Optical Film
The optical film with specific retardation layers formed by polymerizing liquid crystals or stretched films addresses light leakage issues in flat panel displays, enhancing image quality by improving optical compensation.
Patent Information
- Application Number
- JP2022141657
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-01-31
- Filing Date
- 2022-09-06
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2034-08-07
AI Technical Summary
Conventional optical films do not adequately suppress light leakage during black display in flat panel display devices.
The optical film comprises a first and a second retardation layer with specific optical properties, optionally with a third retardation layer, formed by polymerizing polymerizable liquid crystals or stretched films, to achieve optimal optical compensation.
The film effectively suppresses light leakage during black display, ensuring better image quality in flat panel displays.
Smart Images

Figure 0007573000000030 
Figure 0007573000000031 
Figure 0007573000000032
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film. [Background technology]
[0002] In flat panel displays (FPDs), components including optical films such as polarizing plates and retardation plates are used. As such optical films, optical films manufactured by applying a composition containing a polymerizable liquid crystal to a substrate are known. For example, Patent Document 1 describes such optical films that exhibit reverse wavelength dispersion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2010-537955 Summary of the Invention [Problem to be solved by the invention]
[0004] However, conventional optical films are not sufficient in terms of optical compensation properties, that is, suppressing light leakage during black display. [Means for solving the problem]
[0005] The present invention includes the following inventions. [1] An optical film having a first retardation layer and a second retardation layer, The second retardation layer has an optical characteristic represented by formula (3), The optical film has optical properties represented by formulas (1) and (2). Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) nx≒ny <nz (3) (In the formula, Re(450) represents an in-plane retardation value at a wavelength of 450 nm, Re(550) represents an in-plane retardation value at a wavelength of 550 nm, and Re(650) represents an in-plane retardation value at a wavelength of 650 nm. nx represents a principal refractive index in a direction parallel to the film plane in an index ellipsoid formed by the retardation layer. ny represents a refractive index in a direction parallel to the film plane and perpendicular to the direction of nx in an index ellipsoid formed by the retardation layer. nz represents a refractive index in a direction perpendicular to the film plane in an index ellipsoid formed by the retardation layer.) [2] The optical film according to [1], wherein the first retardation layer has an optical property represented by formula (4). 100nm <Re(550)<160nm (4) (In the formula, Re(550) has the same meaning as above.) [3] The optical film according to [1] or [2], wherein the first retardation layer has optical properties represented by formulas (1) and (2). Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) (In the formula, Re(450), Re(550) and Re(650) have the same meanings as above. ) [4] The first retardation layer is A layer A having optical properties represented by formulas (4), (6), and (7); and a layer B having optical properties represented by formulas (5), (6) and (7). 100nm <Re(550)<160nm (4) 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7) (In the formula, Re(450), Re(550) and Re(650) have the same meanings as above. ) [5] An optical film further comprising a third retardation layer, The optical film according to [1] or [2], wherein the third retardation layer has an optical property represented by formula (5). 200nm <Re(550)<320nm (5) (In the formula, Re(550) has the same meaning as above.) [6] The optical film according to [5], wherein the first retardation layer and the third retardation layer have optical properties represented by formulas (6) and (7). Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7) (In the formula, Re(450), Re(550) and Re(650) have the same meanings as above. ) [7] The optical film according to [5] or [6], wherein the third retardation layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals. [8] The optical film according to any one of [5] to [7], wherein the third retardation layer has a thickness of 5 μm or less. [9] The optical film according to any one of [5] to [8], wherein the third retardation layer is formed on the alignment film.
[10] The optical film according to any one of [1] to [9], wherein the first retardation layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
[11] The optical film according to any one of [1] to
[10] , wherein the second retardation layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
[12] The optical film according to any one of [1] to
[11] , wherein the first retardation layer has a thickness of 5 μm or less.
[13] The optical film according to any one of [1] to
[12] , wherein the second retardation layer has a thickness of 5 μm or less.
[14] The optical film according to any one of [1] to
[13] , wherein the first retardation layer and the second retardation layer each have a thickness of 5 μm or less.
[15] The optical film according to any one of [1] to
[14] , wherein the first retardation layer is formed on the alignment film.
[16] The optical film according to any one of [1] to
[15] , wherein the second retardation layer is formed on the alignment film.
[17] The optical film according to [9],
[15] or
[16] , wherein the alignment film is an alignment film that generates an alignment control force by light irradiation.
[18] The optical film according to [9],
[15] or
[16] , wherein the alignment film is an alignment film that exerts a vertical alignment regulating force.
[19] The optical film according to any one of
[15] to
[18] , wherein the thickness of the alignment layer is 500 nm or less.
[20] The optical film according to any one of [1] to
[19] , wherein a first retardation layer is formed on a substrate with or without an alignment film, and a second retardation layer is formed on the first retardation layer with or without an alignment film.
[21] The optical film according to any one of [1] to
[20] , wherein a second retardation layer is formed on a substrate with or without an alignment film, and a first retardation layer is formed on the second retardation layer with or without an alignment film.
[22] The optical film according to any one of [5] to
[21] , which has a first retardation layer, a second retardation layer and a third retardation layer in this order.
[23] The optical film according to any one of
[20] to
[22] , further comprising a protective layer between the first retardation layer and the second retardation layer.
[24] The optical film according to
[22] , further comprising a protective layer between the second retardation layer and the third retardation layer.
[25] The optical film according to any one of [1] to
[19] , wherein a first retardation layer is formed on one surface of a substrate with or without an alignment film, and a second retardation layer is formed on the other surface of the substrate with or without an alignment film.
[26] The optical film according to [4], wherein Layer A is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
[27] The optical film according to [4], wherein Layer B is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
[28] The optical film according to [4], wherein Layer A has a thickness of 5 μm or less.
[29] The optical film according to [4], wherein the thickness of Layer B is 5 μm or less.
[30] The optical film according to [4], wherein the thickness of Layer A and Layer B is 5 μm or less.
[31] The optical film according to [4], wherein a layer A is formed on a substrate with or without an alignment film, a layer B is formed on the layer A with or without an alignment film, and a second retardation layer is formed on the layer B with or without an alignment film.
[32] The optical film according to [4], wherein a layer B is formed on a substrate with or without an alignment film, a layer A is formed on the layer B with or without an alignment film, and a second retardation layer is formed on the layer A with or without an alignment film.
[33] The optical film according to [4], wherein a second retardation layer is formed on a substrate with or without an alignment film, a layer A is formed on the second retardation layer with or without an alignment film, and a layer B is formed on the layer A with or without an alignment film.
[34] The optical film according to [4], wherein a second retardation layer is formed on a substrate with or without an alignment film, a layer B is formed on the second retardation layer with or without an alignment film, and a layer A is formed on the layer B with or without an alignment film.
[35] The optical film according to [4], wherein a layer A is formed on one surface of a substrate with or without an alignment film, a layer B is formed on the layer A with or without an alignment film, and a second retardation layer is formed on the other surface of the substrate with or without an alignment film.
[36] The optical film according to [4], wherein a layer B is formed on one surface of a substrate with or without an alignment film, a layer A is formed on the layer B with or without an alignment film, and a second retardation layer is formed on the other surface of the substrate with or without an alignment film.
[37] The optical film according to any one of
[31] to
[36] , further comprising a protective layer between Layer A and Layer B.
[38] The optical film according to [5], wherein a first retardation layer is formed on a substrate with or without an alignment film, a second retardation layer is formed on the first retardation layer with or without an alignment film, and a third retardation layer is formed on the second retardation layer with or without an alignment film.
[39] The optical film according to [5], wherein a third retardation layer is formed on a substrate with or without an alignment film, a second retardation layer is formed on the third retardation layer with or without an alignment film, and a first retardation layer is formed on the second retardation layer with or without an alignment film.
[40] The optical film according to [5], wherein a first retardation layer is formed on one surface of a substrate with or without an alignment film, a second retardation layer is formed on the first retardation layer with or without an alignment film, and a third retardation layer is formed on the other surface of the substrate with or without an alignment film.
[41] The optical film according to [5], wherein a second retardation layer is formed on one surface of a substrate with or without an alignment film, a first retardation layer is formed on the second retardation layer with or without an alignment film, and a third retardation layer is formed on the other surface of the substrate with or without an alignment film.
[42] The optical film according to [5], wherein a third retardation layer is formed on one surface of a substrate with or without an alignment film, a second retardation layer is formed on the third retardation layer with or without an alignment film, and a first retardation layer is formed on the other surface of the substrate with or without an alignment film.
[43] The optical film according to [5], wherein a second retardation layer is formed on one surface of a substrate with or without an alignment film, a third retardation layer is formed on the second retardation layer with or without an alignment film, and a first retardation layer is formed on the other surface of the substrate with or without an alignment film.
[44] A circularly polarizing plate comprising the optical film according to any one of [1] to
[43] and a polarizing plate.
[45] The circularly polarizing plate according to
[44] , wherein the optical film and the polarizing plate are bonded together with an active energy ray-curable adhesive or a water-based adhesive.
[46] An organic electroluminescence display device comprising the circular polarizer according to
[44] or
[45] .
[47] A touch panel display device comprising the circular polarizer according to
[44] or
[45] . Effect of the Invention
[0006] According to the present invention, it is possible to provide an optical film that is excellent in suppressing light leakage during black display. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of an optical film of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of an optical film of the present invention. [Diagram 3] 1 is a schematic cross-sectional view of a circularly polarizing plate including an optical film of the present invention. [Figure 4] 1 is a schematic cross-sectional view of a circularly polarizing plate including an optical film of the present invention. [Diagram 5] 1 is a cross-sectional schematic diagram of an organic EL display device including an optical film of the present invention. [Figure 6] 1 is a schematic diagram of an organic EL display device including an optical film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The optical film of the present invention (hereinafter sometimes referred to as the present optical film) has a first retardation layer and a second retardation layer. It may also have a third retardation layer. The first retardation layer, the second retardation layer, and the third retardation layer are retardation layers having certain optical properties, and each of the first retardation layer, the second retardation layer, and the third retardation layer may be composed of two or more layers. The present optical film has optical properties represented by formulas (1) and (2). In order for the present optical film to have such optical properties, the first retardation layer, the second retardation layer, or the third retardation layer may have the optical properties represented by formulas (1) and (2), or at least two selected from the first retardation layer, the second retardation layer, and the third retardation layer may be combined to exhibit the optical properties represented by formulas (1) and (2). Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) In this specification, Re(450) represents an in-plane retardation value at a wavelength of 450 nm, Re(550) represents an in-plane retardation value at a wavelength of 550 nm, and Re(650) represents an in-plane retardation value at a wavelength of 650 nm.
[0009] [Phase difference layer] Examples of the retardation layer include a layer formed by polymerizing a polymerizable liquid crystal and a stretched film. The optical properties of the retardation layer can be adjusted by the orientation state of the polymerizable liquid crystal or the stretching method of the stretched film.
[0010] <Layer formed by polymerizing polymerizable liquid crystal> In the present invention, the polymerizable liquid crystal whose optical axis is aligned horizontally to the substrate plane is defined as horizontal alignment, and the polymerizable liquid crystal whose optical axis is aligned perpendicularly to the substrate plane is defined as vertical alignment. The optical axis means the direction in which a cross section cut in a direction perpendicular to the optical axis of an index ellipsoid formed by the orientation of the polymerizable liquid crystal is a circle, that is, the direction in which the refractive indexes in the three directions are all equal.
[0011] The polymerizable liquid crystal may be a rod-shaped polymerizable liquid crystal or a disc-shaped polymerizable liquid crystal. When the rod-shaped polymerizable liquid crystal is aligned horizontally or vertically to the substrate, the optical axis of the polymerizable liquid crystal coincides with the long axis direction of the polymerizable liquid crystal. When the discotic polymerizable liquid crystal is aligned, the optical axis of the polymerizable liquid crystal is in a direction perpendicular to the disc surface of the polymerizable liquid crystal.
[0012] The direction of the slow axis of a stretched film varies depending on the stretching method, and the slow axis and optical axis are determined according to the stretching method, such as uniaxial, biaxial or oblique stretching.
[0013] In order for the layer formed by polymerizing the polymerizable liquid crystal to exhibit an in-plane retardation, the polymerizable liquid crystal may be aligned in an appropriate direction. When the polymerizable liquid crystal is rod-shaped, the in-plane retardation is exhibited by aligning the optical axis of the polymerizable liquid crystal horizontally to the substrate plane, in which case the optical axis direction and the slow axis direction are the same. When the polymerizable liquid crystal is disc-shaped, the in-plane retardation is exhibited by aligning the optical axis of the polymerizable liquid crystal horizontally to the substrate plane, in which case the optical axis and the slow axis are perpendicular to each other. The alignment state of the polymerizable liquid crystal can be adjusted by the combination of the alignment film and the polymerizable liquid crystal.
[0014] The in-plane retardation value of the retardation layer can be adjusted by the thickness of the retardation layer. Since the in-plane retardation value is determined by formula (10), the desired in-plane retardation value (Re(λ)) can be obtained by adjusting Δn(λ) and the film thickness d. Re(λ)=d×Δn(λ) (10) In the formula, Re(λ) represents the in-plane retardation value at a wavelength of λ nm, d represents the film thickness, and Δn(λ) represents the birefringence at a wavelength of λ nm.
[0015] Birefringence Δn(λ) is obtained by measuring the in-plane retardation value and dividing it by the thickness of retardation layer.Specific measuring method is shown in Examples, but in this case, by measuring the film formed on the substrate that does not have the in-plane retardation of the substrate itself such as a glass substrate, the actual characteristics of retardation layer can be measured.
[0016] In the present invention, the refractive indices in three directions in the refractive index ellipsoid formed by the alignment of the polymerizable liquid crystal or the stretching of the film are represented as nx, ny, and nz. nx represents the principal refractive index in the direction parallel to the film plane in the refractive index ellipsoid formed by the retardation layer. ny represents the refractive index in the direction parallel to the film plane and orthogonal to the direction of nx in the refractive index ellipsoid formed by the retardation layer. nz represents the refractive index in the direction perpendicular to the film plane in the refractive index ellipsoid formed by the retardation layer.
[0017] When the optical axis of the rod-shaped polymerizable liquid crystal is oriented horizontally with respect to the substrate plane, the refractive index relationship of the obtained retardation layer is nx > ny ≒ nz (positive A plate), and the axis in the direction of nx in the refractive index ellipsoid coincides with the slow axis.
[0018] Also, when the optical axis of the disk-shaped polymerizable liquid crystal is oriented horizontally with respect to the substrate plane, the refractive index relationship of the obtained retardation layer is nx < ny ≒ nz (negative A plate), and the axis in the direction of ny in the refractive index ellipsoid coincides with the slow axis.
[0019] In order for the layer formed by polymerizing the polymerizable liquid crystal to exhibit a retardation in the thickness direction, the polymerizable liquid crystal may be oriented in a suitable direction. In the present invention, exhibiting a retardation in the thickness direction is defined as a characteristic in which Rth (retardation value in the thickness direction) is negative in formula (20). Rth can be calculated from the retardation value (R 40 ) measured by tilting 40 degrees with the in-plane fast axis as the tilt axis and the in-plane retardation value (Re). That is, Rth can be calculated by obtaining nx, ny, and nz from Re, R 40 , d (thickness of the retardation layer), and n0 (average refractive index of the retardation layer) according to the following formulas (21) to (23) and substituting them into formula (20). Rth = [(nx + ny) / 2 - nz] × d (20) Re = (nx - ny) × d (21) R 40 = (nx - ny') × d / cos(φ) (22) (nx + ny + nz) / 3 = n0 (23) Here, φ = sin -1 [sin(40°) / n0] ny' = ny × nz / [ny 2 × sin 2 (φ) + nz 2 × cos 2 (φ)] 1 / 2 Also, nx, ny, and nz are the same as the aforementioned definitions.
[0020] When the polymerizable liquid crystal is rod-shaped, a retardation in the thickness direction is developed by orienting the optical axis of the polymerizable liquid crystal perpendicular to the substrate plane. When the polymerizable liquid crystal is disk-shaped, a retardation in the thickness direction is developed by orienting the optical axis of the polymerizable liquid crystal horizontally with respect to the substrate plane. In the case of a disk-shaped polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is parallel to the substrate plane, when Re is determined, the thickness is fixed, and thus Rth is uniquely determined. However, in the case of a rod-shaped polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is perpendicular to the substrate plane, Rth can be adjusted without changing Re by adjusting the thickness of the retardation layer.
[0021] When the optical axis of the rod-shaped polymerizable liquid crystal is oriented perpendicular to the substrate plane, the refractive index relationship of the resulting retardation layer is nx ≈ ny < nz (positive C-plate), and the axis in the nz direction in the refractive index ellipsoid coincides with the slow axis direction.
[0022] Also, when the optical axis of the disk-shaped polymerizable liquid crystal is oriented parallel to the substrate plane, the refractive index relationship of the resulting retardation layer is nx < ny ≈ nz (negative A-plate), and the axis in the ny direction in the refractive index ellipsoid coincides with the slow axis direction.
[0023] <Polymerizable Liquid Crystal> The polymerizable liquid crystal is a compound having a polymerizable group and liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred. The liquid crystallinity of the polymerizable liquid crystal may be a thermotropic liquid crystal or a lyotropic liquid crystal, and when the thermotropic liquid crystal is classified according to the degree of order, it may be a nematic liquid crystal or a smectic liquid crystal.
[0024] Examples of the rod-shaped polymerizable liquid crystal include a compound represented by the following formula (A) (hereinafter, sometimes referred to as polymerizable liquid crystal (A)) and a compound containing a group represented by the following formula (X) (hereinafter, sometimes referred to as polymerizable liquid crystal (B)).
[0025] TIFF0007573000000001.tif3280[In formula (A), X 1 is an oxygen atom, a sulfur atom or -NR 1 - represents. R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Y 1 represents a monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms which may have a substituent, or a monovalent aromatic heterocyclic group having 3 to 12 carbon atoms which may have a substituent. Q 3 and Q 4 each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms which may have a substituent, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, -NR 2 R 3 or -SR2 or Q 3 and Q 4 and bond to each other to form an aromatic ring or a heteroaromatic ring together with the carbon atom to which they are attached. 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. D 1 and D. 2 each independently represents a single bond, -C(=O)-O-, -C(=S)-O-, or -CR 4 R 5 -, -CR 4 R 5 -CR 6 R 7 -, -O-CR 4 R 5 -, -CR 4 R 5 -O-CR 6 R 7 -,-CO-O-CR 4 R 5 -, -O-CO-CR 4 R 5 -, -CR 4 R 5 -O-CO-CR 6 R 7 -, -CR 4 R 5 -CO-O-CR 6 R 7 -OR-NR 4 -CR 5 R 6 -or-CO-NR 4 - represents. R 4 , R 5 , R 6 and R 7 each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 4 carbon atoms. G 1 and G 2 each independently represents a divalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, a methylene group constituting the alicyclic hydrocarbon group may be replaced by an oxygen atom, a sulfur atom, or NH-, and a methine group constituting the alicyclic hydrocarbon group may be replaced by a tertiary nitrogen atom. L 1 and L 2 each independently represents a monovalent organic group; L 1 and L 2 At least one of the groups has a polymerizable group.
[0026] L in polymerizable liquid crystal (A) 1 is preferably a group represented by formula (A1), and L 2 is preferably a group represented by formula (A2). P1-F1-(B1-A1)k-E1- (A1) P2-F2-(B2-A2)l-E2- (A2) [In formula (A1) and formula (A2), B1, B2, E1 and E2 each independently represent -CR 4 R 5 -, -CH2-CH2-, -O-, -S-, -CO-O-, -O-CO-O-, -CS-O-, -O-CS-O-, -CO-NR 1 Represents -, -O-CH2-, -S-CH2- or a single bond. A1 and A2 each independently represent a divalent alicyclic hydrocarbon group having 5 to 8 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, a methylene group constituting the alicyclic hydrocarbon group may be replaced by an oxygen atom, a sulfur atom, or NH-, and a methine group constituting the alicyclic hydrocarbon group may be replaced by a tertiary nitrogen atom. k and l each independently represent an integer of 0 to 3. F1 and F2 represent a divalent aliphatic hydrocarbon group having 1 to 12 carbon atoms. P1 represents a polymerizable group. P2 represents a hydrogen atom or a polymerizable group. R 4 and R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms.]
[0027] Preferred examples of the polymerizable liquid crystal (A) include the compounds described in JP-A-2011-207765.
[0028] P11-B11-E11-B12-A11-B13- (X) In formula (X), P11 represents a polymerizable group. A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. A hydrogen atom contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, or a nitro group, and a hydrogen atom contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom. B11 is -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -, -NR 16 Represents -CO-, -CO-, -CS- or a single bond. R 16 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. B12 and B13 each independently represent -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -, -NR 16 It represents -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond. E11 represents an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and a hydrogen atom contained in the alkoxy group may be substituted with a halogen atom. In addition, -CH2- constituting the alkanediyl group may be substituted with -O- or -CO-.]
[0029] The number of carbon atoms in the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. A11 is preferably a cyclohexane-1,4-diyl group or a 1,4-phenylene group.
[0030] E11 is preferably a linear alkanediyl group having 1 to 12 carbon atoms. -CH2- constituting the alkanediyl group may be replaced with -O-. Specific examples include linear alkanediyl groups having 1 to 12 carbon atoms, such as a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a nonane-1,9-diyl group, a decane-1,10-diyl group, an undecane-1,11-diyl group, and a dodecane-1,12-diyl group; -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2-, and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-O-CH2-CH2-. As B11, -O-, -S-, -CO-O-, and -O-CO- are preferable, and among them, -CO-O- is more preferable. As B12 and B13, each independently, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)- or -OC(=O)-O- is preferable, and among them, -O- or -OC(=O)-O- is more preferable.
[0031] As the polymerizable group represented by P11, a radically polymerizable group or a cationic polymerizable group is preferred from the viewpoint of high polymerization reactivity, particularly high photopolymerization reactivity. In addition, the polymerizable group is preferably a group represented by the following formulae (P-11) to (P-15), since it is easy to handle and the liquid crystal compound can be easily produced. TIFF0007573000000002.tif34155 [Formula (P-11) to (P-15), R 17 ~R 21each independently represents an alkyl group having 1 to 6 carbon atoms or a hydrogen atom.
[0032] Specific examples of the groups represented by formulae (P-11) to (P-15) include groups represented by the following formulae (P-16) to (P-20). TIFF0007573000000003.tif29132
[0033] P11 is preferably a group represented by formula (P-14) to formula (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group or an oxetanyl group. The group represented by P11-B11- is more preferably an acryloyloxy group or a methacryloyloxy group.
[0034] The polymerizable liquid crystal (B) may be a compound represented by formula (I), formula (II), formula (III), formula (IV), formula (V) or formula (VI). P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (I) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11 (II) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12 (III) P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (IV) P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (V) P11-B11-E11-B12-A11-B13-A12-F11 (VI) (In the formula, A12 to A14 each independently have the same meaning as A11, B14 to B16 each independently have the same meaning as B12, B17 has the same meaning as B11, and E12 has the same meaning as E11. F11 represents a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxy group, a methylol group, a formyl group, a sulfo group (-SO3H), a carboxy group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and -CH2- constituting the alkyl group and the alkoxy group may be replaced with -O-.
[0035] Specific examples of the polymerizable liquid crystal (B) include compounds having a polymerizable group among the compounds described in “3.8.6 Network (completely crosslinked type)” and “6.5.1 Liquid crystal materials b. Polymerizable nematic liquid crystal materials” in the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), and the polymerizable liquid crystals described in JP-A Nos. 2010-31223, 2010-270108, 2011-6360, and 2011-207765.
[0036] Specific examples of the polymerizable liquid crystal (B) include compounds represented by the following formulae (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2), and (VI-1) to (VI-6). In the following formulae, k1 and k2 each independently represent an integer of 2 to 12. These polymerizable liquid crystals (B) are preferred in terms of ease of synthesis or availability.
[0037] TIFF0007573000000004.tif78147
[0038] TIFF0007573000000005.tif78148
[0039] TIFF0007573000000006.tif152150
[0040] TIFF0007573000000007.tif216147
[0041] TIFF0007573000000008.tif126139
[0042] TIFF0007573000000009.tif248140
[0043] TIFF0007573000000010.tif83142
[0044] TIFF0007573000000011.tif11994
[0045] TIFF0007573000000012.tif141123
[0046] An example of the discotic polymerizable liquid crystal is a compound containing a group represented by formula (W) (hereinafter, sometimes referred to as polymerizable liquid crystal (C)). TIFF0007573000000013.tif3868[In formula (W), R 40 represents the following formulas (W-1) to (W-5).
[0047] TIFF0007573000000014.tif7682
[0048] X 40 and Z 40 represents an alkanediyl group having 1 to 12 carbon atoms, a hydrogen atom contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and a hydrogen atom contained in the alkoxy group may be substituted with a halogen atom. In addition, -CH2- constituting the alkanediyl group may be replaced with -O- or -CO-.
[0049] Specific examples of the polymerizable liquid crystal (C) include the compounds described in "6.5.1 Liquid crystal materials b. Polymerizable nematic liquid crystal materials Figure 6.21" in the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), and the polymerizable liquid crystals described in JP-A Nos. 7-258170, 7-30637, 7-309807, and 8-231470.
[0050] A retardation layer having the optical properties represented by formulas (1) and (2) can be obtained by polymerizing a polymerizable liquid crystal having a specific structure, by stretching a polymer film having a specific structure, or by combining a layer having the optical properties represented by formulas (4), (6), and (7) with a layer having the optical properties represented by formulas (5), (6), and (7) in a specific slow axis relationship. Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) 100nm <Re(550)<160nm (4) 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7)
[0051] When the retardation layer has the optical properties represented by formulas (1) and (2), it is possible to obtain the present optical film having the optical properties represented by formulas (1) and (2). When the present optical film has the optical properties represented by formulas (1) and (2), uniform polarization conversion properties can be obtained for light of each wavelength in the visible light range, and light leakage during black display of a display device such as an organic EL display device can be suppressed.
[0052] The polymerizable liquid crystal having the specific structure may be, for example, the polymerizable liquid crystal (A). By orienting the polymerizable liquid crystal (A) so that the optical axis is horizontal to the substrate plane, a retardation layer having the optical properties represented by formulas (1) and (2) can be obtained, and further, by adjusting the film thickness according to formula (10), a retardation layer having a desired in-plane retardation value such as the optical property represented by formula (4) can be obtained. 100nm <Re(550)<160nm (4)
[0053] Methods for combining layers having the optical properties represented by formulas (4), (6), and (7) with layers having the optical properties represented by formulas (5), (6), and (7) in a specific slow axis relationship include well-known methods. For example, JP-A-10-68816 and JP-A-10-90521 disclose retardation films obtained by laminating two anisotropic polymer films.For example, JP-A-2001-4837, JP-A-2001-21720 and JP-A-2000-206331 disclose retardation films having at least two retardation layers made of liquid crystal compounds.In addition, one of the two retardation layers can be a polymer film and the other can be a retardation layer made of liquid crystal compounds.
[0054] The retardation layer having the optical properties represented by the above formulas (6) and (7) can be obtained by a known method. That is, the retardation layer obtained by a method other than the method for obtaining the retardation layer having the optical properties represented by the above formulas (1) and (2) generally has the optical properties represented by the formulas (6) and (7).
[0055] <Stretched film> A stretched film is usually obtained by stretching a substrate. As a method of stretching a substrate, for example, a roll (winding body) on which the substrate is wound is prepared, the substrate is continuously unwound from the winding body, and the unwound substrate is transported to a heating furnace. The temperature of the heating furnace is set in the range of about the glass transition temperature of the substrate (°C) to [glass transition temperature + 100] (°C), preferably in the range of about the glass transition temperature (°C) to [glass transition temperature + 50] (°C). In the heating furnace, when the substrate is stretched in the traveling direction or in a direction perpendicular to the traveling direction, the transport direction and tension are adjusted to incline at an arbitrary angle, and uniaxial or biaxial heat stretching is performed. The stretching ratio is usually 1.1 to 6 times, preferably 1.1 to 3.5 times. In addition, as a method of stretching in an oblique direction, as long as the orientation axis can be continuously inclined to a desired angle, it is not particularly limited, and a known stretching method can be adopted. Examples of such stretching methods include those described in JP-A-50-83482 and JP-A-2-113920. When imparting retardation properties to the film by stretching, the thickness after stretching is determined by the thickness before stretching and the stretching ratio.
[0056] Examples of the stretched film having retardation in the thickness direction include a stretched film having a refractive index relationship of nx < ny < nz described in JP-A-2008-129465 and a known multilayer extrusion film. Even for a film having a refractive index relationship of nx < ny < nz, since nz is relatively large, an effect equivalent to nx ≒ ny < nz can be obtained.
[0057] The in-plane retardation value and the retardation value in the thickness direction of the stretched film can be adjusted by Δn(λ) and the film thickness d, similar to the layer formed by polymerizing a polymerizable liquid crystal.
[0058] Examples of the stretched film obtained by stretching a polymer film having a specific structure and having the optical properties represented by the above formulas (1) and (2) include a commercially available stretched film made of a polycarbonate resin, specifically, "Pure Ace (registered trademark) WR" (manufactured by Teijin Limited), etc.
[0059] The substrate is usually a transparent substrate. The transparent substrate means a substrate having transparency capable of transmitting light, particularly visible light, and transparency means a property in which the transmittance for light rays having a wavelength of 380 to 780 nm is 80% or more. A specific transparent substrate is a light-transmitting resin substrate. Resins constituting the light-transmitting resin substrate include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene-based polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide, and polyphenylene oxide. From the viewpoints of availability and transparency, polyethylene terephthalate, polymethacrylic acid esters, cellulose esters, cyclic olefin resins, and polycarbonates are preferred.
[0060] Cellulose ester is a material in which some or all of the hydroxyl groups contained in cellulose are esterified, and is easily available on the market. Cellulose ester substrates are also easily available on the market. Examples of commercially available cellulose ester substrates include "FUJITAC (registered trademark) Film" (Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (Konica Minolta Opto Co., Ltd.).
[0061] Polymethacrylic acid esters and polyacrylic acid esters (hereinafter, polymethacrylic acid esters and polyacrylic acid esters may be collectively referred to as (meth)acrylic resins) ) is readily available on the market.
[0062] Examples of the (meth)acrylic resin include homopolymers of methacrylic acid alkyl esters or acrylic acid alkyl esters, and copolymers of methacrylic acid alkyl esters and acrylic acid alkyl esters. Specific examples of the methacrylic acid alkyl esters include methyl methacrylate, ethyl methacrylate, and propyl methacrylate, and specific examples of the acrylic acid alkyl esters include methyl acrylate, ethyl acrylate, and propyl acrylate. As such (meth)acrylic resins, those commercially available as general-purpose (meth)acrylic resins can be used. As the (meth)acrylic resins, those called impact-resistant (meth)acrylic resins may also be used.
[0063] In order to further improve the mechanical strength, it is also preferable to include rubber particles in the (meth)acrylic resin. The rubber particles are preferably acrylic. Here, the acrylic rubber particles are particles having rubber elasticity obtained by polymerizing an acrylic monomer mainly composed of an acrylic acid alkyl ester such as butyl acrylate or 2-ethylhexyl acrylate in the presence of a polyfunctional monomer. The acrylic rubber particles may be formed of a single layer of such particles having rubber elasticity, or may be a multilayer structure having at least one rubber elastic layer. Examples of the acrylic rubber particles having a multilayer structure include those having a particle having rubber elasticity as described above as a core and covered with a hard methacrylic acid alkyl ester polymer, those having a hard methacrylic acid alkyl ester polymer as a core and covered with an acrylic polymer having rubber elasticity as described above, and those having a hard core covered with an acrylic polymer having rubber elasticity, which is further covered with a hard methacrylic acid alkyl ester polymer. The rubber particles formed in the elastic layer usually have an average diameter in the range of about 50 to 400 nm.
[0064] The content of rubber particles in the (meth)acrylic resin is usually about 5 to 50 parts by mass per 100 parts by mass of the (meth)acrylic resin. Since the (meth)acrylic resin and the acrylic rubber particles are commercially available in a mixed state, the commercially available product can be used. Examples of commercially available (meth)acrylic resins containing acrylic rubber particles include "HT55X" and "Technoloy S001" sold by Sumitomo Chemical Co., Ltd. "Technoloy S001" is sold in the form of a film.
[0065] Cyclic olefin resins are easily available on the market. Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) [Ticona Co., Ltd. (Germany)], "Arton" (registered trademark) [JSR Co., Ltd.], "ZEONOR" (registered trademark) [Zeon Corporation, Nippon Zeon Co., Ltd.], "ZEONEX" (registered trademark) [Zeon Corporation, Nippon Zeon Co., Ltd.], and "Apel" (registered trademark) [Mitsui Chemical Co., Ltd.]. Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a substrate. In addition, commercially available cyclic olefin resin substrates can also be used. Examples of commercially available cyclic olefin resin substrates include "S-Cina" (registered trademark) [Sekisui Chemical Co., Ltd.], "SCA40" (registered trademark) [Sekisui Chemical Co., Ltd.], "ZEONOR Film" (registered trademark) [Optes Co., Ltd.], and "Arton Film" (registered trademark) [JSR Co., Ltd.].
[0066] When the cyclic olefin resin is a copolymer of a cyclic olefin and an aromatic compound having a chain olefin or a vinyl group, the content of the structural unit derived from the cyclic olefin is usually 50 mol% or less, preferably 15 to 50 mol%, based on the total structural units of the copolymer. Examples of the chain olefin include ethylene and propylene, and examples of the aromatic compound having a vinyl group include styrene, α-methylstyrene, and alkyl-substituted styrene. When the cyclic olefin resin is a ternary copolymer of a cyclic olefin, a chain olefin, and an aromatic compound having a vinyl group, the content of the structural unit derived from the chain olefin is usually 5 to 80 mol% based on the total structural units of the copolymer, and the content of the structural unit derived from the aromatic compound having a vinyl group is usually 5 to 80 mol% based on the total structural units of the copolymer. Such a ternary copolymer has the advantage that the amount of expensive cyclic olefin used can be relatively reduced in the production thereof.
[0067] [First retardation layer] The first retardation layer preferably has an optical characteristic represented by formula (4), more preferably has an optical characteristic represented by formula (4-1). The in-plane retardation value Re(550) can be adjusted by the same method as the adjustment method of the in-plane retardation value of the retardation layer. 100nm <Re(550)<160nm (4) 130nm <Re(550)<150nm (4-1)
[0068] Furthermore, the first retardation layer preferably has optical properties represented by formulas (1) and (2). Such optical properties can be obtained by the same method as for the above retardation layer. Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2)
[0069] The first retardation layer preferably has a layer A having optical properties represented by formulas (4), (6), and (7), and a layer B having optical properties represented by formulas (5), (6), and (7). Such optical properties can be obtained by the same method as that of the retardation layer. 100nm <Re(550)<160nm (4) 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7) Layer A is preferably a layer having the optical property represented by formula (4-1), and Layer B is preferably a layer having the optical property represented by formula (5-1). 130nm <Re(550)<150nm (4-1) 265nm <Re(550)<285nm (5-1)
[0070] In addition, when the optical film of the present invention has a third retardation layer, the first retardation layer preferably has optical properties represented by formulas (6) and (7). Such optical properties can be obtained by the same method as the above retardation layer. Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7)
[0071] The first retardation layer is preferably a coating layer formed by polymerizing one or more polymerizable liquid crystals. When the first retardation layer is composed of one retardation layer and has the optical properties represented by formulas (1) and (2), the retardation layer is preferably a coating layer formed by polymerizing a polymerizable liquid crystal (A). When the first retardation layer has the optical properties represented by formulas (6) and (7), the retardation layer is preferably a coating layer formed by polymerizing a polymerizable liquid crystal (B).
[0072] The layer A is preferably a coating layer formed by polymerizing a polymerizable liquid crystal (B). The layer B is preferably a coating layer formed by polymerizing a polymerizable liquid crystal (C).
[0073] When the first retardation layer is a stretched film, its thickness is usually 300 μm or less, preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When the first retardation layer is a layer formed by polymerizing a polymerizable liquid crystal, its thickness is usually 20 μm or less, preferably 5 μm or less, more preferably 0.5 μm or more and 3 μm or less. The thickness of the first retardation layer can be measured by an interference thickness meter, a laser microscope, or a stylus thickness meter. When layer A is a stretched film, its thickness is usually 150 μm or less, preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When layer A is a layer formed by polymerizing a polymerizable liquid crystal, its thickness is usually 10 μm or less, preferably 5 μm or less, more preferably 0.5 μm or more and 3 μm or less. The thickness of layer A can be determined by the same method as that of the first retardation layer. When Layer B is a stretched film, its thickness is usually 150 μm or less, preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When Layer B is a layer formed by polymerizing a polymerizable liquid crystal, its thickness is usually 20 μm or less, preferably 10 μm or less, more preferably 0.5 μm or more and 5 μm or less. The thickness of Layer B can be determined by the same method as that of the first retardation layer.
[0074] [Second retardation layer] The second retardation layer has the optical property represented by formula (3). nx≒ny <nz (3)
[0075] The in-plane retardation value Re(550) of the second retardation layer is usually in the range of 0 to 10 nm, preferably in the range of 0 to 5 nm. The thickness direction retardation value Rth is usually in the range of -10 to -300 nm, preferably in the range of -20 to -200 nm. The in-plane retardation value Re(550) and the thickness direction retardation value Rth can be adjusted by the same method as that of the above retardation layer.
[0076] The second retardation layer is preferably a coating layer formed by polymerizing one or more polymerizable liquid crystals, more preferably a coating layer formed by polymerizing a polymerizable liquid crystal (B).
[0077] When the second retardation layer is a stretched film, its thickness is usually 300 μm or less, preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When the second retardation layer is a layer formed by polymerizing a polymerizable liquid crystal, its thickness is usually 10 μm or less, preferably 5 μm or less, more preferably 0.3 μm or more and 3 μm or less. The thickness of the second retardation layer can be determined by the same method as that of the first retardation layer. In addition, it is preferable that the thickness of the first retardation layer and the second retardation layer is each 5 μm or less.
[0078] [Third retardation layer] The third retardation layer has an optical characteristic represented by formula (5), and preferably has an optical characteristic represented by formula (5-1). The in-plane retardation value Re(550) can be adjusted by the same method as the in-plane retardation value of the retardation layer. 200nm <Re(550)<320nm (5) 265nm <Re(550)<285nm (5-1)
[0079] Moreover, the third retardation layer preferably has optical properties represented by the formulas (6) and (7). Such optical properties can be obtained by the same method as that for the above retardation layer. Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7)
[0080] The third retardation layer is preferably a coating layer formed by polymerizing one or more polymerizable liquid crystals, more preferably a coating layer formed by polymerizing the polymerizable liquid crystal (B) or (C).
[0081] When the third retardation layer is a stretched film, its thickness is usually 300 μm or less, preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When the third retardation layer is a layer formed by polymerizing a polymerizable liquid crystal, its thickness is usually 10 μm or less, preferably 5 μm or less, more preferably 0.5 μm or more and 5 μm or less. The thickness of the third retardation layer can be obtained by the same method as that of the first retardation layer.
[0082] <Base material> The optical film of the present invention preferably has a substrate, and examples of the substrate include the same as those mentioned above.
[0083] The surface of the substrate on the side where the alignment film, the first retardation layer, the second retardation layer, and the third retardation layer are formed may be subjected to a surface treatment before forming the alignment film or the retardation layer. Examples of the surface treatment method include a method of treating the surface of the substrate with corona or plasma under vacuum or atmospheric pressure, a method of laser-treating the substrate surface, a method of ozone-treating the substrate surface, a method of saponifying the substrate surface or a method of flame-treating the substrate surface, a primer treatment method in which a coupling agent is applied to the substrate surface, and a graft polymerization method in which a reactive monomer or a polymer having a reactivity is attached to the substrate surface and then reacted by irradiating radiation, plasma, or ultraviolet light. Among these, a method of corona- or plasma-treating the substrate surface under vacuum or atmospheric pressure is preferred.
[0084] Methods for treating the surface of a substrate with corona or plasma include: A method for performing surface treatment of a substrate by placing a substrate between opposing electrodes under a pressure close to atmospheric pressure and generating corona or plasma; A method of flowing a gas between opposing electrodes, converting the gas into plasma between the electrodes, and spraying the plasma gas onto a substrate; and One example of such a method is to generate glow discharge plasma under low pressure conditions and perform surface treatment on a substrate.
[0085] Among these, a method of placing a substrate between opposing electrodes under a pressure close to atmospheric pressure, generating a corona or plasma to perform surface treatment of the substrate, or a method of flowing a gas between opposing electrodes, converting the gas into plasma between the electrodes, and spraying the plasma gas onto the substrate is preferred. Such surface treatment using corona or plasma is usually performed using a commercially available surface treatment device.
[0086] The substrate is preferably a substrate having a small retardation. Examples of substrates having a small retardation include cellulose ester films having no retardation, such as Zerotack (registered trademark) (Konica Minolta Opto Co., Ltd.) and Z-tack (Fujifilm Corporation). Unstretched cyclic olefin resin substrates are also preferred.
[0087] In addition, the surface of the substrate on which the alignment film, the first retardation layer, the second retardation layer, and the third retardation layer are not formed may be subjected to a hard coat treatment, an antistatic treatment, etc. In addition, the substrate may contain an additive such as an ultraviolet absorbing agent within a range that does not affect the performance.
[0088] If the substrate is too thin, the strength decreases and the processability tends to be poor, so the thickness is usually 5 to 300 μm, and preferably 10 to 200 μm.
[0089] <Polymerizable liquid crystal composition> A layer (retardation layer) formed by polymerizing a polymerizable liquid crystal is usually formed by applying a composition containing one or more polymerizable liquid crystals (hereinafter, sometimes referred to as a polymerizable liquid crystal composition) onto a substrate, an alignment film, a protective layer, or a retardation layer, and polymerizing the polymerizable liquid crystal in the resulting coating film.
[0090] The polymerizable liquid crystal composition usually contains a solvent, and the solvent is preferably a solvent capable of dissolving the polymerizable liquid crystal and is inactive in the polymerization reaction of the polymerizable liquid crystal. Specific examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, and phenol; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, methyl amyl ketone, methyl isobutyl ketone, and N-methyl-2-pyrrolidinone; non-chlorinated aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; non-chlorinated aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as propylene glycol monomethyl ether, tetrahydrofuran, and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene. These other solvents may be used alone or in combination.
[0091] The content of the solvent in the polymerizable liquid crystal composition is usually preferably 10 parts by mass to 10,000 parts by mass, more preferably 50 parts by mass to 5,000 parts by mass, relative to 100 parts by mass of the solid content. The solid content means the total of the components excluding the solvent from the polymerizable liquid crystal composition.
[0092] The polymerizable liquid crystal composition is usually applied by a known method such as a coating method such as a spin coating method, an extrusion method, a gravure coating method, a die coating method, a slit coating method, a bar coating method, or an applicator method, or a printing method such as a flexography method. After application, the solvent is usually removed under conditions in which the polymerizable liquid crystal contained in the obtained coating film does not polymerize, thereby forming a dried film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0093] <Alignment film> The alignment film in the present invention has an alignment regulating force for aligning the polymerizable liquid crystal in a desired direction. The alignment film is preferably one that has solvent resistance that does not dissolve the polymerizable liquid crystal composition when applied, and also has heat resistance in a heat treatment for removing the solvent and orienting the polymerizable liquid crystal. Examples of such an alignment film include an alignment film containing an alignment polymer, a photoalignment film, and a groove alignment film that forms a concave-convex pattern or a plurality of grooves on the surface to achieve alignment.
[0094] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. Two or more oriented polymers may be used in combination.
[0095] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an alignment polymer composition) to a substrate and then removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing the substrate (rubbing method).
[0096] Examples of the solvent include water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, and other alcohol solvents, ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, ethyl lactate, and other ester solvents, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, methyl isobutyl ketone, and other ketone solvents, pentane, hexane, heptane, and other aliphatic hydrocarbon solvents, toluene, xylene, and other aromatic hydrocarbon solvents, acetonitrile, and other nitrile solvents, tetrahydrofuran, dimethoxyethane, and other ether solvents, and chloroform, chlorobenzene, and other chlorinated hydrocarbon solvents. These solvents may be used alone or in combination of two or more.
[0097] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.
[0098] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0099] Examples of a method for applying the oriented polymer composition to a substrate include known methods such as spin coating, extrusion, gravure coating, die coating, slit coating, bar coating, and applicator coating, and printing methods such as flexography. When the present optical film is produced by a roll-to-roll continuous production method described below, the coating method usually employs a printing method such as gravure coating, die coating, or flexography.
[0100] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0101] In order to impart an alignment control force to the alignment film, rubbing can be carried out as necessary (rubbing method).
[0102] An example of a method for imparting an orientation control force by a rubbing method is to bring an oriented polymer film formed on the surface of a substrate by applying an oriented polymer composition to the substrate and annealing the composition into contact with a rotating rubbing roll wrapped with a rubbing cloth.
[0103] In order to impart an alignment control force to the alignment film, photo-alignment can be performed as necessary (photo-alignment method).
[0104] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter, sometimes referred to as a "photo-alignment film-forming composition") to a substrate and irradiating the substrate with light (preferably polarized UV). Photo-alignment films are more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated light.
[0105] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that are the origin of liquid crystal alignment ability, such as molecular alignment induction caused by light irradiation or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond) and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0106] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0107] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.
[0108] A photo-alignment-inducing layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the solvent contained in the above-mentioned alignment polymer composition, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.
[0109] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the intended photo-alignment film, but is preferably at least 0.2% by mass, and more preferably in the range of 0.3 to 10% by mass. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.
[0110] The method for applying the composition for forming a photo-alignment film to a substrate may be the same as the method for applying the alignable polymer composition to a substrate. The method for removing the solvent from the applied composition for forming a photo-alignment film may be the same as the method for removing the solvent from the alignable polymer composition.
[0111] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer to irradiate the polarized UV light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.
[0112] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0113] A groove alignment film is a film that aligns liquid crystals by using a concave-convex pattern or multiple grooves on the film surface. HV Kennell et al. reported that when liquid crystal molecules are placed on a substrate with multiple equally spaced linear grooves, the liquid crystal molecules are oriented along the grooves (Physical Review A24(5), p. 2713, 1981).
[0114] Specific examples of obtaining a groove alignment film include a method in which a photosensitive polyimide surface is exposed through an exposure mask having slits in a periodic pattern, followed by development and rinsing to remove unnecessary polyimide film and form a concave-convex pattern; a method in which a UV-cured resin layer is formed on a plate-shaped master having grooves on its surface, the resin layer is transferred to a base film and then cured; and a method in which a base film on which a UV-cured resin layer has been formed is transported, and a roll-shaped master having a plurality of grooves is pressed against the surface of the UV-cured resin layer to form concave-convex patterns and then cured. Methods described in JP-A-6-34976 and JP-A-2011-242743 can be used.
[0115] Among the above methods, a method in which a roll-shaped master having a plurality of grooves is pressed against the surface of a UV-cured resin layer to form projections and recesses and then cured is preferred. Stainless steel (SUS) can be used as the roll-shaped master from the viewpoint of durability.
[0116] As the UV curable resin, a polymer of a monofunctional acrylate, a polymer of a polyfunctional acrylate, or a polymer of a mixture thereof can be used. A monofunctional acrylate is a compound having one group (hereinafter sometimes referred to as a (meth)acryloyloxy group) selected from the group consisting of an acryloyloxy group (CH2=CH-COO-) and a methacryloyloxy group (CH2=C(CH3)-COO-) in the molecule.
[0117] Examples of monofunctional acrylates having one (meth)acryloyloxy group include alkyl (meth)acrylates having 4 to 16 carbon atoms, β-carboxyalkyl (meth)acrylates having 2 to 14 carbon atoms, alkylated phenyl (meth)acrylates having 2 to 14 carbon atoms, methoxypolyethylene glycol (meth)acrylates, phenoxypolyethylene glycol (meth)acrylates, and isobornyl (meth)acrylates.
[0118] The polyfunctional acrylate is usually a compound having 2 to 6 (meth)acryloyloxy groups in the molecule.
[0119] Examples of bifunctional acrylates having two (meth)acryloyloxy groups include 1,3-butanediol di(meth)acrylate; 1,3-butanediol (meth)acrylate; 1,6-hexanediol di(meth)acrylate; ethylene glycol di(meth)acrylate; diethylene glycol di(meth)acrylate; neopentyl glycol di(meth)acrylate; triethylene glycol di(meth)acrylate; tetraethylene glycol di(meth)acrylate; polyethylene glycol diacrylate; bis(acryloyloxyethyl)ether of bisphenol A; ethoxylated bisphenol A di(meth)acrylate; propoxylated neopentyl glycol di(meth)acrylate; ethoxylated neopentyl glycol di(meth)acrylate, and 3-methylpentanediol di(meth)acrylate.
[0120] Examples of polyfunctional acrylates having 3 to 6 (meth)acryloyloxy groups include: Trimethylolpropane tri(meth)acrylate;Pentaerythritol tri(meth)acrylate;Tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate;Ethoxylated trimethylolpropane tri(meth)acrylate;Propoxylated trimethylolpropane tri(meth)acrylate;Pentaerythritol tetra(meth)acrylate;Dipentaerythritol penta(meth)acrylate;Dipentaerythritol hexa(meth)acrylate;Tripentaerythritol tetra(meth)acrylate;Tripentaerythritol penta(meth)acrylate;Tripentaerythritol hexa(meth)acrylate;Tripentaerythritol hepta(meth)acrylate;Tripentaerythritol octa(meth)acrylate; Reaction products of pentaerythritol tri(meth)acrylate with acid anhydride;Reaction products of dipentaerythritol penta(meth)acrylate with acid anhydride; Reaction products of tripentaerythritol hepta(meth)acrylate with acid anhydride; Caprolactone modified trimethylolpropane tri(meth)acrylate;Caprolactone modified pentaerythritol tri(meth)acrylate;Caprolactone modified tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate;Caprolactone modified pentaerythritol tetra(meth)acrylate;Caprolactone modified dipentaerythritol penta(meth)acrylate;Caprolactone modified dipentaerythritol hexa(meth)acrylate;Caprolactone modified tripentaerythritol tetra(meth)acrylate;Caprolactone modified tripentaerythritol tetra(meth)acrylate Examples of the acrylate include erythritol penta(meth)acrylate, caprolactone-modified tripentaerythritol hexa(meth)acrylate, caprolactone-modified tripentaerythritol hepta(meth)acrylate, caprolactone-modified tripentaerythritol octa(meth)acrylate, a reaction product of caprolactone-modified pentaerythritol tri(meth)acrylate and an acid anhydride, a reaction product of caprolactone-modified dipentaerythritol penta(meth)acrylate and an acid anhydride, and a reaction product of caprolactone-modified tripentaerythritol hepta(meth)acrylate and an acid anhydride. In the specific examples of the multifunctional acrylate shown here, (meth)acrylate means acrylate or methacrylate. In addition, caprolactone-modified means that a ring-opened product or a ring-opened polymer of caprolactone is introduced between the alcohol-derived site and the (meth)acryloyloxy group of the (meth)acrylate compound.
[0121] Such polyfunctional acrylates may also be commercially available products. Such commercially available products include A-DOD-N, A-HD-N, A-NOD-N, APG-100, APG-200, APG-400, A-GLY-9E, A-GLY-20E, A-TMM-3, A-TMPT, AD-TMP, ATM-35E, A-TMMT, A-9550, A-DPH, HD-N, NOD-N, NPG, TMPT (manufactured by Shin-Nakamura Chemical Co., Ltd.), "ARONIX M-220", "M-325", "M-240", "M-270", "M-309", "M-310", "M-321", "M-350", "M-360", "M-305", "M-306", and "M-450". , "M-451", "M-408", "M-400", "M-402", "M-403", "M-404", "M-405", "M-406" (manufactured by Toa Gosei Co., Ltd.), "EBECRYL11", "145", "150", "40", "140", "180", DPGDA, HDDA, TPGDA, HPNDA, PETIA, PETRA, TMPTA, TMPEOTA, DPHA, EBECRYL series (manufactured by Daicel-Cytec Co., Ltd.), and the like.
[0122] As for the unevenness of the groove alignment film, the width of the protrusions is preferably 0.05 to 5 μm, the width of the recesses is preferably 0.1 to 5 μm, and the depth of the unevenness is preferably 2 μm or less, more preferably 0.01 to 1 μm. Within these ranges, liquid crystal alignment with little alignment disorder can be obtained.
[0123] The thickness of the alignment film is usually in the range of 10 nm to 10,000 nm, preferably in the range of 10 nm to 1,000 nm, more preferably 500 nm or less, and further preferably in the range of 10 nm to 500 nm.
[0124] The liquid crystal alignment of the polymerizable liquid crystal is controlled by the properties of the alignment film and the polymerizable liquid crystal. For example, if the alignment film is made of a material that exhibits a horizontal alignment regulation force as an alignment regulation force, the polymerizable liquid crystal can form a horizontal alignment or a hybrid alignment, and if the alignment film is made of a material that exhibits a vertical alignment regulation force, the polymerizable liquid crystal can form a vertical alignment or an inclined alignment. When the alignment film is made of an alignment polymer, the alignment regulating force can be adjusted as desired by the surface state or rubbing conditions, and when the alignment film is made of a photoalignment polymer, the alignment regulating force can be adjusted as desired by the polarized light irradiation conditions, etc. In addition, the liquid crystal alignment can be controlled by selecting the physical properties of the polymerizable liquid crystal, such as the surface tension or liquid crystallinity.
[0125] Polymerization of the polymerizable liquid crystal can be carried out by a known method of polymerizing a compound having a polymerizable functional group.Specifically, it can be thermal polymerization or photopolymerization, and photopolymerization is preferred from the viewpoint of ease of polymerization.When polymerizing the polymerizable liquid crystal by photopolymerization, it is preferable to coat a polymerizable liquid crystal composition containing a photopolymerization initiator, dry the polymerizable liquid crystal in the dried coating obtained by drying, and then photopolymerize the polymerizable liquid crystal while maintaining the liquid crystal state.
[0126] Photopolymerization is usually performed by irradiating the dry film with light. The light to be irradiated is appropriately selected according to the type of photopolymerization initiator contained in the dry film, the type of polymerizable liquid crystal (particularly, the type of photopolymerizable group possessed by the polymerizable liquid crystal) and the amount thereof, and specifically includes light selected from the group consisting of visible light, ultraviolet light and laser light, and active electron beams. Among them, ultraviolet light is preferred because it is easy to control the progress of the polymerization reaction and because photopolymerization devices widely used in this field can be used. It is preferable to select the type of polymerizable liquid crystal and photopolymerization initiator so that photopolymerization can be performed by ultraviolet light. In addition, the polymerization temperature can be controlled by irradiating light while cooling the dry film with an appropriate cooling means during polymerization. By adopting such a cooling means, if polymerization of the polymerizable liquid crystal is performed at a lower temperature, even if a substrate with relatively low heat resistance is used, a retardation layer can be appropriately formed. During photopolymerization, a patterned retardation layer can also be obtained by performing masking or development.
[0127] The polymerizable liquid crystal composition may contain a reactive additive. The reactive additive preferably has a carbon-carbon unsaturated bond and an active hydrogen reactive group in its molecule. The "active hydrogen reactive group" here means a group that is reactive to a group having active hydrogen such as a carboxyl group (-COOH), a hydroxyl group (-OH), or an amino group (-NH2), and representative examples thereof include a glycidyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, an isocyanate group, a thioisocyanate group, and a maleic anhydride group. The number of carbon-carbon unsaturated bonds and active hydrogen reactive groups that the reactive additive has is usually 1 to 20, and preferably 1 to 10.
[0128] In the reactive additive, it is preferable that at least two active hydrogen reactive groups are present, and in this case, the multiple active hydrogen reactive groups present may be the same or different.
[0129] The carbon-carbon unsaturated bond of the reactive additive may be a carbon-carbon double bond or a carbon-carbon triple bond, or a combination thereof, but is preferably a carbon-carbon double bond. Among them, the reactive additive preferably contains a carbon-carbon unsaturated bond as a vinyl group and / or a (meth)acrylic group. Furthermore, the active hydrogen reactive group is preferably at least one selected from the group consisting of an epoxy group, a glycidyl group, and an isocyanate group, and a reactive additive having an acrylic group and an isocyanate group is particularly preferred.
[0130] Specific examples of reactive additives include compounds having a (meth)acrylic group and an epoxy group, such as methacryloxyglycidyl ether and acryloxyglycidyl ether; compounds having a (meth)acrylic group and an oxetane group, such as oxetane acrylate and oxetane methacrylate; compounds having a (meth)acrylic group and a lactone group, such as lactone acrylate and lactone methacrylate; compounds having a vinyl group and an oxazoline group, such as vinyl oxazoline and isopropenyl oxazoline; oligomers of compounds having a (meth)acrylic group and an isocyanate group, such as isocyanatomethyl acrylate, isocyanatomethyl methacrylate, 2-isocyanatoethyl acrylate, and 20-isocyanatoethyl methacrylate. In addition, compounds having a vinyl group or a vinylene group and an acid anhydride, such as methacrylic anhydride, acrylic anhydride, maleic anhydride, and vinyl maleic anhydride, can be mentioned. Among these, methacryloxyglycidyl ether, acryloxyglycidyl ether, isocyanatomethyl acrylate, isocyanatomethyl methacrylate, vinyloxazoline, 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate, and oligomers thereof are preferred, and isocyanatomethyl acrylate, 2-isocyanatoethyl acrylate, and oligomers thereof are particularly preferred.
[0131] Specifically, a compound represented by the following formula (Y) is preferred. TIFF0007573000000015.tif1695[In formula (Y), n is an integer from 1 to 10, R 1’ represents a divalent aliphatic or alicyclic hydrocarbon group having 2 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 5 to 20 carbon atoms. 2’ is -NH- on one side and >NC(=O)-R on the other side. 3’ R 3’ represents a hydroxyl group or a group having a carbon-carbon unsaturated bond. R in formula (Y) 3’ At least one R 3’is a group having a carbon-carbon unsaturated bond.
[0132] Among the reactive additives represented by the formula (Y), a compound represented by the following formula (YY) (hereinafter, sometimes referred to as compound (YY)) is particularly preferred (n has the same meaning as above). TIFF0007573000000016.tif42127 Compound (YY) may be a commercially available product, either as is or after purification as necessary. Examples of commercially available products include Laromer (registered trademark) LR-9000 (manufactured by BASF).
[0133] When the polymerizable liquid crystal composition contains a reactive additive, the content thereof is usually 0.1 to 30 parts by mass, and preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal.
[0134] The polymerizable liquid crystal composition preferably contains one or more leveling agents. The leveling agent has a function of adjusting the fluidity of the polymerizable liquid crystal composition and making the coating film obtained by coating the polymerizable liquid crystal composition flatter, and specifically includes a surfactant. The leveling agent is preferably at least one selected from the group consisting of leveling agents mainly composed of a polyacrylate compound and leveling agents mainly composed of a fluorine atom-containing compound.
[0135] Leveling agents based on polyacrylate compounds include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" [BYK Chemie].
[0136] Leveling agents containing fluorine-containing compounds as the main component include "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" [DIC Corporation]; "Surflon (registered trademark) S-381" and "S-3 Examples of such products include "82", "S-383", "S-393", "SC-101", "SC-105", "KH-40" and "SA-100" [AGC Seimi Chemical Co., Ltd.]; "E1830", "E5844" [Daikin Fine Chemical Research Institute Ltd.]; "F-TOP EF301", "F-TOP EF303", "F-TOP EF351" and "F-TOP EF352" [Mitsubishi Materials Electronic Chemicals Co., Ltd.].
[0137] When the polymerizable liquid crystal composition contains a leveling agent, the content is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal. When the content of the leveling agent is within the above range, the polymerizable liquid crystal is easily aligned horizontally, and the obtained polarizing layer tends to be smoother. When the content of the leveling agent relative to the polymerizable liquid crystal is within the above range, the obtained retardation layer tends to be less prone to unevenness.
[0138] The polymerizable liquid crystal composition preferably contains one or more polymerization initiators. The polymerization initiator is a compound capable of initiating the polymerization reaction of the polymerizable liquid crystal, and a photopolymerization initiator is preferred because it can initiate the polymerization reaction under lower temperature conditions. Specifically, a photopolymerization initiator capable of generating active radicals or acids by the action of light is included, and among them, a photopolymerization initiator that generates radicals by the action of light is preferred.
[0139] The polymerization initiator includes a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, and a sulfonium salt.
[0140] Benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether and benzoin isobutyl ether.
[0141] Benzophenone compounds include benzophenone, o-benzoylmethylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0142] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0143] The acylphosphine oxide compounds include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0144] Examples of triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.
[0145] The polymerization initiator may be commercially available. Commercially available polymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", "Irgacure (registered trademark) 369" (Ciba Japan Co., Ltd.); "Seikuol (registered trademark) BZ", "Seikuol (registered trademark) Z", "Seikuol (registered trademark) 100", "Seikuol (registered trademark) 200", "Seikuol (registered trademark) 1 ... Examples of such compounds include "Kayacure (registered trademark) BEE" (Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.); "Kayacure (registered trademark) UVI-6992" (Dow Chemicals); "ADEKA Optomer SP-152", "ADEKA Optomer SP-170" (ADEKA Corporation); "TAZ-A", "TAZ-PP" (Nippon SiberHegner Co., Ltd.); and "TAZ-104" (Sanwa Chemical Co., Ltd.).
[0146] When the polymerizable liquid crystal composition contains a polymerization initiator, the content can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal contained in the composition, but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal. If the content of the polymerization initiator is within this range, the polymerizable liquid crystal can be polymerized without disturbing the alignment.
[0147] When the polymerizable liquid crystal composition contains a photopolymerization initiator, the composition may further contain a photosensitizer.The photosensitizer includes xanthone, thioxanthone, and other xanthone compounds (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, and other); anthracene, anthracene containing an alkoxy group (e.g., dibutoxyanthracene, and other anthracene compounds); phenothiazine and rubrene.
[0148] When the polymerizable liquid crystal composition contains a photopolymerization initiator and a photosensitizer, the polymerization reaction of the polymerizable liquid crystal contained in the composition can be further promoted. The amount of the photosensitizer used can be appropriately adjusted depending on the type and amount of the photopolymerization initiator and the polymerizable liquid crystal, but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal.
[0149] In order to allow the polymerization reaction of the polymerizable liquid crystal to proceed more stably, the polymerizable liquid crystal composition may contain an appropriate amount of a polymerization inhibitor, which makes it easier to control the degree of progress of the polymerization reaction of the polymerizable liquid crystal.
[0150] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (for example, butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.
[0151] When the polymerizable liquid crystal composition contains a polymerization inhibitor, the content can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal, the amount of the photosensitizer used, etc., but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal. If the content of the polymerization inhibitor is within this range, the polymerizable liquid crystal can be polymerized without disturbing the alignment.
[0152] When producing the present optical film, the first retardation layer, the second retardation layer, and the third retardation layer may be formed in any order. Also, the order of forming the layer A and the layer B in the first retardation layer may be arbitrary.
[0153] A layer A may be formed on a substrate with or without an alignment film, a layer B may be formed on the layer A with or without an alignment film, and a second retardation layer may be formed on the layer B with or without an alignment film. A layer B may be formed on a substrate with or without an alignment film, a layer A may be formed on the layer B with or without an alignment film, and a second retardation layer may be formed on the layer A with or without an alignment film. A second retardation layer may be formed on the substrate with or without an alignment film, layer A may be formed on the second retardation layer with or without an alignment film, and layer B may be formed on layer A with or without an alignment film. A second retardation layer may be formed on the substrate with or without an alignment film, layer B may be formed on the second retardation layer with or without an alignment film, and layer A may be formed on layer B with or without an alignment film. A layer A may be formed on one surface of the substrate with or without an alignment film, a layer B may be formed on the layer A with or without an alignment film, and a second retardation layer may be formed on the other surface of the substrate with or without an alignment film. A layer B may be formed on one surface of the substrate with or without an alignment film, a layer A may be formed on the layer B with or without an alignment film, and a second retardation layer may be formed on the other surface of the substrate with or without an alignment film.
[0154] When layer B is formed on layer A with or without an alignment film, or when layer A is formed on layer B with or without an alignment film, a protective layer may be provided between layer A and layer B. When layer A is formed on the second retardation layer with or without an alignment film, when layer A is formed on the second retardation layer with or without an alignment film, when the second retardation layer is formed on layer A with or without an alignment film, or when the second retardation layer is formed on layer B with or without an alignment film, a protective layer may be provided between the second retardation layer and layer A or layer B.
[0155] A first retardation layer may be formed on a substrate with or without an alignment film, a second retardation layer may be formed on the first retardation layer with or without an alignment film, and a third retardation layer may be formed on the second retardation layer with or without an alignment film. A third retardation layer may be formed on a substrate with or without an alignment film, a second retardation layer may be formed on the third retardation layer with or without an alignment film, and a first retardation layer may be formed on the second retardation layer with or without an alignment film. A first retardation layer may be formed on one surface of the substrate with or without an alignment film, a second retardation layer may be formed on the first retardation layer with or without an alignment film, and a third retardation layer may be formed on the other surface of the substrate with or without an alignment film. A second retardation layer may be formed on one surface of the substrate with or without an alignment film, a first retardation layer may be formed on the second retardation layer with or without an alignment film, and a third retardation layer may be formed on the other surface of the substrate with or without an alignment film. A third retardation layer may be formed on one surface of the substrate with or without an alignment film, a second retardation layer may be formed on the third retardation layer with or without an alignment film, and a first retardation layer may be formed on the other surface of the substrate with or without an alignment film. A second retardation layer may be formed on one surface of the substrate with or without an alignment film, a third retardation layer may be formed on the second retardation layer with or without an alignment film, and a first retardation layer may be formed on the other surface of the substrate with or without an alignment film.
[0156] A first retardation layer may be formed on a substrate with or without an alignment film, and a second retardation layer may be formed on the first retardation layer with or without an alignment film. A second retardation layer may be formed on one surface of the substrate with or without an alignment film, and a first retardation layer may be formed on the second retardation layer with or without an alignment film. The second retardation layer may be formed on one surface of the substrate with or without an alignment film, and the first retardation layer may be formed on the other surface of the substrate with or without an alignment film.
[0157] When the second retardation layer is formed on the first retardation layer with or without an alignment film, or when the first retardation layer is formed on the second retardation layer with or without an alignment film, a protective layer may be present between the first retardation layer and the second retardation layer. When the third retardation layer is formed on the second retardation layer with or without an alignment film, or when the second retardation layer is formed on the third retardation layer with or without an alignment film, a protective layer may be present between the second retardation layer and the third retardation layer.
[0158] <Protective layer> The protective layer is preferably formed from a protective layer-forming composition that contains a water-soluble polymer, such as an acrylic oligomer or polymer consisting of a multifunctional acrylate (methacrylate), urethane acrylate, polyester acrylate, epoxy acrylate, etc., polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylpyrrolidone, starches, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc., and a solvent.
[0159] The solvent contained in the composition for forming a protective layer may be the same as the solvent described above, and among them, at least one solvent selected from the group consisting of water, alcohol solvents, and ether solvents is preferred because it does not dissolve the layer forming the protective layer. Examples of the alcohol solvent include methanol, ethanol, butanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether. Examples of the ether solvent include ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate. Among them, ethanol, isopropyl alcohol, propylene glycol monomethyl ether, and propylene glycol monomethyl ether acetate are preferred.
[0160] The thickness of the protective layer is usually 20 μm or less. The thickness of the protective layer is preferably 0.5 μm or more and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. The thickness of the protective layer can usually be measured by an interference thickness meter, a laser microscope, or a stylus thickness meter.
[0161] Next, a method for continuously manufacturing the present optical film will be described. A suitable method for continuously manufacturing the present optical film will be a roll to roll method. Here, a method for manufacturing a retardation layer formed by polymerizing a polymerizable liquid crystal will be described. However, instead of the retardation layer formed by polymerizing a polymerizable liquid crystal, a retardation layer made of a stretched film may be used. In this case, "applying a polymerizable liquid crystal composition" in the following manufacturing steps may be read as "laminating a stretched film". In addition, a manufacturing method for a representative configuration will be exemplified below, but other configurations may be carried out in accordance with the manufacturing method below.
[0162] (1) preparing a roll having a substrate wound around a core; (2) continuously delivering the substrate from the roll; (3) continuously forming an alignment film on the substrate; (4) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first retardation layer; (5) A step of continuously forming a protective layer on the first retardation layer obtained in (4); (6) A step of continuously forming an alignment film on the protective layer obtained in (5); (7) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6) to continuously form a second retardation layer; (8) A step of winding the continuously obtained optical film onto a second core to obtain a second roll. A method in which the above steps are performed in order is exemplified. Note that steps (3), (5) and (6) may be omitted as necessary. In this case, "on the alignment film" in step (4) is replaced with "on the substrate", "the protective layer obtained in step (5)" in step (6) is replaced with "the first retardation layer", and "the alignment film obtained in step (6)" in step (7) is replaced with "the first retardation layer" or "the protective layer obtained in step (5)". In order to prevent wrinkles and curls during transport, a protective film may be attached to the film during transport in each step.
[0163] Also, (1a) preparing a roll having a substrate wound around a core; (2a) continuously delivering the substrate from the roll; (3a) continuously forming an alignment film on the substrate; (4a) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a second retardation layer; (5a) a step of continuously forming a protective layer on the second retardation layer obtained in (4a); (6a) a step of continuously forming an alignment film on the protective layer obtained in (5a); (7a) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6a) to continuously form a first retardation layer; (8a) A method of sequentially winding the continuously obtained optical film on a second core to obtain a second roll may also be mentioned. Note that steps (3a), (5a) and (6a) may be omitted as necessary. In this case, "on the alignment film" in step (4a) is read as "on the substrate", "the protective layer obtained in (5a)" in step (6a) is read as "the second retardation layer", and "the alignment film obtained in (6a)" in step (7a) is read as "the second retardation layer" or "the protective layer obtained in (5a)". In addition, in order to prevent wrinkles and curls during transport, a protective film may be attached to the film during transport in each step.
[0164] Also, (1b) preparing a roll having a substrate wound around a core; (2b) continuously delivering the substrate from the roll; (3b) continuously forming an alignment film on the substrate; (4b) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first retardation layer; (5b) a step of continuously forming an alignment layer on the substrate surface opposite to the first retardation layer obtained in (4b); (6b) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (5b) to continuously form a second retardation layer; (7b) A method of sequentially winding the continuously obtained optical film on a second core to obtain a second roll may also be mentioned. Note that steps (3b) and (5b) may be omitted as necessary, and in this case, "on the alignment film" in step (4b) should be read as "on the substrate", and "on the alignment film obtained in (5b)" in step (6b) should be read as "the substrate surface opposite to the first retardation layer obtained in (4b)". In addition, in order to prevent wrinkles and curls during transport, a protective film may be attached to the film during transport in each step.
[0165] Also, (1c) preparing a roll having a transparent substrate wound around a core; (2c) continuously delivering the transparent substrate from the roll; (3c) continuously forming an alignment film on the transparent substrate; (4c) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a second retardation layer; (5c) a step of continuously forming an alignment layer on the substrate surface opposite to the second retardation layer obtained in (4c); (6c) applying a polymerizable liquid crystal composition onto the alignment film obtained in (5c) to continuously form a first retardation layer; (7c) A method of sequentially winding the continuously obtained optical film on a second core to obtain a second roll can also be mentioned. Note that steps (3c) and (5c) may be omitted as necessary, and in this case, "on the alignment film" in step (4c) should be read as "on the substrate", and "on the alignment film obtained in (5c)" in step (6c) should be read as "the substrate surface opposite to the second retardation layer obtained in (4c)". In addition, in order to prevent wrinkles and curls during transport, a protective film may be attached to the film during transport in each step.
[0166] Also, (1d) preparing a roll having a substrate wound around a core; (2d) continuously delivering the substrate from the roll; (3d) continuously forming an alignment film on the substrate; (4d) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a layer A; (5d) continuously forming a protective layer on the layer A obtained in (4d); (6d) a step of continuously forming an alignment film on the protective layer obtained in (5d); (7d) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6d) to continuously form a layer B; (8d) a step of continuously forming a protective layer on the layer B obtained in (7d); (9d) a step of continuously forming an alignment film on the protective layer obtained in (8d); (10d) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (9d) to continuously form a second retardation layer; (11d) A method in which the optical film obtained continuously is wound around a second core to obtain a second roll is sequentially performed. Note that steps (3d), (5d), (6d), (8d), and (9d) may be omitted as necessary. In this case, "on the alignment film" in step (4d) is replaced with "on the substrate", "the protective layer obtained in (5d)" in step (6d) is replaced with "the layer A", "the alignment film obtained in (6d)" in step (7d) is replaced with "the layer A" or "the protective layer obtained in (5d)", "the protective layer obtained in (8d)" in step (9d) is replaced with "the layer B", and "the alignment film obtained in (9d)" in step (10d) is replaced with "the layer B" or "the protective layer obtained in (9d)". In order to prevent wrinkles and curls during transportation, a protective film may be attached when the film is transported in each step.
[0167] Also, (1e) preparing a roll having a substrate wound on a core; (2e) continuously delivering the substrate from the roll; (3e) continuously forming an alignment film on the substrate; (4e) applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first retardation layer; (5e) a step of continuously forming a protective layer on the first retardation layer obtained in (4e); (6e) a step of continuously forming an alignment film on the protective layer obtained in (5e); (7e) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6e) to continuously form a second retardation layer; (8e) a step of continuously forming an alignment layer on the substrate surface opposite to the first retardation layer obtained in (4e); (9e) a step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (8e) to continuously form a third retardation layer; (10e) A method in which the optical film obtained continuously is wound around a second core to obtain a second roll is also included. Steps (3e), (5e) and (8e) may be omitted if necessary. In this case, In step (4e), "on the alignment film" means "on the substrate"; In step (6e), the "protective layer obtained in (5e)" is applied to the "first retardation layer obtained in (4e)". In step (9e), "on the alignment film obtained in (8e)" is to be read as "on the substrate surface opposite to the first retardation layer obtained in (4e)". In addition, in order to prevent wrinkles and curls during transportation, a protective film may be attached to the film when it is transported in each step. In addition, in order to prevent wrinkles and curls during transportation, a protective film may be attached to the film when it is transported in each step.
[0168] A schematic diagram of the present optical film is shown in Fig. 1. Fig. 1(b) shows the present optical film 100 in which a substrate, a first retardation layer, and a second retardation layer are laminated in this order. Fig. 1(c) shows the present optical film 100 in which a substrate, a second retardation layer, and a first retardation layer are laminated in this order. Fig. 1(d) shows the present optical film 100 in which a first retardation layer, a substrate, and a second retardation layer are laminated in this order.
[0169] By removing the substrate from these optical films, the present optical film without the substrate can be obtained. When the first retardation layer is a stretched film, the present optical film can be produced by forming a second retardation layer, which is a coating layer, on the surface of the stretched film. When the second retardation layer is a stretched film, the present optical film can be produced by forming a first retardation layer, which is a coating layer, on the surface of the stretched film. A schematic diagram of the present optical film without the substrate is shown in FIG. 1(a).
[0170] The present optical film can also be produced by laminating a substrate having a first retardation layer and a substrate having a second retardation layer. Specific examples are shown in Fig. 1(e), Fig. 1(f) and Fig. 1(g). An adhesive described later can be used for lamination.
[0171] FIG. 2 shows the configuration of the optical film when the first retardation layer is composed of layer A and layer B, or when the optical film has a third retardation layer. FIG. 2(c) is an optical film 100 in which a substrate, layer A, layer B, and a second retardation layer are laminated in this order. FIG. 2(d) is an optical film 100 in which a substrate, a first retardation layer, a second retardation layer, and a third retardation layer are laminated in this order. FIG. 2(e) is an optical film 100 in which a substrate, layer B, layer A, and a second retardation layer are laminated in this order. FIG. 2(f) is an optical film 100 in which a substrate, a third retardation layer, a second retardation layer, and a first retardation layer are laminated in this order. FIG. 2(g) is an optical film 100 in which a substrate, a second retardation layer, layer B, and layer A are laminated in this order. FIG. 2(h) is an optical film 100 in which a substrate, a second retardation layer, layer A, and layer B are laminated in this order. By peeling off the substrate from these optical films, the optical films having no substrate can be obtained. Schematic diagrams of the optical films having no substrate are shown in FIG. 2(a) and FIG. 2(b).
[0172] In the case of a configuration including a first retardation layer, layer A, and layer B, or in the case of a third retardation layer, each layer may be laminated on both sides of the substrate. As a specific example, for example, FIG. 2(i) is an optical film 100 in which a second retardation layer, a substrate, a layer A, and a layer B are laminated in this order. FIG. 2(j) is an optical film 100 in which a second retardation layer, a substrate, a layer B, and a layer A are laminated in this order. FIG. 2(k) is an optical film 100 in which a first retardation layer, a substrate, a third retardation layer, and a second retardation layer are laminated in this order. FIG. 2(l) is an optical film 100 in which a first retardation layer, a substrate, a second retardation layer, and a third retardation layer are laminated in this order. FIG. 2(m) is an optical film 100 in which a third retardation layer, a substrate, a first retardation layer, and a second retardation layer are laminated in this order. 2(n) shows an optical film 100 in which a third retardation layer, a substrate, a second retardation layer, and a first retardation layer are laminated in this order. The second retardation layer, layer A, and layer B may be formed by direct coating on each layer, or each layer may be laminated by lamination after production, or each layer may be laminated by sequential transfer.
[0173] <Adhesive> Examples of adhesives include pressure sensitive adhesives, water-based adhesives, and active energy ray curable adhesives.
[0174] Generally, as a pressure-sensitive adhesive, an acrylic pressure-sensitive adhesive is preferably used which is obtained by radically polymerizing an acrylic monomer mixture containing a (meth)acrylic acid ester as a main component and a small amount of a (meth)acrylic monomer having a functional group in the presence of a polymerization initiator, and which contains an acrylic resin with a glass transition temperature Tg of 0°C or lower and a crosslinking agent.
[0175] Of the (meth)acrylic acid esters, alkyl acrylates are preferred, and among these, n-butyl acrylate, 2-methoxyethyl acrylate and ethoxymethyl acrylate are preferred.
[0176] The (meth)acrylic monomer having a functional group, which is another monomer component constituting the acrylic resin, is a compound having one (meth)acryloyl group, which is an olefinic double bond, in the molecule, and having a polar functional group such as a hydroxyl group, a carboxyl group, an amide group, an amino group, or an epoxy group in the same molecule. Among them, an acrylic monomer in which the acryloyl group is an olefinic double bond is preferred. Examples of acrylic monomers having such functional groups include 2-hydroxyethyl acrylate, which has a hydroxyl group, and acrylic acid, which has a carboxyl group.
[0177] The acrylic monomer mixture, which is the raw material of the acrylic resin, may further contain a monomer (hereinafter sometimes referred to as a "third monomer") other than the above-mentioned (meth)acrylic acid ester and (meth)acrylic monomer having a functional group. Examples of such a monomer include a monomer having one olefinic double bond and at least one aromatic ring in the molecule, a styrene-based monomer, a (meth)acrylic acid ester having an alicyclic structure in the molecule, a vinyl-based monomer, and a monomer having multiple (meth)acryloyl groups in the molecule.
[0178] In particular, a monomer having one olefinic double bond and at least one aromatic ring in the molecule is one of the preferred ones. Among them, 2-phenoxyethyl (meth)acrylate, 2-(2-phenoxyethoxy)ethyl (meth)acrylate, (meth)acrylate of ethylene oxide-modified nonylphenol, and 2-(o-phenylphenoxy)ethyl (meth)acrylate are preferred. Among these, 2-phenoxyethyl acrylate is more preferred.
[0179] The monomers (third monomers) other than the (meth)acrylic acid ester and the (meth)acrylic monomer having a functional group may be used alone or in combination of different kinds. The structural units derived from these third monomers can be present in the range of usually 0 to 20% by weight, preferably 0 to 10% by weight, based on the entire acrylic resin.
[0180] The acrylic resin constituting the acrylic adhesive preferably has a weight average molecular weight Mw of 1 to 2 million in terms of standard polystyrene measured by gel permeation chromatography (GPC). When the weight average molecular weight Mw is 1 million or more, the adhesiveness at high temperature and high humidity is improved, the possibility of lifting or peeling between the glass substrate constituting the liquid crystal cell and the adhesive layer tends to be reduced, and reworkability tends to be improved, which is preferable. In addition, when the weight average molecular weight Mw of the acrylic resin is 2 million or less, even if the dimensions of the polarizing plate change, the adhesive layer changes in accordance with the dimensional change, so that light leakage and color unevenness of the display tend to be suppressed, which is preferable. Furthermore, the molecular weight distribution represented by the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is preferably in the range of 3 to 7.
[0181] The acrylic resin contained in the acrylic pressure-sensitive adhesive may be composed of only the above-mentioned relatively high molecular weight resin, or may be composed of a mixture with a different acrylic resin. Examples of acrylic resins that can be used in a mixture include those that have a structural unit derived from a (meth)acrylic acid ester represented by the above formula (I) as the main component and have a weight average molecular weight in the range of 50,000 to 300,000.
[0182] The acrylic resin constituting the acrylic pressure sensitive adhesive can be produced by various known methods such as solution polymerization, emulsion polymerization, bulk polymerization, and suspension polymerization. A polymerization initiator is usually used in the production of this acrylic resin. Examples of the polymerization initiator include azo compounds, organic peroxides, inorganic peroxides, and redox initiators using a combination of peroxides and reducing agents. Among them, 2,2'-azobisisobutyronitrile, benzoyl peroxide, and ammonium persulfate are preferably used. The polymerization initiator is usually used in a ratio of about 0.001 to 5 parts by mass with respect to 100 parts by mass of the total amount of monomers that are raw materials for the acrylic resin.
[0183] A crosslinking agent is added to the acrylic resin thus obtained to produce a pressure-sensitive adhesive. The crosslinking agent is a compound having at least two functional groups in the molecule that can undergo a crosslinking reaction with a structural unit derived from a monomer having a polar functional group in the acrylic resin, and examples of such a crosslinking agent include isocyanate compounds, epoxy compounds, metal chelate compounds, and aziridine compounds.
[0184] Among these crosslinking agents, isocyanate compounds are preferably used. The isocyanate compounds can be used in the form of a compound having at least two isocyanato groups (-NCO) in the molecule, an adduct obtained by reacting the compound with a polyol, a dimer, a trimer, etc. Specific examples include tolylene diisocyanate, an adduct obtained by reacting tolylene diisocyanate with a polyol, a dimer of tolylene diisocyanate, a trimer of tolylene diisocyanate, hexamethylene diisocyanate, an adduct obtained by reacting hexamethylene diisocyanate with a polyol, a dimer of hexamethylene diisocyanate, a trimer of hexamethylene diisocyanate, etc.
[0185] The crosslinking agent is usually blended in a ratio of about 0.01 to 5 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.2 to 3 parts by mass, per 100 parts by mass of the acrylic resin. If the blending amount of the crosslinking agent per 100 parts by mass of the acrylic resin is 0.01 part by mass or more, and more preferably 0.1 part by mass or more, the durability of the pressure-sensitive adhesive layer tends to be improved.
[0186] Other components can be added to the adhesive as necessary. Examples of other components that can be added include conductive fine particles such as metal fine particles, metal oxide fine particles, or fine particles coated with metal, ion conductive compositions, ionic compounds having organic cations or anions, silane coupling agents, crosslinking catalysts, weather stabilizers, tackifiers, plasticizers, softeners, dyes, pigments, inorganic fillers, resins other than the above acrylic resins, and light diffusing fine particles such as organic beads. It is also useful to add an ultraviolet curable compound to the adhesive, form an adhesive layer, and then irradiate ultraviolet light to cure the adhesive layer to make it harder.
[0187] These components constituting the adhesive are usually dissolved in a suitable solvent such as ethyl acetate and used as an adhesive composition. The adhesive composition is applied to a suitable substrate and dried to obtain an adhesive layer. Some components are not soluble in the solvent, but they may be dispersed in the system.
[0188] The method of forming the adhesive layer on the optical film may be, for example, a method of using a release film as a substrate, applying the above-mentioned adhesive composition to form an adhesive layer, and transferring the resulting adhesive layer to the surface of the optical film, or a method of directly applying the above-mentioned adhesive composition to the surface of the optical film to form an adhesive layer. In addition, after forming an adhesive layer on one release film, another release film may be laminated on the adhesive layer to form a double-sided separator type adhesive sheet. When necessary, the release film on one side of such a double-sided separator type adhesive sheet is peeled off and laminated on the optical film. Commercially available double-sided separator type adhesive sheets include, for example, non-carrier adhesive films and non-carrier adhesive sheets sold by Lintec Corporation and Nitto Denko Corporation.
[0189] The release film may be a film made of various resins such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyarylate, polypropylene or polyethylene as a substrate, and the bonding surface of the substrate to be bonded to the pressure-sensitive adhesive layer may be subjected to a release treatment such as silicone treatment. Such a release film is also called a separation film or separator.
[0190] The thickness of the adhesive layer is preferably 5 to 50 μm, and more preferably 5 to 30 μm. By making the thickness of the adhesive layer 30 μm or less, the adhesiveness under high temperature and high humidity is improved, the possibility of lifting or peeling between the display and the adhesive layer tends to be reduced, and reworkability also tends to be improved. In addition, by making the thickness 5 μm or more, even if the dimensions of the polarizing plate attached thereto change, the adhesive layer changes in accordance with the dimensional change, so that the durability against dimensional change is improved.
[0191] A typical aqueous adhesive is a composition that uses, for example, a polyvinyl alcohol resin or a urethane resin as a main component and, in order to improve adhesion, contains a crosslinking agent or a curing compound such as an isocyanate compound or an epoxy compound.
[0192] When a polyvinyl alcohol resin is used as the main component of the aqueous adhesive, modified polyvinyl alcohol resins such as partially saponified polyvinyl alcohol and fully saponified polyvinyl alcohol, carboxyl group-modified polyvinyl alcohol, acetoacetyl group-modified polyvinyl alcohol, methylol group-modified polyvinyl alcohol, and amino group-modified polyvinyl alcohol may be used. An aqueous solution of such a polyvinyl alcohol resin is used as the aqueous adhesive, and the concentration of the polyvinyl alcohol resin in the aqueous adhesive is usually 1 to 10 parts by mass, preferably 1 to 5 parts by mass, based on 100 parts by mass of water.
[0193] In order to improve the adhesiveness as described above, the aqueous adhesive consisting of the aqueous solution of polyvinyl alcohol resin can be blended with a curing compound such as a polyhydric aldehyde, a water-soluble epoxy resin, a melamine compound, a zirconia compound, and a zinc compound. An example of the water-soluble epoxy resin is a water-soluble polyamide epoxy resin obtained by reacting epichlorohydrin with a polyamide polyamine obtained by reacting a polyalkylene polyamine such as diethylenetriamine or triethylenetetramine with a dicarboxylic acid such as adipic acid. Commercially available products of such polyamide epoxy resin include "Sumirez Resin 650" and "Sumirez Resin 675" sold by Sumika Chemtex Co., Ltd., and "WS-525" sold by Nippon PMC Co., Ltd. When a water-soluble epoxy resin is blended, the amount of the resin added is usually about 1 to 100 parts by mass, preferably 1 to 50 parts by mass, based on 100 parts by mass of the polyvinyl alcohol resin.
[0194] In addition, when a urethane resin is used as the main component of the water-based adhesive, it is effective to use a polyester ionomer urethane resin as the main component of the water-based adhesive. The polyester ionomer urethane resin here is a urethane resin having a polyester skeleton, into which a small amount of an ionic component (hydrophilic component) is introduced. Such an ionomer urethane resin can be emulsified directly in water without using an emulsifier to form an emulsion, and therefore can be used as a water-based adhesive. When a polyester ionomer urethane resin is used, it is effective to mix a water-soluble epoxy compound as a crosslinking agent. The use of a polyester ionomer urethane resin as an adhesive for a polarizing plate is described, for example, in JP-A-2005-70140 and JP-A-2005-208456.
[0195] These components constituting the water-based adhesive are usually used in a state dissolved in water. The water-based adhesive is applied to a suitable substrate and dried to obtain an adhesive layer. The components that do not dissolve in water may be in a dispersed state in the system.
[0196] The adhesive layer may be formed on the optical film by directly applying the adhesive composition to the surface of the optical film. The thickness of the adhesive layer is usually about 0.001 to 5 μm, preferably 0.01 μm or more, and more preferably 2 μm or less, and more preferably 1 μm or less. If the adhesive layer is too thick, the appearance of the polarizing plate is likely to be poor.
[0197] Furthermore, for example, a water-based adhesive can be injected between the polarizing plate and the present optical film, and then the adhesive can be heated to evaporate the water while promoting a thermal crosslinking reaction, thereby providing sufficient adhesion between the two.
[0198] The active energy ray curable adhesive may be any adhesive that is cured by irradiation with active energy rays and can bond the polarizing plate and the present optical film with a strength sufficient for practical use. For example, a cationic polymerizable active energy ray curable adhesive containing an epoxy compound and a cationic polymerization initiator, a radical polymerizable active energy ray curable adhesive containing an acrylic curing component and a radical polymerization initiator, an active energy ray curable adhesive containing both a cationic polymerizable curing component such as an epoxy compound and a radical polymerizable curing component such as an acrylic compound, and a cationic polymerization initiator and a radical polymerization initiator are added thereto, and an electron beam curable adhesive that is cured by irradiating an electron beam to an active energy ray curable adhesive that does not contain an initiator, etc. are included. A radical polymerizable active energy ray curable adhesive containing an acrylic curing component and a radical polymerization initiator is preferably used. In addition, a cationic polymerizable active energy ray curable adhesive containing an epoxy compound and a cationic polymerization initiator that can be used substantially without a solvent is preferred.
[0199] An active energy ray curable adhesive prepared by selecting an epoxy compound capable of cationic polymerization, which is liquid at room temperature, has appropriate fluidity even in the absence of a solvent, and provides appropriate cured adhesive strength, and by blending an appropriate cationic polymerization initiator therewith, can eliminate the need for drying equipment that is normally required in the step of bonding a polarizer and a transparent protective film in a polarizing plate manufacturing facility. In addition, the curing speed can be accelerated by irradiating an appropriate amount of active energy rays, thereby improving the production speed.
[0200] The epoxy compound used in such an adhesive may be, for example, a glycidyl etherified product of an aromatic compound or a chain compound having a hydroxyl group, a glycidyl amination product of a compound having an amino group, an epoxidized product of a chain compound having a CC double bond, or an alicyclic epoxy compound in which a glycidyloxy group or an epoxyethyl group is bonded directly or via an alkylene to a saturated carbon ring, or an epoxy group is bonded directly to a saturated carbon ring. These epoxy compounds may be used alone or in combination of different types. Among them, alicyclic epoxy compounds are preferably used because they have excellent cationic polymerizability.
[0201] The glycidyl ethers of aromatic compounds or chain compounds having a hydroxyl group can be produced, for example, by a method of subjecting the hydroxyl group of these aromatic compounds or chain compounds to addition condensation with epichlorohydrin under basic conditions. Such glycidyl ethers of aromatic compounds or chain compounds having a hydroxyl group include diglycidyl ethers of bisphenols, polyaromatic epoxy resins, diglycidyl ethers of alkylene glycols or polyalkylene glycols, etc.
[0202] Examples of diglycidyl ethers of bisphenols include glycidyl ethers of bisphenol A and their oligomers, glycidyl ethers of bisphenol F and their oligomers, and glycidyl ethers of 3,3',5,5'-tetramethyl-4,4'-biphenol and their oligomers.
[0203] Examples of polyaromatic ring epoxy resins include glycidyl ethers of phenol novolac resins, glycidyl ethers of cresol novolac resins, glycidyl ethers of phenol aralkyl resins, glycidyl ethers of naphthol aralkyl resins, glycidyl ethers of phenol dicyclopentadiene resins, etc. Furthermore, glycidyl ethers of trisphenols and their oligomers also belong to the polyaromatic ring epoxy resins.
[0204] Examples of diglycidyl ethers of alkylene glycols or polyalkylene glycols include glycidyl ethers of ethylene glycol, glycidyl ethers of diethylene glycol, glycidyl ethers of 1,4-butanediol, and glycidyl ethers of 1,6-hexanediol.
[0205] The glycidyl amination product of a compound having an amino group can be produced, for example, by a method of adding epichlorohydrin to the amino group of the compound under basic conditions. The compound having an amino group may also have a hydroxyl group. Such glycidyl amination products of a compound having an amino group include glycidyl amination products of 1,3-phenylenediamine and its oligomers, glycidyl amination products of 1,4-phenylenediamine and its oligomers, glycidyl amination products and glycidyl etherification products of 3-aminophenol and its oligomers, glycidyl amination products and glycidyl etherification products of 4-aminophenol and its oligomers, etc.
[0206] The epoxidized product of a chain compound having a CC double bond can be produced by a method of epoxidizing the CC double bond of the chain compound using a peroxide under basic conditions. The chain compound having a CC double bond includes butadiene, polybutadiene, isoprene, pentadiene, hexadiene, etc. Terpenes having a double bond can also be used as an epoxidation raw material, and linalool is an example of an acyclic monoterpene. The peroxide used for epoxidation can be, for example, hydrogen peroxide, peracetic acid, tert-butyl hydroperoxide, etc.
[0207] The alicyclic epoxy compound in which a glycidyloxy group or an epoxyethyl group is bonded to a saturated carbon ring directly or via an alkylene may be a glycidyl etherified product of a hydrogenated polyhydroxy compound obtained by hydrogenating an aromatic ring of an aromatic compound having a hydroxyl group, the typical examples of which are the bisphenols listed above; a glycidyl etherified product of a cycloalkane compound having a hydroxyl group; or an epoxidized product of a cycloalkane compound having a vinyl group.
[0208] The epoxy compounds described above are readily available as commercially available products, and examples of such products include the "jER" series sold by Mitsubishi Chemical Corporation, "Epicron" sold by DIC Corporation, "Epotohto (registered trademark)" sold by Tohto Kasei Co., Ltd., "Adeka Resin (registered trademark)" sold by ADEKA Corporation, "Denacol (registered trademark)" sold by Nagase ChemteX Corporation, "Dow Epoxy" sold by The Dow Chemical Company, and "Tepic (registered trademark)" sold by Nissan Chemical Industries, Ltd.
[0209] On the other hand, alicyclic epoxy compounds in which an epoxy group is directly bonded to a saturated carbon ring can be produced, for example, by a method of epoxidizing the CC double bond of a non-aromatic cyclic compound having a CC double bond in the ring using peroxide under basic conditions. Examples of non-aromatic cyclic compounds having a CC double bond in the ring include compounds having a cyclopentene ring, compounds having a cyclohexene ring, and polycyclic compounds in which at least two carbon atoms are further bonded to a cyclopentene ring or a cyclohexene ring to form an additional ring. A non-aromatic cyclic compound having a CC double bond in the ring may have another CC double bond outside the ring. Examples of non-aromatic cyclic compounds having a CC double bond in the ring include cyclohexene, 4-vinylcyclohexene, and monocyclic monoterpenes limonene and α-pinene.
[0210] The alicyclic epoxy compound in which an epoxy group is directly bonded to a saturated carbon ring may be a compound in which at least two alicyclic structures having an epoxy group directly bonded to the ring as described above are formed in the molecule via a suitable linking group. The linking group here includes, for example, an ester bond, an ether bond, an alkylene bond, etc.
[0211] Specific examples of alicyclic epoxy compounds in which an epoxy group is directly bonded to a saturated carbon ring include the following: 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 1,2-epoxy-4-vinylcyclohexane, 1,2-epoxy-4-epoxyethylcyclohexane, 1,2-epoxy-1-methyl-4-(1-methylepoxyethyl)cyclohexane, 3,4-epoxycyclohexylmethyl (meth)acrylate, Adduct of 2,2-bis(hydroxymethyl)-1-butanol with 4-epoxyethyl-1,2-epoxycyclohexane, Ethylene bis(3,4-epoxycyclohexanecarboxylate), Oxydiethylene bis(3,4-epoxycyclohexanecarboxylate), 1,4-Cyclohexanedimethyl bis(3,4-epoxycyclohexanecarboxylate), 3-(3,4-epoxycyclohexylmethoxycarbonyl)propyl 3,4-epoxycyclohexanecarboxylate, etc.
[0212] The alicyclic epoxy compounds in which an epoxy group is directly bonded to a saturated carbon ring as described above are also readily available as commercially available products, and examples thereof include the "Celloxide" series and "Cyclomer" sold by Daicel Corporation and the "Cyracure UVR" series sold by The Dow Chemical Company, each under a different trade name.
[0213] The curable adhesive containing an epoxy compound may further contain an active energy ray curable compound other than the epoxy compound. Examples of the active energy ray curable compound other than the epoxy compound include an oxetane compound and an acrylic compound. Among them, it is preferable to use an oxetane compound in combination because it may accelerate the curing speed in cationic polymerization.
[0214] The oxetane compound is a compound having a four-membered ring ether in the molecule, and examples thereof include the following: 1,4-bis[(3-ethyloxetan-3-yl)methoxymethyl]benzene, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, bis(3-ethyl-3-oxetanylmethyl) ether, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(cyclohexyloxymethyl)oxetane, Phenol novolac oxetane, 1,3-Bis[(3-ethyloxetan-3-yl)methoxy]benzene, etc.
[0215] Oxetane compounds are also readily available as commercially available products, and examples of such products include the "ARON OXETANE (registered trademark)" series sold by Toagosei Co., Ltd. and the "ETERNACOLL (registered trademark)" series sold by Ube Industries, Ltd.
[0216] It is preferable to use curable compounds including epoxy compounds and oxetane compounds that are not diluted with organic solvents, etc., in order to make the adhesive containing these compounds solvent-free. Also, it is preferable to use other components that make up the adhesive, including the cationic polymerization initiator and sensitizer described below, in the form of powder or liquid of the compound alone from which the organic solvent has been removed and dried, rather than those dissolved in an organic solvent.
[0217] The cationic polymerization initiator is a compound that generates cationic species upon irradiation with active energy rays, such as ultraviolet rays. Any compound that can provide the adhesive with the required adhesive strength and curing speed can be used, and examples of such compounds include aromatic diazonium salts; onium salts such as aromatic iodonium salts and aromatic sulfonium salts; and iron-arene complexes. These cationic polymerization initiators may be used alone or in combination with different types of compounds.
[0218] Examples of aromatic diazonium salts include the following: Benzenediazonium hexafluoroantimonate, benzenediazonium hexafluorophosphate, Benzenediazonium hexafluoroborate, etc.
[0219] Examples of aromatic iodonium salts include the following: diphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, Bis(4-nonylphenyl)iodonium hexafluorophosphate, etc.
[0220] Examples of aromatic sulfonium salts include the following: triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrakis(pentafluorophenyl)borate, Diphenyl(4-phenylthiophenyl)sulfonium hexafluoroantimonate, 4,4'-bis(diphenylsulfonio)diphenyl sulfide bishexafluorophosphate, 4,4'-Bis[di(β-hydroxyethoxyphenyl)sulfonio]diphenyl sulfide bishexafluoroantimonate, 4,4'-bis[di(β-hydroxyethoxyphenyl)sulfonio]diphenyl sulfide bishexafluorophosphate, 7-[di(p-toluyl)sulfonio]-2-isopropylthioxanthone hexafluoroantimonate, 7-[di(p-toluyl)sulfonio]-2-isopropylthioxanthone tetrakis(pentafluorophenyl)borate, 4-phenylcarbonyl-4'-diphenylsulfoniodiphenylsulfide hexafluorophosphate, 4-(p-tert-butylphenylcarbonyl)-4'-diphenylsulfoniodiphenyl sulfide hexafluoroantimonate, 4-(p-tert-butylphenylcarbonyl)-4'-di(p-toluyl)sulfonio-diphenyl sulfide tetrakis(pentafluorophenyl)borate, etc.
[0221] Examples of iron-arene complexes include the following: Xylene-cyclopentadienyliron(II) hexafluoroantimonate, Cumene-cyclopentadienyliron(II) hexafluorophosphate, Xylene-cyclopentadienyliron(II) tris(trifluoromethylsulfonyl)methanide, etc.
[0222] Among the cationic polymerization initiators, aromatic sulfonium salts are preferably used because they have ultraviolet absorption properties even in the wavelength region of 300 nm or more and can provide an adhesive layer with excellent curing properties and good mechanical strength and adhesive strength.
[0223] The cationic polymerization initiator is also easily available as a commercially available product, and examples of such product names include the "Kayarad (registered trademark)" series sold by Nippon Kayaku Co., Ltd., the "Cyracure UVI" series sold by The Dow Chemical Company, the photoacid generator "CPI" series sold by San-Apro Ltd., the photoacid generators "TAZ", "BBI" and "DTS" sold by Midori Chemical Co., Ltd., the "ADEKA Optomer" series sold by ADEKA Corporation, and "RHODORSIL (registered trademark)" sold by Rhodia.
[0224] In the active energy ray curable adhesive, the cationic polymerization initiator is usually mixed in a ratio of 0.5 to 20 parts by mass, preferably 1 to 15 parts by mass, based on 100 parts by mass of the total amount of the active energy ray curable adhesive. If the amount is too small, the curing may be insufficient, and the mechanical strength and adhesive strength of the adhesive layer may be reduced. If the amount is too large, the ionic substance in the adhesive layer increases, and the hygroscopicity of the adhesive layer may increase, which may reduce the durability of the obtained polarizing plate.
[0225] When the active energy ray-curable adhesive is used as an electron beam-curable adhesive, it is not particularly necessary to include a photopolymerization initiator in the composition, but when it is used as an ultraviolet ray-curable adhesive, it is preferable to use a photoradical generator. Examples of the photoradical generator include a hydrogen abstraction type photoradical generator and a cleavage type photoradical generator.
[0226] Examples of the hydrogen abstraction type photoradical generator include naphthalene derivatives such as 1-methylnaphthalene, 2-methylnaphthalene, 1-fluoronaphthalene, 1-chloronaphthalene, 2-chloronaphthalene, 1-bromonaphthalene, 2-bromonaphthalene, 1-iodonaphthalene, 2-iodonaphthalene, 1-naphthol, 2-naphthol, 1-methoxynaphthalene, 2-methoxynaphthalene, and 1,4-dicyanonaphthalene; anthracene, 1,2-benzanthracene, 9,10-dichloroanthracene, and 9,10-dibromoanthracene. anthracene derivatives such as 9,10-diphenylanthracene, 9-cyanoanthracene, 9,10-dicyanoanthracene, and 2,6,9,10-tetracyanoanthracene; pyrene derivatives; carbazole, 9-methylcarbazole, 9-phenylcarbazole, 9-prop-2-ynyl-9H-carbazole, 9-propyl-9H-carbazole, 9-vinylcarbazole, 9H-carbazole-9-ethanol, 9-methyl-3-nitro-9H-carbazole, 9-methyl-3,6-dinitro-9H-carbazole, 9-nitro ... Cutanoylcarbazole, 9-carbazolemethanol, 9-carbazolepropionic acid, 9-carbazolepropionitrile, 9-ethyl-3,6-dinitro-9H-carbazole, 9-ethyl-3-nitrocarbazole, 9-ethylcarbazole, 9-isopropylcarbazole, 9-(ethoxycarbonylmethyl)carbazole, 9-(morpholinomethyl)carbazole, 9-acetylcarbazole, 9-allylcarbazole, 9-benzyl-9H-carbazole, 9-carbazoleacetic acid, 9-(2-nitrophenyl)carbazole carbazole, 9-(4-methoxyphenyl)carbazole, 9-(1-ethoxy-2-methyl-propyl)-9H-carbazole, 3-nitrocarbazole, 4-hydroxycarbazole, 3,6-dinitro-9H-carbazole, 3,6-diphenyl-9H-carbazole, 2-hydroxycarbazole, 3,6-diacetyl-9-ethylcarbazole and other carbazole derivatives; benzophenone, 4-phenylbenzophenone, 4,4'-bis(dimethoxy)benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,Benzophenone derivatives such as 4'-bis(diethylamino)benzophenone, 2-benzoylbenzoic acid methyl ester, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, and 2,4,6-trimethylbenzophenone, aromatic carbonyl compounds, [4-(4-methylphenylthio)phenyl]-phenylmethanone, xanthone, thioxanthone, 2-chlorothioxanthone, 4-chlorothioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 1-chloro-4-propoxythioxanthone, as well as coumarin derivatives.
[0227] The cleavage-type photoradical generator is a type of photoradical generator in which the compound is cleaved to generate radicals by irradiation with active energy rays. Specific examples include, but are not limited to, aryl alkyl ketones such as benzoin ether derivatives and acetophenone derivatives, oxime ketones, acylphosphine oxides, S-phenyl thiobenzoates, titanocenes, and polymerized derivatives thereof. Commercially available cleavage-type photoradical generators include 1-(4-dodecylbenzoyl)-1-hydroxy-1-methylethane, 1-(4-isopropylbenzoyl)-1-hydroxy-1-methylethane, 1-benzoyl-1-hydroxy-1-methylethane, 1-[4-(2-hydroxyethoxy)-benzoyl]-1-hydroxy-1-methylethane, 1-[4-(acryloyloxyethoxy)-benzoyl]-1-hydroxy-1-methylethane, diphenyl ketone, phenyl-1-hydroxy-cyclohexyl ketone, benzyl dimethyl ketal, bis(cyclopentadienyl)-bis(2,6-difluoro-3-pyrryl-phenyl)titanium, (η 6-isopropylbenzene)-(η5-cyclopentadienyl)-iron(II) hexafluorophosphate, trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxy-benzoyl)-(2,4,4-trimethyl-pentyl)-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dipentoxyphenylphosphine oxide or bis(2,4,6-trimethylbenzoyl)phenyl-phosphine oxide, (4-morpholinobenzoyl)-1-benzyl-1-dimethylaminopropane, 4-(methylthiobenzoyl)-1-methyl-1-morpholinoethane and the like, but are not limited thereto.
[0228] Among the active energy curing adhesives used in the present invention, the photoradical generators contained in the electron beam curing type, that is, hydrogen abstraction type or cleavage type photoradical generators, can be used alone or in combination, but in terms of the stability of the photoradical generator alone and curability, a combination of one or more cleavage type photoradical generators is more preferable. Among the cleavage type photoradical generators, acylphosphine oxides are preferred, and more specifically, trimethylbenzoyldiphenylphosphine oxide (trade name "DAROCURE TPO"; Ciba Japan Co., Ltd.), bis(2,6-dimethoxy-benzoyl)-(2,4,4-trimethyl-pentyl)-phosphine oxide (trade name "CGI 403"; Ciba Japan Co., Ltd.), or bis(2,4,6-trimethylbenzoyl)-2,4-dipentoxyphenylphosphine oxide (trade name "Irgacure819"; Ciba Japan Co., Ltd.) are preferred.
[0229] The active energy ray curable adhesive may contain a sensitizer as necessary. By using a sensitizer, the reactivity can be improved, and the mechanical strength and adhesive strength of the adhesive layer can be further improved. As the sensitizer, the above-mentioned ones can be appropriately used.
[0230] When a sensitizer is added, the amount of the sensitizer added is preferably within a range of 0.1 to 20 parts by mass with respect to 100 parts by mass of the total amount of the active energy ray-curable adhesive.
[0231] Various additives can be blended into the active energy ray-curable adhesive within a range that does not impair the effect of the adhesive, such as an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow control agent, a plasticizer, and an antifoaming agent.
[0232] Each of these components constituting the active energy ray curable adhesive is usually used in a state of being dissolved in a solvent. When the active energy ray curable adhesive contains a solvent, the active energy ray curable adhesive is applied to a suitable substrate and dried to obtain an adhesive layer. The components that are not dissolved in the solvent may be in a state of being dispersed in the system.
[0233] The adhesive layer may be formed on the optical film by directly applying the adhesive composition to the surface of the optical film. The thickness of the adhesive layer is usually about 0.001 to 5 μm, preferably 0.01 μm or more, and more preferably 2 μm or less, and more preferably 1 μm or less. If the adhesive layer is too thick, the appearance of the polarizing plate is likely to be poor.
[0234] The active energy ray curable adhesive can be applied to the film by the above-mentioned application method. In this case, the viscosity of the active energy ray curable adhesive may be any viscosity that allows application by various methods, but the viscosity at a temperature of 25°C is preferably in the range of 10 to 30,000 mPa·sec, and more preferably in the range of 50 to 6,000 mPa·sec. If the viscosity is too low, it tends to be difficult to obtain a uniform coating film without unevenness. On the other hand, if the viscosity is too high, it tends to be difficult to flow, and it also tends to be difficult to obtain a uniform coating film without unevenness. The viscosity here is the value measured at 60 rpm after adjusting the temperature of the adhesive to 25°C using a B-type viscometer.
[0235] The active energy ray curable adhesive can be used in the form of an electron beam curable type or an ultraviolet ray curable type. The active energy ray of the present invention is defined as an energy ray capable of decomposing a compound that generates an active species to generate an active species. Examples of such active energy ray include visible light, ultraviolet ray, infrared ray, X-ray, α-ray, β-ray, γ-ray, and electron beam.
[0236] In the electron beam curing type, the irradiation conditions of the electron beam can be any suitable conditions as long as the active energy beam curing adhesive can be cured. For example, the acceleration voltage of the electron beam irradiation is preferably 5 kV to 300 kV, more preferably 10 kV to 250 kV. If the acceleration voltage is less than 5 kV, the electron beam may not reach the adhesive, resulting in insufficient curing, and if the acceleration voltage is more than 300 kV, the penetration power through the sample is too strong, causing the electron beam to bounce back and damaging the transparent protective film and polarizer. The irradiation dose is 5 to 100 kGy, more preferably 10 to 75 kGy. If the irradiation dose is less than 5 kGy, the adhesive will not be cured sufficiently, and if it exceeds 100 kGy, the transparent protective film and polarizer will be damaged, causing a decrease in mechanical strength and yellowing, and the desired optical characteristics cannot be obtained.
[0237] Electron beam irradiation is usually performed in an inert gas, but if necessary, it may be performed in the air or with a small amount of oxygen introduced. Depending on the material of the transparent protective film, by appropriately introducing oxygen, oxygen inhibition is intentionally generated on the transparent protective film surface that is first hit by the electron beam, which makes it possible to prevent damage to the transparent protective film and to efficiently irradiate the electron beam only to the adhesive.
[0238] In the case of the ultraviolet ray curing type, the light irradiation intensity of the active energy ray curing adhesive is determined depending on the composition of the adhesive and is not particularly limited, but is preferably 10 to 5000 mW / cm. 2 It is preferable that the light irradiation intensity of the resin composition is 10 mW / cm 2 If it is less than 5000mW / cm, the reaction time will be too long and 2 If the temperature exceeds this range, the heat radiated from the light source and the heat generated during polymerization of the composition may cause yellowing of the materials constituting the adhesive and deterioration of the polarizer. The irradiation intensity is preferably an intensity in a wavelength region effective for activating the cationic photopolymerization initiator, more preferably an intensity in a wavelength region of 400 nm or less, and further preferably an intensity in a wavelength region of 280 to 320 nm. Irradiation is performed once or multiple times with such a light irradiation intensity, and the accumulated light amount is 10 mJ / cm.2 or more, preferably 10 to 5,000 mJ / cm 2 It is preferable that the integrated light amount to the adhesive is set to 10 mJ / cm. 2 If the cumulative light amount is less than 5,000 mJ / cm2, the generation of active species derived from the polymerization initiator is insufficient, and the adhesive is not cured sufficiently. 2 If the exposure time exceeds this limit, the exposure time will be extremely long, which is detrimental to improving productivity. In this case, the required cumulative light amount in the wavelength range (UVA (320-390 nm), UVB (280-320 nm), etc.) will differ depending on the combination of film and adhesive used.
[0239] The light source used for polymerizing and curing the adhesive by irradiation with active energy rays in the present invention is not particularly limited, and examples thereof include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave excited mercury lamps, and metal halide lamps. From the viewpoint of energy stability and device simplicity, ultraviolet light sources having an emission distribution at wavelengths of 400 nm or less are preferred.
[0240] [Circular polarizing plate] The present optical film can be combined with a polarizing plate to obtain a circular polarizing plate (hereinafter, sometimes referred to as the present circular polarizing plate) that includes the present optical film and a polarizing plate. The present optical film and the polarizing plate are usually bonded together with an adhesive. Preferably, they are bonded together with an active energy ray curable adhesive. When the first retardation layer is composed of only one layer and has only one slow axis, it is preferable to set the transmission axis of the polarizing plate to be substantially 45° with respect to the slow axis (optical axis) of the first retardation layer of the present optical film. Substantially 45° is usually in the range of 45±5°. Figure 3 shows a schematic diagram of the present circular polarizing plate 110.
[0241] The polarizing plate used in the present circular polarizing plate shown in FIG. 3 may have a protective film on one side of the polarizer, or may have protective films on both sides of the polarizer. FIGS. 3(c) to 3(h) show circular polarizing plates made of the present optical film having first and second retardation layers formed on a substrate, and these substrates can also function as a protective film on the other side when a polarizing plate having a protective film on one side of the polarizer is used. The configurations shown in FIGS. 3(a) and 3(b) are formed by laminating the present optical film having no substrate, but the retardation layer may be formed by directly applying a polymerizable liquid crystal composition on the polarizing plate, the retardation layer may be bonded to the polarizer surface using an adhesive, or the retardation layer may be bonded to the polarizing plate using an adhesive.
[0242] Examples of a method for bonding the present optical film without a substrate to other substrates such as a polarizer surface or a polarizing plate include a method of bonding the present optical film from which the substrate has been removed to other substrates using an adhesive, and a method of bonding the present optical film to other substrates using an adhesive and then removing the substrate. In this case, the adhesive may be applied to the retardation layer side of the present optical film, or may be applied to the other substrate side. When an alignment film is present between the substrate and the retardation layer, the alignment film may be removed together with the substrate.
[0243] A substrate having a functional group on its surface that forms a chemical bond with a retardation layer or an alignment film, etc., tends to be difficult to remove due to the formation of a chemical bond with the retardation layer or the alignment film, etc. Therefore, when removing the substrate by peeling, a substrate having a small number of functional groups on its surface is preferred, and a substrate that has not been subjected to a surface treatment that forms a functional group on its surface is preferred. In addition, since an alignment film having a functional group that forms a chemical bond with a substrate tends to have a large adhesive force between the substrate and the alignment film, when the substrate is peeled off and removed, an alignment film having a small number of functional groups that form a chemical bond with the substrate is preferred. In addition, it is preferable that a reagent that crosslinks the substrate and the alignment film is not included, and further, it is preferable that a solution of the alignment polymer composition and the photoalignment film forming composition does not include a component such as a solvent that dissolves the substrate. In addition, the alignment film having a functional group that forms a chemical bond with the retardation layer tends to have a large adhesive force between the retardation layer and the alignment film. Therefore, when removing the alignment film together with the substrate, an alignment film having a small number of functional groups that form a chemical bond with the retardation layer is preferable. In addition, it is preferable that the retardation layer and the alignment film do not contain a reagent that crosslinks the retardation layer and the alignment film. In addition, the retardation layer having a functional group that forms a chemical bond with the alignment film tends to have a large adhesion between the alignment film and the retardation layer. Therefore, when removing the substrate or removing the alignment film together with the substrate, a retardation layer having a small number of functional groups that form a chemical bond with the substrate or alignment film is preferred. In addition, the polymerizable liquid crystal composition preferably does not contain a reagent that crosslinks the substrate or alignment film with the retardation layer.
[0244] For example, a circular polarizing plate having a structure shown in Fig. 3(a) in which a polarizing plate, a first retardation layer, and a second retardation layer are laminated in this order can be manufactured by applying an adhesive to the surface of the first retardation layer of the present optical film in which a substrate, a second retardation layer, and a first retardation layer are laminated in this order, laminating a polarizing plate thereon, and then removing the substrate of the present optical film. Also, a circular polarizing plate having a structure shown in Fig. 3(b) in which a polarizing plate, a second retardation layer, and a first retardation layer are laminated in this order can be manufactured by applying an adhesive to the surface of the second retardation layer of the present optical film in which a substrate, a first retardation layer, and a second retardation layer are laminated in this order, laminating a polarizing plate thereon, and then removing the substrate of the present optical film. The configurations shown in Figs. 3(i) to 3(n) are formed by laminating the present optical films each having two substrates.
[0245] The configuration of the present circular polarizing plate when the first retardation layer includes the layer A and the layer B, or when the first retardation layer includes the third retardation layer, is shown in Fig. 4. In the case of the configuration including the layer A and the layer B, or the third retardation layer, there is a restriction on the position where the polarizing plate is laminated. Specifically, when laminating a layer A having a phase difference of λ / 4 and a layer B having a phase difference of λ / 2, first, layer B is formed so that the slow axis of layer B is at 75° with respect to the absorption axis of the polarizing plate, and then layer A is formed so that the slow axis of layer A is at 15°. In addition, when the first retardation layer has a phase difference of λ / 4 and the third retardation layer has a phase difference of λ / 2, the third retardation layer is first formed so that the slow axis of the third retardation layer is 75° with respect to the absorption axis of the polarizing plate, and then the first retardation layer is formed so that the slow axis of the first retardation layer is 15°. There is no limitation on the position of the second retardation layer, but it is necessary that the polarizing plate, layer B and layer A are laminated in this order, or the polarizing plate, the third retardation layer and the first retardation layer are laminated in this order. By laminating in this way, the obtained circular polarizing plate can function as a wideband λ / 4 plate. Here, there is no limitation on the axial angle forming Layer A and Layer B. For example, as described in JP 2004-126538 A, it is known that the function of a broadband λ / 4 plate can be exhibited even if the slow axis angles of Layer A and Layer B are 30° and −30°, or 45° and −45° with respect to the absorption axis of the polarizing plate. Therefore, it is possible to laminate the layers in a desired manner. The configurations shown in Figures 4(a) and 4(b) are formed by laminating the present optical film without a substrate, and circular polarizing plates having these configurations can be manufactured by a method similar to the manufacturing method of the circular polarizing plate having the configuration shown in Figures 3(a) and 3(b) described above.
[0246] The present circular polarizing plate can be used in various display devices, but can be effectively used in particular in organic electroluminescence (EL) display devices and inorganic electroluminescence (EL) display devices, as well as organic electroluminescence display devices equipped with a touch panel.
[0247] <Polarizing plate> The polarizing plate may be any film having a polarizing function. Examples of the film include a stretched film having a dye with anisotropic absorption adsorbed thereon, or a film including a film coated with a dye with anisotropic absorption as a polarizer. Examples of the dye with anisotropic absorption include a dichroic dye.
[0248] A film including, as a polarizer, a stretched film having adsorbed thereon a dye having absorption anisotropy is usually produced by uniaxially stretching a polyvinyl alcohol-based resin film, dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, treating the polyvinyl alcohol-based resin film having the adsorbed dichroic dye with an aqueous boric acid solution, and washing the film with water after the treatment with the aqueous boric acid solution, and then sandwiching the film between a transparent protective film via an adhesive on at least one surface of the polarizer produced through these steps.
[0249] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. As polyvinyl acetate resins, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith are used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.
[0250] The degree of saponification of the polyvinyl alcohol resin is usually about 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can also be used. The degree of polymerization of the polyvinyl alcohol resin is usually about 1,000 to 10,000, preferably in the range of 1,500 to 5,000.
[0251] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizing plate. The method for forming a film of the polyvinyl alcohol-based resin is not particularly limited, and the film can be formed by a known method. The thickness of the polyvinyl alcohol-based raw film can be, for example, about 10 to 150 μm.
[0252] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. It is also possible to perform the uniaxial stretching at these multiple stages. In the uniaxial stretching, the film may be uniaxially stretched between rolls having different peripheral speeds, or may be uniaxially stretched using a heated roll. The uniaxial stretching may be dry stretching in which stretching is performed in the air, or wet stretching in which stretching is performed in a state where the polyvinyl alcohol-based resin film is swollen using a solvent. The stretching ratio is usually about 3 to 8 times.
[0253] Dyeing of a polyvinyl alcohol-based resin film with a dichroic dye is carried out, for example, by a method of immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye. Specifically, iodine or a dichroic organic dye is used as the dichroic pigment. Examples of the dichroic organic dye include a dichroic direct dye made of a disazo compound such as CI DIRECT RED 39, and a dichroic direct dye made of a compound such as a trisazo or tetrakisazo. The polyvinyl alcohol resin film is preferably immersed in water before the dyeing process.
[0254] When iodine is used as the dichroic dye, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing iodine and potassium iodide is usually adopted. The content of iodine in this aqueous solution is usually about 0.01 to 1 part by mass per 100 parts by mass of water. The content of potassium iodide is usually about 0.5 to 20 parts by mass per 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is usually about 20 to 40°C. The immersion time in this aqueous solution (dyeing time) is usually about 20 to 1,800 seconds.
[0255] On the other hand, when a dichroic organic dye is used as the dichroic coloring matter, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing a water-soluble dichroic dye is usually employed. The content of the dichroic organic dye in this aqueous solution is usually 1×10 -4 ~10 parts by mass, preferably 1 × 10 -3 ~1 part by mass, more preferably 1 × 10 -3 ~1×10 -2 The amount of each component is expressed as parts by mass. This aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing assistant. The temperature of the aqueous dichroic dye solution used for dyeing is usually about 20 to 80°C. The immersion time in this aqueous solution (dyeing time) is usually about 10 to 1,800 seconds.
[0256] The boric acid treatment after dyeing with a dichroic dye can usually be carried out by immersing the dyed polyvinyl alcohol resin film in an aqueous boric acid solution. The content of boric acid in this aqueous boric acid solution is usually about 2 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. When iodine is used as the dichroic dye, this aqueous boric acid solution preferably contains potassium iodide, and in this case, the content of potassium iodide is usually about 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. The immersion time in the aqueous boric acid solution is usually about 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually 50°C or higher, preferably 50 to 85°C, and more preferably 60 to 80°C.
[0257] The polyvinyl alcohol-based resin film after the boric acid treatment is usually washed with water. The washing can be performed, for example, by immersing the polyvinyl alcohol-based resin film treated with boric acid in water. The temperature of the water used in the washing is usually about 5 to 40°C. The immersion time is usually about 1 to 120 seconds.
[0258] After washing with water, a drying treatment is carried out to obtain a polarizer. The drying treatment can be carried out using, for example, a hot air dryer or a far infrared heater. The temperature of the drying treatment is usually about 30 to 100°C, and preferably 50 to 80°C. The time of the drying treatment is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content of the polarizer is reduced to a practical level by the drying treatment. The moisture content is usually about 5 to 20% by weight, and preferably 8 to 15% by weight. If the moisture content is less than 5% by weight, the polarizer loses its flexibility, and the polarizer may be damaged or broken after drying. If the moisture content exceeds 20% by weight, the thermal stability of the polarizer may be deteriorated.
[0259] The polyvinyl alcohol-based resin film is then uniaxially stretched, dyed with a dichroic dye, treated with boric acid, washed with water and dried to obtain a polarizer having a thickness of preferably 5 to 40 μm.
[0260] Examples of the film coated with a dye having absorption anisotropy include a film obtained by coating a composition containing a dichroic dye having liquid crystal properties, or a composition containing a dichroic dye and a polymerizable liquid crystal, etc. The film preferably has a protective film on one or both sides. The protective film may be the same as the above-mentioned substrate.
[0261] The film coated with the dye having absorption anisotropy is preferably thin, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the film is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 μm or more and 3 μm or less.
[0262] Specific examples of the film coated with a dye having absorption anisotropy include the films described in JP-A-2012-33249 and the like.
[0263] A polarizing plate is obtained by laminating a transparent protective film via an adhesive on at least one surface of the polarizer thus obtained. As the transparent protective film, the same transparent film as the above-mentioned substrate can be preferably used, or the optical film of the present invention can be used.
[0264] The present optical film and the present circular polarizer can be used in a variety of display devices. A display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, a touch panel display device, an electron emission display device (e.g., a field emission display device (FED) and a surface field emission display device (SED)), an electronic paper (a display device using electronic ink or an electrophoretic element, a plasma display device, a projection display device (e.g., a grating light valve (GLV) display device, a display device having a digital micromirror device (DMD)), and a piezoelectric ceramic display. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection liquid crystal display device. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images. In particular, the present circular polarizer can be effectively used in an organic electroluminescence (EL) display device and an inorganic electroluminescence (EL) display device, and the present optical compensation polarizer can be effectively used in a liquid crystal display device and a touch panel display device.
[0265] FIG. 5 is a schematic diagram of an organic EL display device 200 equipped with the present circular polarizer. Fig. 5(a) shows an organic EL display device 200 in which a polarizing plate 6, a first retardation layer 1, a second retardation layer 2, and an organic EL panel 7 are laminated in this order. Fig. 5(c) shows an organic EL display device 200 in which a polarizing plate 6, a base material 3, a first retardation layer 1, a second retardation layer 2, and an organic EL panel 7 are laminated in this order. Figs. 5(b), (d) to (h) show a different lamination order from Figs. 5(a) and (c). Examples of a method for laminating a polarizing plate, the present optical film, and an organic EL panel include a method of laminating the present circularly polarizing plate, which is a laminate of a polarizing plate and the present optical film, to an organic EL panel, and a method of laminating the present optical film to an organic EL panel and then laminating a polarizing plate on the surface of the present optical film. An adhesive is usually used for lamination. For example, the organic EL display device 200 shown in Fig. 5(a) can be manufactured by applying an adhesive to the surface of the second retardation layer 2 of the present circular polarizer shown in Fig. 3(a) and laminating an organic EL panel 7 thereto. The organic EL display device 200 shown in Fig. 5(a) can also be manufactured by applying an adhesive to the surface of the second retardation layer 2 of the present optical film shown in Fig. 1(b) and laminating an organic EL panel 7 thereto, removing the base material 3 of the present optical film, applying an adhesive to the surface of the first retardation layer 1 revealed by removing the base material, and laminating a polarizer 6 thereto.
[0266] FIG. 6 is a schematic diagram showing an organic EL display device 30. The organic EL display device 30 shown in FIG. 6(a) includes the present circular polarizer 31, and is formed by stacking a light-emitting layer 35 and a cathode electrode 36 on a substrate 32 on which a pixel electrode 34 is formed, with an interlayer insulating film 33 interposed therebetween. The present circular polarizer 31 is disposed on the opposite side of the substrate 32 to the light-emitting layer 35. The light-emitting layer 35 emits light when a positive voltage is applied to the pixel electrode 34 and a negative voltage is applied to the cathode electrode 36, and a direct current is applied between the pixel electrode 34 and the cathode electrode 36. The light-emitting layer 35 is composed of an electron transport layer, a light-emitting layer, a hole transport layer, and the like. The light emitted from the light-emitting layer 35 passes through the pixel electrode 34, the interlayer insulating film 33, the substrate 32, and the present circular polarizer 31.
[0267] To manufacture the organic EL display device 30, first, a thin-film transistor 38 is formed in a desired shape on a substrate 32. Then, an interlayer insulating film 33 is formed, and then a pixel electrode 34 is formed by sputtering and patterned. After that, a light-emitting layer 35 is laminated.
[0268] Next, the circular polarizer 31 is provided on the surface of the substrate 32 opposite to the surface on which the thin film transistor 38 is provided. In this case, the circular polarizer 31 is disposed so that the polarizer faces outward (opposite the substrate 32).
[0269] Examples of the substrate 32 include ceramic substrates such as sapphire glass substrates, quartz glass substrates, soda glass substrates, and alumina; metal substrates such as copper; and plastic substrates. Although not shown, a thermally conductive film may be formed on the substrate 32. Examples of the thermally conductive film include diamond thin films (DLC, etc.). When the pixel electrodes 34 are reflective, light is emitted in the opposite direction to the substrate 32. Therefore, not only transparent materials but also non-transparent materials such as stainless steel can be used. The substrate may be formed as a single substrate, or may be formed as a laminated substrate by bonding multiple substrates with an adhesive. Moreover, these substrates are not limited to plate-shaped ones, and may be films.
[0270] For example, a polycrystalline silicon transistor may be used as the thin film transistor 38. The thin film transistor 38 is provided at the end of the pixel electrode 34, and has a size of about 10 to 30 μm. The size of the pixel electrode 34 is about 20 μm×20 μm to 300 μm×300 μm.
[0271] Wiring electrodes of thin film transistors 38 are provided on the substrate 32. The wiring electrodes have low resistance and function to keep the resistance low by electrically connecting to pixel electrodes 34, and generally, the wiring electrodes contain one or more of Al, Al and a transition metal (excluding Ti), Ti, or titanium nitride (TiN).
[0272] An interlayer insulating film 33 is provided between the thin film transistor 38 and the pixel electrode 34. The interlayer insulating film 33 may be any insulating material, such as a film formed by sputtering or vacuum deposition of an inorganic material such as silicon oxide such as SiO2 or silicon nitride, a silicon oxide layer formed by SOG (spin-on-glass), or a coating of a resin material such as photoresist, polyimide, or acrylic resin.
[0273] Ribs 39 are formed on the interlayer insulating film 33. The ribs 39 are disposed in the periphery of the pixel electrodes 34 (between adjacent pixels). Examples of materials for the ribs 39 include acrylic resin and polyimide resin. The thickness of the ribs 39 is preferably 1.0 μm or more and 3.5 μm or less, and more preferably 1.5 μm or more and 2.5 μm or less.
[0274] Next, a description will be given of an EL element consisting of a pixel electrode 34, a light-emitting layer 35, and a cathode electrode 36. The light-emitting layer 35 has at least one hole transport layer and one light-emitting layer, and has, for example, an electron injection transport layer, a light-emitting layer, a hole transport layer, and a hole injection layer, in that order.
[0275] Examples of the pixel electrode 34 include ITO (tin-doped indium oxide), IZO (zinc-doped indium oxide), IGZO, ZnO, SnO2, and In2O3, with ITO and IZO being particularly preferred. The pixel electrode 35 only needs to have a certain thickness or more that allows sufficient hole injection, and is preferably about 10 to 500 nm.
[0276] The pixel electrode 34 can be formed by a vapor deposition method (preferably a sputtering method). There is no particular limitation on the sputtering gas, and an inert gas such as Ar, He, Ne, Kr, or Xe, or a mixed gas of these may be used.
[0277] Metal elements such as K, Li, Na, Mg, La, Ce, Ca, Sr, Ba, Al, Ag, In, Sn, Zn, and Zr may be used as the material for the cathode electrode 36, but in order to improve the operational stability of the electrode, it is preferable to use an alloy system of two or three components selected from the metal elements exemplified above. Preferred alloy systems include, for example, Ag·Mg (Ag: 1-20 at%), Al·Li (Li: 0.3-14 at%), In·Mg (Mg: 50-80 at%), and Al·Ca (Ca: 5-20 at%).
[0278] The cathode electrode 36 is formed by a deposition method, a sputtering method, etc. The thickness of the cathode electrode 37 is preferably 0.1 nm or more, and more preferably 1 to 500 nm or more.
[0279] The hole injection layer has a function of facilitating the injection of holes from the pixel electrode 34, and the hole transport layer has a function of transporting holes and blocking electrons, and is also called a charge injection layer or a charge transport layer.
[0280] The thickness of the light-emitting layer, the combined thickness of the hole injection layer and the hole transport layer, and the thickness of the electron injection transport layer are not particularly limited and vary depending on the formation method, but are preferably about 5 to 100 nm. Various organic compounds can be used for the hole injection layer and the hole transport layer. The hole injection transport layer, the light-emitting layer, and the electron injection transport layer can be formed by vacuum deposition, which allows the formation of a homogeneous thin film.
[0281] The light-emitting layer 35 may be one that utilizes light emission (fluorescence) from singlet excitons, one that utilizes light emission (phosphorescence) from triplet excitons, one that includes one that utilizes light emission (fluorescence) from singlet excitons and one that utilizes light emission (phosphorescence) from triplet excitons, one that is made of an organic substance, one that includes one that is made of an organic substance and one that is made of an inorganic substance, a polymeric material, a low molecular weight material, one that includes a polymeric material and a low molecular weight material, etc. However, the light-emitting layer 35 is not limited to these, and various materials known for EL elements can be used in the organic EL display device 30.
[0282] A desiccant (not shown) is placed in the space between the cathode electrode 36 and the sealing layer 37. This is because the light-emitting layer 35 is sensitive to humidity. The desiccant absorbs moisture and prevents the light-emitting layer 35 from deteriorating.
[0283] 6(b) includes the present circular polarizer 31, and is formed by laminating a light-emitting layer 35 and a cathode electrode 36 on a substrate 32 on which a pixel electrode 34 is formed, with an interlayer insulating film 33 interposed therebetween. A sealing layer 37 is formed on the cathode electrode, and the present circular polarizer 31 is disposed on the opposite side to the substrate 32. Light emitted from the light-emitting layer 35 passes through the cathode electrode 36, the sealing layer 37, and the present circular polarizer 31. EXAMPLES
[0284] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified. The cycloolefin polymer film (COP) used was ZF-14 manufactured by Zeon Corporation. The corona treatment device used was AGF-B10 manufactured by Kasuga Denki Co., Ltd. The corona treatment was carried out once using the above corona treatment device under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The polarized UV irradiation device used was a SPOT CURE SP-7 with a polarizer unit manufactured by Ushio Inc. The laser microscope used was LEXT manufactured by Olympus Corporation. The high pressure mercury lamp used was a Uniqure VB-15201BY-A manufactured by Ushio Electric Co., Ltd. The phase difference value was measured using KOBRA-WR manufactured by Oji Scientific Instruments.
[0285] Example 1 [Preparation of composition for forming photoalignment film] The following components were mixed, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photoalignment film (1). Photoalignable material (5 parts): TIFF0007573000000017.tif1750 Solvent (95 parts): Cyclopentanone
[0286] [Preparation of Oriented Polymer Composition (1)] The composition of the oriented polymer composition (1) is shown in Table 1. The oriented polymer composition (1) was obtained by adding 2-butoxyethanol to Sunever SE-610 (manufactured by Nissan Chemical Industries, Ltd.), which is a commercially available oriented polymer.
[0287] [Preparation of Oriented Polymer Composition (2)] The composition of the oriented polymer composition (2) is shown in Table 1. Water was added to commercially available polyvinyl alcohol (polyvinyl alcohol 1000 fully saponified type, manufactured by Wako Pure Chemical Industries, Ltd.), and the mixture was heated at 100°C for 1 hour to obtain the oriented polymer composition (2).
[0288] [Table 1] The values in Table 1 represent the content ratio of each component relative to the total amount of the prepared composition. For SE-610, the solid content was calculated from the concentration listed on the delivery specification.
[0289] [Preparation of Composition (A-1)] The following components were mixed and the resulting mixture was stirred at 80° C. for 1 hour to obtain composition (A-1).
[0290] The polymerizable liquid crystal A1 and the polymerizable liquid crystal A2 were synthesized by the method described in JP-A-2010-31223. Polymerizable liquid crystal A1 (80 parts): TIFF0007573000000019.tif39132
[0291] Polymerizable liquid crystal A2 (20 parts): TIFF0007573000000020.tif31130
[0292] Polymerization initiator (6 parts): 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals) Leveling agent (0.1 part): Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) Solvent: Cyclopentanone (400 parts)
[0293] [Preparation of Composition (B-1)] The composition of composition (B-1) is shown in Table 2. The components were mixed, and the resulting solution was stirred at 80° C. for 1 hour, and then cooled to room temperature to obtain composition (B-1).
[0294] [Table 2] The values in parentheses in Table 2 indicate the content ratio of each component relative to the total amount of the prepared composition. In Table 2, LR9000 represents Laromer (registered trademark) LR-9000 manufactured by BASF Japan, Irg907 represents Irgacure (registered trademark) 907 manufactured by BASF Japan, BYK361N represents a leveling agent manufactured by BYK Japan, LC242 represents a polymerizable liquid crystal manufactured by BASF and represented by the following formula, and PGMEA represents propylene glycol 1-monomethyl ether 2-acetate. TIFF0007573000000022.tif20136
[0295] [Preparation of protective layer forming composition] Dipentaerythritol hexaacrylate (Aronix (registered trademark) M-403, manufactured by Toagosei Co., Ltd.) 50 parts, acrylate resin (Ebecryl 4858, manufactured by Daicel UCB Corporation) 50 parts, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Irgacure (registered trademark) 907, manufactured by Chiba Specialty Chemicals) 3 parts, and propylene glycol 1-monomethyl ether 2-acetate (PGMEA) 250 parts were mixed to obtain a protective layer forming composition (1).
[0296] [Production of the first retardation layer (1-1)] A cycloolefin polymer film (COP) (ZF-14, Zeon Corporation) was treated once using a corona treatment device (AGF-B10, Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The corona-treated surface was coated with a photoalignment film-forming composition (1) using a bar coater, dried at 80°C for 1 minute, and then irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7, Ushio Inc.). 2 The film thickness of the resulting alignment film was measured with a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 100 nm. Next, composition (A-1) was applied onto the alignment film using a bar coater and dried at 120°C for 1 minute, after which ultraviolet light was irradiated using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, integrated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to form a first retardation layer (1-1), and a retardation film (1) was obtained. The retardation values of the obtained retardation film (1) were measured, and found to be Re(550)=140 nm and Rth(550)=68 nm. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured, and found to be Re(450)=121 nm and Re(650)=145 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.86 Re(650) / Re(550)=1.04 That is, the first retardation layer (1-1) had optical properties represented by the following formulas (1), (2), and (4). Note that, since the retardation value of the COP at a wavelength of 550 nm is approximately 0, it does not affect the relationship of the in-plane retardation value. Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) 100nm <Re(550)<160nm (4)
[0297] [Production of the second retardation layer (2-1)] The surface of the COP was treated once using a corona treatment device under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. Orientable polymer composition (1) was applied to the corona-treated surface using a bar coater and dried at 90°C for 1 minute. The thickness of the resulting alignment film was measured using a laser microscope and found to be 34 nm. Next, composition (B-1) was applied onto the alignment film using a bar coater and dried at 90°C for 1 minute, after which ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-1), and a retardation film (2) was obtained. The thickness of the obtained second retardation layer (2-1) was measured by a laser microscope, and the thickness was 450 nm. In addition, the retardation value of the obtained retardation film (2) at a wavelength of 550 nm was measured, and the results were Re(550)=1 nm and Rth(550)=-70 nm. That is, the second retardation layer (2-1) had the optical characteristics represented by the following formula (3). Note that the retardation value of COP at a wavelength of 550 nm is approximately 0, so it does not affect the optical characteristics. n x ≒n y <n z (3)
[0298] [Production of Optical Film (1)] The COP surface of the retardation layer film (1) and the second retardation layer surface of the retardation layer film (2) were bonded with an adhesive to prepare an optical film (1). The retardation values of the obtained optical film (1) were measured to be Re(550)=140 nm and Rth(550)=2 nm. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured to be Re(450)=121 nm and Re(650)=145 nm. The relationship of the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.86 Re(650) / Re(550)=1.04 That is, the optical film (1) had the optical properties represented by the formulas (1), (2) and (4).
[0299] Example 2 [Manufacture of Layer A (A-1)] After subjecting the COP to a corona treatment, the treated surface was coated with oriented polymer composition (2) and dried by heating to obtain an oriented polymer film having a thickness of 82 nm. The surface of the obtained oriented polymer film was subjected to a rubbing treatment at an angle of 15° from the longitudinal direction of the COP, and composition (B-1) was coated thereon using a bar coater and dried at 100°C for 1 minute. After that, ultraviolet light was irradiated using a high-pressure mercury lamp (accumulated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 1200 mJ / cm2). 2 ) to form a layer A (A-1), and a retardation film (3) was obtained. The thickness of the obtained layer A (A-1) was measured with a laser microscope, and the thickness was 973 nm. The retardation value of the obtained retardation film (3) was measured, and Re(550)=135 nm, and the orientation angle was 15° with respect to the longitudinal direction of the COP. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured, and Re(450)=145 nm, Re(650)=132 nm. The relationship of the in-plane retardation value at each wavelength was as follows. Re(450) / Re(550)=1.07 Re(650) / Re(550)=0.98 That is, the layer A (A-1) had the optical properties represented by the following formulas (4), (6), and (7). 100nm <Re(550)<160nm (4) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7)
[0300] [Production of Layer B (B-1)] The COP was subjected to a corona treatment, and the oriented polymer composition (2) was applied thereon and dried by heating to obtain an oriented polymer film having a thickness of 80 nm. The surface of the obtained oriented polymer film was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the COP, and the composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute. After that, the film was irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2).2 ) to form layer B (B-1,) and obtain a retardation film (4). The thickness of the obtained layer B (B-1) was measured with a laser microscope and found to be 1.94 μm. The retardation value of the obtained retardation film (4) was measured to be Re(550)=269 nm, and the orientation angle was 75° with respect to the longitudinal direction of the COP. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured to be Re(450)=290 nm, Re(650)=265 nm. The relationship of the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=1.08 Re(650) / Re(550)=0.99 That is, the layer B (B-1) had the optical properties represented by the following formulas (5), (6), and (7). 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7)
[0301] [Production of Optical Film (2)] The COP surface of the retardation film (3) was bonded to the layer B (B-1) surface of the retardation film (4) with an adhesive, and the COP surface of the retardation film (4) was bonded to the second retardation layer (2-1) surface of the retardation film (2) with an adhesive to prepare an optical film (2). Therefore, the slow axis of the layer A (A-1) was 15° and the slow axis of the layer B (B-1) was 75° relative to the longitudinal direction of the COP. The retardation value of the optical film (2) was measured to be Re(550)=137nm, and the retardation values at wavelengths of 450nm and 650nm were measured to be Re(450)=100nm and Re(650)=160nm. The relationship of the in-plane retardation value at each wavelength was as follows: Re(450) / Re(550)=0.73 Re(650) / Re(550)=1.17 That is, the optical film (2) had the optical properties represented by the formulas (1), (2) and (4).
[0302] Example 3 [Production of optical film (3)] A first retardation layer was formed on the COP in the same manner as in the manufacture of the first retardation layer (1-1) in Example 1, to obtain a first retardation layer (1-2). Next, in the same manner as in the manufacture of the second retardation layer (2-1) in Example 1, an orientation polymer composition (1) was applied onto the first retardation layer (1-2) using a bar coater, and dried at 90°C for 1 minute to obtain an orientation film. Composition (B-1) was applied onto the obtained orientation film using a bar coater, and dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-2) on the first retardation layer (1-2), thereby obtaining an optical film (3). The retardation values of the obtained optical film (3) were measured to find that Re(450)=120 nm, Re(550)=139 nm, and Re(650)=146 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.87 Re(650) / Re(550)=1.05 That is, the optical film (3) had the optical properties represented by the formulas (1), (2) and (4).
[0303] Example 4 [Production of Optical Film (4)] A second retardation layer was formed on the COP in the same manner as in the manufacture of the second retardation layer (2-1) in Example 1, to obtain a second retardation layer (2-3). Next, an orientation polymer composition (2) was applied onto the second retardation layer (2-3) using a bar coater, and dried at 100°C for 1 minute. Subsequently, the orientation film was subjected to a rubbing treatment, and the composition (A-1) was applied onto the treated surface using a bar coater, and dried at 120°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a first retardation layer (1-3) on the second retardation layer (2-3), thereby obtaining an optical film (4). The retardation values of the obtained optical film (3) were measured to find that Re(450)=121 nm, Re(550)=139 nm, and Re(650)=146 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.87 Re(650) / Re(550)=1.05 That is, the optical film (4) had the optical properties represented by the formulas (1), (2) and (4).
[0304] Example 5 [Production of optical film (5)] A retardation layer was formed on the COP treated with a corona treatment device in the same manner as in the production of layer A (A-1) in Example 2, to obtain a first retardation layer (1-4). The slow axis of the first retardation layer (1-4) was at an angle of 15° to the longitudinal direction of the COP. Next, an orientation polymer composition (1) was applied onto the obtained first retardation layer (1-4) using a bar coater, and dried at 90°C for 1 minute to obtain an orientation film. Composition (B-1) was applied onto the obtained orientation film using a bar coater, and dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-4) on the first retardation layer (1-4). Subsequently, the second retardation layer (2-4) was subjected to a corona treatment, and then an alignment polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute. The surface of the dried alignment polymer was subjected to a rubbing treatment at an angle of 75° with respect to the longitudinal direction of the COP to obtain an alignment film. The composition (B-1) was applied on the obtained alignment film using a bar coater and dried at 100°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2) to form a third retardation layer (3-1). Therefore, the slow axis of the first retardation layer (1-3) was 15° and the slow axis of the third retardation layer (3-1) was 75° relative to the longitudinal direction of the COP, and an optical film (5) was obtained in which the COP, the first retardation layer (1-4), the second retardation layer (2-4), and the third retardation layer (3-1) were laminated in this order. The retardation values of the obtained optical film (5) were measured to find that Re(450)=101 nm, Re(550)=138 nm, and Re(650)=160 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.73 Re(650) / Re(550)=1.16 That is, the optical film (3) had the optical properties represented by the formulas (1), (2) and (4).
[0305] Example 6 [Production of optical film (6)] A second retardation layer was formed on the COP in the same manner as in the production of the second retardation layer (2-1) in Example 1, to obtain a second retardation layer (2-5). After the surface of the obtained second retardation layer (2-5) was corona-treated, an orientation polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute. The surface of the dried orientation polymer was subjected to rubbing treatment at an angle of 15° from the longitudinal direction of the COP, and a composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer A (A-2). The surface of the obtained layer A (A-2) was subjected to a corona treatment, and then oriented polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute. The surface of the dried oriented polymer was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the long film, and composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute. After that, ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2) to form layer B (B-2), thereby obtaining an optical film (6). Optical film (6), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0306] Example 7 [Production of Optical Film (7)] Layer A was formed on the COP in the same manner as in the production of layer A (A-1) in Example 2, to obtain layer A (A-3). The surface of the obtained layer A (A-3) was subjected to a corona treatment, and then oriented polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute. The surface of the dried oriented polymer was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the COP, and composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (accumulated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 1200 mJ / cm2). 2 ) to form layer B (B-3). After corona treatment of the surface of the obtained layer B (B-3), the oriented polymer composition (1) was applied using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-6) on the layer B (B-3), and thus an optical film (7) was formed. The retardation values of the obtained optical film (7) were measured, and found to be Re(450)=100 nm, Re(550)=138 nm, and Re(650)=159 nm. The relationship of the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.72 Re(650) / Re(550)=1.15 That is, the optical film (3) had the optical properties represented by the formulas (1), (2) and (4).
[0307] Example 8 [Production of Optical Film (8)] An optical film (8) was produced in the same manner as in Example 3, except that a protective layer (1) was formed between the first retardation layer (1-2) and the alignment film. The protective layer (1) was formed by subjecting the first retardation layer (1-2) to a corona treatment, applying a composition for forming a protective layer thereon using a bar coater, drying the composition at 90° C. for 1 minute, and irradiating the composition with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 500 mJ / cm ). 2 ) and polymerization was carried out to form the film. The retardation values of the obtained optical film (8) were measured, and found to be Re(450) = 120 nm, Re(550) = 139 nm, and Re(650) = 144 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.86 Re(650) / Re(550)=1.04 That is, the optical film (8) had the optical properties represented by the formulas (1), (2) and (4).
[0308] Example 9 [Production of Optical Film (9)] Layer A was formed on the corona-treated COP in the same manner as in the production of layer A (A-1) in Example 2, to obtain layer A (A-4). Next, layer A (A-4) was subjected to corona treatment, and then a composition for forming a protective layer was applied thereon using a bar coater, dried at 90°C for 1 minute, and irradiated with ultraviolet light using a high-pressure mercury lamp (integrated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 500 mJ / cm2). 2 ) to form a protective layer (2). On the obtained protective layer (2), a layer B (B-4) was formed in the same manner as in Example 2, and the second retardation layer (2-1) surface of the retardation film (2) was attached thereon with an adhesive to obtain an optical film (9). Optical film (9), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0309] Example 10 [Production of optical film (10)] An optical film (10) was produced in the same manner as in Example 5, except that a protective layer (3) was formed between the second retardation layer (2-4) and the alignment film (1). The protective layer (3) was formed by applying a composition for forming a protective layer onto the second retardation layer (2-3) using a bar coater, drying the composition at 90° C. for 1 minute, and irradiating the composition with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 500 mJ / cm ). 2 The alignment film (1) was obtained by subjecting the protective layer (3) to a corona treatment, applying the alignment polymer composition (2) thereon using a bar coater, drying at 100°C for 1 minute, and subjecting the surface of the resulting alignment polymer film to a rubbing treatment at an angle of 75° from the longitudinal direction of the COP. Optical film (10), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0310] Example 11 [Production of Optical Film (11)] A first retardation layer (1-5) was formed on a COP in the same manner as the first retardation layer (1-1) in Example 1. The surface of the COP opposite to the surface on which the first retardation layer (1-5) was formed was subjected to corona treatment, and the composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-6), and an optical film (11) having the first retardation layer (1-5), the substrate, and the second retardation layer (2-6) in this order was obtained. The retardation values of the obtained optical film (11) were measured to find that Re(450)=120 nm, Re(550)=139 nm, and Re(650)=146 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.86 Re(650) / Re(550)=1.05 That is, the optical film (11) had the optical properties represented by the formulas (1), (2) and (4).
[0311] Example 12 [Production of optical film (12)] After subjecting the COP to a corona treatment, the composition for forming a photoalignment film (1) was applied with a bar coater, dried at 80°C for 1 minute, and irradiated with 100 mJ / cm using a polarized UV irradiation device. 2 The polarized UV exposure was performed with an integrated light amount of 1200 mJ / cm2. The polarized UV treatment was performed with linearly polarized light at an angle of 75° from the longitudinal direction of the COP. Composition (B-1) was applied to the surface that had been treated with polarized UV using a bar coater, and dried at 100°C for 1 minute. After that, ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer B (B-5). The slow axis direction of layer B (B-5) was 75° to the longitudinal direction of the COP. Next, layer B (B-5) was corona treated, and then oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was rubbed at an angle of 15° from the longitudinal direction of the COP to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 100°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer A (A-5). Subsequently, layer A (A-5) was subjected to a corona treatment, and then an oriented polymer composition (1) was applied thereto using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-7) on the layer A (A-5), and an optical film (12) was obtained. The retardation values of the obtained optical film (12) were measured, and found to be Re(450)=100 nm, Re(550)=138 nm, and Re(650)=160 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.72 Re(650) / Re(550)=1.16 That is, the optical film (12) had the optical properties represented by the formulas (1), (2), and (4).
[0312] Example 13 [Production of optical film (13)] The alignment polymer composition (1) was applied to a saponified triacetyl cellulose film (TAC) (KC4UY, manufactured by Konica Minolta, Inc.) using a bar coater and dried at 90°C for 1 minute to obtain an alignment film. Composition (B-1) was applied to the obtained alignment film using a bar coater and dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (integrated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-8). The obtained second retardation layer (2-8) was corona treated, and an oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was rubbed at an angle of 75° from the longitudinal direction of the TAC, and composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2) to form layer B (B-6). The obtained layer B (B-6) was corona treated, and oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was rubbed at an angle of 15° from the longitudinal direction of the TAC, and composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form a layer A (A-6), and an optical film (13) was obtained. Optical film (13), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0313] Example 14 [Production of optical film (14)] Similarly to Example 5, a layer A (A-7) was formed on the COP. The slow axis of the layer A was 15° to the longitudinal direction of the film. Next, the surface of the layer A (A-7) was corona treated, and then the oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the long film, and the composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer B (B-7). Next, the surface of the COP opposite to the surface on which layer A (A-7) and layer B (B-7) were formed was subjected to a corona treatment, and then orientable polymer composition (1) was applied thereto using a bar coater and dried at 90°C for 1 minute to obtain an alignment film. Composition (B-1) was applied onto the resulting alignment film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-9) on the COP, and thus an optical film (14) was formed. The retardation values of the obtained optical film (14) were measured, and found to be Re(450)=101 nm, Re(550)=138 nm, and Re(650)=160 nm. The relationship of the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.73 Re(650) / Re(550)=1.16 That is, the optical film (14) had the optical properties represented by the formulas (1), (2) and (4).
[0314] Example 15 [Production of optical film (15)] Similarly to Example 12, a layer B (B-8) was formed on the COP. The slow axis of the layer B (B-8) was 75° to the longitudinal direction of the film. Next, the surface of the layer B (B-8) was corona treated, and then the oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was subjected to a rubbing treatment at an angle of 15° from the longitudinal direction of the long film, and the composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer A (A-8). Next, a corona treatment was performed on the COP surface opposite to the surface on which layer A (A-8) and layer B (B-8) were formed, and then an oriented polymer composition (1) was applied using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-10) on the TAC, and thus an optical film (15) was formed. The retardation values of the obtained optical film (15) were measured, and found to be Re(450)=101 nm, Re(550)=138 nm, and Re(650)=160 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.73 Re(650) / Re(550)=1.16 That is, the optical film (15) had the optical properties represented by the formulas (1), (2), and (4).
[0315] Example 16 [Production of optical film (16)] The oriented polymer composition (2) was applied onto the TAC using a bar coater and dried at 100° C. for 1 minute. The surface of the oriented polymer was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the long film, and the composition (B-1) was applied thereon using a bar coater and dried at 100° C. for 1 minute, after which ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm 2 ). 2 ) to form layer B (B-9). Next, the surface of layer B (B-9) was corona-treated, and then an oriented polymer composition (1) was applied thereto using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-11) on layer B (B-9). Next, the second retardation layer (2-11) was corona-treated, and then an orientation polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an orientation polymer film. The surface of the orientation polymer film was rubbed at an angle of 15° from the longitudinal direction of the long film, and composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer A (A-9), and an optical film (16) was obtained. Optical film (16), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0316] Example 17 [Production of optical film (17)] In the same manner as in Example 2, a layer B (B-10) was formed on a COP. The surface opposite to the surface on which the layer B (B-10) was formed was subjected to a corona treatment, and then an oriented polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was subjected to a rubbing treatment at an angle of 15° from the longitudinal direction of the long film, and then a composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (accumulated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 1200 mJ / cm2). 2 ) to form layer A (A-10). Next, the surface of layer A (A-10) was corona-treated, and then an oriented polymer composition (1) was applied thereto using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-12) on the layer A (A-10), thereby obtaining an optical film (17). Optical film (17), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0317] Example 18 [Production of optical film (18)] In the same manner as in Example 2, a layer B (B-11) was formed on a COP. The surface opposite to the surface on which the layer B (B-11) was formed was subjected to a corona treatment, and then an oriented polymer composition (1) was applied thereon using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied on the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-13) on the COP. Next, the second retardation layer surface was corona-treated, and then an oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was rubbed at an angle of 15° from the longitudinal direction of the long film, and then composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form a layer A (A-11), and an optical film (18) was obtained. Optical film (18), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0318] Example 19 [Production of optical film (19)] In the same manner as in Example 2, a layer A (A-12) was formed on a COP. The surface opposite to the surface on which the layer A (A-12) was formed was subjected to a corona treatment, and then an oriented polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the long film, and then a composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer B (B-12). Next, the surface of layer B (B-12) was corona-treated, and then an oriented polymer composition (1) was applied thereto using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied onto the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-14) on the layer B (B-12), thereby obtaining an optical film (19). Optical film (19), which has a structure similar to that of optical film (1) or optical film (2), has the optical properties represented by formulas (1), (2) and (4) similar to those of optical film (1) and optical film (2).
[0319] Example 20 [Production of optical film (20)] In the same manner as in Example 2, a layer A (A-13) was formed on a COP. The surface opposite to the surface on which the layer A (A-13) was formed was subjected to a corona treatment, and then an oriented polymer composition (1) was applied thereon using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. Composition (B-1) was applied on the obtained oriented film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2) to form a second retardation layer (2-15) on the COP. Next, the surface of the second retardation layer (2-15) was corona-treated, and then an oriented polymer composition (2) was applied using a bar coater and dried at 100°C for 1 minute to obtain an oriented polymer film. The surface of the oriented polymer film was rubbed at an angle of 75° from the longitudinal direction of the long film, and then composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer B (B-13), and an optical film (20) was obtained. Optical film (20) having the same configuration as optical film (1) or optical film (2) has the optical properties represented by formulas (1), (2) and (4) like optical film (1) and optical film (2).
[0320] Example 21 [Production of Optical Film (21)] In Example 1, PureAce (registered trademark) WR-S (manufactured by Teijin Limited) was used as the first retardation layer, and the second retardation layer (2-1) was formed on the retardation film (2) and bonded to the liquid crystal surface of the retardation film (2) with an adhesive to obtain an optical film (21). The retardation values of the obtained optical film (21) were measured at wavelengths of 450 nm, 550 nm, and 650 nm, and the results were Re(450) = 127 nm, Re(550) = 142 nm, Re(650) = 145 nm, Rth(450) = -18.5 nm, Rth(550) = -3.7 nm, Rth(650) = 4.1 nm, |Rth(450) / Re(450)| = 0.145, |Rth(550) / Re(550)| = 0.026, |Rth(650) / Re(650)| = 0.028. The relationship of the in-plane retardation values at each wavelength was as follows. Re(450) / Re(550)=0.89 Re(650) / Re(550)=1.02 That is, the optical film (21) had the optical properties represented by the formulas (1), (2), and (4).
[0321] Example 22 [Manufacturing of polarizers] A polyvinyl alcohol film having an average degree of polymerization of about 2,400, a degree of saponification of 99.9 mol% or more, and a thickness of 75 μm was immersed in pure water at 30° C., and then immersed in an aqueous solution having a weight ratio of iodine / potassium iodide / water of 0.02 / 2 / 100 at 30° C. to perform iodine dyeing (iodine dyeing step). The polyvinyl alcohol film that had undergone the iodine dyeing step was immersed in an aqueous solution having a weight ratio of potassium iodide / boric acid / water of 12 / 5 / 100 at 56.5° C. to perform boric acid treatment (boric acid treatment step). The polyvinyl alcohol film that had undergone the iodine dyeing step and the subsequent boric acid treatment step was washed with pure water at 8° C., and then dried at 65° C. to obtain a polarizer (thickness 27 μm after stretching) in which iodine was adsorbed and aligned in the polyvinyl alcohol. At this time, stretching was performed in the iodine dyeing step and the boric acid treatment step. The total stretching ratio in this stretching was 5.3 times. The obtained polarizer and a saponified triacetyl cellulose film (KC4UYTAC 40 μm, manufactured by Konica Minolta) were bonded together by nip rolls via a water-based adhesive. The laminate was dried at 60° C. for 2 minutes while maintaining a tension of 430 N / m to obtain a polarizing plate (1) having a triacetyl cellulose film as a protective film on one side. The water-based adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318, manufactured by Kuraray) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650, manufactured by Sumika Chemtex, aqueous solution with a solid content of 30%) to 100 parts of water.
[0322] [Production of UV-curable adhesive composition] The following components were mixed to prepare an ultraviolet-curable adhesive composition. 3,4-Epoxycyclohexylmethyl 3,4-Epoxycyclohexane carboxylate 40 parts Diglycidyl ether of bisphenol A 60 parts Diphenyl(4-phenylthiophenyl)sulfonium Hexafluoroantimonate (photocationic polymerization initiator) 4 parts
[0323] [Manufacture of circularly polarizing plate (1)] The surface of the first retardation layer of the optical film (1) produced in Example 1 was subjected to a corona treatment, coated with an ultraviolet-curable adhesive composition, and then superimposed on the polarizer surface of the polarizing plate (1), and integrated by passing through two laminating rolls. Here, the angle between the absorption axis of the polarizer (1) and the slow axis of the first retardation layer (1-1) was set to 45°. Of the two laminating rolls, a rubber roll with a rubber surface was used as the first laminating roll, and a metal roll with a chrome-plated surface was used as the second laminating roll. After lamination, an ultraviolet irradiation device using a metal halide lamp as a light source was used, and an integrated light amount at a wavelength of 320 to 400 nm was 20 mJ / cm. 2 The optical film (1) was irradiated with ultraviolet light from the COP surface side to cure the adhesive, and then attached to a polarizer to obtain a circularly polarizing plate (1).
[0324] Example 23 [Circular polarizing plate (4) manufacturing] In the same manner as in Example 22, the first retardation layer surface of the optical film (4) produced in Example 4 was subjected to a corona treatment, and then a polarizing plate (1) was attached thereto using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (4). In this case, ultraviolet irradiation was performed from the COP surface side of the optical film (4), and the polarizing plate (1) was attached so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the first retardation layer was 45°.
[0325] Example 24 [Production of circularly polarizing plates (3) and (8)] As in Example 22, the second retardation layer surfaces of the optical films (3) and (8) obtained in Examples 3 and 8 were subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain circular polarizing plates (3) and (8). In this case, ultraviolet irradiation was performed from the COP side of the optical film (3) or (8), and the polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the first retardation layer was 45°.
[0326] Example 25 [Production of circularly polarizing plate (11)] In the same manner as in Example 22, the second retardation layer surface of the optical film (11) obtained in Example 11 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (11). In this case, ultraviolet irradiation was performed from the first retardation layer side of the optical film (11), and the polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the first retardation layer was 45°.
[0327] Example 26 [Production of circularly polarizing plate (21)] As in Example 22, the COP surface of the optical film (21) obtained in Example 21 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (21). In this case, ultraviolet irradiation was performed from the first retardation layer side of the optical film (21), and the polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the first retardation layer was 45°.
[0328] Example 27 [Manufacture of circularly polarizing plate (2)] As in Example 22, the COP surface of the optical film (2) obtained in Example 2 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (2). In this case, ultraviolet irradiation was performed from the layer A side of the optical film (2), and the circular polarizing plate (2) was laminated in the order of polarizer, second retardation layer, layer B, and layer A, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer A was 15°.
[0329] Example 28 [Manufacture of circularly polarizing plate (9)] As in Example 22, the COP surface of the optical film (9) obtained in Example 9 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (9). In this case, the circular polarizing plate (9) was laminated in the order of the polarizer, the second retardation layer, the layer B, and the layer A, and ultraviolet irradiation was performed from the COP side closer to the layer A. The polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer A was 15°.
[0330] Example 29 [Production of circularly polarizing plates (5), (6), and (10)] As in Example 22, the layer B surface of the optical films (5), (6) and (10) obtained in Examples 5, 6 and 10 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain circular polarizing plates (5), (6) and (10). In this case, ultraviolet irradiation was performed from the COP side of the optical film (5), (6) or (10), and the circular polarizing plate was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B and layer A. In addition, the polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 15°.
[0331] Example 30 [Manufacture of circularly polarizing plate (7)] As in Example 22, the second retardation layer surface of the optical film (7) obtained in Example 7 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (7). In this case, ultraviolet irradiation was performed from the COP side, and the circular polarizing plate (7) was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer A was 15°.
[0332] Example 31 [Production of circularly polarizing plates (15) and (19)] As in Example 22, the second retardation layer surface of the optical films (15) and (19) obtained in Examples 15 and 19 was subjected to a corona treatment, and then a polarizer was attached thereon using an ultraviolet-curable adhesive composition to obtain circular polarizing plates (15) and (19). In this case, ultraviolet irradiation was performed from the layer A side of the optical films (15) and (19), and the circular polarizing plates were laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate (1) was attached so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75° and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 15°.
[0333] Example 32 [Production of circularly polarizing plate (12)] As in Example 22, the COP surface of the optical film (12) obtained in Example 12 was subjected to a corona treatment, and then a polarizing plate (1) was laminated thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (12). In this case, ultraviolet irradiation was performed from the second retardation layer side of the optical film (12), and the circular polarizing plate (12) was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate (1) was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of layer A was 15°.
[0334] Example 33 [Production of circularly polarizing plates (14) and (17)] As in Example 22, the layer B surface of the optical films (14) and (17) obtained in Examples 14 and 17 was subjected to a corona treatment, and then a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain circular polarizing plates (14) and (17). In this case, ultraviolet irradiation was performed from the second retardation layer side of the optical film (14) or (17), and the circular polarizing plate was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate (1) was attached so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75° and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer A was 15°.
[0335] Example 34 [Production of circularly polarizing plates (18) and (20)] As in Example 22, the layer B surfaces of the optical films (18) and (20) obtained in Examples 18 and 20 were subjected to a corona treatment, and then a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain circular polarizing plates (18) and (20). In this case, ultraviolet irradiation was performed from the layer A side of the optical film (18), and the circular polarizing plate was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate (1) was attached so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75° and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer A was 15°.
[0336] Example 35 [Production of circularly polarizing plates (13) and (16)] The TAC surfaces of the optical films (13) and (16) obtained in Examples 13 and 16 were subjected to a corona treatment, and then the polarizing plate (1) was laminated thereon using the same aqueous adhesive as that used in the production of the polarizing plate (1) to obtain the circular polarizing plates (13) and (16). In this case, the circular polarizing plate was laminated so that the layers other than the second retardation layer were in the order of polarizer, layer B, and layer A. The polarizing plate was laminated so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer B was 75°, and the angle between the absorption axis of the polarizing plate (1) and the slow axis of the layer A was 15°.
[0337] Reference example 1 [Manufacturing of circular polarizing plate (Reference 1)] The COP surface of the retardation film (1) prepared in Example 1 was subjected to a corona treatment, and then a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain a circular polarizing plate (Reference 1). At this time, the polarizing plate (1) was attached so that the angle between the absorption axis of the polarizing plate (1) and the slow axis of the retardation film (1) was 45°.
[0338] Reference example 2 [Manufacturing of circular polarizing plate (Reference 2)] In the same manner as in the production of layer A (A-1) in Example 2, layer A was formed on the COP to obtain layer A (A-14). The layer A (A-14) had a slow axis at an angle of 15° from the longitudinal direction of the COP. The surface of the obtained layer A (A-14) was corona-treated, and then an orientation polymer composition (1) was applied thereon using a bar coater and dried at 90°C for 1 minute to form an orientation film. Composition (B-1) was applied on the obtained orientation film using a bar coater and dried at 90°C for 1 minute, and then ultraviolet light was irradiated using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-16). Next, the surface of the COP opposite to the surface on which the layer A (A-14) was formed was corona-treated, and a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain a circularly polarizing plate (Reference 2).
[0339] Reference example 3 [Manufacturing of circular polarizing plate (Reference 3)] In the same manner as in the production of layer B (B-1) in Example 2, layer B was formed on the COP to obtain layer B (B-14). The layer B (B-14) had a slow axis at an angle of 75° from the longitudinal direction of the COP. The surface of the obtained layer B (B-14) was corona-treated, and then the orientable polymer composition (1) was applied thereon using a bar coater and dried at 90°C for 1 minute to form an alignment film. The obtained alignment film was then coated with composition (B-1) using a bar coater and dried at 90°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light amount at a wavelength of 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-17). Next, the surface of the COP opposite to the surface on which the layer B (B-14) was formed was subjected to a corona treatment, and then a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain a circularly polarizing plate (Reference 3).
[0340] Reference example 4 [Manufacture of circular polarizing plate (Reference 4)] Layer A was formed on the COP in the same manner as in the production of layer A (A-1) in Example 7, to obtain layer A (A-15). The layer A (A-15) had a slow axis at an angle of 15° from the longitudinal direction of the COP. The surface of the obtained layer A (A-15) was subjected to a corona treatment, and then an oriented polymer composition (2) was applied thereon using a bar coater and dried at 100°C for 1 minute. The surface of the dried oriented polymer was subjected to a rubbing treatment at an angle of 75° from the longitudinal direction of the COP, and then composition (B-1) was applied thereon using a bar coater and dried at 100°C for 1 minute, followed by irradiation with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 1200 mJ / cm2). 2 ) to form layer B (B-15). Next, the surface of the COP opposite to the surface on which layer A (A-15) was formed was subjected to corona treatment, and then a polarizing plate (1) was attached thereon using an ultraviolet-curable adhesive composition to obtain a circularly polarizing plate (Reference 4).
[0341] The surface opposite to the polarizing plate (1) of each of the circular polarizing plates (1) to (21) obtained in Examples 22 to 35 and the circular polarizing plates (Reference 1) to (Reference 4) obtained in Reference Examples 1 to 4 was attached to a mirror using a pressure-sensitive adhesive. The attached circular polarizing plate was observed from all azimuth angles at a position at an elevation angle of 60° from the front vertical direction. The colors when viewed from two directions where the hue change was particularly large are shown in Table 3. All of the circular polarizing plates (1) to (21) were not colored regardless of the direction from which they were observed, and good black display was obtained.
[0342] [Table 3]
[0343] The above measurement results demonstrate that the circularly polarizing plates of the examples have excellent anti-reflection properties in bright places when observed from all directions, and are therefore useful.
[0344] Example 36 [Preparation of Oriented Polymer Composition (3)] The composition of the oriented polymer composition is shown in Table 1. N-methyl-2-pyrrolidone, 2-butoxyethanol and ethylcyclohexane were added to Sunever SE-610 (Nissan Chemical Industries, Ltd.), a commercially available oriented polymer, to obtain oriented polymer composition (3).
[0345] [Table 4] The values in Table 4 represent the content ratio of each component relative to the total amount of the prepared composition. For SE-610, the solid content was calculated from the concentration listed on the delivery specification.
[0346] The surface of a cycloolefin polymer film (COP) (ZF-14, Zeon Corporation) was treated once using a corona treatment device (AGF-B10, Kasuga Electric Co., Ltd.) under the conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The surface that had been subjected to the corona treatment was coated with an oriented polymer composition (3) using a bar coater and dried at 90°C for 1 minute. The thickness of the obtained oriented film was measured with a laser microscope (LEXT, Olympus Corporation) and found to be 34 nm. Next, the oriented film was coated with a composition (B-1) using a bar coater and dried at 90°C for 1 minute, and then irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm) using a high-pressure mercury lamp (Uniqure VB-15201BY-A, Ushio Electric Co., Ltd.). 2 ) to form a second retardation layer (2-1-01), and a retardation film (1-01) was obtained. The thickness of the obtained second retardation layer (2-1-01) was measured with a laser microscope, and the thickness was 450 nm. In addition, the retardation value of the obtained retardation film (1-01) at a wavelength of 550 nm was measured, and the results were Re(550)=1 nm and Rth(550)=-70 nm. That is, the second retardation layer (2-1-01) has the optical characteristic represented by the following formula (3). Note that the retardation value of the COP at a wavelength of 550 nm is approximately 0, so it does not affect the optical characteristic. n x ≒n y <nz (3)
[0347] Furthermore, the back surface of the cycloolefin polymer film on which the second retardation layer (2-1-01) was formed was treated once using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The corona-treated surface was coated with a photoalignment film-forming composition (1) using a bar coater, dried at 80°C for 1 minute, and irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7, manufactured by Ushio Inc.). 2 The film thickness of the resulting alignment film was measured with a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 100 nm. Next, composition (A-1) was applied onto the alignment film using a bar coater and dried at 120°C for 1 minute, after which ultraviolet light was irradiated using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, integrated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to form a first retardation layer (1-1-01), and an optical film (1-01) was obtained. The thickness of the obtained first retardation layer (1-1-01) was measured with a laser microscope, and the thickness was 2.2 μm. The retardation values of this optical film (1-01) were also measured, and Re(550)=140 nm, Rth(550)=2 nm. The retardation values at wavelengths of 450 nm and 650 nm were also measured, and Re(450)=121 nm, Re(650)=145 nm.
[0348] Example 37 A first retardation layer (1-2-01) was formed on a cycloolefin polymer film in the same manner as in the formation method of the first retardation layer in Example 36 to obtain a retardation film (2-01). The retardation value of the obtained retardation film (2-01) was measured, and it was found to be Re(550)=140 nm and Rth(550)=68 nm. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured, and it was found to be Re(450)=121 nm and Re(650)=145 nm. Since the thickness d was constant, the relationship of the birefringence at each wavelength was as follows. Re(450) / Re(550)=Δn(450) / Δn(550)=0.87 Re(650) / Re(550)=Δn(650) / Δn(550)=1.04 That is, the first retardation layer (1-2-01) has optical properties expressed by the following formulas (1) and (2). Note that, since the retardation value of the COP at a wavelength of 550 nm is approximately 0, it does not affect the birefringence relationship. Δn(450) / Δn(550)≦1.00 (1) 1.00≦Δn(650) / Δn(550) (2)
[0349] Further, a second retardation layer (2-2-01) was formed on the back surface of the cycloolefin polymer film on which the first retardation layer (1-2-01) was formed, in the same manner as in Example 1, to obtain an optical film (2-01). The retardation value of the obtained optical film (2-01) was measured, and it was found to be Re(550)=140 nm and Rth(550)=4 nm. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured, and it was found to be Re(450)=121 nm and Re(650)=145 nm.
[0350] Example 38 A second retardation layer (2-3-01) was formed on a cycloolefin polymer film in the same manner as in the method for forming the second retardation layer in Example 36 to obtain a retardation film (3-01). A composition for forming a protective layer was applied onto the obtained second retardation layer using a bar coater and dried at 90°C for 1 minute. Furthermore, ultraviolet light was irradiated (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm2) using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.). 2 ) to form a protective layer (1-01) and obtain a retardation film (3-2-01). The total thickness of the obtained second retardation layer (2-3-01) and protective layer (1-01) was measured with a laser microscope, and the thickness was 2.5 μm. The retardation value of the retardation film (3-2-01) at a wavelength of 550 nm was measured, and the results were Re(550)=2 nm and Rth(550)=-66 nm. That is, the second retardation layer (2-3-01) has the optical characteristic represented by the following formula (3). Note that the retardation value of the COP and protective layer (1) at a wavelength of 550 nm is approximately 0, so there is no effect on the optical characteristic. n x ≒n y <n z (3)
[0351] Further, a first retardation layer (1-3-01) was formed on the protective film (1-01) in the same manner as in Example 36 to obtain an optical film (3-01). The retardation values of the obtained optical film (3-01) were measured to find that Re(550)=138 nm and Rth(550)=2 nm. In addition, the retardation values at wavelengths of 450 nm and 650 nm were measured to find that Re(450)=118 nm and Re(650)=144 nm.
[0352] Example 39 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the second retardation layer (2-1-01) surface of the optical film (1-01) obtained in Example 36 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-1-01) was 45°, thereby obtaining a circular polarizing plate (1-01).
[0353] Example 40 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the first retardation layer (1-1-01) surface of the optical film (1-01) obtained in Example 36 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-1-01) was 45°, thereby obtaining a circular polarizing plate (2-01).
[0354] Example 41 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the cycloolefin polymer film surface of the optical film (2-01) obtained in Example 37 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-2-01) was 45°, thereby obtaining a circularly polarizing plate (3-01).
[0355] Example 42 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the second retardation layer (2-2-01) surface of the optical film (2-01) obtained in Example 37 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-2-01) was 45°, thereby obtaining a circularly polarizing plate (4-01).
[0356] Example 43 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the cycloolefin polymer film surface of the optical film (3-01) obtained in Example 38 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-3-01) was 45°, thereby obtaining a circularly polarizing plate (5-01).
[0357] Example 44 An iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical) was attached to the first retardation layer (1-3-01) surface of the optical film (3-01) obtained in Example 38 using a pressure-sensitive adhesive so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (1-3-01) was 45°, thereby obtaining a circular polarizing plate (6-01).
[0358] The surface opposite to the polarizing plate of each of the circular polarizing plates (1-01) to (6-01) obtained in Examples 39 to 44 was attached to a mirror using a pressure-sensitive adhesive, and the plate was observed from the slow axis direction and the fast axis direction of the first retardation layer at an elevation angle of 60° from the front vertical direction to evaluate the optical compensation characteristics. The results are shown in Table 3. None of the circular polarizing plates were colored when observed from any direction, and a good black display was obtained. Note that Reference Example 5 shows a circular polarizing plate (7-01) formed with only the same first retardation layer as in Example 36.
[0359] [Table 5]
[0360] For the samples in which the circular polarizing plates of Reference Example 5 and Example 39 were attached to a mirror, the chromaticity coordinates (x, y) were measured using a luminance meter from an elevation angle of 60°. Note that a high color rendering CCFL light source (x, y) = (0.3494, 0.3600) was used as the light source.
[0361] Hue of the circularly polarizing plate (7-01) of Reference Example 5: In the slow axis direction (+45° to the polarizer absorption axis) it is (0.3292, 0.3569) In the direction of the slow axis (-45° to the absorption axis of the polarizer), it is (0.3282, 0.3561) (0.3651, 0.3634) in the fast axis direction (+45° to the polarizer absorption axis) In the fast axis direction (-45° to the absorption axis of the polarizer), it is (0.3641, 0.3626)
[0362] Hue of the circularly polarizing plate (1-01) of Example 39: In the slow axis direction (+45° to the polarizer absorption axis) it is (0.3457, 0.3548) Slow axis direction (-45° to the absorption axis of the polarizer) is (0.3475, 0.3533) (0.3445, 0.3557) in the fast axis direction (+45° to the polarizer absorption axis) (0.3626, 0.3543) in the fast axis direction (-45° to the absorption axis of the polarizer)
[0363] It can also be seen from the above measurement results that the circularly polarizing plate (1-01) of Example 39 has a small deviation in hue from the light source and has improved optical compensation characteristics.
[0364] Example 45 [Manufacture of circular polarizing plate (8-01)]
[0365] [Preparation of composition (C-1)] The following components were mixed and the resulting mixture was stirred at 80° C. for 1 hour to obtain composition (C-1).
[0366] The polymerizable liquid crystal A3 was synthesized by the method described in JP-A-2010-24438. Polymerizable liquid crystal A1 (86 parts): TIFF0007573000000026.tif39132
[0367] Polymerizable liquid crystal A3 (14 parts): TIFF0007573000000027.tif32107
[0368] Polymerization initiator (6 parts): 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals) Leveling agent (0.1 part): Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) Antioxidant (part 1): Dibutylhydroxytoluene (manufactured by Wako Pure Chemical Industries, Ltd.) Solvent: N-methyl-2-pyrrolidinone (160 parts), cyclopentanone (240 parts)
[0369] [Preparation of Oriented Polymer Composition (4)] The composition of the oriented polymer composition is shown in Table 1. N-methyl-2-pyrrolidone, 2-butoxyethanol and propylene glycol 1-monomethyl ether 2-acetate (PGMEA) were added to Sunever SE-610 (Nissan Chemical Industries, Ltd.), a commercially available oriented polymer, to obtain oriented polymer composition (3).
[0370] [Table 6]
[0371] [Manufacture of the first retardation layer (2-4-01)] The photoalignment film-forming composition (1) was applied to the surface of a polyethylene terephthalate film (Diafoil T140E25, manufactured by Mitsubishi Plastics, Inc.), dried at 80°C for 1 minute, and then irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7, manufactured by Ushio Inc.). 2 The resulting photo-alignment film had a thickness of 100 nm. Next, the composition (C-1) was applied onto the photo-alignment film using a bar coater and dried at 120°C for 1 minute. After that, ultraviolet light was irradiated using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to form a first retardation layer (2-4-01). A film (2-4-10) having a polyethylene terephthalate film and a first retardation layer (2-4-01) was obtained.
[0372] The surface of the obtained first retardation layer (2-4-01) was subjected to a corona treatment, and then a UV-curable adhesive composition was applied thereto by a bar coating method. Then, a COP film whose surface had been corona-treated was pressed onto the adhesive surface, and an exposure dose of 1000 mJ / cm was applied from the COP film side using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2The film was cured by irradiating ultraviolet light (365 nm standard). The first retardation layer (2-4-01) was transferred onto the COP film, and the polyethylene terephthalate was removed to obtain a COP film (2-4-02) having a first retardation layer. The thickness of the first retardation layer including the adhesive layer was 4.7 μm.
[0373] The retardation values of the COP film (2-4-02) having the first retardation layer were measured, and the results were Re(450)=119 nm, Re(550)=137 nm, and Re(650)=141 nm. The relationship between the in-plane retardation values at each wavelength was as follows: Re(450) / Re(550)=0.87 Re(650) / Re(550)=1.03 That is, the first retardation layer (2-4-01) had the optical properties represented by the following formulas (1), (2), and (4). Note that the retardation value of the COP at a wavelength of 550 nm is approximately 0, so there is no effect on the relationship of the in-plane retardation value. Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) 100nm <Re(550)<160nm (4)
[0374] [Manufacture of the second retardation layer (2-4-03)] The oriented polymer composition (4) was applied to the surface of a polyethylene terephthalate film (Diafoil T140E25, manufactured by Mitsubishi Plastics, Inc.) by bar coating, and the film was dried by heating in an oven at 90°C for 1 minute to form an oriented film. Next, the composition (B-1) was applied onto the oriented film using a bar coater, and the film was dried at 90°C for 1 minute, after which ultraviolet light was irradiated using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to form a second retardation layer (2-4-03).
[0375] The surface of the obtained second retardation layer (2-4-03) was subjected to a corona treatment, and then a UV-curable adhesive composition was applied thereto by a bar coating method. Then, a COP film whose surface had been corona-treated was pressed onto the adhesive surface, and an exposure dose of 1000 mJ / cm was applied from the COP film side using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 The film was cured by irradiating ultraviolet light (365 nm standard). The second retardation layer (2-4-03) was transferred onto the COP film, and the polyethylene terephthalate was removed to obtain a COP film (2-4-04) having a second retardation layer. The thickness of the second retardation layer including the adhesive layer was 3.0 μm.
[0376] The retardation value of the COP film (2-4-04) having the second retardation layer was measured using a measuring instrument (KOBRA-WR, manufactured by Oji Scientific Instruments) and the retardation value at a wavelength of 550 nm was measured to be Re(550)=1 nm and Rth(550)=-85 nm. That is, the COP film (2-4-04) having the second retardation layer has the optical characteristic represented by the following formula (3). Note that the retardation value of the COP at a wavelength of 550 nm is approximately 0, so there is no effect on the optical characteristic. n x ≒n y <n z (3)
[0377] [Transfer of the first retardation layer and the second retardation layer]
[0378] After the first retardation layer surface of the film (2-4-10) was subjected to a corona treatment, the alignment polymer composition (4) was applied thereon by a bar coating method and dried by heating in an oven at 90°C for 1 minute to form an alignment film. Next, the composition (B-1) was applied onto the alignment film obtained using a bar coater and dried at 90°C for 1 minute, and then irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm2) using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.). 2) to form a second retardation layer. This resulted in a laminate having a polyethylene terephthalate film, a photoalignment film, a first retardation layer (2-4-01), an alignment film, and a second retardation layer in this order.
[0379] The surface of the obtained second retardation layer was subjected to a corona treatment, and then a UV-curable adhesive composition was applied thereto by a bar coating method. Then, the TAC surface of an iodine-PVA polarizing plate (SRW061A manufactured by Sumitomo Chemical Co., Ltd.) whose surface had been corona-treated was pressed onto the adhesive surface, and the polyethylene terephthalate film side was exposed to light at a dose of 1000 mJ / cm using a UV irradiation device (SPOT CURE SP-7 manufactured by Ushio Inc.). 2 The film was cured by irradiating ultraviolet light of 365 nm (based on 365 nm). At this time, the film was laminated so that the angle between the absorption axis of the polarizing plate and the slow axis of the first retardation layer (2-4-01) was 45°. Then, the polyethylene terephthalate film and the photo-alignment film were simultaneously removed, and the second retardation layer, the alignment film layer, and the first retardation layer (2-4-01) were transferred onto the polarizing plate at once. This resulted in a circular polarizing plate (8-01) in which the polarizing plate, the adhesive layer, the second retardation layer, the alignment film, and the first retardation layer (2-4-01) were laminated in this order. At this time, the thickness of the layer including the adhesive layer, the second retardation layer, and the first retardation layer was 5.2 μm.
[0380] Example 46 The surface of the circular polarizing plate (8-01) obtained in Example 45 opposite to the polarizing plate was attached to a mirror using a pressure-sensitive adhesive, and the plate was observed from the slow axis direction and the fast axis direction of the first retardation layer at an elevation angle of 60° from the front vertical direction to evaluate the optical compensation characteristics. The results are shown in Table 5. A good black display was obtained without any coloring.
[0381] [Table 7] [Industrial Applicability]
[0382] The optical film of the present invention is useful as an optical film excellent in suppressing light leakage during black display. [Explanation of symbols]
[0383] 1. First retardation layer 2 Second retardation layer 3, 3' base material 100 Optical Films 4 layer A 5 layer B 6 Polarizing Plate 8 Third retardation layer 7. Organic EL Panel 110-piece circular polarizer 200 Organic EL display device 30 Organic EL display device 31 circular polarizers 32 Substrate 33 Interlayer insulating film 34 Pixel electrode 35 Light-emitting layer 36 Cathode Electrode 37 Sealing layer 38 Thin Film Transistor 39 Ribs
Claims
1. A circularly polarizing plate (not including a surface reflection suppressing layer) comprising a polarizing plate, an adhesive layer, an optical film having a first retardation layer and a second retardation layer, and a pressure-sensitive adhesive layer in this order, wherein the adhesive layer has a thickness of 2 μm or less, the polarizing plate has a protective film on one surface of a polarizer, and the polarizer surface of the polarizing plate is bonded to the optical film via the adhesive layer, The first retardation layer is A layer A having optical properties represented by formulas (4), (6), and (7); and a layer B having optical properties represented by formulas (5), (6), and (7), Each of the layer A and the layer B is a coating layer formed by polymerizing one or more polymerizable liquid crystals, The second retardation layer has an optical characteristic represented by formula (3), The optical film has optical properties represented by formulas (1) and (2), A circularly polarizing plate according to the above optical film, wherein a second retardation layer is formed on the first retardation layer with or without an alignment film therebetween. Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) nx ≈ ny < nz (3) 100nm<Re(550)<160nm (4) 200nm<Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7) (In the formula, Re(450) represents an in-plane retardation value at a wavelength of 450 nm, Re(550) represents an in-plane retardation value at a wavelength of 550 nm, and Re(650) represents an in-plane retardation value at a wavelength of 650 nm. nx represents a principal refractive index in a direction parallel to the film plane in an index ellipsoid formed by the retardation layer. ny represents a refractive index in a direction parallel to the film plane and perpendicular to the direction of nx in an index ellipsoid formed by the retardation layer. nz represents a refractive index in a direction perpendicular to the film plane in an index ellipsoid formed by the retardation layer.)
2. 2. The circularly polarizing plate according to claim 1, wherein the first retardation layer has optical properties represented by formulas (1) and (2). Re(450) / Re(550)≦1.00 (1) 1.00≦Re(650) / Re(550) (2) (In the formula, Re(450), Re(550) and Re(650) have the same meanings as above.)
3. The optical film further has a third retardation layer, 3. The circularly polarizing plate according to claim 1, wherein the third retardation layer has an optical characteristic represented by formula (5). 200nm<Re(550)<320nm (5) (In the formula, Re(550) has the same meaning as above.)
4. The circularly polarizing plate according to claim 3 , wherein the third retardation layer has optical properties represented by formulas (6) and (7). Re(450) / Re(550)≧1.00 (6) 1.00≧Re(650) / Re(550) (7) (In the formula, Re(450), Re(550) and Re(650) have the same meanings as above.)
5. 5. The circularly polarizing plate according to claim 3, wherein the third retardation layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
6. 6. The circularly polarizing plate according to claim 3, wherein the third retardation layer has a thickness of 5 μm or less.
7. 7. The circularly polarizing plate according to claim 3, wherein the third retardation layer is formed on the alignment film.
8. 8. The circularly polarizing plate according to claim 1, wherein the second retardation layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals.
9. 9. The circularly polarizing plate according to claim 1, wherein the first retardation layer has a thickness of 5 μm or less.
10. 10. The circularly polarizing plate according to claim 1, wherein the second retardation layer has a thickness of 5 μm or less.
11. 11. The circularly polarizing plate according to claim 1, wherein the first retardation layer and the second retardation layer each have a thickness of 5 μm or less.
12. 12. The circularly polarizing plate according to claim 1, wherein the first retardation layer is formed on an alignment film.
13. 13. The circularly polarizing plate according to claim 1, wherein the second retardation layer is formed on the alignment film.
14. 13. The circularly polarizing plate according to claim 7, wherein the alignment film for forming the first retardation layer or the third retardation layer is an alignment film which generates an alignment regulating force by light irradiation.
15. 14. The circularly polarizing plate according to claim 7, wherein the alignment film for forming the second retardation layer or the third retardation layer is an alignment film that exerts a vertical alignment regulating force.
16. 16. The circularly polarizing plate according to claim 12, wherein the thickness of the alignment film is 500 nm or less.
17. 8. The circularly polarizing plate according to claim 3, comprising a first retardation layer, a second retardation layer and a third retardation layer in this order.
18. 18. The circularly polarizing plate according to claim 1, wherein the layer A has a thickness of 5 μm or less.
19. 19. The circularly polarizing plate according to claim 1, wherein the thickness of Layer B is 5 μm or less.
20. 20. The circularly polarizing plate according to claim 1, wherein each of Layer A and Layer B has a thickness of 5 μm or less.
21. 21. The circularly polarizing plate according to claim 1, wherein the adhesive layer is formed from an active energy ray-curable adhesive or a water-based adhesive.
22. An organic EL display device comprising the circular polarizer according to any one of claims 1 to 21.
23. A touch panel display device comprising the circular polarizer according to any one of claims 1 to 22.
Citation Information
Patent Citations
Phase plate
JP2003121645A
Stacked phase differential optical element, manufacturing method therefor, and liquid crystal display device
JP2004118185A
Method of producing elliptically polarizing plate and image display device using the elliptically polarizing plate
JP2006268007A
Fluorene derivatives
JP2010537955A
Alignment film composition, alignment film manufactured thereby, method for manufacturing the alignment film, optical film containing the same, and display apparatus containing the optical film.
JP2012523581A