Lithium secondary battery

Electrochemical reduction of graphene oxide in electrodes addresses the inefficiencies of conventional electrodes by improving conductivity and durability, leading to enhanced charge/discharge capacity and reliability in lithium secondary batteries.

JP7573013B2Active Publication Date: 2024-10-24SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022201888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2011-09-30
Filing Date
2022-12-19
Publication Date
2024-10-24
Estimated Expiration
2032-09-25

AI Technical Summary

Technical Problem

Conventional electrodes for lithium secondary batteries face challenges in efficiently increasing charge/discharge capacity per volume, as well as issues with durability and deformation due to binder swelling when in contact with electrolytes.

Method used

The use of graphene oxide as a conductive layer in electrodes, reduced electrochemically using electrical energy to enhance conductivity and stability, forming a conductive path for ions and reducing graphene oxide to graphene.

Benefits of technology

Improves the charge/discharge capacity, reliability, and durability of power storage devices by increasing the proportion of carbon-carbon double bonds in graphene, enhancing conductivity and maintaining electrode integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573013000001
    Figure 0007573013000001
  • Figure 0007573013000002
    Figure 0007573013000002
  • Figure 0007573013000003
    Figure 0007573013000003
Patent Text Reader

Abstract

Graphene produced from graphene oxide has improved conductivity The present invention also provides a method for manufacturing the same, which can improve charge / discharge capacity and reliability. Provided are a power storage device having excellent electrical characteristics including durability and a manufacturing method thereof. A layer containing graphene oxide is formed on a first conductive layer, and the first conductive layer is a working electrode. The graphene oxide is reduced in an electrolyte solution in which the first conductive layer and the second conductive layer, which is the counter electrode, are immersed. This is a method for producing graphene by supplying a potential that generates the above phenomenon to the potential of the first conductive layer. In a power storage device having at least a positive electrode, a negative electrode, an electrolyte, and a separator, A method for manufacturing a power storage device in which graphene is produced by the above-described manufacturing method on one or both of the electrodes. be.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to graphene, an electrode including the graphene, and a power storage device having the electrode. The present invention relates to a manufacturing method, and also to a graphene, an electrode, and a power storage device manufactured by the manufacturing method. In this specification, the term "power storage device" refers to any element or device having a power storage function. For example, lithium primary batteries, lithium secondary batteries, and lithium ion batteries There are also Pacita etc. [Background technology]

[0002] In recent years, graphene has been shown to have excellent electrical properties, such as high electrical conductivity, high flexibility, and Due to its excellent physical property of mechanical strength, it is being considered for use in a variety of products. It has been done.

[0003] One of these applications is in power storage devices such as lithium secondary batteries and lithium ion capacitors. For example, in order to improve the conductivity of the electrode material for a lithium secondary battery, The laphene can be coated.

[0004] In addition, as a method for producing graphene, a method for preparing a graphite oxide or a graphene oxide using a base In the method for producing graphene, the graphene oxide is reduced in the presence of The methods for forming the oxidizing agent include a method using sulfuric acid, nitric acid, and potassium chlorate as oxidizing agents, a method using sulfuric acid, and potassium permanganate as an oxidizing agent; potassium chlorate and fuming nitric acid as an oxidizing agent. There is a method in which the compound is used as a curing agent (see Patent Document 1).

[0005] Graphite oxide was prepared by using sulfuric acid and potassium permanganate as oxidizing agents. The method is the Modified Hummers method. A method for producing graphene using the Hummers method will be described with reference to FIG. do.

[0006] Graphite is oxidized in a solvent using an oxidizing agent such as potassium permanganate to obtain graphite oxide. A mixture 1 containing phyto is formed. After this, the oxidizing agent remaining in the mixture 1 is removed. To do this, hydrogen peroxide and water are added to the mixture 1 to form the mixture 2 (step S101). In this case, the unreacted potassium permanganate is reduced by hydrogen peroxide, and sulfuric acid is produced. The graphite oxide reacts with manganese sulfate to form manganese sulfate. Next, the acid remaining on or attached to the collected graphite oxide is removed (step S102). To further remove the acid, the graphite oxide was washed with an acidic solution and then with water. The graphite oxide is washed using the washing agent (step S103). The cleaning process is repeated. Then, the graphite oxide is diluted with a large amount of water and centrifuged. The acid is separated from the graphite, and graphite oxide is recovered (step S104). Then, ultrasonic waves are applied to the mixture containing the recovered graphite oxide to form graphite oxide. The oxidized carbon layer is peeled off to form graphene oxide (step S105). Then, graphene can be produced by reducing the graphene oxide (step Top S106).

[0007] Heat treatment can be used as a method for reducing graphene oxide to produce graphene. can. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2011-500488 A Summary of the Invention [Problem to be solved by the invention]

[0009] By the way, in the graphene produced by reducing graphene oxide, The electrical conductivity of graphene can vary depending on the bonding state in the graphene.

[0010] In view of the above, one embodiment of the present invention is to provide a method for producing graphene from graphene oxide, which has a conductive property. To provide graphene having improved properties and a method for producing the same. The objective is to:

[0011] The electrodes included in the electricity storage device are composed of a current collector and an active material layer. In addition to the active material, the active material layer contains a conductive additive and a binder. In the case of electrodes, it is difficult to efficiently increase only the weight of the active material, and the electrode weight or It is difficult to increase the charge / discharge capacity per volume. Furthermore, conventional electrodes have a high charge / discharge capacity in the active material layer. When the binder contained in the electrode comes into contact with the electrolyte, it swells, causing the electrode to deform and become easily damaged. There is also the problem that:

[0012] Therefore, one aspect of the present invention is to improve the charge / discharge capacity, reliability and durability per electrode weight or electrode volume. To provide a power storage device having improved durability, and further to provide a method for manufacturing the power storage device The objective is to: [Means for solving the problem]

[0013] Oxides such as graphite oxide and graphene oxide can be reduced by heat treatment. However, the present invention uses electrical energy to electrochemically reduce graphene oxide, In the present specification, the supply of a potential that promotes the reduction reaction of the active material layer is Reduction by electrochemical reduction is sometimes called electrochemical reduction.

[0014] In this specification, graphene refers to a material that has voids that allow ions to pass through and has double bonds (s p 2 A sheet made of one atomic layer of carbon molecules having a bond, or the sheet The term "multilayer graphene" refers to a laminate of 2 to 100 graphene sheets. In addition, the graphene may have a ratio of elements other than carbon of 30 atomic % or less, or It is preferable that the ratio of elements other than hydrogen and carbon is 15 atomic % or less. The graphene analogue may be doped with an alkali metal such as potassium. is also included in the graphene.

[0015] In this specification, graphene oxide refers to a compound having a six-membered ring or a multi-membered ring composed of carbon. Graphene with oxygen atoms bonded to it, specifically, a six-membered ring or polycyclic ring composed of carbon. The membered ring has an epoxy group, a carbonyl group such as a carboxyl group, or a hydroxyl group bonded to it. Graphene oxide is also called graphene oxide salt, depending on the method of production. The graphene oxide salt may form, for example, a six-membered ring composed of carbon. or an epoxy group, a carbonyl group such as a carboxyl group, or a hydroxyl group bonded to a polymembered ring It is a salt formed by reacting ammonia, amine, alkali metal, etc. with the amine. In this regard, "graphene oxide" includes "graphene oxide salt." The graphene and graphene oxide salt are each formed of a single sheet or a stack of 2 to 100 sheets. The laminate is also called multi-layer graphene oxide and multi-layer graphene oxide salt. You can call.

[0016] In one embodiment of the present invention, a layer including graphene oxide is formed on a first conductive layer, and a second conductive layer is formed on the second conductive layer. The graphene oxide was reduced in an electrolyte solution in which the first conductive layer and the second conductive layer, which was the counter electrode, were immersed. This is a method for producing graphene by supplying a potential at which the primary reaction occurs to the first conductive layer. In principle, the potential supplied to the first conductive layer is a potential at which a reduction reaction of graphene oxide occurs. , 1.6V to 2.4V (based on the redox potential of lithium), The purpose of this study is to reduce graphene oxide to produce graphene. The chemical potential is based on the Li / Li + " may be written as ".

[0017] In one embodiment of the present invention, a layer including graphene oxide is formed in a first conductive layer, and In an electrolyte solution in which a first conductive layer and a second conductive layer serving as a counter electrode are immersed, at least an acid is present. The potential of the first conductive layer is swept to include a potential at which a reduction reaction of the oxidized graphene occurs, This is a method for producing graphene by reducing phene. The potential at which graphene can be reduced is 1.4 V to 2.6 V (vs. Li / Li + ), Preferably 1.6V or more and 2.4V or less (vs. Li / Li + ) range is included at least The potential of the first conductive layer is swept so as to reach the range. The periodic sweep may be performed to sufficiently reduce the graphene oxide. This can be done.

[0018] The above-described method can be used to manufacture a power storage device. A method for manufacturing an energy storage device having a positive electrode, a negative electrode, an electrolyte, and a separator, comprising: One or both of the current collectors are formed with an active material layer containing at least an active material and graphene oxide. A potential at which the graphene oxide reduction reaction occurs is applied to the current collector, and the graphene is generated. Specifically, the present invention relates to a method for producing a current collector in one or both of a positive electrode and a negative electrode. The potential supplied to the body should be between 1.4V and 2.6V (vs. Li / Li + ), preferably 1. 6V or more and 2.4V or less (vs.Li / Li + ) to reduce the graphene oxide, The aim of the study was to produce phenes.

[0019] Another embodiment of the present invention is a current collector including at least an active material and graphene oxide. A layer is formed, and the potential of the current collector is set to a potential at least at which a reduction reaction of the graphene oxide occurs. A method for producing an electrode that reduces graphene oxide by sweeping a current and produces graphene, and a method for producing the electrode Specifically, as described above, The potential at which the compound can be reduced is 1.4V to 2.6V (vs. Li / Li + ), preferably 1 .6V or more and 2.4V or less (vs.Li / Li + ) range is included at least The potential of the body is swept, and at this time, graphene is formed on the surface of the active material or within the active material layer. The potential of the current collector may be periodically swept within the range. By periodically sweeping the temperature, for example, the graphene oxide present in the active material layer can be sufficiently reduced. It is possible.

[0020] In addition, the graphene produced by the above-mentioned graphene production method was found to be Optical method (X-ray photoelectron spectroscopy: XPS) The carbon atom composition measured by is 80% or more and 90% or less, and the oxygen atom composition is 10% or less. In addition, the carbon atoms in the graphene measured by XPS are sp 2 The carbon atoms forming bonds are 50% or more and 80% or less, and the carbon atoms are 60 % or more and 70% or less, or 70% or more and 80% or less, is preferable, that is, 60% or more and 80% or less. is preferred.

[0021] Note that one embodiment of the present invention includes a graphene-containing electrode and one or more of a positive electrode and a negative electrode. Both of the above-mentioned graphene-containing power storage devices are also included. Effect of the Invention

[0022] According to one aspect of the present invention, compared to graphene produced by heat treatment, sp 2 In conjunction Graphene having an increased proportion of carbon-carbon double bonds and improved electrical conductivity; and Furthermore, the graphene can be used as a charge / discharge electrode. To provide a power storage device having improved capacity, reliability and durability, and a method for manufacturing the power storage device It is possible. [Brief description of the drawings]

[0023] [Figure 1] 1A to 1C illustrate a method for manufacturing graphene according to one embodiment of the present invention and an apparatus used for the method. [Diagram 2] 1A to 1C illustrate a method for manufacturing graphene oxide according to one embodiment of the present invention. [Diagram 3] 1A to 1C illustrate a method for manufacturing graphene oxide according to one embodiment of the present invention. [Figure 4] FIG. 2 illustrates a positive electrode according to one embodiment of the present invention. [Diagram 5] FIG. 2 illustrates a negative electrode according to one embodiment of the present invention. [Figure 6] 1A and 1B are diagrams illustrating a power storage device according to one embodiment of the present invention. [Figure 7] FIG. 1 is a diagram illustrating an electrical device. [Figure 8] FIG. 1 is a diagram illustrating an electrical device. [Figure 9] FIG. 1 shows the results of cyclic voltammetry measurements. [Figure 10] FIG. 1 shows the results of cyclic voltammetry measurements. [Figure 11] FIG. 1 shows the results of cyclic voltammetry measurements. [Figure 12] FIG. 1 shows the results of an XPS analysis of the surface elemental composition. [Figure 13] FIG. 1 shows the results of an XPS analysis of the atomic bonding state. [Figure 14] 1A to 1C are diagrams illustrating a conventional method for producing graphene. [Figure 15] FIG. 1 shows the results of cyclic voltammetry measurements. [Figure 16] FIG. 1 shows the results of cyclic voltammetry measurements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] An embodiment and an example of the present invention will be described below with reference to the drawings. The present invention is not limited to the following description, and the scope of the present invention is not limited to the following description. It will be readily understood by those skilled in the art that various changes in form and details may be made. The present invention should not be construed as being limited to the description of the following embodiment. In referring to the drawings in the description, reference numerals that refer to the same objects are used commonly among the different drawings. In addition, the same hatch pattern is used to indicate similar items, and the symbols are It may not be attached.

[0025] (Embodiment 1) In this embodiment, a method for manufacturing graphene according to one embodiment of the present invention will be described below with reference to FIG. The following description will be given with reference to FIG. 1(A) and FIG. 1(B). ) is a schematic diagram of an apparatus for producing graphene.

[0026] In the method for producing graphene according to one embodiment of the present invention, a heat treatment is performed to produce graphene. Therefore, instead of reducing graphene oxide, it is electrochemically oxidized using electrical energy. The first step is to reduce graphene.

[0027] <Step S111> In step S111 shown in FIG. 1A, a layer including graphene oxide is formed on the surface of the conductive layer. For example, a dispersion liquid containing graphene oxide is applied onto the conductive layer. The dispersion liquid containing the oxidized grit may be a commercially available product, or may be prepared by the method described with reference to FIG. A dispersion liquid in which laphene is dispersed in a solvent may be used. Alternatively, a dispersion liquid in which graphene oxide (graphene oxide salt) is dispersed in a solvent may be used.

[0028] The conductive layer may be made of any material having electrical conductivity. For example, aluminum (Al ), copper (Cu), nickel (Ni), titanium (Ti), or other metal materials, The alloy material may be, for example, Al. The conductive layer may be in the form of a foil, a plate, a mesh, or the like. The shape can be appropriately used, and the metal material or the alloy material can be formed on a substrate separately. Alternatively, the composition may be peeled off and the peeled off product may be used as the conductive layer.

[0029] The method of applying the dispersion liquid containing graphene oxide onto the conductive layer includes a coating method, a spin coating method, and the like. There are several methods, such as the dipping method, the dip coating method, and the spray coating method. For example, a dispersion containing graphene oxide may be applied to the conductive layer by a dip coating method. After applying the liquid, the conductive layer is rotated in the same manner as in the spin coating method to remove the oxide film. The uniformity in thickness of the graphene-containing dispersion can be increased.

[0030] A dispersion liquid containing graphene oxide is applied onto a conductive layer, and then the solvent in the dispersion liquid is removed. For example, by performing vacuum drying for a certain period of time, the graphene oxide-containing conductive layer coated on the conductive layer The solvent can be removed from the dispersion. Depending on the amount of the dispersion to be applied, vacuum drying may be used. The time for vacuum drying varies. In addition, the graphene oxide is not heated to a degree that reduces it. For example, the thickness of the graphene oxide after step S111 may be about 10 μm. In this case, the conductive layer is heated at a temperature between room temperature and 100°C and vacuum dried for 1 hour. After that, it is preferable to perform vacuum drying at room temperature for about 1 hour.

[0031] <Step S112> Next, the graphene oxide provided on the conductive layer is reduced to generate graphene. Then, as described above, graphene oxide is electrochemically reduced using electrical energy. Conceptually, this step is to form a film by providing the graphene oxide formed in step S111. A closed circuit is formed using the conductive layer, and a reduction reaction of the graphene oxide occurs in the conductive layer. A potential or a potential at which the graphene oxide is reduced is applied to the graphene oxide. In this specification, the electric field that causes the reduction reaction of graphene oxide is The potential at which the graphene oxide is reduced is called a reduction potential.

[0032] The method for reducing graphene oxide will be specifically described with reference to FIG. 1(B). The electrode is filled with a solution 114, and a conductive layer 115 having graphene oxide and a counter electrode 116 are inserted therein. In this step, the graphene oxide formed in step S111 is placed in the The conductive layer 115 is used as a working electrode, and at least a counter electrode 116 and an electrolyte 114 are used to conduct electricity. An electrochemical cell (open circuit) was assembled, and the reduction potential of graphene oxide was set to the potential of the conductive layer 115 (working electrode). This is a step of reducing the graphene oxide to graphene by supplying an electrolyte 114. For the ethylene carbonate and diethyl carbonate, A solvent can be used. The reduction potential to be applied is based on the counter electrode 116. Reduction potential, or reduction potential when a reference electrode is provided in an electrochemical cell and the reference electrode is used as a reference For example, when the counter electrode 116 and the reference electrode are made of lithium metal, the reduction potential to be applied is Redox potential based on the redox potential of lithium metal (vs. Li / Li + ) This By this step, the electrochemical cell (closed circuit) generates a reduction current when the graphene oxide is reduced. Therefore, to confirm the reduction of graphene oxide, the reduction current must be monitored. When the reduction current falls below a certain value (when the peak corresponding to the reduction current disappears), The state in which the graphene oxide is reduced (the state in which the reduction reaction is completed) may be regarded as a state in which the graphene oxide is reduced (the state in which the reduction reaction is completed).

[0033] In addition, in this step, when controlling the potential of the conductive layer 115, The potential of 5 may be fixed to the reduction potential of graphene oxide, or the reduction potential of graphene oxide may be The sweep may include a periodic sweep such as cyclic voltammetry. The sweep speed of the potential of the conductive layer 115 is not limited, but may be 0. The potential of the conductive layer 115 is preferably swept at a rate of 0.05 mV / s or more and 1 mV / s or less. When the potential is swept, the potential may be swept from the high potential side to the low potential side, or from the low potential side to the high potential side. This is also fine.

[0034] The reduction potential of graphene oxide depends on the composition of the graphene oxide (presence or absence of functional groups and oxidation graph). The values ​​vary slightly depending on the potential control method (e.g., the formation of phenylalanine salts) and the potential control method (e.g., the sweep rate). Approximately 2.0V (vs. Li / Li + Specifically, it is about 1.4V to 2.6V. (vs. Li / Li + ), preferably 1.6V to 2.4V (vs. Li / Li + ) The potential of the conductive layer 115 may be controlled within a range of This will be described in detail in the Examples below.

[0035] Through the above steps, graphene can be formed on the conductive layer 115.

[0036] In addition, the graphene produced by the method for producing graphene according to one embodiment of the present invention may have a structure in which X The carbon atom composition measured by PS is 80% or more and 90% or less, and the oxygen atom composition is 10 % or more and 20% or less of the carbon atoms, 2 The carbon atoms forming the bond are 50% to 80%, and the carbon atoms are 60% to 70% or 70% to 80%. % or less, that is, 60% or more and 80% or less is preferable.

[0037] The method for reducing graphene oxide is electrochemically using electrical energy. In addition to the method of reducing the oxygen atoms in graphene oxide to carbon dioxide by heat treatment, The graphene according to one embodiment of the present invention is then desorbed and reduced (also called thermal reduction). The graphene produced by thermal reduction has at least the following differences: The graphene according to one embodiment of the present invention can be electrochemically oxidized using electrical energy. By reducing 2 The ratio of carbon-carbon bonds in double bonds, which are bonds, is reduced by thermal reduction. Therefore, the graphene according to one embodiment of the present invention is not localized at a specific position. Since it has more π electrons that contribute widely to carbon-carbon bonds than graphene obtained by thermal reduction, It can be said that the conductivity is increased compared to that of graphene obtained by thermal reduction.

[0038] By the way, an example of a method for producing graphene oxide that can be used in step S111 is as follows. The method described with reference to FIG. 14 includes the step S103 of cleaning graphene oxide. In the process, a large amount of water is required. Furthermore, by repeatedly performing step S103, It is possible to remove acid from graphite oxide, but the acid content decreases. As the temperature drops, it becomes difficult to separate the precipitate of graphite oxide from the acid in the supernatant. However, the yield of graphite oxide decreases, which ultimately leads to a decrease in the yield of graphene. Connect.

[0039] Here, in step S111, a method for producing an oxidized graph different from the method described with reference to FIG. We will explain how to make Fen.

[0040] FIG. 2 is a diagram illustrating a production process of graphene oxide (or graphene oxide salt).

[0041] <Graphite oxidation treatment> As shown in step S121, the graphite is oxidized with an oxidizing agent to form a graphite oxide. Form a .

[0042] The oxidizing agent may be sulfuric acid, nitric acid and potassium chlorate, sulfuric acid and potassium permanganate, or In this case, potassium chlorate and fuming nitric acid are used. In this case, graphite, sulfuric acid and manganese peroxide are used. Mix potassium phosphate to oxidize the graphite. Add water to make graphite oxide. A mixture 1 is formed comprising:

[0043] After this, hydrogen peroxide and water may be added to Mixture 1 to remove any remaining oxidizing agent. The unreacted potassium permanganate is reduced by hydrogen peroxide, which reacts with sulfuric acid to form potassium sulfate. Manganese sulfate is water-soluble, so it can be dissolved in water to form an oxide. It can be separated from graphite.

[0044] <Recovery of graphite oxide> Next, as shown in step S122, graphite oxide is collected from the mixture 1. The mixed liquid 1 is subjected to one or more processes such as filtration and centrifugation to obtain graphite oxide. The precipitate 1 containing graphite is collected. Note that the precipitate 1 may contain unreacted graphite. do.

[0045] <Cleaning graphite oxide> Next, as shown in step S123, an acidic solution is used to extract the precipitate containing graphite oxide. Metal ions and sulfate ions are removed from the product 1. By dissolving metal ions derived from an oxidizing agent in an acidic solution, metals are converted from graphite oxide to ions and sulfate ions can be removed.

[0046] In this way, by using an acidic solution to clean graphite oxide, Therefore, the graphene oxide salt yield can be improved by the method shown in FIG. can increase the productivity of graphene oxide and even graphene.

[0047] Representative examples of acid solutions include hydrochloric acid, dilute sulfuric acid, and nitric acid. Generally, if the treatment is carried out with hydrochloric acid, the remaining acidic solution can be easily removed in the subsequent drying process. This is preferable because

[0048] As a method for removing metal ions and sulfate ions from the precipitate 1, the precipitate 1 and an acid After mixing the solutions, one or more of the following methods are performed: filtration, centrifugation, dialysis, etc.; precipitation on filter paper In this example, the precipitate 1 is placed on a filter paper and an acidic solution is poured onto the precipitate 1. Then, the metal ions and sulfate ions are washed out from the precipitate 1 using an acidic solution, and the precipitate is subjected to oxidation graphite. The precipitate 2 containing graphite is collected. Note that the precipitate 2 may contain unreacted graphite. be.

[0049] <Generation of graphene oxide> Next, as shown in step S124, the precipitate 2 is mixed with water to disperse the precipitate 2. A mixed liquid 2 is formed. Next, the graphite oxide contained in the mixed liquid 2 is peeled off to obtain graphite oxide. The method of exfoliating graphite oxide to produce graphene oxide is The mixed liquid in which the graphene oxide is dispersed is called mixed liquid 3. do.

[0050] In addition, the graphene oxide formed by this process has six-membered rings composed of carbon aligned in a planar direction. In some parts, multi-membered rings such as seven-membered rings, eight-membered rings, nine-membered rings, and ten-membered rings are formed. The poly-membered ring is a ring in which some carbon bonds are broken and the number of carbon atoms is increased. A ring-shaped carbon skeleton in which carbon bonds are broken so as to increase in number. The area surrounded by carbon atoms that form a six-membered or multi-membered ring is a gap. The carbonyl groups, such as epoxy groups, carboxyl groups, and hydroxyl groups, are bonded to the dispersion. Instead of dispersed graphene oxide, multi-layer graphene oxide may be dispersed.

[0051] <Recovery of graphene oxide> Next, as shown in step S125, the mixture 3 is subjected to one or more of filtration, centrifugation, etc. The graphene oxide-containing mixture was separated from the graphite-containing precipitate 3. The mixture containing graphene oxide is referred to as mixture 4. In particular, graphene oxide with carbonyl groups is able to catalyze hydrogen transport in polar mixtures. As the graphene oxide is ionized, it becomes easier for the graphene oxide to disperse among itself.

[0052] The mixture 4 prepared by the above steps is used in step S111 shown in FIG. The present invention can be applied to dispersions in which

[0053] There is a possibility that impurities are present in the mixture 4. In order to improve the purity of graphene obtained in the method for producing graphene, step S125 It is preferable to purify the graphene oxide contained in the mixture 4 prepared in step 1. It is preferable to perform steps S126 and S127 after step S125. Next, steps S126 and S127 will be described.

[0054] <Generation of graphene oxide salt> As shown in step S126, a basic solution is mixed into the mixture 4 to form graphene oxide salt. After the formation, an organic solvent is added to produce a mixture 5 in which graphene oxide salt precipitates as a precipitate 4. Complete.

[0055] A typical example of a basic solution is a solution that removes oxygen bound to the carbon of graphene oxide by reduction. A mixture containing a base that does not react with graphene oxide and that neutralizes the graphene oxide is preferred. Sodium hydroxide solution, potassium hydroxide solution, ammonia solution, methylamine solution, Examples include ethanolamine solution, dimethylamine solution, and trimethylamine solution.

[0056] The organic solvent is used to precipitate the graphene oxide salt. Examples include acetone, methanol, and ethanol.

[0057] <Recovery of graphene oxide salt> Next, as shown in step S127, the mixture 5 is subjected to one or more of filtration, centrifugation, etc. By this, the graphene oxide salt is separated into a solvent and a precipitate 4 containing the graphene oxide salt. The precipitate 4 is collected.

[0058] The precipitate 4 can then be dried to obtain graphene oxide salt.

[0059] The graphene oxide salt prepared by the above steps was dispersed in a solvent as shown in Figure 1(A By applying the same to the dispersion liquid of step S111 shown in FIG. 1, a graphene according to one embodiment of the present invention can be obtained. The purity of the graphene obtained by the method for producing the graphene can be improved.

[0060] In addition, in the steps after step S123 in FIG. 2, graphene oxide is generated. Instead, a graphite oxide salt is generated (step S134), and the graphite oxide salt is After recovery (step S135), graphene oxide salt may be produced (see FIG. 3).

[0061] In step S134, the precipitate 2 obtained in step S123 is mixed with water and then subjected to a basic The solutions are mixed to produce graphite oxide salt, and then an organic solvent is added to produce the graphite oxide salt. The basic solution and the organic solvent are used in step S126 to produce a mixture in which the nucleophile precipitates. The basic solution and organic solvent may be selected and used accordingly.

[0062] Step S135 is a step of precipitating the graphite oxide salt obtained in step S134. The liquid is subjected to one or more of filtration, centrifugation, etc., to obtain a solution containing an organic solvent and a graphite oxide salt. The precipitate containing the graphite oxide salt is recovered.

[0063] In the method for preparing graphene oxide salt shown in FIG. 3, the other steps are the same as those shown in FIG. Similar to steps.

[0064] As described above, in this embodiment, compared with graphene produced by heat treatment, sp 2 join The ratio of carbon-carbon double bonds, which is the double bond, is increased, and the graphene with improved electrical conductivity is obtained. It can be made.

[0065] This embodiment mode may be appropriately combined with the configurations described in other embodiment modes and examples. It is possible to implement.

[0066] (Embodiment 2) In this embodiment, a power storage device according to one embodiment of the present invention will be described. Regarding a power storage device having an electrode manufactured by using the graphene manufacturing method described in the first embodiment, Note that in this embodiment, a power storage device according to one embodiment of the present invention will be described using a lithium secondary battery. It will be described as a battery.

[0067] First, the positive electrode 311 will be described.

[0068] 4A is a cross-sectional view of the positive electrode 311. The positive electrode 311 is a positive electrode active material on a positive electrode current collector 307. The positive electrode active material layer 309 is formed. and graphene 323 (not shown), as well as binders and conductive additives. It may include.

[0069] The active material is an ion that serves as a carrier in the power storage device (hereinafter, referred to as a carrier ion). Therefore, the active material and the active material layer are distinguished.

[0070] The positive electrode current collector 307 is made of a highly conductive material such as platinum, aluminum, copper, titanium, or stainless steel. The material can be used. Also, the positive electrode current collector 307 can be suitably used in a shape such as foil, plate, net, etc.

[0071] The positive electrode active material 321 contained in the positive electrode active material layer 309 can be used as a material such as lithium compounds like LiFeO2, LiCoO2, LiNiO2, LiMn2O4, V2O5, Cr2O5, MnO2, etc.

[0072] Alternatively, as the positive electrode active material 321, a lithium-containing phosphate having an olivine-type structure (general formula LiMPO4 (M is one or more of Fe(II), Mn(II), Co(II), Ni(II))) can be used. Representative examples of the general formula LiMPO4 include LiFePO4, LiNiPO4, LiCoPO4, LiMnPO4, LiFeNiPO4, LiFeCoPO4, LiFeMnPO4, LiNiCoPO4, LiNiMnPO4 (a + b is 1 or less, 0 < a < 1, 0 < b < 1), LiFeNiCoPO4, LiFeNiMnPO4, LiNiCoMnPO4 (c + d + e is 1 or less, 0 < c < 1, 0 < d < 1, 0 < e < 1), LiFeNiCoMnPO4 (f + g + h + i is 1 or less, 0 < f < 1, 0 < g < 1, 0 < h < 1, 0 < i < 1), etc. a b a b a b a b a b c d e c d e c d e f g h i ​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​ can be used as a material.

[0073] Alternatively, as the positive electrode active material 321, a lithium-containing silicate such as a general formula Li2MSiO4 (M is one or more of Fe(II), Mn (II), Co(II), Ni(II)) etc. can be used. Examples of the representative general formula Li2MSiO4 include Li2FeSiO4, Li2N iSiO4, Li2CoSiO4, Li2MnSiO4, Li2Fe k Ni l SiO4, Li2Fe k Co l SiO4, Li2Fe k Mn l SiO4, Li2Ni k Co l SiO 4, Li2Ni k Mn l SiO4 (k + l is 1 or less, 0 < k < 1, 0 < l < 1), Li2 Fe m Ni n Co q SiO4, Li2Fe m Ni n Mn q SiO4, Li2Ni m Co n Mn q SiO4 (m + n + q is 1 or less, 0 < m < 1, 0 < n < 1, 0 < q < 1), Li2 Fe r Ni s Co t Mn u SiO4 (r + s + t + u is 1 or less, 0 < r < 1, 0 < s < 1 , 0 < t < 1, 0 < u < 1) etc. lithium compounds can be used as a material.

[0074] In addition, when the carrier ion is an alkali metal ion, alkaline earth metal ion, beryllium ion, or magnesium ion other than lithium ion, the positive electrode active material 321 ​In the above lithium compound, a carrier may be used instead of lithium. The same alkali metals as the ions (e.g., sodium, potassium, etc.), or alkaline earth metals Metals (e.g., calcium, strontium, barium, etc.), or beryllium or ma A compound in which magnesium is replaced is used.

[0075] As shown in FIG. 4B, which is a plan view of a part of the positive electrode active material layer 309, The layer 309 is made of a particulate positive electrode active material 321 capable of absorbing and releasing carrier ions, and a positive electrode active material The positive electrode active material 321 is packed inside the graphene 323, which covers the positive electrode active material 321. In addition, in plan view, the positive electrode active material layer 309 is formed on the surface of the plurality of positive electrode active materials 321. The positive electrode active material layer 309 is covered with different graphenes 323. The electrode active material 321 may be exposed.

[0076] The particle size of the positive electrode active material 321 is preferably 20 nm or more and 100 nm or less. Since the carrier ions (electrolytes and carrier ions) move within the positive electrode active material layer 309, the surface of the positive electrode active material 321 In order to increase the area and shorten the distance that electrons (and carrier ions) travel, the positive electrode active material 3 The smaller the particle size of 21, the more preferable it is.

[0077] Furthermore, sufficient characteristics can be obtained even if the surface of the positive electrode active material 321 is not covered with a carbon film. However, when graphene is used in combination with a positive electrode active material covered with a carbon film, hopping conduction This is more preferable because a current flows between the positive electrode active materials 321 .

[0078] FIG. 4(C) is a cross-sectional view of a portion of the positive electrode active material layer 309 in FIG. C) shows a positive electrode active material 321 and a positive electrode active material layer 309 in a plan view. In the cross-sectional view, the graphene 323 is The same graphene or multiple graphenes are observed in multiple positive electrode active materials 321. A plurality of positive electrode active materials 32 are overlapped with each other or are formed by the same graphene or a plurality of graphenes. The graphene 323 has a bag shape, and a plurality of positive electrodes are disposed inside the bag. The graphene 323 may contain an electrode active material 321. In this region, the positive electrode active material 321 may be exposed.

[0079] The thickness of the positive electrode active material layer 309 is selected from the range of 20 μm to 100 μm. The thickness of the positive electrode active material layer 309 is appropriately adjusted so as to prevent cracks and peeling. It is preferable.

[0080] The positive electrode active material layer 309 contains acetylene having a volume 0.1 to 10 times the volume of graphene. Lenblack particles and carbon particles with one-dimensional expansion (carbon nanofibers, etc.) ) and a known conductive assistant such as polyvinylidene fluoride (PVDF) may have the following structure:

[0081] The positive electrode active material may be a material whose volume expands due to the absorption of carrier ions. When using such a positive electrode active material, the positive electrode active material layer becomes brittle during charging and discharging, and If the part collapses, the reliability of the electricity storage device (for example, cycle characteristics) will decrease. However, in the positive electrode of the power storage device of one embodiment of the present invention, the positive electrode active material 321 is surrounded by graphene 3. Since the positive electrode active material 321 is covered with the graphene 23, even if the positive electrode active material 321 expands in volume due to charging and discharging, The positive electrode active material layer 309 can be prevented from being pulverized by the positive electrode active material layer 323 and from being destroyed by the positive electrode active material layer 309. That is, the graphene 323 included in the positive electrode of the power storage device of one embodiment of the present invention Even if the volume of the positive electrode active material 321 expands and contracts with discharge, the positive electrode active material 321 maintains its adhesion to each other. Therefore, the use of the positive electrode 311 improves the durability of the power storage device. It is possible.

[0082] In other words, there is no need to use a binder when forming the positive electrode active material layer 309, and a certain weight In the positive electrode active material layer, it is possible to increase the amount of positive electrode active material. This increases the charge / discharge capacity per unit area.

[0083] In addition, the graphene 323 has conductivity and is in contact with the plurality of positive electrode active material particles 321. In other words, when the positive electrode active material layer 309 is formed, the conductive additive is used. It is not necessary to use a binder, and the amount of the positive electrode active material can be increased in a positive electrode active material layer of a constant weight. Therefore, the charge / discharge capacity per electrode weight can be increased.

[0084] The graphene 323 is a graphene according to one embodiment of the present invention. The ion 323 is electrochemically reduced using electrical energy as described in the first embodiment. The graphene has improved electrical conductivity compared to graphene reduced by heat treatment. The graphene has an efficient and sufficient conductive path (carrier ion) in the positive electrode active material layer 309. Since the conductive path of the positive electrode 311 is formed, the positive electrode active material layer 309 and the positive electrode 311 have excellent conductivity. Therefore, in the power storage device having the positive electrode 311, the capacity of the positive electrode active material 321 is set to the theoretical capacity. Since the battery can be utilized as efficiently as possible, the discharge capacity can be increased sufficiently.

[0085] Next, a method for producing the positive electrode 311 will be described.

[0086] A slurry containing particles of the positive electrode active material 321 and graphene oxide is formed. Specifically, The positive electrode active material 321 and a dispersion liquid containing graphene oxide are mixed together to form a slurry. The dispersion liquid containing graphene oxide was prepared by the method described in the first embodiment. It is possible.

[0087] Next, the above slurry is applied onto the positive electrode current collector 307, and then dried for a certain period of time to form a positive electrode. The solvent is removed from the slurry applied onto the electrode current collector 307. For details, refer to the first embodiment as appropriate. At this time, pressure molding may be performed as necessary.

[0088] After that, similarly to the graphene manufacturing method described in Embodiment 1, Graphene oxide is electrochemically reduced to produce graphene 323. As a result, a positive electrode active material layer 309 can be formed on the positive electrode current collector 307, and a positive electrode 311 can be produced. can.

[0089] In addition, when the positive electrode 311 is formed, since graphene oxide contains oxygen, it is difficult to form the positive electrode 311 in a polar solvent. As a result, the graphene oxide particles are dispersed among each other. In the process of producing the positive electrode 311, the positive electrode active material 321 is less likely to aggregate. Therefore, the increase in the internal resistance can be suppressed, and the positive electrode Since the electrons (and carrier ions) in the active material 321 can easily move, the positive electrode active material layer 3 The conductivity of the positive electrode 311 and the conductivity of the positive electrode 312 can be increased.

[0090] When the positive electrode 311 is formed, graphene oxide is reduced to generate graphene 323. This step may be carried out after assembling an electricity storage device using the negative electrode, the electrolyte, and the separator. In other words, after assembling the power storage device, the potential at which the reduction reaction of graphene oxide occurs is applied to the positive electrode. The body 307 may be provided with

[0091] Next, the negative electrode and the method for producing the same will be described.

[0092] 5A is a cross-sectional view of the negative electrode 205. The negative electrode 205 is formed by forming a negative electrode active layer on a negative electrode current collector 201. The material layer 203 is formed. The negative electrode active material layer 203 is formed by forming at least the negative electrode active material 211. and graphene 213, and may further include a binder and a conductive additive. .

[0093] The negative electrode current collector 201 is made of a highly conductive material such as copper, stainless steel, iron, or nickel. The negative electrode current collector 201 may be in a foil, plate, mesh, or other suitable shape. can.

[0094] The negative electrode active material layer 203 is made of a negative electrode active material 211 capable of absorbing and releasing carrier ions. Representative examples of the negative electrode active material 211 include lithium, aluminum, graphite, Silicon, tin, and germanium. Or lithium, aluminum, graphene, etc. Compounds containing one or more selected from the group consisting of arsenic, silicon, tin, and germanium. Even if the negative electrode current collector 201 is not used and each negative electrode active material layer 203 is used alone as a negative electrode, As the negative electrode active material 211, germanium, silicon, Lithium and aluminum have a larger theoretical capacity. When the theoretical capacity is large, the amount of negative electrode active material is This allows the load to be reduced, leading to cost savings and a smaller power storage device.

[0095] FIG. 5B is a plan view of a part of the negative electrode active material layer 203. The negative electrode active material layer 203 is , the negative electrode active material 211 is coated with the negative electrode active material 211 while covering the negative electrode active material 211. The negative electrode active material layer 203 in plan view is composed of graphene 213 filled with The surfaces of the negative electrode active materials 211 are covered with different graphenes 213. In this case, the negative electrode active material 211 may be exposed.

[0096] FIG. 5C is a cross-sectional view of a part of the negative electrode active material layer 203 in FIG. The material 211 and the graphite covering the negative electrode active material 211 in a plan view of the negative electrode active material layer 203. In the cross-sectional view, the graphene 213 is observed as a line. The same graphene or multiple graphenes overlap with multiple negative electrode active materials 211, or The negative electrode active material 211 is contained within the same graphene or multiple graphenes. Note that the graphene 213 has a bag shape and contains a plurality of negative electrode active materials. In addition, the graphene 213 has a partly open area, and the negative charge is applied to the part. The electrode active material 211 may be exposed.

[0097] The thickness of the negative electrode active material layer 203 is selected from the range of 20 μm to 100 μm. do.

[0098] The negative electrode active material layer 203 contains acetylene having a volume 0.1 to 10 times the volume of graphene. Lenblack particles and carbon particles with one-dimensional expansion (carbon nanofibers, etc.) and a known binder such as polyvinylidene fluoride. stomach.

[0099] The negative electrode active material layer 203 may be pre-doped with lithium. As a method, a lithium layer is formed on the surface of the negative electrode active material layer 203 by a sputtering method. Alternatively, a lithium foil may be provided on the surface of the negative electrode active material layer 203. In particular, after assembling the storage device, the positive electrode When graphene 323 is to be formed on the positive electrode active material layer 309 of 311, It is preferable to pre-dope the material with lithium.

[0100] In addition, the volume of the negative electrode active material 211 expands due to the absorption of carrier ions. For this reason, the negative electrode active material layer becomes brittle during charging and discharging, and part of the negative electrode active material layer collapses. This reduces the reliability of the power storage device (e.g., cycle characteristics, etc.). In the negative electrode of the power storage device of one embodiment of the present invention, the negative electrode active material 211 is surrounded by graphene 213. Therefore, even if the negative electrode active material 211 expands in volume due to charging and discharging, the graphene 213 covers the negative electrode active material 211. This can prevent the negative electrode active material 211 from being pulverized and the negative electrode active material layer 203 from being destroyed. The graphene 213 included in the negative electrode of the power storage device of one embodiment of the present invention changes with charging and discharging. Even if the volume of the negative electrode active material 211 expands and contracts, the negative electrode active material 211 has a function of maintaining the adhesion between the negative electrode active materials 211. Therefore, by using the negative electrode 205, it is possible to improve the durability of the power storage device. can.

[0101] In other words, there is no need to use a binder when forming the negative electrode active material layer 203, and a certain weight ( In a negative electrode active material layer of a given volume, it is possible to increase the amount of negative electrode active material. Therefore, the charge / discharge capacity per electrode weight (electrode volume) can be increased.

[0102] The graphene 213 has electrical conductivity and is in contact with the plurality of negative electrode active materials 211. In other words, when forming the negative electrode active material layer 203, the conductive additive is used. There is no need to use a binder, and the amount of negative electrode active material in a negative electrode active material layer of a constant weight (constant volume) is Therefore, the charge / discharge capacity per electrode weight (electrode volume) can be increased. It can be done.

[0103] The graphene 213 is a graphene according to one embodiment of the present invention. The ion 213 is electrochemically reduced using electrical energy as described in the first embodiment. The graphene has improved electrical conductivity compared to graphene reduced by heat treatment. The graphene has an efficient and sufficient conductive path (carrier ion) in the negative electrode active material layer 203. Since the conductive path of the negative electrode 205 is formed, the conductive property of the negative electrode active material layer 203 and the conductive property of the negative electrode 205 are Therefore, the capacity of the negative electrode active material 211 in the power storage device having the negative electrode 205 is Since it can be used as efficiently as the theoretical capacity, the charging capacity can be increased sufficiently. do.

[0104] In addition, graphene 213 can also function as a negative electrode active material capable of absorbing and releasing carrier ions. This allows the charge capacity of the negative electrode 205 to be improved.

[0105] Next, a method for forming the negative electrode active material layer 203 shown in FIGS.

[0106] A slurry containing particles of the negative electrode active material 211 and graphene oxide is formed. Specifically, The mixture is kneaded with a dispersion liquid containing particulate negative electrode active material 211 and graphene oxide to obtain a slurry. The dispersion liquid containing graphene oxide was prepared by the method described in the first embodiment. It is possible.

[0107] Next, the above slurry is applied onto the negative electrode current collector 201, and then vacuum dried for a certain period of time. The solvent is removed from the slurry applied onto the negative electrode current collector 201. In this case, pressure molding may be performed as necessary.

[0108] After that, similarly to the graphene manufacturing method described in Embodiment 1, Graphene oxide is electrochemically reduced to produce graphene 213. As a result, a negative electrode active material layer 203 can be formed on the negative electrode current collector 201, and a negative electrode 205 can be produced. can.

[0109] In addition, when manufacturing a power storage device including the positive electrode 311 and the negative electrode 205, In the case where graphene is formed by the method described in Embodiment 1, the positive electrode 31 and the negative electrode 205 are both Either the negative electrode 205 or the negative electrode 206 is formed by adding graphene to the negative electrode 205 before assembling the power storage device. It is preferable to form the graphite oxide in the cathode 311 and the anode 205. Even if the electricity storage device is assembled with the ion implanted, the potential can be efficiently applied to the positive electrode 311 and the negative electrode 205. The graphene oxide is not fully reduced, or the graphene oxide is not fully reduced. This is because it takes time.

[0110] In addition, when the negative electrode 205 is formed, since graphene oxide contains oxygen, it is difficult to form the negative electrode 205 in a polar solvent. As a result, the graphene oxide particles are dispersed among each other. The negative electrode active material 211 is less likely to aggregate in the process of producing the negative electrode 205. Therefore, the increase in the internal resistance can be suppressed, and the negative electrode Since the electrons (and carrier ions) in the active material 211 move easily, the negative electrode active material layer 2 The conductivity of the negative electrode 203 and the conductivity of the negative electrode 205 can be increased.

[0111] Next, the structure of the negative electrode shown in FIG. 5(D) will be described.

[0112] FIG. 5D is a cross-sectional view of a negative electrode in which a negative electrode active material layer 203 is formed on a negative electrode current collector 201. The negative electrode active material layer 203 is made of a negative electrode active material 221 having an uneven surface. The graphene 223 covers the surface of the substrate 221 .

[0113] The uneven negative electrode active material 221 has a common portion 221a and a protruding portion 2 protruding from the common portion 221a. The protrusions 221b are cylindrical, prismatic, or other cylindrical, conical, or pyramidal, needle-shaped, The top of the protrusion may be curved. 1, like the negative electrode active material 211, absorbs carrier ions (typically lithium ions). The common portion 221a and the protruding portion 221b are formed using a negative electrode active material capable of releasing charge. The common portion 221a and the protruding portion 221b may be made of the same material. It may be constructed using a material.

[0114] Silicon, which is an example of a negative electrode active material, has a volume that increases due to the absorption of ions that act as carriers. The negative electrode active material becomes brittle during charging and discharging, and the negative electrode active material If a part of the layer collapses, the reliability of the energy storage device (e.g., cycle characteristics) will decrease. However, in the case where silicon is used as the negative electrode active material 221 in the negative electrode shown in FIG. Since the negative electrode active material 221 is covered with the graphene 223, the negative electrode active material 22 Even if the negative electrode active material layer 203 expands in volume due to charging and discharging, the negative electrode active material layer 203 The collapse of the

[0115] In addition, the surface of the negative electrode active material layer is brought into contact with the electrolyte that constitutes the electricity storage device, thereby The liquid reacts with the negative electrode active material to form a coating on the surface of the negative electrode. The interface between the negative electrode and the electrolyte is called the id electrolyte interface. However, the thickness of the coating is thought to be necessary to soften and stabilize the When the temperature drops, carrier ions are less likely to be absorbed by the negative electrode, and the carrier ions between the electrode and the electrolyte However, there are problems such as a decrease in conductivity and consumption of electrolyte.

[0116] By covering the surface of the negative electrode active material layer 203 with graphene 213, the thickness of the film is increased. It is possible to suppress the decrease in charge / discharge capacity.

[0117] Next, a method for forming the negative electrode active material layer 203 shown in FIG. 5(D) will be described.

[0118] The negative electrode active material 221 having a concave-convex shape is applied to the negative electrode current collector by a printing method, an inkjet method, a CVD method, or the like. Alternatively, a film of a negative electrode active material is formed on the negative electrode 201 by a coating method, a sputtering method, a vapor deposition method, or the like. After providing the negative electrode active material 221, the negative electrode active material 221 is selectively removed to provide the negative electrode active material 221 on the negative electrode current collector 201. or a foil or a material made of lithium, aluminum, graphite, and silicon. A part of the surface of the plate is removed to form an uneven negative electrode current collector 201 and an uneven negative electrode active material 221. A network formed of lithium, aluminum, graphite, and silicon is used as the negative electrode active material and It can be used as a negative electrode current collector.

[0119] Next, a dispersion liquid containing graphene oxide is applied onto the uneven surface of the negative electrode active material 221. As a method for applying the dispersion liquid containing graphene, the method described in the first embodiment may be appropriately used. That's good.

[0120] Next, the solvent in the dispersion liquid containing graphene oxide is removed as described in the first embodiment. Then, as described in the first embodiment, the electrochemical Graphene oxide may be reduced to produce graphene 213.

[0121] In this way, by producing graphene using a dispersion liquid containing graphene oxide, The surface of the negative electrode active material 221 can be covered with the graphene 213 having a uniform thickness. .

[0122] In addition, when manufacturing a power storage device including the positive electrode 311 and the negative electrode illustrated in FIG. When graphene is formed on both the positive electrode 311 and the negative electrode by the method described in Embodiment 1, In this case, either the positive electrode 311 or the negative electrode is preliminarily grounded before assembling the power storage device. It is preferable to generate laphene in advance because both the positive electrode 311 and the negative electrode are oxidized. Even if the power storage device is assembled with the graphene provided, the positive electrode 311 and the negative electrode The graphene oxide is not sufficiently reduced because the potential cannot be supplied. This is because it takes time to be able to do so.

[0123] In addition, negative ions are produced by the LPCVD method using silane, silane chloride, silane fluoride, etc. as raw material gases. A negative electrode active material 221 (hereinafter, referred to as silicon) having a concave-convex shape is formed on a negative electrode current collector 201. It is possible to provide a whisker.

[0124] The silicon whiskers may be of an amorphous structure. By using it for the negative electrode active material layer 203, it is possible to prevent the volume change caused by the absorption and release of carrier ions. (For example, to relieve stress caused by volume expansion) The pulverization of the whiskers and the collapse of the negative electrode active material layer 203 can be prevented, and the cycle characteristics are further improved. It is possible to manufacture a highly improved power storage device.

[0125] Alternatively, the silicon whiskers may be crystalline. In this case, the electrical conductivity and carrier ions are improved. The crystalline structure, which has excellent crystallinity and ion mobility, is in contact with the current collector over a wide area. The conductivity of the entire negative electrode can be further improved, enabling faster charging and discharging. A power storage device with further improved discharge capacity can be manufactured.

[0126] Alternatively, the silicon whisker may have a core, which is a region having crystallinity, and a layer covering the core. , and an outer shell which is an amorphous region.

[0127] The amorphous structure of the outer shell is resistant to volume changes caused by the absorption and release of carrier ions (for example, In addition, the core has crystallinity, which is a characteristic of the material. The structure has excellent electrical conductivity and carrier ion mobility, and is capable of absorbing carrier ions. The core and shell have the characteristic that the speed and release rate are fast per unit mass. By using silicon whiskers with this property as the negative electrode active material layer, high-speed charging and discharging is possible. As a result, a power storage device with improved charge / discharge capacity and cycle characteristics can be manufactured.

[0128] Next, a method for assembling a power storage device of one embodiment of the present invention will be described. 1 is a cross-sectional view of a secondary battery 400, and the cross-sectional structure will be described below.

[0129] The lithium secondary battery 400 is a negative electrode comprising a negative electrode current collector 407 and a negative electrode active material layer 409. a positive electrode 405 constituted by a positive electrode current collector 401 and a positive electrode active material layer 403; The separator 413 is sandwiched between the positive electrode 405 and the positive electrode 405. The negative electrode current collector 407 is connected to an external terminal 419. The positive electrode current collector 401 is connected to an external terminal 417. The end of the external terminal 419 is provided with a gasket. That is, the external terminals 417 and 419 are embedded in the gasket 421. It is insulated.

[0130] The negative electrode current collector 407 and the negative electrode active material layer 409 are the same as those of the negative electrode current collector 201 and the negative electrode active material layer 409 described above. A layer 203 may be used as appropriate.

[0131] The positive electrode current collector 401 and the positive electrode active material layer 403 are the same as the positive electrode current collector 307 and The positive electrode active material layer 309 can be used as appropriate.

[0132] An insulating porous body is used for the separator 413. Representative examples of the separator 413 include: For example, paper, nonwoven fabric, glass fiber, ceramics, nylon (polyamide), vinyl Lon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, poly It is possible to use a material made of synthetic fibers using urethane. However, the electrolyte 415 It is necessary to choose materials that will not melt.

[0133] In addition, when a positive electrode having a spacer on a positive electrode active material layer is used as the positive electrode 405, The parameter 413 may not be provided.

[0134] The solute of the electrolyte 415 is a material capable of transporting carrier ions and having carrier ions. Representative examples of the solute are LiClO4, LiAsF6, LiBF4, and Li Lithium salts include iPF6 and Li(C2F5SO2)2N.

[0135] In addition, the carrier ions are alkali metal ions other than lithium ions, alkaline earth metal ions, etc. In the case of metal ions, beryllium ions, or magnesium ions, the solutes in the electrolyte 415 are In the above lithium salt, an alkali metal (e.g., sodium and potassium), alkaline earth metals (e.g., calcium, strontium, barium, etc. ), beryllium, or magnesium may also be used.

[0136] The solvent of the electrolyte 415 is a material that can transport carrier ions. The solvent for the solution 415 is preferably an aprotic organic solvent. Representative examples include ethylene carbonate, propylene carbonate, and dimethyl carbonate. diethyl carbonate, γ-butyrolactone, acetonitrile, dimethoxyethane, tetrahydrofuran, etc., and one or more of these can be used. By using a polymer material that gels as a solvent for liquid 415, safety, including leakage, is improved. In addition, the lithium secondary battery 400 can be made thinner and lighter. Representative examples of polymeric materials are silicone gel, acrylic gel, acrylonitrile gel, poly Examples include polyethylene oxide, polypropylene oxide, and fluorine-based polymers. As a solvent for the electrolyte 415, a flame-retardant and non-volatile ionic liquid (room-temperature molten salt) was used. By using multiple batteries, even if the internal temperature of the storage device rises due to an internal short circuit or overcharging, This can prevent the electricity storage device from exploding or catching fire.

[0137] In addition, a solid electrolyte such as Li3PO4 can be used as the electrolyte 415. The solid electrolyte is Li3PO4 mixed with nitrogen. x PO y N z (x, y, z are positive (real number), Li2S-SiS2, Li2S-P2S5, Li2S-B2S3, etc. The above-listed solid electrolytes can also be doped with LiI or the like. When a solid electrolyte is used as electrolytic solution 415, separator 413 is not necessary.

[0138] The external terminals 417 and 419 are made of metal members such as stainless steel plates and aluminum plates. There can be.

[0139] In this embodiment, the lithium secondary battery 400 is a button-type lithium secondary battery. The following shows the sealed lithium secondary battery, cylindrical lithium secondary battery, and square lithium secondary battery. Lithium secondary batteries of various shapes such as 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 3 The structure may be a structure in which a plurality of electrodes are stacked, or a structure in which a positive electrode, a negative electrode, and a separator are wound. stomach.

[0140] Lithium secondary batteries have a small memory effect, high energy density, and large capacity. In addition, the output voltage is high. These features make it possible to reduce the size and weight of the battery. There is little deterioration due to repeated use, so it can be used for a long period of time, and costs can be reduced.

[0141] The positive electrode 40 is produced by appropriately using the methods for producing the positive electrode and the negative electrode shown in the first embodiment and the second embodiment. 5 and the negative electrode 411 are prepared.

[0142] Next, the positive electrode 405 , the separator 413 , and the negative electrode 411 are immersed in an electrolyte solution 415 . Next, the positive electrode 405, the separator 413, the gasket 421, and the negative electrode 41 are connected to the external terminal 417. 1 and external terminal 419 are stacked in that order, and then external terminal 417 and external terminal 419 are crimped with a "coin crimping machine". By crimping the terminal 419, a coin-type lithium secondary battery can be produced.

[0143] In addition, between the external terminal 417 and the positive electrode 405, or between the external terminal 419 and the negative electrode 411 , a spacer, and a washer are inserted, and the external terminal 417 and the positive electrode 405 are connected, and the external The connection between the terminal 419 and the negative electrode 411 may be higher.

[0144] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0145] (Embodiment 3) A power storage device according to one embodiment of the present invention can be used as a power source for various electric devices driven by electric power. There can be.

[0146] Examples of electrical devices using a power storage device according to one embodiment of the present invention include a display device and a lighting device. , desktop or notebook personal computers, DVD (Digital Plays still images or videos stored on recording media such as a Versatile Disc. Image playback devices, mobile phones, portable game consoles, personal digital assistants, electronic books, video cameras, Digital still cameras, microwave ovens and other high-frequency heating devices, electric rice cookers, electric washing machines, air conditioners Air conditioning equipment such as conditioners, electric refrigerators, electric freezers, electric refrigerator-freezers, DNA storage Examples of such equipment include refrigerators, dialysis machines, etc. The moving object that propels the vehicle is also included in the category of electrical equipment. For example, electric vehicles, hybrid cars that combine internal combustion engines and electric motors, Examples include motorized bicycles, including electrically assisted bicycles.

[0147] The above electrical equipment is used as a power storage device (called the main power source) to cover almost all of the power consumption. The power storage device according to one embodiment of the present invention can be used for the electric device. When the power supply from the main power source or commercial power source is stopped, the power supply to the electrical equipment is As a power storage device that can be used for the above-mentioned purposes (referred to as an uninterruptible power supply), a power storage device according to one embodiment of the present invention is Alternatively, the electrical equipment can be supplied with power from the main power source or commercial power source. In parallel with the supply of power to the electric appliance, a power storage device (called an auxiliary power source) is used to supply power to the electric appliance. The power storage device according to one embodiment of the present invention can be used as the power storage device.

[0148] FIG. 7 shows a specific configuration of the above-mentioned electric device. In FIG. 7, the display device 5000 has a storage The display device 5000 is an example of an electrical device using the display device 5004. This corresponds to a display device for transmission and reception, and includes a housing 5001, a display unit 5002, a speaker unit 5003, The power storage device 5004 is provided inside the housing 5001. The power storage device according to one embodiment of the present invention is used as the power storage device 5004. The power supply device 5000 can receive power from a commercial power source, or can store power in a power storage device 5004. Therefore, when power is not supplied from the commercial power source due to a power outage, etc., Even when the power supply is not available, the power storage device 5004 can be used as an uninterruptible power supply to keep the display device 5000 running. will be available for use.

[0149] The display unit 5002 is a display device having a light emitting element such as a liquid crystal display device or an organic EL element in each pixel. Optical devices, electrophoretic displays, DMD (Digital Micromirror Devices) ice), PDP (Plasma Display Panel), FED (Field A semiconductor display device such as a 3D Emission Display can be used.

[0150] In addition, display devices are used for TV broadcast reception, personal computers, advertising displays, etc. This includes all display devices for displaying information, such as

[0151] In FIG. 7, a stationary lighting device 5100 is an electric device using a power storage device 5103. Specifically, the lighting device 5100 includes a housing 5101, a light source 5102, a power storage device The power storage device 5103 includes a power storage device according to one embodiment of the present invention. In FIG. 7, a power storage device 5103 is installed in a housing 5101 and a light source 5102. Although the case where the power storage device 5103 is provided inside a ceiling 5104 is illustrated, The lighting device 5100 may be provided inside the lighting device 5101. The power can be received or stored in the power storage device 5103 can be used. Therefore, even when power cannot be supplied from the commercial power source due to a power outage, the power storage device 5103 By using this as an uninterruptible power supply, the lighting device 5100 can be used.

[0152] In addition, FIG. 7 illustrates a lighting device 5100 that is installed on a ceiling 5104. However, in the power storage device of one embodiment of the present invention, for example, a side wall 5105, a floor 5106, and a ceiling 5104 are not included. 106, the window 5107, etc., or a tabletop lighting device. The present invention can also be used in lighting devices of this type.

[0153] In addition, the light source 5102 can be an artificial light source that artificially obtains light using electric power. Specifically, this applies to incandescent lamps, discharge lamps such as fluorescent lamps, and light-emitting diodes and organic electroluminescence (EL) elements. An example of the artificial light source is a light element.

[0154] In FIG. 7, an air conditioner having an indoor unit 5200 and an outdoor unit 5204 is as follows: The indoor unit 5200 is an example of an electric device using a power storage device 5203. 201, an air outlet 5202, a power storage device 5203, etc. In FIG. 7, a power storage device 5203 is used in an indoor unit 520. 5203 is provided in the outdoor unit 5204. Alternatively, both the indoor unit 5200 and the outdoor unit 5204 may be provided with a power storage device 5203. The air conditioner may be provided with a power supply from a commercial power source. In particular, the indoor unit can use the electric power stored in the power storage device 5203. When the power storage device 5203 is provided in both the outdoor unit 5200 and the outdoor unit 5204, Even when power cannot be supplied from a commercial power source, the power storage device 5203 can be used as an uninterruptible power source. By using this, it becomes possible to use the air conditioner.

[0155] In Figure 7, a separate type air conditioner consisting of an indoor unit and an outdoor unit is shown. As an example, an all-in-one air conditioner that has both indoor and outdoor unit functions in a single housing. The power storage device according to one embodiment of the present invention can also be used for the conditioner.

[0156] In FIG. 7, an electric refrigerator-freezer 5300 includes a power storage device 5304 according to one embodiment of the present invention. Specifically, an electric refrigerator-freezer 5300 includes a housing 5301, a refrigerator The storage compartment door 5302, the freezer compartment door 5303, the power storage device 5304, etc. In FIG. 7, a power storage device according to one embodiment of the present invention is used. The electric refrigerator-freezer 5300 is provided inside a housing 5301. The power can be supplied or stored in the power storage device 5304 can be used. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the power storage device 53 By using 04 as an uninterruptible power supply, it becomes possible to use the electric refrigerator-freezer 5300.

[0157] Among the above-mentioned electrical appliances, high-frequency heating devices such as microwave ovens and electric rice cookers Electrical appliances require high power for a short period of time. Therefore, they need to supplement the power that cannot be supplied by commercial power sources. By using a power storage device according to one embodiment of the present invention as an auxiliary power source for supporting This can prevent the commercial power breaker from tripping when using the device.

[0158] In addition, during periods when electrical equipment is not being used, the total amount of power that can be supplied by commercial power suppliers is also a concern. During periods when the ratio of the amount of electricity actually used (called the electricity usage rate) is low, By storing electricity in the electrical equipment, it is possible to prevent the power usage rate from increasing outside the above-mentioned time periods. For example, in the case of the electric refrigerator-freezer 5300, when the temperature is low, the refrigerator compartment door 53 02, during the night when the freezer door 5303 is not opened or closed, power is supplied to the power storage device 5304. Then, as the temperature rises, the refrigerator door 5302 and the freezer door 5303 are opened and closed. During the daytime, when the electricity is consumed, the power storage device 5304 is used as an auxiliary power source. The rate can be kept low.

[0159] Next, a portable information terminal including a power storage device of one embodiment of the present invention will be described with reference to FIGS. This will be explained with reference to FIG. 8(B) and FIG. 8(C).

[0160] Figures 8(A) and 8(B) show tablet terminals that can be folded in half. Figure 8(A) shows In the open state, the tablet terminal includes a housing 9630, a display unit 9631a, and a display unit 96 31b, a display mode changeover switch 9034, a power switch 9035, a power saving mode changeover switch It has a changeover switch 9036, a fastener 9033, and an operation switch 9038.

[0161] A part of the display unit 9631a can be used as a touch panel area 9632a. By touching the operation keys 9637 displayed on the display unit 96, data can be input. In 31a, as an example, half of the area has a display function only, and the other half The display unit 96 has a touch panel function, but is not limited to this. The entire area of ​​the display unit 931a may have a touch panel function. The entire surface of 631a is made to display keyboard buttons to serve as a touch panel, and the display section 9631b is made to display It can be used as a display screen.

[0162] In addition, in the display unit 9631b, as in the display unit 9631a, The part of the touch panel can be the area 9632b of the touch panel. Touch the area where the mode display switch button 9639 is displayed with your finger or a stylus. A keyboard button can be displayed on the display portion 9631b.

[0163] In addition, the touch panel area 9632a and the touch panel area 9632b are simultaneously You can also use touch input.

[0164] A display mode changeover switch 9034 is used to change the display orientation, such as vertical or horizontal. You can choose between black and white and color display. The 9036 is a tablet-type device that detects external light during use using a built-in light sensor. The tablet device has a light sensor, which can adjust the display brightness to suit the amount of light. In addition to the sensor, other detection devices such as gyro, acceleration sensor, etc. that detect the inclination are also included. It may be built-in.

[0165] FIG. 8A shows an example in which the display area of ​​the display portion 9631b is the same as that of the display portion 9631a. However, there is no particular limitation, and one size may be different from the other size. For example, one display panel may have a higher resolution than the other. It is also possible to use the following.

[0166] FIG. 8B shows the tablet terminal in a closed state. The tablet terminal includes a housing 9630 and a solar cell 96 33, a charge / discharge control circuit 9634, a battery 9635, and a DCDC converter 9636 In addition, in FIG. 8B, a battery 9635 is used as an example of the charge and discharge control circuit 9634. The configuration shown has a DC-DC converter 9636, and the battery 9635 is The power storage device according to one embodiment of the present invention is used.

[0167] In addition, since the tablet device can be folded in half, the case 9630 can be folded when not in use. Therefore, the display portions 9631a and 9631b can be protected. This makes it possible to provide a tablet device that is highly durable and reliable even when used for a long period of time.

[0168] In addition, the tablet terminals shown in Figs. 8(A) and 8(B) can display various information. Functions that display (still images, videos, text images, etc.), calendars, dates, or times, etc. A function to display information on the display unit, and a touch input function to operate or edit information displayed on the display unit Functions such as the ability to control processing using various software (programs) can be done.

[0169] The solar cell 9633 attached to the surface of the tablet device supplies power to the touch panel. The solar cell 9633 can supply the solar cell 9633 with the following components: The housing 9630 is configured to efficiently charge the battery 9635 on one or both sides. Note that the battery 9635 is preferably a battery storage device according to one embodiment of the present invention. The use of the device has the advantage of enabling miniaturization.

[0170] The configuration and operation of the charge / discharge control circuit 9634 shown in FIG. A block diagram is shown and explained in FIG. 8(C). , DC-DC converter 9636, converter 9638, switches SW1 to SW3, display The figure shows the part 9631, the battery 9635, the DCDC converter 9636, The inverter 9638 and the switches SW1 to SW3 are connected to the charge / discharge control circuit 96 shown in FIG. This corresponds to 34.

[0171] First, an example of operation in which power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell is converted to DC voltage to charge the Battery 9635. The voltage is increased or decreased by the DC converter 9636. When power is being used from the solar cell 9633, switch SW1 is turned on and the converter 9 In step 638, the voltage is increased or decreased to a voltage required for the display unit 9631. When not displaying on the 631, turn SW1 off and SW2 on to charge the battery. 635 may be configured to charge the battery.

[0172] The solar cell 9633 is shown as an example of a power generating means, but is not limited thereto. Other power generation methods such as piezoelectric elements and thermoelectric conversion elements (Peltier elements) For example, the battery 9635 may be charged. A non-contact power transmission module that receives and charges, or a structure that combines other charging methods It may also be composed of.

[0173] In addition, if the power storage device described in the above embodiment is provided, the electric device shown in FIG. It goes without saying that there is no particular limitation.

[0174] This embodiment mode can be implemented in appropriate combination with other embodiment modes. EXAMPLES

[0175] In this embodiment, a lithium secondary battery (referred to as lithium secondary battery 1) is manufactured by using one embodiment of the present invention. The lithium secondary battery 1 was subjected to cyclic voltammetry. c Voltammetry (CV) was measured.

[0176] First, the structure and manufacturing method of the lithium secondary battery 1 will be described.

[0177] The lithium secondary battery 1 is a coin-type lithium secondary battery. As a result, LiFePO4 and graphene oxide were deposited on a current collector made of aluminum. The electrode used had an active material layer that was made of lithium metal. A polypropylene sheet was used as the separator. 1M electrolyte was used. LiPF6 (ethylene carbonate solvent) and diethyl carbonate were mixed in a 1:1 (volume ratio) ) was used.

[0178] Here, a method for producing the working electrode will be described.

[0179] <Synthesis method of LiFePO4> Lithium carbonate (Li2CO3), iron oxalate (Fe2CO4·2H2O), and ammonium dihydrogen phosphate (NH4H2PO4), which are raw materials, were weighed in a molar ratio of 1:2:2. Next, using a wet ball mill with a rotation speed of 300 rpm (ball diameter 3 mm, using acetone as the solvent), the raw materials were pulverized and mixed for 2 hours, and then dried.

[0180] Next, heating was performed in a nitrogen atmosphere at 350 °C for 10 hours to perform preliminary firing of the pulverized and mixed raw materials. After that, again using a wet ball mill with a rotation speed of 300 rpm (ball diameter 3 mm, using acetone as the solvent), pulverization and mixing were performed for 2 hours. Then, firing was performed in a nitrogen atmosphere at 600 °C for 10 hours to obtain LiFePO4.

[0181] <Synthesis method of graphene oxide> 2 g of graphite and 92 ml of concentrated sulfuric acid were mixed to produce mixture A. Next, while stirring in an ice bath, 12 g of potassium permanganate was added to mixture A to produce mixture B. Next, the ice bath was removed, and after stirring at room temperature for 2 hours, it was left standing at 35 °C for 30 minutes to oxidize the graphite and obtain mixture C having graphene oxide.

[0182] Next, while stirring in an ice bath, 184 ml of water was added to mixture C to obtain mixture D. Next, in an oil bath at approximately 98 °C, mixture D was stirred for 15 minutes to react. Then, while stirring, 580 ml of water and 36 ml of hydrogen peroxide solution (concentration 30 wt%) were added to mixture D to reduce the unreacted potassium permanganate and obtain mixture E having soluble manganese sulfate and graphene oxide.

[0183] Next, the mixture E was filtered by suction using a membrane filter with a pore size of 0.45 μm. After obtaining precipitate A, precipitate A was mixed with 3 wt% hydrochloric acid to add manganese ions to the mixture. Mixture F containing dissolved potassium ions and sulfate ions was obtained. Mixture F was then filtered under suction. After filtration, precipitate B containing graphite oxide was obtained.

[0184] Precipitate B was mixed with 500 ml of water to obtain mixed solution G, which was then subjected to a 40 kHz frequency test. Ultrasonic waves of 1000 nm were applied for 1 hour to peel off the carbon layers that make up the graphite oxide. Laphene was produced.

[0185] Next, the mixture was centrifuged at 4000 rpm for approximately 30 minutes, and the supernatant containing graphene oxide was The supernatant was collected as mixed solution H.

[0186] Next, add ammonia water to the mixture H to adjust the pH to approximately 11, and mix I After that, 2500 ml of acetone was added to the mixed solution I and mixed to obtain mixed solution J. At this time, the graphene oxide contained in the mixed solution H was dissolved in the ammonia contained in the ammonia water. The graphene oxide reacts with the ammonium salt of graphene oxide, which is mixed with the graphene oxide. Precipitation occurred in the combined solution J.

[0187] Mixture J was filtered, and the precipitate of mixture J was dried in vacuum at room temperature to obtain graphene oxide salt. Recovered.

[0188] <Method of Producing Active Material Layer> The mixture is made up of 97wt% LiFePO4 and 3wt% graphene oxide salt, with the total weight of these being approximately Mix with 2 times the amount of NMP (N-methylpyrrolidone) to form a paste. After that, the paste was applied onto an aluminum current collector and heated at 120°C for 15 minutes. After drying through ventilation, the current collector is heated to 100°C and vacuum dried for 1 hour. A working electrode having an active material layer thereon was prepared.

[0189] Next, a procedure for assembling the lithium secondary battery 1 will be described. First, the inside of the first battery can A working electrode soaked in an electrolyte is placed on the separator, which is also soaked in an electrolyte, and the separator is placed on the working electrode. A gasket was placed on the separator. Then, lithium gold was applied to the separator and the gasket. The metal was placed on the lithium electrode, and a spacer and a spring washer were placed on the lithium electrode. After placing the second battery can on the ring washer, the first battery can is crimped to secure the lithium A secondary battery 1 was fabricated.

[0190] Next, the CV measurement was performed on the lithium secondary battery 1. The sweep rate was set to 1 mV / s. In the first step, the sweep potential is set to 3-4V, and the applied potential is swept from 3V to 4V. After that, the process of sweeping from 4V to 3V was repeated four times. Next, as the second step, ,The sweep potential is 1.5-3V, and the applied potential is swept from 3V to 1.5V, and then 1. The process of sweeping from 5 V to 3 V was repeated four times. Next, in the third step, the sweep voltage The potential was set to 3 to 4 V, and the potential was swept from 3 V to 4 V, and then from 4 V to 3 V. The process of sweeping the potential at 400 V was repeated four times. The current-potential curves obtained at this time are shown in FIG.

[0191] In FIG. 9, the horizontal axis represents the potential of the working electrode (vs. Li / Li + ), and the vertical axis represents the amount of oxidation The current generated by the element is shown. Note that a negative current value indicates a reduction current, and a positive current value indicates The oxidation current is shown.

[0192] The current having a peak current surrounded by the dashed line 501_R is the reduction current in the first step. The current having a peak current surrounded by the dashed line 501_O is the oxidation current in the first step. The current having a peak current surrounded by the dashed line 502_R is the first current in the second step. The current indicated by the dashed line 502 is the reduction current during the second to fourth potential sweeps of the second step. The reduction current in the th potential sweep and the oxidation current in the 1st to 4th potential sweeps are shown in the dashed line. The current with a peak current surrounded by 503_R is the reduction current of the third step, and the dashed line The current having a peak current surrounded by 503_O is the oxidation current of the third step.

[0193] Between the first and third steps, a potential sweep from 1.5V to 3V was performed. It can be seen that the current value of the lithium secondary battery 1 increased. The resistance of the active material layer is reduced by a reduction process, i.e., an electrochemical reduction process, by supplying a potential that promotes the reduction of the active material layer. In the third step, the current value increased. Considering that the redox potential of the LiFePO4 contained in it is about 3.4V, The reduction current around 2 V is the current that occurs when graphene oxide is reduced. It can be said that the reduction potential of graphene is about 2V.

[0194] Next, an enlarged view of the current-potential curve in the second step in FIG. 9 is shown in FIG.

[0195] In FIG. 10, curve 511_R indicates the reduction current during the first potential sweep, and curve 511 Curve 512_O indicates the oxidation current during the first potential sweep. Curve 512_R indicates the oxidation current during the second to fourth potential sweeps. The curve 512_O shows the reduction current during the potential sweep, and the curve 512_O shows the oxidation current during the second to fourth potential sweeps. Indicates the flow.

[0196] As shown in Fig. 10, the reduction current in the first potential sweep peaked at around 2 V. However, a peak appears around 2 V in the second and subsequent potential sweeps. In addition, there is no significant change in the oxidation current in the first to fourth potential sweeps.

[0197] From the above, it can be seen that a reduction reaction occurs at the working electrode by sweeping the reduction potential around 2V. However, it was found that the reduction reaction did not occur in the second and subsequent potential sweeps.

[0198] Here, in order to confirm the reduction reaction occurring around 2 V, graphene oxide A comparative battery cell having only the active material layer of the working electrode was prepared, and the CV of the comparative battery cell was measured. did.

[0199] First, the structure and manufacturing method of the comparative battery cell will be described.

[0200] The comparative battery cell is a coin-type battery. The current collector is made of aluminum. The structure is the same as that of lithium secondary battery 1, except that only graphene oxide is used for the active material layer of the electrode. It is made of.

[0201] In addition, the graphene oxide is the same as the graphene oxide used in the active material layer of the working electrode of the lithium secondary battery 1. It was produced by a process similar to that of laphene.

[0202] In addition, 50 mg of graphene oxide was mixed with 4.5 g of water to form a paste, which was then The paste is applied onto a current collector made of aluminum, and dried in a vacuum at 40°C to form a collector. A working electrode having an active material layer on a conductive body was prepared.

[0203] The procedure for assembling the comparative battery cell is the same as that for the lithium secondary battery 1.

[0204] Next, the comparative battery cell was subjected to CV measurement. The sweep rate was set to 0.1 mV / s. The sweep potential was The voltage was set to 1.5 to 3 V, and the voltage was swept from 3 V to 1.5 V, and then from 1.5 V to 3 V. The process of sweeping from 0 to 1000 volts was repeated three times. The potential-current curves obtained at this time are shown in FIG.

[0205] In FIG. 11, the horizontal axis represents the potential of the working electrode (vs. Li / Li + ) and the vertical axis indicates the oxidation The current generated by reduction is shown. Curve 531_R is the reduction current during the first potential sweep. The curve 531_O represents the oxidation current during the first potential sweep, and the curve 532_R represents the oxidation current during the second potential sweep. Curve 532_O represents the reduction current during the first potential sweep, and curve 532_O represents the oxidation current during the second potential sweep. Curve 533_R represents the reduction current during the third potential sweep, and curve 533_O represents the reduction current during the third potential sweep. The oxidation current during potential sweep is shown.

[0206] As shown in Fig. 11, the reduction current in the first potential sweep peaked at around 2 V. This also shows that the reduction potential of graphene oxide is about 2V. However, no peak is observed near 2 V in the second and subsequent potential sweeps. The oxidation currents in the second and third potential sweeps are higher than those in the first potential sweep. However, there is no significant change in the oxidation current in the second and third potential sweeps.

[0207] Next, the carbon and oxygen in the working electrode of the comparative battery cell were measured before and after the electrochemical reduction treatment. The surface elemental composition and atomic bonding state of the , and other elements were analyzed by X-ray photoelectron spectroscopy. (XPS: X-ray Photoelectron Spectroscopy) The results of the analysis are shown in Figures 12 and 13.

[0208] The graphene oxide-containing mixed solution H described in the process of preparing the working electrode of the lithium secondary battery 1 was The sample placed on an aluminum substrate and heated in a vacuum at 40°C for 1 hour is designated as sample 1. In addition, the sample 1 is immersed in the electrolyte contained in the lithium secondary battery 1 for one day, and then The sample was washed with diethyl ether and dried in vacuum at room temperature for 3 hours to obtain sample 2. Samples 1 and 2 are samples before electrochemical reduction treatment. In addition, a comparative battery cell was prepared. After one CV measurement, the working electrode of the comparative battery cell was disassembled and then soaked in diethyl carbonate. The sample was washed with and dried in vacuum at room temperature for 3 hours to obtain sample 3.

[0209] On the other hand, instead of reducing graphene oxide by electrochemical reduction treatment, The graphene was produced by thermal reduction of graphite. The material was used as a comparative example.

[0210] The graphene oxide-containing mixed solution H described in the process for preparing the working electrode of the lithium secondary battery 1 was The sample in which the dried powdered graphene oxide was provided on an indium foil was designated Comparative Example 1. In addition, Comparative Example 1 was heated in a vacuum at 300° C. for 10 hours to reduce the graphene oxide. The sample in which the graphene obtained was provided on the indium foil is referred to as Comparative Example 2. The sample in which indium powder was provided on an indium foil was used as Comparative Example 3.

[0211] The surface elemental compositions of Samples 1 to 3 and Comparative Examples 1 to 3 were determined by X-ray photoelectron spectroscopy. The results of the composition analysis are shown in Figure 12.

[0212] In FIG. 12, when comparing sample 1 and sample 2 with sample 3, the oxygen ratio in sample 3 is The amount of carbon in the SiO2 solution decreased, while the amount of carbon in the SiO2 solution increased. The oxygen content of Sample 3 was 14.8 atomic %. It was found that the oxygen ratio was reduced in Comparative Example 2. The oxygen content of Comparative Example 2 was 13.4 atomic %. From these results, the oxidation graph It was found that graphene oxide was reduced by electrochemical reduction of graphene. It was also found that graphene oxide was reduced by thermal reduction.

[0213] Next, the surfaces of Samples 1 to 3 and Comparative Examples 1 to 3 were analyzed by X-ray photoelectron spectroscopy. The results of analyzing the bonding states of nearby atoms are shown in FIG.

[0214] FIG. 13 shows the relationship between C═C in Samples 1 to 3 and Comparative Examples 1 to 3. sp 2 C sp bonds, CC, CH etc. 3 bond, CO bond, C=O bond, CO2 bond 1 is a graph showing the evaluation of the proportions of (O=CO bond), and CF2 bond.

[0215] When comparing Sample 1 and Sample 2 with Sample 3, the sp 2 The proportion of bonds increases, and the sp bonds of C such as CC and CH 3 bond, CO bond, C=O bond, It was found that the ratio of CO2 bonds was decreased. By sp 3 The bond, CO bond, C=O bond, and CO2 bond react, forming sp 2 The bond It was found that sp 2 The binding was 67.2%.

[0216] On the other hand, when comparing Comparative Example 1 and Comparative Example 2, similar to Sample 3, in Comparative Example 2, sp 2 The binding is increased, but compared to sample 3, sp 2 The amount of binding is low. p 2 The bond was 44.1%. In other words, the electrochemical reduction treatment resulted in the sp 2 It was found that the binding rate was more than 50% and less than 70%.

[0217] From the above, in Figs. 11 to 13, by sweeping the reduction potential around 2V, Graphene is reduced to sp 2 It was found that graphene with many bonds was produced. 10 and 12, the resistance of the active material layer is reduced by sweeping the reduction potential around 2 V. It was found that it is possible to increase the current value of a lithium secondary battery. From the analysis results of 3, it was found that the reduction in resistance was due to the electrochemical reduction of the low-conductivity graphite oxide. This is thought to be due to the production of highly conductive graphene from phene. EXAMPLES

[0218] In this example, the reduction of graphene oxide was measured using a measurement system that excluded electrode resistance components. The electric potential will now be described.

[0219] The graphene oxide-containing electrode prepared by the method shown in Example 1 has a layered structure of graphene oxide. It can be said that the resistance of the entire electrode is increased by this.

[0220] In this embodiment, graphene oxide is loosely attached to the electrode, and the graphene oxide is laminated. The reduction potential of graphene oxide was measured using a measurement system that eliminated the resistance components generated by the

[0221] Specifically, the working electrode is glassy carbon, the counter electrode is platinum, and the solvent is water. The graphene oxide was dispersed in a graphene oxide dispersion at a ratio of 0.0027 g / L. A voltage of 10 V was applied to the working electrode and the counter electrode for 30 seconds. The glassy carbon with graphene oxide attached was vacuum dried. The graphene oxide electrode A is made of the graphene oxide. was prepared in the same manner as in Example 1.

[0222] In this way, by electrophoresis in a graphene oxide dispersion while controlling the conditions, By sparsely attaching graphene oxide to the glassy carbon working electrode, This can be done.

[0223] Next, the graphene oxide electrode A was used as the working electrode, platinum as the counter electrode, and lithium as the reference electrode. CV measurements were performed. The electrolyte used in the CV measurements was a 1:1 mixture of EC and DEC. A solution of 1M LiPF6 dissolved in the mixed solvent was used.

[0224] In the CV measurement, the sweep speed was set to three conditions, Condition 1 to Condition 3. Condition 1 The sweep speed is 10 mV / s in condition 1. The sweep speed is 50 mV / s in condition 2. Condition 3 The sweep rate was 250 mV / s. The potential range swept was the same for all conditions 1 to 3. The potential is swept from the low potential side in the range of 1.8 V to 3.0 V from the immersion potential. The potential was swept back and forth three times.

[0225] The CV measurement results under conditions 1 to 3 are shown in FIGS. 15(A), (B) and 16(A). FIG. 15(A) shows the results under condition 1, FIG. 15(B) shows the results under condition 2, and FIG. 16(A) shows the results under condition 3. The results are for condition 3. Figure 16(B) shows the results for the case where only glassy carbon was used as the working electrode. CV measurement results for the comparative example. The CV measurement for the comparative example was performed under the same conditions except that the potential was swept twice. 15 and 16, the horizontal axis represents the potential of the working electrode (vs. Li / Li + ) and the vertical axis represents the current generated by oxidation-reduction.

[0226] As shown in FIG. 16B, the comparative example in which graphene oxide was not attached to the working electrode had a voltage of 1.8 V or higher. It was found that no redox reaction was observed within the range of 3.0 V.

[0227] On the other hand, the graphene oxide electrode A to which the graphene oxide was attached under conditions 1 to 3 was Only in the second potential sweep, peaks were observed at 2.3 V and 2.6 V as irreversible reduction reactions. In the second and third potential sweeps, the peak was not observed, as in the comparative example. No defects were observed (see Figures 15(A) and (B) and Figure 16(A)).

[0228] In addition, under conditions 1 to 3, the magnitude of the current flowing through the measurement system according to the potential sweep speed However, the position of the peak did not depend on the potential sweep rate and was about 2.3 V under all conditions. It was found that the voltage was about 2.6V.

[0229] From the above, the peaks confirmed at 2.3 V and 2.6 V correspond to the reduction reaction of graphene oxide. This can be said to be the corresponding peak.

[0230] As described above, in one embodiment of the present invention, a potential at which a reduction reaction of graphene oxide occurs is supplied. It was confirmed that graphene can be produced by this method. [Explanation of symbols]

[0231] S111 Step S112 Step S121 Step S122 Step S123 Step S124 Step S125 Step S126 Step S127 Step 113 Container 114 Electrolyte 115 Conductive Layer 116 Opposite 201 Negative electrode current collector 203 Negative electrode active material layer 205 Negative electrode 211 Anode active material 213 Graphene 221 Negative electrode active material 221a Common area 221b Convex 223 Graphene 307 Positive electrode current collector 309 Positive electrode active material layer 311 Positive electrode 321 Cathode active material 323 Graphene 400 Lithium secondary battery 401 Positive electrode current collector 403 Positive electrode active material layer 405 Positive electrode 407 Negative electrode current collector 409 Negative electrode active material layer 411 Negative electrode 413 Separator 415 Electrolyte 417 External terminal 419 External terminal 421 Gasket 501_O dashed line 501_R dashed line 502 dashed line 502_R dashed line 503_O dashed line 503_R dashed line 511_O curve 511_R curve 512_O curve 512_R curve 531_O curve 531_R curve 532_O curve 532_R curve 533_O curve 533_R curve 5000 display devices 5001 Case 5002 Display section 5003 Speaker section 5004 Electricity storage device 5100 Lighting equipment 5101 Case 5102 Light source 5103 Energy storage devices 5104 Ceiling 5105 Side wall 5106 Bed 5107 Windows 5200 indoor unit 5201 Case 5202 Ventilator 5203 Energy storage devices 5204 Outdoor unit 5300 Electric refrigerator-freezer 5301 Case 5302 Refrigerator door 5303 Freezer door 5304 Energy storage devices 9630 Case 9631 Display section 9631a Display section 9631b Display section 9632a Touch Panel Area 9632b Touch Panel Area 9033 Fastener 9034 Display mode switch 9035 Power Switch 9036 Power saving mode switch 9038 Operation switch 9639 Keyboard display switch button 9633 Solar Cells 9634 Charge / discharge control circuit 9635 Battery 9636 DC-DC Converter 9637 Operation key 9638 Converter

Claims

1. A lithium secondary battery comprising a positive electrode and a negative electrode, the positive electrode includes a positive electrode active material and a first multilayer graphene having a region covering the positive electrode active material, the negative electrode includes a negative electrode active material and a second multilayer graphene having a region covering the negative electrode active material, In each of the first multilayer graphene and the second multilayer graphene, a carbon ratio is 80 atomic % or more and less than 90 atomic %, an oxygen ratio is 10 atomic % or more and less than 20 atomic %, and a ratio of the carbon forming sp 2 bonds is 50 atomic % or more and 80 atomic % or less as a result of measurement by X-ray photoelectron spectroscopy. Lithium secondary battery.

2. A lithium secondary battery comprising a positive electrode and a negative electrode, The positive electrode includes a positive electrode active material and a first multilayer graphene having a region that covers the periphery of the positive electrode active material, the negative electrode includes a negative electrode active material and a second multilayer graphene having a region covering the periphery of the negative electrode active material, In each of the first multilayer graphene and the second multilayer graphene, a carbon ratio is 80 atomic % or more and less than 90 atomic %, an oxygen ratio is 10 atomic % or more and less than 20 atomic %, and a ratio of the carbon forming sp 2 bonds is 50 atomic % or more and 80 atomic % or less as a result of measurement by X-ray photoelectron spectroscopy. Lithium secondary battery.

3. A lithium secondary battery comprising a positive electrode and a negative electrode, The positive electrode includes a positive electrode active material and a first multilayer graphene encapsulating the positive electrode active material, the negative electrode includes a negative electrode active material and a second multilayer graphene encapsulating the negative electrode active material, In each of the first multilayer graphene and the second multilayer graphene, a carbon ratio is 80 atomic % or more and less than 90 atomic %, an oxygen ratio is 10 atomic % or more and less than 20 atomic %, and a ratio of the carbon forming sp 2 bonds is 50 atomic % or more and 80 atomic % or less as a result of measurement by X-ray photoelectron spectroscopy. Lithium secondary battery.

4. In any one of claims 1 to 3, The positive electrode active material is LiFeO 2 , LiCoO 2 , LiNiO 2 , or LiMn 2 O 4 A lithium secondary battery comprising:

5. In any one of claims 1 to 4, The negative electrode active material comprises one selected from the group consisting of lithium, aluminum, graphite, silicon, tin, and germanium.

6. In any one of claims 1 to 4, The negative electrode active material comprises a compound containing one or more elements selected from the group consisting of lithium, aluminum, graphite, silicon, tin, and germanium.

Citation Information

Patent Citations

  • Stable dispersion of single and multiple graphene layers in solution

    JP2010275186A

  • Graphene manufacturing method

    JP2011500488A

  • Flexible asymmetric electrochemical cells using nano graphene platelet as an electrode material

    US20110183180A1

  • Electrophoretic deposition and reduction of graphene oxide to make graphene film coatings and electrode structures

    US20110227000A1

  • Lithium iron phosphate positive electrode active material modified by graphene, preparation method and lithium ion secondary battery thereof

    WO2011069348A1