Adhesive Film
The adhesive film with a polyethylene resin slipping layer and controlled elastic modulus difference addresses cuttability issues, enabling efficient manual cutting and maintaining adhesiveness.
Patent Information
- Application Number
- JP2023510996
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-29
- Filing Date
- 2022-03-18
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-03-18
AI Technical Summary
Existing adhesive cleaners face challenges with insufficient cuttability, requiring machine-assisted cutting and separate cuts, which increases costs and complexity.
An adhesive film with a specific design comprising a polyethylene resin-containing slipping layer of 8 μm or less, a thermoplastic resin base layer, and a controlled elastic modulus difference between machine and transverse directions, enhancing cuttability and adhesiveness.
The adhesive film achieves excellent cuttability, allowing for straight-line cutting with human power, maintaining adhesiveness, and reducing the need for machine-assisted cutting processes.
Smart Images

Figure 0007572543000003 
Figure 0007572543000001 
Figure 0007572543000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive film. [Background technology]
[0002] 2. Description of the Related Art Adhesive cleaners using adhesive films are known as a means for removing hair, dust, dirt, and the like that has adhered to objects to be cleaned, such as clothing, furniture, interior materials, and daily necessities. Adhesive cleaners are also used to remove fine debris from the surfaces of IC chips, which are generated during processing such as cutting and polishing in the manufacturing process of IC chips for electronic devices.
[0003] Adhesive cleaners usually have a structure in which an adhesive film having a substrate and an adhesive layer formed on one side of the substrate is wound so that the adhesive layer faces outward. The adhesive cleaner can be pressed against an object and rotated to transfer dust and the like to the adhesive layer, thereby cleaning the object. When the surface of the adhesive layer becomes filled with dust and the like, the adhesive film can be peeled off and cut to expose a new adhesive surface, which can be reused.
[0004] Here, the other side of the substrate and the adhesive layer must be in close contact without peeling off during storage and use of the cleaner, and when the adhesive film is cut off after use of the cleaner, it must be possible to peel them off without impairing the adhesiveness of the adhesive layer. In order to facilitate peeling of the other side of the substrate and the adhesive layer, attempts have been made to provide a layer containing a release agent (lubricant) such as silicone or wax on the other side of the substrate. However, there is a risk that the release agent is transferred to the adhesive layer side, reducing the adhesiveness or contaminating the IC chip, and therefore an adhesive cleaner that does not use a release agent has been demanded.
[0005] Patent Document 1 describes an adhesive cleaner that does not use a release agent by using a two-component urethane adhesive as an adhesive component and a polyethylene film as a material that forms the release surface. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2002-307554 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the adhesive cleaner described in Patent Document 1, the adhesive film has insufficient cutting ability, making it difficult to cut in a straight line by hand, and this requires a separate mechanical cutting process or the adhesive film to have separate cuts for cutting, which may lead to increased costs.
[0008] An object of the present invention is to provide an adhesive film that has excellent adhesive properties and peelability as well as excellent cuttability. [Means for solving the problem]
[0009] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, it was found that the above-mentioned problems can be solved by using a polyethylene-based resin-containing film having a specific thickness as a slipping layer and setting the orientation of the adhesive film within a specific range. That is, the present invention relates to the following pressure-sensitive adhesive film, etc. [1] An adhesive film having an adhesive layer, a base layer, and a slipping layer in this order, The adhesive layer contains an adhesive resin having an elastic modulus of 100 MPa or less, The substrate layer is a thermoplastic resin film, The slipping layer contains a polyethylene resin and has a thickness of 8 μm or less, The adhesive film has a modulus of elasticity E MD and the normal elastic modulus E TD The absolute value of the difference |ΔE| between the two is 500 MPa or more. [2] The adhesive film described in [1], wherein the slipping layer has a surface roughness of 0.05 μm or more and 5 μm or less. [3] The adhesive film according to [1] or [2], wherein the base layer contains a polypropylene-based resin and a filler. [4] The pressure-sensitive adhesive film according to any one of [1] to [3], wherein the base layer is porous. [5] A coating layer is further provided between the adhesive layer and the base layer, The pressure-sensitive adhesive film according to any one of [1] to [4], wherein the coating layer contains one or more resins selected from a urethane-based resin, an olefin-based copolymer, a styrene-based resin, and an ethyleneimine-based resin. [6] The pressure-sensitive adhesive film according to any one of [1] to [5], wherein the slipping layer is a uniaxially stretched resin film. [7] An adhesive film laminate, in which the adhesive film according to any one of [1] to [6] is laminated so that the adhesive layer and the slipping layer are in contact with each other. [8] A laminated film having a base layer and a slipping layer in this order, The substrate layer is a thermoplastic resin film, The slipping layer contains a polyethylene resin and has a thickness of 8 μm or less, The laminated film has a modulus of elasticity E MD and the normal elastic modulus E TD The absolute value of the difference |ΔE| between the two is 500 MPa or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide an adhesive film that has excellent adhesive properties and peeling properties as well as excellent cuttability. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an adhesive film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The pressure-sensitive adhesive film of the present invention will be described in detail below. The following is an example (representative example) of the present invention, and the present invention is not limited thereto.
[0013] <Adhesive film> An example of the adhesive film of the present invention is shown in Fig. 1. As shown in Fig. 1, the adhesive film 10 has an adhesive layer 3, a base layer 1, and a slipping layer 2 in this order. The adhesive layer 3 contains an adhesive resin having an elastic modulus of 100 MPa or less. This configuration can impart adhesiveness to the film of the present invention. The substrate layer 1 is a thermoplastic resin film. The slipping layer 2 contains a polyethylene resin and has a thickness of 8 μm or less. By containing a polyethylene resin, it is possible to impart easy peeling to the adhesive film. In addition, since the slipping layer is thin, it is possible to maintain good cuttability of the adhesive film without deterioration.
[0014] The adhesive film 10 has a modulus of elasticity E MD and the normal elastic modulus E TD The absolute value of the difference |ΔE| between the tension and the tension is 500 MPa or more. The adhesive film has a specific orientation, and as a result, the cuttability of the adhesive film is improved, resulting in an adhesive film with excellent linear cuttability that can be torn and cut linearly even with the force of a human hand.
[0015] The flow direction is the direction in which the resin flows (machine direction). r The vertical direction means the direction perpendicular to the flow direction. rIt means the storage modulus measured by a solid viscoelasticity measuring device (TA Instruments Japan: RSA-III) after cutting the adhesive film into a test piece of 30 mm length x 15 mm width. The measurement conditions are 20 mm between the chucks, 10 Hz measurement frequency, 0.1% strain, 10 °C heating rate / min, and tensile mode, at 23 °C. From the viewpoint of linear cuttability, the elastic modulus difference |ΔE| is preferably larger. The linear cuttability is improved from 500 MPa or more, preferably 1000 MPa or more, more preferably 2000 MPa or more. On the other hand, from the viewpoint of the stretching limit of the resin, it is usually 4000 MPa or less.
[0016] The direction in which the modulus of elasticity is large may be either the machine direction or the perpendicular direction. However, the direction of winding during manufacturing can be made the same as the direction of winding for the adhesive film product, and an additional process can be eliminated. Therefore, the modulus of elasticity in the perpendicular direction E TD is the elastic modulus in the flow direction E MD It is preferable that it is greater than . That is, it is preferable that the following relational expression is satisfied. E TD -E MD ≧500(MPa)
[0017] The adhesive film preferably has a modulus of elasticity in the cutting direction (tear direction) of 500 MPa or more, more preferably 1000 MPa or more, and particularly preferably 2000 MPa or more. The difference in modulus of elasticity |ΔE| is 500 MPa or more, and the modulus of elasticity in the cutting direction is high, so that the adhesive film can be cut in a straight line more easily. The cutting direction may be either the machine direction or the vertical direction, but is preferably the vertical direction from the viewpoint of making the winding direction during production the same as the winding direction in the product.
[0018] In addition, since the specific elastic modulus difference |ΔE| is a property that is mainly imparted by the orientation of the base material layer, in order to obtain an adhesive film in which the elastic modulus difference |ΔE| is a specific value or more, for example, it is possible to provide a base material layer having an orientation, as described below.
[0019] In addition, the laminated film of the present invention having the base layer and the slipping layer in this order also has a modulus of elasticity E in the machine direction, similar to the pressure-sensitive adhesive film laminate. MD and the normal elastic modulus E TD The absolute value of the difference |ΔE| is 500 MPa or more.
[0020] Each layer will be described below.
[0021] <Adhesive layer> The adhesive layer contains an adhesive resin and has the function of imparting adhesiveness to the film. Here, the elastic modulus of the adhesive resin is 100 MPa or less, preferably 80 MPa or less, more preferably 50 MPa or less. When the elastic modulus is within the above range, the adhesiveness tends to be increased. In addition, the elastic modulus is preferably 0.1 MPa or more, more preferably 0.5 MPa or more, from the viewpoint of maintaining the strength of the adhesive layer and not having excessive adhesiveness. The elastic modulus of the adhesive resin means the indentation elastic modulus in the thickness direction of the adhesive layer surface measured by a nanoindenter.
[0022] As described above, the adhesive resin may be any resin that is relatively soft and has an elastic modulus of 100 MPa or less. Among them, for example, acrylic resin, elastomer resin, ethylene-vinyl acetate copolymer (EVA), etc. are mentioned, preferably acrylic resin or elastomer resin, more preferably acrylic resin. These may be used alone or in combination of two or more.
[0023] Examples of the acrylic resin include an acrylic acid ester copolymer, a methacrylic acid ester copolymer, and an acrylic acid amide-acrylic acid ester copolymer.
[0024] The elastomer resin is not particularly limited as long as it has thermoplasticity and rubber-like elasticity at room temperature, and various known resins can be used. Specific examples include olefin thermoplastic elastomers having a hard segment component made of a polyolefin such as polyethylene or polypropylene, and a soft segment component such as another polyolefin, an α-olefin such as 1-butene, or an ethylene-propylene rubber.
[0025] The thickness of the adhesive layer is preferably 1 μm or more, more preferably 3 μm or more, from the viewpoints of formability and maintaining adhesive strength, and is preferably 30 μm or less, more preferably 20 μm or less, from the viewpoints of cost control, maintaining linear cutability and maintaining peelability.
[0026] <Base material layer> The substrate layer is a thermoplastic resin film, and is provided as a support for the pressure-sensitive adhesive film.
[0027] The base layer preferably has orientation from the viewpoint that the adhesive film easily satisfies the above-mentioned specific elastic modulus difference |ΔE| and has linear cutability. Specifically, the base layer also preferably has an elastic modulus difference |ΔE| of 500 MPa or more, more preferably 1000 MPa or more, and particularly preferably 2000 MPa or more. On the other hand, from the viewpoint of the stretching limit of the resin, it is usually 4000 MPa or less.
[0028] The elastic modulus of the base layer in the cutting direction (tear direction) is preferably 500 MPa or more, more preferably 1000 MPa or more, and particularly preferably 2000 MPa or more. The elastic modulus difference |ΔE| is 500 MPa or more, and the elastic modulus in the cutting direction is high, so that the linear cut property of the base layer is further improved. The cutting direction may be either the machine direction or the vertical direction, but is preferably the vertical direction from the viewpoint of making the winding direction during production the same as the winding direction in the product.
[0029] In order to make the elastic modulus difference |ΔE| of the base material layer 500 MPa or more, for example, the base material layer should be a stretched resin film stretched in at least one direction. The base material layer may be stretched in one direction or in two directions, but a biaxially stretched resin film is particularly preferred from the viewpoints of improving the strength, stiffness, and porosity of the base material layer.
[0030] The thermoplastic resin constituting the base layer is not particularly limited, but for example, polyolefin resins are preferred from the viewpoints of moldability and cost.
[0031] <Polyolefin resin> Specific examples of polyolefin resins include polypropylene resins, polyethylene resins, polymethyl-1-pentene, etc., with polypropylene resins and polyethylene resins being preferred, and polypropylene resins being more preferred.
[0032] The polypropylene resin is not particularly limited as long as it is a resin in which propylene is used as the main monomer. For example, an isotactic polymer or a syndiotactic polymer obtained by homopolymerizing propylene can be mentioned. In addition, a propylene-α-olefin copolymer, which is a copolymer of propylene as the main component and an α-olefin such as ethylene or 1-butene, can also be used. The copolymer may be a binary or ternary or higher multi-component system of monomer components, and may be a random copolymer or a block copolymer. Among them, a propylene homopolymer is preferable. A propylene homopolymer and a propylene copolymer may be used in combination.
[0033] As the polyethylene resin, for example, a polyethylene having a density of 0.940 g / cm 3 ~0.965g / cm 3 High density polyethylene, density is 0.920g / cm 3 ~0.935g / cm 3 of medium density polyethylene, with a density of 0.900 g / cm 3 More than 0.920g / cm 3Examples of such polyethylene include linear low density polyethylene having a molecular weight of less than 1000, copolymers mainly composed of ethylene and copolymerized with α-olefins such as propylene, butene, and hexene, ethylene-cyclic olefin copolymers, and maleic acid modified polyethylene.
[0034] Furthermore, as the polyolefin resin, a graft-modified product can also be used as necessary from the viewpoint of improving the adhesiveness or moldability of the resin film. A known method can be used for the graft modification. Specifically, a graft modification using an unsaturated carboxylic acid or a derivative thereof as a graft monomer can be mentioned. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, and citraconic acid. Examples of the derivatives of the unsaturated carboxylic acid include anhydrides, esters, amides, imides, and metal salts of the unsaturated carboxylic acids.
[0035] Specific examples of the graft monomer include maleic anhydride, itaconic anhydride, citraconic anhydride, methyl (meth)acrylate, ethyl (meth)acrylate, monoethyl maleate, and monomethyl fumarate.
[0036] The graft monomer can be used in an amount of usually 0.005% by mass to 10% by mass, and preferably 0.01% by mass to 5% by mass, based on the polyolefin resin.
[0037] The polyolefin resin used in the base layer may be one of the above alone or two or more of them in combination. From the viewpoint of moldability, mechanical strength, cost reduction, etc., the base layer is preferably a resin film of a polypropylene resin or a polyethylene resin, and more preferably a polypropylene resin. Among them, a propylene homopolymer is easy to handle as the main raw material of the base layer and is therefore preferred.
[0038] From the viewpoint of film formability, the polypropylene-based resin film can be used in combination with a resin having a melting point equal to or lower than that of the propylene homopolymer. Such a resin can be a polyethylene-based resin, specifically, a high-density or low-density polyethylene. The blending amount of the polyethylene-based resin can be, for example, 2% by mass to 25% by mass.
[0039] <Filler> The substrate layer may contain a filler. By containing a filler, pores are easily formed inside the substrate layer, and a porous substrate layer is obtained. This makes it easy to adjust the whiteness or opacity of the film, and also makes it possible to reduce the weight of the substrate layer, and thus the adhesive film. Examples of fillers that can be used include inorganic fillers and organic fillers.
[0040] <<Inorganic filler>> Examples of inorganic fillers that can be used include inorganic particles such as calcium carbonate, calcined clay, silica, diatomaceous earth, white clay, talc, titanium oxide, barium sulfate, barium titanate, alumina, zeolite, mica, sericite, bentonite, sepiolite, vermiculite, dolomite, wollastonite, and glass fiber. The average particle size of the inorganic filler measured with a particle size distribution meter using laser diffraction is usually 0.01 μm to 15 μm, and preferably 0.1 μm to 5 μm.
[0041] <<Organic filler>> As the organic filler, it is preferable to select a resin different from the polyolefin resin that is the main component of the base layer. As such an organic filler, for example, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, nylon-6, nylon-6,6, cyclic polyolefin, polystyrene, polymethacrylate, or other polymers, which have a melting point (e.g., 170 to 300°C) higher than the melting point of the polyolefin resin or a high glass transition temperature (e.g., 170 to 280°C) and are incompatible with the polyolefin resin, can be used.
[0042] As the filler, the above-mentioned inorganic fillers and organic fillers can be used alone or in combination. The content of the filler in the base layer (the total amount when an inorganic filler and an organic filler are used in combination) is preferably 10% by mass or more, more preferably 15% by mass or more, from the viewpoint of improving whiteness and making dirt on the cleaning roll easier to see, while it is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 35% by mass or less, from the viewpoint of suppressing paper dust.
[0043] <Other ingredients> The base layer may further contain, as necessary, a heat stabilizer (antioxidant), a light stabilizer, a dispersant, a lubricant, a nucleating agent, or the like, within a range that does not impair the effects of the present invention. As the heat stabilizer, for example, a sterically hindered phenol-based antioxidant, a phosphorus-based antioxidant, or an amine-based antioxidant can be used usually within the range of 0.001% by mass to 1% by mass. As the light stabilizer, for example, a sterically hindered amine light stabilizer, a benzotriazole light stabilizer, or a benzophenone light stabilizer can be used usually within the range of 0.001% by mass to 1% by mass. Examples of dispersants or lubricants include silane coupling agents, higher fatty acids such as oleic acid and stearic acid, metal soaps, polyacrylic acid, polymethacrylic acid, and salts thereof, etc. These can be used in an amount of usually 0.01% by mass to 4% by mass, for example, to disperse fillers.
[0044] <Structure of base layer> The substrate layer may be a single layer structure or a multi-layer structure of two or more layers. By forming a multi-layer structure, it is possible to impart various functions such as mechanical properties, writability, abrasion resistance, and secondary processing suitability to the substrate layer.
[0045] The thickness of the base layer is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more from the viewpoints of strength and stiffness, while it is preferably 500 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less from the viewpoints of linear cutting ability and the number of turns when wound into a roll.
[0046] <Stretched film> The base layer is preferably a uniaxially stretched film from the viewpoint of the linear cutability, since the elastic modulus difference |ΔE| is likely to occur. On the other hand, when the base layer contains a filler, a biaxially stretched film is preferable from the viewpoint of weight reduction and whitening due to porosity as the number of stretching axes increases. However, when biaxial stretching is performed, the elastic modulus difference |ΔE| caused by uniaxial stretching is reduced, and linear cutability is likely to be impaired. Therefore, when biaxial stretching is performed, it is preferable to perform it to the extent that linear cutability is not impaired. When the base layer has a multi-layer structure, the number of stretching axes of each layer may be the same or different. By combining layers with different numbers of stretching axes, it is possible to design a base layer that has both the advantages of uniaxial stretching and biaxial stretching. The number of stretching axes of each layer can be, for example, uniaxial / uniaxial, uniaxial / biaxial, biaxial / uniaxial, uniaxial / uniaxial / biaxial, uniaxial / biaxial / uniaxial, biaxial / uniaxial / uniaxial, uniaxial / biaxial / biaxial, biaxial / biaxial / uniaxial, or biaxial / biaxial / biaxial.
[0047] <Porosity> From the viewpoint of weight reduction or improvement of whiteness, the porosity of the base layer is preferably more than 0%, and is preferably 50% or less, more preferably 40% or less. The porosity can be determined from the ratio of the area occupied by pores in a certain region of the cross section of the film observed with an electron microscope.
[0048] <Smooth layer> The slipping layer is formed on the other surface of the substrate. The slipping layer is required to adhere closely to the adhesive layer when the adhesive film is laminated, and to be peelable without impairing the adhesiveness of the adhesive layer when the adhesive film is peeled off, i.e., to have both peel resistance and ease of peeling.
[0049] In order to achieve both of these properties, the slipping layer contains a polyethylene resin. By including a polyethylene resin in the slipping layer, the slipping property is improved and the amount of lubricant (release agent) can be reduced, so that the adhesive layer can be easily peeled off without losing its adhesiveness. This makes it possible to obtain a slipping layer with excellent peelability even when the amount of lubricant is reduced. Moreover, by reducing the thickness to 8 μm or less, the strength of the slipping layer is reduced, and there is no risk of impairing the cutting ability of the base layer, which is preferable.
[0050] Examples of the polyethylene resin include the polyethylene resins in the substrate layer described above. Among them, low-density polyethylene is preferred.
[0051] In addition, as the polyethylene resin, a graft-modified product can be used as necessary from the viewpoint of improving the adhesiveness or moldability of the resin film. The graft-modification method and specific graft monomer are the same as those exemplified in the description of the polyolefin resin in the base layer.
[0052] The slipping layer preferably contains a polyethylene resin as a main component. Here, "containing a polyethylene resin as a main component" means that the content of the polyethylene resin in the slipping layer is 50% by mass or more. When the main component of the slipping layer is a polyethylene resin, the peelability becomes appropriate. The slipping layer may contain other resins, for example polypropylene-based resins, within the range that does not impair the effects of the present invention.
[0053] The surface roughness of the slipping layer is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.5 μm or more. On the other hand, it is preferably 5 μm or less, more preferably 2 μm or less. If the surface roughness is above the lower limit, the contact area between the slipping layer and the adhesive layer is reduced during lamination of the adhesive film, improving the peelability. On the other hand, if the surface roughness is below the upper limit, it is possible to prevent the surface roughness shape of the slipping layer from being transferred to the adhesive layer, thereby preventing a decrease in adhesive strength. The surface roughness is the three-dimensional center plane average roughness (SRa) based on JIS-B-0601:2001.
[0054] In order to obtain a slipping layer having the above-mentioned specific surface roughness, for example, the surface of the slipping layer may be embossed, or the slipping layer may contain a filler, and these methods may be used alone or in combination.
[0055] The shape of the embossing is not particularly limited, and it is preferable that the embossing is performed so as to obtain the desired surface roughness. The embossing method may be a known method.
[0056] Examples of the filler that the slipping layer can contain include inorganic fillers and organic fillers, and specific examples of the inorganic fillers and organic fillers are the same as those in the above-mentioned base layer. It is also possible to indirectly roughen the surface of the slipping layer by blending a filler not in the slipping layer but in a layer inside the slipping layer.
[0057] As the filler, the above-mentioned inorganic fillers and organic fillers can be used alone or in combination. The content of the filler in the slipping layer (when an inorganic filler and an organic filler are used in combination, the total amount of the fillers) is preferably 1% by mass to 20% by mass, and more preferably 5% by mass to 10% by mass.
[0058] <Other ingredients> Like the base layer, the slipping layer may further contain a heat stabilizer (antioxidant), a light stabilizer, a dispersant, a lubricant, a nucleating agent, or the like, as necessary, within a range that does not impair the effects of the present invention.
[0059] <Structure of the slip layer> The slipping layer may have a single-layer structure or a multi-layer structure consisting of two or more layers. The thickness of the slipping layer is 8 μm or less, preferably 5 μm or less, from the viewpoint of cuttability as described above, and is preferably 0.1 μm or more, more preferably 1 μm or more, from the viewpoint of preventing exposure of the base layer.
[0060] <Stretched film> Since the polyethylene resin which is the main component of the slipping layer is a resin which is difficult to orient, it is considered that a difference in elastic modulus is unlikely to occur even when the layer is stretched, and the change in the linear cut property of the slipping layer itself is small. On the other hand, a thinner slipping layer is preferable because it is less likely to impair the linear cutting ability of the base layer. Therefore, in order to make the thickness of the slipping layer 8 μm or less as described above, the slipping layer may be a stretched film. However, from the viewpoint of not impeding linear cuttability, the thinner the film the better, and the most common means for thinning the film is stretching.
[0061] <Other layers> The pressure-sensitive adhesive film of the present invention may have other layers in addition to the above-mentioned pressure-sensitive adhesive layer, base layer, and slipping layer. For example, in order to increase the adhesion between the pressure-sensitive adhesive layer and the base layer, a coating layer may be provided between the pressure-sensitive adhesive layer and the base layer.
[0062] <Coating layer> The coating layer contains a resin having adhesive properties, such as a urethane-based resin, an olefin-based copolymer, a styrene-based resin, and an ethyleneimine-based resin, and one or more of these may be used. The coating layer can be formed by applying a coating liquid onto the surface of the base layer and drying it.
[0063] When the resin having adhesiveness is a water-soluble resin such as an ethyleneimine-based resin, the coating liquid can be prepared by dissolving the resin in water. The content of the ethyleneimine-based resin in the coating liquid is preferably 2 parts by mass or more, more preferably 10 parts by mass or more, in terms of solid content, while it is preferably 40 parts by mass or less, more preferably 30 parts by mass or less. If the content is within this range, sufficient adhesiveness is easily obtained.
[0064] When the resin having adhesive properties is a water-insoluble resin such as a urethane resin, an olefin copolymer, or a styrene resin, a coating liquid containing an emulsion of the resin dispersed in a dispersion medium can be prepared. In this case, the coating layer contains a component derived from the emulsion of resin particles (hereinafter, sometimes simply referred to as an emulsion).
[0065] Here, the emulsion-derived component refers to a residual component remaining after the dispersion medium of the emulsion in the coating liquid for the coating layer evaporates. For example, the residual component is the resin particles in the emulsion and other components added as necessary. These components may contain modified substances that are modified during the process of forming the coating layer. The resin particles in the residual component are present in the form of particles in the coating layer, but may melt and deform due to overheating during printing.
[0066] An emulsion is a liquid in which fine resin particles are emulsified or dispersed in a dispersion medium. In the present invention, the resin particles refer to fine resin particles that are dispersed in a dispersion medium to form an emulsion. From the viewpoint of ease of handling, an O / W emulsion in which resin particles are emulsified or dispersed in an aqueous dispersion medium is preferred.
[0067] When the coating layer contains a component derived from the emulsion, it is possible to obtain adhesion to various laminates.
[0068] The volume average particle size of the resin particles contained in the emulsion is preferably 0.01 μm or more, more preferably 0.05 μm or more, from the viewpoint of handling, and is preferably 3.0 μm or less, more preferably 2.0 μm or less, from the viewpoint of film-forming property and ink adhesion. The volume average particle size of the resin particles is measured using a laser diffraction type particle size distribution measuring device (Shimadzu Corporation: SALD-2200).
[0069] The content of the resin particles in the emulsion is preferably 5% by mass to 80% by mass, from the viewpoint of easily obtaining an emulsion having the above-mentioned particle size. The content of solids of the components derived from the emulsion in the coating layer is preferably 10% by mass to 99% by mass based on the total solids content of the coating layer, from the viewpoints of printability and ease of emulsion preparation.
[0070] The coating liquid may be either the aqueous solution or the emulsion, or a mixture of the two.
[0071] <<Other ingredients>> The coating layer may contain other additives such as an antistatic agent, if necessary, to the extent that the adhesion is not impaired.
[0072] <<<Antistatic agent>>> The antistatic agent can reduce problems such as adhesion of dust due to charging of the film surface or problems due to static electricity during printing. The antistatic agent is not particularly limited, and cationic, anionic, amphoteric or nonionic antistatic agents can be used. As the antistatic agent, a nitrogen-containing polymer type antistatic agent is preferably used, and more preferably a tertiary nitrogen- or quaternary nitrogen-containing acrylic resin is used. These antistatic agents may be used alone or in combination of two or more. The amount of the antistatic agent added in the coating liquid is preferably 5 parts by mass or more, and preferably 60 parts by mass or less, calculated as solid content. If the amount of the antistatic agent added is equal to or more than the lower limit, antistatic performance is easily obtained, and if it is equal to or less than the upper limit, sufficient adhesion is easily obtained.
[0073] <<Coating layer thickness>> The thickness of the coating layer is preferably 0.05 μm or more, more preferably 0.1 μm or more, while it is preferably 5 μm or less, more preferably 1 μm or less. If the thickness is within this range, sufficient adhesion is likely to be obtained.
[0074] <Characteristics of adhesive film> The pressure-sensitive adhesive film of the present invention having the above-mentioned configuration has excellent cuttability in addition to high adhesive properties and peelability. The thickness of the adhesive film of the present invention is preferably 20 μm or more, more preferably 40 μm or more, and particularly preferably 60 μm or more, from the viewpoints of strength and stiffness, and is preferably 550 μm or less, more preferably 300 μm or less, particularly preferably 150 μm or less, and most preferably 100 μm or less, from the viewpoints of straight cuttability and the ability to increase the number of turns when rolled up.
[0075] <Adhesive properties> The adhesive film of the present invention has an adhesive strength of preferably 50 mN / 25 mm or more, more preferably 80 mN / 25 mm or more, and also preferably 1000 mN / 25 mm or less, more preferably 500 mN / 25 mm or less. When the adhesive strength is equal to or greater than the lower limit, a good adhesive effect can be obtained. On the other hand, when the adhesive strength is equal to or less than the upper limit, the adhesive strength is not too strong and inconvenient to handle. The adhesive strength is measured in accordance with JIS Z 0237:2000.
[0076] <Peeling properties> The adhesive film of the present invention has a peel strength of preferably 0.01 mN / 15 mm or more, more preferably 0.1 mN / 15 mm or more, when two adhesive films are laminated so that one slip layer overlaps the other adhesive layer. When the peel strength is equal to or more than the lower limit, an adhesive film having excellent peel resistance during use can be obtained. The peel strength is preferably 3 mN / 15 mm or less, more preferably 1 mN / 15 mm or less. By keeping the peel strength below the upper limit, a pressure-sensitive adhesive film with excellent peelability can be obtained. The peel strength can be measured using a Tensilon universal testing machine (product name: RTM-250, manufactured by Orientec Co., Ltd.).
[0077] <Adhesive film laminate> The adhesive film laminate of the present invention is a laminate in which a plurality of the above-mentioned adhesive films of the present invention are laminated so that the adhesive layer and the slipping layer are in contact with each other. The number of layers is not particularly limited, and when used as an adhesive cleaner, for example, it is preferably 3 to 500. The laminate may be a laminate of a plurality of adhesive films, or a laminate in which a long and narrow strip-shaped adhesive film is wound.
[0078] <Method of manufacturing adhesive film> The adhesive film of the present invention can be produced by laminating an adhesive layer, a base layer, and a slipping layer in this order, and the production method is not particularly limited. For example, the adhesive film of the present invention can be produced by forming a laminated film having a base layer and a slipping layer in this order, and applying a coating liquid for forming an adhesive layer on the base layer to form an adhesive layer.
[0079] <Film forming and lamination> Examples of methods for forming a film include cast molding in which a molten resin is extruded into a sheet shape using a single-layer or multi-layer T-die, I-die, etc. connected to a screw-type extruder, calendar molding, rolling molding, inflation molding, etc. Alternatively, a film may be formed by casting or calendar molding a mixture of a thermoplastic resin and an organic solvent or oil, and then removing the solvent or oil.
[0080] Examples of film lamination methods include co-extrusion, extrusion lamination, and coating, and these methods can be combined. In the co-extrusion method, resin compositions for each layer melt-kneaded in separate extruders are laminated and extruded in a feed block or multi-manifold, and film formation and lamination are performed in parallel. In the extrusion lamination method, a resin composition is extruded onto a preformed film to laminate the film. In the coating method, a resin solution, emulsion, or dispersion is applied onto a film and dried to form and laminate the film.
[0081] <Stretching> Each layer may be stretched individually before lamination, or may be stretched together after lamination, or the unstretched layer and the stretched layer may be laminated together and then stretched again.
[0082] Examples of the stretching method for stretching the film include a longitudinal stretching method using the difference in peripheral speed between rolls, a transverse stretching method using a tenter oven, a sequential biaxial stretching method, a rolling method, a simultaneous biaxial stretching method, etc., which are combinations of these. A simultaneous biaxial stretching (inflation molding) method, etc. can also be used.
[0083] The stretching temperature during stretching is preferably in the range of the glass transition temperature of the resin or higher when the resin used for the film is a non-crystalline resin, and in the range of the glass transition temperature of the non-crystalline part of the resin or higher and the melting point of the crystalline part of the resin or lower, specifically, a temperature 2 to 60° C. lower than the melting point of the resin is preferable when the resin used for the film is a crystalline resin.
[0084] The stretching speed is not particularly limited, but from the viewpoint of stable stretch forming, it is preferably within the range of 20 m / min to 350 m / min. The stretching ratio can also be appropriately determined in consideration of the properties of the resin used. For example, when a resin film containing a propylene homopolymer or a copolymer thereof is stretched in one direction, the lower limit of the stretching ratio is usually 1.2 times or more, preferably 2 times or more, while the upper limit is usually 12 times or less, preferably 10 times or less. When biaxially stretching, the stretching ratio is an areal stretching ratio, and the lower limit is usually 1.5 times or more, preferably 10 times or more, while the upper limit is usually 60 times or less, preferably 50 times or less.
[0085] <Formation of Coating Layer> When a coating layer is provided between the adhesive layer and the base layer, a coating liquid for forming the coating layer is prepared and applied onto the base layer to form the coating layer. The coating liquid can be prepared by blending additives, etc., as necessary, with the above-mentioned aqueous resin solution or emulsion of resin particles.
[0086] When using cationic urethane resin particles, an emulsion can be prepared by dispersing a copolymer having cationic hydrophilic groups introduced into a polyurethane resin skeleton in water.Specific examples of the method include a method of emulsifying and dispersing monomers constituting the target polymer in water and polymerizing the monomers, and a method of obtaining the target polymer by bulk polymerization or the like, and then melt-kneading and emulsifying the raw resins successively using a twin-screw extruder.
[0087] When using resin particles of an olefin copolymer, the method for preparing the emulsion is not particularly limited, but for example, the following method (1) or (2) can be used.
[0088] (1) An olefin copolymer is put into an aromatic hydrocarbon solvent and dissolved by heating to prepare a resin solution. A dispersant is added to this resin solution, and the mixture is stirred and mixed. Water is then added to cause phase inversion. The aromatic hydrocarbon solvent is then distilled off, and the resulting aqueous dispersion is used as an emulsion.
[0089] (2) An olefin copolymer is melted using a twin-screw extruder, and then an aqueous solution of a dispersant is added and kneaded to obtain an aqueous dispersion, which is used as an emulsion (see Japanese Patent Publication No. 62-29447).
[0090] When preparing the emulsion by these methods, it is preferable to use a polymer emulsifier such as a cationic water-soluble polymer as a dispersant, and furthermore, it is preferable to use the dispersion method using a twin-screw extruder described above in (2). This makes it possible to easily adjust the volume average particle size of the resin particles of the olefin copolymer in the emulsion to 0.01 μm to 3.00 μm. In the above method (2), the volume average particle size of the resin particles of the olefin copolymer in the emulsion can be adjusted, for example, by controlling the amount of water relative to the olefin copolymer, the cylinder temperature and its profile, the residence time of the resin in the extruder, the barrel rotation speed of the extruder, etc., among the operating conditions of the twin-screw extruder.
[0091] The solids concentration of the coating fluid is preferably 0.1% by mass or more, more preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, based on the total amount of the coating fluid.
[0092] The coating of the coating liquid can be carried out using a coating device such as a roll coater, a bar coater, a size press coater, or a spray coater.
[0093] The coating amount of the coating solution was 0.05 g / m2 in terms of solid content after drying. 2 It is preferable that the content is 0.10 g / m or more. 2 More preferably, it is 0.15 g / m or more. 2 More preferably, the thickness is 1.40 g / m or more. 2 Preferably, it is 0.50 g / m or less. 2 More preferably, it is 0.30 g / m or less. 2 More preferably, it is 0.24 g / m or less. 2 It is particularly preferred that:
[0094] <Formation of adhesive layer> The adhesive layer can be formed by a known method such as coating (spraying or spraying) or bonding via an adhesive. EXAMPLES
[0095] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the terms "parts", "%", and the like are based on mass unless otherwise specified.
[0096] [Raw materials] The raw materials used in the examples and comparative examples are as shown in the table below.
[0097] [Table 1]
[0098] [Preparation of coating solution for coating layer] (Dispersant (H)) A reactor having an internal volume of 150 L equipped with a cooler, a nitrogen inlet tube, a stirrer, a monomer dropping funnel, and a jacket for heating was charged with 40 kg of isopropanol (Tokuyama Corporation: trade name Tokuso IPA). Next, while stirring, 12.6 kg of N,N-dimethylaminoethyl methacrylate (Sanyo Chemical Industries, Ltd.: trade name Methacrylate DMA), 12.6 kg of butyl methacrylate (Mitsubishi Rayon Co., Ltd.: trade name Acrylate B), and 2.8 kg of higher alcohol methacrylate ester (Mitsubishi Rayon Co., Ltd.: trade name Acrylate SL, a mixture of lauryl methacrylate and tridecyl methacrylate) were charged. After nitrogen replacement, the internal temperature was raised to 80°C, and 0.3 kg of azobisisobutyronitrile (Wako Pure Chemical Industries, Ltd.: trade name V-60 (AIBN)) was added as a polymerization initiator to start polymerization.
[0099] After polymerization for 4 hours while maintaining the reaction temperature at 80°C, the obtained copolymer was neutralized with 4.3 kg of glacial acetic acid (manufactured by Wako Pure Chemical Industries, Ltd.). Next, 48.3 kg of ion-exchanged water was added to replace the inside of the system while distilling off isopropanol, and an aqueous solution (solid content concentration 35% by weight) of the neutralized cationic polymer emulsifier made of a (meth)acrylic acid-based copolymer was obtained as a dispersant (H). The weight-average molecular weight of the obtained polymer emulsifier was 40,000.
[0100] (Emulsion of urethane copolymer resin (E1)) A cationic polyurethane water dispersion (product name: Hydran CP-7050, manufactured by DIC Corporation) was used as emulsion (E1). The solid content of this emulsion (E1) was 25 mass%, and the volume average particle size of the resin particles in the emulsion (E1) was 0.07 μm. The volume average particle size was measured using a laser diffraction particle size distribution measuring device (manufactured by Shimadzu Corporation: SALD-2200).
[0101] (Ethyleneimine resin solution (F)) Into a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen gas inlet, 100 parts by mass of a 25% by mass aqueous solution of polyethyleneimine (manufactured by Nippon Shokubai Co., Ltd., product name: Epomin P-1000), 10 parts by mass of 1-chlorobutane (manufactured by Wako Pure Chemical Industries, Ltd., reagent), and 10 parts by mass of propylene glycol monomethyl ether (manufactured by Wako Pure Chemical Industries, Ltd., reagent) were introduced. The mixture was then stirred under a nitrogen stream and subjected to a modification reaction at a temperature of 80°C for 20 hours. Water was then added to this solution to adjust the solid content concentration to 20% by mass, thereby obtaining an ethyleneimine-based resin solution (F).
[0102] (Antistatic agent (G)) 35 parts by mass of N,N-dimethylaminoethyl methacrylate (manufactured by Mitsubishi Gas Chemical Co., Ltd.), 20 parts by mass of ethyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), 20 parts by mass of cyclohexyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), 25 parts by mass of stearyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), 150 parts by mass of ethyl alcohol, and 1 part by mass of 2,2'-azobis(isobutyronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., reagent) were introduced into a four-neck flask equipped with a stirrer, a reflux condenser (condenser), a thermometer, and a dropping funnel. The system was replaced with nitrogen, and a polymerization reaction was carried out at 80°C for 6 hours under a nitrogen stream. Then, 85 parts by mass of a 50% by mass aqueous solution of 3-chloro-2-hydroxypropyltrimethylammonium chloride (manufactured by Wako Pure Chemical Industries, Ltd., reagent) was added. After further reacting at 80° C. for 15 hours, ethyl alcohol was distilled off while adding water dropwise, to obtain a solution of an antistatic agent made of a quaternary ammonium salt type copolymer with a solid content concentration of 20% by mass.
[0103] (Coating fluid) An aqueous solution containing 13% by mass of the urethane resin emulsion (E1), 0.5% by mass of the ethyleneimine resin solution (F), and 0.5% by mass of the antistatic agent (G) was prepared and used as coating solution (1). The concentration of each component above indicates the solid content concentration of each component relative to the entire coating solution.
[0104] [Manufacturing of adhesive films] Example 1 A resin composition consisting of 80 parts by mass of a polypropylene resin (Novatec PP FY-4) and 20 parts by mass of filler 1 (Softon 1800) was melt-kneaded in an extruder set at 230°C. It was then fed to an extrusion die set at 250°C and extruded into a sheet, which was then cooled to 60°C by a cooling device to obtain an unstretched sheet. This unstretched sheet was heated to 135°C and stretched 5 times in the flow direction (longitudinal direction) using the difference in peripheral speed of the roll group to form the base layer 1.
[0105] Next, a resin composition consisting of 60 parts by mass of a polypropylene resin and 40 parts by mass of the filler 1 was melt-kneaded in an extruder set at 250° C., and then extruded into a sheet shape onto the base layer 1. As a result, the base layer 2 consisting of the resin composition was laminated on the base layer 1.
[0106] On the other hand, 100 parts by mass of a polyethylene resin (Novatec LD LC540) was melt-kneaded in one extruder set at 250 ° C., and a resin composition consisting of 60 parts by mass of a polypropylene resin and 40 parts by mass of a filler 1 was melt-kneaded in the other extruder set at 250 ° C., and then a slipping layer consisting of a polyethylene resin and a base layer 3 consisting of a resin composition were stacked in this order to form a sheet, and the two layers were co-extruded into a sheet on the main surface of the base layer 1 opposite to the main surface on which the base layer 2 was laminated. Immediately after that, the sheet was passed through an embossing roll (150 lines per inch, reverse gravure type) consisting of a metal roll and a rubber roll, and a pattern was embossed at intervals of 0.17 mm on the surface of the slipping layer. As a result, a four-layer sheet was obtained in which the base layer 2 / base layer 1 / base layer 3 / slipping layer were stacked in this order.
[0107] The four-layer sheet obtained was cooled to 60°C by a cooling device, and then the laminated sheet was heated to about 150°C using a tenter oven and stretched 8.5 times in the direction perpendicular to the flow (transverse direction), then heated to 160°C for heat treatment, cooled to 60°C, and the edge portions were slit. Next, a corona discharge treatment was applied to the base layer 2 of the four-layer sheet using a continuous coating device. The corona discharge treatment was performed with an applied energy density of 4200 J / m 2 Next, the coating liquid was applied onto the base layer 2 and dried in a hot air blowing dryer at 60°C to form a coating layer. The solid content of the coating layer after drying was 0.2 g / m 2 It was. As a result, a five-layer sheet was obtained in which coating layer / substrate layer 2 / substrate layer 1 / substrate layer 3 / slip layer were laminated in this order. Total thickness of all layers: 74μm Each layer thickness:- / 20μm / 30μm / 20μm / 4μm Number of stretching axes for each layer: - / 1-axis / 2-axis / 1-axis / 1-axis
[0108] An acrylic resin (Olivine BPS5978) was applied onto the coating layer to a dry thickness of 5 μm, and dried to laminate an adhesive layer.
[0109] In this manner, an adhesive film of Example 1 was produced.
[0110] Example 2 An adhesive film was produced in the same manner as in Example 1, except that the extrusion amount of the polyethylene-based resin extruded onto the base layer 1 was adjusted to set the film thickness of the slipping layer as shown in the table below.
[0111] Example 3 An adhesive film was produced in the same manner as in Example 1, except that a composition containing 92 parts by mass of polyethylene resin and 8 parts by mass of filler 2 was used to form the slipping layer, and embossing was not performed.
[0112] Example 4 An adhesive film was produced in the same manner as in Example 1, except that the embossing process was not carried out in forming the slipping layer.
[0113] Comparative Example 1 An adhesive film was produced in the same manner as in Example 1, except that the extrusion amount of the polyethylene-based resin extruded onto the base layer 1 was adjusted to set the film thickness of the slipping layer as shown in the table below.
[0114] Comparative Example 2 An adhesive film was produced in the same manner as in Example 1, except that a polypropylene-based resin was used instead of a polyethylene-based resin in forming the slipping layer.
[0115] Comparative Example 3 An adhesive film was produced in the same manner as in Comparative Example 2, except that an embossing roll with an 8 times deeper groove was used for forming the slipping layer.
[0116] Comparative Example 4 An adhesive film was produced in the same manner as in Comparative Example 2, except that a composition containing 90 parts by mass of polypropylene-based resin and 10 parts by mass of lubricant (aluminum stearate) was used to form the slipping layer, and embossing was not performed.
[0117] <Evaluation of the elastic modulus of the adhesive layer> The elastic modulus of the acrylic resin in the pressure-sensitive adhesive film was measured by the following method. A drop of instant adhesive (Toagosei Co., Ltd., Aron Alpha (registered trademark), professional impact resistance) was applied to the surface of the support layer of the measuring device, and the support layer and the adhesive layer of the adhesive film were bonded via the instant adhesive to fix the adhesive film to a sample fixing table dedicated to the measuring device, and then the indentation elastic modulus of the adhesive layer was measured. The measuring device used was a nanoindenter "ENT-2100" manufactured by Elionix Co., Ltd. The measurement conditions were as follows: a triangular pyramid diamond indenter (Berkovich indenter) with an inter-edge angle of 115° was used, measurement mode: load-unload test, maximum load: 3 μN, holding time when the maximum load was reached: 1 second, loading speed / unloading speed: 10 μN / sec, and the obtained measurement data was processed using a dedicated analysis software (version 6.18) attached to the measuring device to obtain the elastic modulus of the acrylic resin (indentation elastic modulus in the thickness direction) (MPa).
[0118] <Evaluation of Elasticity of Adhesive Film> The adhesive film was cut into a test piece measuring 30 mm in length and 15 mm in width, and dynamic viscoelasticity measurements were performed in both the machine direction and the perpendicular direction using a solid viscoelasticity measuring device (TA Instruments Japan: RSA-III). The measurement conditions were chuck distance 20 mm, measurement frequency 10 Hz, strain amount 0.1%, heating rate 10°C / min, and tension mode, and the storage modulus at 23°C was taken as the tensile modulus.
[0119] <Evaluation of surface roughness of slipping layer> The surface roughness of the slipping layer was measured in accordance with JIS-B-0601:2001.
[0120] <Evaluation of adhesive strength of adhesive layer> The adhesive strength of the adhesive layer in the adhesive film was measured after two adhesive films were laminated so that the slipping layer of one was overlapped with the adhesive layer of the other, pressed, and then peeled off. Pressure conditions: Adhesion area 200mm x 25mm, pressure 4MPa, pressure time 5 minutes Peeling conditions: Peeling angle 180°, peeling speed 300mm / min The peel strength of the adhesive layer after peeling was measured in accordance with JIS Z 0237:2000. Specifically, the adhesive film was cut into a test piece measuring 200 mm in length and 25 mm in width, the adhesive layer portion was attached to an adherend SUS430BA plate whose surface had been cleaned with toluene, and a 2 kg roller was moved back and forth once on the surface of the support layer to press the adherend. Thirty minutes after pressing, the test piece was peeled in a 180° direction at a tensile speed of 300 mm / min to measure the adhesive strength. The adhesive strength was evaluated according to the following criteria. A:50[mN / 25mm] or more (good) C: Less than 50 [mN / 25mm] (not acceptable)
[0121] <Evaluation of peelability between slip layer and adhesive layer> Two adhesive films were laminated so that the slipping layer of one was overlapped with the adhesive layer of the other, and after pressure was applied, they were peeled off. Pressure conditions: Adhesion area 200mm x 15mm, pressure 4MPa, pressure time 5 minutes Peeling conditions: Peeling angle 180°, peeling speed 300mm / min The peel strength was measured three times under the above conditions, and the average value was taken as the peel strength [mN / 15 mm]. A Tensilon universal testing machine was used as the measuring device.
[0122] The peel strength was evaluated from the following two perspectives. (Resistance to slipping during use (peel resistance)) A: 0.01[mN / 15mm] or more (good) C: Less than 0.01 [mN / 15 mm] (not acceptable) (Smoothness when peeling (ease of peeling)) A: 1[mN / 15mm] or less (good) B: Over 1 [mN / 15mm] and under 3 [mN / 15mm] (acceptable) C:3[mN / 15mm] or more (not possible)
[0123] <Linear cutting ability (cuttability) of adhesive film> The straight line cutting performance was evaluated by carrying out an evaluation experiment according to the following procedure. (1) The adhesive film was cut into test samples measuring 20 mm in width and 297 mm in length, and 10 sets were prepared. (2) A 1 mm cut was made with a cutter in the center of the short side of the sample so that it could be torn in the direction perpendicular to the flow direction (TD). (3) The material was torn in the TD direction starting from the cut at an angle of 180° at a speed of 300 m / min. If the sample was torn to the short side on the opposite side, one point was added. The same test was repeated 10 times and the sample was evaluated based on the following criteria. A: 9 points or more (good) B: 7~8 points (acceptable) C: 6 points or less (not possible)
[0124] The evaluation results are shown in the table below.
[0125] [Table 2]
[0126] From the above results, the adhesive strength, peelability, and linear cutability of the adhesive layer of all of the adhesive films of the Examples were all rated A (good) or B (acceptable). In addition, a comparison of Example 4 with Examples 1 and 3 showed that the ease of peeling after use, among other peelability properties, was further improved by adjusting the surface roughness of the slipping layer to an appropriate range by embossing or adding a filler. On the other hand, the adhesive film of Comparative Example 1, which has a thick slipping layer, had a decreased linear cut property. The adhesive films of Comparative Examples 2 and 3, which use a propylene-based resin in the slipping layer, did not improve peel resistance during use even when the slipping layer was embossed, and the adhesive performance of Comparative Example 3, which was strongly embossed, actually worsened. The adhesive film of Comparative Example 4, which uses a propylene-based resin in the slipping layer and contains a lubricant, had good peelability and linear cut property, but showed significantly poor adhesive performance.
[0127] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2021-055636) filed on March 29, 2021, the contents of which are incorporated herein by reference. [Industrial Applicability]
[0128] The adhesive films of the present invention are useful in adhesive cleaners for removing dust, fibers, particulates, and the like. The adhesive film of the present invention can also be used as cellophane tape or sticky notes. [Explanation of symbols]
[0129] 10...adhesive film, 1...base layer, 2...slip layer, 3...adhesive layer
Claims
1. An adhesive film having an adhesive layer, a base layer, and a slipping layer in this order, The adhesive layer contains an adhesive resin having an elastic modulus of 100 MPa or less, The substrate layer is a thermoplastic resin film, the slipping layer contains a polyethylene resin, has a thickness of 8 μm or less, and has a surface roughness of 0.05 μm or more and 5 μm or less; The pressure-sensitive adhesive film has an absolute value |ΔE| of the difference between the elastic modulus E MD in the machine direction and the elastic modulus E TD in the perpendicular direction of the film, of 500 MPa or more.
2. An adhesive film having an adhesive layer, a base layer, and a slipping layer in this order, The adhesive layer contains an adhesive resin having an elastic modulus of 100 MPa or less, the base layer is a thermoplastic resin film containing a polypropylene-based resin and a filler, The slipping layer contains a polyethylene resin and has a thickness of 8 μm or less, The pressure-sensitive adhesive film has an absolute value |ΔE| of the difference between the elastic modulus E MD in the machine direction and the elastic modulus E TD in the perpendicular direction of the film, of 500 MPa or more.
3. An adhesive film having an adhesive layer, a coating layer, a base layer, and a slipping layer in this order, The adhesive layer contains an adhesive resin having an elastic modulus of 100 MPa or less, the coating layer contains one or more selected from a urethane-based resin, an olefin-based copolymer, a styrene-based resin, and an ethyleneimine-based resin; The substrate layer is a thermoplastic resin film, The slipping layer contains a polyethylene resin and has a thickness of 8 μm or less, The pressure-sensitive adhesive film has an absolute value |ΔE| of the difference between the elastic modulus E MD in the machine direction and the elastic modulus E TD in the perpendicular direction of the film, of 500 MPa or more.
4. An adhesive film having an adhesive layer, a base layer, and a slipping layer in this order, The adhesive layer contains an adhesive resin having an elastic modulus of 100 MPa or less, The substrate layer is a thermoplastic resin film, the slipping layer contains a polyethylene resin, has a thickness of 8 μm or less, and is a uniaxially stretched resin film; The pressure-sensitive adhesive film has an absolute value |ΔE| of the difference between the elastic modulus E MD in the machine direction and the elastic modulus E TD in the perpendicular direction of the film, of 500 MPa or more.
5. The pressure-sensitive adhesive film according to any one of claims 1 to 4, wherein the base layer is porous.
6. 6. An adhesive film laminate comprising the adhesive film according to claim 1 laminated on the adhesive layer so that the adhesive layer and the slipping layer are in contact with each other.
Citation Information
Patent Citations
Easily releasable laminate film
JP2002113817A
Cleaning roll
JP2002307554A
Cleaning tape
JP2003210382A