Pore-forming agent

A polymer-based pore-forming agent with specific structural units forms uniform pores, addressing the limitations of hollow and resin particles by enhancing porosity and uniformity in matrices.

JP7573422B2Active Publication Date: 2024-10-25NIPPON SHOKUBAI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020193244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-20
Publication Date
2024-10-25
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

Hollow particles have low strength and are easily crushed during kneading, while resin particles fail to form pores effectively and can cause matrix cracking, leading to reduced porosity and uniformity.

Method used

A pore-forming agent composed of a polymer with a structural unit derived from a specific general formula, containing alkyl groups, alkali metals, alkaline earth metals, or ammonium, which can be polymerized and hydrolyzed to form uniform pores.

Benefits of technology

The polymer-based pore-forming agent easily forms uniform pores, suitable for various applications including fibers, ceramics, coatings, and thermosetting resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573422000001
    Figure 0007573422000001
  • Figure 0007573422000002
    Figure 0007573422000002
  • Figure 0007573422000003
    Figure 0007573422000003
Patent Text Reader

Abstract

To provide a pore-forming agent which facilitates formation of pores and realizes high uniformity of the pores.SOLUTION: A pore-forming agent comprises a polymer comprising a structural unit derived from a general formula (1) in the figure, where R1 represents a C1-4 alkyl group, a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pore-forming agent. [Background technology]

[0002] 2. Description of the Related Art Hollow particles and resin particles have been used as pore-forming agents in producing various matrices, for example, porous ceramic molded bodies (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-292596 A [Patent Document 2] JP 2019-147870 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the case of hollow particles, the strength of the particles is low, so for example, when they are mixed with various matrices, the particles are crushed, and there is an issue of reduced porosity. In the case of resin particles, they cannot be fully decomposed and removed even under high temperature and long-term conditions, so pores are difficult to form, and there is also the problem of cracks occurring in the matrix.

[0005] Therefore, an object of the present invention is to provide a pore-forming agent which easily forms pores and which also has high uniformity in the formed pores. [Means for solving the problem]

[0006] The present inventors have conducted various studies to achieve the above object and have arrived at the present invention. That is, the pore-forming agent of the present disclosure is a pore-forming agent containing a polymer containing a structural unit derived from the following general formula (1).

[0007] [ka]

[0008] (In general formula (1), R 1 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium. Effect of the Invention

[0009] The pore-forming agent of the present disclosure can easily form pores and the formed pores have uniformity, which makes it possible to apply the agent to various fields such as fibers, ceramics, coatings, thermoplastic resins, thermosetting resins, and various films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. Note that a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.

[0011] [Pore-forming agent of the present disclosure] <Structural unit represented by general formula (1)> The pore-forming agent of the present disclosure contains a polymer (hereinafter also referred to as the "polymer of the present disclosure"), and the polymer (hereinafter sometimes referred to as an RHMA-based polymer) contains a structural unit derived from the following general formula (1).

[0012] [ka]

[0013] (In general formula (1), R 1 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium. Above R 1 The alkyl group having 1 to 4 carbon atoms represented by the following formula is preferably an alkyl group having 1 to 2 carbon atoms, and more preferably an alkyl group having 1 carbon atom (a methyl group).

[0014] R 1The alkali metal atom represented by the formula (I) is preferably lithium, sodium or potassium, more preferably sodium or potassium, and even more preferably sodium.

[0015] R 1 Examples of the alkaline earth metal atom represented by the formula (I) include calcium and magnesium.

[0016] R 1 Ammonium, represented by NH 4+ The term "organic ammonium" is defined as including, but not limited to, organic ammonium. Examples of organic ammonium include quaternary ammonium such as tetraalkyl ammonium such as tetramethyl ammonium and tetrabutyl ammonium; and ammonium (primary to tertiary ammonium) formed by protonating amines. 1 The amine is preferably ammonia or ammonium formed by protonation of an amine. The amine is preferably a trialkylamine such as trimethylamine, triethylamine, or tributylamine (preferably triC 1-10 Alkylamines; hydroxyalkylamines such as diethanolamine and triethanolamine (preferably di- or tri(hydroxy C 1-10 Alkyl)amines, etc., are preferred, with hydroxyalkylamines being preferred.

[0017] The structural unit represented by the above general formula (1) may be formed by a polymerization reaction of a monomer represented by the following general formula (2), but may also be formed by other methods. 1 is an alkyl group having 1 to 4 carbon atoms, and then hydrolyzed to obtain a monomer represented by the general formula (1) represented by R 1 may form an alkali metal structural unit, an alkaline earth metal structural unit, or an ammonium structural unit.

[0018] [ka]

[0019] (In general formula (2), R 1 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium. In the above general formula (2), R 1 R may be one type or two or more types. 1 In the case where there are two or more types of monomers represented by the above general formula (2), R 1 The ester group may be formed by polymerizing a monomer represented by the above general formula (2), in which R is an alkyl group having 1 to 4 carbon atoms, and then partially hydrolyzing the ester group or by hydrolysis with two or more basic substances.

[0020] The polymer of the present disclosure preferably contains 40% by mass or more of the structural unit represented by the above general formula (1), more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more. On the other hand, the polymer of the present disclosure preferably contains 99.9% by mass or less of the structural unit represented by the above general formula (1), more preferably 99% by mass or less, even more preferably 97% by mass or less, and most preferably 95% by mass or less. By containing within the above range, pH and hydrophilicity can be adjusted, so that the pore-forming agent of the present disclosure can easily form pores, and the formed pores tend to be highly uniform.

[0021] The polymer of the present disclosure may have a multilayer structure, for example, a core-shell structure composed of a core portion and a shell portion provided on the surface of the core portion.

[0022] <Structural units derived from other monomers> The polymer of the present disclosure may contain one or more structural units derived from a monomer other than the structural unit represented by the above general formula (1) (hereinafter also referred to as "structural units derived from other monomers"). That is, the polymer may contain one or more structural units derived from a monomer other than the monomer represented by the above general formula (2) (hereinafter also referred to as "other monomers").

[0023] The other monomers are not particularly limited, and examples thereof include (meth)acrylic monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; styrene-based monomers such as styrene, α-methylstyrene, p-methylstyrene, tert-butylstyrene, chlorostyrene, and vinyltoluene; (meth)acrylic acid, malic acid, and the like. Carboxyl group-containing monomers such as oleic acid, fumaric acid, crotonic acid, itaconic acid, and maleic anhydride; silane group-containing monomers such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, 2-styrylethyltrimethoxysilane, vinyltrichlorosilane, γ-(meth)acryloyloxypropylhydroxysilane, and γ-(meth)acryloyloxypropylmethylhydroxysilane; 2-hydroxyethyl(meth)acryloyloxypropylmethylhydroxysilane; Hydroxyl group-containing monomers such as acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; nitrogen atom-containing monomers such as (meth)acrylamide, N,N-dimethyl (meth)acrylamide, dimethylaminoethyl (meth)acrylamide, N-vinylpyrrolidone, and (meth)acrylonitrile; ethylene glycol methoxy (meth)acrylate, diethylene glycol methoxy (meth)acrylamide, and the like. fluorine atom-containing monomers such as trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, etc.; epoxy group-containing monomers such as glycidyl (meth)acrylate, etc.; light stabilizing monomers such as 2,2,6,6-tetramethylpiperidine-4-(meth)acrylate, etc.; ultraviolet absorbing monomers such as benzotriazole-based ultraviolet absorbing monomers, benzophenone-based ultraviolet absorbing monomers, etc.; polyfunctional ethylenically unsaturated monomers, etc.

[0024] The polyfunctional ethylenically unsaturated monomer is not particularly limited as long as it is a compound containing two or three or more ethylenic carbon-carbon double bonds, and examples thereof include compounds containing two or three or more ethylenic carbon-carbon double bonds of one or more types selected from a CH2=CH- group, a CH2=CH-O- group, a CH2=CH-CH2-O- group, a CH2=C(CH3)-CH2-O- group, a CH2=CH-CH2-CH2-O- group, a CH2=C(CH3)-CH2-CH2-O- group, a CH2=CH-CO-O- group, a CH2=C(CH3)-CO-O- group, and a CH2=CH-CO-NH- group.

[0025] In the present disclosure, the polyfunctional ethylenically unsaturated monomer preferably has a molecular weight of 50 or more and 1,000 or less, and more preferably 100 or more and 400 or less.

[0026] In the present disclosure, the polyfunctional ethylenically unsaturated monomer is not particularly limited, but from the viewpoint of handleability during pore formation and uniformity of the formed pores, it is preferable that the polyfunctional ethylenically unsaturated monomer is a polyfunctional ethylenically unsaturated monomer in which n-1 or more ethylenically unsaturated groups are CH2=CH-CO-O- groups or CH2=CH-CO-NH- groups, relative to the number n (n is an integer of 2 or more) of ethylenically unsaturated groups contained in one molecule of the polyfunctional ethylenically unsaturated monomer (hereinafter also referred to as a "hydrolyzable polyfunctional ethylenically unsaturated monomer").

[0027] Examples of the polyfunctional ethylenically unsaturated monomer include polyfunctional acrylic esters and N,N'-methylenebisacrylamide.

[0028] Examples of polyfunctional acrylic acid esters include ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, polypropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, and acrylic-modified polydimethylsiloxane.

[0029] The structural unit derived from the other monomer refers to a structural unit in which at least one carbon-carbon double bond of the other monomer is replaced with a carbon-carbon single bond. For example, in the case of ethylene glycol diacrylate, CH2=CH-CO-O-CH2CH2O-CO-CH=CH2, the structural unit derived from ethylene glycol diacrylate can be expressed as, for example, -CH2-CH-CO-O-CH2CH2O-CO-CH-CH2-. The structural unit derived from the other monomer can be formed, for example, by radical polymerization of the other monomer. Note that the structural unit derived from the other monomer is not limited to a structural unit formed by polymerization of the other monomer, as long as it has the same structure as the structure in which the carbon-carbon double bond of the other monomer is replaced with a carbon-carbon single bond, and may be, for example, a structural unit formed by a reaction after polymerization.

[0030] The polymer of the present disclosure preferably contains 0.01% by mass or more of structural units derived from other monomers, more preferably 0.1% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, and particularly preferably 5% by mass or more. On the other hand, the polymer of the present disclosure preferably contains 60% by mass or less of structural units derived from other monomers, more preferably 40% by mass or less, even more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less.

[0031] The polymer of the present disclosure preferably contains 0.01% by mass or more of the structural unit derived from the polyfunctional ethylenically unsaturated monomer, more preferably contains 0.1% by mass or more, even more preferably contains 1% by mass or more, even more preferably contains 2% by mass or more, and particularly preferably contains 5% by mass or more. On the other hand, the polymer of the present disclosure preferably contains 60% by mass or less of the structural unit derived from the polyfunctional ethylenically unsaturated monomer, more preferably contains 40% by mass or less, even more preferably contains 20% by mass or less, even more preferably contains 15% by mass or less, and particularly preferably contains 10% by mass or less.

[0032] The polymer of the present disclosure preferably contains 0.01% by mass or more of structural units derived from hydrolyzable polyfunctional ethylenically unsaturated monomers, more preferably contains 0.1% by mass or more, even more preferably contains 0.5% by mass or more, even more preferably contains 2% by mass or more, and particularly preferably contains 5% by mass or more. On the other hand, the polymer of the present disclosure preferably contains 60% by mass or less, more preferably contains 50% by mass or less, even more preferably contains 40% by mass or less, even more preferably contains 20% by mass or less, and particularly preferably contains 10% by mass or less.

[0033] The polymer of the present disclosure may contain one or more structural units derived from a hydrolyzable polyfunctional ethylenically unsaturated monomer.

[0034] The polymer of the present disclosure may have a particle shape (hereinafter, also referred to as "polymer particles of the present disclosure"). The preferred particle size of the polymer particles of the present disclosure is a volume average particle size of preferably 10 nm to 10 μm, more preferably 50 nm to 5 μm, even more preferably 100 nm to 1 μm, and particularly preferably 150 to 850 nm. The volume average particle size of the polymer of the present disclosure can be measured, for example, by a dynamic light scattering method.

[0035] The polymer of the present disclosure may have a multilayer structure, for example, a core-shell structure composed of a core portion and a shell portion provided on the surface of the core portion.

[0036] [Method of producing the pore-forming agent of the present disclosure] <Polymerization method> The RHMA polymer is a monomer represented by the above formula (2), 1 is an alkyl group having 1 to 4 carbon atoms (hereinafter referred to as hydroxymethyl acrylate ester), is polymerized in an aqueous solvent, and if necessary, is partially or completely hydrolyzed to obtain R 1 The copolymer can be obtained by converting a part or all of the moieties corresponding to the above to hydrogen atoms, alkali metal atoms, alkaline earth metal atoms, ammonium, etc. Hydroxymethyl acrylic ester may be polymerized together with other monomers (hereinafter, these may be collectively referred to as "raw monomer components"). When hydroxymethyl acrylic ester is used as a raw monomer, the product can be made into particles even when polymerized in an aqueous solvent.

[0037] Examples of the polymerization method include suspension polymerization, emulsion polymerization, and dispersion polymerization. Among them, emulsion polymerization is preferred in which the raw material monomer components are dispersed in a reaction solvent in the presence of an emulsifier to carry out a (radical) polymerization reaction. Specifically, the method for producing the polymer of the present invention preferably includes emulsion polymerization in which at least one monomer represented by formula (2) is dispersed in an aqueous solvent in the presence of an emulsifier to carry out a polymerization reaction. The emulsion polymerization may be carried out in one stage or multiple stages.

[0038] The emulsifier may be one or more kinds, and may be a non-reactive surfactant or a reactive surfactant having a radically polymerizable group in its structure.

[0039] The non-reactive surfactant includes anionic and nonionic surfactants. Examples of the anionic surfactant include fatty acid salts, alkyl (aryl) sulfonates, alkyl sulfates, polyoxyethylene alkyl (phenyl) ether sulfates, etc., and examples of the nonionic surfactant include polyoxyethylene alkyl (phenyl) ethers, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene polyoxypropylene block polymers, etc.

[0040] The reactive surfactant includes anionic and nonionic surfactants. Examples of the anionic reactive surfactant include, but are not limited to, ether sulfate reactive surfactants and phosphate ester reactive surfactants.

[0041] The amount of the emulsifier is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the total of the raw material monomer components, and is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less.

[0042] In the present disclosure, the aqueous solvent may be water alone or a mixed solvent of water and a water-miscible organic solvent, but water alone is preferred. The aqueous solvent typically refers to a solvent with a water content of more than 50% by volume. As the water, ion-exchanged water (deionized water), distilled water, pure water, etc. can be used. As the water-miscible organic solvent, an organic solvent (such as a lower alcohol) that can be mixed uniformly with water can be used. From the viewpoint of minimizing the amount of organic solvent remaining in the polymer, an aqueous solvent in which 80% by volume or more of the aqueous solvent is water is preferred, an aqueous solvent in which 90% by volume or more of the aqueous solvent is water is more preferred, an aqueous solvent in which 95% by volume or more of the aqueous solvent is water is even more preferred, an aqueous solvent substantially composed of water (an aqueous solvent in which 99.5% by volume or more of water) is particularly preferred, and water alone is most preferred.

[0043] When polymerizing the raw material monomer components, for example, a polymerization initiator, irradiation with ultraviolet rays or radiation, application of heat, or other means is used. It is preferable to use a polymerization initiator, and from the viewpoint of efficiently reacting the raw material monomer components and sufficiently reducing the amount of residual monomer, a polymerization initiator in combination with an oxidizing agent and a reducing agent (redox type polymerization initiator) is preferable.

[0044] The hydrolysis of the polymer of the present disclosure can be carried out by adding a basic aqueous solution such as an aqueous sodium hydroxide solution, an aqueous calcium hydroxide solution, an aqueous ammonia solution, or an aqueous cyclohexylamine solution. In addition, partial or complete neutralization can be carried out by appropriately adding an acid to the hydrolysis solution. By carrying out hydrolysis and neutralization, R in formula (1) can be 1 The group corresponding to can be a hydrogen atom, an alkali metal atom, an alkali metal atom, or an ammonium atom. The amount of acid or base used during polymerization, hydrolysis, and neutralization can be adjusted, and R 1 By adjusting the ratio of monomer units in which R is a hydrogen atom, the pH and hydrophilicity of the polymer can be adjusted, and the ease of pore formation and the uniformity of the formed pores can be improved.

[0045] <Water dispersion> The scope of the present invention also includes a pore-forming agent in which the polymer is dispersed in water (aqueous dispersion) by dispersing the polymer in water to form an aqueous dispersion. The aqueous dispersion has a hydroxymethyl group, and is excellent in hydrophilicity. The aqueous dispersion has good dispersibility in water, has high storage stability as a dispersion, and can easily undergo hydrolysis. When hydrolysis and subsequent neutralization are performed as necessary, hydrolysis can be performed by adding a basic aqueous solution such as an aqueous sodium hydroxide solution, an aqueous ammonia solution, an aqueous diethanolamine solution, or an aqueous cyclohexylamine solution to the polymer contained in the aqueous dispersion. Furthermore, partial or complete neutralization can be performed by adding an acid to the hydrolysis liquid as appropriate. By performing hydrolysis and neutralization, R in formula (1) can be obtained. 1 The group corresponding to R can be a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium. The amount of acid or base used during polymerization, hydrolysis, and neutralization can be adjusted, and R 1 By adjusting the ratio of monomer units in which R is a hydrogen atom, the volume average particle size of the polymer can be easily adjusted, and therefore the pore-forming agent can be used in a wide range of applications.

[0046] The aqueous dispersion preferably contains 5% by mass or more of the polymer, more preferably 10% by mass or more, and preferably 100% by mass or less, more preferably 50% by mass or less.

[0047] The volume average particle diameter of the polymer contained in the aqueous dispersion is preferably 10 nm to 10 μm, more preferably 50 nm to 5 μm, further preferably 100 nm to 1 μm, and particularly preferably 150 to 850 nm. The volume average particle diameter of the polymer contained in the aqueous dispersion was measured by dynamic light scattering.

[0048] [Hole formation method according to the present disclosure] The polymer of the present disclosure or the pore-forming agent of the present disclosure (hereinafter also referred to as the "polymer, etc. of the present disclosure") can be added to various matrices such as resins, and then treated with, for example, an alkali, to form pores in the matrix under mild conditions.

[0049] The method for adding the polymer, etc. of the present disclosure to various matrices is not limited, and examples thereof include a method of melt-mixing the polymer, etc. of the present disclosure with a resin, etc., and a method of applying a solvent containing the polymer, etc. of the present disclosure and a resin, and then drying and removing the solvent.

[0050] The method of treating with an alkali (also referred to as an "alkali washing step") is not particularly limited. For example, it is preferably carried out by contacting an alkali solution with a matrix containing the polymer of the present disclosure, but it may also be carried out by contacting an alkali solution with a solvent containing the polymer of the present disclosure and a resin.

[0051] The alkali treatment step may be carried out at room temperature, or under heating or cooling conditions, but is preferably carried out at a temperature of 40° C. or lower. The alkali treatment step may be carried out under normal pressure, under pressure, or under reduced pressure.

[0052] The alkaline component used in the alkaline treatment step may be an inorganic base or an organic base. The alkaline solution, for example, in the case of an aqueous solution, preferably has a pH of 7 or more and 13 or less. The concentration of the alkaline solution is preferably 0.1% by weight or more and 30% by weight or less. The amount of the alkali used is preferably 0.01 mol or more and 200 mol or less per mol of the structural unit derived from the general formula (1) below.

[0053] The pore-forming method of the present disclosure preferably requires an alkali washing step, but may further include any steps such as a step of adding the polymer or the like of the present disclosure, a water washing step, a solvent washing step, or the like.

[0054] [Uses of the pore-forming agent of the present disclosure] The pore-forming agent used in the present invention is not limited in its use, and can be suitably used as a pore-forming agent for fibers because it can achieve high porosity. Examples of fibers include inorganic fibers such as glass fiber, rock wool, and carbon fiber; organic fibers such as wool, cellulose, hemp, nylon, and polyester; and the like. In addition, it can be applied to various fields such as ceramics, coatings, thermoplastic resins, thermosetting resins, various films, solid fuel cells, secondary battery separators, catalyst carriers, heat insulating materials, and low reflection materials. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0056] <Volume average particle size> The polymer dispersion was diluted with ion-exchanged water and measured using a light scattering particle size distribution measuring device (Spectris's "Zetasizer Ultra") to determine the volume average particle size (nm) of the polymer by dynamic light scattering.

[0057] <Evaluation of void formation> (Optical property evaluation) The haze (%) of the film-formed sample was evaluated using a haze meter ("NDH7000" manufactured by Nippon Denshoku Industries Co., Ltd.). (Presence or absence of holes) The film-formed sample was cut out and attached to a sample stand with the surface on which the coating film was formed facing upward to prepare a sample for evaluation. The film shape of the sample was observed using an electron microscope (JEOL Ltd., "JSM-7600FA"). The obtained microscopic images were visually evaluated qualitatively according to the following criteria. ○: Holes are formed. ×: No pores were formed.

[0058] <Polar uniformity evaluation> The microscopic images obtained in the pore formation evaluation were visually inspected and qualitatively evaluated according to the following criteria. ◎: The pores are of uniform size. ○: Some of the pores vary in size. ×: The pore size varies or no pores are formed.

[0059] [Polymer synthesis] <Production Example A1> In a stainless steel reaction kettle equipped with a stirrer, a thermometer, and a cooler, 832.0 parts by mass of deionized water and 0.96 parts by mass of anionic reactive surfactant ADEKA REASOAP SR-20 (active ingredient 100% by mass, manufactured by ADEKA) diluted with ion-exchanged water to 25.0% by mass of active ingredient (hereinafter referred to as "SR-20 (active ingredient 25.0% by mass)") were added, and the internal temperature was raised to 75°C and maintained at the same temperature. On the other hand, in a container different from the reaction kettle, 200.0 parts by mass of a monomer composition composed of 200.0 parts by mass of methyl 2-hydroxymethyl methacrylate (hereinafter referred to as "RHMA") was prepared.

[0060] After replacing the inside of the reaction vessel with nitrogen gas, 40.0 parts by mass of the monomer composition, 21.0 parts by mass of hydrogen peroxide solution (hydrogen peroxide concentration 1.28% by mass), and 21.0 parts by mass of L-ascorbic acid aqueous solution (L-ascorbic acid concentration 1.90% by mass) were added to the reaction vessel to carry out an initial polymerization reaction. Next, the remaining 160.0 parts by mass of the monomer composition, 479.0 parts by mass of hydrogen peroxide solution (hydrogen peroxide concentration 0.22% by mass), and 479.0 parts by mass of L-ascorbic acid aqueous solution (L-ascorbic acid concentration 0.33% by mass) and 486.04 parts by mass of a mixture of 479.0 parts by mass of SR-20 (active ingredient 25.0% by mass) were uniformly dropped into the reaction vessel from different inlets over 4 hours. After the dropwise addition was completed, the internal temperature was raised to 85° C. and the reaction solution was aged by maintaining it at that temperature for 2 hours, and then cooled to obtain a polymer water dispersion (1a) in which the polymer (1) was dispersed.

[0061] <Manufacturing example A2> A polymer water dispersion (2a) in which the polymer (2) was dispersed was obtained in the same manner as in Production Example A1, except that the monomer composition described in Production Example A1 was changed from 200 parts by mass of RHMA to 160 parts by mass of RHMA and 40 parts by mass of normal butyl acrylate (hereinafter referred to as "BA").

[0062] <Manufacturing example A3> A polymer water dispersion (3a) having the polymer (3) dispersed therein was obtained in the same manner as in Production Example A1, except that the monomer composition described in Production Example A1 was changed from 200 parts by mass of RHMA to 100 parts by mass of RHMA and 100 parts by mass of BA.

[0063] <Manufacturing example A4> A polymer water dispersion (4a) in which the polymer (4) was dispersed was obtained in the same manner as in Production Example A1, except that the monomer composition described in Production Example A1 was changed from 200 parts by mass of RHMA to 180 parts by mass of RHMA and 20 parts by mass of triethylene glycol diacrylate (hereinafter referred to as "3EG-A").

[0064] <Manufacturing example A5> A polymer water dispersion (5a) in which the polymer (5) was dispersed was obtained in the same manner as in Production Example A1, except that the monomer composition described in Production Example A1 was changed from 200 parts by mass of RHMA to 170 parts by mass of RHMA, 10 parts by mass of BA, and 20 parts by mass of 3EG-A.

[0065] <Manufacturing example B1> In a stainless steel reaction kettle equipped with a stirrer, a thermometer, and a cooler, 832.0 parts by mass of deionized water and 0.92 parts by mass of an aqueous sodium dodecylbenzenesulfonate solution (6.5% by mass of active ingredient, hereinafter referred to as "DBSNa (6.5% by mass of active ingredient)") were added, and the internal temperature was raised to 75°C and maintained at the same temperature. Meanwhile, in a container different from the reaction kettle, 140.0 parts by mass of methyl methacrylate (hereinafter referred to as "MMA") and 60.0 parts by mass of divinylbenzene 810 (hereinafter referred to as "DVB810") were mixed to prepare 200.0 parts by mass of a monomer composition. Next, after replacing the inside of the reaction vessel with nitrogen gas, 40.0 parts by mass of the monomer composition, 21.0 parts by mass of hydrogen peroxide solution (hydrogen peroxide concentration 1.28% by mass), and 21.0 parts by mass of L-ascorbic acid aqueous solution (L-ascorbic acid concentration 1.90% by mass) were added to the reaction vessel to carry out an initial polymerization reaction. Next, the remaining 160.0 parts by mass of the monomer composition, 479.0 parts by mass of hydrogen peroxide solution (hydrogen peroxide concentration 0.22% by mass), and 485.77 parts by mass of a mixture of 479.0 parts by mass of L-ascorbic acid aqueous solution (L-ascorbic acid concentration 0.33% by mass) and 6.77 parts by mass of DBSNa (active ingredient 6.5% by mass) were uniformly dropped into the reaction vessel from different inlets over 4 hours. After the dropwise addition was completed, the internal temperature was raised to 85° C. and kept at that temperature for 2 hours for aging, and then the reaction solution was cooled to obtain a crosslinked microparticle dispersion (6a) in which the crosslinked microparticles (6) were dispersed.

[0066] <Manufacturing example B2> A 10 L glass reactor equipped with a stirrer, a dropping device and a thermometer was charged with 4266.5 g of methyl alcohol as an organic solvent and 333.0 g of 28 wt % ammonia water (water and catalyst), and the liquid temperature was adjusted to 20±0.5° C. while stirring. Meanwhile, a solution obtained by dissolving 333.0 g of tetramethoxysilane as a silicon compound in 533.0 g of methyl alcohol was charged in the dropping device. Then, the solution was dropped from the dropping device over 1 hour. After the end of the dropping, the mixture was stirred for another 1 hour to carry out hydrolysis and condensation of tetramethoxysilane, and a suspension (7a) of silica fine particles (7) was obtained.

[0067] [Example 1] (Preparation of Paint Composition) The polymer water dispersion (1a) was mixed with 10.0 parts by mass of an acrylic resin emulsion ("U-DOUBLE EF-015" manufactured by Nippon Shokubai Co., Ltd., polymer solid content: 50% by mass) so that the polymer content was 1.0 part by mass, and then thoroughly stirred with a stirrer tip to obtain a coating composition. (Preparation of film samples) The coating composition was applied to a transparent polyethylene terephthalate film (hereinafter referred to as "PET film", Toyobo Co., Ltd., Cosmoshine A4300, length: 297 mm, width: 210 mm, thickness: 0.100 mm) with a bar coater so that the film thickness after coating was 50 μm, and dried at 100 ° C for 10 minutes in a constant temperature incubator (Yamato Scientific Co., Ltd. "DNF400") to obtain a PET film laminated with a coating film. The PET film was immersed in a 1 wt % sodium hydroxide aqueous solution for 1 minute and subjected to an alkali treatment to obtain a film-formed sample.

[0068] [Examples 2 to 5, Comparative Examples 1 and 2] A film-forming sample was prepared in the same manner as in Example 1, except that the type of polymer aqueous dispersion to be blended was changed to that shown in Table 1.

[0069] [Table 1]

[0070] From the results in Table 1, it is apparent that an object of the present invention is to provide a pore-forming agent which easily forms pores and which also has high uniformity in the formed pores.

Claims

1. A pore-forming agent comprising polymer particles containing a structural unit derived from the following general formula (1), the polymer particles having a volume average particle size of 10 nm to 10 μm, which is added to a resin for use: 【Chemistry 1】 (In general formula (1), R 1 represents an alkyl group having 1 to 4 carbon atoms, a hydrogen atom, an alkali metal atom, an alkaline earth metal atom, or ammonium.

2. 2. The pore-forming agent according to claim 1, which is an aqueous dispersion containing said polymer particles.

3. 3. The pore-forming agent according to claim 1, which is for use in fibers.

4. A method for producing the pore-forming agent described in claim 1, comprising emulsion polymerization in which at least one type of monomer represented by formula (2) is dispersed in an aqueous solvent in the presence of an emulsifier to carry out a polymerization reaction. 【Chemistry 2】

Citation Information

Patent Citations

  • Composition for molding product, molding product and separation membrane

    JP1999049826A

  • Optical functional sheet

    JP2004272153A

  • Hollow resin particle, manufacturing method therefor, and cell-forming agent for porous ceramic

    JP2004292596A

  • Direct backlight

    JP2005032537A

  • Pore-forming material for porous ceramic

    JP2008247630A