described below is repeatedly performed 100,000 times, 200,000 times, 500,000 times, or 1 million times. If the optical film 10 cracks or breaks when the optical film 10 is repeatedly performed 100,000 times, the foldability of the optical film 10 is insufficient. The reason why the number of folding times in the continuous folding test is at least 100,000 times is as follows. For example, assuming that the optical film is incorporated into a foldable smartphone, the frequency of folding (frequency of opening and closing) becomes very high. For this reason, if the number of folding times in the continuous folding test is, for example, 10,000 times or 50,000 times, it may not be possible to perform an evaluation at a practical level. Specifically, for example, assuming that a person who always uses a smartphone opens and closes the smartphone 5 to 10 times during the morning commute alone, it is assumed that the smartphone is opened and closed at least 30 times in a single day. Therefore, assuming that the smartphone is opened and closed 30 times a day, the number of times of folding in a continuous folding test of 10,000 times is 30 times x 365 days = 10950 times, which is a test assuming one year of use. That is, even if the result of the continuous folding test of 10,000 times of folding is good, after one year has passed, there is a risk that the optical film will develop creases or cracks. Therefore, the evaluation of the number of times of folding in the continuous folding test of 10,000 times can only confirm a level that cannot be used as a product, and even products that are usable but insufficient will be good and cannot be evaluated. For this reason, in order to evaluate whether or not it is at a practical level, the number of times of folding in the continuous folding test needs to be evaluated at least 100,000 times. The continuous folding test may be performed by folding the optical film 10 so that the hard coat layer 14 is on the outside, or may be performed by folding the optical film 10 so that the hard coat layer 14 is on the inside. In either case, it is preferable that the optical film does not crack or break.
[0025] The continuous folding test is carried out as follows. In the continuous folding test, as shown in FIG. 3(A), first, the optical film 10 is cut out to a size of 30 mm×100 mm. If the optical film 10 cannot be cut out to a size of 30 mm×100 mm, the optical film 10 may be cut out to a size of, for example, 10 mm×100 mm. Then, the side portion 10E of the cut optical film 10 and the side portion 10F opposite to the side portion 10E are fixed by fixing parts 21 and 22 of a folding durability tester (for example, product name "U-shaped stretch tester DLDMLH-FS", manufactured by Yuasa System Devices Co., Ltd., compliant with IEC62715-6-1) arranged in parallel. Fixing by the fixing parts 21 and 22 is carried out by holding a portion of the optical film 10 of about 10 mm on one side in the longitudinal direction of the optical film 10. However, if the optical film 10 is smaller than the above size, and the portion of the optical film 10 required for this fixing is up to about 20 mm, measurement is possible by attaching it to the fixing parts 21, 22 with tape. Also, as shown in Fig. 3(A), the fixing part 21 is slidable in the horizontal direction. Note that the above device is preferable because it makes it possible to evaluate the durability against bending load without generating tension or friction in the optical film, unlike conventional methods such as winding an optical film around a rod.
[0026] Next, as shown in Figure 3(B), fixed portion 21 is moved closer to fixed portion 22, thereby deforming optical film 10 so as to fold bending region 10C, and further, as shown in Figure 3(C), fixed portion 21 is moved to a position where the distance φ between the two opposing sides of optical film 10 fixed by fixed portions 21, 22 is 30 mm, and then fixed portion 21 is moved in the opposite direction to eliminate the deformation of optical film 10.
[0027] As shown in Figs. 3(A) to (C), the optical film 10 can be folded 180° in the bent region 10C by moving the fixing portion 21. The interval φ between the two opposing sides 10E and 10F of the optical film 10 can be set to 30 mm by preventing the bent portion 10G of the optical film 10 from protruding from the lower ends of the fixing portions 21 and 22 and performing a continuous folding test under the following conditions and controlling the interval φ when the fixing portions 21 and 22 are closest to each other to 30 mm. In this case, the outer diameter of the bent portion 10G is considered to be 30 mm. Note that the thickness of the optical film 10 is sufficiently small compared to the interval (30 mm) between the fixing portions 21 and 22, so that the results of the continuous folding test of the optical film 10 can be considered not to be affected by the difference in thickness of the optical film 10. In this specification, the "bent portion" refers to a portion that is actually bent. Furthermore, it is even more preferable that the optical film 10 does not crack or break even when a continuous folding test is repeated 100,000 times with the distance between the two opposing sides 10E, 10F being 20 mm, 10 mm, 6 mm, or 3 mm (the smaller the distance between the two opposing sides 10E, 10F, the more preferable). (Folding conditions) Reciprocating speed: 90 rpm (revolutions per minute) Test stroke: 70mm Bending angle: 180°
[0028] In the optical film 10, as shown in Fig. 4(A), the side 10E of the optical film 10 and the side 10F opposite to the side 10E are fixed by the fixing parts 25 arranged in parallel so that the distance between the side 10E and the side 10F is 30 mm, and the optical film 10 is folded at the bending region 10C and left to stand at 70 ° C. for 240 hours in a folding standstill test, and as shown in Fig. 4(B), the fixing parts 25 are removed from the side 10E after the folding standstill test to open the folded state, and the opening angle θ, which is the angle at which the optical film 10 naturally opens, is measured in the optical film 10 after 30 minutes at room temperature. It is preferable that the opening angle θ of the optical film 10 is 100 ° or more. The larger the opening angle θ, the better the restorability, and the maximum opening angle is 180 °. The folding static test may be performed by folding the optical film 10 so that the hard coat layer 14 is on the inside, or may be performed by folding the optical film 10 so that the hard coat layer 14 is on the outside. In either case, it is preferable that the opening angle θ is 100° or more.
[0029] In addition, when another film such as a polarizing plate is provided on the back side of the optical film via an adhesive layer or a pressure-sensitive adhesive layer, the other film is peeled off together with the adhesive layer by the same method as above, and then the folding and standing test is performed. Even if such a peeling process is performed, it does not have a significant effect on the folding and standing test.
[0030] The surface 10A of the optical film 10 (surface 14A of the hard coat layer 14) preferably has a hardness (pencil hardness) of B or more, more preferably H or more, when measured by a pencil hardness test specified in JIS K5600-5-4:1999. The pencil hardness test is performed by placing the optical film 10 cut to a size of 50 mm x 100 mm on a glass plate so that the glass plate side is the back surface 10B of the optical film 10, fixing it with Cellotape (registered trademark) manufactured by Nichiban Co., Ltd. so as not to be folded or wrinkled, and using a pencil hardness tester (product name "Pencil Scratch Coating Hardness Tester (Electric)" manufactured by Toyo Seiki Seisakusho Co., Ltd.) to move a pencil (product name "Uni", manufactured by Mitsubishi Pencil Co., Ltd.) at a moving speed of 1 mm / sec while applying a load of 750 g to the surface of the optical film. The pencil hardness is the highest hardness that does not scratch the surface of the optical film in the pencil hardness test. In addition, when measuring the pencil hardness, multiple pencils with different hardnesses are used, and the pencil hardness test is performed five times for each pencil. If the surface of the optical film is not scratched four or more times out of the five, it is determined that the pencil of that hardness did not scratch the surface of the optical film. The above scratches refer to those that are visually observed when the surface of the optical film that has been subjected to the pencil hardness test is observed through transmission under a fluorescent lamp.
[0031] The optical film 10 preferably has a yellow index (YI) of 15 or less. If the YI of the optical film 10 is 15 or less, the yellowness of the optical film can be suppressed, and the optical film can be applied to applications requiring transparency. The upper limit of the yellow index (YI) of the optical film 10 is more preferably 10 or less, 5 or less, or 1.5 or less. The yellow index (YI) is a value calculated according to the formula described in JIS Z8722:2009 from the chromaticity tristimulus values X, Y, and Z measured on an optical film cut to a size of 50 mm x 100 mm using a spectrophotometer (product name "UV-3100PC", manufactured by Shimadzu Corporation, light source: tungsten lamp and deuterium lamp) in an environment of a temperature of 23±5°C and a relative humidity of 30% to 70%, and calculated according to the formula described in ASTM D1925:1962 from the tristimulus values X, Y, and Z. The yellow index (YI) is determined by measuring three times for one optical film and averaging the three measured values. The upper limit of the yellow index (YI) of the optical film 10 is more preferably 10 or less.
[0032] In order to adjust the yellow index (YI) of the optical film 10, for example, a blue pigment, which is a complementary color to yellow, may be contained in the resin substrate 11. Even in cases where a substrate made of a polyimide resin is used as the resin substrate and yellowness becomes a problem, the yellow index (YI) of the optical film can be reduced by containing a blue pigment in the resin substrate.
[0033] The blue pigment may be either a pigment or a dye, but for example, when the optical film 10 is used in an organic light-emitting diode display device, it is preferable to use one that has both light resistance and heat resistance. As the blue pigment, polycyclic organic pigments and metal complex organic pigments are less susceptible to molecular cleavage by ultraviolet rays and have significantly better light resistance than molecular dispersion of dyes, and are therefore preferable for applications requiring light resistance, etc., and more specifically, phthalocyanine organic pigments are suitable. However, since pigments are dispersed in a solvent, there is a possibility of transparency being hindered by particle scattering, so it is preferable to set the particle size of the pigment dispersion in the Rayleigh scattering region. On the other hand, when the transparency of the optical film is important, it is preferable to use a dye that is molecularly dispersed in a solvent as the blue pigment.
[0034] The haze value (total haze value) of the optical film 10 is preferably 3.0% or less. If the haze value of the optical film 10 is 3.0% or less, whitening of the image display surface can be suppressed when the optical film 10 is used in a mobile terminal. The haze value can be measured by a method conforming to JIS K7136:2000 using a haze meter (product name "HM-150", manufactured by Murakami Color Research Laboratory Co., Ltd.). The haze value is the arithmetic average value of the values obtained by measuring the haze three times for the optical film 10. The haze value is more preferably 2.0% or less, and even more preferably 1.0% or less.
[0035] The haze value can be measured in an environment of 23±5°C temperature and 30% to 70% relative humidity using a haze meter (product name "HM-150", manufactured by Murakami Color Research Laboratory Co., Ltd.) according to a method conforming to JIS K7136:2000. The haze value is the arithmetic average value of the values obtained by cutting the optical film into pieces of 50 mm×100 mm, setting them in a state free of curls and wrinkles and free of fingerprints and dust, and measuring three times for each optical film. In this specification, "measured three times" does not mean measuring the same place three times, but measuring three different places. In the optical film 10, the surface 10A when viewed with the naked eye is flat, and the laminated layers such as the hard coat layer 14 are also flat, and the variation in film thickness is within the range of ±10%. Therefore, it is considered that the average value of the haze value of the entire in-plane of the optical film can be obtained by measuring the haze value at three different places of the cut optical film. The variation in haze value is within ±10%, even if the measurement target is as long as 1m x 3000m, or the size of a 5-inch smartphone. If the optical film cannot be cut to the above size, for example, the entrance opening for measurement of the HM-150 is 20mmφ, so a sample size with a diameter of 21mm or more is required. For this reason, the optical film may be appropriately cut to a size of 22mm x 22mm or more. If the optical film is small, the measurement points are set to three by shifting the light source spot little by little or by changing the angle, as long as the light source spot does not move.
[0036] The total light transmittance of the optical film 10 is preferably 85% or more. When the total light transmittance of the optical film 10 is 85% or more, excellent light transmittance can be obtained. The total light transmittance of the optical film 10 is more preferably 88% or more, and further preferably 90% or more.
[0037] The total light transmittance can be measured in an environment with a temperature of 23±5° C. and a relative humidity of 30% to 70% by a method conforming to JIS K7361-1:1997 using a haze meter (product name "HM-150", manufactured by Murakami Color Research Laboratory Co., Ltd.) Specifically, the total light transmittance is measured by the same method as the method for measuring the haze value.
[0038] In addition, when another film such as a polarizing plate is provided on the back side of the optical film via an adhesive layer or a bonding layer, the other film is peeled off together with the adhesive layer or the bonding layer, and then the continuous folding test, the yellow index measurement, the haze value measurement, and the total light transmittance measurement are performed. The peeling off of the other film can be performed, for example, as follows. First, a laminate in which the optical film is attached to the other film via an adhesive layer or a bonding layer is heated with a dryer, and the tip of a cutter is inserted into the area that is thought to be the interface between the optical film and the other film, and the film is slowly peeled off. By repeating such heating and peeling, the adhesive layer, the bonding layer, and the other film can be peeled off. The other film is peeled off together with the adhesive layer or the bonding layer by the same method as above, and then the total light transmittance of the optical film is measured. Even if such a peeling process is performed, it does not have a significant effect on these tests and measurements. The haze value is measured after the adhesive layer or the bonding layer is peeled off, and dirt on the adhesive layer or the bonding layer is wiped off with alcohol.
[0039] The use of the optical film 10 is not particularly limited, but examples of the use of the optical film 10 include image display devices such as smartphones, tablet terminals, personal computers (PCs), wearable terminals, digital signage, televisions, and car navigation systems. The optical film 10 is also suitable for in-vehicle use. The form of each of the above image display devices is also preferable for use in applications that require flexibility, such as foldable and rollable.
[0040] The optical film 10 may be cut to a desired size, or may be in a roll shape. When the optical film 10 is cut to a desired size, the size of the optical film is not particularly limited and is appropriately determined according to the size of the display surface of the image display device. Specifically, the size of the optical film 10 may be, for example, 2.8 inches or more and 500 inches or less. In this specification, "inch" means the length of the diagonal line when the optical film is rectangular, the diameter when the optical film is circular, and the average value of the sum of the short diameter and the long diameter when the optical film is elliptical. Here, when the optical film is rectangular, the aspect ratio of the optical film when calculating the above inch is not particularly limited as long as it does not cause any problem as a display screen of the image display device. For example, length:width = 1:1, 4:3, 16:10, 16:9, 2:1, etc. can be mentioned. However, in particular, in-vehicle applications and digital signage that are rich in design, such aspect ratios are not limited. Furthermore, when the size of the optical film 10 is large, it is cut into A5 size (148 mm x 210 mm) from an arbitrary position, and then cut into the size of each measurement item. For example, when the optical film 10 is in a roll form, a predetermined length of the optical film 10 is unwound from the roll, and the desired size is cut from the effective area near the center where the quality is stable, not from the non-effective area including both ends extending along the longitudinal direction of the roll.
[0041] The optical film 10 may be disposed inside the image display device, but is preferably disposed near the surface of the image display device. When used near the surface of the image display device, the optical film 10 functions as a cover film used in place of a cover glass.
[0042] <<Resin substrate>> The resin substrate 11 is a substrate made of a resin having optical transparency. The thickness of the resin substrate 11 is preferably 10 μm or more and 100 μm or less. If the thickness of the resin substrate 11 is 10 μm or more, curling of the optical film can be suppressed, sufficient hardness can be obtained, and even if the optical film is manufactured by roll to roll, wrinkles are unlikely to occur, and there is no risk of causing deterioration of the appearance. On the other hand, if the thickness of the resin substrate 11 is 100 μm or less, the folding performance of the optical film is good, the requirements of the continuous folding test can be satisfied, and it is preferable in terms of reducing the weight of the optical film. The thickness of the resin substrate 11 is measured at 20 points by the same method as that of the reinforced portion 12 described later, and the arithmetic average value of the thicknesses at the 20 points is taken as the thickness of the resin substrate 11. The lower limit of the resin substrate 11 is more preferably 20 μm or more, 30 μm or more, or 40 μm or more, and the upper limit of the resin substrate 11 is more preferably 80 μm or less, 70 μm or less, or 60 μm or less.
[0043] Examples of the resin constituting the resin substrate 11 include polyimide resins, polyamideimide resins, polyamide resins, polyester resins (for example, polyethylene terephthalate resins and polyethylene naphthalate resins), and mixtures of two or more of these resins.
[0044] Among these resins, polyimide-based resins, polyamide-based resins, or mixtures thereof are preferred, since they are not only less likely to crack or break in a continuous folding test, but also have excellent hardness and transparency, and are also excellent in heat resistance, and can be imparted with even better hardness and transparency by baking.
[0045] The polyimide resin is obtained by reacting a tetracarboxylic acid component with a diamine component. The polyimide resin is not particularly limited, but it is preferable that the polyimide resin has at least one structure selected from the group consisting of structures represented by the following general formula (1) and the following general formula (3) in terms of excellent light transmittance and excellent rigidity.
[0046] [ka]
[0047] In the above general formula (1), R 1 is a tetravalent group which is a tetracarboxylic acid residue, R 2 represents at least one divalent group selected from the group consisting of trans-cyclohexanediamine residue, trans-1,4-bismethylenecyclohexanediamine residue, 4,4'-diaminodiphenylsulfone residue, 3,4'-diaminodiphenylsulfone residue, and divalent groups represented by the following general formula (2). n represents the number of repeating units and is 1 or more. In this specification, the term "tetracarboxylic acid residue" refers to a residue obtained by removing four carboxyl groups from a tetracarboxylic acid, and represents the same structure as the residue obtained by removing an acid dianhydride structure from a tetracarboxylic dianhydride. In addition, the term "diamine residue" refers to a residue obtained by removing two amino groups from a diamine.
[0048] [ka] In the above general formula (2), R 3 and R 4 each independently represents a hydrogen atom, an alkyl group, or a perfluoroalkyl group.
[0049] [ka]
[0050] In the above general formula (3), R 5 R represents at least one tetravalent group selected from the group consisting of a cyclohexanetetracarboxylic acid residue, a cyclopentanetetracarboxylic acid residue, a dicyclohexane-3,4,3',4'-tetracarboxylic acid residue, and a 4,4'-(hexafluoroisopropylidene)diphthalic acid residue; 6 represents a divalent group which is a diamine residue. n' represents the number of repeating units and is 1 or more.
[0051] In the above general formula (1), R 1 R in the above general formula (1) is a tetracarboxylic acid residue, and can be a residue obtained by removing the acid dianhydride structure from the tetracarboxylic acid dianhydride as exemplified above. 1 Among them, from the viewpoint of improving light transmittance and improving rigidity, it is preferable to include at least one selected from the group consisting of 4,4'-(hexafluoroisopropylidene)diphthalic acid residue, 3,3',4,4'-biphenyltetracarboxylic acid residue, pyromellitic acid residue, 2,3',3,4'-biphenyltetracarboxylic acid residue, 3,3',4,4'-benzophenonetetracarboxylic acid residue, 3,3',4,4'-diphenylsulfonetetracarboxylic acid residue, 4,4'-oxydiphthalic acid residue, cyclohexanetetracarboxylic acid residue, and cyclopentanetetracarboxylic acid residue, and it is further preferable to include at least one selected from the group consisting of 4,4'-(hexafluoroisopropylidene)diphthalic acid residue, 4,4'-oxydiphthalic acid residue, and 3,3',4,4'-diphenylsulfonetetracarboxylic acid residue.
[0052] R 1 In the present invention, the total amount of these suitable residues is preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more.
[0053] Also, R 1It is also preferable to use a mixture of a tetracarboxylic acid residue group (Group A) suitable for improving rigidity, such as at least one selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic acid residues, 3,3',4,4'-benzophenonetetracarboxylic acid residues, and pyromellitic acid residues, and a tetracarboxylic acid residue group (Group B) suitable for improving transparency, such as at least one selected from the group consisting of 4,4'-(hexafluoroisopropylidene)diphthalic acid residues, 2,3',3,4'-biphenyltetracarboxylic acid residues, 3,3',4,4'-diphenylsulfonetetracarboxylic acid residues, 4,4'-oxydiphthalic acid residues, cyclohexanetetracarboxylic acid residues, and cyclopentanetetracarboxylic acid residues.
[0054] In this case, the content ratio of the tetracarboxylic acid residue group suitable for improving the rigidity (Group A) to the tetracarboxylic acid residue group suitable for improving the transparency (Group B) is preferably 0.05 mol or more and 9 mol or less, more preferably 0.1 mol or more and 5 mol or less, and even more preferably 0.3 mol or more and 4 mol or less, of the tetracarboxylic acid residue group suitable for improving the rigidity (Group A) per 1 mol of the tetracarboxylic acid residue group suitable for improving the transparency (Group B).
[0055] R in the above general formula (1) 2 Among these, from the viewpoints of improving light transmittance and improving rigidity, R is preferably at least one divalent group selected from the group consisting of a 4,4'-diaminodiphenyl sulfone residue, a 3,4'-diaminodiphenyl sulfone residue, and a divalent group represented by the above general formula (2), and further preferably at least one divalent group selected from the group consisting of a 4,4'-diaminodiphenyl sulfone residue, a 3,4'-diaminodiphenyl sulfone residue, and a divalent group represented by the above general formula (2) in which R3 and R4 are perfluoroalkyl groups.
[0056] R in the above general formula (3) 5Among these, from the viewpoints of improving light transmittance and improving rigidity, it is preferable that the diphthalic acid residue contains 4,4'-(hexafluoroisopropylidene)diphthalic acid residue, 3,3',4,4'-diphenylsulfonetetracarboxylic acid residue, and oxydiphthalic acid residue.
[0057] R 5 In the above, these suitable residues are preferably contained in an amount of 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more.
[0058] R in the above general formula (3) 6 is a diamine residue, and may be a residue obtained by removing two amino groups from the diamines exemplified above. Among them, R6 in the above general formula (3) may be, from the viewpoints of improving light transmittance and improving rigidity, a 2,2'-bis(trifluoromethyl)benzidine residue, a bis[4-(4-aminophenoxy)phenyl]sulfone residue, a 4,4'-diaminodiphenylsulfone residue, a 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane residue, a bis[4-(3-aminophenoxy)phenyl]sulfone residue, a 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether residue, a 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene residue, a 2,2-bis[4-(4-amino-2-trifluoromethyl ... It is preferable that the aryl group contains at least one divalent group selected from the group consisting of a 2,2'-bis(trifluoromethyl)benzidine residue, a bis[4-(4-aminophenoxy)phenyl]hexafluoropropane residue, a 4,4'-diamino-2-(trifluoromethyl)diphenyl ether residue, a 4,4'-diaminobenzanilide residue, an N,N'-bis(4-aminophenyl)terephthalamide residue, and a 9,9-bis(4-aminophenyl)fluorene residue, and it is further preferable that the aryl group contains at least one divalent group selected from the group consisting of a 2,2'-bis(trifluoromethyl)benzidine residue, a bis[4-(4-aminophenoxy)phenyl]sulfone residue, and a 4,4'-diaminodiphenyl sulfone residue.
[0059] R 6In the present invention, the total amount of these suitable residues is preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more.
[0060] Also, R 6 and a diamine residue group (Group C) suitable for improving rigidity, such as at least one selected from the group consisting of bis[4-(4-aminophenoxy)phenyl]sulfone residue, 4,4'-diaminobenzanilide residue, N,N'-bis(4-aminophenyl)terephthalamide residue, paraphenylenediamine residue, metaphenylenediamine residue, and 4,4'-diaminodiphenylmethane residue; and a diamine residue group (Group C) suitable for improving rigidity, such as at least one selected from the group consisting of 2,2'-bis(trifluoromethyl)benzidine residue, 4,4'-diaminodiphenylsulfone residue, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane residue, bis[4-(3-aminophenoxy)phenyl]hexafluoropropane residue, It is also preferred to use a mixture of diamine residues suitable for improving transparency (Group D), such as at least one selected from the group consisting of 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether residue, 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene residue, 2,2-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane residue, 4,4'-diamino-2-(trifluoromethyl)diphenyl ether residue, and 9,9-bis(4-aminophenyl)fluorene residue.
[0061] In this case, the content ratio of the diamine residue group suitable for improving rigidity (Group C) to the diamine residue group suitable for improving transparency (Group D) is preferably 0.05 mol or more and 9 mol or less of the diamine residue group suitable for improving rigidity (Group C) per 1 mol of the diamine residue group suitable for improving transparency (Group D), more preferably 0.1 mol or more and 5 mol or less, and even more preferably 0.3 mol or more and 4 mol or less.
[0062] In the structures represented by the above general formula (1) and general formula (3), n and n' each independently represent the number of repeating units and are 1 or more. The number of repeating units in the polyimide, n, may be appropriately selected according to the structure so as to show a preferred glass transition temperature described later, and is not particularly limited. The average number of repeating units is usually 10 to 2000, and more preferably 15 to 1000.
[0063] The polyimide resin may contain a polyamide structure in part thereof, for example, a polyamideimide structure containing a tricarboxylic acid residue such as trimellitic anhydride, or a polyamide structure containing a dicarboxylic acid residue such as terephthalic acid.
[0064] From the viewpoint of heat resistance, the polyimide resin preferably has a glass transition temperature of 250° C. or higher, and more preferably 270° C. or higher. On the other hand, from the viewpoints of ease of stretching and reduction of the bake temperature, the glass transition temperature is preferably 400° C. or lower, and more preferably 380° C. or lower.
[0065] Specifically, examples of polyimide resins include compounds having a structure represented by the following formula: In the following formula, n is a repeating unit and represents an integer of 2 or more. [ka]
[0066] [ka]
[0067] [ka]
[0068] [ka]
[0069]
change
[0070]
change
[0071]
change
[0072]
change
[0073]
change
[0074]
change
[0075]
change
[0076]
change
[0077]
change
[0078]
change
[0079]
change
[0080] [ka]
[0081] [ka]
[0082] Among the above polyimide-based resins, polyimide-based resins or polyamide-based resins having a structure in which intramolecular or intermolecular charge transfer is unlikely to occur are preferred because they have excellent transparency. Specific examples thereof include fluorinated polyimide-based resins such as those represented by the above formulas (4) to (11) and polyimide-based resins having an alicyclic structure such as those represented by the above formulas (13) to (16).
[0083] In addition, the fluorinated polyimide resins of the above formulas (4) to (11) and the like have a fluorinated structure, and therefore have high heat resistance and are not discolored by heat during the production of a polyimide film made of the polyimide resin, and therefore have excellent transparency.
[0084] The polyamide resin is a concept including not only aliphatic polyamides but also aromatic polyamides (aramids). Examples of polyamide resins include compounds having skeletons represented by the following formulas (21) to (23). In the following formulas, n is a repeating unit and represents an integer of 2 or more.
[0085] [ka]
[0086] [ka]
[0087] [ka]
[0088] The substrate containing the polyimide-based resin or polyamide-based resin represented by the above formulas (4) to (20) and (23) may be commercially available. Examples of commercially available polyimide-based resins include Neoprim (registered trademark) manufactured by Mitsubishi Gas Chemical Company, Inc., and examples of commercially available substrates containing the polyamide-based resins include Miktron (registered trademark) manufactured by Toray Industries, Inc.
[0089] The polyimide-based resins or polyamide-based resins represented by the above formulas (4) to (20) and (23) may be synthesized by a known method. For example, a method for synthesizing the polyimide-based resin represented by the above formula (4) is described in JP-A-2009-132091, and specifically, the polyimide-based resin can be obtained by reacting 4,4'-hexafluoropropylidenebisphthalic dianhydride (FPA) represented by the following formula (24) with 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB). [ka]
[0090] The weight average molecular weight of the polyimide resin or polyamide resin is preferably in the range of 3000 to 500,000, more preferably in the range of 5000 to 300,000, and even more preferably in the range of 10,000 to 200,000. If the weight average molecular weight is less than 3000, sufficient strength may not be obtained, and if it exceeds 500,000, the viscosity increases and the solubility decreases, so that a substrate with a smooth surface and a uniform film thickness may not be obtained. In this specification, the "weight average molecular weight" is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0091] From the viewpoint of being able to improve the hardness, it is preferable to use a substrate containing a fluorinated polyimide resin represented by the above formulas (4) to (11) or a polyamide resin having a halogen group represented by the above formula (23), for the resin substrate 11. Among them, from the viewpoint of being able to further improve the hardness, it is more preferable to use a substrate containing a polyimide resin represented by the above formula (4).
[0092] Examples of polyester-based resins include resins containing at least one of polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate as a constituent component.
[0093] <<Hard coat layer>> The hard coat layer 14 is provided on the second surface 11B side of the resin substrate 11. In this specification, the term "hard coat layer" refers to a layer having optical transparency and a Martens hardness higher than that of the resin substrate. The Martens hardnesses of the resin substrate 11 and the hard coat layer 14 are measured by the same method as that of the reinforced portion 12 described later.
[0094] The thickness of the hard coat layer 14 is preferably 1 μm or more and 20 μm or less. If the thickness of the hard coat layer 14 is 1 μm or more, sufficient hardness as a hard coat layer can be obtained, and if it is 20 μm or less, deterioration of processability can be suppressed. In this specification, the "thickness of the hard coat layer" means the thickness (total thickness) of the hard coat layer in the case where the hard coat layer has a multi-layer structure. The lower limit of the hard coat layer 14 is preferably 2 μm or more, 3 μm or more, or 5 μm or more, and the upper limit is more preferably 15 μm or less, 10 μm or less, or 8 μm or less.
[0095] The film thickness of the hard coat layer is determined by photographing a cross section of the hard coat layer using a scanning transmission electron microscope (STEM) or a transmission electron microscope (TEM), measuring the film thickness of the hard coat layer 14 at 20 points on the image of the cross section, and calculating the arithmetic average value of the film thicknesses at the 20 points.
[0096] A specific method for taking a cross-sectional photograph is described below. First, a block is prepared by embedding an optical film cut into a size of 1 mm x 10 mm in an embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm is cut from this block by a general slice preparation method. For example, an ultramicrotome EM UC7 made by Leica Microsystems can be used to prepare the slice. Then, this uniform slice without holes is used as a measurement sample. Then, a cross-sectional photograph of the measurement sample is taken using a scanning transmission electron microscope (STEM). An example of a scanning transmission electron microscope (STEM) is the S-4800 made by Hitachi High-Technologies Corporation. When taking a cross-sectional photograph using the S-4800, the detector is set to "TE", the acceleration voltage is set to "30 kV", and the emission current is set to "10 μA", and the cross-section is observed. The magnification is adjusted by adjusting the focus and adjusting the contrast and brightness appropriately between 5,000 times and 200,000 times while observing whether each layer can be distinguished. The preferred magnification is 10,000 to 100,000, more preferably 10,000 to 50,000, and most preferably 25,000 to 50,000. When taking a cross-sectional photograph using the S-4800, the beam monitor aperture may be set to "3", the objective lens aperture may be set to "3", and the WD may be set to "8 mm". When measuring the thickness of the hard coat layer, it is important that the interface contrast between the hard coat layer and other layers (e.g., resin substrate) can be observed as clearly as possible when observing the cross section. If the interface is difficult to see due to insufficient contrast, a dyeing process using osmium tetroxide, ruthenium tetroxide, tungstophosphoric acid, or the like may be performed to make the interface between the organic layers easier to see, so a dyeing process may be performed. In addition, the contrast of the interface may be difficult to see at a high magnification. In that case, a low magnification is also observed at the same time. For example, the film is observed at two magnifications, high and low, such as 25,000x and 50,000x, or 50,000x and 100,000x, and the arithmetic average value is calculated at both magnifications. The average value is then used as the film thickness of the hard coat layer.
[0097] The hard coat layer may have a single layer structure, but is preferably a multi-layer structure of two or more layers from the viewpoint of improving folding performance. Fig. 1 shows an example in which the hard coat layer 14 is composed of a first hard coat layer 15 and a second hard coat layer 16 laminated on the first hard coat layer 15. When the hard coat layer has a multi-layer structure, the Martens hardness of each layer is higher than the Martens hardness of the resin substrate.
[0098] <First hard coat layer> The first hard coat layer 15 is a layer for mainly imparting hardness to the optical film 10. The first hard coat layer 15 preferably has a Martens hardness of 500 MPa or more and 2000 MPa or less at the center of the cross section of the first hard coat layer 15. If the Martens hardness at the center of the cross section of the first hard coat layer 15 is 500 MPa or more, the hardness of the hard coat layer 14 will not be insufficient, and if it is 2000 MPa or less, better folding properties can be obtained. The lower limit of the Martens hardness at the center of the cross section of the first hard coat layer 15 is preferably 600 MPa or more, 700 MPa or more, or 800 MPa or more, and the upper limit is preferably 1500 MPa or less, 1400 MPa or less, or 1300 MPa or less.
[0099] The Martens hardness of the first hard coat layer 15 is preferably greater than that of the second hard coat layer 16. Such a relationship between the Martens hardnesses allows the optical film 10 to have a particularly good pencil hardness. This is because, when the optical film 10 is subjected to a pencil hardness test and pressed with a load applied to a pencil, the optical film 10 is prevented from being deformed, resulting in less scratches and dents. As a method for making the Martens hardness of the first hard coat layer 15 greater than that of the second hard coat layer 16, for example, a method of controlling the content of inorganic particles to be contained more on the first hard coat layer 15 side, which will be described later, can be mentioned. In addition, when the hard coat layer has a single layer structure, it is preferable that the inorganic particles are unevenly distributed on the resin substrate side in the hard coat layer, that is, the content ratio of the inorganic particles in the hard coat layer is greater on the resin substrate side and is smaller toward the surface side of the optical film.
[0100] The first hard coat layer 15 contains a resin. It is preferable that the first hard coat layer 15 further contains inorganic particles dispersed in the resin.
[0101] (resin) The resin contains a polymer (cured product) of a polymerizable compound (curable compound). The polymerizable compound has at least one polymerizable functional group in the molecule. Examples of the polymerizable functional group include ethylenically unsaturated groups such as (meth)acryloyl group, vinyl group, and allyl group. The term "(meth)acryloyl group" includes both "acryloyl group" and "methacryloyl group".
[0102] The polymerizable compound is preferably a polyfunctional (meth)acrylate. Examples of the polyfunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and the like. acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and those modified with PO, EO, caprolactone, etc.
[0103] Among these, those having three to six functional groups are preferred because they can suitably satisfy the above-mentioned Martens hardness, and examples thereof include pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), trimethylolpropane tri(meth)acrylate, tripentaerythritol octa(meth)acrylate, and tetrapentaerythritol deca(meth)acrylate. In this specification, (meth)acrylate means acrylate and methacrylate.
[0104] In addition, the composition may further contain a monofunctional (meth)acrylate monomer in order to adjust the hardness or viscosity of the composition, improve adhesion, etc. Examples of the monofunctional (meth)acrylate monomer include hydroxyethyl acrylate (HEA), glycidyl methacrylate, methoxypolyethylene glycol (meth)acrylate, isostearyl (meth)acrylate, 2-acryloyloxyethyl succinate, acryloylmorpholine, N-acryloyloxyethylhexahydrophthalimide, cyclohexyl acrylate, tetrahydrofuryl acrylate, isobornyl acrylate, phenoxyethyl acrylate, and adamantyl acrylate.
[0105] From the viewpoint of improving the hardness of the resin layer, the weight average molecular weight of the monomer is preferably less than 1000, and more preferably from 200 to 800. The weight average molecular weight of the polymerizable oligomer is preferably from 1000 to 20,000, more preferably from 1000 to 10,000, and even more preferably from 2000 to 7000.
[0106] (Inorganic particles) The inorganic particles are not particularly limited as long as they can improve hardness, but from the viewpoint of obtaining excellent hardness, silica particles are preferred. Among the silica particles, reactive silica particles are preferred. The reactive silica particles are silica particles that can form a crosslinked structure with the polyfunctional (meth)acrylate, and the hardness of the first hard coat layer 15 can be sufficiently increased by including the reactive silica particles.
[0107] The reactive silica particles preferably have a reactive functional group on the surface thereof, and as the reactive functional group, for example, the above-mentioned polymerizable functional group is preferably used.
[0108] The reactive silica particles are not particularly limited, and conventionally known ones can be used, for example, reactive silica particles described in JP-A-2008-165040, etc. In addition, commercially available reactive silica particles include MIBK-SD, MIBK-SDMS, MIBK-SDL, MIBK-SDZL manufactured by Nissan Chemical Industries, Ltd., and V8802, V8803, etc. manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0109] The silica particles may be spherical silica particles, but are preferably irregular silica particles. Spherical silica particles and irregular silica particles may be mixed. In this specification, the term "spherical silica particles" refers to silica particles that are, for example, spherical or elliptical, and the term "irregular silica particles" refers to silica particles that have random irregularities on the surface, such as potato-shaped (aspect ratio when observed in cross section is 1.2 or more and 40 or less). The irregular silica particles have a larger surface area than spherical silica particles, so that the contact area with the polyfunctional (meth)acrylate or the like is increased by including such irregular silica particles, and the hardness of the hard coat layer can be improved. Whether the silica particles contained in the hard coat layer are irregular silica particles can be confirmed by observing the cross section of the hard coat layer with a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM). When spherical silica particles are used, the smaller the particle diameter of the spherical silica particles, the higher the hardness of the hard coat layer. In contrast, irregularly shaped silica particles can achieve a hardness equivalent to that of spherical silica particles, even if they are not as small as the smallest particle size spherical silica particles available on the market.
[0110] The average particle diameter of the silica particles is preferably 5 nm or more and 200 nm or less. If the average particle diameter of the silica particles is less than 5 nm, it becomes difficult to manufacture the particles themselves, and the particles may aggregate with each other, and it may be extremely difficult to make them into irregular shapes. Furthermore, the irregular silica particles may have poor dispersibility and aggregate at the ink stage before the coating. On the other hand, if the average particle diameter of the irregular silica particles exceeds 200 nm, problems such as large irregularities being formed in the hard coat layer and an increase in haze may occur. When the silica particles are spherical silica particles, the average particle diameter of the silica particles is determined by measuring the particle diameters of 20 particles from an image of the cross section of the particles taken using a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM), and the arithmetic average value of the particle diameters of the 20 particles. In addition, when the silica particles are irregularly shaped silica particles, the average particle diameter of the silica particles is determined by measuring the maximum (long axis) and minimum (short axis) of the distance between two points on the outer periphery of the particles from an image of the cross section of the hard coat layer taken using a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM), averaging them to determine the particle diameter, and using this as the arithmetic mean value of the particle diameters of 20 particles. When taking a cross-sectional photograph using a scanning transmission electron microscope (STEM) (product name "S-4800 (TYPE2)", manufactured by Hitachi High-Technologies Corporation), observation is performed with the detector (selection signal) set to "TE", the acceleration voltage set to "30kV", and the emission set to "10μA".
[0111] By controlling the size and amount of the inorganic particles, it is possible to control the hardness (Martens hardness) of the first hard coat layer 15. For example, when forming the first hard coat layer 15, it is preferable that the silica particles have a diameter of 5 nm or more and 200 nm or less, and are contained in an amount of 25 to 60 parts by mass relative to 100 parts by mass of the polymerizable compound.
[0112] <Second hard coat layer> The second hard coat layer 16 is a layer for satisfying the above-mentioned continuous folding test. The second hard coat layer 16 preferably has a Martens hardness of 375 MPa or more and 1500 MPa or less at the center of the cross section of the second hard coat layer 16. If the Martens hardness at the center of the cross section of the second hard coat layer 16 is 375 MPa or more, the scratch resistance of the hard coat layer 14 will not be insufficient, and if it is 1500 MPa or less, better folding properties can be obtained. The lower limit of the Martens hardness at the center of the cross section of the second hard coat layer 16 is more preferably 450 MPa or more, 470 MPa or more, or 490 MPa or more, and the upper limit is more preferably 575 MPa or less, 550 MPa or less, or 530 MPa or less.
[0113] The second hard coat layer 16 contains a resin. The second hard coat layer 16 may further contain inorganic particles dispersed in the resin.
[0114] (resin) The resin contains a polymer (cured product) of a polymerizable compound (curable compound). The polymerizable compound is preferably a polyfunctional (meth)acrylate. Examples of the polyfunctional (meth)acrylate include the same polyfunctional (meth)acrylates as those in the section on the first hard coat layer 15. The second hard coat layer 16 may contain, in addition to the polyfunctional (meth)acrylates, a polyfunctional urethane (meth)acrylate and / or a polyfunctional epoxy (meth)acrylate.
[0115] (Inorganic particles) Examples of the inorganic particles include the same inorganic particles as those in the column for the first hard coat layer 15. The content of the inorganic particles in the second hard coat layer 16 is not particularly limited, but is preferably, for example, 0% by mass or more and 50% by mass or less with respect to the second hard coat layer 16.
[0116] At least one of the first hard coat layer 15 and the second hard coat layer 16 may contain materials other than the above-mentioned materials within a range that satisfies the above-mentioned Martens hardness. For example, the resin component may contain a polymerizable monomer or a polymerizable oligomer that forms a cured product by irradiation with ionizing radiation. Examples of the polymerizable monomer or oligomer include a (meth)acrylate monomer having a radical polymerizable unsaturated group in the molecule, or a (meth)acrylate oligomer having a radical polymerizable unsaturated group in the molecule. Examples of the (meth)acrylate monomer having a radical polymerizable unsaturated group in the molecule or a (meth)acrylate oligomer having a radical polymerizable unsaturated group in the molecule include monomers or oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, epoxy (meth)acrylate, melamine (meth)acrylate, polyfluoroalkyl (meth)acrylate, and silicone (meth)acrylate. These polymerizable monomers or oligomers may be used alone or in combination of two or more. Among them, polyfunctional (six or more functional) urethane (meth)acrylates having a weight average molecular weight of 1,000 to 10,000 are preferred.
[0117] The hard coat layer 14 (at least one of the first hard coat layer 15 and the second hard coat layer 16) may further contain an ultraviolet absorbing agent, a spectral transmittance adjusting agent, and / or an antifouling agent.
[0118] <<Reinforcement section>> The multiple reinforced portions 12 are arranged in a plane on the first surface 11A side of the resin base material 11. The reinforced portions 12 are attached to the first surface 11A of the resin base material 11 via the adhesive layer 17 as described above.
[0119] The thickness of the reinforced portion 12 is 150 μm or more. The lower limit of the thickness of the reinforced portion 12 is more preferably 200 μm or more, 300 μm or more, or 400 μm or more, and the upper limit is preferably 1000 μm or less, 700 μm or less, or 500 μm or less, from the viewpoint of designing a thin and light optical film.
[0120] The thickness of the reinforced portion 12 is determined by photographing a cross section of the reinforced portion using a scanning electron microscope (SEM), measuring the thickness of the reinforced portion at 20 points in the image of the cross section, and calculating the arithmetic average value of the thicknesses at the 20 points. The specific method of photographing the cross section is as follows. First, a block is prepared by embedding an optical film cut to 1 mm x 10 mm in an embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm without holes is cut out from this block by a general slice preparation method. Here, the slice having a thickness of 70 nm to 100 nm is cut out because the remaining block from which the slice is cut out is used for measurement, and cutting out a slice of this thickness improves the flatness of the cross section of the remaining block. Note that if the flatness of the remaining block is poor, the measurement accuracy may deteriorate. For example, an ultramicrotome EM UC7 by Leica Microsystems Inc. is used to prepare the slice. The remaining block from which the uniform slice without holes is cut out is used as the measurement sample. Then, a cross-sectional photograph of the measurement sample is taken using a scanning electron microscope (SEM). An example of a scanning electron microscope (SEM) is the S-4800 manufactured by Hitachi High-Technologies Corporation. When taking a cross-sectional photograph using the S-4800, the detector is set to "SE", the acceleration voltage is set to "5 kV", and the emission current is set to "10 μA" to observe the cross section. The magnification is adjusted appropriately from 100 to 100,000 times by adjusting the focus and observing whether the contrast and brightness of each layer can be distinguished. Furthermore, the beam monitor aperture is set to "3", the objective lens aperture is set to "3", and the WD is set to "8 mm". The thickness of the resin substrate and the resin layer are also measured using the same method as the thickness of the reinforced part.
[0121] The Martens hardness of the reinforced portion 12 is 30 MPa or more. In this specification, "Martens hardness" refers to the hardness when an indenter is pressed 500 nm in hardness measurement by nanoindentation method. The lower limit of the Martens hardness of the reinforced portion 12 is preferably 50 MPa or more, 100 MPa or more, or 200 MPa or more. The upper limit of the Martens hardness of the reinforced portion 12 is preferably 5000 MPa or less, 4000 MPa or less, 3000 MPa or less, or 1000 MPa or less, from the viewpoint of suppressing breakage when dropped.
[0122] The Martens hardness can be measured as follows using a nanoindenter (for example, TI950 TriboIndenter manufactured by Bruker). Specifically, first, a block is prepared by embedding an optical film cut to 1 mm×10 mm in an embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm without holes is cut out from this block by a general slice preparation method. Here, the slice having a thickness of 70 nm to 100 nm is cut out because the remaining block from which the slice is cut out is used for measurement, and by cutting out a slice of this thickness, the cross-section of the remaining block is made good in flatness. Note that if the remaining block is poorly flat, the measurement accuracy may be deteriorated. For example, an ultramicrotome EM UC7 manufactured by Leica Microsystems Co., Ltd. can be used to prepare the slice. The remaining block from which the uniform slice without holes is cut out is used as the measurement sample. Next, in the cross section obtained by cutting out the above-mentioned piece of the measurement sample, a Berkovich indenter (triangular pyramid, TI-0039 manufactured by Bruker) is pressed 500 nm into the center of the cross section of the reinforced part under the following measurement conditions. Here, the Berkovich indenter is pressed into a portion 500 nm or more away from each of both ends of the reinforced part toward the center of the reinforced part in order to avoid the influence of the side edges of the reinforced part. Thereafter, the specimen is held for a certain period of time to relax the residual stress, and then the load is removed and the maximum load after relaxation is measured, and the maximum load P max(μN) and the area A of the 500 nm deep indentation (nm 2 ) and P max Martens hardness is calculated by multiplying the measured value by (AB) / B x 100 (%). Martens hardness is the arithmetic average of the values obtained by measuring at 10 locations. If any of the measured values deviate from the arithmetic average by more than ±20%, those values are to be excluded and remeasured. Whether or not any of the measured values deviate from the arithmetic average by more than ±20% is determined by whether the value (%) calculated by (AB) / B x 100, where A is the measured value and B is the arithmetic average, is more than ±20%. (Measurement conditions) ·Loading speed: 10nm / sec ·Holding time: 5 seconds ·Loading and unloading speed: 10nm / sec ·Measurement temperature: 23~28℃ Relative humidity: 30%~70%
[0123] From the viewpoint of thinning, the reinforced portion 12 is preferably plate-shaped, and the planar shape of the reinforced portion 12 is not particularly limited, but may be, for example, a polygonal shape, a circular shape, or an elliptical shape. In this specification, the term "polygonal shape" refers to a concept including a triangular shape, or a rectangular shape such as a rectangular shape or a square shape. The reinforced portion 12 shown in FIG. 2 is rectangular.
[0124] From the viewpoint of ease of folding the optical film 10, it is preferable that a gap 12A exists between the reinforced parts 12. As described above, in the optical film 10, the region corresponding to this gap 12A becomes the bending region 10C. The width of the gap 12A is preferably 300 nm or more and 10 mm or less. If the width of the gap 12A is 300 nm or more, the reinforced parts 12 do not interfere with the folding of the optical film 10, and the folding can be performed smoothly. If the width of the gap 12A is 10 mm or less, the region where the reinforced parts 12 exist becomes large, and therefore the impact resistance can be further improved.
[0125] Examples of materials constituting the reinforced portion 12 include glass, acrylic resin, inorganic (silica)-organic hybrid resin, etc. Among these, acrylic resin is preferable from the viewpoint of ease of adjusting the refractive index and thickness and ease of processing.
[0126] <<Resin layer>> The resin layer 13 is a layer containing a resin. The resin layer 13 is provided on the first surface 11A side of the resin substrate 11, and at least a part of the reinforced portion 12 is covered with the resin layer 13. In FIG. 1, the surfaces of the reinforced portion 12 other than the surface on the resin substrate 11 side are covered with the resin layer 13. That is, a part of the resin layer 13 also enters the gap 12A between the reinforced portions 12, and the side surface of the reinforced portion 12 is covered with the resin layer 13. The resin layer may have a multilayer structure consisting of two or more resin layers.
[0127] The resin layer 13 preferably has a function of suppressing the shape of the reinforced portion 12 from being visually recognized. Specifically, the absolute value of the refractive index difference between the reinforced portion 12 and the resin layer 13 is preferably 0.02 or less. When a plurality of reinforced portions 12 are arranged in the optical film 10, there is a risk that the shape of the reinforced portion 12 will be visually recognized. However, if the refractive index difference between the reinforced portion 12 and the resin layer 13 is 0.02 or less, the shape of the reinforced portion 12 will be difficult to visually recognize. The refractive index of the reinforced portion 12 can be calculated by taking out 10 pieces of the reinforced portion 12 by cutting out or the like, measuring the refractive index of the reinforced portion 12 for each of the taken out pieces by the Becke method, and averaging the measured refractive indexes of the reinforced portion 12 for the 10 pieces. The Becke method is a method in which a refractive index standard solution with a known refractive index is used, the above-mentioned piece is placed on a slide glass or the like, the refractive index standard solution is dropped onto the sample, the piece is immersed in the refractive index standard solution, the state is observed under a microscope, and the refractive index of the refractive index standard solution at which the bright line (Becke line) that appears on the surface of the reinforced part due to the difference in refractive index between the surface of the reinforced part and the refractive index standard solution cannot be visually observed is determined as the refractive index of the reinforced part. The refractive index of the resin layer 13 is also determined by the same method as that of the reinforced part 12. The difference in refractive index between the reinforced part 12 and the resin layer 13 is more preferably 0.01 or less, and most preferably 0.
[0128] In the region where the reinforcement portion 12 exists, excellent impact resistance can be obtained, but in the gap 12A between the reinforcement portions 12 where the reinforcement portion 12 does not exist, the impact resistance may be poor. For this reason, in order to improve the impact resistance of the gap 12A between the reinforcement portions 12, the resin layer 13 is preferably a layer having impact resistance. When the resin layer 13 has impact resistance, it is preferable that the shear storage modulus G' of the resin layer 13 at 25°C in a frequency range of 500 Hz to 1000 Hz is 1 MPa to 1500 MPa. If the shear storage modulus G' of the resin layer 13 is 1 MPa or more, when an impact is applied to the surface 10A of the optical film 10, not only the deformation of the optical film itself but also the plastic deformation of the adhesive layer can be more suppressed even when the adhesive layer is disposed inside the image display device rather than the optical film. In addition, if the shear storage modulus G' of the resin layer 13 is 1500 MPa or less, cracking of the optical film when folded can be more suppressed. The lower limit of the shear storage modulus G' of the resin layer 13 is more preferably 100 MPa or more, 200 MPa or more, or 300 MPa or more, and the upper limit of the shear storage modulus G' of the resin layer 13 is more preferably 1200 MPa or less, 1000 MPa or less, or 800 MPa or less. By setting the upper limit in such a manner, good restorability can be obtained when the resin layer 13 is folded, left to stand, and then opened again.
[0129] In the resin layer 13, the shear loss modulus G" at 25°C in the frequency range of 500 Hz to 1000 Hz is preferably 0.1 MPa or more and 200 MPa or less. If the shear loss modulus G" of the resin layer 13 is 0.1 MPa or more, better impact absorption performance can be obtained. Furthermore, if the shear loss modulus G" of the resin layer 13 is 200 MPa or less, there is no risk of the hardness of the resin layer 13 decreasing. The lower limit of the shear loss modulus G" of the resin layer 13 is preferably 1 MPa or more, 10 MPa or more, or 30 MPa or more, and from the viewpoint of making the resin layer 13 thinner, the upper limit of the shear loss modulus G" of the resin layer 13 is more preferably 150 MPa or less, 130 MPa or less, or 100 MPa or less.
[0130] The shear storage modulus G' and shear loss modulus G'' of the resin layer 13 can be measured by a dynamic viscoelasticity measuring device (DMA). When measuring the shear storage modulus G' and shear loss modulus G'' of the resin layer 13 by a dynamic viscoelasticity measuring device (DMA), first, two rectangular optical films 10 cut to a size of 10 mm x 5 mm are prepared and attached to a solid shear jig, which is an option of a dynamic viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.). Specifically, as shown in FIG. 5, the solid shear jig 30 includes one metal solid shear plate 31 having a thickness of 1 mm and two L-shaped metal fittings 32 arranged on both sides of the solid shear plate 31, and one optical film 10 is sandwiched between the solid shear plate 31 and one of the L-shaped metal fittings 32, and the other optical film 10 is sandwiched between the solid shear plate 31 and the other L-shaped metal fitting 32. In this case, the optical film 10 is sandwiched so that the resin layer 13 faces the solid shear plate 31 and the hard coat layer 14 faces the L-shaped metal fitting 32. Then, the L-shaped metal fittings 32 are tightened with screws 33 to fix the optical film 10. Next, a tensile test chuck consisting of an upper chuck and a lower chuck is attached to a dynamic viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.), and then a solid shear jig is attached between the upper chuck and the lower chuck with a chuck distance of 20 mm. The chuck distance is the distance between the upper chuck and the lower chuck. The set temperature is 25°C and the temperature is increased at 2°C / min. In this state, while the solid shear plate is fixed, a longitudinal vibration with a strain of 1% and a frequency in the range of 500 Hz to 1000 Hz is applied to the two L-shaped metal fittings, and dynamic viscoelasticity measurement of the solid is performed at 25°C to measure the shear storage modulus G' and shear loss modulus G'' of the resin layer 13. Here, the optical film 10 includes the resin substrate 11, the reinforced portion 12, and the hard coat layer 14 in addition to the resin layer 13, but since the resin substrate 11, the reinforced portion 12, and the hard coat layer 14 are harder than the resin layer 13, the influences of the resin substrate 11, the reinforced portion 12, and the hard coat layer 14 can be ignored.For this reason, even if the optical film 10 includes the resin substrate 11, the reinforced portion 12, and the hard coat layer 14 in addition to the resin layer 13, the shear storage modulus G' and shear loss modulus G" measured for the optical film 10 can be regarded as the shear storage modulus G' and shear loss modulus G" of the resin layer 13. The shear storage modulus G' and shear loss modulus G" of the resin layer 13 in the frequency range of 500 Hz to 1000 Hz are determined by applying longitudinal vibrations of frequencies of 500 Hz, 750 Hz, and 950 Hz to the L-shaped fitting 32, measuring the shear storage modulus G' and shear loss modulus G" of the resin layer 13 at each frequency, determining the arithmetic mean value of these shear storage modulus G' and shear loss modulus G", and further repeating this measurement three times to obtain the arithmetic mean value of the three arithmetic mean values obtained. In the above, the frequency range is set to 500 Hz or more and 1000 Hz or less because this frequency range is such that when an object is allowed to freely fall from a height of several centimeters, the surface of the optical film is deformed by several microns to several tens of microns, and is also such a frequency that the optical film can damage a display panel or the like inside the image display device.
[0131] The thickness of the resin layer 13 is preferably 50 μm or more and 600 μm or less. If the thickness of the resin layer 13 is 50 μm or more, the hardness of the resin layer 13 does not decrease, and if the thickness is 600 μm or less, the thickness is not too thick, so that it is suitable for thinning and there is no risk of deterioration in processability. In this specification, the "thickness of the resin layer" means the thickness of the resin layer in the non-bending region. The thickness of the resin layer is measured at 20 points in the non-bending region by the same method as the thickness of the reinforced portion, and the arithmetic average value of the thicknesses at the 20 points is used. The lower limit of the resin layer 13 is more preferably 50 μm or more, 100 μm or more, or 200 μm or more, and the upper limit of the resin layer 13 is more preferably 550 μm or less, 450 μm or less, or 300 μm or less.
[0132] Examples of the resin constituting the resin layer 13 include urethane-based resin, epoxy-based resin, acrylic gel, urethane gel, silicone gel, etc. Among these, urethane-based resin and acrylic gel are preferred. "Gel" generally refers to a dispersion system that has high viscosity and has lost fluidity. The resin layer 13 may contain rubber or a thermoplastic elastomer in addition to the acrylic gel and urethane-based resin.
[0133] (Urethane resin) The urethane resin is a resin having a urethane bond. Examples of the urethane resin include a cured product of an ionizing radiation curable urethane resin composition and a cured product of a thermosetting urethane resin composition. Among these, a cured product of an ionizing radiation curable urethane resin composition is preferred from the viewpoints of obtaining high hardness, a fast curing speed, and excellent mass productivity.
[0134] The ionizing radiation curable urethane resin composition contains a urethane (meth)acrylate, and the thermosetting urethane resin contains a polyol compound and an isocyanate compound. The urethane (meth)acrylate, the polyol compound, and the isocyanate compound may be any one of a monomer, an oligomer, and a prepolymer.
[0135] The number of (meth)acryloyl groups (functional groups) in the urethane (meth)acrylate is preferably 2 or more and 4 or less. If the number of (meth)acryloyl groups in the urethane (meth)acrylate is less than 2, the pencil hardness may be low, and if it exceeds 4, the curing shrinkage may be large, the optical film may curl, and the resin layer may crack when folded. It is more preferable that the upper limit of the number of (meth)acryloyl groups in the urethane (meth)acrylate is 3 or less. The term "(meth)acryloyl group" includes both "acryloyl group" and "methacryloyl group".
[0136] The weight average molecular weight of the urethane (meth)acrylate is preferably 1500 or more and 20000 or less. If the weight average molecular weight of the urethane (meth)acrylate is less than 1500, the impact resistance may decrease, and if it exceeds 20000, the viscosity of the ionizing radiation curable urethane resin composition may increase, resulting in poor coatability. The lower limit of the weight average molecular weight of the urethane (meth)acrylate is more preferably 2000 or more, and the upper limit is more preferably 15000 or less.
[0137] Examples of the repeating unit having a structure derived from a urethane (meth)acrylate include structures represented by the following general formula (25), (26), (27) or (28). [ka] In the above general formula (25), R 7 represents a branched alkyl group, and R 8 represents a branched alkyl group or a saturated cyclic aliphatic group, R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydrogen atom, a methyl group or an ethyl group, m represents an integer of 0 or more, and x represents an integer of 0 to 3.
[0138] [ka] In the above general formula (26), R 7 represents a branched alkyl group, and R 8 represents a branched alkyl group or a saturated cyclic aliphatic group, R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydrogen atom, a methyl group or an ethyl group, n represents an integer of 1 or more, and x represents an integer of 0 to 3.
[0139] [ka] In the above general formula (27), R 7 represents a branched alkyl group, and R 8represents a branched alkyl group or a saturated cyclic aliphatic group, R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydrogen atom, a methyl group or an ethyl group, m represents an integer of 0 or more, and x represents an integer of 0 to 3.
[0140] [ka] In the above general formula (28), R 7 represents a branched alkyl group, and R 8 represents a branched alkyl group or a saturated cyclic aliphatic group, R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydrogen atom, a methyl group or an ethyl group, n represents an integer of 1 or more, and x represents an integer of 0 to 3.
[0141] (Acrylic gel) As the acrylic gel, various types of polymers obtained by polymerizing a monomer containing an acrylic acid ester, which are used in adhesives, etc., can be used. Specifically, examples of acrylic gels that can be used include polymerized or copolymerized acrylic monomers such as ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-hexyl (meth)acrylate, n-amyl (meth)acrylate, i-amyl (meth)acrylate, octyl (meth)acrylate, i-octyl (meth)acrylate, i-myristyl (meth)acrylate, lauryl (meth)acrylate, nonyl (meth)acrylate, i-nonyl (meth)acrylate, i-decyl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, and i-stearyl (meth)acrylate. In this specification, the term "(meth)acrylate" includes both "acrylate" and "methacrylate." The acrylic acid ester used in the (co)polymerization may be used alone or in combination of two or more kinds.
[0142] The structure of the polymer chain (repeating unit) of the resin constituting the resin layer 13 can be determined by analyzing the resin layer 13 by, for example, pyrolysis GC-MS and FT-IR. In particular, pyrolysis GC-MS is useful because it can detect the monomer units contained in the resin layer 13 as monomer components.
[0143] The resin layer 13 may contain an ultraviolet absorbing agent, a spectral transmittance adjusting agent, an antifouling agent, inorganic particles and / or organic particles, etc. As the ultraviolet absorbing agent, etc., the same ultraviolet absorbing agent, etc. as described in the section on the hard coat layer 14 can be used, and therefore the description thereof will be omitted here.
[0144] <<adhesive layer>> The adhesive layer 17 is for attaching the reinforcing portion 12 to the resin substrate 11. In this specification, the term "adhesive layer" is a concept including a pressure-sensitive adhesive layer. Examples of the adhesive layer 17 include a cured product of a liquid curable adhesive layer composition containing a polymerizable compound such as OCR (Optically Clear Resin) and a pressure-sensitive adhesive sheet such as OCA (Optical Clear Adhesive).
[0145] <<Optical film manufacturing method>> The optical film 10 can be produced as follows: First, a first hard coat layer composition is applied onto the second surface 11B of the resin substrate 11 using a coating device such as a bar coater to form a coating film of the first hard coat layer composition.
[0146] <First hard coat layer composition> The first hard coat layer composition contains a polymerizable compound for forming the first hard coat layer 15. The first hard coat layer composition may further contain an ultraviolet absorber, a spectral transmittance adjuster, an antifouling agent, inorganic particles, a leveling agent, a solvent, and a polymerization initiator, as necessary.
[0147] (solvent) Examples of the solvent include alcohols (e.g., methanol, ethanol, propanol, isopropanol, n-butanol, s-butanol, t-butanol, benzyl alcohol, PGME, ethylene glycol, and diacetone alcohol), ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, heptanone, diisobutyl ketone, diethyl ketone, and diacetone alcohol), esters (methyl acetate, ethyl acetate, butyl acetate, n-propyl acetate, isopropyl acetate, and methyl formate), and Examples of the solvent include ethyl, PGMEA), aliphatic hydrocarbons (e.g., hexane, cyclohexane), halogenated hydrocarbons (e.g., methylene chloride, chloroform, carbon tetrachloride), aromatic hydrocarbons (e.g., benzene, toluene, xylene), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone), ethers (e.g., diethyl ether, dioxane, tetrahydrofuran), ether alcohols (e.g., 1-methoxy-2-propanol), carbonates (dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate), and the like. These solvents may be used alone or in combination of two or more. Among them, the above-mentioned solvents are preferably methyl isobutyl ketone and methyl ethyl ketone, in that they can dissolve or disperse components such as urethane (meth)acrylate and other additives and can be suitably applied with the first hard coat layer composition.
[0148] (Polymerization initiator) The polymerization initiator is a component that is decomposed by irradiation with ionizing radiation to generate radicals and initiate or advance the polymerization (crosslinking) of a polymerizable compound.
[0149] The polymerization initiator is not particularly limited as long as it can release a substance that initiates radical polymerization by irradiation with ionizing radiation. The polymerization initiator is not particularly limited, and known initiators can be used, and specific examples thereof include acetophenones, benzophenones, Michler's benzoyl benzoate, α-amyloxime ester, thioxanthones, propiophenones, benzils, benzoins, and acylphosphine oxides. It is also preferable to use a photosensitizer in combination, and specific examples thereof include n-butylamine, triethylamine, and poly-n-butylphosphine.
[0150] After forming a coating film of the composition for the first hard coat layer, the coating film is dried by various known methods, for example, by heating at a temperature of 30°C or higher and 120°C or lower for 10 to 120 seconds to evaporate the solvent.
[0151] After drying the coating film, the coating film is irradiated with ionizing radiation such as ultraviolet light to semi-cure the coating film. In this specification, "semi-cure" means that further irradiation with ionizing radiation will substantially advance the curing. However, at this stage, the coating film may be completely cured (fully cured). In this specification, "completely cured" means that further irradiation with ionizing radiation will not substantially advance the curing.
[0152] After the coating film is semi-cured, a composition for forming a second hard coat layer 16 is applied onto the coating film using a coating device such as a bar coater to form a coating film of the composition for the second hard coat layer.
[0153] <Composition for second hard coat layer> The second hard coat layer composition contains a polymerizable compound for forming the second hard coat layer 16. The second hard coat layer composition may further contain an ultraviolet absorber, a solvent, and a polymerization initiator, if necessary. The second hard coat layer composition preferably has a total solid content of 25 to 55%, similar to the first hard coat layer composition. The solvent and polymerization initiator are the same as those described in the first hard coat layer composition, and therefore will not be described here.
[0154] After forming a coating film of the composition for the second hard coat layer, the coating film is dried by heating it at a temperature of 30°C or higher and 120°C or lower for 10 to 120 seconds using various known methods, for example, to evaporate the solvent.
[0155] After drying the coating film, the coating film of the composition for the second hard coat layer is irradiated with ionizing radiation such as ultraviolet light to completely cure the coating film of the composition for the first hard coat layer and the coating film of the composition for the second hard coat layer, thereby forming a first hard coat layer 15 and a second hard coat layer 16, and obtaining a hard coat layer 14.
[0156] After the hard coat layer 14 is formed, the reinforced portion 12 is arranged in a planar manner on the first surface 11A of the resin substrate 11 via the adhesive layer 17. After the reinforced portion 12 is arranged, a resin layer composition for forming the resin layer 13 is applied from above the reinforced portion 12 using an application device such as a bar coater to form a coating film of the resin layer composition, and the coating film is then cured to form the resin layer 13. In this way, the optical film 10 can be obtained.
[0157] <Composition for resin layer> When the resin layer is made of a urethane-based resin, for example, the ionizing radiation-curable urethane-based resin composition described above in the section on urethane resins can be used as the resin layer composition.
[0158] <<<Image display devices>>> The optical film 10 can be incorporated into a foldable image display device for use. FIG. 6 is a schematic diagram of the image display device according to the present embodiment. As shown in FIG. 6, the image display device 40 mainly includes a housing 41 in which a battery and the like are stored, a protective film 42, a display panel 43, a circular polarizer 44, a touch sensor 45, and an optical film 10 laminated in this order toward the observer side. An adhesive layer 46 having optical transparency is disposed between the display panel 43 and the circular polarizer 44, between the circular polarizer 44 and the touch sensor 45, and between the touch sensor 45 and the optical film 10, and these members are fixed to each other by the adhesive layer 46. The adhesive layer 46 is disposed between the display panel 43 and the circular polarizer 44, between the circular polarizer 44 and the touch sensor 45, and between the touch sensor 45 and the optical film 10, but the location of the adhesive layer is not particularly limited as long as it is between the optical film and the display panel.
[0159] The optical film 10 is disposed so that the resin substrate 11 is closer to the viewer than the reinforced portion 12. In the image display device 40, the surface 14A of the hard coat layer 14 of the optical film 10 (the surface of the second hard coat layer 16) constitutes the surface 40A of the image display device 40. Note that the optical film 10 may be disposed so that the reinforced portion 12 is closer to the viewer than the resin substrate 11.
[0160] In the image display device 40, the display panel 43 is an organic light-emitting diode panel including organic light-emitting diodes and the like. The circularly polarizing plate 44 is disposed closer to the display panel 43 than the touch sensor 45, but may be disposed between the touch sensor 45 and the optical film 10. The touch sensor 45 may be of an on-cell type or an in-cell type.
[0161] For example, OCA (Optical Clear Adhesive) can be used as the adhesive layer 46. However, from the viewpoint of improving impact resistance and preventing damage to the display panel 43, it is preferable to use an adhesive layer made of the acrylic gel. When an adhesive layer made of the acrylic gel is used for the adhesive layer 46, the adhesive layer may be disposed at least between the display panel 43 and the circular polarizer 44, between the circular polarizer 44 and the touch sensor 45, or between the touch sensor 45 and the optical film 10. Since the acrylic gel has adhesiveness, when the resin layer 13 is made of the acrylic gel, the touch sensor 45 and the optical film 10 can be fixed by directly attaching the resin layer 13 to the touch sensor 45 without providing the adhesive layer 46 between the touch sensor 45 and the optical film 10.
[0162] According to this embodiment, since the reinforced portion 12 has a thickness of 150 μm or more and a Martens hardness of 30 MPa or more, excellent impact resistance can be obtained in the non-bending region 10D, which is a region corresponding to the reinforced portion 12. That is, even if the thickness of the reinforced portion is thick, if the Martens hardness of the reinforced portion is low, it may be too soft and excellent impact resistance may not be obtained. Also, even if the Martens hardness of the reinforced portion is high, if the thickness of the reinforced portion is thin, it may deform instantaneously when an impact is applied, and excellent impact resistance may not be obtained. In contrast, in this embodiment, the reinforced portions 12 are thick, 150 μm or more, and have a high Martens hardness of 30 MPa or more, so that excellent impact resistance can be obtained in the non-bending region 10D, which is a region corresponding to the reinforced portion 12. On the other hand, in the bending region 10C, which is a region between the reinforced portions 12, the reinforced portion 12 does not exist, so it is softer than the non-bending region 10D. For this reason, it becomes possible to fold. As a result, excellent impact resistance can be obtained while maintaining good foldability. EXAMPLES
[0163] In order to explain the present invention in detail, the following examples are given, but the present invention is not limited to these examples. Note that the "value calculated based on 100% solid content" below is the value when the solid content in the solvent-diluted product is 100%.
[0164] <Preparation of composition for hard coat layer> First, the components were mixed so as to obtain the composition shown below, thereby obtaining a composition for a hard coat layer. (Hardcoat layer composition 1) Mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (product name "M403", manufactured by Toa Gosei Co., Ltd.): 25 parts by mass Dipentaerythritol EO modified hexaacrylate (product name "A-DPH-6E", manufactured by Shin-Nakamura Chemical Co., Ltd.): 25 parts by weight - Irregularly shaped silica particles (average particle size 25 nm, manufactured by JGC Catalysts and Chemicals Co., Ltd.): 50 parts by weight (based on 100% solids) Photopolymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 4 parts by mass Fluorine-based leveling agent (product name "F568", manufactured by DIC Corporation): 0.2 parts by weight (based on 100% solids) Methyl isobutyl ketone (MIBK): 150 parts by weight
[0165] (Hardcoat layer composition 2) Urethane acrylate (product name "UX5000", manufactured by Nippon Kayaku Co., Ltd.): 25 parts by weight Mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (product name "M403", manufactured by Toa Gosei Co., Ltd.): 50 parts by mass Multifunctional acrylate polymer (product name "Acrylit 8KX-014", manufactured by Taisei Fine Chemical Co., Ltd.): 25 parts by weight (based on 100% solids) Antifouling agent (product name "BYKUV3500", manufactured by BYK-Chemie): 1.5 parts by weight (based on 100% solids) Photopolymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 4 parts by mass Methyl isobutyl ketone (MIBK): 150 parts by weight
[0166] <Preparation of Resin Layer Composition> The components were mixed so as to obtain the composition shown below, thereby obtaining a composition for a resin layer. (Composition 1 for resin layer) Urethane acrylate (product name "UV3310B", manufactured by Nippon Synthetic Chemical Industry Co., Ltd., bifunctional): 85 parts by weight Phenoxyethyl acrylate (product name "Viscoat #192", manufactured by Osaka Organic Chemical Industry Co., Ltd.): 5 parts by weight Mixture of tripentaerythritol acrylate, mono- and dipentaerythritol acrylate, and polymenthaerythritol acrylate (product name: Viscoat #802, manufactured by Osaka Organic Chemical Industry Co., Ltd.): 10 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 5 parts by mass Methyl isobutyl ketone: 10 parts by weight
[0167] (Composition 2 for resin layer) Urethane acrylate (product name "UV3310B", manufactured by Nippon Synthetic Chemical Industry Co., Ltd., bifunctional): 85 parts by weight Phenoxyethyl acrylate (product name "Viscoat #192", manufactured by Osaka Organic Chemical Industry Co., Ltd.): 15 parts by weight Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Irgacure (registered trademark) 184", manufactured by BASF Japan Ltd.): 5 parts by mass Methyl isobutyl ketone: 10 parts by weight
[0168] <Example 1> A polyimide substrate (product name "Neoprim", manufactured by Mitsubishi Gas Chemical Co., Inc.) measuring 200 mm long x 200 mm wide and 50 μm thick was prepared as the resin substrate, and the hard coat layer composition 1 was applied to the second surface, which was one of the surfaces of the polyimide substrate, using a bar coater to form a coating film. Note that the above Neoprim (registered trademark) is a commercially available polyimide film. Thereafter, the formed coating film was heated at 70°C for 1 minute to evaporate the solvent in the coating film, and ultraviolet light was irradiated in air using an ultraviolet irradiation device (light source H bulb manufactured by Fusion UV Systems Japan Co., Ltd.) until the accumulated light amount was 100 mJ / cm. 2 The coating film was semi-cured (half-cured) by irradiating it so that the hard coat layer composition 2 was applied to the surface of the semi-cured coating film of the hard coat layer composition 1 with a bar coater to form a coating film. The formed coating film was heated at 70°C for 1 minute to evaporate the solvent in the coating film, and ultraviolet rays were irradiated using an ultraviolet irradiator (manufactured by Fusion UV Systems Japan Co., Ltd., light source H bulb) under conditions of an oxygen concentration of 200 ppm or less with an accumulated light amount of 200 mJ / cm. 2 The coating film was completely cured (fully cured) by irradiating the coating film so that the coating film was completely cured (fully cured). As a result, a hard coat layer was formed on the polyimide substrate, consisting of a first hard coat layer having a thickness of 10 μm and a second hard coat layer having a thickness of 5 μm laminated on the first hard coat layer. Then, on the first surface opposite to the second surface of the polyimide substrate, two reinforced parts made of glass plates having a size of 200 mm length x 95 mm width and a thickness of 400 μm were arranged in a plane state via an adhesive layer (product name "8146-1", manufactured by 3M Japan Co., Ltd.) having a thickness of 25 μm so that the gap between the reinforced parts was 2.5 mm. Then, the resin layer composition 1 was applied from above the glass plate with a bar coater to form a coating film. Then, the formed coating film was heated at 70°C for 1 minute to evaporate the solvent in the coating film, and ultraviolet rays were irradiated in air with an ultraviolet ray irradiation device (manufactured by Fusion UV System Japan Co., Ltd., light source H bulb) with an integrated light amount of 1200 mJ / cm. 2 The coating was cured by irradiating the coating with light so as to form a resin layer made of a urethane resin having a thickness of 500 μm, thereby obtaining an optical film.
[0169] The thickness of the reinforced part was measured by photographing the cross section of the reinforced part using a scanning electron microscope (SEM), measuring the thickness of the reinforced part at 20 points on the image of the cross section, and taking the arithmetic average value of the thicknesses at the 20 points. The specific method of photographing the cross section was as follows. First, a block was prepared by embedding an optical film cut to 1 mm x 10 mm in embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm without holes was cut out from this block by a general slice preparation method. An ultramicrotome EM UC7 made by Leica Microsystems was used to prepare the slices. The remaining block from which the uniform slice without holes was cut out was used as the measurement sample. Then, a cross section photograph of the measurement sample was taken using a scanning electron microscope (SEM) (product name "S-4800", manufactured by Hitachi High-Technologies Corporation). When photographing the cross section using the S-4800, the cross section was observed with the detector set to "SE", the acceleration voltage set to "5 kV", and the emission current set to "10 μA". The magnification was adjusted appropriately from 100 to 100,000 times while adjusting the focus and observing whether the contrast and brightness could be distinguished from each other. Furthermore, the beam monitor aperture was set to "3", the objective lens aperture was set to "3", and the WD was set to "8 mm". The thicknesses of the polyimide substrate and the resin layer were also measured in the same manner as the thickness of the reinforced portion. In Examples 2 to 5 and Comparative Examples 1 to 5, the thicknesses of the polyimide substrate and the reinforced portion, and the film thickness of the resin layer were also measured in the same manner as in Example 1.
[0170] The thickness of the hard coat layer was measured by photographing the cross section of the hard coat layer using a scanning transmission electron microscope (STEM) (product name "S-4800", manufactured by Hitachi High-Technologies Corporation), measuring the thickness of the hard coat layer at 20 points on the image of the cross section, and taking the arithmetic average value of the film thickness at the 20 points. The cross-sectional photograph of the hard coat layer was taken as follows. First, a block was prepared by embedding an optical film cut to 1 mm x 10 mm in an embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm without holes was cut from this block by a general slice preparation method. An ultramicrotome EM UC7 made by Leica Microsystems was used to prepare the slice. The uniform slice without holes was used as the measurement sample. Then, a cross-sectional photograph of the measurement sample was taken using a scanning transmission electron microscope (STEM). When taking this cross-sectional photograph, STEM observation was performed with the detector set to "TE", the acceleration voltage set to "30 kV", and the emission current set to "10 μA". The magnification was adjusted appropriately from 5,000 to 200,000 times while adjusting the focus and observing whether the contrast and brightness of each layer could be distinguished. When taking the cross-sectional photograph, the beam monitor aperture was set to "3", the objective lens aperture was set to "3", and the WD was set to "8 mm". In Examples 2 to 5 and Comparative Examples 1 to 5, the film thickness of the hard coat layer was measured by the same method as in Example 1.
[0171] <Example 2> In Example 2, an optical film was obtained in the same manner as in Example 1, except that two reinforced parts made of acrylic resin plates measuring 200 mm in length x 95 mm in width and 400 μm in thickness were used instead of the two reinforced parts made of glass plates.
[0172] <Example 3> In Example 3, an optical film was obtained in the same manner as in Example 1, except that the composition 2 for resin layer was used instead of the composition 1 for resin layer.
[0173] <Example 4> In Example 4, an optical film was obtained in the same manner as in Example 1, except that two reinforced parts made of transparent polyvinyl sheets measuring 200 mm in length x 95 mm in width and 400 μm in thickness were used instead of the two reinforced parts made of glass plates.
[0174] <Example 5> In Example 5, an optical film was obtained in the same manner as in Example 1, except that two reinforced portions each consisting of a glass plate measuring 200 mm in length × 95 mm in width and 200 μm in thickness were used instead of the two reinforced portions each consisting of a glass plate measuring 200 mm in length × 95 mm in width and 400 μm in thickness.
[0175] <Comparative Example 1> A polyimide substrate (product name "Neoprim", manufactured by Mitsubishi Gas Chemical Company, Inc.) measuring 200 mm long x 200 mm wide and 50 μm thick was prepared as the resin substrate, and the hard coat layer composition 1 was applied to the first surface, which was one surface of the polyimide substrate, using a bar coater to form a coating film. The formed coating film was then heated at 70°C for 1 minute to evaporate the solvent in the coating film, and ultraviolet light was irradiated in air using an ultraviolet irradiation device (light source H bulb, manufactured by Fusion UV Systems Japan Co., Ltd.) until the accumulated light amount was 100 mJ / cm. 2 The coating film was semi-cured (half-cured) by irradiating it so that the hard coat layer composition 2 was applied to the surface of the semi-cured coating film of the hard coat layer composition 1 with a bar coater to form a coating film. The formed coating film was heated at 70°C for 1 minute to evaporate the solvent in the coating film, and ultraviolet rays were irradiated using an ultraviolet irradiator (manufactured by Fusion UV Systems Japan Co., Ltd., light source H bulb) under conditions of an oxygen concentration of 200 ppm or less with an accumulated light amount of 200 mJ / cm. 2The coating film was completely cured (fully cured) by irradiating the coating film so that the coating film was completely cured (fully cured). As a result, a hard coat layer was formed on the polyimide substrate, which consisted of a first hard coat layer having a thickness of 10 μm and a second hard coat layer having a thickness of 5 μm laminated on the first hard coat layer. Thereafter, the resin layer composition 1 was applied to the second surface of the polyimide substrate opposite to the first surface with a bar coater to form a coating film. The formed coating film was then heated at 70° C. for 1 minute to evaporate the solvent in the coating film, and ultraviolet rays were irradiated in air using an ultraviolet irradiator (manufactured by Fusion UV Systems Japan Co., Ltd., light source H bulb) until the accumulated light amount was 1200 mJ / cm 2 . 2 The coating was cured by irradiating the coating with light so as to form a resin layer made of a urethane resin having a thickness of 500 μm, thereby obtaining an optical film.
[0176] <Comparative Example 2> In Comparative Example 2, an optical film was obtained in the same manner as in Example 1, except that two reinforced parts made of triacetyl cellulose film (product name "TD40UL", manufactured by Fujifilm Corporation) measuring 200 mm in length, 95 mm in width, and 40 μm in thickness were used instead of the two reinforced parts made of glass plates.
[0177] <Comparative Example 3> In Comparative Example 3, an optical film was obtained in the same manner as in Example 1, except that two reinforced parts made of polyethylene terephthalate films (product name "A4300", manufactured by Toyobo Co., Ltd.) measuring 200 mm in length x 200 mm in width and 100 μm in thickness were used instead of the two reinforced parts made of glass plates.
[0178] <Comparative Example 4> In Comparative Example 4, an optical film was obtained in the same manner as in Example 1, except that instead of the two reinforced parts made of glass plates, one reinforced part made of a glass plate measuring 200 mm in length x 200 mm in width and 400 μm in thickness was used.
[0179] <Comparative Example 5> In Comparative Example 5, an optical film was obtained in the same manner as in Example 1, except that instead of the two reinforced parts made of glass plates, two reinforced parts made of a sheet consisting of two transparent adhesive layer sheets (product name "8146", manufactured by 3M Japan Co., Ltd.) measuring 200 mm in length x 200 mm in width and 100 μm in thickness, stacked together, were used.
[0180] <Martens hardness measurement> The Martens hardness of the two reinforced parts of the optical films according to Examples 1 to 5 and Comparative Examples 2 to 5 was measured. The Martens hardness of the reinforced parts was measured using a TI950 TriboIndenter manufactured by Bruker. Specifically, first, a block was prepared by embedding an optical film cut to 1 mm×10 mm in an embedding resin, and a uniform slice having a thickness of 70 nm to 100 nm without holes was cut out from this block by a general slice preparation method. An ultramicrotome EM UC7 manufactured by Leica Microsystems was used to prepare the slices. The remaining block from which the uniform slice without holes was cut out was used as a measurement sample. Next, a Berkovich indenter (triangular pyramid, TI-0039 manufactured by Bruker) was used as an indenter to indent 500 nm from the center of the cross section of the reinforced part under the following measurement conditions in the cross section obtained by cutting out the slice in such a measurement sample. Here, the Berkovich indenter was pressed into the reinforced portion at a distance of 500 nm or more from each of both ends toward the center of the reinforced portion to avoid the influence of the side edges of the reinforced portion. After that, the specimen was held for a certain period of time to relax the residual stress, and then the load was removed. The maximum load after relaxation was measured, and the maximum load P max (μN) and the area A of the 500 nm deep indentation (nm 2 ) and P maxMartens hardness was calculated by (AB) / B×100. Martens hardness was the arithmetic average value of the values measured at 10 points. In Table 1 shown later, one of the reinforced parts of the two sheets was designated as the first reinforced part, and the other reinforced part was designated as the second reinforced part. If the measured values included any value that deviated from the arithmetic average value by ±20% or more, that measured value was excluded and remeasured. Whether or not any measured values included any value that deviated from the arithmetic average value by ±20% or more was determined by whether the value (%) calculated by (AB) / B×100, where A is the measured value and B is the arithmetic average value, was ±20% or more. (Measurement conditions) ·Loading speed: 10nm / sec ·Holding time: 5 seconds ·Loading and unloading speed: 10nm / sec ·Measurement temperature: 25℃ Relative humidity: 50%
[0181] <Continuous folding test> The optical films according to the examples and comparative examples were cut into pieces measuring 30 mm × 100 mm. The optical films thus cut were attached to a durability tester (product name: "U-shaped stretch tester DLDMLH-FS", manufactured by Yuasa System Devices Co., Ltd., compliant with IEC 62715-6-1) with the short sides (30 mm) of the optical films fixed at the fixing parts, and the optical films were attached so that the minimum distance φ between the two opposing sides was 30 mm, as shown in FIG. 3(C). A continuous folding test was then performed under the following conditions in which the surface of the hard coat layer side of the optical film was folded 180° (a test in which the hard coat layer was folded so that the resin layer was on the outside) 100,000 times, and the occurrence of cracks or breaks in the bent parts was examined. In addition, new optical films according to the examples and comparative examples were attached to the durability tester in the same manner as above, and a continuous folding test (a test in which the hard coat layer was folded on the outside and the polyimide substrate was folded on the inside) was performed 100,000 times under the following conditions, in which the surface of the optical film on the polyimide substrate side was folded 180°, and the occurrence of cracks or breaks in the bent portion was examined. The results of the continuous folding test were evaluated according to the following criteria. The continuous folding test was performed in an environment with a temperature of 23°C and a relative humidity of 50%. The evaluation criteria were as follows. Note that the optical films according to Examples 1 to 5 and Comparative Examples 2, 3, and 5 were adjusted so that they were folded in the bent region, which is the gap between the reinforced portions. (Folding conditions) Reciprocating speed: 90 rpm (revolutions per minute) Test stroke: 70mm Bending angle: 180° (Evaluation Criteria) ◯: No cracks or breaks were observed in the bent portion in any of the continuous folding tests. ×: In any of the continuous folding tests, cracks or breaks occurred at the bent portion.
[0182] <Impact resistance test> The optical films cut to a size of 50 mm x 100 mm according to the examples and comparative examples were placed directly on the surface of a 0.7 mm thick soda glass so that the soda glass side was the resin layer side, and an impact resistance test A was performed three times for each case in which an iron ball weighing 100 g and having a diameter of 30 mm was dropped onto the surface of the hard coat layer of the optical film from a position 30 cm high. In addition, the optical films cut to a size of 50 mm x 100 mm according to the examples and comparative examples were placed on a 0.7 mm thick soda glass so that the soda glass side was the polyimide substrate side or the resin layer side via an adhesive sheet having a thickness of 200 μm (product name: "Highly transparent double-sided tape 8146-2", manufactured by 3M Japan Co., Ltd.), and an impact resistance test B was performed three times for each case in which an iron ball weighing 100 g and having a diameter of 30 mm was dropped onto the surface of the hard coat layer of the optical film from a position 30 cm high. In the impact resistance tests A and B, the position at which the iron ball was dropped was changed each time. However, in the optical films according to Examples 1 to 5 and Comparative Examples 2 to 5, the iron ball was dropped into the area corresponding to the reinforced portion. After the impact resistance test A, the optical films were visually evaluated for the presence of dents on the surface of the hard coat layer, and for the presence of cracks in the soda glass. After the impact resistance test B, the optical films were visually evaluated for the presence of dents on the surface of the hard coat layer. The evaluation results were as follows. (Evaluation of dents on the surface of the hard coat layer) ⊚: No depressions were found on the surface of the hard coat layer both when the hard coat layer was observed from the front and from an oblique direction. ◯: When the hard coat layer was observed either from the front or from an oblique direction, depressions were found on the surface of the hard coat layer, but were not of a level that would cause any problems in practical use. Δ: When the hard coat layer was observed from the front, no dents were observed on the surface of the hard coat layer, but when observed obliquely, dents were confirmed on the surface of the hard coat layer. ×: When the hard coat layer was observed from the front and from an oblique angle, obvious depressions were observed on the surface of the hard coat layer. (Soda glass cracking evaluation) ◎: The soda glass did not break. ○: The soda glass was scratched but did not break. △: The soda glass cracked once or twice. ×: The soda glass cracked all three times.
[0183] <Pencil hardness> The pencil hardness of the surface (surface of the hard coat layer) of the optical film according to the examples and comparative examples was measured based on JIS K5600-5-4:1999. The pencil hardness test was performed by placing an optical film cut to a size of 50 mm x 100 mm with the hard coat layer facing up on a glass plate, fixing it with Cellotape (registered trademark) manufactured by Nichiban Co., Ltd. so as not to bend or wrinkle, and moving a pencil (product name "Uni", manufactured by Mitsubishi Pencil Co., Ltd.) at a moving speed of 1 mm / sec while applying a load of 750 g to the pencil (product name "Uni", manufactured by Mitsubishi Pencil Co., Ltd.) against the surface of the optical film. The pencil hardness is the highest hardness that does not scratch the surface of the optical film in the pencil hardness test. In addition, when measuring the pencil hardness, multiple pencils with different hardnesses are used, and the pencil hardness test is performed five times for each pencil. If no scratches are visually observed on the surface of the optical film when the surface of the optical film is observed through a fluorescent lamp four or more times out of the five times, it is determined that the pencil of that hardness did not scratch the surface of the optical film. In addition, the pencil hardness test for optical films having reinforced parts was performed in the area where the reinforced parts exist.
[0184] <G´、G´´、tanδ> The shear storage modulus G', shear loss modulus G'', and shear loss tangent tanδ of the resin layer of the optical film according to the embodiment were measured. Specifically, first, two optical films cut to a size of 10 mm x 5 mm according to the embodiment were prepared and attached to a solid shearing jig, which is an option of a dynamic viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.). Specifically, the solid shearing jig includes a metal solid shearing plate having a thickness of 1 mm and two L-shaped metal fittings arranged on both sides of the solid shearing plate, and one optical film is sandwiched between the solid shearing plate and one of the L-shaped metal fittings, and the other optical film is sandwiched between the solid shearing plate and the other L-shaped metal fitting. In this case, the optical film is sandwiched so that the resin layer is on the solid shearing plate side and the hard coat layer is on the L-shaped metal fitting side. A tensile test chuck consisting of an upper chuck and a lower chuck was attached to a dynamic viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.), and then a solid shear jig was attached between the upper chuck and the lower chuck with a chuck distance of 20 mm. The temperature was set to 25°C and increased at a rate of 2°C / min. In this state, while the solid shear plate was fixed, a vertical vibration with a distortion of 1% and a frequency range of 500Hz to 1000Hz was applied to the two L-shaped metal fittings, and dynamic viscoelasticity of the solid was measured at 25°C, and the shear storage modulus G', shear loss modulus G'', and shear loss tangent tanδ of the resin layer were measured. Here, the shear storage modulus G', shear loss modulus G'', and shear loss tangent tan δ of the resin layer in the frequency range of 500 Hz or more and 1000 Hz or less were measured by applying longitudinal vibrations of frequencies of 500 Hz, 750 Hz, and 950 Hz to the L-shaped metal fitting, respectively, and measuring the shear storage modulus G', shear loss modulus G'', and shear loss tangent tan δ of the resin layer at each frequency, and calculating the arithmetic mean values of these shear storage modulus G', shear loss modulus G'', and shear loss tangent tan δ. Furthermore, this measurement was repeated three times, and the three arithmetic mean values obtained were further arithmetically averaged to obtain the value.
[0185] <Refractive index difference> The refractive indexes of the two reinforced parts and the resin layer of the optical film according to the embodiment were measured, and the absolute value of the refractive index difference between the resin layer and one of the reinforced parts and the absolute value of the refractive index difference between the resin layer and the other reinforced part were obtained. The refractive index of the reinforced part was measured by cutting out 10 pieces of the reinforced part by cutting out, measuring the refractive index of the reinforced part by the Becke method for each of the 10 pieces, and taking the average value of the 10 measured refractive indexes of the reinforced part as the refractive index of the reinforced part. The refractive index of the resin layer was also measured in the same manner as the refractive index of the reinforced part. In Table 2 shown later, one of the two reinforced parts is referred to as the first reinforced part, and the other reinforced part is referred to as the second reinforced part.
[0186] <Appearance evaluation> When the optical films according to the examples were viewed in plan, they were visually evaluated to see whether the shape of the reinforced portion was visible or not. The evaluation criteria were as follows. ○: The shape of the reinforced part was not confirmed. △: The shape of the reinforced portion was slightly observed, but it was at a level that did not cause any problems in practical use. ×: The shape of the reinforced portion was clearly confirmed.
[0187] The results are shown in Tables 1 and 2 below. [Table 1]
[0188] [Table 2]
[0189] The results are described below. The optical film according to Comparative Example 1 does not have a reinforced portion, and the optical films according to Comparative Examples 2 and 3 have a thickness of less than 150 μm for the first reinforced portion and the second reinforced portion. Therefore, although the optical film has good folding properties, it cannot absorb impacts, and in the impact resistance test A, dents were confirmed on the surface of the hard coat layer, and cracks were sometimes generated in the soda glass. In the impact resistance test B, the surface of the hard coat layer was greatly dented due to following the plastic deformation of the adhesive sheet. In the optical film according to Comparative Example 4, one glass plate was used, so the folding properties were poor. In the optical film according to Comparative Example 5, the Martens hardness of the first reinforced portion and the second reinforced portion were each less than 30 MPa, so although the optical film has good folding properties, it cannot absorb impacts, and in the impact resistance test A, the surface of the hard coat layer was greatly dented, and cracks were generated in the soda glass. In the impact resistance test B, the surface of the hard coat layer was greatly dented due to following the plastic deformation of the adhesive sheet.
[0190] In contrast, in the optical films of Examples 1 to 5, the first reinforced portion and the second reinforced portion each had a thickness of 150 μm or more and a Martens hardness of 30 MPa or more, and therefore had excellent impact resistance while maintaining good foldability.
[0191] The Martens hardness of the polyimide substrate and the hard coat layer of the optical films according to the examples and comparative examples was measured, and the Martens hardness of the polyimide substrate was 250 MPa, the Martens hardness of the first hard coat layer was 835 MPa, and the Martens hardness of the second hard coat layer was 470 MPa. The Martens hardness of the polyimide substrate and the hard coat layer was measured under the same conditions as those for the Martens hardness of the reinforced portion. [Explanation of symbols]
[0192] 10...Optical film 10A…Surface 10B…Back side 11...Resin substrate 11A...First side 11B...Second side 12…Reinforcement part 12A…Gap 13...Resin layer 14...Hard coat layer 15…First hard coat layer 16…Second hard coat layer 40...Image display device 43...Display panel 46…adhesive layer
Claims
1. A foldable optical film, comprising: A resin substrate; A plurality of reinforcing portions arranged in a plane on a first surface side of the resin base material; A resin layer provided on the first surface side of the resin substrate; a hard coat layer in contact with a second surface of the resin substrate opposite to the first surface, the hard coat layer having a Martens hardness higher than the Martens hardness of the resin substrate and a thickness of 1 μm or more and 20 μm or less; The resin layer covers each of the reinforcement parts and fills the gaps between the reinforcement parts, The thickness of each of the reinforced parts is 150 μm or more, The Martens hardness of the reinforced portions is 30 MPa or more and 1000 MPa or less, The resin layer has a shear storage modulus G' of 1 MPa or more and 1500 MPa or less in a frequency range of 500 Hz or more and 1000 Hz or less at 25°C, and a shear loss modulus G'' of 0.1 MPa or more and 200 MPa or less in a frequency range of 500 Hz or more and 1000 Hz or less at 25°C.
2. The optical film according to claim 1 , wherein an absolute value of a refractive index difference between the resin layer and the reinforcing portion is 0.02 or less.
3. 3. The optical film according to claim 1, which does not crack or break when a test in which the optical film is folded 180 degrees so that the distance between opposing sides of the optical film is 30 mm is repeated 100,000 times.
4. 4. The optical film according to claim 1, wherein the resin substrate is a substrate made of a polyimide resin, a polyamide resin, or a mixture thereof.
5. A foldable image display device, A display panel; The optical film according to claim 1 , which is disposed on a viewer side relative to the display panel; An image display device comprising:
6. The image display device according to claim 5 , wherein the display panel is an organic light-emitting diode panel.
Citation Information
Patent Citations
Window film for display device, and display device including the same
JP2016125063A
Optical film and image display device
JP2018159913A
Glass article, and display unit
JP2018197183A
Foldable transparent composite cover window, manufacturing method of the same, and foldable display device containing the same
US20150004334A1
Optical laminated body, and image display device
WO2017200042A1