Photothermal conversion element, its manufacturing method, photothermal power generation device, and micro-object integration system

Laser processing of thermoelectric materials forms fine particles for high-efficiency light-to-heat conversion, integrated with thermoelectric elements for efficient power generation, addressing the complexity and inefficiency of traditional photothermal conversion methods.

JP7572731B2Active Publication Date: 2024-10-24PUBLIC UNIVERSITY CORPORATION OSAKA CITY UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021543083
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-29
Filing Date
2020-08-28
Publication Date
2024-10-24
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Existing photothermal conversion elements require complex chemical treatments for manufacturing and do not efficiently convert light into heat.

Method used

A method involving laser processing to form fine particles on a solid material, such as a thermoelectric material or metal thin film, causing localized surface plasmon resonance for high-efficiency heat conversion, and integrating these elements with thermoelectric conversion sections for power generation.

Benefits of technology

The method allows for high-efficiency conversion of light into heat and subsequent electricity generation, with simplified manufacturing and reduced complexity compared to traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572731000002
    Figure 0007572731000002
  • Figure 0007572731000003
    Figure 0007572731000003
  • Figure 0007572731000004
    Figure 0007572731000004
Patent Text Reader

Abstract

A production method for a photothermal conversion element (1, 2), the production method comprising a step for preparing a solid material and a step for radiating laser light at the solid material and thereby forming a processed region. The step for forming the processed region includes a step for micronizing the solid material such that the processed region (LP) turns black.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a photothermal conversion element, a manufacturing method for a photothermal conversion element, a photothermal power generation device using the photothermal conversion element, and an integration system for micro-objects using the photothermal conversion element. [Background technology]

[0002] In recent years, photothermal conversion elements that convert white light such as sunlight into heat and utilize the heat have been attracting attention. The manufacture of photothermal conversion elements often requires complicated methods including chemical processing. Therefore, a technology for manufacturing photothermal conversion elements using a simpler manufacturing method has been proposed.

[0003] For example, a photothermal conversion element disclosed in Japanese Patent Laid-Open Publication No. 2013-254940 (Patent Document 1) includes a plurality of metallic nanoparticle assembly structures and a substrate. Each of the plurality of metallic nanoparticle assembly structures is formed by accumulating a plurality of metallic nanoparticles. The substrate has a fixing surface to which the plurality of metallic nanoparticle assembly structures are fixed. A region in which the plurality of metallic nanoparticle assembly structures are densely packed is formed on this fixing surface. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-254940 A [Patent Document 2] International Publication No. 2017 / 195872 [Patent Document 3] JP 2017-202446 A [Non-patent literature]

[0005] [Non-Patent Document 1] Atsuko Kosuga, Yasuyuki Yamamoto, Moe Miyai, Mie Matsuzawa, Yushi Nishimura, Shimpei Hidaka, Kohei Yamamoto, Shin Tanaka, Yojiro Yamamoto, Shiho Tokonami and Takuya Iida, "A high performance photothermal film with spherical shell-type metallic nanocomposites for solar thermoelectric conversion", Nanoscale, 2015, 7, 7580-7584 Summary of the Invention [Problem to be solved by the invention]

[0006] Photothermal conversion elements that convert light into heat are required to be able to convert light into heat as efficiently as possible, and further, it is desired that such photothermal conversion elements can be manufactured by a simple manufacturing method.

[0007] The present disclosure has been made to solve the above problems, and an object of the present disclosure is to provide a photothermal conversion element capable of converting light into heat with high efficiency. Another object of the present disclosure is to provide a simple method for manufacturing the photothermal conversion element. [Means for solving the problem]

[0008] (1) A method for manufacturing a photothermal conversion element according to an aspect of the present disclosure includes the steps of preparing a solid material and forming a processed region by irradiating the solid material with laser light. The forming step includes the step of microparticulating the solid material so that the processed region is blackened.

[0009] (2) The forming step includes a step of scanning a laser beam so that a fine groove is cut in the processing area.

[0010] (3) The solid-state material includes at least one of a thermoelectric material that exhibits a thermoelectric effect and a metal thin film.

[0011] (4) A photothermal conversion element according to another aspect of the present disclosure includes a solid material, the solid material including a region in which a plurality of particles made of the solid material are dispersed to blacken the solid material, and the plurality of particles generate localized surface plasmon resonance on a surface of each of the plurality of particles when irradiated with light.

[0012] (5) The solid material includes at least one of a thermoelectric material that exhibits a thermoelectric effect and a metal thin film.

[0013] (6) A photothermal power generation device according to still another aspect of the present disclosure is capable of supplying generated electric power to a load. The photothermal power generation device includes a photothermal conversion element and a thermoelectric conversion unit thermally connected to the photothermal conversion element and converting heat into electricity. The thermoelectric conversion unit includes a P-type thermoelectric element, a first electrode electrically connected to the low-temperature side of the P-type thermoelectric element, an N-type thermoelectric element, and a second electrode electrically connected to the low-temperature side of the N-type thermoelectric element. The first electrode and the second electrode are connected to the load.

[0014] (7) The photothermal conversion element and one of the P-type thermoelectric element and the N-type thermoelectric element are integrally formed into a photothermal conversion thermoelectric element.

[0015] (8) A photothermal conversion element according to still another aspect of the present disclosure includes a substrate and a metal thin film disposed on the substrate. The metal thin film includes a region where the metal thin film is blackened by the accumulation of a plurality of particles made of a material of the metal thin film. The plurality of particles generate localized surface plasmon resonance on a surface of each of the plurality of particles when irradiated with light.

[0016] (9) A micro-object accumulation system according to yet another aspect of the present disclosure accumulates a plurality of micro-objects contained in a liquid. The micro-object accumulation system includes a holder configured to hold a photothermal conversion element, and a light source that emits light that induces localized surface plasmon resonance on the surface of each of a plurality of microparticles. The light source accumulates the plurality of micro-objects by irradiating a region with light while the liquid is held on the region to induce convection in the liquid.

[0017] (10) A liquid is held on the upper surface of the region. Light from a light source is irradiated from below to above the region. The thickness of the metal thin film is determined so that the region is optically transparent to the light from the light source. Effect of the Invention

[0018] According to the present disclosure, it is possible to provide a photothermal conversion element capable of converting light into heat with high efficiency, and further, according to the present disclosure, it is possible to easily manufacture such a photothermal conversion element. [Brief description of the drawings]

[0019] [Figure 1] 1 is a diagram illustrating roughly the overall configuration of a laser processing system according to a first embodiment. [Diagram 2] FIG. 2 is a diagram showing a configuration of a photothermal conversion element according to the first embodiment. [Diagram 3] 1 is a photograph of the fabricated photothermal conversion element. [Figure 4] 5 is a diagram showing the configuration of another photothermal conversion element according to the first embodiment. FIG. [Diagram 5] 1 is a photograph of the fabricated photothermal conversion element. [Figure 6] FIG. 1 is a first diagram for explaining laser processing conditions for a photothermal conversion element. [Figure 7] FIG. 2 is a second diagram for explaining the laser processing conditions for the photothermal conversion element. [Figure 8] 4 is a flowchart showing a method for manufacturing the photothermal conversion element according to the first embodiment. [Figure 9]FIG. 4 is a diagram showing laser processing conditions for a photothermal conversion element in an example of the first embodiment. [Figure 10] FIG. 2 is a diagram showing the observation results of a photothermal conversion element in an example of the first embodiment. [Figure 11] FIG. 13 is a diagram showing the measurement results of the absorbance spectrum of a photothermal conversion element manufactured according to condition 1A. [Figure 12] FIG. 13 is a diagram showing the measurement results of the absorbance spectrum of a photothermal conversion element manufactured according to condition 1B. [Figure 13] FIG. 13 is a diagram showing the measurement results of the absorbance spectrum of a photothermal conversion element manufactured according to condition 1C. [Figure 14] FIG. 13 is a diagram showing the measurement results of the absorbance spectrum of a photothermal conversion element manufactured according to condition 1D. [Figure 15] FIG. 13 is a diagram showing laser processing conditions for another photothermal conversion element in the example of the first embodiment. [Figure 16] FIG. 2 is a diagram showing the observation results of a photothermal conversion element in an example of the first embodiment. [Figure 17] FIG. 13 is a diagram showing the measurement results of the reflection spectra of photothermal conversion elements manufactured according to conditions 2A to 2E. [Figure 18] FIG. 11 is a diagram showing the overall configuration of a photothermal power generation device according to a second embodiment. [Figure 19] FIG. 2 is a diagram illustrating an example of a more detailed configuration of a photothermal power generation device. [Figure 20] FIG. 13 is a diagram showing another example of a more detailed configuration of a photothermal power generation device. [Figure 21] 13 is a diagram for explaining the simulation conditions for the amount of temperature rise caused by the photoheating effect of the photothermal conversion element 2. FIG. [Figure 22] 11A and 11B are diagrams showing the results of a simulation of the amount of temperature rise of a photothermal conversion element due to a photoheating effect. [Diagram 23] FIG. 13 is a diagram for explaining simulation conditions for the amount of power generated by photothermal conversion and thermoelectric conversion in a photothermal power generation device. [Figure 24] FIG. 11 is a diagram showing a simulation result of power generation in a photothermal power generation device. [Diagram 25] FIG. 11 is a diagram showing the overall configuration of a micro-object accumulation system according to a third embodiment. [Figure 26] FIG. 2 is an enlarged view of a photothermal conversion element held on an XYZ axis stage. [Figure 27] 1 is a photograph showing the state of a sample when irradiated with laser light. [Figure 28] FIG. 1 is a conceptual diagram for explaining the accumulation mechanism of microbeads. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the present embodiment will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.

[0021] <Terminology explanation> In the present disclosure and its embodiments, the term "thermoelectric material" refers to a material that exhibits a thermoelectric effect (Seebeck effect), and more specifically, refers to a material whose absolute value of thermoelectromotive force at room temperature (20°C) is 50 [μV / K] or more and whose electrical resistivity (specific resistance) at room temperature is 100 [mΩ·cm] or less. Although materials whose absolute value of thermoelectromotive force is 50 [μV / K] or more may include insulators, insulators are excluded from thermoelectric materials under the condition that their electrical resistivity is 100 [mΩ·cm] or less. Examples of thermoelectric materials include alloys (specifically, constantan, Heusler alloys, half-Heusler alloys, etc.), silicides (iron silicide, etc.), metals, semiconductors, ceramics, etc.

[0022] The absolute value of the thermoelectromotive force of constantan is about 75 [μV / K], and the electrical resistivity of constantan is about 4.8 × 10 -2 For comparison, the absolute value of the thermoelectromotive force of gold is about 1.94 [μV / K], and the electrical resistivity of gold is about 2.4×10 -3 [mΩ·cm].

[0023] In the present disclosure and its embodiments, the term "microparticle" refers to a particle having a size ranging from the nanometer order to the micrometer order. The shape of the microparticle is not limited to a spherical shape, and may be an elliptical spherical shape or a rod shape. Examples of the microparticle include metal nanoparticles, metal microparticles, semiconductor nanoparticles, semiconductor microparticles, metal nanoparticle aggregates, aggregates of metal nanoparticles and metal microparticles, aggregates of semiconductor nanoparticles and semiconductor microparticles, and the like.

[0024] In the present disclosure and its embodiments, the term "micro object" refers to a substance having a size ranging from nanometer order to micrometer order. The shape of the micro object is not limited to a sphere, and may be an ellipsoid or a rod. When the micro object is an ellipsoid, at least one of the length in the long axis direction and the length in the short axis direction of the ellipsoid may be within a range from nanometer order to micrometer order. When the micro object is a rod, at least one of the width and length of the rod may be within a range from nanometer order to micrometer order. Examples of the micro object include metal nanoparticles, metal nanoparticle aggregates, metal nanoparticle assembly structures, semiconductor nanoparticles, organic nanoparticles, resin beads, and particulate matter (PM).

[0025] A "metal nanoparticle" is a metal particle having a size on the order of nanometers. A "metal microparticle" is a metal particle having a size on the order of micrometers. A "metal nanoparticle aggregate" is an aggregate formed by the aggregation of multiple metal nanoparticles. A "metal nanoparticle assembly structure" is, for example, a structure in which multiple metal nanoparticles are fixed to the surface of a bead via interaction sites, and are arranged with gaps between them at intervals less than the diameter of the metal nanoparticles. A "semiconductor nanoparticle" is a semiconductor particle having a size on the order of nanometers. A "semiconductor microparticle" is a semiconductor particle having a size on the order of micrometers. An "organic nanoparticle" is a particle made of an organic compound having a size on the order of nanometers. A "resin bead" is a particle made of a resin having a size ranging from the order of nanometers to the order of micrometers. A "PM" is a particulate matter having a size on the order of micrometers.

[0026] The microscopic objects may be biological materials (biological materials). More specifically, the microscopic objects may include cells, microorganisms (bacteria, fungi, etc.), biopolymers (proteins, nucleic acids, lipids, polysaccharides, etc.), antigens (allergens, etc.), and viruses.

[0027] In the present disclosure and its embodiments, the term "microgroove" refers to a groove having a width on the order of micrometers. When multiple microgrooves are cut, the distance between a groove and its adjacent groove is preferably also on the order of micrometers. The shape of the microgroove is not limited to a straight line, and may be a curved shape. In addition, the microgroove may include a portion where one groove branches into multiple grooves, or a portion where multiple grooves are integrated into one groove. The microgroove may be a broken line.

[0028] In the present disclosure and its embodiments, "nanometer order" includes a range of 1 nm to 1,000 nm (= 1 μm). "Micrometer order" includes a range of 1 μm to 1,000 μm (= 1 mm). Therefore, "nanometer order to micrometer order" includes a range of 1 nm to 1,000 μm. The term "nanometer order to micrometer order" typically means a range of several nm to several hundred μm, preferably a range of 100 nm to 100 μm, and more preferably a range of 1 μm to several tens of μm.

[0029] In the present disclosure and its embodiments, the term "white light" refers to light having a wavelength range from ultraviolet to near infrared (for example, a wavelength range of 200 nm to 1100 nm). The white light may be continuous light or pulsed light.

[0030] In the present disclosure and its embodiments, "having optical transparency" means a property in which the intensity of light passing through a material is greater than zero. When light passes through a material, the remaining energy of the light may be absorbed, scattered, or reflected by the material. The wavelength region of the light may be any of the ultraviolet, visible, and near-infrared regions, a region spanning two of these three regions, or a region spanning all three regions. Optical transparency can be defined, for example, by the range of transmittance. In this case, the lower limit of the range of transmittance may be greater than 0, and is not particularly limited.

[0031] In the present disclosure and its embodiments, "microbubbles" refer to air bubbles on the order of micrometers.

[0032] [Embodiment 1] In the first embodiment, two types of photothermal conversion elements 1 and 2 and their manufacturing methods are described. The photothermal conversion elements 1 and 2 according to the first embodiment are manufactured using a laser processing system. In the following, the x direction and the y direction represent the horizontal direction. The x direction and the y direction are mutually perpendicular. The z direction represents the vertical direction. The direction of gravity is downward in the z direction.

[0033] <Laser processing system configuration> Fig. 1 is a diagram illustrating an overall configuration of a laser processing system in the embodiment 1. With reference to Fig. 1, the laser processing system 100 includes an XYZ axis stage 110, a laser oscillator 120, a laser driver 130, an objective lens 140, a scanning mechanism 150, and a control device 160.

[0034] The XYZ axis stage 110 is configured to hold the photothermal conversion element 1 (or the photothermal conversion element 2). The configurations of the photothermal conversion elements 1 and 2 will be described with reference to FIGS.

[0035] The laser oscillator 120 emits a pulsed laser light L. For example, a femtosecond laser that emits ultrashort pulsed light can be used as the laser oscillator 120. A specific example of such a laser oscillator 120 is a titanium sapphire laser. The titanium sapphire laser emits light with a wavelength included in the near-infrared range (a wavelength in the range of 650 nm to 1,100 nm, for example, with a central wavelength of 1,040 nm).

[0036] The laser driver 130 supplies a drive current to the laser oscillator 120 and controls the characteristics of the pulsed laser light L emitted from the laser oscillator 120 (specifically, the laser output, pulse width, repetition frequency, etc.) in accordance with instructions from the control device 160.

[0037] The objective lens 140 focuses the pulsed laser light L from the laser oscillator 120. The light focused by the objective lens 140 is irradiated onto the photothermal conversion element 1 held on the XYZ axis stage 110 and before or during processing.

[0038] The scanning mechanism 150 is configured to be able to adjust the position of the XYZ-axis stage 110 in the x-, y-, and z-directions in response to a command from the control device 160. In this embodiment, the scanning mechanism 150 first sets the distance between the photothermal conversion element 1 held on the XYZ-axis stage 110 and the objective lens 140 (a spot height H of the pulsed laser light L, which will be described later). The scanning mechanism 150 then scans the photothermal conversion element 1 with the pulsed laser light L by adjusting the positions of the XYZ-axis stage 110 in the x- and y-directions while keeping the spot height H constant.

[0039] 1, the scanning of the pulsed laser light L on the photothermal conversion element 1 is realized by fixing the irradiation position of the pulsed laser light L and then moving the photothermal conversion element 1. However, conversely, the irradiation position of the pulsed laser light L may be moved with respect to the fixed photothermal conversion element 1.

[0040] The control device 160 is a microcomputer including a processor such as a CPU (Central Processing Unit), memories such as a ROM (Read Only Memory) and a RAM (Random Access Memory), and input / output ports, all of which are not shown. The control device 160 controls each device (the laser driver 130 and the scanning mechanism 150) in the laser processing system 100. Specifically, the control device 160 sets irradiation conditions (laser processing conditions) of the pulsed laser light L, and outputs a command to the laser driver 130 for realizing processing in accordance with the laser processing conditions. The control device 160 also outputs a command to the scanning mechanism 150 for scanning the pulsed laser light L.

[0041] Fig. 2 is a diagram showing a configuration of photothermal conversion element 1 according to embodiment 1. With reference to Fig. 2, photothermal conversion element 1 includes a substrate 11 and a metal thin film 12 disposed on substrate 11.

[0042] The substrate 11 is made of a material that does not affect photothermal conversion and thermoelectric conversion (described later) and is transparent to the pulsed laser light L (near-infrared light in this example) from the laser oscillator 120. Examples of such materials include quartz, silicon, and resin film. In this embodiment, a glass substrate (cover glass) is used as the substrate 11.

[0043] The material of the thin metal film 12 is preferably a material with high light-to-heat conversion efficiency in the wavelength range of light (white light WL in the example described below) irradiated to the thin metal film 12. In the example shown in Fig. 2, the thin metal film 12 is a gold thin film with a thickness on the order of nanometers. The gold thin film can be formed on the glass substrate by using a known method such as sputtering or electroless plating.

[0044] The thin metal film 12 does not have to be formed on the entire surface of the substrate 11, but may be formed on at least a part of the substrate 11. The material of the thin metal film 12 is not limited to gold, and may be silver or an alloy such as constantan as long as it is a material capable of generating photothermal conversion. The thin metal film 12 is an example of a "solid material" according to the present disclosure.

[0045] The metal thin film 12 includes a processed region LP that has been processed by irradiating the metal thin film 12 with a pulsed laser beam L. Although details will be described later, the processed region LP is a blackened region that includes metal nanoparticles that have been formed by atomizing the metal thin film 12 by the irradiation with the pulsed laser beam L (see FIG. 10).

[0046] FIG. 3 is a photograph of the fabricated photothermal conversion element 1. In the example shown in FIG. 3, the photothermal conversion element 1 includes two processing regions LP (processing regions LP1, LP2). Thus, the number of processing regions LP is not limited to one, and can be any number equal to or greater than two. The processing region LP may be formed in only a part of the metal thin film 12, or the entire surface of the metal thin film 12 may be laser processed to form the processing region LP over the entire surface. In FIG. 3, tape is attached to the top, bottom, left and right of the photothermal conversion element 1 to fix the photothermal conversion element 1.

[0047] FIG. 4 is a diagram showing the configuration of another photothermal conversion element 2 according to the first embodiment. FIG. 5 is a photograph of the fabricated photothermal conversion element 2. With reference to FIGS. 4 and 5, the photothermal conversion element 2 may be a metal plate. In other words, the substrate 11 as a base for forming the metal thin film 12 is not essential. In this example, the material of the photothermal conversion element 2 is a copper-nickel alloy. In particular, constantan, which is a copper alloy with a nickel content of about 40% to 50%, can be adopted. The metal plate made of constantan or the like is another example of the "solid material" according to the present disclosure. However, the "solid material" may be another thermoelectric material that exhibits a thermoelectric effect.

[0048] Like the metal thin film 12, the photothermal conversion element 2 includes a processed region LP formed by irradiating a metal material with a pulsed laser beam L. In the photograph shown in Fig. 5, the photothermal conversion element 2 is provided with two blackened processed regions LP3 and LP4.

[0049] <Laser processing conditions> Next, the irradiation conditions (laser processing conditions) of the pulsed laser light L for forming an appropriate processed region LP will be described. The laser processing conditions are defined by three parameters. Since the method for setting each parameter is common to both the photothermal conversion elements 1 and 2, the laser processing conditions for the photothermal conversion element 1 will be representatively described below.

[0050] Fig. 6 is a first diagram for explaining the laser processing conditions of the photothermal conversion element 1. Referring to Fig. 6, the first parameter that defines the laser processing conditions is the spot height H [μm]. The spot size of the pulsed laser light L (the radius of the pulsed laser light L) is smallest at the position of the beam waist. The spot height H is the distance on the optical axis between the beam waist and the upper surface of the photothermal conversion element 1 (the surface of the metal thin film 12 in the example shown in Fig. 6) with the position of the beam waist as the reference (H = 0).

[0051] 7 is a second diagram for explaining the laser processing conditions of the photothermal conversion element 1. The second parameter that defines the laser processing conditions is the scanning interval D [μm] of the pulsed laser light L. In this embodiment, the pulsed laser light L is scanned so that a plurality of parallel straight lines are arranged at regular intervals. The scanning interval D is the distance between a certain straight line and another straight line adjacent to the certain straight line. The size of the processing area LP where the laser processing is performed by the pulsed laser light L is several mm square (6 mm×6 mm in the example described later).

[0052] The third parameter that determines the laser processing conditions is the laser power P out [mW]. Laser power P out is the output of the pulsed laser light L after it has passed through the objective lens 140 (that is, at the position of the photothermal conversion element 1).

[0053] Spot height H, scan interval D and laser power P out The characteristics (optical characteristics and light-to-heat conversion characteristics) exhibited by the processed region LP can be adjusted by appropriately combining these three parameters. The measurement results of the characteristics of the processed region LP will be described in detail later.

[0054] <Production flow of photothermal conversion elements> 8 is a flowchart showing a method for manufacturing the photothermal conversion element 1 according to the first embodiment. This flowchart is executed when a predetermined condition is met (for example, when a user operates a start button, not shown). Each step included in this flowchart is basically realized by software processing by the control device 160, but some or all of the steps may be realized by hardware (electrical circuits) created within the control device 160. Hereinafter, steps are abbreviated as "ST".

[0055] 8, in ST1, the control device 160 sets the above three parameters (spot height H, scanning interval D, and laser output P) as the laser processing conditions. out) is set. More specifically, by conducting experiments in advance, an appropriate combination of the three parameters can be found depending on the type of photothermal conversion element 1 (material and thickness of metal thin film 12) and application, etc. Therefore, the control device 160 can select an appropriate combination depending on the type and application, etc. of the photothermal conversion element 1 from a plurality of combinations prepared in advance. Alternatively, the control device 160 may receive a user operation specifying a combination of the above three parameters from an input device (such as a mouse or keyboard) not shown.

[0056] In ST2, the control device 160 places the unprocessed photothermal conversion element 1 on the XYZ axis stage 110. This process can be realized, for example, by a feed mechanism (not shown) for the photothermal conversion element 1. The process of ST2 corresponds to the "preparation step" according to the present disclosure.

[0057] In ST3, the control device 160 outputs a command to the scanning mechanism 150 to control the height (position in the z direction) of the XYZ axis stage 110. In this way, the control device 160 adjusts the spot height H to the value set in ST1.

[0058] In ST4, the control device 160 controls the laser driver 130 to start (or continue) irradiation of the pulsed laser light L according to the laser processing conditions set in ST1. The control device 160 also controls the scanning mechanism 150 to scan with the pulsed laser light L according to a preset scanning pattern. The process in ST4 corresponds to the "fabricating step" according to the present disclosure.

[0059] In ST5, the control device 160 determines whether a predetermined end condition for laser processing is satisfied. The control device 160 determines that the end condition for laser processing is satisfied when drawing of the scan pattern is completed. If the end condition is not satisfied (NO in ST4), the control device 160 returns the process to ST4. This allows the irradiation of the pulsed laser light L to continue. If the end condition is satisfied (YES in ST5), the control device 160 advances the process to ST6.

[0060] In ST6, the control device 160 controls the laser driver 130 to stop the irradiation of the pulsed laser light L. Then, the control device 160 controls the feed mechanism of the photothermal conversion element 1 to remove the processed photothermal conversion element 1 from the XYZ axis stage 110 (ST7). This completes the series of processes.

[0061] [Example of the first embodiment] Next, we will explain the observation results and spectrum measurement results of the photothermal conversion elements 1 and 2 fabricated using the laser processing system 100. First, we will explain the evaluation results of the photothermal conversion element 1 (see Figures 2 and 3) in which a gold thin film formed on a glass substrate was laser processed. In this example, the gold thin film had a thickness of 100 μm.

[0062] 9 is a diagram showing the laser processing conditions for the photothermal conversion element 1 in the example of the embodiment 1. With reference to FIG. 9, the above-mentioned photothermal conversion element 1 was subjected to laser processing under four conditions 1A to 1D shown in FIG. 9. The laser output P out = 800 mW and scanning interval D = 50 μm are common to all conditions. On the other hand, the spot height H differs among conditions 1A to 1D. The pulse width of the pulsed laser light L was set to 400 fs, and the repetition frequency of the pulsed laser light L was set to 100 kHz.

[0063] FIG. 10 is a diagram showing the observation results of the photothermal conversion element 1 in the example of the first embodiment. FIG. 10 shows a scanning electron microscope (SEM) image of the photothermal conversion element 1 manufactured under conditions 1A to 1D described in FIG. 9. Referring to FIG. 10, in the image at a magnification of 350 times, the light-colored region (the region between two black lines) is the region irradiated with the pulsed laser light L. From the images at a magnification of 2,000 times or 5,000 times, gold particles were confirmed in the fine grooves formed by the irradiation of the pulsed laser light L under all of conditions 1A to 1D. The size (diameter) of most of the gold particles was in the range of several tens of nanometers to several hundreds of nanometers, but some gold particles had a size on the order of micrometers.

[0064] When light having a specific wavelength is irradiated onto gold nanoparticles (or gold microparticles), the free electrons of the gold nanoparticles form surface plasmons and vibrate with the resonant light. This causes polarization. The energy of this polarization is converted into lattice vibration energy through the Coulomb interaction between the free electrons and atomic nuclei. As a result, the gold nanoparticles generate heat. Hereinafter, this effect is also referred to as the "photothermal effect." By utilizing the photothermal effect of gold nanoparticles, it is possible to absorb light in a wide band and convert it into heat with high efficiency (see Figure 22 described later).

[0065] Fig. 11 is a diagram showing the measurement results of the absorbance spectrum of the photothermal conversion element 1 manufactured under condition 1A. Fig. 12 is a diagram showing the measurement results of the absorbance spectrum of the photothermal conversion element 1 manufactured under condition 1B. Fig. 13 is a diagram showing the measurement results of the absorbance spectrum of the photothermal conversion element 1 manufactured under condition 1C. Fig. 14 is a diagram showing the measurement results of the absorbance spectrum of the photothermal conversion element 1 manufactured under condition 1D.

[0066] In each of Figures 11 to 14, the upper part shows the results of localized measurement of the spectrum in the area above the black line (area not irradiated with the pulsed laser light L), and the lower part shows the results of localized measurement of the spectrum in the area between the black lines (area where gold nanoparticles were observed). In the area above the black line, a flat spectrum was obtained, similar to that of an unprocessed gold thin film. In contrast, in the area between the black lines, the spectrum was observed to be broad, and a peak due to the localized surface plasmon of the gold nanoparticles was confirmed at a wavelength of approximately 530 nm.

[0067] Thus, the absorbance spectrum of the region irradiated with the pulsed laser beam L is broadened and has a peak shift compared to the absorbance spectrum of a region not irradiated with the pulsed laser beam L or the absorbance spectrum obtained from a single metal nanoparticle. This spectral change indicates the following.

[0068] Gold nanoparticles can be densely assembled using only the physical process (non-chemical process) of irradiating pulsed laser light L. This enhances the interaction of the electronic system (localized surface plasmon, etc.) in each gold nanoparticle via the electromagnetic field, broadening the absorbance spectrum. As a result, compared to unprocessed solid materials or single microparticles, it becomes possible to convert a broadband of light into heat with high efficiency (enhanced photothermal effect). The blackening of the light irradiated area can be said to be an observable change from the outside that indicates the realization of an enhanced photothermal effect.

[0069] It should be noted that blackening does not occur simply by generating fine particles (gold nanoparticles in this example) from a solid material by irradiating it with laser light. Blackening occurs when the fine particles made of the solid material generated by irradiating it with laser light are densely accumulated, in other words, when the fine particles are close to each other but dispersed.

[0070] By cutting fine grooves by irradiating the pulsed laser light L, the surface area of ​​the gold thin film can be increased. This means that the area of ​​the region where the generated gold nanoparticles can be dispersed while still being close to each other (in other words, the area that serves as a receptacle for the gold nanoparticles densely accumulated) can be increased. Therefore, by cutting fine grooves, it is possible to further enhance the photothermal effect.

[0071] Next, the evaluation results of the photothermal conversion element 2 (see Figs. 4 and 5) obtained by laser processing of flat-plate constantan will be described. The thickness of the photothermal conversion element 2 was 500 µm.

[0072] 15 is a diagram showing laser processing conditions for another photothermal conversion element 2 in an example of embodiment 1. In this example, laser processing was performed according to five sets of conditions 2A to 2E shown in FIG.

[0073] Fig. 16 is a diagram showing the observation results of the photothermal conversion element 2 in the example of the embodiment 1. Referring to Fig. 16, it was confirmed that a large number of finely divided constantan particles were densely accumulated in the irradiation area of ​​the pulsed laser light L in the photothermal conversion element 2 as well. The size of most of the constantan particles was in the range from several tens of nanometers to several hundreds of nanometers.

[0074] Fig. 17 is a diagram showing the measurement results of the reflection spectrum of the photothermal conversion element 2 manufactured under conditions 2A to 2E. The upper part of Fig. 17 shows the reflection spectrum before laser processing (average of the measurement results of three samples) for comparison. The middle part shows the reflection spectrum after laser processing. The lower part shows enlarged views of the reflection spectra obtained under conditions 2B to 2D.

[0075] The reflectance of the photothermal conversion element 2 in the visible range (wavelength range of 400 nm to 800 nm) before laser processing was approximately within the range of 40% to 50%. On the other hand, when laser processing was performed, the reflectance of the photothermal conversion element 2 in the visible range became less than 10% under all of conditions 2A to 2E. Among them, the average reflectance (average reflectance in the visible range) of the photothermal conversion element 2 laser processed according to condition 2C was 0.42%. The average reflectance of the photothermal conversion element 2 laser processed according to condition 2D was 0.31%. It was also observed by visual inspection that the photothermal conversion element 2 after laser processing was blackened. Blackening by plating is known as a method for reducing the reflectance of a metal plate. The average reflectance of constantan blackened by plating is about 2%. Therefore, it can be said that the average reflectance obtained under conditions 2C and 2D is significantly lower than the average reflectance that can be achieved by plating. It is believed that these significant decreases in reflectance were caused by the fact that the absorbance spectrum of the densely packed constantan particles generated by laser processing became broadened and the peak shifted compared to the absorbance spectrum obtained from a single constantan particle.

[0076] In addition, the laser output P out is 400mW, while the laser output P out The laser output P is 800 mW (see FIG. 15). Since the average reflectance of the photothermal conversion element 2 after the laser processing according to conditions 2B to 2E is lower than the average reflectance of the photothermal conversion element 2 after the laser processing according to condition 2A, out It can be seen that the higher the value, the lower the average reflectance.

[0077] The average reflectance of the photothermal conversion element 2 laser-processed under conditions 2C and 2D is particularly low, less than 0.5%. Under conditions 2C and 2D, the scanning interval D of the pulsed laser light L is dense (D=50 μm), and the spot diameter of the pulsed laser light L is relatively large (spot height H>50 μm). From this, it is considered that the interval between the regions where constantan has been atomized is narrow, and the atomization of constantan has occurred over a wide area, which has led to the decrease in the average reflectance.

[0078] As described above, in the first embodiment, the processed region LP is formed in the photothermal conversion elements 1 and 2 by scanning with the pulsed laser beam L. The scanning with the pulsed laser beam L can be realized by using a general laser processing device that is easily available. As described with reference to FIG. 8, the manufacturing procedure of the photothermal conversion elements 1 and 2 does not include chemical treatment, and the time required to manufacture the photothermal conversion elements 1 and 2 is about 10 to 20 minutes. Furthermore, compared with the photothermal conversion element disclosed in Patent Document 1, it can be said to be easier in that it does not require the generation of a metal nanoparticle assembly structure. Thus, according to the first embodiment, the photothermal conversion elements 1 and 2 can be manufactured by a simple manufacturing method.

[0079] [Embodiment 2] In the second embodiment, a photothermal power generation device capable of generating power using the photothermal conversion elements 1 and 2 according to the first embodiment will be described.

[0080] Fig. 18 is a diagram showing a schematic overall configuration of a photothermal power generation device according to embodiment 2. Referring to Fig. 18, a white light source 91 is a light source that emits white light WL. The white light source 91 is, for example, the sun, but may be other light sources such as pseudo-sunlight illumination, an incandescent light bulb, a white LED (Light Emitting Diode), or a fluorescent lamp. Moreover, instead of the white light source 91, a monochromatic light source that emits light in a wavelength range included in the ultraviolet to near-infrared range may be used, or a light source that emits light in a plurality of wavelength ranges may be used.

[0081] The photothermal power generation device 200 generates power by utilizing white light WL from a white light source 91, and supplies the generated power to an electrical load 92. The photothermal power generation device 200 includes a photothermal conversion unit 210 and a thermoelectric conversion unit 220. The photothermal conversion unit 210 receives the white light WL from the white light source 91 and generates heat by a photoheating effect. The thermoelectric conversion unit 220 converts the thermal energy generated by the photothermal conversion unit 210 into electrical energy. That is, the thermoelectric conversion unit 220 generates power by using the heat from the photothermal conversion unit 210. This power is supplied to the electrical load 92.

[0082] The electric load 92 is an electric circuit or a motor, etc., but is not particularly limited as long as it is a device that consumes electric power. Although not shown, instead of the electric load 92, a power storage device (such as a secondary battery) that stores the electric power supplied from the photothermal power generation device 200 may be connected to the photothermal power generation device 200. The electric load 92 or the power storage device corresponds to the "load" according to the present disclosure.

[0083] Fig. 19 is a diagram showing an example of a more detailed configuration of the photothermal power generation device 200. Referring to Fig. 19, in this example, the photothermal conversion section 210 includes a photothermal conversion element 1. For the substrate 11 of the photothermal conversion element 1, for example, a conductive film (such as an ITO-PEN film) can be used.

[0084] Thermoelectric conversion unit 220 includes a P-type thermoelectric element 221, an N-type thermoelectric element 222, a heat sink 223, electrodes 231 to 234, and conductive pastes 241, 242A, 242B, 243, 244A, and 244B.

[0085] The P-type thermoelectric element 221 is thermally and electrically connected to the electrode 231 via the conductive paste 241. The electrode 231 is thermally and electrically connected to the substrate 11 (conductive film) of the photothermal conversion element 1. The P-type thermoelectric element 221 is thermally and electrically connected to the electrode 232 via the conductive paste 242A. The electrode 232 (first electrode) is thermally connected to the heat sink 223 via the conductive paste 242B, but is electrically insulated from the heat sink 223.

[0086] Like the P-type thermoelectric element 221, the N-type thermoelectric element 222 is thermally and electrically connected to the electrode 233 via the conductive paste 243. The electrode 233 is thermally and electrically connected to the substrate 11 of the photothermal conversion element 1. The N-type thermoelectric element 222 is thermally and electrically connected to the electrode 234 via the conductive paste 244A. The electrode 234 (second electrode) is thermally connected to the heat sink 223 via the conductive paste 244B, but is electrically insulated from the heat sink 223.

[0087] The heat sink 223 is made of an insulating material (for example, alumina).

[0088] White light WL emitted from a white light source 91 is irradiated onto the metal thin film 12 of the photothermal conversion element 1. This causes localized surface plasmon resonance of a plurality of particles (for example, gold nanoparticles or gold microparticles) in the processing region LP, enhancing heat generation (photothermal heat effect). The heat generated by the photothermal conversion element 1 is transferred to the P-type thermoelectric element 221 and the N-type thermoelectric element 222. Then, a temperature difference occurs between both ends of each of the P-type thermoelectric element 221 and the N-type thermoelectric element 222. More specifically, in the P-type thermoelectric element 221, the temperature of the side of the P-type thermoelectric element 221 closer to the photothermal conversion element 1 (the side of the electrode 231 and the conductive paste 241) increases with heating by the photothermal conversion element 1. On the other hand, the temperature of the side of the P-type thermoelectric element 221 closer to the heat sink 223 (the side of the conductive paste 242A, the electrode 232, and the conductive paste 242B) decreases due to heat dissipation from the heat sink 223. The same applies to the N-type thermoelectric element 222.

[0089] In the following, the side of the P-type thermoelectric element 221 or the N-type thermoelectric element 222 closer to the photothermal conversion element 1 is also referred to as the "high temperature side", and the side closer to the heat sink 223 is also referred to as the "low temperature side".

[0090] Inside the P-type thermoelectric element 221, holes diffuse and gather on the low temperature side. Therefore, in the P-type thermoelectric element 221, the potential on the low temperature side becomes higher than the potential on the high temperature side. On the other hand, inside the N-type thermoelectric element 222, electrons diffuse to the low temperature side. Therefore, in the N-type thermoelectric element 222, the potential on the low temperature side becomes lower than the potential on the high temperature side. As a result, a potential difference occurs between the low temperature side of the P-type thermoelectric element 221 and the low temperature side of the N-type thermoelectric element 222. Therefore, by connecting the electric load 92 between the electrode 232 and the electrode 234, a current can be taken out from the electrode 232 to the electric load 92. In this way, the photothermal power generation device 200 is configured to be able to convert light energy into thermal energy and further convert the thermal energy into electrical energy.

[0091] 19 shows a configuration in which the thermoelectric conversion unit 220 includes one P-type thermoelectric element 221 and one N-type thermoelectric element 222. However, the thermoelectric conversion unit 220 may include a plurality of pairs of the P-type thermoelectric element 221 and the N-type thermoelectric element 222.

[0092] FIG. 20 is a diagram showing another example of a more detailed configuration of the photothermal power generation device 200. Referring to FIG. 20, in this example, the photothermal conversion section 210 includes a photothermal conversion element 1 and a photothermal conversion element 2 (for example, a flat plate of constantan processed by laser). In this manner, the photothermal conversion element 1 and the photothermal conversion element 2 may be combined. Also, the photothermal conversion element 2 may be used in place of the photothermal conversion element 1. The electrode 233 connected to the photothermal conversion element 2 is electrically connected to the electrode 231 connected to the photothermal conversion element 1.

[0093] 20, the photothermal conversion element 2 also functions as an N-type thermoelectric element. That is, the photothermal conversion element 2 and the N-type thermoelectric element 222 are integrally configured, thereby realizing a "photothermal conversion thermoelectric element." Note that in this example, the photothermal conversion element 2 and the N-type thermoelectric element 222 are integrally configured, but depending on the material of the photothermal conversion element 2, the photothermal conversion element 2 and the P-type thermoelectric element 221 may also be integrally configured.

[0094] When the photothermal conversion element 1 and the N-type thermoelectric element 222 are separately configured as described in FIG. 19, the photothermal conversion element 1 and the N-type thermoelectric element 222 are thermally connected via the substrate 11. The thermal conductivity of the substrate 11 is lower than that of many metals. Specifically, the thermal conductivity of constantan is 23 [W / m·K], whereas the thermal conductivity of glass is 1.0 [W / m·K] and the thermal conductivity of a PET (polyethylene terephthalate) film is 0.20 to 0.33 [W / m·K]. Therefore, by integrally configuring the photothermal conversion element 2 and the N-type thermoelectric element without using the substrate 11, thermal energy can be transferred more efficiently than in a configuration in which the photothermal conversion element 1 and the N-type thermoelectric element 222 are separately configured.

[0095] <Light-to-heat conversion simulation> An estimate was made of the extent to which the temperature of the photothermal conversion element 2 included in the photothermal power generation device 200 would rise from room temperature when white light WL (sunlight) was irradiated onto the photothermal power generation device 200. The results will be described below.

[0096] 21 is a diagram for explaining the simulation conditions for the amount of temperature rise caused by the photoheating effect of the photothermal conversion element 2. With reference to FIG. 21, the irradiation time of the white light WL from the white light source 91 is set to t [s], and the illuminance of the white light WL (sunlight in this example) is set to P(λ) [W / m 2 The area of ​​the surface of the photothermal conversion element 2 irradiated with the white light WL (the area of ​​the processing area LP) is S [m 2 ], where λ [m] is the wavelength of the white light WL.

[0097] Furthermore, the absorptance of white light WL by the photothermal conversion element 2 is defined as A(λ) [%]. The absorptance A is expressed as A=1-RT using reflectance R and transmittance T. When the photothermal conversion element 2 is a flat plate of constantan, the transmittance T is 0, so the absorptance A can be approximated as 1-R. Therefore, the absorptance A can be calculated from the measurement results of the reflectance R of the photothermal conversion element 2 (see FIG. 17).

[0098] In this case, the amount of heat absorption Q [J] by the photothermal conversion element 2 is calculated according to the following formula (1).

[0099]

number

[0100] Furthermore, if the specific heat of the photothermal conversion element 2 is C [J / k g] and the mass of the photothermal conversion element 2 is m [g], the temperature rise of the photothermal conversion element 2 based on room temperature (25°C) is T up [K] can be calculated using the following formula (2).

[0101] T up = Q / (C × m) (2) In this simulation, the irradiation time of the white light WL was set to t = 120 [s]. The area S of the irradiation surface of the photothermal conversion element 2 was set to 3.2 × 10 -4 [m 2 The specific heat of the photothermal conversion element 2, C, was set to 0.41 [J / g K], and the mass of the photothermal conversion element 2, m, was set to 1.4 [g].

[0102] FIG. 22 shows the temperature rise T up 22 shows the results of a simulation of the temperature rise in an unprocessed constantan substrate (a substrate on which no processed region LP is provided) calculated for a comparative example, which was about 27°C. In contrast, in the photothermal conversion element 2 that was laser processed, the temperature rise T up was over 45°C.

[0103] 21 and 22 have described an example in which a photothermal conversion element 2 is used. However, a photothermal conversion element 1 (see Figs. 2 and 3) may be used instead of the photothermal conversion element 2. Heat can also be generated with high efficiency by irradiating light onto the metal thin film 12 provided on the photothermal conversion element 1 due to the photoheating effect.

[0104] <Photo-thermoelectric conversion simulation> Next, a simulation result of the generated power (output power) in the photothermal power generation device 200 when the photothermal power generation device 200 is irradiated with white light WL (sunlight) will be described.

[0105] Fig. 23 is a diagram for explaining the simulation conditions for the amount of power generated by photothermal power conversion (photothermal conversion and thermoelectric conversion) in the photothermal power generation device 200. With reference to Fig. 23, the material properties of the P-type thermoelectric element 221 and the N-type thermoelectric element 222 were set as follows.

[0106] Seebeck coefficient S(T) of N-type thermoelectric element 222 = -40 × 10 -6 ~-36×10 -6[V / K]. Electrical resistivity ρ = 0.44 × 10 -6 ~0.46×10 -6 The thermal conductivity κ was set to 23–27 [W / m K]. This thermal conductivity κ is two orders of magnitude higher than the thermal conductivity of PET film (≒0.20–0.33 [W / m K]).

[0107] Similarly, the Seebeck coefficient S(T) for the P-type thermoelectric element 221 is 1.7×10 -6 ~2.4×10 -6 [V / K]. Electrical resistivity ρ = 17×10 -9 ~24×10 -9 The thermal conductivity was set to κ = 400 [W / m K].

[0108] Regarding the thermal conditions, the temperatures of the P-type thermoelectric element 221 and the N-type thermoelectric element 222 are the temperature rise amounts T up Calculated using (Temperature = Room temperature + Temperature rise T up The heat flux input to and output from the P-type thermoelectric element 221 and the N-type thermoelectric element 222 was calculated by dividing the amount of heat absorption Q (see formula (1)) by the area S of the surface irradiated with the white light WL.

[0109] Furthermore, each of the P-type thermoelectric element 221 and the N-type thermoelectric element 222 was formed into a rectangular parallelepiped shape. The cross-sectional area (=area S) of the rectangular parallelepiped was set to 1×3 [mm 2 ] and the height of the rectangular prism was set to 4 [mm].

[0110] Fig. 24 is a diagram showing the results of a simulation of the amount of power generated in the photothermal power generation device 200. In Fig. 24, the horizontal axis represents the output current from the photothermal power generation device 200. The vertical axis on the left represents the output voltage from the photothermal power generation device 200, and the vertical axis on the right represents the output power from the photothermal power generation device 200. As shown in Fig. 24, the photothermal power generation device 200 produced results showing that the output power was more than three times higher than that of the case where an unprocessed constantan substrate was used (comparative example).

[0111] As described above, according to the photothermal power generation device 200 of the second embodiment, by using the photothermal conversion section 210 including the laser-processed photothermal conversion element 2 (which may be the photothermal conversion element 1), it is possible to convert light into heat with high efficiency, as compared to a comparative example in which laser processing is not performed, and the amount of heat generated by the photothermal conversion element 2 can be increased (see FIG. 22). Furthermore, by converting the increased heat into electricity by the thermoelectric conversion section 220, the generated power can be increased (see FIG. 24). Thus, according to the second embodiment, light can be converted into electricity with high efficiency.

[0112] [Embodiment 3] In embodiment 3, a micro-object accumulation system that accumulates a plurality of micro-objects contained in a liquid will be described using the photothermal conversion element 1 according to embodiment 1. In the following example, beads (microbeads) having a size on the order of micrometers are accumulated.

[0113] Fig. 25 is a diagram showing an overall configuration of an integration system for micro objects according to embodiment 3. Referring to Fig. 25, integration system 300 includes XYZ axis stage 310, adjustment mechanism 320, laser light source 330, illumination light source 340, optical component 350, objective lens 360, camera 370, and control device 380.

[0114] The XYZ axis stage 310 is configured to hold the photothermal conversion element 1. The XYZ axis stage 310 corresponds to the "holder" according to the present disclosure.

[0115] Fig. 26 is an enlarged view of the photothermal conversion element 1 held on the XYZ axis stage 310. As shown in Fig. 26, a sample SP is dropped onto the photothermal conversion element 1. Microbeads B are dispersed in the sample SP. In one embodiment (see Fig. 27), the material of the microbeads B is polystyrene, and the diameter of the microbeads B is 1 µm. The dispersion medium of the sample SP is pure water.

[0116] Returning to FIG. 25, the adjustment mechanism 320 adjusts the position of the XYZ axis stage 310 in the x, y, and z directions in response to a command from the control device 380. In this embodiment, the position of the objective lens 360 is fixed. Therefore, by adjusting the position of the XYZ axis stage 310, the relative positional relationship between the photothermal conversion element 1 and the objective lens 360 is adjusted. The adjustment mechanism 320 may adjust the position of the objective lens 360 with respect to the fixed photothermal conversion element 1.

[0117] The laser light source 330 emits a laser light L1 in response to a command from the control device 380. The wavelength of the laser light L1 is, for example, a wavelength included in the near infrared region (1064 nm in this embodiment). The laser light source 330 corresponds to the "light source" according to the present disclosure.

[0118] The illumination light source 340 emits white light L2 for illuminating the sample SP on the photothermal conversion element 1 in response to a command from the control device 380. As an example, the illumination light source 340 can be a halogen lamp.

[0119] The optical component 350 includes, for example, a mirror, a dichroic mirror, a prism, an optical fiber, etc. The optical system of the integrated system 300 is adjusted so that the laser light L1 from the laser light source 330 is guided to the objective lens 360 by the optical component 350.

[0120] The objective lens 360 collects the laser light L1 from the laser light source 330. The light collected by the objective lens 360 is irradiated onto the sample SP on the photothermal conversion element 1. The objective lens 360 is also used to capture white light L2 irradiated onto the photothermal conversion element 1 from the illumination light source 340. The white light L2 collected by the objective lens 360 is guided to the camera 370 by the optical component 350.

[0121] In response to a command from the control device 380, the camera 370 captures an image of the sample SP on the photothermal conversion element 1 irradiated with the white light L2, and outputs the captured image to the control device 380.

[0122] The control device 380 is a microcomputer including a processor such as a CPU, memories such as a ROM and a RAM, and input / output ports, all of which are not shown in the figure. The control device 380 controls each device in the integrated system 300 (the adjustment mechanism 320, the laser light source 330, the illumination light source 340, and the camera 370).

[0123] The thickness of the metal thin film 12 is determined so that the processing area LP has optical transparency to the laser light L1. In the following example, the thickness of the gold thin film was 100 nm. By making the processing area LP optically transparent in this way, it becomes possible to irradiate the processing area LP with the laser light L1 from below to above the processing area LP as shown in FIG. 25, and it becomes possible to observe the state of the processing area LP from below with a camera 270.

[0124] FIG. 27 is a photograph of the state of the sample SP when irradiated with the laser light L1. The photothermal conversion element 1 was prepared under the four laser processing conditions described in FIG. 9 and FIG. 10. The output P of the laser light L1 irradiated to the photothermal conversion element 1 was out The power of the objective lens 360 was 50 mW. The magnification of the objective lens 360 was 40. The irradiation time of the laser light L1 was 100 seconds.

[0125] The generation of microbubbles MB was confirmed by irradiating the area between the black lines, where gold nanoparticles (gold microparticles can also be generated) were observed by irradiating with pulsed laser light L1. In addition, the accumulation of microbeads B toward the microbubbles MB was observed. The accumulation mechanism of microbeads B can be explained as follows.

[0126] Fig. 28 is a conceptual diagram for explaining the accumulation mechanism of microbeads B. Referring to Fig. 28, when irradiation of laser light L1 is started, the area near the laser spot is locally heated due to the photothermal effect. When the temperature of the liquid (sample SP) around this heated area rises, microbubbles MB are generated. The microbubbles MB grow near the laser spot over time.

[0127] The closer to the laser spot, the higher the temperature of the liquid. In other words, light irradiation creates a temperature gradient in the liquid. This temperature gradient causes regular thermal convection to steadily occur in the liquid. The direction of the thermal convection is toward the laser spot and then away from the laser spot, as shown by the arrow AR. Therefore, microbead B is carried by the thermal convection toward the laser spot.

[0128] Between the microbubbles MB and the metal thin film 12, a ring-shaped "stagnation region" where the convection flow rate is zero is generated. As the thermal convection is blocked by the microbubbles MB, some of the microbeads B carried toward the laser spot are retained near the stagnation region. As a result, the microbeads B are accumulated near the laser spot. For details of the accumulation mechanism of the microbeads B, refer to, for example, Patent Document 2 or Patent Document 3.

[0129] As described above, in the third embodiment, the photothermal conversion element 1 generates microbubbles MB and generates convection currents by using the photothermal conversion element 1's photoheating effect. This convection current causes a plurality of microbeads B dispersed in the sample SP to accumulate in a stagnation region that occurs below the microbubbles MB. By utilizing this mechanism, a large number of microbeads B can be accumulated with high efficiency.

[0130] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, not by the description of the embodiments described above, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0131] 1,2 Photothermal conversion element, 11 Substrate, 12 Metal thin film, 91 White light source, 92 Electric load, 100 Laser processing system, 110 XYZ axis stage, 120 Laser oscillator, 130 Laser driver, 140 Objective lens, 150 Scanning mechanism, 160 Control device, 200 Photothermal power generation device, 210 Photothermal conversion unit, 220 Thermoelectric conversion unit, 221 P-type thermoelectric element, 222 N-type thermoelectric element, 223 Heat sink, 231-234 Electrode, 241, 242A, 242B, 243, 244A, 244B Conductive paste, 300 Integrated system, 310 XYZ axis stage, 320 Adjustment mechanism, 330 Laser light source, 340 Illumination light source, 350 Optical component, 360 Objective lens, 370 Camera, 380 Control device, LP, LP1~LP4 processing area.

Claims

1. Providing a solid material; and forming a processed region by irradiating the solid material with laser light, The forming step includes a step of particulating the solid material so that the processed area is blackened; the processing region includes a plurality of integrated particles made of the solid material; The method for manufacturing a photothermal conversion element includes irradiating the plurality of particles with light to generate localized surface plasmon resonance on a surface of each of the plurality of particles.

2. The method for manufacturing a photothermal conversion element according to claim 1 , wherein the forming step includes a step of scanning the laser light so as to cut a fine groove in the processing region.

3. The method for producing a photothermal conversion element according to claim 1 , wherein the solid material includes at least one of a thermoelectric material exhibiting a thermoelectric effect and a metal thin film.

4. A solid material is provided, the solid material includes a region in which the solid material is blackened by accumulation of a plurality of fine particles made of the solid material; A photothermal conversion element in which the plurality of particles generate localized surface plasmon resonance on a surface of each of the plurality of particles when irradiated with light.

5. The photothermal conversion element according to claim 4 , wherein the solid material includes at least one of a thermoelectric material exhibiting a thermoelectric effect and a metal thin film.

6. A photothermal power generation device capable of supplying generated power to a load, The photothermal conversion element according to claim 4 or 5, a thermoelectric conversion unit that is thermally connected to the photothermal conversion element and converts heat into electricity; The thermoelectric conversion unit is A P-type thermoelectric element; A first electrode electrically connected to the low temperature side of the P-type thermoelectric element; An N-type thermoelectric element; a second electrode electrically connected to the low temperature side of the N-type thermoelectric element; The first electrode and the second electrode are connected to the load.

7. The photothermal power generation device according to claim 6 , wherein the photothermal conversion element and one of the P-type thermoelectric element and the N-type thermoelectric element are integrally configured as a photothermal conversion thermoelectric element.

8. A substrate; a thin metal film disposed on the substrate; the metal thin film includes a region in which the metal thin film is blackened by dispersing a plurality of fine particles made of a material of the metal thin film; A photothermal conversion element in which the plurality of particles generate localized surface plasmon resonance on a surface of each of the plurality of particles when irradiated with light.

9. A micro-object accumulation system for accumulating a plurality of micro-objects contained in a liquid, comprising: A holder configured to hold the photothermal conversion element according to claim 8; a light source that emits light that generates localized surface plasmon resonance on a surface of each of the plurality of microparticles, The light source accumulates the plurality of micro-objects by irradiating the region with light while the liquid is held above the region, thereby generating convection in the liquid.

10. the liquid is held on an upper surface of the region; The light from the light source is emitted from below to above the area, 10. The system for integrating minute objects according to claim 9, wherein the thickness of the thin metal film is determined so that the region is optically transparent to light from the light source.

Citation Information

Patent Citations

  • Formation method of high adhesiveness metal nanoparticle sintered compact film

    JP2009283783A

  • Photothermal conversion element and method of manufacturing the same, photothermal power generation device, and method of detecting material to be detected

    JP2013254940A

  • Collection device of micro object, collection kit, and collection method of the micro object

    JP2017202446A

  • Accumulation device and accumulation method, manufacturing device for microscopic object accumulation structural body, microscopic organism accumulation and elimination device, detection-substance detection device, separation-substance separation device, and introduction-substance introduction device

    WO2015170758A1

  • Low-voltage fuse production method and low-voltage fuse

    WO2017037876A1