Optical film, optical laminate, functional glass and head-up display
The optical film with a block layer and thermoplastic resin stabilizes the retardation value, addressing double image issues and enhancing HUD performance by maintaining optical stability under varying conditions.
Patent Information
- Application Number
- JP2021146303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-23
- Filing Date
- 2021-09-08
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-08-12
AI Technical Summary
Existing head-up displays (HUDs) suffer from double image issues due to the reflection of display light by two surfaces of the windshield, and the retardation value of retardation elements in automobile windshields changes under varying environmental conditions, affecting optical performance.
An optical film with a block layer containing a thermoplastic resin and an ultraviolet curable resin is used to stabilize the retardation value, maintaining optical performance even in high-temperature conditions, and includes a support substrate and optical functional layers like 1/2 wavelength plates to enhance durability and reduce double images.
The optical film maintains stable optical performance and durability, reducing double images and improving visibility in HUD systems, especially under high-temperature conditions.
Smart Images

Figure 0007572927000010 
Figure 0007572927000011 
Figure 0007572927000012
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film suitable for use in, for example, a head-up display, an optical laminate and functional glass using the same, and also to a head-up display using these. [Background technology]
[0002] Navigation systems, head-up displays (hereinafter also referred to as "HUD"), etc. are used as methods for displaying information to drivers of automobiles, aircraft, etc. HUD is a system that projects an image projected from an image projection means such as a liquid crystal display (hereinafter also referred to as "LCD") onto, for example, the windshield of an automobile.
[0003] The light emitted from the image display means is reflected by a reflector and then by the windshield before reaching the observer. The observer sees the image projected onto the windshield, but the image appears to be located at a position farther away than the windshield. This method allows the driver to obtain various information while gazing at the road ahead through the windshield with almost no movement of the eyes, making it safer than conventional car navigation systems that require the driver to move their eyes.
[0004] In HUD systems, the displayed information is projected and superimposed on the view actually seen through the windshield. However, because the displayed light is reflected by two surfaces, one on the inside and one on the outside of the windshield, the reflected image appears as a double image, making the displayed information difficult to see.
[0005] It is known that the problem of reflected double images can be improved by using a phase difference element that can change the polarization direction by 90° on an automobile windshield. For example, Patent Document 1 discloses that when S-polarized display light is incident at Brewster's angle on an automobile windshield equipped with a film-like optical rotator inside, part of the S-polarized light is reflected on the surface of the windshield on the inside of the vehicle, the S-polarized light that passes through the surface is converted to P-polarized light by the optical rotator, and all of the P-polarized light is emitted outside the vehicle on the surface of the windshield on the outside of the vehicle, thereby preventing double images.
[0006] On the other hand, in such automobile windshields, the phase difference value of the phase difference element is important for the phase difference element to perform appropriate polarization conversion at a desired wavelength, but there is a problem that the phase difference value changes under various environmental conditions, for example, under a high temperature atmosphere, a high temperature and high humidity atmosphere, etc.
[0007] To solve this problem, for example, Patent Document 2 discloses a technology that uses a blocking layer that prevents degradation factors from reaching the light reflective layer. However, the durability (mainly heat resistance) required for the blocking layer, and the appearance and adhesion when used in laminated glass are not disclosed in detail. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 6-40271 [Patent Document 2] JP 2017-198981 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention aims to provide an optical film that is excellent in durability, exhibits little change in the retardation value of a retardation element in a high-temperature atmosphere, and can maintain stable optical performance, as well as an optical laminate, functional glass, and a head-up display system that use the optical film. [Means for solving the problem]
[0010] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and found that providing an optical film with a block layer containing a thermoplastic resin makes it possible to maintain stable optical performance even in a high-temperature atmosphere and to provide the optical film with excellent durability, thereby completing the present invention.
[0011] That is, the present invention relates to the following 1) to 14). 1) An optical film comprising (A) an optical functional layer and (B) a blocking layer, The optical film, wherein the (B) blocking layer has a cured product of a resin composition containing (B-1) a thermoplastic resin and (B-2) an ultraviolet-curable resin. 2) The optical film according to the above 1), wherein the thermoplastic resin (B-1) is a polyvinyl acetal resin. 3) The optical film according to the above 1) or 2), wherein the thermoplastic resin (B-1) is a thermoplastic resin having a molecular weight of 10,000 or more and 60,000 or less. 4) The optical film according to any one of 1) to 3) above, wherein the thermoplastic resin (B-1) is a polyvinyl acetoacetal resin. 5) The optical film according to any one of 1) to 4) above, wherein the content of the thermoplastic resin (B-1) in the block layer is from 1% by mass to 80% by mass. 6) The optical film according to any one of 1) to 5) above, wherein the ultraviolet-curable resin (B-2) is a resin having a (meth)acryloyl group. 7) 7. The optical film according to 6) above, wherein the resin having a (meth)acryloyl group is an epoxy (meth)acrylate resin. 8) The optical film according to any one of 1) to 7) above, wherein the blocking layer (B) has a glass transition temperature of 80° C. or higher and 300° C. or lower. 9) The optical film according to any one of 1) to 8) above, wherein the optical functional layer (A) is any one of the following (A-1) to (A-4). (A-1) 1 / 2 wavelength plate, (A-2) 1 / 4 wavelength plate, (A-3) A laminate of a half-wave plate and a circularly polarized light reflective layer, and (A-4) Laminate of a quarter-wave plate and a circularly polarized light reflective layer 10) The optical film according to 9) above, wherein the half-wave plate or the quarter-wave plate contains a polymerizable liquid crystal layer as a layer having a function of converting a polarization axis. 11) The optical film according to any one of 1) to 10) above, further comprising (C) a supporting substrate. 12) An optical laminate comprising an intermediate film laminated on the optical film according to any one of 1) to 11) above. 13) A functional glass comprising the optical laminate according to 12) above and a glass plate. 14) A head-up display system comprising the optical film according to any one of 1) to 11), the optical laminate according to 12), or the functional glass according to 13), and an image display means for emitting display light showing an image display. Effect of the Invention
[0012] According to the present invention, it is possible to provide an optical film that is excellent in durability, exhibits little change in the retardation value of a retardation element in a high-temperature atmosphere, and can maintain stable optical performance, as well as a functional glass, an optical laminate, and a head-up display system using the same. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram showing an embodiment of a head-up display system according to the present invention. [Diagram 2] FIG. 11 is a schematic diagram showing another embodiment of a head-up display system according to the present invention. [Diagram 3] 1 is a side cross-sectional view showing one embodiment of an optical film according to the present invention. [Figure 4] 1 is a side cross-sectional view showing one embodiment of an optical laminate according to the present invention. [Diagram 5] FIG. 1 is a side cross-sectional view showing one embodiment of functional glass according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments according to the present invention will be described with reference to the drawings. Note that the following embodiments merely exemplify some representative embodiments of the present invention, and various modifications can be made within the scope of the present invention. In addition, in the following, terms such as "(meth)acryloyl" mean "acryloyl" or "methacryloyl", and for example, "(meth)acrylate" means "acrylate" or "methacrylate". In addition, the superscript "RTM" means a registered trademark.
[0015] The optical film of the present invention includes an optical functional layer (A) and a blocking layer (B). Fig. 3 shows one embodiment of the optical film of the present invention, and the optical film 10 has a configuration in which an optical functional layer 101 and a blocking layer 102 are laminated. In Fig. 3, the blocking layer 102 is laminated on one surface of the optical functional layer 101, but the blocking layer 102 may be laminated on both surfaces of the optical functional layer 101. In addition, when the blocking layer 102 is laminated on one surface of the optical functional layer 101, it is preferable that a supporting substrate (C) described later is provided on the other surface of the optical functional layer 101.
[0016] [(A) Optical functional layer] The optical functional layer used in the present invention is not particularly limited as long as it has the function of converting the polarization axis of incident light, and can be appropriately designed to obtain the desired polarized light. For example, a retardation element such as a 1 / 2 wavelength plate or a 1 / 4 wavelength plate, a laminate of a plurality of such retardation elements, or a laminate of a retardation element and a circularly polarized light reflective layer can be mentioned. Specifically, (A-1) 1 / 2 wavelength plate, (A-2) 1 / 4 wavelength plate, (A-3) a laminate of a 1 / 2 wavelength plate and a circularly polarized light reflective layer, or (A-4) a laminate of a 1 / 4 wavelength plate and a circularly polarized light reflective layer can be exemplified, but for example, when the optical film is used in the above-mentioned HUD system, it is preferable to use a 1 / 2 wavelength plate.
[0017] When a half-wave plate is used as the optical functional layer, the half-wave plate is a retardation element that converts P-polarized light into S-polarized light or S-polarized light into P-polarized light, i.e., converts the polarization axis. For example, the half-wave plate can be obtained by uniaxially stretching a film made of polycarbonate or cycloolefin polymer so that the retardation is 1 / 2 of the wavelength, or by orienting a horizontally oriented polymerizable liquid crystal to a thickness such that the retardation is 1 / 2 of the wavelength. In general, a half-wave plate using a horizontally oriented polymerizable liquid crystal is composed of a polymerizable liquid crystal layer as a layer that has the function of converting the polarization axis, and a support substrate on which a coating liquid that forms the polymerizable liquid crystal layer is applied. The upper limit of the thickness of such a half-wave plate is preferably 10 μm or less from the viewpoint of the orientation of the liquid crystal, and more preferably 5 μm or less. On the other hand, the lower limit of the thickness of the half-wave plate is preferably 0.3 μm or more from the viewpoint of the polymerizability of the liquid crystal, and more preferably 0.5 μm or more. When light is incident on the main surface of the half-wave plate from an oblique position, the phase difference may change depending on the incident angle of the light. In such a case, in order to more strictly match the phase difference, for example, a phase difference element whose refractive index is adjusted can be used to suppress the change in phase difference associated with the incident angle. For example, when the refractive index in the slow axis direction in the plane of the phase difference element is nx, the refractive index in the direction perpendicular to nx in the plane of the phase difference element is ny, and the refractive index in the thickness direction of the phase difference element is nz, the coefficient Nz shown in the following formula (1) is preferably controlled to be 0.3 or more and 1.0 or less, more preferably 0.5 or more and 0.8 or less.
[0018]
number
[0019] When an optical film using such a half-wave plate is provided in the functional glass of the present invention described later and the functional glass is applied to a HUD system, in order to efficiently convert P polarized light to S polarized light or S polarized light to P polarized light in the HUD system, it is preferable to control the angle θ between the polarization axis of S polarized light or the polarization axis of P polarized light incident from a position tilted at 45° to 65° from the axis perpendicular to the surface of the functional glass and the slow axis of the half-wave plate to 35° to 47°. By setting the incident angle of S polarized light or P polarized light incident on the half-wave plate to a range of 45° to 65°, when P polarized light is incident on the functional glass, the reflectance on the surface of the functional glass can theoretically be suppressed to 2% or less. The transmitted P polarized light is converted to S polarized light by the half-wave plate, and the converted S polarized light is reflected at the interface between the incident side and the air of the functional glass on the opposite side. The reflected S polarized light is converted again to P polarized light by the half-wave plate, and this P polarized light reaches the observer. In addition, when S-polarized light is incident on the functional glass, it is reflected on the surface of the functional glass, and this S-polarized light reaches the viewer. A part of the S-polarized light that passes through is converted to P-polarized light by the half-wave plate, and the converted P-polarized light passes through without being reflected by the functional glass on the opposite side to the incident side or the interface between the functional glass and air. In this way, the occurrence of double images can be suppressed by controlling the incident angle of S-polarized light or P-polarized light that is incident on the functional glass. In addition, if the angle θ is less than 35° or greater than 47°, the polarization axis conversion performance of converting P-polarized light incident on the functional glass to S-polarized light or S-polarized light to P-polarized light is low, and as a result, the image displayed on the display may become dark. By appropriately controlling this angle θ, the half-wave plate exhibits good polarization axis conversion performance, and as a result, the displayed image becomes clearer.
[0020] In order to appropriately control the conversion performance of the polarization axis exhibited by the half-wave plate, the angle θ is preferably a value calculated from the following formulas (2) and (3). Here, the technical significance of the following formulas (2) and (3) will be explained. When S-polarized or P-polarized light incident on the functional glass passes through the half-wave plate, which is a medium having a refractive index different from that of air, the angle of incidence at which the light is incident on the half-wave plate changes. Here, if the angle of incidence of the S-polarized or P-polarized light on the functional glass is α, the angle of incidence that actually enters the half-wave plate, i.e., the refraction angle of the half-wave plate is β, the refractive index of air is nαα, and the refractive index of the half-wave plate is nβ, then according to Snell's law, sinα / sinβ=nβ / nα holds, and by simplifying this formula into an equation for finding β, formula (3) is derived. On the other hand, when the polarization axis of S-polarized light incident on the functional glass is the x-axis, the polarization axis of P-polarized light is the y-axis, and the angle between the y-axis and the slow axis of the half-wave plate is θ, the phase difference value is Re. In vector analysis, the y-axis is expressed as Re·cosθ and the x-axis is expressed as Re·sinθ. Here, It is known that the polarization axis conversion performance of a long plate is maximized when light is incident at 45° to the slow axis of the half-wave plate, so theoretically, it is desirable for the incident angle to the slow axis of the half-wave plate to be 45°. However, as mentioned above, even if the incident angle of S-polarized or P-polarized light incident on the functional glass is θ, the actual incident angle to the half-wave plate is β. Therefore, when the y-axis (theoretical y-axis) of Re·cosθ is inclined at an angle β around the x-axis, the y-axis (effective y-axis) is calculated, Re·cosθ / effective y-axis = sin(90°-β), and the effective y-axis is expressed as Re·cosθcosβ. In order to make the angle between the polarization axis of S-polarized or P-polarized light incident on the functional glass and the slow axis of the half-wave plate the desired incident angle of 45°, the x-axis (Re·sinθ) and the effective y-axis (Re ·cosθcosβ) must be equal. Therefore, Re·sinθ=Re·cos By calculating θcosβ and simplifying this equation, we obtain equation (2). In this way, by strictly controlling the angle θ in relation to the angle β at which the light actually enters the 1 / 2 polarizing plate based on the values calculated from equations (2) and (3) below, we can maximize the polarization axis conversion performance of the 1 / 2 wave plate.
[0021]
number
[0022] The range of the angle θ is preferably controlled within a range of ±5° of the value of the angle θ, and more preferably within a range of ±3°. If the angle θ is outside the range of ±5° of the angle that satisfies the value calculated from the formulas (2) and (3), the efficiency of the conversion of the polarization axis from P polarization to S polarization exhibited by the half-wave plate decreases. By controlling the range of the angle θ based on the value calculated from the formulas (2) and (3), it is possible to suppress a decrease in the efficiency of the conversion of the polarization axis from P polarization to S polarization exhibited by the half-wave plate.
[0023] The refractive index of the half-wave plate substituted into formula (3) is the average refractive index obtained by averaging the sum of nx, ny, and nz, which are the refractive index in the direction perpendicular to nx in the plane of the half-wave plate, and nz, respectively. When using a commercially available half-wave plate, the average refractive index can be the value listed in a catalog or the like. When using a polymerizable liquid crystal, which will be described later, as the material for the half-wave plate, the average refractive index can be expressed as (nx + ny + nz) / 3=(no+ne) / 2, using the ordinary refractive index no and extraordinary refractive index ne of the liquid crystal. A specific example of θ calculated from formulas (2) and (3) is as follows: for example, when the refractive index of air is 1.00, a ½ wavelength plate with a refractive index of 1.55 is used, and the incident angle of S-polarized or P-polarized light is 45°, the value of θ is 42° based on formulas (2) and (3), so the range of θ is preferably 37° to 47°, more preferably 39° to 45°. When the incident angle of S-polarized or P-polarized light is 50°, the value of θ is 41° based on formulas (2) and (3), so the range of θ is preferably 36° to 46°, more preferably 38° to 44°. When the incident angle of S-polarized or P-polarized light is 56°, the value of θ is 40° based on formulas (2) and (3), so the range of θ is preferably 35° to 45°, more preferably 37° to 43°. Furthermore, when the incident angle of S-polarized or P-polarized light is 65°, the value of θ is 39° based on formulas (2) and (3), so the range of θ is preferably 34° to 44°, and more preferably 36° to 42°. By controlling the angle between the polarization axis of S-polarized or P-polarized light incident from a position tilted at an angle of 45° to 65° from the axis perpendicular to the surface of the functional glass and the slow axis of the half-wave plate to 35° to 47°, the half-wave plate exhibits good polarization axis conversion performance, and as a result, a HUD system can be provided in which the displayed image is more clearly visible.
[0024] As described above, in the present invention, the polarization axis conversion performance of the half-wave plate can be improved by controlling the angle θ between the polarization axis of P-polarized or S-polarized light incident on the functional glass and the slow axis of the half-wave plate. In such a case, from the viewpoint of controllability of the slow axis of the half-wave plate and production costs, it is particularly preferable to use a half-wave plate including a polymerizable liquid crystal layer as a layer having the function of converting the polarization axis.
[0025] A polymerizable liquid crystal is a nematic liquid crystal monomer that has a polymerizable group in the molecule and exhibits liquid crystallinity in a certain temperature range or concentration range. Examples of the polymerizable group include (meth)acryloyl group, vinyl group, chalconyl group, cinnamoyl group, and epoxy group. In addition, in order for the polymerizable liquid crystal to exhibit liquid crystallinity, it is preferable that the polymerizable liquid crystal has a mesogenic group in the molecule. The mesogenic group means, for example, a rod-shaped or plate-shaped substituent such as a biphenyl group, a terphenyl group, a (poly)benzoic acid phenyl ester group, a (poly)ether group, a benzylideneaniline group, or an acenaphthoquinoxaline group, or a disc-shaped substituent such as a triphenylene group, a phthalocyanine group, or an azacrown group, that is, a group that has the ability to induce liquid crystal phase behavior. Liquid crystal compounds having rod-shaped or plate-shaped substituents are known in the art as calamitic liquid crystals. Examples of such nematic liquid crystal monomers having a polymerizable group include the polymerizable liquid crystals described in JP-A-2003-315556 and JP-A-2004-29824, the PALIOCOLOR series (manufactured by BASF) and the RMM series (manufactured by Merck), etc. These nematic liquid crystal monomers having a polymerizable group may be used alone or in combination.
[0026] Furthermore, it is also possible to add a polymerizable compound that does not have liquid crystallinity but is capable of reacting with a nematic liquid crystal monomer having a polymerizable group, such as an ultraviolet-curable resin. Examples of ultraviolet curable resins include dipentaerythritol hexa(meth)acrylate, a reaction product of dipentaerythritol penta(meth)acrylate and 1,6-hexamethylene diisocyanate, a reaction product of a triisocyanate having an isocyanuric ring and pentaerythritol tri(meth)acrylate, a reaction product of pentaerythritol tri(meth)acrylate and isophorone diisocyanate, dipentaerythritol penta(meth)acrylate, dipentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, tris(acryloxyethyl)isocyanurate, tris(meth ... tris(acryloxyethyl)isocyanurate, reaction products of glycerol triglycidyl ether and (meth)acrylic acid, caprolactone modified tris(acryloxyethyl)isocyanurate, reaction products of trimethylolpropane triglycidyl ether and (meth)acrylic acid, triglycerol-di-(meth)acrylate, reaction products of propylene glycol-di-glycidyl ether and (meth)acrylic acid, polypropylene glycol-di-(meth)acrylate, tripropylene glycol-di-(meth)acrylate, polyethylene glycol-di-(meth)acrylate, tetraethylene glycol-di-(meth)acrylate, triethylene glycol-di-(meth)acrylate, pentaerythritol-di-(meth)acrylate, reaction products of 1,6-hexanediol-di-glycidyl ether and (meth)acrylic acid, 1,6-Hexanediol-di-(meth)acrylate, glycerol-di-(meth)acrylate, reaction products of ethylene glycol-di-glycidyl ether and (meth)acrylic acid, reaction products of diethylene glycol-di-glycidyl ether and (meth)acrylic acid, bis(acryloxyethyl)hydroxyethyl isocyanurate, bis(methacryloxyethyl)hydroxyethyl isocyanurate, reaction products of bisphenol A-di-glycidyl ether and (meth)acrylic acid, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polypropylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, phenoxy hydroxypropyl Examples of the acrylates include butyl (meth)acrylate, acryloyl morpholine, methoxy polyethylene glycol (meth)acrylate, methoxy tetraethylene glycol (meth)acrylate, methoxy triethylene glycol (meth)acrylate, methoxy ethylene glycol (meth)acrylate, methoxy ethyl (meth)acrylate, glycidyl (meth)acrylate, glycerol (meth)acrylate, ethyl carbitol (meth)acrylate, 2-ethoxyethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, a reaction product of butyl glycidyl ether and (meth)acrylic acid, butoxy triethylene glycol (meth)acrylate, and butanediol mono (meth)acrylate. These may be used alone or in combination. These ultraviolet-curable resins that do not have liquid crystallinity must be added to such an extent that the composition containing the nematic liquid crystal monomer does not lose its liquid crystallinity, and are preferably added in an amount of 0.1 to 20 parts by mass, more preferably 1.0 to 10 parts by mass, per 100 parts by mass of the nematic liquid crystal monomer having a polymerizable group.
[0027] When the nematic liquid crystal monomer having a polymerizable group and the polymerizable compound not having liquid crystallinity are of the ultraviolet curing type, a photopolymerization initiator is added to cure the composition containing them by ultraviolet light. Examples of the photopolymerization initiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1 (Irgacure RTM907 manufactured by BASF), 1-hydroxycyclohexylphenyl ketone (Irgacure RTM184 manufactured by BASF), 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone (Irgacure RTM2959 manufactured by BASF), 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropane-1-one (M acetophenone compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ... Benzoin compounds such as ethyl ether and 2,2-dimethoxy-2-phenylacetophenone (Irgacure RTM651, manufactured by BASF); benzophenone compounds such as benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3'-dimethyl-4-methoxybenzophenone (Kayacure RTMMBP, manufactured by Nippon Kayaku); and thioxanthone, 2-chlorothio Examples of thioxanthone compounds include xanthone (Kayacure RTMCTX, manufactured by Nippon Kayaku Co., Ltd.), 2-methylthioxanthone, 2,4-dimethylthioxanthone (Kayacure RTMRTX), isopropylthioxanthone, 2,4-dichlorothioxanthone (Kayacure RTMCTX, manufactured by Nippon Kayaku Co., Ltd.), 2,4-diethylthioxanthone (Kayacure RTMDETX, manufactured by Nippon Kayaku Co., Ltd.), and 2,4-diisopropylthioxanthone (Kayacure RTMDITX, manufactured by Nippon Kayaku Co., Ltd.).Preferably, the photopolymerization initiator includes, for example, Irgacure TPO, Irgacure TPO-L, Irgacure OXE01, Irgacure OXE02, Irgacure 1300, Irgacure 184, Irgacure 369, Irgacure 379, Irgacure 819, Irgacure 127, Irgacure 907 and Irgacure 1173 (all manufactured by BASF), and particularly preferably, Irgacure TPO, Irgacure TPO-L, Irgacure OXE01, Irgacure OXE02, Irgacure 1300 and Irgacure 907. These photopolymerization initiators can be used alone or in combination in any ratio.
[0028] When a benzophenone-based compound or a thioxanthone-based compound is used as a photopolymerization initiator, an auxiliary agent can be used in combination to promote the photopolymerization reaction. Examples of such auxiliary agents include amine compounds such as triethanolamine, methyldiethanolamine, triisopropanolamine, n-butylamine, N-methyldiethanolamine, diethylaminoethyl methacrylate, Michler's ketone, 4,4'-diethylaminophenone, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate.
[0029] The amounts of the photopolymerization initiator and auxiliary are preferably used within a range that does not affect the liquid crystallinity of the composition, and the amounts are preferably 0.5 to 10 parts by mass, more preferably 2 to 8 parts by mass, relative to 100 parts by mass of the ultraviolet-curable compound in the composition. The auxiliary is preferably 0.5 to 2 times the amount of the photopolymerization initiator.
[0030] In addition, by adding at least one compound (hereinafter, also simply referred to as "additive compound") selected from the group consisting of compounds represented by the following formula (4), compounds represented by the following formula (5), and compounds represented by the following formula (6) together with the liquid crystal compound, the heat resistance of the 1 / 2 wavelength plate is further improved, and the change in the retardation value of the 1 / 2 wavelength plate can be further reduced even in a high-temperature atmosphere.
[0031] [ka]
[0032] In formulas (4) to (6), R 1-1 , R 1-2 and R 1-3 R each independently represents an alkyl group having a branched structure and having 5 or more carbon atoms. 1-1 , R 1-2 and R 1-3 When R is each independently an alkyl group having a branched structure, the change in retardation value of the half-wave plate in a high-temperature atmosphere is particularly small. The number of carbon atoms is preferably 6 or more and 18 or less. 1-1 , R 1-2 and R 1-3 are each independently CH3-(CH2) m More preferably, it is a -CHRX- group, where RX represents an alkyl group having 1 to 5 carbon atoms, and R 1-1 , R 1-2 and R 1-3 are each independently CH3-(CH2) m A -CH(C2H5)- group is more preferable, and a 2-ethylhexyl group or a 2-ethylbutyl group is particularly preferable. Here, m represents an integer in the range of 1 to 6. In formula (5), R 3 represents a -(CH2)p- group or a phenylene group, and p represents an integer of 4 to 8. 3 In the case where R is a phenylene group, the phenylene group may have a substituent at any of the o-position, m-position, and p-position, but preferably has a substituent at the o-position. 4represents a substituted phenylene group, and the substituted phenylene group may have a substituent at any of the o-position, m-position, and p-position, but preferably has a substituent at the o-position and p-position. 2 represents a -CH2-CH2- group, a -CH2-CH(CH3)- group or a -CH2-CH2-CH2- group, with a -CH2-CH2- group being preferred.
[0033] Examples of the compound represented by formula (4) include triethylene glycol-di-2-ethylhexanoate (3GO), tetraethylene glycol-di-2-ethylhexanoate (4GO), triethylene glycol-di-2-ethylbutyrate (3GH), tetraethylene glycol-di-2-ethylbutyrate, pentaethylene glycol-di-2-ethylhexanoate, octaethylene glycol-di-2-ethylhexanoate, nonaethylene glycol-di-2-ethylhexanoate, and decaethylene glycol-di-2-ethylhexanoate.
[0034] Examples of the compound represented by formula (5) include bis(2-ethylhexyl) adipate, bis(2-ethylbutyl) adipate, bis(2-ethylhexyl) azelate, bis(2-ethylbutyl) azelate, di-2-ethylhexyl sebacate, di-2-ethylbutyl sebacate, di-2-ethylhexyl phthalate, and di-2-ethylbutyl phthalate.
[0035] Examples of the compound represented by formula (6) include tri-2-ethylhexyl trimellitate and tri-2-ethylbutyl trimellitate.
[0036] The compound represented by formula (4), the compound represented by formula (5), and the compound represented by formula (6) may be used alone or in combination of two or more. Among these, the compound represented by formula (4) is preferable because it has excellent compatibility with the above-mentioned liquid crystal compound and can obtain a stable retardation element. Among the compounds represented by formula (4), triethylene glycol-di-2-ethylhexanoate (3GO), tetraethylene glycol-di-2-ethylhexanoate (4GO), and triethylene glycol-di-2-ethylbutyrate (3GH) are more preferable, and triethylene glycol-di-2-ethylhexanoate (3GO) is even more preferable, because they have excellent compatibility with the liquid crystal compound and are particularly excellent in suppressing the change in the retardation value of the 1 / 2 wavelength plate under a high temperature atmosphere.
[0037] The content of at least one additive compound selected from the group consisting of the compound represented by formula (4), the compound represented by formula (5) and the compound represented by formula (6) is not particularly limited, but is preferably 0.1 parts by mass or more and 300 parts by mass or less, more preferably 0.5 parts by mass or more and 50 parts by mass or less, even more preferably 0.8 parts by mass or more and 30 parts by mass or less, and particularly preferably 1 part by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the liquid crystal compound. If the content of the additive compound is less than 0.1 parts by mass, the effect of suppressing the change in the retardation value of the 1 / 2 wavelength plate in a high-temperature atmosphere may not be obtained. On the other hand, even if the content of the additive compound exceeds 300 parts by mass, the effect of suppressing the change in the retardation value of the 1 / 2 wavelength plate in a high-temperature atmosphere does not change, so the upper limit of the content of the additive compound is preferably 300 parts by mass or less from the viewpoint of material cost.
[0038] Depending on the design of the HUD system, a quarter-wave plate can also be used as the optical functional layer. The quarter-wave plate is a retardation element that has a function of converting circularly polarized light into linearly polarized light, and can be obtained, for example, by uniaxially stretching a film made of polycarbonate or cycloolefin polymer so that the retardation is 1 / 4 of the wavelength, or by orienting a horizontally oriented polymerizable liquid crystal to a thickness such that the retardation is 1 / 4 of the wavelength. In addition, the quarter-wave plate preferably includes the above-mentioned polymerizable liquid crystal layer. In such a case, the quarter-wave plate is composed of the above-mentioned polymerizable liquid crystal layer as a layer having the function of converting the polarization axis, and a support substrate on which a coating liquid forming the polymerizable liquid crystal layer is applied.
[0039] When the phase difference due to wavelength dispersion is large, a phase difference element called a wideband quarter-wave plate may be used as the quarter-wave plate. The wideband quarter-wave plate is a phase difference element with reduced wavelength dependency of phase difference, and examples thereof include a phase difference element in which a half-wave plate and a quarter-wave plate having the same wavelength dispersion are laminated so that the angle between their slow axes is 60°, and a polycarbonate-based phase difference element (Teijin: Pure Ace WR-S) with reduced wavelength dependency of phase difference. Furthermore, when the incident angle of light is obliquely incident on the quarter-wave plate as in a HUD, the phase difference may change depending on the incident angle of light depending on the phase difference element. In such a case, as a method of more strictly matching the phase difference, for example, a phase difference element with an adjusted refractive index of the phase difference element is used to suppress the change in phase difference associated with the incident angle. As such an example, when the refractive index in the slow axis direction in the plane of the retardation element is nx, the refractive index in the direction perpendicular to nx in the plane of the retardation element is ny, and the refractive index in the thickness direction of the retardation element is nz, the coefficient Nz shown in the above formula (1) is preferably controlled to be 0.3 to 1.0, and more preferably 0.5 to 0.8.
[0040] When an optical film using such a quarter-wave plate is provided in the functional glass of the present invention described later and the functional glass is applied to a HUD system, the optical functional layer is preferably a laminate of a quarter-wave plate and a circularly polarized reflective layer. Specifically, it is preferable that the optical functional layer is composed of a circularly polarized reflective layer, a first quarter-wave plate laminated on one surface of the circularly polarized reflective layer, and a second quarter-wave plate 7 laminated on the other surface of the circularly polarized reflective layer. As the circularly polarized reflective layer, a light reflective layer using a cholesteric liquid crystal is preferably used. In such a configuration, in the HUD system, of the two quarter-wave plates, the first quarter-wave plate is provided on the side on which S-polarized or P-polarized light is incident, and the second quarter-wave plate is provided on the side on which the circularly polarized light transmitted through the circularly polarized reflective layer is incident. For example, when the circularly polarized reflective layer has a right-handed circularly polarized light reflection function, when P-polarized light is incident on the first quarter-wave plate, almost no P-polarized light is reflected at the interface of the first quarter-wave plate, and it is transmitted through the first quarter-wave plate. The transmitted P-polarized light is converted to right-handed circularly polarized light by the first quarter-wave plate, and part of this right-handed circularly polarized light is reflected by the circularly polarized light reflective layer due to the right-handed circularly polarized light conversion performance of the circularly polarized light reflective layer. The reflected right-handed circularly polarized light is converted back to the original P-polarized light by the first quarter-wave plate, and this P-polarized light reaches the observer. In addition, the right-handed circularly polarized light that is not reflected by the circularly polarized light reflective layer and passes through the circularly polarized light reflective layer is returned to the original P-polarized light by the second quarter-wave plate, but this P-polarized light is transmitted without being reflected at the outer interface of the second quarter-wave plate. On the other hand, when S-polarized light is incident on the first quarter-wave plate, the S-polarized light is reflected by the surface of the first quarter-wave plate, and this S-polarized light reaches the observer. The S-polarized light that is not reflected by the first quarter-wave plate and passes through the first quarter-wave plate is converted to left-handed circularly polarized light by the first quarter-wave plate. This left-handed circularly polarized light is not reflected by the circularly polarized light reflective layer that has the function of reflecting right-handed circularly polarized light, but passes through the circularly polarized light reflective layer and is returned to its original S-polarized light by the second quarter-wave plate, but this S-polarized light also passes through the second quarter-wave plate without being reflected at the outer interface.Even if the circularly polarized light reflective layer has the function of reflecting left-handed circularly polarized light, P-polarized light or S-polarized light reaches the viewer due to the same principle.
[0041] The upper limit of the thickness of the quarter-wave plate is preferably 10 μm or less, more preferably 5 μm or less, from the viewpoint of the alignment of the liquid crystal. On the other hand, the lower limit of the thickness of the quarter-wave plate is preferably 0.3 μm or more, more preferably 0.5 μm or more. Also, the upper limit of the thickness of the circularly polarized reflective layer is preferably 10 μm or less, more preferably 5 μm or less, from the viewpoint of the alignment of the liquid crystal. On the other hand, the lower limit of the thickness of the circularly polarized reflective layer is preferably 0.3 μm or more, more preferably 0.5 μm or more, from the viewpoint of the polymerizability of the liquid crystal.
[0042] In the optical film of the present invention, two or more optical functional layers (A) may be provided. In this case, nothing may be used between the optical functional layers, i.e., each optical functional layer may be directly laminated, but it is preferable that an adhesive layer using an adhesive is provided between the optical functional layers. Examples of adhesives include acrylic or rubber-based adhesives, and acrylic adhesives are preferable because they are easy to adjust the adhesion and holding power. Examples of adhesives include ultraviolet-curable resin compositions, thermosetting resin compositions, and mixtures thereof. In the case of an ultraviolet-curable resin composition, the optical functional layers can be bonded together by irradiating ultraviolet light in the presence of a photopolymerization initiator to cure a composition in which multiple monomers having an acryloyl group or an epoxy group are mixed. In the case of a thermosetting resin composition, the optical functional layers can be bonded together by heating and curing a composition in which multiple monomers having an epoxy group are mixed in the presence of an acid catalyst. Alternatively, the optical functional layers can be bonded together by heating and curing a composition consisting of multiple monomers or polymers having amino groups, carboxyl groups, and hydroxyl groups in the presence of an isocyanate group or a compound having melamine.
[0043] [(B) Block layer] In the optical film of the present invention, the block layer has a cured product (cured film) of a resin composition (hereinafter also referred to as "resin composition for forming a block layer") containing (B-1) a thermoplastic resin and (B-2) an ultraviolet curable resin. By providing a block layer containing a thermoplastic resin in the optical film, (A) the retardation element provided as the optical functional layer can be protected from deterioration factors. In addition, an optical film having such a block layer is excellent in durability, mainly in hue change (ΔE) after a heat resistance test, and is also excellent in appearance and adhesion when the optical film is used to form a laminated glass. Therefore, it is possible to provide an optical film that has high durability, especially heat resistance, in a high-temperature atmosphere while maintaining a high visible light transmittance, and can suppress changes in the retardation value of the retardation element over a long period of time. The block layer may be a single layer, or two or more layers may be laminated.
[0044] [(B-1) Thermoplastic resin] The thermoplastic resin (B-1) is not particularly limited as long as it is a resin that can obtain a thermoplasticity sufficient to be molded by heating. Examples of such thermoplastic resins include polyvinyl acetal resin, high-density polyethylene resin, low-density polyethylene resin, linear low-density polyethylene resin, very low-density polyethylene resin, polypropylene resin, polybutadiene resin, cyclic olefin resin, polymethylpentene resin, polystyrene resin, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-vinyl alcohol copolymer resin, ethylene-ethyl acrylate copolymer, acrylonitrile-styrene resin, acrylonitrile-chlorinated polystyrene-styrene copolymer resin, acrylonitrile-acrylic rubber-styrene copolymer resin, acrylonitrile-butadiene-styrene copolymer resin, acrylonitrile-EPDM-styrene copolymer resin, silicone rubber-acrylonitrile-styrene copolymer resin, cellulose acetate-butyrate resin, cellulose acetate resin, methacrylic resin, ethylene-methyl methacrylate copolymer resin, ethylene-ethyl acrylate resin, polyvinyl chloride resin, chlorinated polyethylene resin, polytetrafluoroethylene resin, tetrafluoroethylene-hexafluoropropylene ... Examples of the polypropylene copolymer resin include propylene copolymer resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer resin, tetrafluoroethylene-ethylene copolymer resin, polytrifluorochloroethylene resin, polyvinylidene fluoride resin, nylon 4,6, nylon 6, nylon 6,6, nylon 6,10, nylon 6,12, nylon 12, nylon 6T, nylon 9T, aromatic nylon resin, polyacetal resin, ultra-high molecular weight polyethylene resin, polybutylene terephthalate resin, polyethylene terephthalate resin, polyethylene naphthalate resin, amorphous copolyester resin, polycarbonate resin, modified polyphenylene ether resin, thermoplastic polyurethane elastomer, polyphenylene sulfide resin, polyether ether ketone resin, liquid crystal polymer, polytetrafluoroethylene resin, polyfluoroalkoxy resin, polyetherimide resin, polysulfone resin, polyketone resin, thermoplastic polyimide resin, polyamideimide resin, polyarylate resin, polysulfone resin, polyethersulfone resin, biodegradable resin, biomass resin, and the like.The thermoplastic resins may be used alone or in combination of two or more kinds.
[0045] Examples of commercially available thermoplastic resins include S-LEC RTM BL-1, BL-1H, BL-2, BL-2H, BL-5, BL-10, BL-S, BL-L, BM-1, BM-2, BM-5, BM-S, BH-3, BH-6, BH-S, BX-1, BX-1, BX-5, KS-10, KS-1, KS-3, and KS-5 (all manufactured by Sekisui Chemical Co., Ltd.); the Vylon RTM series of amorphous polyester resins and crystalline polyester resins, the Vylonal RTM series of water-dispersed polyester resins, the Vylon RTM UR series of polyester urethane resins, and the Vyloecol RTM series of amorphous polylactic acid resins (all manufactured by Toyobo Co., Ltd.); the Septon RTM series and Hybra RTM series of styrene-based elastomers, and Acrylonitrile RTM series. Examples of such resins include the Clarity RTM series of vinyl block copolymers, the Arneston RTM series of thermoplastic elastomer compounds, and the isoprene-based Kuraprene RTM series (all manufactured by Kuraray Co., Ltd.); the polyvinyl alcohol Denka Poval RTM (manufactured by Denka Co., Ltd.); the terpene resins YS Resin RTMPX series, YS Resin RTMPXN series, and the aromatic modified terpene resin YS Resin RTMTO (all manufactured by Yasuhara Chemical Co., Ltd.); and the terpene phenol resins YS Polystar RTMU, YS Polystar RTMT, YS Polystar RTMS, YS Polystar RTMG, YS Polystar RTMN, YS Polystar RTMK, and YS Polystar RTMTH (all manufactured by Yasuhara Chemical Co., Ltd.).
[0046] Among these, polyvinyl acetal resins are preferred from the viewpoints of appearance when the optical film is used to make laminated glass, adhesion, hue change (ΔE) before and after heat resistance testing, optical properties before and after heat resistance testing, etc. Polyvinyl acetal resins are resins obtained by reacting polyvinyl alcohol with aldehyde, and are compounds represented by the following formula (7).
[0047] [ka]
[0048] In formula (7), R represents a C1-C10 linear, branched or cyclic alkyl group, preferably a C1-C6 linear alkyl group, more preferably a C1-C4 linear alkyl group, particularly preferably C1, i.e., a methyl group (polyvinyl acetoacetal resin), or C4, i.e., an n-butyl group (polyvinyl butyral resin), and most preferably a methyl group. When R is a methyl group, i.e., when the thermoplastic resin is a polyvinyl acetoacetal resin, there is little change in hue, particularly before and after a durability test, and the material is highly practical.
[0049] In the above formula (7), n represents the number of repeating units and is preferably 50 or more and 1500 or less. The upper limit of n is more preferably 1000, even more preferably 800, particularly preferably 600, and most preferably 200. The lower limit of n is more preferably 70, even more preferably 100, particularly preferably 120, and most preferably 150.
[0050] The preferred molecular weight (weight average molecular weight: Mw) of the thermoplastic resin is 6,000 or more and 1,000,000 or less. The upper limit of the molecular weight is more preferably 120,000, even more preferably 96,000, particularly preferably 60,000, and most preferably 20,000. The lower limit of the molecular weight is more preferably 8,500, even more preferably 10,000, particularly preferably 12,000, and most preferably 16,000. That is, the molecular weight of the thermoplastic resin is most preferably 10,000 or more and 60,000 or less. The weight average molecular weight is measured by gel permeation chromatography (GPC).
[0051] In one preferred embodiment, the content of the thermoplastic resin in the block layer is 1% by mass or more and 80% by mass or less. The upper limit of the content of the thermoplastic resin in the block layer is more preferably 50% by mass, even more preferably 40% by mass, and particularly preferably 30% by mass. The lower limit of the thermoplastic resin in the block layer is more preferably 2% by mass, even more preferably 5% by mass, and particularly preferably 10% by mass. In other words, the content of the thermoplastic resin in the block layer is most preferably 10% by mass or more and 30% by mass or less.
[0052] [(B-2) Ultraviolet curable resin] The (B) block layer has an ultraviolet curing resin (B-2). Examples of the ultraviolet curing resin include resins having a vinyl group, a vinyl ether group, an allyl group, a maleimide group, a (meth)acryloyl group, and the like. Among them, from the viewpoint of reactivity and versatility, the ultraviolet curing resin is preferably a resin having a (meth)acryloyl group, such as a (meth)acrylate compound. The ultraviolet curing resin may be used alone or in combination of two or more kinds.
[0053] Examples of resins having a (meth)acryloyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 1,4-butanediol mono(meth)acrylate, carbitol (meth)acrylate, acryloylmorpholine, half esters which are reaction products of hydroxyl group-containing (meth)acrylates and acid anhydrides of polycarboxylic acid compounds, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, and glycerin polypropoxy. Examples of (meth)acrylate resins include tri(meth)acrylate, di(meth)acrylate of ε-caprolactone adduct of neopentyl glycol hydroxypivalate (e.g., KAYARADRTMHX-220, HX-620, etc., manufactured by Nippon Kayaku Co., Ltd.), pentaerythritol tetra(meth)acrylate, poly(meth)acrylate of reaction product of dipentaerythritol and ε-caprolactone, dipentaerythritol poly(meth)acrylate (e.g., KAYARADRTMDPHA, etc., manufactured by Nippon Kayaku Co., Ltd.), and epoxy(meth)acrylate which is reaction product of mono- or polyglycidyl compound and (meth)acrylic acid. Of these, epoxy(meth)acrylate resins are most preferably used.
[0054] The glycidyl compound used in the epoxy (meth)acrylate, which is a reaction product of a mono- or polyglycidyl compound and (meth)acrylic acid, is not particularly limited, and examples thereof include bisphenol A, bisphenol F, bisphenol S, 4,4'-biphenylphenol, tetramethylbisphenol A, dimethylbisphenol A, tetramethylbisphenol F, dimethylbisphenol F, tetramethylbisphenol S, dimethylbisphenol S, tetramethyl-4,4'-biphenol, dimethyl-4,4'-biphenylphenol, 1-(4-hydroxyphenyl)-2-[4-(1,1-bis-(4-hydroxyphenyl)ethyl)phenyl]propane, 2,2'-methyl Examples of the glycidyl ethers of polyphenols include 4,4'-butylidene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidene-bis(3-methyl-6-tert-butylphenol), trishydroxyphenylmethane, resorcinol, hydroquinone, pyrogallol, phenols having a diisopropylidene skeleton, phenols having a fluorene skeleton such as 1,1-di-4-hydroxyphenylfluorene, phenolized polybutadiene, brominated bisphenol A, brominated bisphenol F, brominated bisphenol S, brominated phenol novolac, brominated cresol novolac, chlorinated bisphenol S, and chlorinated bisphenol A.
[0055] Epoxy (meth)acrylate, which is a reaction product of these mono- or polyglycidyl compounds and (meth)acrylic acid, can be obtained by esterifying the epoxy group with an equivalent amount of (meth)acrylic acid. This synthesis reaction can be carried out by a generally known method. For example, an equivalent amount of (meth)acrylic acid is added to resorcinol diglycidyl ether together with a catalyst (e.g., benzyldimethylamine, triethylamine, benzyltrimethylammonium chloride, triphenylphosphine, triphenylstibine, etc.) and a polymerization inhibitor (e.g., methoquinone, hydroquinone, methylhydroquinone, phenothiazine, dibutylhydroxytoluene, etc.), and the esterification reaction is carried out, for example, at 80 to 110°C. The (meth)acrylated resorcinol diglycidyl ether thus obtained is a resin having a radically polymerizable (meth)acryloyl group. In addition, it is particularly preferable that the binder resin has both a polar functional group and two or more (meth)acryloyl groups in the molecule.
[0056] In addition, the resin having a (meth)acryloyl group is particularly preferably a binder resin having both a polar functional group and two or more (meth)acryloyl groups in the molecule. Examples of the polar functional group include a hydroxy group, a carboxy group, a phospho group, an amino group, an imino group, a carbamoyl group, a cyano group, an isocyanato group, a nitro group, a nitroso group, a hydrazino group, a ureido group, a guanidino group, a sulfanyl group, a sulfino group, a sulfo group, a furyl group, a thienyl group, a pyrrolyl group, a pyrrolidinyl group, a pyridyl group, a pyrrolidino group, a piperidinyl group, a morpholino group, and a quinolyl group. In addition, the polar functional group may be substituted with an alkyl group, an alkoxy group, or the like. In addition, polar bond sites different from the substituents such as urethane bonds, ether bonds, and ester bonds (excluding the ester bonds in the (meth)acryloyl group) are also included as polar functional groups.
[0057] Examples of binder resins having both two or more (meth)acryloyls having a polar functional group and a polar functional group include (meth)acrylate monomer compounds such as pentaerythritol triacrylate (KAYARADRTMPET-30, manufactured by Nippon Kayaku Co., Ltd.), a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (KAYARADRTMDPHA, manufactured by Nippon Kayaku Co., Ltd.), 2-hydroxy-3-acryloyloxypropyl methacrylate (701A, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethoxylated isocyanuric acid triacrylate (A-9300, manufactured by Shin-Nakamura Chemical Co., Ltd.), and ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate (A-9300-1CL, manufactured by Shin-Nakamura Chemical Co., Ltd.); bisphenol A type epoxy acrylate (R-115F, R-1 epoxy acrylate resins such as bisphenol F type epoxy acrylate (ZFA-266H, Nippon Kayaku Co., Ltd.), acid-modified epoxy acrylate (ZAR series, ZFR series, ZCR series, Nippon Kayaku Co., Ltd.); and urethane acrylate resins such as polyester-based urethane acrylate (UX3204, UX-4101, UXT-6100, Nippon Kayaku Co., Ltd.), mixed urethane acrylate (UX-6101, UX-8101, Nippon Kayaku Co., Ltd.), polyether-based urethane acrylate (UX-937, UXF-4001-M35, Nippon Kayaku Co., Ltd.), and ester-based urethane acrylate (DPHA-40H, UX-5000, UX-5102D-M20, UX-5103D, UX-5005, Nippon Kayaku Co., Ltd.).
[0058] The ultraviolet curable resin is more preferably a binder resin having both a (meth)acryloyl group and a polar functional group with a number of from 2 to 9, and even more preferably a binder resin having both a (meth)acryloyl group and a polar functional group with a number of from 3 to 6. If the number of (meth)acryloyl groups as reactive groups is 10 or more, the obtained cured product may become too rigid, leading to a decrease in adhesive strength.
[0059] In the blocking layer, the content of the ultraviolet curable resin is preferably 10% by mass or more and 99% by mass or less. The upper limit of the content of the ultraviolet curable resin is more preferably 95% by mass, even more preferably 90% by mass, and particularly preferably 85% by mass. The lower limit of the ultraviolet curable resin is more preferably 20% by mass, even more preferably 50% by mass, and particularly preferably 75% by mass. In other words, the content of the ultraviolet curable resin is most preferably 75% by mass or more and 85% by mass or less.
[0060] The blocking layer further contains a radical polymerization initiator that cures the ultraviolet curable resin. The radical polymerization initiator means a photoradical polymerization initiator and / or a thermal radical polymerization initiator.
[0061] The photoradical polymerization initiator is not particularly limited as long as it is a compound that generates radicals or acids and initiates a chain polymerization reaction upon irradiation with ultraviolet light, and examples thereof include benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, diethylthioxanthone, benzophenone, 2-ethylanthraquinone, 2-hydroxy-2-methylpropiophenone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, camphorquinone, 9-fluorenone, and diphenyl disulfide. Specific examples include IRGACURER™ 651, 184, 2959, 127, 907, 369, 379EG, 819, 784, 754, 500, OXE01, OXE02, DAROCURER™ 1173, LUCIRINR™ TPO (all manufactured by BASF), Seikuol RTM Z, BZ, BEE, BIP, and BBI (all manufactured by Seiko Chemical Co., Ltd.).
[0062] When a photoradical polymerization initiator is used, the content is preferably 0.01 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the total amount of the ultraviolet curable resin. The upper limit of the content of the photoradical polymerization initiator is more preferably 7 parts by mass, even more preferably 5 parts by mass, particularly preferably 4 parts by mass, and most preferably 3 parts by mass. The lower limit of the photoradical polymerization initiator is more preferably 0.01 parts by mass, even more preferably 0.1 parts by mass, particularly preferably 1 part by mass, and most preferably 1.5 parts by mass.
[0063] The thermal radical polymerization initiator is not particularly limited as long as it is a compound that generates radicals by heating and initiates a chain polymerization reaction, and examples thereof include organic peroxides, azo compounds, benzoin compounds, benzoin ether compounds, acetophenone compounds, and benzopinacol, with benzopinacol being preferred. For example, examples of organic peroxides include Kayamec RTMA, M, R, L, LH, SP-30C, Perkadox CH-50L, BC-FF, Kadox B-40ES, Perkadox 14, Trigonox RTM22-70E, 23-C70, 121, 121-50E, 121-LS50E, 21-LS50E, 42, 42LS, Kayaester RTMP-70, TMPO-70, CND-C70, OO-50E, AN, and Kayabuchi. Commercially available products include AL RTMB, Perkadox 16, Kayacarvone RTMBIC-75, AIC-75 (manufactured by Kayaku Akzo Co., Ltd.), Permec RTMN, H, S, F, D, G, Perhexa RTMH, HC, TMH, C, V, 22, MC, Percure RTMAH, AL, HB, Perbutyl RTMH, C, ND, L, Percumyl RTMH, D, Peroyl RTMIB, IPP, and Perocta RTMND (manufactured by NOF Corp.). Commercially available azo compounds include VA-044, V-070, VPE-0201, and VSP-1001 (manufactured by Wako Pure Chemical Industries, Ltd.).
[0064] When a thermal radical polymerization initiator is used, the content is preferably 0.01 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total amount of the ultraviolet curable resin. The upper limit of the content of the thermal radical polymerization initiator is preferably 7 parts by mass, more preferably 5 parts by mass, particularly preferably 4 parts by mass, and most preferably 3 parts by mass. The lower limit of the thermal radical polymerization initiator is preferably 0.01 parts by mass, more preferably 0.1 parts by mass, particularly preferably 1 part by mass, and most preferably 1.5 parts by mass.
[0065] In addition to the above components, the block layer may contain, as necessary, a leveling agent, an antifoaming agent, an ultraviolet absorber, a light stabilizer, an antioxidant, a polymerization inhibitor, a crosslinking agent, a plasticizer, inorganic fine particles, a filler, etc., to impart the desired functionality. Examples of the leveling agent include fluorine-based compounds, silicone-based compounds, and acrylic-based compounds. Examples of the ultraviolet absorber include benzotriazole-based compounds, benzophenone-based compounds, and triazine-based compounds. Examples of the light stabilizer include hindered amine-based compounds and benzoate-based compounds. Examples of the antioxidant include phenol-based compounds. Examples of the polymerization inhibitor include methoquinone, methylhydroquinone, and hydroquinone. Examples of the crosslinking agent include the polyisocyanates and melamine compounds. The amount of each of these components added can be appropriately determined depending on the purpose.
[0066] The glass transition temperature (Tg) of the block layer is preferably 80°C or more and 300°C or less, more preferably 90°C or more and 200°C or less, and even more preferably 150°C or more and 250°C or less. The glass transition temperature can be measured, for example, by the DMA method under the following measurement conditions. Using a dynamic viscoelasticity measuring device (DMS-6100: manufactured by SII NanoTechnology Co., Ltd.), the measurement is performed in tension mode under the conditions of a frequency of 10 Hz and a temperature rise rate of 2°C / min. The loss factor Tanδ is obtained from the ratio of the loss modulus to the storage modulus (JIS: K 7244-1: 1998). The temperature at which the obtained loss factor Tanδ is maximum is regarded as the glass transition temperature.
[0067] The thickness of the block layer is preferably 0.1 μm or more and 50 μm or less, more preferably 0.5 μm or more and 20 μm or less, and even more preferably 1 μm or more and 10 μm or less. When the block layer has a thickness of 0.1 μm or more, when the optical film is applied to an optical laminate described later, the block layer has an effect of preventing a change in the retardation value of the optical functional layer due to the intrusion of a plasticizer used as an intermediate film. In addition, when the block layer has a thickness of 50 μm or less, the appearance when the optical film is produced and the appearance when the functional glass including the optical film is produced are excellent. The block layer can be obtained by applying the resin composition for forming the block layer so that the film thickness after drying is in the above-mentioned preferred range, and curing the composition by UV irradiation after drying to form a cured film.
[0068] Examples of methods for applying the resin composition for forming the block layer include bar coater coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, microgravure coating, micro reverse gravure coater coating, die coater coating, dip coating, spin coat coating, and spray coating.
[0069] The block layer having the cured product of the resin composition containing the thermoplastic resin (B-1) and the ultraviolet-curable resin (B-2) has excellent adhesion to the intermediate film of the optical laminate described below and excellent durability. In particular, wrinkles are unlikely to occur during the formation of the block layer, and in terms of durability, there is little change in the polarization conversion transmittance, hue, and adhesion before and after a heat resistance test.
[0070] The resin composition for forming the block layer is irradiated with ultraviolet light for curing, but electron beams and the like can also be used. When curing with ultraviolet light, an ultraviolet irradiator having a xenon lamp, a high-pressure mercury lamp, a metal halide lamp, an LED, etc. can be used as a light source, and the amount of light, the arrangement of the light source, etc. are adjusted as necessary. When using a high-pressure mercury lamp, it is preferable to cure at a conveying speed of 5 to 60 m / min for one lamp having an energy of 80 to 120 W / cm2. On the other hand, when curing the resin composition for forming the block layer with electron beams, it is preferable to use an electron beam accelerator having an energy of 100 to 500 eV, and in that case, a photopolymerization initiator may not be used.
[0071] [(C) Support board] In the optical film of the present invention, when the blocking layer (B) is provided only on one side of the optical functional layer (A), the other side of the optical functional layer is preferably a film-like supporting substrate (C). Such a supporting substrate is preferably transparent in the visible light region in order to maintain the visibility of the displayed image. Specifically, the non-polarized light transmittance at a wavelength of 380 to 780 nm may be 50% or more, preferably 70% or more, and more preferably 85% or more. Here, the non-polarized light transmittance means the transmittance of light with no regularity in the vibration of light, that is, the transmittance of natural light. In addition, the supporting substrate may be colored, but it is preferable that it is not colored or is less colored. Furthermore, the refractive index of the supporting substrate is preferably 1.2 to 2.0, more preferably 1.4 to 1.8. The thickness of the supporting substrate may be appropriately selected depending on the application, and is preferably 5 μm to 1000 μm, more preferably 10 μm to 250 μm, and particularly preferably 15 μm to 150 μm.
[0072] (C) The support substrate may be a single layer or a laminate of two or more layers. Examples of the support substrate include triacetyl cellulose (TAC), acrylic, polycarbonate, polyvinyl chloride, polyolefin, and polyethylene terephthalate (PET). Among these, triacetyl cellulose (TAC), polyolefin, and acrylic, which have low birefringence, are preferred in order not to change the polarization axis of the incident P-polarized or S-polarized light.
[0073] [Method of manufacturing optical film] Next, an example of a method for producing the optical film of the present invention will be described. As such a method, for example, a nematic liquid crystal monomer having a polymerizable group is dissolved in a solvent as a material for producing a retardation element constituting an optical functional layer, and then a photopolymerization initiator is added. Such a solvent is not particularly limited as long as it can dissolve the liquid crystal monomer to be used, but examples thereof include cyclopentanone, toluene, methyl ethyl ketone, methyl isobutyl ketone, etc., and cyclopentanone and toluene are preferred. Then, this solution is applied to a plastic substrate such as a TAC film used as a support substrate so that the thickness is as uniform as possible, and the solution is left for a certain period of time under temperature conditions that the liquid crystal becomes liquid crystal and is aligned on the plastic substrate while removing the solvent by heating. At this time, the alignment of the liquid crystal can be made more uniform by performing an alignment treatment such as rubbing treatment in a desired alignment direction before application on the surface of the plastic substrate, or forming a film of a photoalignment material that exhibits photoalignment by polarized light irradiation on the surface of the plastic substrate and irradiating it with polarized light. This makes it possible to control the slow axis of a retardation element such as a half-wave plate, a quarter-wave plate, or a circularly polarized light reflective layer to a desired angle and reduce the haze value of the retardation element. Next, while maintaining this orientation state, the nematic liquid crystal monomer is irradiated with ultraviolet light from a high-pressure mercury lamp or the like to fix the orientation of the liquid crystal, thereby obtaining a retardation element having a desired slow axis.
[0074] In the case where the polymerizable liquid crystal monomer is directly applied onto the support substrate that has been subjected to the above-mentioned alignment treatment, that is, in the case where the retardation element constituting the optical functional layer has a polymerizable liquid crystal layer provided on the support substrate that has been subjected to the alignment treatment, the support substrate has a function of preventing the retardation value of the retardation element from decreasing in the same manner as the block layer. By having the retardation element have such a configuration, for example, a substance that may cause a change in the retardation value, such as an intermediate film described later, does not come into direct contact with the polymerizable liquid crystal layer of the retardation element, and as a result, the decrease in the retardation value of the retardation element can be suppressed. In addition, such a configuration can reduce the manufacturing process of applying one block layer compared to a configuration in which a block layer is provided on both sides of the optical functional layer, so that the optical laminate used in the present invention can be produced more inexpensively.
[0075] <Optical laminate> The optical laminate of the present invention is obtained by laminating an intermediate film on the above-mentioned optical film. The intermediate film is preferably a resin film of a thermoplastic resin, and more preferably a film of polyvinyl butyral. The intermediate film may be one or more, but the optical laminate is preferably structured such that the optical film is sandwiched between two intermediate films.
[0076] 4 shows one embodiment of the optical laminate of the present invention, in which the optical laminate 20 has a configuration in which an optical film 10 is sandwiched between two intermediate films 201, and the optical film 10 corresponds to, for example, the optical film in FIG. 3. The optical film 10 may have a configuration in which the blocking layer is provided only on the side of the optical functional layer 101 where the layer having the function of converting the polarization axis is provided. In such a case, the intermediate film 201 only needs to be provided on the blocking layer side, and may also be provided on the supporting substrate side of the half-wave plate.
[0077] <Interlayer film> The interlayer film can be made of a thermoplastic resin, and it is preferable to use a commonly used interlayer film for vehicles. Examples of such interlayer films for vehicles include polyvinyl butyral resin (PVB), polyvinyl alcohol resin (PVA), ethylene-vinyl acetate copolymer resin (EVA), and cycloolefin polymer (COP). Interlayer films made of these resins are preferred because they are versatile as interlayer films for laminated glass. In addition, the thickness of the interlayer film is not particularly limited as long as it does not affect the reflection of display light when the optical laminate is applied to a HUD system described later, and can be appropriately designed according to the application.
[0078] When the interlayer for laminated glass is made of PVB resin, retardation elements such as a 1 / 2 wavelength plate, a 1 / 4 wavelength plate, and a circularly polarized light reflective layer made of a polymerizable liquid crystal in contact with the interlayer may deteriorate under high temperature conditions, resulting in a decrease in retardation value. This is considered to be due to the erosion of the PVB resin itself adjacent to the retardation element, and the influence of a plasticizer contained in the PVB resin. In the optical laminate of the present invention, even if such an interlayer made of a PVB resin or an interlayer made of a PVB resin containing a plasticizer is laminated so as to be in direct contact with an optical film, the deterioration of retardation elements such as a 1 / 2 wavelength plate, a 1 / 4 wavelength plate, and a circularly polarized light reflective layer can be suppressed, and the change in retardation value can be suppressed.
[0079] Examples of plasticizers that reduce the retardation value of a retardation element made of polymerizable liquid crystal include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and organic phosphoric acid plasticizers such as organic phosphoric acid and organic phosphorous acid. Examples of the monobasic organic acid esters include glycol esters obtained by reacting glycols such as triethylene glycol, tetraethylene glycol, and tripropylene glycol with monobasic organic acids such as butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, pelargonic acid (n-nonylic acid), and decylic acid.
[0080] Examples of the polybasic organic acid ester include ester compounds of a polybasic organic acid such as adipic acid, sebacic acid, azelaic acid, etc., and an alcohol having a linear or branched structure having 4 to 8 carbon atoms.
[0081] Examples of the organic ester plasticizer include triethylene glycol-di-2-ethylbutyrate, triethylene glycol-di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol-di-n-octanoate, triethylene glycol-di-n-heptanoate, tetraethylene glycol-di-2-ethylhexanoate, tetraethylene glycol-di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol-di-2-ethylbutyrate, 1,3-propylene glycol-di-2-ethylbutyrate, 1,4-butylene glycol-di-2-ethylbutyrate, diethylene glycol-di-2-ethylbutyrate, and diethylene glycol-di. 2-ethylhexanoate, dipropylene glycol-di-2-ethylbutyrate, triethylene glycol-di-2-ethylpentanoate, tetraethylene glycol-di-2-ethylbutyrate, diethylene glycol dicaprylate, triethylene glycol-di-n-heptanoate, tetraethylene glycol-di-n-heptanoate, triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacic acid, a mixture of a phosphate ester and an adipate ester, and the like.
[0082] Examples of the organic phosphoric acid plasticizer include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.
[0083] The interlayer film for laminated glass may be appropriately mixed with ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, colorants, adhesion adjusters, etc., and in particular, an interlayer film in which infrared absorbing particles are dispersed is important for producing a high-performance heat-shielding laminated glass. For the infrared absorbing particles, particles of conductive materials such as metals Sn, Ti, Zn, Fe, Al, Co, Ce, Cs, In, Ni, Ag, Cu, Pt, Mn, Ta, W, V, and Mo, oxides of the metals, nitrides of the metals, or composites containing at least two or more of these are used. These materials may be doped with Sn, Sb, F, etc. In particular, tin-doped indium oxide (ITO), antimony-doped tin oxide (ATO), and fluorine-doped tin oxide, which are transparent in the visible light range, are preferred when laminated glass is used as a window for buildings or automobiles where transparency is required. The particle size of the infrared absorbing particles dispersed in the interlayer film is preferably 0.2 μm or less. If the particle size of the particles is 0.2 μm or less, it can absorb infrared rays while suppressing light scattering in the visible light range, does not cause haze in the laminated glass, ensures radio wave transmission and transparency, maintains physical properties such as adhesion, transparency, and durability equivalent to those of an interlayer film without the additive, and can be laminated using a normal laminated glass manufacturing line. When using PVB as the interlayer film, the lamination process is performed in a room with constant temperature and humidity to keep the moisture content of the interlayer film at an optimum level. In addition, interlayer films that are partially colored, sandwiched with a layer that has sound insulation properties, and have a gradient in thickness (wedge shape) to reduce the ghost phenomenon (double image) in HUDs can be used.
[0084] There is no particular limitation on the method for laminating the interlayer for laminated glass and the optical film having an optical functional layer such as a half-wave plate or a quarter-wave plate, but an example is a method of laminating the interlayer and the optical film by pressure bonding at the same time using a nip roll. If the nip roll can be heated during lamination, pressure bonding can also be performed while heating. In addition, if the adhesion between the interlayer and the optical film is poor, the lamination may be performed after previously performing a surface treatment such as a corona treatment or a plasma treatment.
[0085] The interlayer may be directly laminated on one or both sides of the optical film in a state of being dissolved in a solvent. When a polyvinyl butyral resin (PVB) is used as the interlayer, the butyralization degree is preferably 40 mol% or more and 85 mol% or less, and the lower limit of the butyralization degree is more preferably 5 mol%, and particularly preferably 60 mol%. On the other hand, the upper limit of the butyralization degree is more preferably 80 mol%, and particularly preferably 75 mol%. The butyralization degree can be measured by an infrared absorption spectrum (IR) method, for example, using FT-IR.
[0086] The amount of hydroxyl groups in the polyvinyl butyral resin is preferably 15 mol% or more and 35 mol% or less. If the amount of hydroxyl groups is less than 15 mol%, the adhesion between the interlayer film for laminated glass and glass may decrease, and the penetration resistance of the laminated glass may decrease. On the other hand, if the amount of hydroxyl groups exceeds 35 mol%, the interlayer film may become hard.
[0087] The polyvinyl butyral resin can be prepared by acetalizing polyvinyl alcohol with an aldehyde. Polyvinyl alcohol is usually obtained by saponifying polyvinyl acetate, and polyvinyl alcohol with a saponification degree of 80 to 99.8 mol% is generally used. The degree of polymerization of polyvinyl alcohol is preferably 4000 or less, more preferably 3000 or less, and particularly preferably 2500 or less. If the degree of polymerization exceeds 4000, it may be difficult to form the interlayer film.
[0088] <Functional glass> The functional glass of the present invention comprises the above-mentioned optical laminate and a glass plate. The glass plate may be one or more, but the functional glass having a structure in which the optical laminate is sandwiched between two glass plates is preferred. Such functional glass is preferably used as a display medium in a HUD system.
[0089] The functional glass is produced, for example, by laminating the above-mentioned optical laminate to a glass plate. As an example of a method for laminating the optical laminate to a glass plate, a pressure-sensitive adhesive or a bonding agent is applied to one or both sides of the optical laminate, and then the glass plate is laminated. There is no particular limitation on the pressure-sensitive adhesive or bonding agent, but if there is a possibility of peeling off later, a material with excellent reworkability and good adhesion, such as a silicone pressure-sensitive adhesive or an acrylic pressure-sensitive adhesive, is preferred.
[0090] The glass plate is not particularly limited as long as it has transparency that allows the forward view to be sufficiently visible even when the functional glass of the present invention is used as a windshield. The refractive index of the glass plate is preferably 1.2 to 2.0, more preferably 1.4 to 1.8. The thickness and shape of the glass plate are not particularly limited as long as they do not affect the reflection of the display light when the functional glass is applied to the HUD system described later, and can be appropriately designed according to the application. The glass plate may be provided on the reflective surface with an enhanced reflection film made of a multilayer film, a metal thin film that also has a heat shielding function, etc. These films can improve the reflectance of incident polarized light, but when the functional glass of the present invention is used as a windshield for an automobile, for example, it is preferable to adjust the reflectance so that the visible light transmittance of the functional glass is 70% or more.
[0091] When the optical laminate of the present invention is used, the optical laminate is placed between two glass plates and pressed at high temperature and high pressure to obtain a functional glass in which the optical laminate is placed in the laminated glass. FIG. 5 shows one embodiment of the functional glass according to the present invention. The functional glass 30 shown in FIG. 5 has a configuration in which the optical laminate 20 is sandwiched between two glass plates 301, and the optical laminate 20 corresponds to the optical laminate of FIG. 4, for example. The optical film 10 constituting the optical laminate 20 has a block layer 102 on one side of the optical functional layer 101 as shown in FIG. 3, and the other side may be a support substrate (not shown), or may have the block layer 102 on both sides of the optical functional layer 101. As shown in FIG. 5, when the optical laminate 20 constitutes the functional glass 30, the intermediate film 201 also functions as an adhesive or bonding agent for maintaining the adhesion between the two glass plates 301 and the optical laminate 20.
[0092] An example of a method for producing functional glass using the optical film of the present invention will be specifically described. First, two glass sheets are prepared. When used as a laminated glass for an automobile windshield, soda lime glass produced by the float method is used. The glass may be either transparent or colored green, and there is no particular restriction. The thickness of these glass sheets is usually about 2 mmt, but glass sheets with a thickness slightly thinner than this can also be used in response to recent demands for lighter glass. The glass sheets are cut into a predetermined shape, the glass edges are chamfered, and then washed. When a black frame-like or dot-like print is required, it is printed on the glass sheet. When a curved shape is required, such as a windshield, the glass sheets are heated to 650°C or higher, and then shaped so that the two sheets have the same surface shape by pressing with a mold or bending under its own weight, and the glass is cooled. At this time, if the cooling rate is too fast, a stress distribution occurs in the glass sheets, resulting in tempered glass, so they are cooled slowly. One of the glass sheets produced in this way is placed horizontally, the optical film of the present invention is placed on it, and the other glass sheet is placed on top of it. Alternatively, the intermediate film, optical film, and intermediate film may be stacked on top of a glass plate in this order, and the other glass plate may be placed at the end. In this case, the retardation element as an optical functional layer in the optical film is arranged so that it faces the outside of the vehicle. Next, the optical film and intermediate film that protrude from the edge of the glass plate are cut and removed with a cutter. After that, the sandwiched glass plate, intermediate film, and optical film are heated to a temperature of 80°C to 100°C while degassing the air that exists between them, and preliminary bonding is performed. There are two methods for degassing the air: the bag method, in which the laminate of glass plate / intermediate film / optical film / intermediate film / glass plate is wrapped in a rubber bag made of heat-resistant rubber, etc., and the ring method, in which only the edge of the glass is covered and sealed with a rubber ring, and either method may be used. After preliminary bonding is completed, the laminate of glass plate / intermediate film / optical film / intermediate film / glass plate taken out of the rubber bag, or the laminate with the rubber ring removed, is placed in an autoclave and heated at 10 to 15 kg / cm. 2The mixture is heated to 120°C to 150°C under high pressure and heated and pressurized for 20 to 40 minutes under these conditions. After the treatment, the mixture is cooled to 50°C or lower and the pressure is released, and the functional glass of the present invention consisting of glass / interlayer / optical film / interlayer / glass is taken out from the autoclave.
[0093] In the above embodiment, the intermediate film is disposed between the glass plate and the optical film as one independent film, but instead, the intermediate film may be disposed in a state in which it is directly laminated on the optical film in advance, that is, in the state of an optical laminate. Specifically, an optical laminate in which at least one of the two intermediate films is directly laminated on the optical film in advance may be used. By using such an intermediate film, the process of disposing the intermediate film between the optical film and the glass plate can be omitted, and as a result, it is possible to reduce the manufacturing cost.
[0094] The functional glass thus obtained can be used as the windshield, side glass, rear glass, and roof glass of ordinary cars, small cars, and light cars, as well as large and small special purpose cars. It can also be used as windows for railroad cars, ships, and aircraft, and as window materials for building materials and industrial use. As for the form of use, it can be laminated or pasted with members having UV-cutting or dimming functions.
[0095] <Head-up display system> The optical film of the present invention is suitable for use in a head-up display system because it has excellent adhesion and appearance when laminated with the optical film. FIG. 1 shows an embodiment of the HUD system of the present invention. The HUD system shown in FIG. 1 includes a display device 2 that outputs display light showing a display image as P-polarized light, a reflector 3 that reflects the display light emitted from the display device 2, and the functional glass 4 of the present invention to which the P-polarized light or S-polarized light emitted from the display device 2 is incident. The P-polarized light or S-polarized light emitted from the display device 2 is reflected by the reflector 3, and the reflected display light is irradiated onto the functional glass 4 of the present invention that functions as a windshield, whereby the P-polarized light or S-polarized light reaches the observer 1 via the optical path 5, and the observer 1 can view the display image 6 as a virtual image. In the HUD system shown in FIG. 1, the display light emitted from the display device 2 is incident on the functional glass 4 via the reflector 3, but may be incident directly from the display device 2 onto the functional glass 4.
[0096] <Display> The display 2 is not particularly limited as long as it can emit the desired P-polarized or S-polarized light before finally reaching the functional glass 4, and examples thereof include a liquid crystal display (LCD) and an organic electroluminescence display (OELD). When the display 2 is a liquid crystal display, the emitted light is usually linearly polarized, and can be used as is. On the other hand, when the display 2 is an organic electroluminescence display, the display 2 may be composed of a light source 2A and a polarizing plate 2B capable of emitting P-polarized or S-polarized light, as shown in FIG. 2. When the HUD system is used in an automobile, the liquid crystal display and the organic electroluminescence display can be adjusted so that P-polarized or S-polarized light can be emitted from the display 2 by arranging optical members such as a polarizing plate and a half-wave plate at a light exit such as a dashboard. The light source used in the display 2 is also not particularly limited, and a laser light source, an LED light source, or the like can be used. In addition, the central reflection wavelength of the retardation element constituting the optical functional layer can be set to correspond to the emission spectrum of the above-mentioned light source, thereby making the displayed image clearer more effectively.
[0097] In the HUD system of the present invention, the display light emitted from the display 2 is P-polarized light, and further, when the Brewster angle of the P-polarized light with respect to the functional glass is α, the incident angle of the P-polarized light incident on the functional glass 4 is preferably in the range of α-10° to α+10°. That is, by making the P-polarized light from the display 2 incident on the functional glass 4 at an incident angle close to the Brewster angle, the reflection of the P-polarized light on the glass plate surface of the functional glass 4 is significantly reduced. In the optical laminate constituting the functional glass 4, when an optical film having a 1 / 2 wavelength plate is used as the optical functional layer, the P-polarized light transmitted through the glass plate is converted to S-polarized light by the 1 / 2 wavelength plate constituting the optical functional layer, and the converted S-polarized light is reflected at the interface of the other glass plate. The reflected S-polarized light is converted back to P-polarized light by the 1 / 2 wavelength plate, and this P-polarized light reaches the observer. As a result, the display image is visible to the observer as a virtual image. On the other hand, when the incident angle of P polarized light is less than α-10° or more than α+10°, the incident angle of P polarized light deviates from the vicinity of Brewster's angle, so the reflectance of P polarized light increases and double images may occur. In this way, by adjusting the incident angle of P polarized light to the vicinity of Brewster's angle, the occurrence of double images can be significantly reduced. In addition, since the reflected light from the road surface is generally S polarized, the observer may use polarized sunglasses. Since polarized sunglasses are designed to absorb S polarized light, the visibility of the HUD display image through the polarized sunglasses is extremely reduced in conventional HUD systems using S polarized light. On the other hand, if the HUD system uses P polarized light, which allows P polarized light to reach the observer, the occurrence of double images can be suppressed and the visibility of the display image can be improved even when wearing polarized sunglasses.
[0098] <Reflector> The HUD system of the present invention may include a reflecting mirror as necessary. The reflecting mirror is not particularly limited as long as it can reflect the display light from the display device toward the optical laminate, and may be, for example, a flat mirror, a concave mirror, or the like. When a concave mirror is used as the reflecting mirror, the concave mirror can also magnify the display light from the display device at a predetermined magnification ratio. EXAMPLES
[0099] The present invention will be described in detail below with reference to examples. Note that the present invention is not limited to the following examples as long as it does not depart from the spirit of the invention, and in the examples, "parts" means parts by mass.
[0100] [Example 1] <Preparation of Coating Solution (Liquid Crystal Composition)> A coating solution A having the composition shown in Table 1 was prepared.
[0101] [Table 1]
[0102] <Preparation of UV-curable resin coating solution for forming blocking layer> A coating solution B of an ultraviolet curable resin composition (resin composition for forming a blocking layer) having the composition shown in Table 2 was prepared.
[0103] [Table 2]
[0104] <Preparation of optical film> Each optical film was produced by the following procedure using the prepared coating solution A. The plastic substrate used as the supporting substrate was a TAC film (thickness: 80 μm) that had been previously subjected to a rubbing treatment by the method described in Example 1 of JP-A No. 2002-90743.
[0105] (1) Coating solution A was applied at room temperature onto the rubbed surface of a TAC film using a wire bar so that the thickness of the half-wave plate as the optical functional layer obtained after drying would be 2 μm. (2) The obtained coating film was heated at 50°C for 2 minutes to remove the solvent and to form a liquid crystal phase. Next, a high-pressure mercury lamp (manufactured by Harrison Toshiba Lighting Co., Ltd.) was used for 120 W output and UV irradiation was performed for 5 to 10 seconds to fix the liquid crystal phase, thereby producing a 1 / 2 wavelength plate in which a polymerizable liquid crystal layer was laminated on a TAC film. (3) Coating solution B, which is a resin composition for forming a block layer, was applied to the polymerizable liquid crystal layer side of the 1 / 2 wavelength plate at room temperature using a wire bar so that the thickness of the resulting block layer after drying would be 3.0 μm. (4) The obtained coating film was heated at 80°C for 1 minute to remove the solvent, and then irradiated with UV light from a high pressure mercury lamp (Harrison Toshiba Lighting Co., Ltd.) at 120 W output for 5 to 10 seconds to laminate a block layer on the polymerizable liquid crystal layer side of the 1 / 2 wavelength plate. In this way, an optical film was produced in which one side of the 1 / 2 wavelength plate had a block layer and one side of the 1 / 2 wavelength plate was a support substrate (TAC film). The obtained optical film was placed between polarizing plates arranged in parallel, and the transmittance when polarized light was converted was measured using Shimadzu Corporation's "UV-3600 ultraviolet-visible-near infrared spectrophotometer," and the wavelength at which the transmittance was minimum, i.e., the wavelength at which the polarization conversion (performance) was maximum, was measured. As a result of the measurement, the wavelength at which the polarization conversion (performance) of the optical film was maximum was 545 nm.
[0106] <Preparation of optical laminate> Two transparent intermediate films made of polyvinyl butyral resin containing triethylene glycol-di-2-ethylhexanoate as a plasticizer and having a thickness of 0.38 mm were used, and the prepared optical film was placed between the intermediate films of polyvinyl butyral film. Next, the optical film and the two intermediate films were pressurized and bonded together by a laminator to prepare an optical laminate.
[0107] <Production of functional glass> The produced optical laminate was placed between two glass plates, each having a thickness of 2 mm, and then pressure and heat were applied by the following method to produce functional glass.
[0108] First, the prepared optical laminate and a transparent glass plate were stacked on top of each other in this order on a transparent glass plate. Next, the excess part of the optical laminate that protruded from the edge of the glass plate was cut and removed. This was wrapped in a rubber bag and degassed for 10 minutes in an autoclave heated to 90°C for preliminary bonding. The pre-pressurized optical laminate was cooled to room temperature, then removed from the rubber bag, and heated and pressed again in an autoclave at 135°C and a high pressure of 12 kg / cm2 for 30 minutes. In this way, functional glass with good appearance was produced. The total light transmittance of the prepared functional glass was measured to be 89.5%, which was an excellent transmittance. The total light transmittance was measured using a fully automatic haze meter "TC-HIIIDPK" manufactured by Tokyo Denshoku Co., Ltd., in accordance with JIS standard product K7105.
[0109] [Examples 2 to 8, Comparative Examples 1 to 3] The optical films, optical laminates, and functional glass according to Examples 2 to 8 and Comparative Examples 1 to 3 were produced in the same manner as in Example 1, except that the thermoplastic resin (B-1) in Table 2 was changed to the thermoplastic resin shown in Table 3. Comparative Example 1 did not have a block layer, and Comparative Examples 2 and 3 had a configuration in which the block layer did not contain a thermoplastic resin. The total light transmittance of the functional glass of Comparative Example 3 was measured in the same manner as in Example 1, and was 88.5%.
[0110] The properties of the optical films and the functional glasses according to Examples 1 to 8 and Comparative Examples 1 to 3 were measured and evaluated as follows.
[0111] <Amount of wavelength shift due to autoclave processing> The minimum wavelength in the polarization conversion when functional glass was produced from the optical film was measured, and the difference was calculated as the amount of wavelength shift S1 (nm) due to autoclave processing. The results are shown in Table 3. The amount of wavelength shift S1 (nm) due to autoclave processing was calculated as follows.
[0112]
number
[0113] <Heat resistance evaluation> The functional glasses obtained in the examples and comparative examples were placed in a high-temperature atmosphere at 120°C for 1200 hours, and the wavelength shift was measured before and after placement. The results are shown in Table 3. The wavelength shift amount S2 (nm) by the durability test, which indicates the degree of change in retardation value, was calculated as follows.
[0114]
number
[0115] <Hue change (ΔE)> In the C region, optical film measurement test pieces according to Examples 1 to 8 and Comparative Examples 1 to 3 were cut out with dimensions of 50 mm x 50 mm, and the test pieces were set so that the normal line of the film plane coincided with the incident light using a spectrophotometer CM-3600A manufactured by Konica Minolta, Inc., and the chromaticity a*, chromaticity b*, and lightness L* of arbitrary points on the test pieces were measured with transmitted light under target mask conditions with a measurement diameter of Φ8 mm. Then, the test pieces were moved so that they were spaced 20 mm or more from the center of the measurement point, and the same measurement was repeated four times, and the chromaticity a*, chromaticity b*, and lightness L* of the C region were determined as a*C, b*C, and L*C, respectively, from the average values of the five measurements. Similar measurements were also performed on area E, and the chromaticity a*, chromaticity b*, and lightness L* of area E were determined as a*E, b*E, and L*E, respectively, from the average values of five measurements. The hue change ΔE was calculated using the combination of chromaticity a*, chromaticity b*, and lightness L* of areas C and E using formulas (V) to (VIII). The results of the hue change ΔE are shown in Table 3. The hue change test was performed for 1200 hours under 100℃-dry conditions using a heat resistance accelerated tester.
[0116] ΔL*=L*CL*E (V) Δa*=a*Ca*E (VI) Δb*=b*Cb*E (VII) ΔE=((ΔL*)2+(Δa*)2+(Δb*)2)1 / 2...(VIII)
[0117] <Haze measurement> The functional glass was measured and evaluated using a haze meter, and the results are shown in Table 3.
[0118] <Adhesion> The adhesion was evaluated by a pummel test. Specifically, the functional glass was placed in a freezer at a temperature of -18°C ± 0.6°C for 16 hours, and then the center of the functional glass (a portion measuring 150 mm in length x 150 mm in width) was hit with a hammer with a 0.45 kg head to crush the glass until the particle size was 6 mm or less. The degree of exposure of the block layer after the glass was partially peeled off was judged by the pummel value. The pummel value obtained was evaluated according to the following criteria, with a grade of "△" or higher deemed a pass. The results are shown in Table 3.
[0119] ○: No peeling △: No peeling after hitting with a hammer, but can be peeled off by hand ×: Peeling occurs after hitting with a hammer
[0120] <Optical distortion> The functional glass was visually evaluated for the presence or absence of optical distortion when viewed through it and when light was reflected. When no distortion was observed in the image, it was rated as "○", when slight distortion was observed in the image, it was rated as "△", and when distortion was observed in the image, it was rated as "×". A rating of "△" or higher was considered a pass. The results are shown in Table 3.
[0121] [Table 3]
[0122] KS-10: Polyvinyl acetoacetal resin (manufactured by Sekisui Chemical Co., Ltd., product name "S-LEC KS-10") BL-1: Polyvinyl butyral resin (manufactured by Sekisui Chemical Co., Ltd., product name "S-LEC BL-1") BM-S: Polyvinyl butyral resin (manufactured by Sekisui Chemical Co., Ltd., product name "S-LEC BM-S") BL-S: Polyvinyl butyral resin (manufactured by Sekisui Chemical Co., Ltd., product name "S-LEC BL-S") MD-1480: Polyester resin (manufactured by Toyobo Co., Ltd., product name "Vylonal MD-1480") MD-2000: Polyester resin (manufactured by Toyobo Co., Ltd., product name "Vylonal MD-2000") UR-1700: Polyester urethane resin (manufactured by Toyobo Co., Ltd., product name "Vylon UR1700") LIR-403: Isoprene resin (manufactured by Kuraray, product name "Kuraray LIR-403") PET30: Pentaerythritol triacrylate (manufactured by Nippon Kayaku Co., Ltd., product name "KAYARAD PET30") UX-4101: Urethane resin (manufactured by Nippon Kayaku Co., Ltd., product name "KAYARAD UX-4101")
[0123] From Table 3, the functional glasses produced in Examples 1 to 8 having a block layer containing a thermoplastic resin all exhibited superior properties in wavelength shift S1 during autoclave processing, wavelength shift amount S2 in durability test, and hue change ΔE, compared to the functional glasses produced in Comparative Examples 1 to 3. Therefore, in Examples 1 to 8, optical films having high durability and capable of suppressing changes in the retardation value of a retardation element over a long period of time under a high-temperature atmosphere could be provided.
[0124] On the other hand, the functional glass produced in Comparative Example 1, which does not have a blocking layer, had a large wavelength shift S1 during autoclave processing and a large wavelength shift S2 in the durability test, and was poor in durability and optical performance in a high-temperature atmosphere. Also, peeling was observed between the blocking layer and the PVB layer in the adhesion test.
[0125] The functional glasses produced in Comparative Examples 2 and 3, which did not have a thermoplastic resin in the block layer, also showed a large wavelength shift S1 during autoclave processing and a large wavelength shift S2 in the durability test, and were inferior in durability and optical performance in a high-temperature atmosphere. Also, distortion was observed in the image in the optical distortion evaluation.
[0126] Thus, the present invention can provide an optical film that effectively improves the reflectance of only a specific polarized light while maintaining a high visible light transmittance, has high durability, and can suppress changes in retardation value over a long period of time, as well as an optical laminate, functional glass, and a head-up display system using the same. In addition, the block layer used in the optical film of the present invention can be easily laminated with the optical laminate such as the retardation element, and is useful because it has excellent workability. [Explanation of symbols]
[0127] 1: Observer 2: Display 2A: Light source 2B: Polarizing plate 3:Reflector 4: Functional glass 5: Optical path 6: Display image 10: Optical film 101: Optical functional layer 102: Block layer 20: Optical laminate 201: Interlayer 30: Functional glass 301: Glass plate
Claims
1. An optical film comprising (A) an optical functional layer and (B) a blocking layer, the (B) blocking layer has a cured product of a resin composition containing (B-1) a thermoplastic resin and (B-2) an ultraviolet-curable resin, The (B-1) thermoplastic resin is a polyvinyl acetal resin, The optical film, wherein the ultraviolet-curable resin (B-2) is a resin having a (meth)acryloyl group.
2. 2. The optical film according to claim 1, wherein the thermoplastic resin (B-1) is a thermoplastic resin having a molecular weight of 10,000 or more and 60,000 or less.
3. 3. The optical film according to claim 1, wherein the thermoplastic resin (B-1) is a polyvinyl acetoacetal resin.
4. 4. The optical film according to claim 1, wherein the content of the thermoplastic resin (B-1) in the block layer is from 1% by mass to 80% by mass.
5. 5. The optical film according to claim 1, wherein the resin having a (meth)acryloyl group is an epoxy (meth)acrylate resin.
6. 6. The optical film according to claim 1, wherein the blocking layer (B) has a glass transition temperature of 80°C or higher and 300°C or lower.
7. 7. The optical film according to claim 1, wherein the optical functional layer (A) is any one of the following (A-1) to (A-4): (A-1) 1 / 2 wavelength plate, (A-2) 1 / 4 wavelength plate, (A-3) A laminate of a half-wave plate and a circularly polarized light reflective layer, and (A-4) Laminate of a quarter-wave plate and a circularly polarized light reflective layer
8. 8. The optical film according to claim 7, wherein the half-wave plate or the quarter-wave plate includes a polymerizable liquid crystal layer as a layer having a function of converting a polarization axis.
9. The optical film according to claim 1 , further comprising: (C) a supporting substrate.
10. An optical laminate comprising the optical film according to claim 1 and an intermediate film laminated thereon.
11. A functional glass comprising the optical laminate according to claim 10 and a glass plate.
12. A head-up display system comprising: the optical film according to any one of claims 1 to 9; the optical laminate according to claim 10; or the functional glass according to claim 11; and an image display means that emits display light showing an image display.
Citation Information
Patent Citations
Head up display and automobile
CN108761789A
Scratching resistant antidazzle film, polarizing plate and its production
JP1994018706A
Display device
JP1994040271A
Optical element and image projection system having the same
JP2017198951A
Light reflection film, and optical film using the same, functional glass, and head-up display