Manufacturing method of meltblown nonwoven fabric, and meltblown nonwoven fabric
The method enhances melt-blown nonwoven fabric strength and air permeability by controlling resin discharge and hot air fiberization parameters, addressing the weakness of non-calendered fabrics while maintaining breathability.
Patent Information
- Application Number
- JP2021512092
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Melt-blown nonwoven fabrics produced without calendering have weak fiber adhesion, leading to reduced strength, and calendering to enhance strength results in crushed surfaces and reduced air permeability, which is crucial for filter applications.
A method involving controlled resin discharge, hot air fiberization, and nonwoven fabric formation without calendering, with specific parameters for temperature, air flow rate, resin amount, and conveyor distance to achieve strong and breathable fabrics.
Produces melt-blown nonwoven fabrics with good strength and air permeability without calendering, maintaining mechanical properties and ventilation performance.
Smart Images

Figure 0007573515000010 
Figure 0007573515000011 
Figure 0007573515000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a meltblown nonwoven fabric, and a meltblown nonwoven fabric. [Background technology]
[0002] A resin ejection process in which a molten resin is ejected from a spinning die head having a nozzle with a plurality of holes; a fiber forming step in which hot air flowing from the nozzle holes toward a conveyor provided opposite the spinning die head is blown toward the nozzle holes to fiberize the discharged molten resin and form fibers; The meltblown nonwoven fabric is produced by a so-called meltblown method including a nonwoven fabric forming step of depositing the fibers on a conveyer by a hot air current to form a meltblown nonwoven fabric.
[0003] According to this method, a nonwoven fabric made of ultrafine fibers and having a large specific surface area can be produced inexpensively and easily. In the meltblown nonwoven fabric produced by this method, the adhesion between the fibers is weak when the fabric is piled up on the conveyor, and there is a problem in terms of strength. For this reason, the meltblown nonwoven fabric is used in a state in which its strength is increased by a thermal compression process using a calendar roll, which is called a calendar process (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 06-136656 Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the calendered meltblown nonwoven fabric has high strength, its surface is crushed, resulting in a decrease in breathability, which is an important property when the meltblown nonwoven fabric is used for filters and the like.
[0006] The present invention has been made in consideration of the above problems, and has an object to provide a method for producing a meltblown nonwoven fabric that can produce a meltblown nonwoven fabric having good strength even without calendaring, and a meltblown nonwoven fabric that can be produced by the method. [Means for solving the problem]
[0007] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.
[0008] That is, the present invention provides the following (1) to (8). (1) a resin discharge step of discharging molten resin from a spinning die head having a nozzle with a plurality of holes; a fiber forming step in which hot air flowing from the nozzle holes toward a conveyor provided opposite the spinning die head is blown toward the nozzle holes to fiberize the discharged molten resin and form fibers; A nonwoven fabric forming step of depositing the fibers on a conveyor by a hot air current to form a meltblown nonwoven fabric, After the nonwoven fabric formation process, no calendaring is performed. The temperature of the hot air is above the melting point of the resin and below (melting point + 100℃), The hot air flow rate is between 1000NL / min / m and 7000NL / min / m. The amount of resin discharged per nozzle hole is 0.006 cm 3 / min or more 0.3cm 3 / min or less, The temperature of the resin in the nozzle hole is equal to or higher than the melting point of the resin and equal to or lower than (melting point + 100°C), The shortest distance between the nozzle hole and the conveyor is 10 mm or more and 75 mm or less, A method for producing a meltblown nonwoven fabric, wherein the temperature of the atmosphere between the nozzle hole and the conveyor is 110°C or higher and 160°C or lower. (2) The method for producing a meltblown nonwoven fabric according to (1), wherein the resin is a polyester-based resin or a polyolefin-based resin. (3) The ultrasonic reflection intensity values on both sides of the meltblown nonwoven fabric are different from each other. The value of the larger reflection intensity is between 1.2 and 3.0 times the value of the smaller reflection intensity, The reflection intensity is measured under the following conditions: Distance between ultrasonic transmitter and receiver and nonwoven surface: 155mm Frequency: 360kHz Measurement temperature: 22℃ Applied voltage: 500V Wave number: 5 (burst wave) Sharp ratio: 100% Number of measurement points: 100 or more points within an area of 25 mm x 40 mm The method for producing a meltblown nonwoven fabric according to (1) or (2), wherein the average value of 100 or more measured values is measured according to the method. (4) The ultrasonic reflection intensity values on each side are different from each other. The value of the larger reflection intensity is between 1.2 and 3.0 times the value of the smaller reflection intensity, The reflection intensity is measured under the following conditions: Distance between ultrasonic transmitter and receiver and nonwoven surface: 155mm Frequency: 360kHz Measurement temperature: 22℃ Applied voltage: 500V Wave number: 5 (burst wave) Sharp ratio: 100% Number of measurement points: 100 or more points within an area of 25 mm x 40 mm The meltblown nonwoven fabric is measured according to the average value of 100 or more measurements. (5) The meltblown nonwoven fabric according to (4), having a thickness of 0.1 mm or more and 0.4 mm or less. (6) Apparent density is 50 kg / m 3 More than 350kg / m 3The meltblown nonwoven fabric according to (4) or (5), which is as follows: (7) The meltblown nonwoven fabric according to any one of (4) to (6), having an average pore size measured by a perm porometer of 2.5 μm or more and 5.0 μm or less. (8) The meltblown nonwoven fabric according to any one of (4) to (7), wherein the average fiber diameter, which is the average value of fiber diameters of 100 or more fibers determined from an electron microscope image, is 0.5 μm or more and 3.0 μm or less. Effect of the Invention
[0009] According to the present invention, it is possible to provide a method for producing a meltblown nonwoven fabric that can produce a meltblown nonwoven fabric having good strength even without calendaring, and a meltblown nonwoven fabric that can be produced by the method. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram showing an outline of the configuration of a meltblown nonwoven fabric manufacturing apparatus. [Diagram 2] FIG. 2 is a perspective view showing an outline of a spinning die head provided in a meltblown nonwoven fabric manufacturing apparatus. [Diagram 3] 1 is a graph showing the relationship between the position in the thickness direction and the fiber occupancy rate of the meltblown nonwoven fabrics of Examples 2 and 4, analyzed by X-ray CT. [Figure 4] 1 is a graph showing the relationship between the position in the thickness direction and the fiber occupancy rate of the meltblown nonwoven fabrics of Comparative Examples 6 and 7, analyzed by X-ray CT. [Diagram 5] 1 is a grayscale image of the center of the thickness direction of the meltblown nonwoven fabric of Example 2 obtained by X-ray CT analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Meltblown nonwoven fabric manufacturing method> Hereinafter, the method for producing a meltblown nonwoven fabric will be described with reference to the drawings as necessary. Fig. 1 shows an outline of a meltblown nonwoven fabric production apparatus. Fig. 2 shows an outline of a spinning die head provided in the meltblown nonwoven fabric production apparatus as a perspective view.
[0012] The manufacturing method of meltblown nonwoven fabric is as follows: a resin ejection step of ejecting molten resin from a spinning die head 10 having a plurality of nozzle holes 11; a fiber forming step in which hot air flowing from the nozzle holes 11 toward the conveyor 12 provided opposite the spinning die head 10 is blown toward the nozzle holes 11 to fiberize the discharged molten resin and form fibers; and forming a nonwoven fabric by depositing the fibers on a conveyor using a hot air current to form a meltblown nonwoven fabric. In addition, no calendaring is carried out after the nonwoven fabric formation process.
[0013] <Resin discharge process> In the resin ejection step, molten resin is ejected from a spinning die head 10 having a plurality of nozzle holes 11 .
[0014] There is no particular limitation on the method of supplying the molten resin to the spinning die head 10. A typical method is to melt the resin supplied from a hopper 100 by passing it through an extruder 101, and supply the molten resin to the spinning die head 10 through a kneader 104.
[0015] The type of extruder 101 is not particularly limited as long as it is capable of melting the resin. As the type of extruder 101, various extruders such as a single screw extruder, a co-rotating intermeshing twin screw extruder, a co-rotating non-intermeshing twin screw extruder, a counter-rotating non-intermeshing twin screw extruder, and a multi-screw extruder can be used. Among them, a single screw extruder is preferred because it has a small resin retention area in the extruder, which makes it possible to prevent thermal deterioration of the resin during extrusion, and also because the equipment cost is low. In addition, when a resin that generates residual volatile matter is used, the extruder 101 may have a vent structure.
[0016] The form of the resin raw material to be fed into the extruder 101 is preferably a solid resin. More preferably, a pellet-shaped resin is used. The pellet-shaped resin is generally fed into the extruder 101 through a hopper 100 attached to the raw material feed port of the extruder 101.
[0017] The resin to be supplied to the extruder 101 is preferably dried by heating in advance to prevent hydrolysis or oxidative deterioration of the resin. The moisture content in the resin is preferably 200 mass ppm or less. Drying conditions vary depending on the resin, but are preferably 100° C. for 3 hours or more.
[0018] During drying, it is preferable to remove oxygen from the atmosphere in which the resin is dried, or to remove oxygen from the resin in which the resin is dried. The atmosphere during drying is preferably an inert gas atmosphere such as nitrogen. Taking into consideration the required drying time and the resin consumption time, it is preferable to use a method using a hopper-type dryer in which a drying mechanism is provided in the hopper 100 that supplies pellets to the extruder 101, a method in which a dryer is used to dry the resin before supplying it to the hopper 100, and then the resin is supplied to the hopper 100 so as not to absorb moisture, or a method using both.
[0019] Among these methods, the method using a hopper-type dryer is preferable because it allows the resin to be kept dry until immediately before it is supplied to the extruder 101 . It is even more preferable to use a dryer before the hopper 100 to quickly dry the material at high temperature in the dryer before the hopper 100 and to create a dehumidified atmosphere in the hopper-type dryer to prevent moisture from entering, because this prevents moisture from entering even at low temperatures. If the temperature in the hopper 100 is too high, problems such as blocking may occur. Specifically, the resin is dried at 120°C for 3 hours or more in a dryer before the hopper 100, and then the temperature inside the hopper-type dryer is set to 40 to 100°C, which makes it easier to achieve both suppression of the moisture content of the resin and extrusion stability.
[0020] Regarding the extruder 101, for example, a screw (not shown) used in a single screw extruder or the like can be a typical full-flight screw for an extruder with or without a vent and with a compression ratio of about 2 to 3. It is also possible to employ a special kneading mechanism such as a barrier flight to prevent the presence of unmelted material.
[0021] In the resin discharging step, the resin is discharged from each nozzle hole 11 of the spinning die head 10 at a rate of 0.006 cm 3 / min or more 0.3cm 3 The molten resin is discharged at a rate of 1 / min or less. The above-mentioned discharge rate is the discharge rate from one nozzle hole 11. The amount of resin discharged from one nozzle hole 11 is set to 0.01 cm because it is easy to stably extrude the resin and it is easy to form well-crystallized fibers with excellent strength. 3 / min or more 0.2cm 3 / min or less is preferable, and 0.02 cm 3 / min or more 0.1cm 3 / min or less is more preferable.
[0022] In the resin ejection step, the molten resin is ejected so that the temperature of the resin in the nozzle hole 11 is equal to or higher than the melting point of the resin and equal to or lower than (melting point + 100° C.). For this reason, the extrusion conditions of the extruder 101, such as the cylinder temperature, resin residence time, and extrusion amount, are adjusted so that the above conditions regarding the discharge amount and the temperature of the discharged resin are satisfied. In the subsequent fiber formation step, the temperature of the resin in the nozzle hole 11 is preferably equal to or higher than the melting point of the resin and equal to or lower than (melting point + 70° C.) so that the discharged resin can be easily and satisfactorily fiberized.
[0023] The molten resin obtained by melting means such as extruder 101 is preferably supplied to the spinning die head using gear pump 102. By using gear pump 102, fluctuations in the discharge rate in extruder 101 are absorbed, the supply quantification is significantly improved, and the discharge of the resin from nozzle hole 11 equipped in spinning die head 10 is also stabilized. The molten resin supplied quantitatively by the gear pump 102, or the molten resin supplied directly from the extruder 101, is supplied to the spinning die head 10 through, for example, a tubular flow path, and is extruded from multiple nozzle holes 11 provided in the spinning die head 10.
[0024] It is preferable to provide a foreign matter removal device such as a filter 103 in the resin flow path from the gear pump 102 to the die, or in the resin flow path from a melting means such as an extruder 101 to the spinning die head 10 if the resin does not pass through the gear pump 102 or the like. This makes it possible to trap foreign matter contained in the raw resin or foreign matter generated in the extruder or gear pump 102, thereby reducing the amount of foreign matter entering the nonwoven fabric.
[0025] As the filter 103 as a foreign matter removal device, a screen mesh, a pleated filter, a leaf disk filter, etc. can be used. Among these, a leaf disk filter is preferable in terms of filtration accuracy, filtration area, pressure resistance, time until the filter becomes clogged with foreign matter, etc. As the filter material of the filter 103, for example, a sintered nonwoven fabric of metal fibers can be used.
[0026] The molten resin discharged from the gear pump 102 is supplied to the spinning die head 10 with or without passing through a filter 103. The molten resin is supplied from the gear pump 102 or from the filter 103 to the spinning die head 10 through, for example, a kneader 104.
[0027] The molten resin supplied to spinning die head 10 by the above-described method is discharged from a plurality of nozzle holes 11 provided in spinning die head 10 as shown in FIG. The arrangement of the multiple nozzle holes 11 in the spinning die head 10 is not particularly limited as long as it is possible to produce a meltblown nonwoven fabric 2 with desired properties. Typically, the multiple nozzle holes 11 are arranged to form a row at appropriate intervals in the same direction as the width direction of the meltblown nonwoven fabric 2 formed on the conveyor 12 described below. The interval between the nozzle holes 11 is preferably, for example, 0.10 mm or more and 1.0 mm or less, and more preferably 0.25 mm or more and 0.75 mm or less. The interval between the nozzle holes 11 may be uniform or not, but is preferably uniform in terms of ease of producing a homogeneous nonwoven fabric.
[0028] The shape of the opening of each nozzle hole 11 is not particularly limited, but is usually circular, approximately circular, elliptical, approximately elliptical, etc. The opening diameter of each nozzle hole 11 is not particularly limited, and is appropriately selected depending on the fiber diameter of the fibers constituting the nonwoven fabric.
[0029] The resin used in the resin discharge step as the raw material of the meltblown nonwoven fabric 2 is not particularly limited as long as it is a resin that has been conventionally used as a raw material for meltblown nonwoven fabrics. Examples of the resin include polyolefin-based resins, polystyrene-based resins, (meth)acrylic-based resins, polyester-based resins, polyamide-based resins, and polycarbonate-based resins.
[0030] Examples of polyolefin resins include low-density polyethylene, high-density polyethylene, polypropylene, ethylene-propylene copolymer, poly-1-butene, and poly-4-methyl-1-pentene. Examples of (meth)acrylic resins include polymers of one or more (meth)acrylate monomers selected from (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. Examples of (meth)acrylic resins include polymethyl (meth)acrylate. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PNE), and polylactic acid (PLA). Examples of polyamide resins include nylon 6, nylon 6,6, nylon 12, nylon 6,12, and MXD nylon.
[0031] Among these resins, polyolefin-based resins and polyester-based resins are preferred because of their good processability when producing meltblown nonwoven fabrics, and polypropylene, polyethylene terephthalate, and polybutylene terephthalate are more preferred.
[0032] <Fiber formation process> In the fiber formation process, hot air flowing from nozzle hole 11 toward conveyor 12 provided opposite spinning die head 10 is blown toward nozzle hole 11, and the extruded molten resin is fiberized to form fibers.
[0033] When hot air is blown near the nozzle hole 11, the molten resin discharged from the nozzle hole 11 is stretched by the hot air and turned into fibers. The hot air also flows from the vicinity of the nozzle holes 11 toward the conveyor 12 disposed opposite the spinning die head 10. Therefore, the fibers stretched by the hot air are carried by the hot air current and deposited on the conveyor 12 to form the meltblown nonwoven fabric 2 in the subsequent nonwoven fabric forming process.
[0034] The method of blowing hot air is not particularly limited. Typically, hot air can be generated by heating air or an inert gas such as nitrogen pressurized by a compressor (not shown) with a heater (not shown). In addition, by colliding the hot air on the side of the conveyor 12 in the traveling direction and the hot air on the opposite side of the conveyor 12 in the traveling direction near the nozzle hole 11, the direction of the hot air flow toward the vicinity of the nozzle hole 11 can be changed to the direction from the nozzle hole 11 toward the conveyor 12.
[0035] The temperature of the hot air is above the melting point of the resin and below (melting point + 100°C), preferably above (melting point + 30°C) and below (melting point + 90°C), and more preferably above (melting point + 40°C) and below (melting point + 80°C). When the temperature of the hot air is within the above range, the resin discharged from the nozzle holes 11 can be easily stretched satisfactorily, and the fibers can be easily heat-sealed to each other on the conveyor 12 in the subsequent nonwoven fabric forming process.
[0036] The flow rate of the hot air is from 1000 NL / min / m to 7000 NL / min / m, preferably from 2000 NL / min / m to 6800 NL / min / m, and more preferably from 3000 NL / min / m to 6500 NL / min / m. When the volume of hot air is within the above range, the resin discharged from the nozzle holes 11 can be easily stretched satisfactorily, and the fibers can be easily heat-sealed to each other on the conveyor 12 in the subsequent nonwoven fabric forming process.
[0037] <Nonwoven fabric forming process> In the nonwoven fabric forming process, the fibers are deposited on the conveyor 12 by the hot air current generated in the fiber forming process to form the meltblown nonwoven fabric 2.
[0038] In the nonwoven fabric forming process, the shortest distance between the nozzle holes 11 and the conveyor 12 is set to be 10 mm or more and 75 mm or less. The nonwoven fabric forming step is performed so that the temperature of the atmosphere between the nozzle holes 11 and the conveyor 12 is 110°C or higher and 160°C or lower. By setting the shortest distance between the nozzle hole 11 and the conveyor 12 within the above range and by setting the temperature of the atmosphere between the nozzle hole 11 and the conveyor 12 within the above range, the thermal fusion property of the resin fibers near the surface of the conveyor 12 can be set within a good range that enables the formation of a meltblown nonwoven fabric with good mechanical properties. As a result, even without the calendaring process, the meltblown nonwoven fabric 2 can be manufactured with good strength. Furthermore, when the calendaring process is not performed, the breathability of the meltblown nonwoven fabric is good.
[0039] The method of setting the temperature of the atmosphere between the nozzle hole 11 and the conveyor 12 to the above range is not particularly limited. For example, the space between the nozzle hole 11 and the conveyor 12 may be surrounded by a wall in order to prevent a drop in temperature. Such a wall may be any wall capable of preventing the inflow of outside air into the space between the nozzle hole 11 and the conveyor 12. The material of such a wall may be a heat-resistant insulating material such as glass wool, rock wool, or porous ceramic. A heater may be provided to heat the space between the nozzle hole 11 and the conveyor 12. If the temperature of the space between the nozzle hole 11 and the conveyor 12 becomes too high due to the relationship between the hot air temperature and the resin temperature, a cooler may be provided to cool the space between the nozzle hole 11 and the conveyor 12.
[0040] The shortest distance between the nozzle hole 11 and the conveyor 12 is appropriately set within a range of 10 mm to 75 mm, taking into consideration the thickness and strength of the meltblown nonwoven fabric. As the shortest distance between the nozzle hole 11 and the conveyor 12 is longer, the thickness of the obtained meltblown nonwoven fabric 2 tends to increase, and the apparent density and tensile strength tend to decrease. If the shortest distance between the nozzle holes 11 and the conveyor 12 exceeds 75 mm, the apparent density of the resulting meltblown nonwoven fabric will be significantly reduced, and the meltblown nonwoven fabric will not maintain the desired strength unless it is subjected to calendaring.
[0041] The temperature of the atmosphere between the nozzle hole 11 and the conveyor 12 is 110°C or higher and 160°C or lower, as described above, preferably 115°C or higher and 155°C or lower, and more preferably 125°C or higher and 150°C or lower. The temperature of the atmosphere between the nozzle hole 11 and the conveyor 12 can be measured, for example, according to the following method. Specifically, the temperature of the atmosphere between the nozzle hole 11 and the conveyor 12 is measured by thermography from a position 2 m away from the front of the spinning die head 10 (a surface parallel to the width direction of the meltblown nonwoven fabric 2 to be produced). More specifically, for the atmosphere between the nozzle hole 11 and the conveyor 12, temperature data of 100 pixels equivalent to 2.5 mm square in actual size is measured by thermography at any position near directly above the nonwoven fabric within a range of ±250 mm away from the center position in the width direction of the spinning die head 10. The average value of the obtained temperature data of the 100 points is taken as the temperature of the atmosphere between the nozzle hole 11 and the conveyor 12.
[0042] The material of conveyor 12 is not particularly limited as long as it has heat resistance to the temperature conditions involved in the production of meltblown nonwoven fabric 2, does not fuse excessively to meltblown nonwoven fabric 2, and is a material from which meltblown nonwoven fabric 2 can be peeled off. Moreover, it is preferable that the conveyor 12 is made of a material having air permeability, and that a current of hot air is sucked by suction (not shown) from the side of the conveyor 12 on which the meltblown nonwoven fabric is formed to the back side. This makes it easier to prevent the fibers made of resin from bouncing off the conveyor 12, and makes it easier to form the meltblown nonwoven fabric 2 in which the fibers are well fused together.
[0043] The conveyor 12 is driven by rollers 13 and transports the meltblown nonwoven fabric 2 formed on the conveyor 12 to a winding device 14. The moving speed of the conveyor 12 is appropriately determined taking into consideration the amount of resin discharged and the apparent density of the resulting meltblown nonwoven fabric 2. Typically, the moving speed of the conveyor is within a range of 1.5 m / min to 6.0 m / min. The meltblown nonwoven fabric 2 formed in the nonwoven fabric forming process is wound into a roll by the winding device 14. The meltblown nonwoven fabric 2 may be cut to a predetermined length and collected as a product in the form of a sheet rather than in the form of a roll.
[0044] According to the method described above, it is possible to produce the meltblown nonwoven fabric 2 having good strength even without carrying out a calendar process. After the nonwoven fabric formation step, various treatments and processes that are conventionally performed on nonwoven fabrics can be applied to the meltblown nonwoven fabric 2. However, after the nonwoven fabric formation step, the meltblown nonwoven fabric 2 is not subjected to a calendar process because the breathability of the meltblown nonwoven fabric 2 would decrease if calendar process was performed.
[0045] In the meltblown nonwoven fabric 2 produced by the above-mentioned method for producing a meltblown nonwoven fabric, the surface state of the surface in contact with the conveyor 12 is different from that of the surface opposite to the surface in contact with the conveyor 12 . In nonwoven fabrics, the reflection intensity of ultrasonic waves is determined by the elastic modulus and density of the surface. In meltblown nonwoven fabrics, there is usually a difference between the front and back of the nonwoven fabric immediately after production. The fact that the difference between the front and back of the nonwoven fabric is reduced by calendaring indicates that the elastic modulus and density of at least one side have changed. This is thought to be the reason why the breathability performance is reduced by calendaring.
[0046] As a result, when the reflection intensity of ultrasonic waves is measured on both sides of the meltblown nonwoven fabric 2, the values of the reflection intensity of ultrasonic waves on both sides are different from each other. Specifically, the value of the larger reflection intensity is preferably 1.2 to 3.0 times the value of the smaller reflection intensity, more preferably 1.2 to 2.5 times. A meltblown nonwoven fabric having the ultrasonic reflection intensity magnification on both sides within the above range tends to have excellent strength and breathability.
[0047] The above ultrasonic reflection intensity is the average value of 100 or more measured values measured under the following measurement conditions. If the reflected wave is weak, a gain may be set in the output signal as necessary. (Reflection intensity measurement conditions) Distance between ultrasonic transmitter and receiver and nonwoven surface: 155mm Frequency: 360kHz Measurement temperature: 22℃ Applied voltage: 500V Wave number: 5 (burst wave) Sharp ratio: 100% Number of measurement points: 100 or more points within an area of 25 mm x 40 mm
[0048] The thickness of the meltblown nonwoven fabric that satisfies the above-mentioned predetermined reflectance ratio is preferably 0.1 mm or more and 0.4 mm or less, more preferably 0.1 mm or more and 0.3 mm or less. When the thickness of the meltblown nonwoven fabric is within the above range, stable production of the meltblown nonwoven fabric is easy, and a homogeneous nonwoven fabric is easily obtained after fabrication.
[0049] The apparent density of the meltblown nonwoven fabric that satisfies the above specified reflectance ratio is 50 kg / m 3 More than 350kg / m 3 Less than 100kg / m is preferable. 3 More than 350kg / m 3 The following is more preferable. When the apparent density of the meltblown nonwoven fabric is within the above range, it is easy to achieve both good strength and good breathability in the meltblown nonwoven fabric.
[0050] The average pore size of the meltblown nonwoven fabric satisfying the above-mentioned predetermined reflectance ratio, as measured by a perm porometer, is preferably 2.5 μm or more and 5.0 μm or less, more preferably 2.5 μm or more and 4.6 μm or less. When the average pore size of the meltblown nonwoven fabric is within the above range, the meltblown nonwoven fabric is likely to have both good breathability and good collection performance.
[0051] For a meltblown nonwoven fabric that satisfies the above-mentioned specified reflectance ratio, the average fiber diameter, which is the average value of the fiber diameters of 100 or more fibers determined from an electron microscope image, is preferably 0.5 μm or more and 3.0 μm or less, and more preferably 0.5 μm or more and 2.5 μm or less.
[0052] The tensile strength in the MD direction of the meltblown nonwoven fabric that satisfies the above specified reflectance ratio is 2.0 N / m 2 More than 15.0N / m 2 Less than 3.0N / m is preferable. 2 More than 10.0N / m 2 The tensile modulus in the MD direction is preferably 100 MPa or more and 400 MPa or less, more preferably 120 MPa or more and 350 MPa or less. The tensile strength in the TD direction is 2.0 N / m 2 More than 8.0N / m 2 Less than 2.5N / m is preferable. 2 More than 6.0N / m 2 The tensile modulus in the TD direction is preferably from 50 MPa to 200 MPa, more preferably from 70 MPa to 130 MPa. The tensile strength and tensile modulus are values measured according to the measurement methods in the examples described later. The MD direction is the direction along which the meltblown nonwoven fabric moves when the meltblown nonwoven fabric is produced, and the TD direction is the direction perpendicular to the MD direction.
[0053] In addition, for meltblown nonwoven fabrics, the meltblown nonwoven fabric is scanned in the thickness direction of the meltblown nonwoven fabric according to the method described later in the Examples, and X-ray CT analysis is performed to obtain data on the fiber distribution in a plane perpendicular to the thickness direction of the meltblown nonwoven fabric, thereby determining the fiber occupancy rate at each position in the thickness direction of the meltblown nonwoven fabric. According to the above-mentioned X-ray CT analysis, for a meltblown nonwoven fabric, the average fiber occupancy FO1 of a 15% area from the surface of one side, the average fiber occupancy FO2 of a 15% area from the surface of the other side, and the average fiber occupancy AFO of the meltblown nonwoven fabric can be calculated. For meltblown nonwoven fabrics, having a gradient in the fiber occupancy in a plane perpendicular to the thickness direction tends to provide excellent strength and breathability. Specifically, the occupancy change rate calculated by the following formula is preferably 10% or more, more preferably 12% to 30%, and even more preferably 13% to 25%. Meltblown nonwoven fabrics having an occupancy change rate within the above range tend to provide excellent strength and breathability. Occupancy change rate (%) = (│FO1-FO2│) / AFO×100
[0054] The meltblown nonwoven fabric described above can be easily produced by the above-mentioned method. The meltblown nonwoven fabric has both good strength and good breathability, and is therefore suitable for use in filters. More specifically, the meltblown nonwoven fabric is preferably used as a filter for extracorporeal circulation therapy, purification of antibody drugs, purification of viruses for gene therapy, and the like. EXAMPLES
[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0056] [Examples 1 to 4 and Comparative Examples 1 to 7] Using the meltblown nonwoven fabric manufacturing apparatus 1 having the configuration shown in FIG. 1, a meltblown nonwoven fabric having a width of 600 mm was manufactured under the conditions shown in Table 1. Polyethylene terephthalate (PET, melting point 260°C) was used as the resin. The spinning nozzle used had a nozzle hole diameter of 0.25 mm, a hole interval of 0.25 mm, and 1200 holes. The conveyor movement speed was 2.9 m / min.
[0057] In the examples, no calendering was performed after the meltblown nonwoven fabric was obtained. For the comparative example, the meltblown nonwoven fabric was subjected to calendering using calender rolls having the roll temperatures shown in Table 1, with the inter-roll clearance being 0.10 to 0.11 mm.
[0058] The meltblown nonwoven fabrics obtained in Examples 1 to 4 and the calendered meltblown nonwoven fabrics obtained in Comparative Examples 1 to 7 were measured for thickness and apparent density. In addition, the average pore size, average fiber diameter, coefficient of variation, tensile strength, tensile modulus, ultrasonic reflection intensity, and air permeability were measured according to the following methods. The measurement results are shown in Tables 2 to 4.
[0059] <Average pore diameter> The mean flow pore size measured using a Perm Porometer (PMI) was used as the average pore size.
[0060] <Average fiber diameter, coefficient of variation> A part of the meltblown nonwoven fabric was used as a sample and observed with a scanning electron microscope. Based on the obtained electron microscope image, the diameters of 100 or more randomly selected fibers were measured. The number average of the 100 or more measured values was taken as the average fiber diameter. The standard deviation of the fiber diameter was divided by the average fiber diameter to obtain the coefficient of variation.
[0061] <Tensile strength, tensile modulus> The meltblown nonwoven fabric was measured for tensile strength and tensile modulus in both the MD and TD directions. The MD direction is the direction along which the meltblown nonwoven fabric moves when the meltblown nonwoven fabric is produced, and the TD direction is the direction perpendicular to the MD direction. A test piece measuring 8 mm in width and 40 mm in length was cut out from the obtained meltblown nonwoven fabric. Both ends of the test piece were fixed with a chuck using a universal testing machine (A&D, RTG-1210), and the test piece was pulled at a chuck distance of 20 mm and a pulling speed of 20 mm / min. The relationship between the chuck distance and the load was plotted, and the tensile strength and tensile modulus were calculated based on the following formula. Tensile strength (N / m 2) = (load at break) / cross-sectional area of specimen Tensile modulus (MPa) = (load change when the chuck distance is stretched by 0-2% before the start of the test / cross-sectional area of the test piece) / (0-2% stretch / initial length of the test piece)
[0062] <Ultrasonic reflection intensity> In an area of 75 mm x 75 m in the meltblown nonwoven fabric, 100 or more ultrasonic reflection intensity measurements were taken according to the following measurement conditions. The average ultrasonic reflection intensity of the 100 or more points was taken as the ultrasonic reflection intensity. The ultrasonic reflection intensity was measured on the surface that was in contact with the conveyor 12 during the production of the meltblown nonwoven fabric and on the surface that faced the nozzle hole 11.
[0063] (Reflection intensity measurement conditions) Distance between ultrasonic transmitter and receiver and nonwoven surface: 155mm Frequency: 360kHz Measurement temperature: 22℃ Applied voltage: 500V Wave number: 5 (burst wave) Sharp ratio: 100% Number of measurement points: 100 or more points within an area of 25 mm x 40 mm
[0064] Specifically, ultrasonic waves were transmitted and received from an ultrasonic transducer (ultrasonic transmitter and receiver) connected to a pulsar receiver (ULTRA SONIC RECEIVER JPR600C, manufactured by Japan Probe Co., Ltd.), and the ultrasonic reflection intensity was measured. The pulsar receiver was connected to a high-speed digitizer (NI PIX-1033 (chassis), NI PIX-5114, manufactured by National Instruments Co., Ltd.), and the high-speed digitizer was connected to a personal computer for data processing.
[0065] <Breathability> Four or eight sheets of the meltblown nonwoven fabric obtained in the Examples and Comparative Examples were stacked together to form a sheet having an area of 642 mm 2300mL of air was passed through the ventilation surface of the material with a weight of 567g, and the time (seconds) required for the entire 300mL of air to pass through was measured to evaluate the breathability. A Gurley densometer (manufactured by TOYOSEIKI) was used to evaluate the breathability. With respect to the meltblown nonwoven fabric, the surface that was in contact with the conveyor 12 during production of the meltblown nonwoven fabric is designated as surface A, and the surface that faced the nozzle hole 11 of the meltblown nonwoven fabric is designated as surface B. The surfaces were stacked such that the surfaces A and the surfaces B did not come into contact with each other. Air was supplied from side B. For Example 2 and Comparative Example 1, the breathability of the 32-ply meltblown nonwoven fabric was also evaluated.
[0066] [Table 1]
[0067] [Table 2]
[0068] [Table 3]
[0069] [Table 4]
[0070] For example, when comparing the meltblown nonwoven fabric of Example 2 with the meltblown nonwoven fabrics of Comparative Examples 2 and 3, which have similar thickness, apparent density, average pore size, and average fiber diameter, it is found that the tensile strength and tensile modulus of the meltblown nonwoven fabric of Example 2 are equivalent to or superior to those of the meltblown nonwoven fabrics of Comparative Examples 2 and 3, even though the meltblown nonwoven fabric of Example 2 was not calendared. In addition, a comparison between the meltblown nonwoven fabric of Example 2 and the meltblown nonwoven fabric of Comparative Example 2 reveals that the meltblown nonwoven fabric of Example 2, which is not calendared, has better breathability than the meltblown nonwoven fabric of Comparative Example 2, which is calendared.
[0071] From Table 4, it can be seen that the ratio of ultrasonic reflection intensity on both sides of the meltblown nonwoven fabric of the embodiment is 1.2 or more and 3.0 or less because it is not calendared. Furthermore, Tables 1 to 3 show that in Comparative Example 1, in which the nozzle hole-to-conveyor distance exceeded 75 mm, the apparent specific gravity of the resulting meltblown nonwoven fabric was low and the strength of the meltblown nonwoven fabric was poor.
[0072] [Examples 5, 6, and Comparative Examples 8 to 10] Using the meltblown nonwoven fabric manufacturing apparatus 1 having the configuration shown in Fig. 1, a meltblown nonwoven fabric was manufactured under the conditions shown in Table 5. Polypropylene (PP, melting point 160°C) was used as the resin. The meltblown nonwoven fabrics obtained in Examples 5, 6, and Comparative Examples 8 to 10 were measured for thickness, apparent density, average pore size, average fiber diameter, and coefficient of variation in the same manner as in Example 1. The measurement results are shown in Tables 2 to 6.
[0073] [Table 5]
[0074] [Table 6]
[0075] For the meltblown nonwoven fabrics of Examples 5 and 6, the ratio of ultrasonic reflection intensity between both surfaces was measured in the same manner as in Example 1, and all were 1.2 or more and 3.0 or less. In addition, the meltblown nonwoven fabrics of Comparative Examples 8 to 10 were produced under conditions where the nozzle hole-to-conveyor distance exceeded 75 mm, and therefore had significantly low apparent densities. For this reason, the meltblown nonwoven fabrics of Comparative Examples 8 to 10 cannot ensure the desired strength unless they are calendered.
[0076] In addition, the meltblown nonwoven fabrics of Example 2, Example 4, Comparative Example 6, and Comparative Example 7 were analyzed by X-ray CT. This analysis allows us to determine the fiber occupancy rate at each position in the thickness direction of the meltblown nonwoven fabric. Graphs of the analysis results are shown in Figures 3 and 4. In the graphs of Figures 3 and 4, the plus side of the thickness direction (µm) axis is the direction toward the conveyor side of the meltblown nonwoven fabric in the thickness direction, and the minus side is the direction toward the nozzle side of the meltblown nonwoven fabric in the thickness direction.
[0077] Specifically, the analysis using X-ray CT was carried out as follows. As the X-ray CT device, a micro X-ray CT scanner (MicroXCT-400) manufactured by Xradia was used. The meltblown nonwoven fabric was scanned in the thickness direction by the device to obtain fiber distribution data in the meltblown nonwoven fabric. From the scan data, two-dimensional data on the distribution of fibers was obtained at intervals of 0.05 mm in thickness. The obtained two-dimensional data was then grayscaled. As an example of a grayscaled image, a grayscale image of the center in the thickness direction of the meltblown nonwoven fabric of Example 2 is shown in FIG. 4. Pixel values were generated from the data of the grayscaled image. Based on the obtained pixel values, a predetermined binarization process was performed on the grayscale image. For the binarized grayscale image, the ratio of the total area of the fiber portion to the total area of the image (fiber occupancy rate (%)) was calculated.
[0078] The binarization process will be explained below. When performing the binarization process, a histogram of the distribution of pixels for each luminance (256 levels of gradation (0 to 255) in an 8-bit image) was first obtained for the grayscaled image. The obtained histogram, with luminance on the horizontal axis, has two peaks. From the obtained histogram, the maximum luminance value I max and the minimum luminance value I min and the average brightness μ 0 I asked for max and I min An arbitrary threshold T was selected between . The histogram was divided into two classes, class 1 and class 2, at the boundary of threshold T. Class 1 and class 2 each contain one peak. The variance for class 1, σ 1 2 and the average μ 1 and frequency n 1 The variance for class 2, σ 2 2 and the average μ 2 and frequency n 2 He asked for:
[0079] Next, the within-class variance σ w 2 and the between-class variance σ b 2 He asked for:
number
[0080] The obtained within-class variance σ w 2 and the between-class variance σ b 2 From this, the resolution S was calculated using the following formula.
number
[0081] Maximum I max and the minimum value I minThe degree of separation S was calculated according to the above method for all threshold values T between and . The threshold value T at which the degree of separation S was maximized was adopted as the threshold value in the binarization method.
[0082] Table 7 below shows the average fiber occupancy (%) (AFO) at each position in the thickness direction of the meltblown nonwoven fabric obtained from the above X-ray CT analysis results, the average fiber occupancy within a range of 15% from the surface on the nozzle hole side (FO1), the average fiber occupancy within a range of 15% from the surface on the conveyor side (FO2), the difference in the average fiber occupancy on both sides (15% from the surface of each side) (│(FO1-FO2│), and the occupancy change rate (%) calculated by the following formula. Occupancy change rate (%) = (│FO1-FO2│) / AFO×100 [Table 7]
[0083] As described above, the meltblown nonwoven fabrics of Examples 2 and 4, which are excellent in strength and breathability, exhibit a high occupancy change rate of 10% or more. [Explanation of symbols]
[0084] 1: Meltblown nonwoven fabric manufacturing equipment 2: Meltblown nonwoven fabric 10: Spinning die head 11: Nozzle hole 12: Conveyor 13: Roller 14: Winding device 100: Hopper 101: Extruder 102: Gear pump 103: Filter 104: Kneading machine
Claims
1. The reflected ultrasonic intensity values on both sides are different from each other. the greater reflection intensity value is 1.2 times or more and 3.0 times or less than the smaller reflection intensity value, The reflection intensity is measured under the following conditions: Distance between ultrasonic transmitter and receiver and nonwoven surface: 155 mm Frequency: 360kHz Measurement temperature: 22℃ Applied voltage: 500V Wave number: 5 (burst wave) Sharp ratio: 100% Number of measurement points: 100 or more points within a 25 mm x 40 mm area is the average value of 100 or more measured values measured according to The thickness is 0.1 mm or more and 0.4 mm or less, Apparent density 50 kg / m 3 More than 350kg / m 3 is as follows: The average pore size measured by a perm porometer is 2.5 μm or more and 5.0 μm or less, The average fiber diameter, which is the average value of fiber diameters of 100 or more fibers determined from an electron microscope image, is 0.5 μm or more and 3.0 μm or less, A meltblown nonwoven fabric made of a polyolefin resin, a polystyrene resin, a (meth)acrylic resin, a polyester resin, or a polycarbonate resin.
2. The meltblown nonwoven fabric is scanned in the thickness direction of the meltblown nonwoven fabric to obtain data on the fiber distribution in a plane perpendicular to the thickness direction of the meltblown nonwoven fabric. The average fiber occupancy FO1 of a 15% region from the surface of one side, the average fiber occupancy FO2 of a 15% region from the surface of the other side, and the average fiber occupancy AFO of the meltblown nonwoven fabric are calculated from the results of the X-ray CT analysis, and the following formula is used: Occupancy rate change rate (%) = (│FO1-FO2│) / AFO × 100 The occupancy rate change rate calculated based on is 10% or more, The thickness is 0.1 mm or more and 0.4 mm or less, Apparent density 50 kg / m 3 More than 350kg / m 3 is as follows: The average pore size measured by a perm porometer is 2.5 μm or more and 5.0 μm or less, The average fiber diameter, which is the average value of fiber diameters of 100 or more fibers determined from an electron microscope image, is 0.5 μm or more and 3.0 μm or less, A meltblown nonwoven fabric made of a polyolefin resin, a polystyrene resin, a (meth)acrylic resin, a polyester resin, or a polycarbonate resin.
3. The meltblown nonwoven fabric is scanned in the thickness direction of the meltblown nonwoven fabric to obtain data on the fiber distribution in a plane perpendicular to the thickness direction of the meltblown nonwoven fabric. The average fiber occupancy FO1 of a 15% region from the surface of one side, the average fiber occupancy FO2 of a 15% region from the surface of the other side, and the average fiber occupancy AFO of the meltblown nonwoven fabric are calculated from the results of the X-ray CT analysis, and the following formula is used: Occupancy rate change rate (%) = (│FO1-FO2│) / AFO × 100 The meltblown nonwoven fabric according to claim 1, wherein the occupancy rate change rate calculated based on is 10% or more.
Citation Information
Patent Citations
Production of pierced melt-blown nonwoven fabric and device therefor
JP1991260153A
Paper-like non-woven fabric
JP1994136656A
Polyamide ultrafine fiber nonwoven fabric and its production
JP1996144166A
Laminated nonwoven fabric, its manufacture, thermal stencil base sheet and its manufacture
JP2000238156A
Porous sheet
JP2001248057A