Welding method and can body manufacturing method
The welding method for plate materials with bent portions stabilizes the welding process by restricting movement and enhancing heat transfer, addressing misalignment and shifting issues to achieve high-quality and efficient welding.
Patent Information
- Application Number
- JP2023002519
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-01-11
AI Technical Summary
Existing welding methods for thin and lightweight plate materials, such as those used in hot water storage tanks, fail to prevent misalignment and shifting during the welding process, which compromises welding quality and productivity.
A welding method involving a first plate material with a first bent portion and a second plate material with a flare bent portion, where the bent portions are in contact and heated from the outside in the radial direction, restricting movement and stabilizing the welding process.
The method effectively prevents misalignment and shifting of plate materials during welding, ensuring stable welding quality and improved productivity by using the bent portions to restrict movement and facilitate heat transfer.
Smart Images

Figure 0007573203000001 
Figure 0007573203000002 
Figure 0007573203000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a welding method and a method for manufacturing a can body. [Background technology]
[0002] Patent Document 1 discloses a welding method that can reduce misalignment between plate materials when welding the two plate materials together. This welding method involves bringing the L-shaped ends of two plate materials into contact with each other, and then providing a gap between the L-shaped end of the second plate material and the eaves portion of the first plate material, so that the gap absorbs the misalignment between the plate materials. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-148304 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a welding method in which plate materials are less likely to shift during welding, and a method for manufacturing a can body. [Means for solving the problem]
[0005] A welding method according to the present disclosure is a welding method for joining a first plate material and a second plate material, wherein the first plate material has a cylindrical first surface portion and a first end portion which is an end of the first surface portion, the second plate material has a cylindrical second surface portion and a second end portion which is an end of the second surface portion, the first end portion has a first bent portion which rises at an acute angle radially outwardly of the first surface portion and a second bent portion which bends in the opposite direction to the first bent portion at a tip side of the first end portion relative to the first bent portion, and the second end portion has a flared bent portion which rises at an obtuse angle radially outwardly of the second surface portion, and the first bent portion, the second bent portion, and the flared bent portion are in contact with each other inside the bend between the first bent portion and the second bent portion, and the second bent portion is heated from the radially outwardly of the second bent portion to weld the first end portion and the second end portion. Effect of the Invention
[0006] In the welding method and can body manufacturing method of the present disclosure, the flare bent portion comes into contact with the second bent portion and the first bent portion, which makes it difficult for the plates to slip apart during welding. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a perspective view of a can body according to a first embodiment; [Diagram 2] 1 is a cross-sectional view of a can body according to a first embodiment. [Diagram 3] Enlarged view of Fig. 2 [Figure 4] FIG. 1 is a cross-sectional view of a head plate and a body in a state where they are set in a welding device according to the first embodiment; [Diagram 5] Enlarged view of Fig. 4 [Figure 6] 1 is a cross-sectional view of the head plate and the fuselage after pressing in accordance with the first embodiment; [Figure 7] Enlarged view of Fig. 6 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] (The knowledge and other information that formed the basis of this disclosure) At the time when the inventors came to this disclosure, the technology of the welding method between plate materials was in a state where both ensuring the quality of the welding and improving productivity were required. Therefore, in the industry, a technology was proposed to reduce the misalignment between the plate materials by deforming the ends of the plate materials as described in Patent Document 1, with the aim of improving the quality and productivity of the welding. Under such circumstances, the inventors discovered that when a gap as described in Patent Document 1 is provided, while the gap acts as a buffer to absorb the misalignment, there is a problem that it can cause the plate materials to be misaligned when aligned or welded. In particular, a thin-walled body and a head plate that are easily bent are sometimes adopted for the hot water storage tank of a hot water supply device, which requires a thin-walled, lightweight tank from the standpoint of environmental consideration and cost. When such a body and a head plate are welded, the plate materials are more likely to be misaligned with each other in the conventional welding method as described in Patent Document 1. Therefore, in order to solve this problem, the inventors have come to constitute the subject of the present disclosure. Therefore, the present disclosure provides a welding method that prevents plate materials from shifting from each other during welding.
[0009] Hereinafter, the embodiments will be described in detail with reference to the drawings. However, more detailed description than necessary may be omitted. For example, detailed description of already well-known matters or duplicate description of substantially the same configuration may be omitted. It should be noted that the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present disclosure, and are not intended to limit the subject matter described in the claims.
[0010] (Embodiment 1) Hereinafter, the first embodiment will be described with reference to FIGS. [1-1. Structure of the can body] Fig. 1 is a perspective view of a can body 1 manufactured using the welding method of the present disclosure. Fig. 2 is a cross-sectional view of the can body 1 cut along an axis AX. The axis AX in the figure is an axis passing through the center of the cylindrical shape formed by the first surface portion 11 and the second surface portion 21. The can body 1 is a generally cylindrical container and is used as a hot water storage tank for a hot water supply system. The can body 1 has two generally hemispherical end plates (first plate material) 10 and a cylindrical body (second plate material) 20. The can body 1 is manufactured by joining the end plates 10 and the body 20, each formed as an individual plate material, by arc welding.
[0011] The head plate 10 is a metal plate having a cylindrical first surface portion 11 and a dome-shaped dome portion 19. The thickness of the first surface portion 11 is a plate thickness T1. In this embodiment, the metal constituting the head plate 10 is stainless steel. The head plate 10 is work-hardened by processing during manufacturing, and has a higher rigidity than the body 20.
[0012] The body 20 is a metal plate having a cylindrical second surface portion 21. The second surface portion 21 is oriented along the first surface portion 11, and their respective axes AX coincide. The thickness of the second surface portion 21 is a plate thickness T2. The inner diameter D2 of the second surface portion 21 is equal to the inner diameter D1 of the first surface portion 11. In this embodiment, the metal constituting the body 20 is stainless steel.
[0013] In the can body 1, a bead 30 is formed between a first end 13 which is an end of the first surface portion 11 and a second end 23 which is an end of the second surface portion 21. The bead 30 is a portion of the first end 13 and the second end 23 which were present before welding and which solidified after being melted by welding.
[0014] Fig. 3 is an enlarged view of a bead 30 in the cross-sectional view of Fig. 2. As shown in Fig. 3, in the can body 1 of the first embodiment, the first surface 11 and the second surface 21 are arranged at the same position in the radial direction. The cross-sectional shape of the bead 30 connecting the head plate 10 and the body 20 is a flat shape with little bulge in the radial direction. When the bead 30 has such a flat shape, stress concentration in the bead 30 is reduced. The radially outward direction DO is the direction from the inside to the outside of the radial direction of the cylindrical shape formed by the first surface 11 and the second surface 21.
[0015] [1-2. Manufacturing method of can body] Next, a method for manufacturing the above-mentioned can body 1 by welding the head panel 10 and the body 20 together will be described. [1-2-1. Pre-welding process] Fig. 4 is a cross-sectional view of the head plate 10 and the body 20 when set in the welding device W, showing a cross-section of the head plate 10 and the body 20 cut vertically along the axis AX. Fig. 5 is an enlarged view of Fig. 4, showing the first end 13 and the second end 23.
[0016] As shown in FIG. 4, the welding device W has a clamp W1 and two torches W2. The clamp W1 holds two end plates 10 aligned in the direction of the axis AX, and holds the body 20 between the two end plates 10. At this time, the axis AX is horizontal. The clamp W1 is movable in the direction of the axis AX of the first surface portion 11 and the second surface portion 21. The clamp W1 is also rotatable in the circumferential direction of the first surface portion 11 and the second surface portion 21 around the axis AX of the first surface portion 11 and the second surface portion 21. The torch W2 is a device that generates heat by arc discharge and performs welding by the generated heat. The torch W2 is provided near the first end portion 13 and the second end portion 23, and performs arc discharge vertically from above to below. Also, as shown in FIG. 4, the welding device W may be configured to have a ring-shaped jig W3 that fixes the center of the body 20. The jig W3 is a tool that fastens and fixes substantially the entire circumference of the body 20 from the radially outward direction DO side, and is rotatable around the axis AX in the circumferential direction of the first surface portion 11 and the second surface portion 21. The jig W3 prevents the body 20, which has a lower rigidity than the head plate 10, from bending and deforming. The jig W3 also makes it easier to position the body 20 relative to the head plate 10.
[0017] As shown in Fig. 5, a first bent portion 15 rising radially outward and a second bent portion 17 bending in the opposite direction to the first bent portion 15 are formed in the first end portion 13 of the head plate 10 before welding. The first bent portion 15 is formed rising in a direction such that the bending angle between the first surface portion 11 and the first bent portion 15 is angle A1, and has a substantially linear shape in the cross section of Fig. 5. The angle A1 is an acute angle. The first bent portion 15 is formed around the entire circumference of the first end portion 13.
[0018] The second bent portion 17 is formed closer to the tip 13a of the first end portion 13 than the first bent portion 15, and has a substantially linear shape in the cross-sectional view of FIG. 5. The second bent portion 17 is bent in a direction such that the bending angle between the second bent portion 17 and the first bent portion 15 is angle A2. In this embodiment, angle A2 is an acute angle and is equal to angle A1. Therefore, the second bent portion 17 extends along the first surface portion 11 and has a cylindrical shape parallel to the axis AX. In addition, the second bent portion 17 is perpendicular to the radially outward direction DO.
[0019] A curved first corner portion 14 is formed between the portion of first end portion 13 along first surface portion 11 and first bent portion 15. First corner portion 14 is a fold formed by the process of forming first bent portion 15, and is a rounded corner.
[0020] Further, a curved second corner portion 16 is formed between the first bent portion 15 and the second bent portion 17. The second corner portion 16 is a fold formed by the process of forming the second bent portion 17, and is a rounded corner.
[0021] Before welding, the second end 23 has a flat shape and extends in the direction of the axis AX and parallel to the second surface portion 21. Therefore, the thickness of the second end 23 is the plate thickness T2, similar to the second surface portion 21. In addition, a flat end face 23a is formed at the tip of the second end 23 and is approximately perpendicular to the second end 23. The end face 23a faces the first corner portion 14 of the first end 13.
[0022] 4 and 5, after the head plates 10 and the body 20 are completely set on the welding device W, the welding device W applies pressure by moving the clamps W1 in a direction in which the two head plates 10 press against each other in the direction of the axis AX. As a result, the head plates 10 and the body 20 are strongly pressed against each other along the direction of the axis AX.
[0023] Fig. 6 is a cross-sectional view of the head 10 and body 20 in the state set in the welding device W after pressure is applied, showing a cross section of the head 10 and body 20 cut vertically along the axis AX. Fig. 7 is an enlarged view of Fig. 6, showing the first end 13 and the second end 23. Fig. 6 shows the pressure direction of the clamp W1.
[0024] As shown in Figures 6 and 7, in this embodiment, the clamp W1 moves and the head 10 and the body 20 are pressed firmly against each other along the direction of the axis AX, thereby forming a flare bend portion 25 at the second end 23.
[0025] Flare bent portion 25 is formed by pressing first corner portion 14 and first bent portion 15 firmly against end face 23a of second end portion 23 by applying pressure, and is raised from second surface portion 21 in radially outward direction DO. Flare bent portion 25 is raised in a direction such that the angle between itself and second surface portion 21 is angle A3. Angle A3 is an obtuse angle. In this embodiment, the sum of angle A1 and angle A3 is equal to or greater than 180°.
[0026] When the flare bent portion 25 is formed, the end face 23a moves radially outward while sliding on the outer side surface 14a, which is the outer surface of the curve of the first corner portion 14, and the inner side surface 15a, which is the inner surface of the bend between the first bent portion 15 and the second bent portion 17 of the first bent portion 15. The radially outward movement of the end face 23a stops when it comes into contact with the inner side surface 17a, which is the inner surface of the bend between the first bent portion 15 and the second bent portion 17 of the second bent portion 17. For this reason, in this embodiment, the end face 23a of the second end portion 23, which is the tip of the flare bent portion 25, makes line contact with the inner sides 15a, 17a of the first bent portion 15 and the second bent portion 17 in the circumferential direction.
[0027] In this embodiment, the radius of curvature of inner surface 16a, which is the inner surface of the curve of second corner portion 16, is smaller than plate thickness T2 of second surface portion 21 and second end portion 23. For this reason, end surface 23a, which is the tip of flared bent portion 25, is likely to come into line contact in the circumferential direction with inner surfaces 15a, 17a of first bent portion 15 and second bent portion 17, respectively.
[0028] In the present embodiment, the second end 23 where the flare bent portion 25 is formed is formed in the body 20, which has a lower rigidity than the head plate 10. This makes it easier to form the flare bent portion 25 at the second end 23.
[0029] When the flare bent portion 25 is formed, the pre-welding process is completed, and the welding process begins.
[0030] [1-2-2. Welding process] In the welding process, the welding device W performs arc welding with the torch W2 while the clamp W1 rotates the head plate 10 and the body 20 around the axis AX. At this time, the clamp W1 applies a force along the axis AX to the head plate 10 in a direction in which the head plate 10 and the body 20 press against each other. This makes it easier for the end face 23a to make line contact with both the inner surfaces 15a, 17a of the first bent portion 15 and the second bent portion 17. In addition, the end face 23a is sandwiched from the radial inside and the radial outside by the two inner surfaces 15a, 17a. Therefore, the end face 23a is restricted from moving in the radial direction, and the first end 13 and the second end 23 are less likely to shift from each other in the direction along the axis AX and in the radial direction.
[0031] In this way, the end face 23a is restricted in the radial direction and the direction along the axis AX relative to the inner faces 15a, 17a over its entire circumference. Therefore, in addition to the misalignment caused by the arrangement of the head plate 10 and the body 20, the misalignment caused by the bending of the first end 13 and the second end 23 can also be suppressed.
[0032] The welding device W has a touch sensor (not shown) that detects the position of a portion of the tip 13a of the first end 13 that is located vertically above. Using information on the position of the tip 13a detected by the touch sensor, the welding device W moves the torch W2 in the direction of the axis AX and in the radial direction, and causes the torch W2 to discharge an arc toward the inside of the target range R in FIG. 7. In this embodiment, the target range R is the outer side surface 17b, which is the outer surface of the bend between the first bent portion 15 and the second bent portion 17, of the second bent portion 17, and the second corner portion 16. The outer side surface 17b and the second corner portion 16 are heated from the radial outside by the torch W2.
[0033] The first bent portion 15 and the second bent portion 17 are melted by the heat from the torch W2. The flare bent portion 25 is melted by the heat conducted from the first bent portion 15 and the second bent portion 17. In this manner, in the present embodiment, welding is performed by melting the flare bent portion 25, the first bent portion 15, and the second bent portion 17, so that the amount of melted metal can be increased and welding with stable quality can be performed. In addition, the melted flare bent portion 25, the first bent portion 15, and the second bent portion 17 act as a filler material that fills the gap between the first end portion 13 and the second end portion 23, so that the first end portion 13 and the second end portion 23 can be welded without using a filler material.
[0034] Here, in this embodiment, the length L of the second bent portion 17 along the axis AX is more than twice the plate thickness T2, which is the thickness of the second surface portion 21 and the second end portion 23. Therefore, the target range R can be made wider, and the area of the outer surface 17b of the second bent portion 17 becomes larger, making it easier to heat and easier to weld. In addition, since the second bent portion 17 is long, the end surface 23a of the second end portion 23 is less likely to come off the inner surface 17a of the second bent portion 17. Therefore, during welding, the head plate 10 and the body 20 are less likely to be displaced in the radial direction. Furthermore, since the second bent portion 17 is long, the amount of metal melted during welding can be increased, making it easier to stabilize the quality of the welding without using a filler metal.
[0035] In addition, in this embodiment, since the end face 23a is likely to be in line contact with both the inner surfaces 15a, 17a of the first bent portion 15 and the second bent portion 17, heat is likely to be transferred from the first end portion 13 to the second end portion 23 via the end face 23a. Therefore, the flare bent portion 25 is likely to melt, and the quality of the welding is likely to be stable. In particular, in this embodiment, the end face 23a is in contact with the inner surface 17a, which is the surface opposite to the outer surface 17b of the second bent portion 17 heated by the torch W2. As a result, the heat applied to the outer surface 17b from the torch W2 is quickly transferred to the second end portion 23 via the inner surface 17a and the end face 23a, making it easier to melt the flare bent portion 25.
[0036] Furthermore, in this embodiment, since the second bent portion 17 has a generally cylindrical shape extending along the first surface 11, the torch W2 located radially outward of the second bent portion 17 can easily heat the outer surface 17b. Also, since the second bent portion 17 is along the first surface 11 and is generally perpendicular to the radially outward direction DO, when the end surface 23a tries to shift radially outward, the inner surface 17a of the second bent portion 17 can easily restrict the movement of the end surface 23a.
[0037] The torch W2 performs arc discharge on the outer surface 17b and the second corner portion 16 of the entire circumference, which is the target range R, so that the first end portion 13 and the second end portion 23 are joined together along the entire circumference via the bead 30, as shown in Fig. 3. This completes the welding process and the manufacture of the can body 1.
[0038] [1-3. Effects, etc.] As described above, in this embodiment, the welding method is a welding method for joining a head plate 10 and a body 20, in which the head plate 10 has a cylindrical first surface portion 11 and a first end portion 13 which is an end portion of the first surface portion 11, the body 20 has a cylindrical second surface portion 21 and a second end portion 23 which is an end portion of the second surface portion 21, and the first end portion 13 has a first bent portion 15 which rises at an acute angle radially outward from the first surface portion 11, and a second end portion 23 which is closer to the tip 13a of the first end portion 13 than the first bent portion 15. and a second bent portion 17 that bends in the opposite direction to the first bent portion 15 at the inner circumferential direction, and the second end portion 23 has a flare bent portion 25 that rises at an obtuse angle radially outward from the second surface portion 21. Inside the bend between the first bent portion 15 and the second bent portion 17, the first bent portion 15 and the second bent portion 17 are in contact with an end face 23a located at the tip of the flare bent portion 25, and the second bent portion 17 is heated from the radially outward side, thereby welding the first end portion 13 and the second end portion 23 together. According to this configuration, the end face 23a comes into contact with the first bent portion 15 and the second bent portion 17, thereby restricting the radial movement of the flare bent portion 25. Therefore, the head plate 10 and the body 20 are less likely to shift during welding. Furthermore, during welding, the second bent portion 17 is heated from the radially outer side with the end face 23a in contact with the first bent portion 15 and the second bent portion 17. Therefore, the heat applied to the second bent portion 17 is easily transferred to the flare bent portion 25 via the end face 23a, making it easier to stabilize the quality of the welding.
[0039] Furthermore, as in this embodiment, the welding method may be configured to weld the first end 13 and the second end 23 while pressing the head plate 10 and the body 20 against each other along the axis AX of the first surface portion 11. According to this configuration, the end face 23a easily comes into contact with the first bent portion 15 and the second bent portion 17, and radial movement is easily restricted. Therefore, the head plate 10 and the body 20 are less likely to shift during welding. In addition, because the end face 23a easily comes into contact with the first bent portion 15 and the second bent portion 17, heat is easily transferred from the second bent portion 17 to the flare bent portion 25 via the end face 23a, and the quality of the welding is easily stabilized.
[0040] Furthermore, as in this embodiment, in the welding method, the flare bend portion 25 may be formed by pressing the head plate 10 and the body 20 against each other along the axis AX of the first surface portion 11 with the second end portion 23 in contact with the first bend portion 15. According to this configuration, the step of forming the flare bent portion 25 and the welding can be carried out continuously, improving the productivity of the welding.
[0041] Also, as in this embodiment, the radius of curvature of the inner surface 16a of the second corner portion 16 between the second bent portion 17 and the first bent portion 15 may be configured to be less than or equal to the plate thickness T2, which is the thickness of the second end portion. According to this configuration, end surface 23a of flared bent portion 25 is more likely to come into line contact with first bent portion 15 and second bent portion 17.
[0042] Further, as in this embodiment, the bending angle A2 between the first bent portion 15 and the second bent portion 17 may be configured to be equal to the bending angle A1 between the first surface portion 11 and the first bent portion 15. According to this configuration, the second bent portion 17 extends in a direction substantially perpendicular to the radial direction, which makes it easier to restrict the movement of the end face 23a toward the radial outside. This makes it easier to prevent the head plate 10 and the body 20 from being misaligned during welding. In addition, the second bent portion 17 is heated from the radial outside, so extending in a direction substantially perpendicular to the radial direction makes it easier to heat the second bent portion 17.
[0043] Furthermore, as in this embodiment, the length L, which is the dimension of the second bent portion 17 in the direction along the axis AX of the first surface portion 11, may be configured to be more than twice the plate thickness T2, which is the thickness of the second end portion 23. According to this configuration, the length L of the second bent portion 17 is more than twice the plate thickness T2 of the second end portion 23, so that the inner surface 17a of the second bent portion 17 easily presses the end surface 23a from the radial outside. Therefore, the head plate 10 and the body 20 are less likely to shift during welding. In addition, since the second bent portion 17 is heated from the radial outside, the second bent portion 17 can be easily heated by setting the dimension along the axis AX intersecting the radial direction to be large. Furthermore, since the dimension of the second bent portion 17 is large, the amount of metal melted during welding increases, so that the quality of the welding can be easily stabilized without using a filler metal.
[0044] (Other embodiments) As described above, the first embodiment has been described as an example of the technology disclosed in the present application. However, the technology in the present disclosure is not limited to this, and can be applied to embodiments in which modifications, substitutions, additions, omissions, etc. are made. In addition, it is also possible to combine the components described in the first embodiment to create new embodiments. Therefore, other embodiments will be exemplified below.
[0045] In the method for manufacturing a can body according to the first embodiment, it has been described that the plate material having the first end 13 on which the first bent portion 15 and the second bent portion 17 are formed is the head plate 10, and the plate material having the flared bent portion 25 and the flat end surface 23a is the body 20, but this is merely an example. For example, the first bent portion and the second bent portion may be formed in the body 20, and the flared bent portion and the flat end surface may be formed in the head plate 10.
[0046] That is, the method for manufacturing a can body is a method for manufacturing a can body in which a head plate 10 and a cylindrical body 20 are welded to produce a can body 1, in which one of a first plate material having a first bent portion 15 and a second bent portion 17 formed therein, and a second plate material having a flare bent portion 25 formed therein, is used as the head plate 10, and the other of the first plate material and the second plate material, which is different from the other plate material, is used as the body 20, and the head plate and the body are welded together using the welding method described in the above embodiment. According to this configuration, when the head plate 10 and the body 20 are welded together during the manufacture of the can body 1, misalignment between the first end portion 13 and the second end portion 23 can be suppressed, and the quality of the welding can be more easily stabilized.
[0047] In the first embodiment, the inner diameter D1 of the first surface portion 11 and the inner diameter D2 of the second surface portion 21 are described as being equal to each other, but this is only an example. For example, the inner diameter D2 may be larger than the inner diameter D1, and the end face 23a may be located radially outward from the first surface portion 11 before the flare bent portion 25 is formed. In this case, the end face 23a does not contact the outer surface 14a of the first corner portion 14 but contacts the inner surface 15a of the first bent portion 15, so that the end face 23a is easily guided radially outward along the inner surface 15a. This makes it easier to form the flare bent portion 25. It should be noted that the flare bent portion 25 can also be easily formed by expanding the second end portion 23 before the flare bent portion 25 is formed.
[0048] In the first embodiment, the head plate 10 and the body 20 are described as being made of stainless steel, but this is just one example. The head plate 10 and the body 20 may each be made of a metal other than stainless steel. Also, the head plate 10 and the body 20 may each be made of a different type of metal.
[0049] In the first embodiment, the welding device W detects the position of the tip 13a of the first end 13 by a touch sensor, but this is just one example. For example, the welding device W may detect the position of the tip 13a by a non-contact sensor such as an optical sensor, such as a visual sensor or a laser displacement sensor, instead of a touch sensor.
[0050] In the welding method described in the first embodiment, welding may be performed while inserting a filler material such as a filler rod or a filler wire into the arc atmosphere.
[0051] It should be noted that the above-described embodiments are intended to illustrate the technology of the present disclosure, and various modifications, substitutions, additions, omissions, and the like can be made within the scope of the claims or their equivalents.
[0052] [Configuration supported by the above embodiment] The above embodiment supports the following configurations.
[0053] (Additional Note) (Technology 1) A welding method for joining a first plate and a second plate, wherein the first plate has a cylindrical first surface portion and a first end portion that is an end of the first surface portion, the second plate has a cylindrical second surface portion and a second end portion that is an end of the second surface portion, the first end portion has a first bent portion that rises at an acute angle radially outwardly of the first surface portion, and a second bent portion that bends in an opposite direction to the first bent portion at a tip side of the first end portion relative to the first bent portion, and the second end portion has a flared bent portion that rises at an obtuse angle radially outwardly of the second surface portion, and the first bent portion, the second bent portion, and the flared bent portion are in contact with each other on the inside of the bend between the first bent portion and the second bent portion, and the second bent portion is heated from the radially outwardly of the second bent portion to weld the first end and the second end. As a result, the flare bent portion comes into contact with the first bent portion and the second bent portion, restricting radial movement. This makes it difficult for the first plate material and the second plate material to shift during welding. Also, during welding, the second bent portion is heated from the radially outer side while the flare bent portion is in contact with the first bent portion and the second bent portion, so the heat applied to the second bent portion is easily transferred to the flare bent portion. This makes it easier to stabilize the quality of the welding.
[0054] (Technical Technique 2) The welding method according to Technical Technique 1, wherein the first end portion and the second end portion are welded together while the first plate material and the second plate material are pressed against each other along the axis of the first surface portion. This makes it easier for the flare bent portion to come into contact with the first bent portion and the second bent portion, and makes it easier to restrict radial movement. This makes it harder for the first plate material and the second plate material to shift during welding. In addition, because the flare bent portion comes into contact with the first bent portion and the second bent portion, heat is more easily transferred from the second bent portion to the flare bent portion, making it easier to stabilize the quality of the welding.
[0055] (Technology 3) The welding method according to Technology 1 or 2, wherein the flare bent portion is formed by pressing the first plate material and the second plate material against each other along an axis of the first surface portion with the second end portion in contact with the first bent portion. This allows the step of forming the flare bent portion and the welding to be carried out consecutively, improving welding productivity.
[0056] (Technology 4) The welding method according to any one of Techniques 1 to 3, wherein a radius of curvature between the second bent portion and the first bent portion is equal to or smaller than a thickness of the second end portion. This makes it easier for the flare bent portion to come into line contact with the first bent portion and the second bent portion.
[0057] (Technology 5) The welding method according to any one of Technologies 1 to 4, wherein a bending angle between the first bent portion and the second bent portion is equal to a bending angle between the first surface portion and the first bent portion. Since the second bent portion extends substantially perpendicular to the radial direction, it is easy to restrict the movement of the flare bent portion toward the radial outside. Therefore, it is easy to prevent the first plate material and the second plate material from being misaligned during welding. In addition, since the second bent portion is heated from the radial outside, the second bent portion 17 is easily heated by extending in a direction substantially perpendicular to the radial direction.
[0058] (Technology 6) A welding method according to any one of Techniques 1 to 5, wherein a dimension of the second bent portion in a direction along the axis of the first surface portion is at least twice the thickness of the second end portion. As a result, the dimension of the second bent portion 17 along the axis is more than twice the thickness of the second end portion, so that the second bent portion can easily press the flare bent portion from the radially outer side. This makes it difficult for the first plate material and the second plate material to shift during welding. In addition, since the second bent portion is heated from the radially outer side, the second bent portion can be easily heated by setting the dimension along the axis intersecting the radial direction to be large. Furthermore, since the dimension of the second bent portion is large, the amount of metal melted during welding increases, making it easier to stabilize the quality of the welding.
[0059] (Technology 7) A method for manufacturing a can body, in which a head plate and a cylindrical body are welded to produce a can body, wherein one of the first plate material and the second plate material is used as the head plate, and the other of the first plate material and the second plate material, which is different from the one of the first plate material and the second plate material, is used as the body, and the head plate and the body are welded using a welding method described in any one of Technologies 1 to 6. This makes it possible to suppress misalignment between the head plate and the body when welding them together during the manufacture of the can body, and also makes it easier to stabilize the quality of the welding. [Industrial Applicability]
[0060] The present disclosure is applicable to a welding method for welding plate materials together, and in particular, the present disclosure is suitably applicable to a welding method for manufacturing a container having a body and a head plate, such as a hot water storage tank. [Explanation of symbols]
[0061] 1 can body 10 Head plate 11 First side 13 First end 13a Tip 14 1st corner 14a External surface 15 First bending section 15a Inside surface 16 Second corner 16a Inside surface 17 Second bending section 17a Inside surface 17b External surface 19 Dome section 20. Torso 21 Second side part 23 Second end 23a End face 25 Flare bend 30 Beads W welding equipment W1 Clamp W2 Torch W3 Jig
Claims
1. A welding method for joining a first plate material and a second plate material, comprising: The first plate member has a cylindrical first surface portion and a first end portion which is an end portion of the first surface portion, The second plate member has a cylindrical second surface portion and a second end portion which is an end portion of the second surface portion, the first end portion has a first bent portion that rises at an acute angle toward the radially outer side of the first surface portion, and a second bent portion that is bent in an opposite direction to the first bent portion on a tip side of the first end portion relative to the first bent portion, The second end portion has a flare bent portion that rises at an obtuse angle toward a radially outer side of the second surface portion, In a state where the first bent portion and the second bent portion are in contact with the flare bent portion on the inside of the bend between the first bent portion and the second bent portion, the second bent portion is heated from the radially outer side to weld the first end portion and the second end portion. Welding method.
2. The first end portion and the second end portion are welded together while pressing the first plate material and the second plate material against each other along the axis of the first surface portion. The welding method according to claim 1.
3. The flare bent portion is formed by pressing the first plate material and the second plate material against each other along an axis of the first surface portion with the second end portion in contact with the first bent portion. The welding method according to claim 1.
4. A radius of curvature between the second bent portion and the first bent portion is equal to or less than a thickness of the second end portion. The welding method according to claim 1.
5. A bending angle between the first bending portion and the second bending portion is equal to a bending angle between the first surface portion and the first bending portion. The welding method according to claim 1.
6. A dimension of the second bent portion in a direction along the axis of the first surface portion is equal to or greater than twice the thickness of the second end portion. The welding method according to claim 1.
7. A method for manufacturing a can body, comprising the steps of: manufacturing a can body by welding a head plate and a cylindrical body, the method comprising the steps of: one of the first plate material and the second plate material is used as the end plate; As the fuselage, a plate material different from the one of the first plate material and the second plate material is used, The head plate and the fuselage are welded together using the welding method according to any one of claims 1 to 6. Manufacturing method of can body.
Citation Information
Patent Citations
Ferritic stainless steel for warm water vessel with welded structure and warm water vessel
JP2007302995A
Method of manufacturing can body, weld joint configuration of can body, and can shell
JP2009183963A
Liquid tank and water heater
JP2010203697A
Method for welding thin plate member and method for manufacturing can body using the method
JP2012148304A