Antifouling paint composition

The antifouling paint composition with photocurable organopolysiloxane and slip agent addresses low-temperature adhesion issues, providing a durable and cost-effective solution for substrates by enhancing adhesion and reducing maintenance needs.

JP7573638B2Active Publication Date: 2024-10-25CHUGOKU MARINE PAINTS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022553830
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-29
Filing Date
2021-09-17
Publication Date
2024-10-25
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

Organopolysiloxane-based antifouling coatings face challenges with low adhesion to substrates, particularly in low-temperature environments, requiring special undercoat films and frequent repainting, which complicates application and increases costs.

Method used

An antifouling paint composition containing photocurable organopolysiloxane, a slip agent, and a photopolymerization initiator, which forms a coating film with excellent adhesion to substrates even at low temperatures and enhances antifouling properties.

Benefits of technology

The composition enables the formation of a durable antifouling coating with improved adhesion and reduced maintenance intervals, particularly in cold conditions, thereby reducing economic burdens associated with frequent repainting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573638000001
    Figure 0007573638000001
  • Figure 0007573638000002
    Figure 0007573638000002
  • Figure 0007573638000003
    Figure 0007573638000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide an antifouling coating composition whereby it is possible to form an antifouling coating film having excellent adhesion to a substrate (base material) even in a low-temperature environment, as well as excellent antifouling properties. Another purpose of the present invention is to provide an antifouling coating film formed from the antifouling coating composition, a layered antifouling coating film, an antifouling tape, a base material provided with the antifouling coating film, and a method for manufacturing the same, and an antifouling method. This antifouling coating composition contains a photocurable organopolysiloxane (A), a lubricant (B), and a photopolymerization initiator, the content of the photocurable organopolysiloxane (A) with respect to the solid content of the antifouling coating composition being 50-98% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antifouling coating composition, an antifouling coating film using the same, a laminated antifouling coating film, an antifouling tape, a substrate with an antifouling coating film, a method for producing the same, and an antifouling method. [Background technology]

[0002] Organopolysiloxane-based antifouling coating films are widely used to prevent adhesion of aquatic organisms to ships, underwater structures, fishing equipment, etc. Due to their properties such as low surface free energy and low elastic modulus, these antifouling coating films are able to prevent the attachment and settlement of macroorganisms such as barnacles and mussels, and also have the excellent advantage of being less environmentally hazardous than conventional antifouling coating films of the hydration decomposition type or hydrolysis type, which release coating components into the environment.

[0003] For example, Patent Document 1 discloses an antifouling coating film formed from a curable polysiloxane composition. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 077204 Summary of the Invention [Problem to be solved by the invention]

[0005] Although organopolysiloxane-based antifouling coating films can reduce adhesion to aquatic organisms, they have the disadvantage that they have low adhesion to the substrate and it is difficult to obtain strong adhesion to the substrate. This tendency is particularly noticeable in low temperature environments (e.g., 5°C), and as in the above-mentioned Patent Document 1, a special undercoat coating film is required, and even if such a film is used, there are drawbacks such as a long coating interval being required between the application of the undercoat and the application of the antifouling coating composition. The object of the present invention is to provide an antifouling coating composition capable of forming an antifouling coating film having excellent adhesion to a substrate (base material) even in a low temperature environment and also excellent antifouling properties. Another object of the present invention is to provide an antifouling coating film formed from the antifouling coating composition, a laminated antifouling coating film, an antifouling tape, a substrate with an antifouling coating film, a method for producing the same, and an antifouling method. [Means for solving the problem]

[0006] Means for Solving the Problems The present inventors have conducted intensive research in view of the above-mentioned problems and have found that a coating film formed from an antifouling coating composition containing a photocurable organopolysiloxane (A), a slipping agent (B), and a photopolymerization initiator (C) has good adhesion to the substrate even at low temperatures and also has excellent antifouling properties, thereby completing the present invention.

[0007] The present invention relates to the following [1] to

[16] . [1] An antifouling coating composition comprising a photocurable organopolysiloxane (A), a slipping agent (B), and a photopolymerization initiator (C), wherein the content of the photocurable organopolysiloxane (A) in the solid content of the antifouling coating composition is 50 mass% or more and 98 mass% or less. [2] The antifouling coating composition according to [1], wherein the photocurable organopolysiloxane (A) has a (meth)acryloyl group. [3] The antifouling coating composition according to [1] or [2], wherein the photocurable organopolysiloxane (A) is represented by the following formula (I):

[0008] X p R 1 (3-p) SiO(SiR 1 2O) m (SiX q R 1 (2-q) O) n Six p R 1 (3-p) (I) (In formula (I), R 1each independently represents an alkyl group, an aryl group, an aralkyl group, an alkoxy group, or a halogenated alkyl group having 1 to 10 carbon atoms; each X independently represents a monovalent organic group having one or more (meth)acryloyl groups and not containing a silicon atom; m represents 10 or more and 10,000 or less; n represents 0 or more and 50 or less; each p independently represents an integer of 0 or more and 2 or less; each q independently represents 1 or 2; and at least one of p and n is 1 or more.

[0009] [4] The antifouling coating composition according to any one of [1] to [3], wherein the photocurable organopolysiloxane (A) has a weight average molecular weight (Mw) of 10,000 or more and 100,000 or less. [5] The antifouling coating composition according to any one of [1] to [4], wherein the photocurable organopolysiloxane (A) has a functional group equivalent of 300 g / mol or more and 50,000 g / mol or less. [6] The antifouling coating composition according to any one of [1] to [5], wherein the slipping agent (B) is at least one selected from the group consisting of phenyl-modified silicones, polyether-modified silicones, and acrylic polymers having a hydrophilic group. [7] The antifouling coating composition according to any one of [1] to [6], wherein the content of the slip agent (B) in the solid content of the antifouling coating composition is from 0.1% by mass to 40% by mass. [8] The antifouling coating composition according to any one of [1] to [7], wherein the total content of the photocurable organopolysiloxane (A) and the slipping agent (B) in the solid content of the antifouling coating composition is 70 mass% or more and 99 mass% or less. [9] The antifouling coating composition according to any one of [1] to [8], further comprising a silane coupling agent (D).

[10] An antifouling coating film formed from the antifouling coating composition according to any one of [1] to [9].

[11] A laminated antifouling coating film comprising an undercoat coating film and the antifouling coating film described in

[10] .

[12] An antifouling tape having the antifouling coating film according to

[10] or the laminated antifouling coating film according to

[11] , and an adhesive layer.

[13] A substrate with an antifouling coating film, comprising the antifouling coating film according to

[10] , the laminated antifouling coating film according to

[11] , or the antifouling tape according to

[12] on the substrate.

[14] The substrate with an antifouling coating film according to

[13] , wherein the substrate is one selected from the group consisting of ships, underwater structures, fishing equipment, and cables.

[15] A method for producing a substrate with an antifouling coating film, comprising the steps of applying the antifouling coating composition according to any one of [1] to [9] to a substrate, and irradiating the applied coating film with active energy rays.

[16] An antifouling method, which uses the antifouling coating film described in

[10] , the laminated antifouling coating film described in

[11] , or the antifouling tape described in

[12] . Effect of the Invention

[0010] According to the present invention, it is possible to provide an antifouling coating composition capable of forming an antifouling coating film having excellent adhesion to a base (substrate) even in a low-temperature environment and also excellent antifouling properties. In addition, according to the present invention, it is possible to provide an antifouling coating film formed from the antifouling coating composition, a laminated antifouling coating film, an antifouling tape, a substrate with an antifouling coating film, a manufacturing method thereof, and an antifouling method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The antifouling coating composition according to the present invention, the antifouling coating film using the same, the laminated antifouling coating film, the antifouling tape, the substrate with an antifouling coating film, the production method thereof, and the antifouling method will be described in detail below. In the following description, "(meth)acryloyl", "(meth)acrylate", "(meth)acrylic acid", and "(meth)acrylic" mean "acryloyl and / or methacryloyl", "acrylate and / or methacrylate", "acrylic acid and / or methacrylic acid", and "acrylic and / or methacrylic", respectively.

[0012] [Anti-fouling paint composition] The antifouling coating composition of the present invention (hereinafter also simply referred to as "the composition" or "coating composition") contains a photocurable organopolysiloxane (A), a slipping agent (B), and a photopolymerization initiator (C), and is characterized in that the content of the photocurable organopolysiloxane (A) in the solid content of the antifouling coating composition is 50 mass % or more and 98 mass % or less. According to the present invention, it is possible to provide an antifouling coating composition capable of forming an antifouling coating film having excellent adhesion to a substrate (base material) even in a low temperature environment and also excellent antifouling properties. Furthermore, by using the antifouling coating of the present invention, antifouling work including the formation of an antifouling coating film can be completed in a short time. In particular, in the case of work on ships, there is a great advantage in that the economic burden such as docking costs required according to the time required for work can be reduced. Although the detailed mechanism of action by which the above-mentioned effects are obtained is not necessarily clear, part of it is presumed to be as follows. That is, in order for a conventional organopolysiloxane-based antifouling coating film to suppress biofouling in water, it is necessary to compound a slipping agent that promotes aquatic organisms to slide off the surface by the water flow generated when the substrate moves through the water or the water flow generated in the water when the aquatic organisms come into contact with the coating film surface and when they grow on the surface after contact. Meanwhile, this slipping agent is usually liquid at room temperature (hereinafter, 25°C) or becomes liquid by interaction with water in the external environment, and further, in order to function as a slipping agent, it is necessary to have a certain difference in polarity from the curable organopolysiloxane used in combination. Therefore, even if the curable organopolysiloxane and the slipping agent are in a certain mixed state or in a micro-separated state due to the mixing operation before the coating composition is applied, phase separation may progress before the applied coating composition dries and hardens, and the liquid slipping agent may become unevenly distributed in the vicinity of the base (substrate), and in the worst case, a liquid layer may be formed, which may inhibit adhesion to the base (substrate). In particular, in a low temperature environment, the compatibility of components with different polarities decreases, making phase separation more likely to progress, and the effects of the above phenomenon are thought to be significant. However, by using the photocurable organopolysiloxane (A) in the present composition, the drying and curing time can be significantly shortened, which is believed to suppress the occurrence of the above-mentioned phase separation phenomenon and enable the composition to exhibit good adhesion to the base (substrate).

[0013] <Photocurable organopolysiloxane (A)> The present composition contains a photocurable organopolysiloxane (A) for the purpose of improving the substrate adhesion in a low-temperature environment (hereinafter also simply referred to as "low-temperature adhesion") and the antifouling properties of the antifouling coating film to be formed. The photocurable organopolysiloxane (A) is an organopolysiloxane compound that initiates polymerization by irradiation with active energy rays, due to active species such as radicals generated by a photopolymerization initiator (C) described below. The proportion of organopolysiloxane in the molecules of the photocurable organopolysiloxane (A) is preferably 50% by mass or more, more preferably 70% by mass or more, from the viewpoint of ensuring that the antifouling coating film formed has good antifouling properties.

[0014] Examples of the photocurable organopolysiloxane (A) include photoradical curable organopolysiloxanes in which the active species generated by irradiation with active energy rays to initiate polymerization is radical, photocationic curable organopolysiloxanes in which the active species is cation, and photoanionic curable organopolysiloxanes in which the active species is anion. Photoradical curable organopolysiloxanes are preferred from the viewpoints of curability of the coating composition, excellent strength and durability of the coating film formed, and low environmental load, while photocationic curable organopolysiloxanes and photoanionic curable organopolysiloxanes are preferred from the viewpoints of excellent adhesion to the substrate and resistance to curing inhibition by oxygen.

[0015] When the photocurable organopolysiloxane (A) is a photoradical curable organopolysiloxane, from the viewpoints of providing the antifouling coating composition with suitable storage stability, pot life, and curability, and of providing an antifouling coating film that is formed with good low-temperature adhesion and antifouling properties, it is preferably an organopolysiloxane having a (meth)acryloyl group, and is, for example, a compound represented by the following formula (I): In addition, examples of the photoradical polymerizable group include vinyl groups and allyl groups, but from the viewpoint of curability, (meth)acryloyl groups are preferred as the photoradical polymerizable group. In addition, vinyl groups directly bonded to silicon atoms have low radical polymerizability, and in the present invention, vinyl groups directly bonded to silicon atoms do not correspond to photoradical polymerizable groups.

[0016] X p R 1 (3-p) SiO(SiR 1 2O) m (SiX q R 1 (2-q) O) n Six p R 1 (3-p) (I) (In formula (I), R 1 each independently represents an alkyl group, an aryl group, an aralkyl group, an alkoxy group, or a halogenated alkyl group having 1 to 10 carbon atoms; each X independently represents a monovalent organic group having one or more (meth)acryloyl groups and not containing a silicon atom; m represents 10 or more and 10,000 or less; n represents 0 or more and 50 or less; each p independently represents an integer of 0 or more and 2 or less; each q independently represents 1 or 2; and at least one of p and n is 1 or more.

[0017] In formula (I), R 1 each independently represents an alkyl group having from 1 to 10 carbon atoms, an aryl group, an aralkyl group, an alkoxy group, or a halogenated alkyl group. R 1The alkyl group in the formula (I) has 1 to 10 carbon atoms, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and a heptyl group. R 1 The aryl group in the formula (I) has 6 to 10 carbon atoms and may have a substituent such as an alkyl group on the aromatic ring. Examples of the aryl group include a phenyl group, a tolyl group (methylphenyl group), a xylyl group (dimethylphenyl group), and a naphthyl group. R 1 The aralkyl group in the formula (I) has 7 to 10 carbon atoms, and examples thereof include a benzyl group, a 2-phenylethyl group, a 2-naphthylethyl group, and a diphenylmethyl group. R 1 The halogenated alkyl group in the formula (I) has 1 to 10 carbon atoms, and examples thereof include groups in which some or all of the hydrogen atoms contained in the alkyl group are replaced with halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. Among these, R in formula (I) 1 is preferably an alkyl group, an aryl group, an aralkyl group, or a halogenated alkyl group, more preferably an alkyl group or an aryl group, and further preferably a methyl group. In this specification, R 1 When a plurality of the same groups are present, they may be the same or different.

[0018] In formula (I), each X independently represents a monovalent organic group having one or more (meth)acryloyl groups and not containing a silicon atom. In view of the good curability of the coating composition, it is preferable for it to be a group having an acryloyl group, and more preferable for it to be a group having an acryloyloxy group.

[0019] X is preferably a group represented by the following formula (II):

[0020] [ka] (In formula (II), R 2each independently represents a hydrogen atom or a methyl group; R 3 represents a (1+x)-valent hydrocarbon group having 2 to 100 carbon atoms, and R 3 any methylene group may be substituted with an ether bond, an ester bond, a thioether bond, a urethane bond, or an amide bond, a portion of the hydrogen atoms in the hydrocarbon group may be substituted with a hydroxyl group or a halogen atom, and x represents an integer of 1 or more and 10 or less.

[0021] In formula (II), R 2 is a hydrogen atom or a methyl group, and is preferably a hydrogen atom. R 3 represents a (1+x)-valent hydrocarbon group having 2 or more and 100 or less carbon atoms, and the number of carbon atoms is preferably 2 or more and 50 or less, more preferably 2 or more and 30 or less, and further preferably 2 or more and 10 or less. R 3 In the above, any methylene group may be substituted with an ether bond, an ester bond, a thioether bond, or an amide bond, and is preferably substituted with an ether bond or an ester bond, and more preferably substituted with an ether bond. x is an integer of 1 or more and 10 or less, and is preferably 1 or 2.

[0022] Examples of X include the following (IIa) to (IIg).

[0023] [ka]

[0024] [ka]

[0025] Among these, (IIa) to (IIf) are preferable, and (IIb) and (IId) are more preferable.

[0026] In this specification, when two or more different repeating units are described in parallel between [ ], it means that those repeating units may be repeated in any form and order of random, alternating or block. That is, for example, in the formula -[X3-Y3]- (where X and Y represent repeating units), the repeating units may be random, such as -XXYXYY-, alternating, such as -XYXYXY-, or block, such as -XXXYYY- or -YYYXXX-.

[0027] In formula (I), m is 10 or more and 10,000 or less, and from the viewpoint of improving the physical properties such as flexibility, elongation, base conformability, strength, impact resistance, and other properties of the antifouling coating film to be formed, and is preferably 100 or more, more preferably 200 or more, and is preferably 1,000 or less, more preferably 500 or less. In formula (I), n is 0 or more and 50 or less. However, when each of p's described below is 0, n is 1 or more and 50 or less. For the same reasons as above, n is preferably 2 or more and 20 or less, and n / m is preferably 0 or more and 1 / 5 or less, more preferably 0 or more and 1 / 20 or less, and even more preferably 0 or more and 1 / 50 or less. Here, m and n respectively represent the average repeating number of the corresponding partial structures, and can be appropriately adjusted so as to satisfy the weight average molecular weight below. In formula (I), each p is independently an integer of 0 or more and 2 or less. When the aforementioned n is 0, at least 1 p is 1 or 2.

[0028] On the other hand, when the photocurable organopolysiloxane (A) is a photocationically curable organopolysiloxane, an organopolysiloxane having a glycidyl group in the molecule can be used, and on the other hand, when it is a photoanionically curable organopolysiloxane, an organopolysiloxane having a glycidyl group or a cyanoacrylate group in the molecule can be used.

[0029] The weight average molecular weight (Mw) of the photocurable organopolysiloxane (A) is usually 5,000 or more and 200,000 or less, and from the viewpoint of improving the production workability of the coating composition, the coating workability, the curing property, and the strength of the antifouling coating film formed, it is preferably 10,000 or more, more preferably 12,000 or more, even more preferably 15,000 or more, and is preferably 100,000 or less, more preferably 70,000 or less, even more preferably 50,000 or less. From the viewpoints of improving the production workability of the coating composition, the coating workability, and the curing properties, and the strength of the antifouling coating film formed, the number average molecular weight of the photocurable organopolysiloxane (A) is preferably 3,000 or more, more preferably 4,000 or more, and even more preferably 5,000 or more, and is preferably 50,000 or less, more preferably 30,000 or less, and even more preferably 20,000 or less. In the present invention, the "weight average molecular weight (Mw)" and "number average molecular weight (Mn)" of the photocurable organopolysiloxane (A) and other oligomers / polymers (N) described below are measured using GPC (gel permeation chromatography) and calculated using standard polystyrene of known molecular weight.

[0030] From the viewpoint of improving the curability and the strength and antifouling properties of the antifouling coating film formed, the functional group equivalent of the photocurable organopolysiloxane (A) (mass per mole of curable functional group) is preferably 300 g / mol or more, more preferably 500 g / mol or more, even more preferably 700 g / mol or more, still more preferably 1,000 g / mol or more, and is preferably 50,000 g / mol or less, more preferably 30,000 g / mol or less, even more preferably 20,000 g / mol or less, still more preferably 15,000 g / mol or less, and particularly preferably 10,000 g / mol or less. When two or more types of photocurable organopolysiloxanes (A) are used, it is preferred that the functional group equivalent of the photocurable organopolysiloxanes (A) as a whole falls within the above range. The functional group equivalent may be approximated by a value obtained by dividing the number average molecular weight by the number of functional groups per molecule.

[0031] The viscosity of the photocurable organopolysiloxane (A) at 23°C is preferably at least 100 mPa·s, more preferably at least 200 mPa·s, and is preferably at most 50,000 mPa·s, more preferably at most 2,000 mPa·s, from the viewpoints of improving the production workability of the coating composition, the coating workability, and the curing property, and the strength of the antifouling coating film formed. In this specification, the viscosity of the photocurable organopolysiloxane (A) at 23° C. refers to the viscosity measured with a B-type rotational viscometer (for example, Model BM, manufactured by Tokyo Keiki Co., Ltd.).

[0032] The photocurable organopolysiloxane (A) may be used alone or in combination of two or more. In the following description, when two or more types are used in combination, the preferred content is the preferred range of the total amount of the components. From the viewpoint of improving the antifouling properties and strength of the antifouling coating film to be formed, the content of the photocurable organopolysiloxane (A) in the coating composition is preferably 40 mass % or more, more preferably 50 mass % or more, even more preferably 60 mass % or more, and is preferably 98 mass % or less, more preferably 95 mass % or less, even more preferably 90 mass % or less. The content of the photocurable organopolysiloxane (A) in the solid content of the antifouling coating composition is 50 mass% or more, preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 80 mass% or more, and is 98 mass% or less, preferably 97 mass% or less, and more preferably 95 mass% or less. In this specification, the "solid content of the coating composition" refers to the components excluding the non-reactive solvent (E) described below and the volatile components contained as solvents in each component, and the "content in the solid content of the coating composition" can be calculated as the content in the residue obtained by drying the coating composition in a hot air dryer at 125°C for 1 hour. Therefore, the "solid content of the coating composition" does not necessarily mean that it is in a solid state, but may be in a liquid state.

[0033] From the viewpoint of improving the antifouling properties and strength of the antifouling coating film formed, the total content of the photocurable organopolysiloxane (A) and the slipping agent (B) described below in the solids of the antifouling coating composition of the present invention is preferably 70 mass % or more, more preferably 80 mass % or more, and is preferably 99 mass % or less, more preferably 98 mass % or less.

[0034] As the photocurable organopolysiloxane (A), a commercially available product may be used. For example, the commercially available product is "TEGO Rad 2650" manufactured by Evonik Industries AG (wherein R 1 are methyl groups, all p's are 1, n is 0, X is a group represented by formula (IId) (a=3), Mw: 17,000, viscosity (23°C): 380 mPa s), Siltech's "SILMER OH ACR C50" (R 1 are methyl groups, all p's are 0, q's are 1, n's are 3, X's are a group represented by formula (IIb) (a=3), Mw: 24,000, viscosity (23°C): 550 mPa s), "SILMER OH ACR Di-400" (R 1 are methyl groups, all p's are 1, n is 0, X is a group represented by formula (IIb) (a=3), Mw: 31,000, and viscosity (23°C): 1,030 mPa s).

[0035] <Slip agent (B)> The composition contains a slip agent (B). The slipping agent (B) can improve the adhesion inhibition (antifouling property) of aquatic organisms by imparting slipping property to the antifouling coating film formed. Furthermore, the inclusion of the slipping agent (B) in the present composition can make the surface of the antifouling coating film slippery in water, thereby reducing damage caused when a substrate coated with the antifouling coating film comes into contact with drifting objects, etc., and improving the workability when installing a substrate (such as an antifouling coating for cables used underwater).

[0036] The content of the slip agent (B) in the solid content of the antifouling coating composition is, from the viewpoint of improving the antifouling properties of the antifouling coating film to be formed, preferably 0.1 mass % or more, more preferably 0.5 mass % or more, even more preferably 1.0 mass % or more, and is preferably 40 mass % or less, more preferably 30 mass % or less, even more preferably 25 mass % or less.

[0037] The slipping agent (B) is preferably one having fluidity at 25°C, and more preferably in a liquid state. It is considered that the slipping agent (B) having fluidity has high mobility in the antifouling coating film, and can enhance the effect of making the surface slippery (slipperiness). In addition, the viscosity of the antifouling coating composition described later can be reduced, and the coating property can be improved. The slipping agent (B) is preferably at least one selected from oils and polymers having a hydrophilic group.

[0038] Examples of the oils include silicone oils other than the photocurable organopolysiloxane (A), paraffin oils, and fats and oils, with silicone oils being preferred. The paraffin oil includes liquid paraffin. The oils and fats are esters of fatty acids and glycerin, and examples of the oils and fats include animal oils and fats, vegetable oils and fats, etc.

[0039] From the viewpoint of the antifouling properties and adhesion of the antifouling coating film to be formed, examples of the polymer having a hydrophilic group include an acrylic polymer having a hydrophilic group and a polyalkylene glycol, and an acrylic polymer having a hydrophilic group is preferred. Examples of the polyalkylene glycol include polyethylene glycol, polypropylene glycol, copolymers of ethylene glycol and propylene glycol, and alkyl ethers thereof.

[0040] That is, the slipping agent (B) is preferably one or more selected from silicone oil, paraffin oil, oils and fats, acrylic polymers having hydrophilic groups, and polyalkylene glycols, more preferably one or more selected from silicone oil and acrylic polymers having hydrophilic groups, and even more preferably one or more selected from the group consisting of phenyl-modified silicone, polyether-modified silicone, and acrylic polymers having hydrophilic groups. In addition, from the viewpoint of coating workability and coating that provides good antifouling and damage resistance of the antifouling coating film formed, it is also preferable to contain both silicone oil and acrylic polymers having hydrophilic groups. The silicone oil and the acrylic polymer having a hydrophilic group, which are suitable slipping agents (B), will be described in detail below.

[0041] [Silicone oil (B1)] Examples of the silicone oil (B1) used in the antifouling coating composition of the present invention include dimethyl silicone (polydimethylsiloxane, unmodified silicone) and modified silicone. Modified silicone is a dimethyl silicone in which some of the methyl groups have been replaced with organic groups other than methyl groups, and does not substantially contain photocurable reactive groups such as those in the above-mentioned photocurable organopolysiloxane (A). Silicone oil has low interfacial tension and its properties do not change easily even in low temperature environments, so it easily migrates to the surface of the antifouling coating film, efficiently improving the resistance to adhesion of aquatic organisms (antifouling properties) and damage resistance.

[0042] The viscosity of the silicone oil (B1) at 25°C is, from the viewpoints of improving the coatability of the antifouling coating composition, imparting slipperiness to the antifouling coating film formed, and improving the antifouling properties, preferably 10 mPa·s or more, more preferably 20 mPa·s or more, even more preferably 40 mPa·s or more, still more preferably 60 mPa·s or more, even more preferably 80 mPa·s or more, and is preferably 50,000 mPa·s or less, more preferably 20,000 mPa·s or less, and even more preferably 10,000 mPa·s or less. In this specification, the viscosity of the silicone oil (B1) at 25° C. refers to the viscosity measured with a B-type rotational viscometer.

[0043] The kinetic viscosity of the silicone oil (B1) at 25° C. is preferably 10 mm from the viewpoint of improving the coatability of the antifouling coating composition, imparting slipperiness to the antifouling coating film formed, and improving the antifouling properties. 2 / sec or more, preferably 20 mm 2 / sec or more, more preferably 40 mm 2 / sec or more, and even more preferably 60 mm 2 / sec or more, and even more preferably 80 mm 2 / sec or more, and preferably 50,000 mm 2 / sec or less, preferably 20,000 mm 2 / sec or less, more preferably 10,000 mm 2 / sec or less. In this specification, the kinematic viscosity of the silicone oil (B1) at 25° C. refers to the viscosity measured with an Ubbelohde viscometer in accordance with JIS Z 8803:2011.

[0044] Examples of modified silicones include phenyl-modified silicone, polyether-modified silicone, long-chain alkyl-modified silicone, higher fatty acid ester-modified silicone, fluoroalkyl-modified silicone, carbinol-modified silicone, carboxy-modified silicone, amino-modified silicone, mercapto-modified silicone, and phenol-modified silicone. Among these modified silicones, from the viewpoints of imparting an appropriate degree of thixotropy to the antifouling coating composition, improving its coatability, and improving the antifouling properties and damage resistance of the antifouling coating film formed, the silicone oil (B1) is preferably one or more selected from phenyl-modified silicones and polyether-modified silicones, more preferably polyether-modified silicones, and it is also preferable to use a combination of phenyl-modified silicones and polyether-modified silicones.

[0045] The structure of the modified silicone may be a side chain modified type, a both end modified type, a one end modified type, a block type, or a side chain and both end modified type.

[0046] As the dimethyl silicone, a commercially available product may be used. For example, "KF-96-1,000cs" (manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity (25°C): 1,000 mm 2 / sec) etc.

[0047] From the viewpoints of facilitating the formation of an antifouling coating film and improving the antifouling properties of the antifouling coating film thus formed, the phenyl modification rate of the phenyl-modified silicone is preferably 3% or more, more preferably 4% or more, and is preferably 50% or less, more preferably 20% or less, and even more preferably 10% or less. The phenyl modification rate is the number of phenyl groups relative to the total number of phenyl groups and methyl groups bonded to silicon, expressed as a percentage. The kinetic viscosity of the phenyl-modified silicone at 25° C. is preferably 10 mm from the viewpoint of improving the coating workability of the antifouling coating composition and the antifouling properties of the antifouling coating film formed. 2 / sec or more, preferably 30 mm 2 / sec or more, more preferably 50 mm 2 / sec or more, and preferably 50,000 mm 2 / sec or less, preferably 10,000 mm 2 / sec or less, more preferably 6,000 mm 2 / sec or less. As the phenyl-modified silicone, a commercially available product may be used. For example, "KF-50-1,000cs" (manufactured by Shin-Etsu Chemical Co., Ltd., phenyl modification rate = 5%, kinematic viscosity (25 ° C): 1,000 mm 2 / sec), "KF-50-100cs" (Shin-Etsu Chemical Co., Ltd., phenyl modification rate = 5%, kinematic viscosity (25 ° C): 100 mm 2 / sec) etc.

[0048] When the composition contains a phenyl-modified silicone, from the viewpoint of obtaining good antifouling properties, formation efficiency, and damage resistance of the antifouling coating film, the content of this silicone in the solid content of the antifouling coating composition is preferably 0.1 mass % or more, more preferably 1 mass % or more, even more preferably 3 mass % or more, and is preferably 40 mass % or less, more preferably 30 mass % or less, and even more preferably 20 mass % or less.

[0049] The structure of the polyether-modified silicone may be a side-chain-modified type, a both-terminal-modified type, a block type, or a side-chain- and both-terminal-modified type, with the side-chain-modified type and the both-terminal-modified type being preferred. Examples of the polyether (polyalkylene glycol) constituting the polyether group (polyalkylene glycol group) of the polyether-modified silicone include polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol, with polyethylene glycol being preferred. From the viewpoints of facilitating the formation of an antifouling coating film and improving the antifouling properties of the antifouling coating film thus formed, the proportion of polyether partial structures in the structure of the polyether-modified silicone is preferably 10 mass % or more, more preferably 15 mass % or more, and preferably 50 mass % or less, more preferably 40 mass % or less.

[0050] When the antifouling coating composition contains a polyether-modified silicone, from the viewpoints of facilitating the formation of an antifouling coating film and improving the antifouling properties of the antifouling coating film formed, the content of this polyether-modified silicone in the solid content of the antifouling coating composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, even more preferably 1 mass % or more, and is preferably 20 mass % or less, more preferably 10 mass % or less, even more preferably 7 mass % or less.

[0051] When the present composition contains a polyether-modified silicone containing an ethyleneoxy (-C2H4O-) structural unit and / or an acrylic polymer (B2) having a hydrophilic group having an ethyleneoxy (-C2H4O-) structure described below, from the viewpoint of imparting good antifouling properties and damage resistance to the antifouling coating film formed, the total mass of the ethyleneoxy (-C2H4O-) partial structures per 100 parts by mass of the dimethylsiloxane partial structures (-(CH3)2Si-O-) in the antifouling coating film is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less. The dimethylsiloxane partial structure includes dimethylsiloxane partial structures derived from the above-mentioned photocurable organopolysiloxane (A), silicone oil (B1), organopolysiloxane (N1) described below, and other photocurable oligomers and polymers (N2).

[0052] The kinematic viscosity of the polyether-modified silicone at 25° C. is preferably 10 mm from the viewpoint of improving the coating workability of the antifouling coating composition and the antifouling properties of the antifouling coating film formed. 2 / sec or more, preferably 50 mm 2 / sec or more, more preferably 100 mm 2 / sec or more, and preferably 5000 mm 2 / sec or less, preferably 2000mm 2 / sec or less, more preferably 500 mm 2 / sec or less. As the polyether-modified silicone, a commercially available product may be used. For example, "X-22-4272" (manufactured by Shin-Etsu Chemical Co., Ltd., double-ended type, kinematic viscosity (25°C): 270 mm 2 / sec), "KF-6020" (Shin-Etsu Chemical Co., Ltd., side chain type, proportion of polyether partial structure = 20 mass%, kinetic viscosity (25 ° C): 180 mm 2 / sec), "FZ-2203" (manufactured by Dow Corning Toray Co., Ltd., side chain type), and "FZ-2160" (manufactured by Dow Corning Toray Co., Ltd., block type).

[0053] When the composition contains silicone oil (B1), the content of this silicone oil in the solid content of the antifouling coating composition is, from the viewpoints of facilitating the formation of an antifouling coating film and improving the antifouling properties of the antifouling coating film formed, preferably not less than 0.1 mass %, more preferably not less than 1 mass %, even more preferably not less than 3 mass %, and is preferably not more than 40 mass %, more preferably not more than 30 mass %, even more preferably not more than 25 mass %.

[0054] [Acrylic polymer having hydrophilic group (B2)] The acrylic polymer (B2) having a hydrophilic group used in the present composition preferably contains a structural unit derived from a monomer having a hydrophilic group, more preferably contains a structural unit derived from a monomer having a hydrophilic group and a structural unit derived from a hydrophobic monomer, and even more preferably consists of a structural unit derived from a monomer having a hydrophilic group and a structural unit derived from a hydrophobic monomer. The content of structural units derived from monomers having a hydrophilic group in the acrylic polymer (B2) having a hydrophilic group is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, still more preferably 10 mass% or more, particularly preferably 20 mass% or more, and is 100 mass% or less, preferably 80 mass% or less, more preferably 70 mass% or less, still more preferably 60 mass% or less, and still more preferably 50 mass% or less. It is believed that when the acrylic polymer has a hydrophilic group and the antifouling coating film formed is placed in water, the hydrophilic portion of the acrylic polymer dissolves or swells and gradually migrates to the surface of the antifouling coating film, which effectively prevents the attachment of aquatic organisms. In addition, because it has an acrylic structure, it is slowly hydrolyzed and its affinity for water changes, so that the acrylic polymer gradually migrates to the surface of the antifouling coating film, which is believed to enable the antifouling properties to be maintained for a long period of time. As the hydrophilic group of the monomer having a hydrophilic group, from the viewpoint of improving the antifouling properties and damage resistance of the antifouling coating film to be formed, an ether group or a hydroxyl group is preferable, an ether group is more preferable, a polyether group is even more preferable, and a polyethyleneoxy group is even more preferable.

[0055] Furthermore, the content of structural units derived from hydrophobic monomers in the acrylic polymer (B2) having a hydrophilic group is preferably 99% by mass or less, more preferably 97% by mass or less, even more preferably 95% by mass or less, still more preferably 90% by mass or less, particularly preferably 80% by mass or less, and preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and still more preferably 50% by mass or more. It is believed that the acrylic polymer contains a hydrophobic monomer, which gives it high affinity with the other components of the antifouling coating composition, such as the photocurable organopolysiloxane (A), and enables the antifouling coating film surface to exhibit uniform slip properties.

[0056] As the monomer having a hydrophilic group, from the viewpoint of improving the antifouling properties and damage resistance of the antifouling coating film to be formed, a monomer having a polyalkylene glycol group and a monomer having a hydroxyl group are preferred, and a monomer having a polyalkylene glycol group is more preferred. Specifically, from the viewpoint of improving the antifouling properties, one or more selected from polyalkylene glycol (meth)acrylate, hydroxyalkyl (meth)acrylate, alkoxyalkyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 4-(meth)acryloylmorpholine, and vinylpyrrolidone are preferred, one or more selected from polyalkylene glycol (meth)acrylate and hydroxyalkyl (meth)acrylate are more preferred, and polyalkylene glycol (meth)acrylate is even more preferred.

[0057] Examples of the polyalkylene glycol (meth)acrylate include those in which one end of the polyalkylene glycol is bonded to (meth)acrylic acid directly via an ester bond or a linking group, and the remaining end is a hydroxyl group or an alkoxy group, and those which are alkoxy groups are preferred. Among these, polyalkylene glycols in which one end is directly ester-bonded to (meth)acrylic acid are preferred, and those in which the remaining end is an alkoxy group are more preferred. The terminal (meth)acrylic acid is preferably acrylic acid or methacrylic acid, and more preferably acrylic acid. Examples of the terminal alkoxy group include a methoxy group, a phenoxy group, and an octoxy group, with a methoxy group and a phenoxy group being preferred, and a methoxy group being more preferred.

[0058] The polyalkylene glycol constituting the polyalkylene glycol (meth)acrylate is preferably polyethylene glycol, polypropylene glycol, or a copolymer of ethylene glycol and propylene glycol, and more preferably polyethylene glycol. The average number of alkylene glycol units constituting the polyalkylene glycol in the polyalkylene glycol (meth)acrylate is preferably 2 or more, more preferably 3 or more, even more preferably 5 or more, and is preferably 25 or less, more preferably 15 or less, even more preferably 12 or less.

[0059] Specific examples of polyalkylene glycol (meth)acrylates include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-butylene glycol) mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, allyloxypoly(ethylene glycol-propylene glycol) mono(meth)acrylate, phenoxypoly(ethylene glycol-propylene glycol) methacrylate, octoxypoly(ethylene glycol-propylene glycol) mono(meth)acrylate, dodecyloxypolyethylene glycol mono(meth)acrylate, octadecyloxypolyethylene glycol mono(meth)acrylate, nonylphenoxypolypropylene glycol acrylate, and the like, with methoxypolyethylene glycol mono(meth)acrylate being preferred.

[0060] As the polyalkylene glycol (meth)acrylate, commercially available products may be used, such as NK Ester AM-90G (methoxypolyethylene glycol #400 acrylate), NK Ester AM-130G (methoxypolyethylene glycol #550 acrylate), NK Ester M-90G (methoxypolyethylene glycol #400 methacrylate), and NK Ester 130G (methoxypolyethylene glycol #550 acrylate), all manufactured by Shin-Nakamura Chemical Co., Ltd. M-230G (methoxypolyethylene glycol #1000 methacrylate); Light Acrylate MTG-A (methoxy-triethylene glycol acrylate), Light Acrylate EC-A (ethoxy-diethylene glycol acrylate), Light Acrylate EHDG-AT (2-ethylhexyl-diethylene glycol acrylate), Light Ester 041MA (methoxypolyethylene glycol methacrylate) manufactured by Kyoeisha Chemical Co., Ltd.; Blemmer ANP-300 (nonylphenoxy polypropylene glycol acrylate), Blemmer AP-400 (polypropylene glycol monoacrylate), Blemmer 70PEP-350B (polyethylene glycol polypropylene glycol monomethacrylate), Blemmer 55PET-800 (polyethylene glycol tetramethylene glycol monomethacrylate), Blemmer 50POEP-800B (octoxypolyethylene glycol polypropylene glycol methacrylate) manufactured by NOF Corporation; and Viscoat #MTG (methoxypolyethylene glycol acrylate) manufactured by Osaka Organic Chemical Industry Co., Ltd.

[0061] Examples of the hydroxyalkyl (meth)acrylate include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate. As the hydroxyalkyl (meth)acrylate, commercially available products may be used, such as Light Ester HOA(N) (2-hydroxyethyl acrylate), Light Ester HO-250(N) (2-hydroxyethyl methacrylate), and Light Ester HOP(N) (2-hydroxypropyl methacrylate), all of which are manufactured by Kyoeisha Chemical Co., Ltd.

[0062] Examples of the alkoxyalkyl (meth)acrylate include methoxyethyl (meth)acrylate.

[0063] As the tetrahydrofurfuryl (meth)acrylate, tetrahydrofurfuryl acrylate and tetrahydrofurfuryl methacrylate are preferred, and tetrahydrofurfuryl acrylate is more preferred. As the 4-(meth)acryloylmorpholine, 4-acryloylmorpholine and 4-methacryloylmorpholine are preferable, and 4-acryloylmorpholine is more preferable. Examples of vinylpyrrolidone include 1-vinyl-2-pyrrolidone (N-vinyl-2-pyrrolidone), 3-acetyl-1-vinylpyrrolidin-2-one, and 3-benzoyl-1-vinylpyrrolidin-2-one, with 1-vinyl-2-pyrrolidone being preferred.

[0064] Another example of the monomer having a hydrophilic group is (meth)acrylic acid.

[0065] Examples of the hydrophobic monomer include alkyl(meth)acrylates having a branched, linear or cyclic alkyl group having from 1 to 30 carbon atoms, aryl(meth)acrylates having an aromatic group having from 6 to 10 carbon atoms, and (meth)acrylic group-containing silicones. Of these, alkyl(meth)acrylates and (meth)acrylic group-containing silicones are preferred, and alkyl(meth)acrylates are more preferred.

[0066] The number of carbon atoms in the alkyl group of the alkyl (meth)acrylate is preferably 1 or more and 30 or less, more preferably 4 or more and 18 or less, even more preferably 4 or more and 8 or less, and even more preferably 4 or more and 6 or less. The alkyl group may be branched, straight-chained or cyclic, preferably branched or straight-chained, and more preferably branched.

[0067] Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate. acrylate, 2-ethylhexyl (meth)acrylate, 3,5,5-trimethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate, and among these, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred.

[0068] The aromatic group of the aryl(meth)acrylate preferably has 6 or more and 10 or less carbon atoms, and more preferably has 6 or more and 7 or less carbon atoms. Specific examples of the aryl(meth)acrylate include phenyl(meth)acrylate and benzyl(meth)acrylate.

[0069] Examples of the (meth)acrylic group-containing silicone include methacrylic group-containing silicone and acrylic group-containing silicone, with methacrylic group-containing silicone being preferred. The (meth)acrylic group-containing silicone is preferably one in which a (meth)acrylic group is bonded to one end of the silicone main chain via a linking group, or one in which a (meth)acrylic group is bonded directly to one end of the silicone main chain, and more preferably one in which a (meth)acrylic group is bonded to one end of the silicone main chain via a linking group. The linking group is preferably a trimethylene group. The silicone main chain is preferably made of linear or branched dimethyl silicone (polydimethylsiloxane), and more preferably made of linear dimethyl silicone. Furthermore, it is more preferable that an alkyl group having 1 to 6 carbon atoms is present at the end opposite to the (meth)acrylic group, and it is more preferable that a butyl group is present. As the (meth)acrylic group-containing silicone, commercially available products may be used, such as Silaplane TM-0701T (tris(trimethylsiloxy)silylpropyl methacrylate), Silaplane FM-0711 (methacrylic group-containing dimethylpolysiloxane, number average molecular weight 1,000), and Silaplane FM-0721 (methacrylic group-containing dimethylpolysiloxane, number average molecular weight 5,000), all of which are manufactured by JNC Corporation. By including a (meth)acrylic group-containing silicone, the antifouling properties of the antifouling coating film that is formed can be improved.

[0070] The acrylic polymer (B2) having a hydrophilic group can be obtained by polymerizing the above-mentioned hydrophilic monomer and hydrophobic monomer, and as the polymerization method, a known method using a polymerization initiator can be used.

[0071] The weight average molecular weight (Mw) of the hydrophilic group-containing acrylic polymer (B2) is, from the viewpoint of improving the viscosity of the antifouling coating composition and the antifouling properties of the antifouling coating film formed, preferably 1,000 or more, more preferably 3,000 or more, even more preferably 5,000 or more, still more preferably 7,000 or more, and is preferably 30,000 or less, more preferably 15,000 or less. It is preferable that the weight average molecular weight (Mw) of the hydrophilic group-containing acrylic polymer (B2) is within the above range, since good antifouling properties and damage resistance can be imparted to the formed antifouling coating film.

[0072] When the present composition contains an acrylic polymer (B2) having a hydrophilic group, the content thereof in the solid content of the antifouling coating composition is, from the viewpoint of the antifouling properties and damage resistance of the antifouling coating film to be formed, preferably 0.1 mass % or more, more preferably 1 mass % or more, even more preferably 3 mass % or more, and preferably 40 mass % or less, more preferably 20 mass % or less, even more preferably 10 mass % or less, and even more preferably 5 mass % or less.

[0073] <Photopolymerization initiator (C)> The composition contains a photopolymerization initiator (C). The photopolymerization initiator (C) may be any initiator that generates active species such as radicals when irradiated with active energy rays. Examples of initiators that generate radicals upon irradiation with active energy rays include conventionally known photopolymerization initiators such as phosphine oxide-based polymerization initiators, acetophenone-based polymerization initiators, benzoin-based polymerization initiators, benzophenone-based polymerization initiators, and thioxanthone-based polymerization initiators. Of these, it is preferable to use a phosphine oxide-based polymerization initiator, since the coating composition has good curability even when exposed to ultraviolet light with a relatively long wavelength.

[0074] Examples of the phosphine oxide polymerization initiator include acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; Examples thereof include bisacylphosphine oxides such as bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-(2,4-bis-pentyloxyphenyl)phosphine oxide. Examples of acetophenone-based polymerization initiators include benzyl dimethyl ketal (also known as 2,2-dimethoxy-2-phenylacetophenone), diethoxyacetophenone, 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, 4-tert-butyl-trichloroacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.

[0075] Examples of the benzoin-based polymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of the benzophenone-based polymerization initiator include benzophenone, [4-(methylphenylthio)phenyl]phenylmethanone, 4-hydroxybenzophenone, 4-phenylbenzophenone, and 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone. Examples of the thioxanthone-based polymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone.

[0076] On the other hand, examples of initiators that generate cations upon irradiation with active energy rays include sulfonium salt compounds and iodonium salt compounds, and examples of initiators that generate anions include 2-(9-oxoxanthen-2-yl)propionic acid 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and the like.

[0077] The photopolymerization initiator (C) may be used alone or in combination of two or more kinds. In the present composition, the content of the photopolymerization initiator (C) in the solid content of the antifouling coating composition is preferably 0.1 part by mass or more, more preferably 1.0 part by mass or more, even more preferably 1.5 parts by mass or more, per 100 parts by mass of the total of the solid contents of components (A) and (B), and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less.

[0078] <Optional ingredients> In addition to the photocurable organopolysiloxane (A), the slipping agent (B), and the photopolymerization initiator (C), the composition may contain, as necessary, a silane coupling agent (D), a non-reactive solvent (E), a polymerization inhibitor (F), an antifoaming agent (G), a light stabilizer (H), an ultraviolet absorber (I), an inorganic filler (J), an organic coloring pigment (K), a photosensitizer (L), a photopolymerizable monomer (M), other oligomers / polymers (N), a biological repellent (O), a dehydrating agent (P), an anti-sagging / anti-settling agent (Q), a curing catalyst (R), an organosilicon crosslinker (S), an antistatic agent (T), an enzyme (U), a flame retardant (V), a thermal conductivity improver (W), and an anti-fogging agent (X) within the scope of the invention.

[0079] [Silane coupling agent (D)] The present composition may contain a silane coupling agent (D) for the purpose of improving adhesion between the antifouling coating film formed and the substrate or base. The silane coupling agent (D) is a compound having a silane bonded to a hydrolyzable group and a reactive group, or a partial condensate thereof. For example, it is preferable to use a compound represented by the following formula (D1) or a partial condensate thereof.

[0080] [ka]

[0081] In formula (D1), R 21 and R 22each independently represents an alkyl group, an alkenyl group, an aryl group, or a halogenated alkyl group having from 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group. In formula (D1), R 23 is a divalent hydrocarbon group having from 1 to 20 carbon atoms which may be interrupted by an amino group (-NR-, where R represents a hydrogen atom or a hydrocarbon group having from 1 to 10 carbon atoms), an ether group (-O-), a thioether group (-S-), an ester group (-C(=O)-O-), or an amide group (-C(=O)-NR-, where R represents a hydrogen atom or a hydrocarbon group having from 1 to 10 carbon atoms), and is preferably a propylene group. In formula (D1), Z is a reactive group, and from the viewpoint of improving the antifouling properties of the coating film to be formed, it is preferably a (meth)acryloyloxy group, and more preferably an acryloyloxy group. In formula (D1), w is an integer of 2 or 3, and is preferably 3.

[0082] Examples of such silane coupling agents (D) include 3-acryloyloxypropyltrimethoxysilane, 3-acryloyloxypropylmethyldimethoxysilane, 3-acryloyloxypropyltriethoxysilane, 3-acryloyloxypropylmethyldiethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropylmethyldimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-methacryloyloxypropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, and 3-aminopropyltriethoxysilane. It is preferable to use 3-acryloyloxypropyltrimethoxysilane. As the silane coupling agent (D), a commercially available product may be used, for example, "KBM-5103" (3-acryloyloxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., and the like.

[0083] These silane coupling agents (D) may be used alone or in combination of two or more kinds. When the present composition contains a silane coupling agent (D), the content of the silane coupling agent (D) in the solid content of the paint composition is, from the viewpoint of improving the adhesion of the antifouling coating film formed to the substrate or the undercoat coating film, preferably 0.1 mass % or more, more preferably 0.2 mass % or more, even more preferably 0.5 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less, even more preferably 3 mass % or less.

[0084] [Non-reactive solvent (E)] The present composition may contain a non-reactive solvent (E) for the purpose of improving the ease of production and coating of the composition. Examples of the non-reactive solvent (E) include aromatic hydrocarbon organic solvents, aliphatic hydrocarbon organic solvents, alicyclic hydrocarbon organic solvents, ketone organic solvents, and ester organic solvents. Among these, aromatic hydrocarbon organic solvents, aliphatic hydrocarbon organic solvents, and alicyclic hydrocarbon organic solvents are preferred. Examples of aromatic hydrocarbon organic solvents include toluene, xylene, and mesitylene. Examples of the aliphatic hydrocarbon organic solvent include pentane, hexane, heptane, octane, and mineral spirits. Examples of the alicyclic hydrocarbon organic solvent include cyclohexane, methylcyclohexane, and ethylcyclohexane. Examples of the ketone organic solvent include acetylacetone, acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone (also known as 2-heptanone), and dimethyl carbonate. An example of the ester-based organic solvent is propylene glycol monomethyl ether acetate.

[0085] These non-reactive solvents (E) may be used alone or in combination of two or more kinds. When the present composition contains a non-reactive solvent (E), the content of the non-reactive solvent (E) in the coating composition can be appropriately adjusted depending on the viscosity of the coating composition, but is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more, and from the viewpoint of suppressing sagging during coating, is preferably 40 mass % or less, more preferably 25 mass % or less, and even more preferably 15 mass % or less. The non-reactive solvent may be added during preparation of the antifouling coating composition, or may be mixed in advance with the other components. In the present invention, by keeping the content of the non-reactive solvent (E) low, it is possible to carry out the photocuring step without carrying out the drying step, and this is preferable because it allows the antifouling coating film to be formed in a shorter time.

[0086] [Polymerization inhibitor (F)] The present composition may contain a polymerization inhibitor (F) for the purpose of improving the storage stability, manufacturing operability, and coating operability of the coating composition. Examples of the polymerization inhibitor (F) include quinones such as p-benzoquinone, naphthoquinone, toluquinone, 2,5-diphenyl-p-benzoquinone, hydroquinone, 2,5-di-tert-butylhydroquinone, methylhydroquinone, and mono-tert-butylhydroquinone, aromatics such as 4-methoxyphenol and 2,6-di-tert-butylcresol (also known as dibutylhydroxytoluene, BHT), and p-tert-butylcatechol. Among these, aromatics are preferred, and 4-methoxyphenol and 2,6-di-tert-butylcresol are particularly preferred. These can be used alone or in combination of two or more.

[0087] When the composition contains a polymerization inhibitor (F), the content of the polymerization inhibitor (F) in the solid content of the coating composition is preferably 0.001 mass % or more, more preferably 0.005 mass % or more, and preferably 0.1 mass % or less, more preferably 0.05 mass % or less.

[0088] [Antifoaming agent (G)] The present composition may contain an antifoaming agent (G) for the purposes of improving the ease of production and application of the composition and improving the strength and antifouling properties of the antifouling coating film formed. As the defoaming agent (G), a fluorine-based, silicone-based or acrylic-based defoaming agent can be used, and a fluorine-based defoaming agent is particularly preferred. The defoaming agent (G) may be used in combination of two or more kinds. As the defoaming agent (G), a commercially available product can be used, for example, "BYK-066N" (fluorine-based defoaming agent) manufactured by BYK Japan K.K. When the present composition contains an antifoaming agent (G), the content of the antifoaming agent (G) in the solid content of the coating composition is preferably 0.001 mass % or more, more preferably 0.01 mass % or more, and is preferably 5 mass % or less, more preferably 1 mass % or less.

[0089] [Light stabilizer (H)] The present composition may contain a light stabilizer (H) for the purpose of further suppressing yellowing of the antifouling coating film due to ultraviolet rays such as those from sunlight. Examples of the light stabilizer (H) include hindered amine light stabilizers, which may be modified or oligomerized. These may be used alone or in combination of two or more. As the hindered amine-based light stabilizer, commercially available products can be used. For example, "TINUVIN 123" manufactured by BASF Japan Ltd. (a mixture of decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester, a reaction product of 1,1-dimethylethyl hydroperoxide and octane, and a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) and "TINUVIN 111FDL" (N,N',N'',N'''-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazin-2-yl)-4,7-diazadecane-1,10-diamine), "TINUVIN144" (bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate), "TINUV IN292" (a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate), ADEKA CORPORATION's "ADEKA STAB LA-82" (1,2,2,6,6-pentamethylpiperidin-4-yl methacrylate), "ADEKA STAB LA-87" (2,2,6,6-pentamethylpiperidin-4-yl methacrylate), Clariant Japan Co., Ltd.'s "HOSTAVIN 3058" (1-(1-acetyl-2,2,6,6-tetramethylpiperidin-4-yl)-3-dodecylpyrrolidine-2,5-dione), and the like. When the light stabilizer (H) is used, its content is not particularly limited, but is preferably from 0.1% by mass to 5% by mass based on the solid content of the coating composition.

[0090] [Ultraviolet absorber (I)] The present composition may contain an ultraviolet absorber (I) for the purpose of maintaining good antifouling properties of the antifouling coating film formed and good adhesion to the substrate or base. Examples of the ultraviolet absorber (I) include benzotriazole-based ultraviolet absorbers such as 2-(2-hydroxy-5-methylphenyl)benzotriazole and 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole; Benzophenone-based ultraviolet absorbers such as 2,4-dihydroxybenzophenone and 2-hydroxy-4-methoxybenzophenone; Hydroxyphenyltriazine ultraviolet absorbers; Salicylate-based ultraviolet absorbers such as phenyl salicylate and 4-tert-butylphenyl salicylate; Examples of the cyanoacrylate ultraviolet absorbers include ethyl 2-cyano-3,3-diphenylcyanoacrylate and 2-ethylhexyl 2-cyano-3,3-diphenylcyanoacrylate. The ultraviolet absorber (I) may also have a functional group that reacts with other components in the coating composition when irradiated with active energy rays. The ultraviolet absorbent (I) may be used alone or in combination of two or more kinds.

[0091] As the ultraviolet absorber (I), commercially available products can be used. Benzotriazole-based ultraviolet absorbers include, for example, "RUVA-93" (2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole) manufactured by Otsuka Chemical Co., Ltd., "DAINSORBT-84" (2-(4-allyloxy-2-hydroxyphenyl)-2H-benzotriazole) manufactured by Daiwa Kasei Co., Ltd., "Tinuvin928" (2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3,-tetramethylbutyl)phenol) manufactured by BASF Japan Ltd., An example of a benzophenone-based UV absorber is "Chimassorb81" (2-hydroxy-4-octoxybenzophenone) manufactured by BASF Japan Ltd., and an example of a hydroxyphenyltriazine-based UV absorber is "Tinuvin400" (2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-[(2-hydroxy-3-tri ... and mixtures of 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine), "Tinuvin 460" (2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine), "Tinuvin 405" (2-[4-[(2-hydroxy-3-(2-ethylhexyloxy)propyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine), and "Tinuvin 479" (2-(2-hydroxy-4-(isooctyloxycarbonylethoxy)phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine).

[0092] When the present composition contains an ultraviolet absorber (I), the content of the ultraviolet absorber (I) in the solid content of the coating composition is 10 mass % or less, more preferably 5 mass % or less.

[0093] [Inorganic filler (J)] The present composition may contain an inorganic filler (J) for the purpose of improving the strength, antifouling properties and visibility of the antifouling coating film to be formed. Examples of the inorganic filler (J) include silica, alumina, titanium oxide, iron oxide, zinc oxide, zirconium oxide, indium oxide, vanadium oxide, cerium oxide, antimony oxide, talc, tungsten carbide, titanium carbide, silicon carbide, calcium carbonate, magnesium carbonate, aluminum sulfate, barium sulfate, calcium sulfate, magnesium sulfate, glass fiber, and glass flakes. Of these, it is preferable to contain silica.

[0094] Among inorganic fillers (J), those with high transmittance of active energy rays such as silica are preferably used as fine particles having an average particle diameter of 1 nm or more and 200 nm or less, more preferably 10 nm or more and 100 nm or less, from the viewpoint of improving the curing property of the coating composition and the adhesion of the formed antifouling coating film to the substrate or the underside. The average particle diameter is the median diameter (d50) of the volume-based particle size distribution measured by the dynamic light scattering method, and can be measured, for example, using a laser diffraction type particle size distribution measuring device ("SALD-2200" manufactured by Shimadzu Corporation). Alternatively, it can be calculated as the average diameter of the fine particles when the cured coating film is observed using a scanning electron microscope or a transmission electron microscope.

[0095] When the present composition contains silica, surface-untreated hydrophilic silica may be used, or surface-treated silica may be used. Examples of surface-treated silica include silica surface-treated by reaction with methyltrichlorosilane, dimethyldichlorosilane, hexamethyldisilazane, coupling agents, or polymers. By performing such surface treatment, silica is made hydrophobic, thereby preventing aggregation in the antifouling paint composition and improving storage stability. Examples of surface-treated silica include reactive silica having a (meth)acryloyl group on the silica surface. The reactive silica can be obtained, for example, by reacting silica with a hydrolyzable silane having a (meth)acryloyl group and a hydrolyzable group such as a methoxy group or an ethoxy group in the molecule. In such an embodiment, when the present composition is cured by irradiation with active energy rays, the reactive silica reacts with component (A) and is incorporated into the coating film, thereby improving the strength of the coating film formed.

[0096] The inorganic filler (J) may be in the form of a powder, or may be in the form of an inorganic fine particle sol in which fine particles of the inorganic filler are dispersed in a dispersion medium. Examples of the dispersion medium for the inorganic fine particle sol include water; monohydric alcohol solvents such as methanol, ethanol, isopropanol, n-propanol, isobutanol, and n-butanol; polyhydric alcohol solvents such as ethylene glycol and propylene glycol; polyhydric alcohol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monobutyl ether; and ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, diacetone alcohol, and cyclohexanone. Among these, water, methanol, ethanol, isopropanol, methyl ethyl ketone, methyl isobutyl ketone, and propylene glycol monomethyl ether are preferred from the viewpoint of ease of production of the coating composition. The content of the inorganic filler (J) in the present composition does not include the dispersion medium. Such inorganic fillers (J) may be used alone or in combination of two or more kinds.

[0097] Commercially available inorganic fillers (J) can be used. Examples of powdered inorganic fillers include "Aerosil 50" (average primary particle size 30 nm, silica without surface treatment), "Aerosil 300" (average primary particle size 7 nm, silica without surface treatment), "Aerosil R972" (average primary particle size 7 nm, silica surface-treated with dimethyldichlorosilane), "Aerosil R202" (average primary particle size 14 nm, silica surface-treated with dimethylsilicone oil), "AluC" (average primary particle size 13 nm, alumina), and "TiO2 P25" (average primary particle size 21 nm, titanium oxide), all of which are manufactured by Nippon Aerosil Co., Ltd. Examples of inorganic fine particle sols include "MIBK-SD" (silica sol dispersed in methyl isobutyl ketone, silica content 30%, particle size 10 to 15 nm), "PGM-AC-4130Y" (silica sol dispersed in propylene glycol monomethyl ether, silica content 30%, particle size 40 to 50 nm), and "MEK-ST-ZL" (silica sol dispersed in methyl ethyl ketone, silica content 30%, particle size 70 to 100 nm) manufactured by Nissan Chemical Co., Ltd., and "SIRMIBK30WT%-H24" (silica sol dispersed in methyl isobutyl ketone, silica content 30%, particle size 70 to 100 nm) manufactured by CIK Nanotech Co., Ltd. Examples of silica sol dispersed in propylene glycol monomethyl ether, silica content 30%), "SIRPA15WT%-H10" (silica sol dispersed in methyl isobutyl ketone, silica content 15%), "SIRPGM30WT%-E80" (silica sol dispersed in propylene glycol monomethyl ether, silica content 30%), "RTTMIBK20WT%-H36" (titanium oxide sol dispersed in methyl isobutyl ketone, titanium oxide content 15%), and "ZNMIBK15WT%-E05" (zinc oxide sol dispersed in methyl isobutyl ketone, zinc oxide content 15%).

[0098] When the composition contains an inorganic filler (J), the content of the inorganic filler (J) in the solid content of the coating composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and preferably 20 mass % or less, more preferably 10 mass % or less.

[0099] [Organic color pigment (K)] The present composition may contain an organic coloring pigment (K) for the purpose of improving the visibility of the antifouling coating composition and the antifouling coating film formed, thereby improving the ease of production and painting workability. Specific examples of the organic coloring pigment (K) include soluble azo pigments such as Lake Red C and Brilliant Carmine 6B, insoluble azo pigments such as Toluidine Red, Permanent Carmine FB, Fast Yellow G, Disazo Yellow AAA, and Disazo Orange PMP, condensed azo pigments such as Chromophthal Yellow 3G, chelate azo pigments, phthalocyanine pigments such as Phthalocyanine Blue and Phthalocyanine Green, condensed polycyclic pigments such as Indanthrone Blue, Quinacridone Red, and Dioxazine Violet Red, organic pigments such as Alkali Blue, Aniline Black, Daylight Fluorescent Pigments, nitro pigments, and nitroso pigments, and carbon black.

[0100] The organic color pigment (K) may be used alone or in combination of two or more kinds. When the composition contains an organic color pigment (K), the content of the organic color pigment (K) in the solid content of the coating composition is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less.

[0101] [Photosensitizer (L)] The present composition may contain a photosensitizer (L) for the purpose of improving the curability of the antifouling coating composition. In the present composition, a photosensitizer (L) can be used in combination with the photopolymerization initiator (C). Specific examples of the photosensitizer (L) include triethanolamine, methyldiethanolamine, triisopropanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 4,4-dimethylaminobenzophenone, and 4,4-diethylaminobenzophenone.

[0102] The photosensitizer (L) may be used alone or in combination of two or more kinds. When the composition contains a photosensitizer (L), the content of the photosensitizer (L) in the solid content of the coating composition is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less.

[0103] [Photopolymerizable monomer (M)] The present composition may contain a photopolymerizable monomer (M) other than the components described in the preceding paragraphs for the purposes of improving the ease of production and application of the antifouling coating composition, the antifouling properties of the coating film formed, and adhesion to the substrate or undercoat, and for the purpose of acting as a diluent for other components. Examples of the photopolymerizable monomer (M) include monofunctional monomers such as those exemplified as the monomers from which the acrylic polymer (B2) is derived; Isocyanato group-containing monofunctional monomers such as 2-acryloyloxyethyl isocyanate; 1,9-Nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, di(meth)acrylate of ethylene oxide adduct of neopentyl glycol, di(meth)acrylate of propylene oxide adduct of neopentyl glycol, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, di(meth)acrylate of ethylene oxide adduct of bisphenol A, glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol Examples of polyfunctional monomers include dipentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, tetra(meth)acrylate of an ethylene oxide adduct of pentaerythritol, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, hexa(meth)acrylate of an ε-caprolactone adduct of dipentaerythritol, and hexa(meth)acrylate of an ethylene oxide adduct of dipentaerythritol. Among these, from the viewpoint of achieving good adhesion in a short time after curing (irradiation with active energy rays), photopolymerizable monomers having a polar group are preferred, photopolymerizable monomers having at least one of a carboxylic acid, an isocyanato group, a hydroxyl group, and an amino group are more preferred, and acrylic acid is even more preferred.

[0104] The photopolymerizable monomer (M) may be used alone or in combination of two or more kinds. When the present composition contains a photopolymerizable monomer (M), the content of the photopolymerizable monomer (M) in the solid content of the coating composition is preferably 1 mass % or more, more preferably 2 mass % or more, and preferably 30 mass % or less, more preferably 15 mass % or less.

[0105] [Other oligomers and polymers (N)] The present composition may contain an oligomer / polymer (N) other than components (A) and (B) for the purpose of improving the strength of the antifouling coating film formed and the adhesion to the substrate or base. The oligomer polymer (N) other than the components (A) and (B) may be used alone or in combination of two or more. Other examples of the oligomer / polymer (N) include organopolysiloxane (N1) (hereinafter, simply referred to as "organopolysiloxane (N1)") that does not have photocurability. The proportion of organopolysiloxane in the molecule of the organopolysiloxane (N1) is preferably 50 mass% or more. Examples of such organopolysiloxanes (N1) include those that have reactive groups in the molecule, and that cure by forming a three-dimensional crosslinked structure by reacting the reactive groups with each other or with the reactive groups of the photocurable organopolysiloxane (A) or the organosilicon crosslinking agent (S) described below. Reactions of these reactive groups include, for example, condensation reactions and addition reactions, and examples of condensation reactions include dealcoholization reactions, deoxime reactions, and deacetone reactions. As such organopolysiloxane (N1), commercially available products can be used, for example, "DMS-S35" manufactured by GELEST, and "KE-441" and "KE-445" manufactured by Shin-Etsu Chemical Co., Ltd. When the present composition contains an organopolysiloxane (N1), the content of the organopolysiloxane (N1) in the solid content of the coating composition is preferably 1 mass % or more, more preferably 3 mass % or more, and preferably 40 mass % or less, more preferably 30 mass % or less.

[0106] The other oligomer / polymer (N) may be a photocurable oligomer / polymer (N2) other than the photocurable organopolysiloxane (A) among compounds that initiate polymerization due to active species such as radicals generated by the photopolymerization initiator (C) upon irradiation with active energy rays. The proportion of organopolysiloxane in the molecule of the other photocurable oligomer / polymer (N2) is less than 50 mass%. Such other photocurable oligomers and polymers (N2) include urethane (meth)acrylates, polyester (meth)acrylates, and epoxy (meth)acrylates. Urethane (meth)acrylates are oligomers or polymers that have one or more (meth)acryloyloxy groups and urethane bonds in the molecule, and are obtained, for example, by the reaction of a (meth)acrylate that has a hydroxyl group in the molecule with a polyisocyanate, or by the reaction of a hydroxyl-containing polyester with a (meth)acrylate that has an isocyanato group. Other photocurable oligomers and polymers (N2) that can be used include commercially available products such as "CN991" (aliphatic urethane acrylate, functional group number 2, weight average molecular weight 1,500) manufactured by Sartomer, "KRM8200" (aliphatic urethane acrylate, functional group number 6, weight average molecular weight 1,000) and "EBECRYL220" (aromatic urethane acrylate, functional group number 6, weight average molecular weight 1,000) manufactured by Daicel-Allnex Corporation, "Aronix M-8560" (polyester acrylate) manufactured by Toa Gosei Co., Ltd., and "VR-77" (epoxy acrylate, functional group number 1.9, weight average molecular weight 510) manufactured by Showa Denko K.K. When the present composition contains other photocurable oligomer / polymer (N2), the content of the photocurable oligomer / polymer (N2) in the solid content of the coating composition is preferably 1 mass % or more, more preferably 2 mass % or more, and preferably 40 mass % or less, more preferably 25 mass % or less.

[0107] The other oligomer polymers (N) include other oligomer polymers (N3) other than the organopolysiloxane (N1) and the other photocurable oligomer polymers (N2). Examples of such other oligomers / polymers (N3) include poorly water-soluble or water-insoluble resins other than component (B), such as acrylic resins, acrylic silicone resins, unsaturated polyester resins, fluororesins, polybutene resins, urethane resins (rubber), polyamide resins, vinyl chloride copolymer resins, chlorinated rubber (resins), chlorinated olefin resins, styrene-butadiene copolymer resins, ethylene-vinyl acetate copolymer resins, vinyl chloride resins, alkyd resins, coumarone resins, and petroleum resins.

[0108] [Biological repellents (O)] The present composition may contain a biological repellent (O) for the purpose of further improving the antifouling properties of the antifouling coating film formed. Examples of biological repellents (O) include 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (also known as DCOIT), (+ / -)-4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (also known as medetomidine), 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile (also known as tralopyril), borane-nitrogen base adducts (pyridinetriphenylborane, 4-isopropylpyridinediphenylmethylborane, etc.), N,N-dimethyl-N'-(3,4-dichlorophenyl)urea (also known as D Organic biological repellents such as CMU), N-(2,4,6-trichlorophenyl)maleimide, 2-methylthio-4-tert-butylamino-6-cyclopropylamino-1,3,5-triazine, 2,4,5,6-tetrachloroisophthalonitrile, chloromethyl-n-octyl disulfide, N,N-dimethyl-N'-phenyl-(N'-fluorodichloromethylthio)sulfamide, tetraalkylthiuram disulfide, 2,3-dichloro-N-(2',6'-diethylphenyl)maleimide, and 2,3-dichloro-N-(2'-ethyl-6'-methylphenyl)maleimide; Inorganic biological repellents such as cuprous oxide, copper rhodanide, and copper; Examples of the organic-inorganic composite biological repellents include copper pyrithione, zinc pyrithione, bisdimethyldithiocarbamoylzinc ethylene bisdithiocarbamate, zinc dimethyldithiocarbamate, and zinc ethylene bisdithiocarbamate. From the viewpoint of improving the curing properties of the antifouling coating composition and the adhesion of the antifouling coating film formed to the base, it is preferable to use an organic biological repellent, and it is more preferable to use DCOIT and medetomidine. The biological repellent (O) may be used alone or in combination of two or more kinds. When an inorganic biological repellent or an organic-inorganic composite biological repellent is used as the biological repellent (O), it is preferable to use fine particles. When the present composition contains a biological repellent (O), the content of the biological repellent (O) in the solid content of the paint composition is preferably 0.05 mass % or more, more preferably 0.1 mass % or more, from the viewpoint of improving the antifouling properties of the antifouling coating film to be formed, and is preferably 20 mass % or less, more preferably 10 mass % or less.

[0109] [Dehydrating agent (P)] The present composition may contain a dehydrating agent (P) for the purpose of improving the storage stability of the coating composition. As the dehydrating agent (P), for example, zeolite, commonly known as "molecular sieve", porous alumina, orthoester such as orthoformic acid alkyl ester, orthoboric acid, isocyanate, etc. These dehydrating agents may be used alone or in combination of two or more kinds. When the present composition contains a dehydrating agent (P), the content of the dehydrating agent (P) in the solid content of the coating composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less, from the viewpoint of improving the storage stability of the coating composition.

[0110] [Anti-sagging / anti-settling agent (Q)] The composition may also contain an anti-sagging-anti-settling agent (Q). Examples of the sagging prevention / settling prevention agent (Q) include organic clay waxes (stearate salts of Al, Ca, Zn, lecithin salts, alkylsulfonates, etc.), organic waxes (polyethylene wax, oxidized polyethylene wax, amide wax, polyamide wax, hydrogenated castor oil wax, etc.), and mixtures of organic clay waxes and organic waxes. As the sagging prevention / settling prevention agent (Q), commercially available products can be used, for example, "Disparlon 305", "Disparlon 4200-20", and "Disparlon A630-20X" manufactured by Kusumoto Chemicals Co., Ltd. When the present composition contains an anti-sagging / anti-settling agent (Q), the content of the anti-sagging / anti-settling agent (Q) in the solid content of the coating composition is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and preferably 10 mass % or less, more preferably 3 mass % or less.

[0111] [Curing catalyst (R)] The present composition may contain a curing catalyst (R) for the purpose of improving the curability of the composition and the coating strength of the antifouling coating film formed. In particular, when the present composition contains the component (N1), it is preferable that it contains a curing catalyst (R). Examples of the curing catalyst (R) include, for example, tin catalysts such as dibutyltin dilaurate when component (N1) contains a condensation reaction curable organopolysiloxane, and platinum catalysts when component (N1) contains an addition reaction curable organopolysiloxane.

[0112] [Organosilicon Crosslinking Agent (S)] The present composition may contain an organosilicon crosslinking agent (S) other than the components described in the preceding paragraphs, for the purpose of improving the curability of the composition and the strength of the antifouling coating film formed. The organosilicon crosslinking agent (S) is preferably a compound represented by the following formula (S1) and / or a partial condensate thereof.

[0113] R 51 d SiY (4-d) (S1) (In formula (S1), R 51 represents a hydrocarbon group having 1 to 6 carbon atoms, each Y independently represents a hydrolyzable group, and d represents an integer of 0 to 2.

[0114] In formula (S1), R 51each independently represents a hydrocarbon group having 1 to 6 carbon atoms, examples of which include linear or branched alkyl groups such as methyl, ethyl, and propyl groups, cyclic alkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl groups, and aryl groups such as phenyl groups. Among these, methyl and ethyl groups are preferred. When d is 2, there are multiple R 51 may be the same or different. In formula (S1), each Y independently represents a hydrolyzable group. Examples of the hydrolyzable group include alkoxy groups such as a methoxy group and an ethoxy group, and oxime groups such as an ethylmethylketoxime group. d represents an integer of 0 or more and 2 or less, and is preferably 0 from the viewpoint of improving the curability and film strength of the antifouling coating film.

[0115] As the organosilicon crosslinking agent (S), commercially available products can be used, such as "Ethyl Silicate 28" (tetraethyl orthosilicate) manufactured by Colcoat Co., Ltd., "WACKER SILICATE TES 40 WN" (condensate of tetraethyl orthosilicate) manufactured by Wacker Asahi Kasei Silicones Co., Ltd., and "KBM-13" (trimethoxymethylsilane) manufactured by Shin-Etsu Chemical Co., Ltd.

[0116] The organosilicon crosslinking agent (S) may be used alone or in combination of two or more kinds. When the antifouling coating composition of the present invention contains an organosilicon crosslinking agent (S), the content of the organosilicon crosslinking agent (S) in the solids of the coating composition is preferably 0.1 mass % or more, more preferably 0.2 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less, from the viewpoints of adjusting the curing rate of the composition and improving the coating strength of the antifouling coating film formed.

[0117] [Antistatic agent (T)] The composition may contain an antistatic agent (T). Specific examples of the antistatic agent include cationic antistatic agents such as amidinium salts, guanidinium salts, and quaternary ammonium salts, anionic antistatic agents such as sulfonates, higher alcohol sulfates, alkylene oxide adduct sulfates of higher alcohols, higher alcohol phosphates, and alkylene oxide adduct phosphates of higher alcohols, and nonionic antistatic agents such as alkylene oxide adducts of higher alcohols and fatty acid esters of polyhydric alcohols. The antistatic agent (T) may be used alone or in combination of two or more. When the present composition contains an antistatic agent (T), the content of the antistatic agent (T) in the solid content of the composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less.

[0118] [Enzyme (U)] The present composition may contain an enzyme (U) for the purpose of improving the antifouling properties of the antifouling coating film formed. Examples of the enzyme (U) include serine protease, cysteine ​​protease, metalloproteinase, cellulase, hemicellulase, pectinase, and glycosidase. When the composition contains an enzyme (U), the content of the enzyme (U) in the solid content of the paint composition is preferably 0.0005 mass% or more, more preferably 0.01 mass% or more, and preferably 5 mass% or less, more preferably 0.1 mass% or less.

[0119] [Flame retardants (V)] The composition may contain a flame retardant (V). Examples of the flame retardant (V) include antimony oxide and paraffin oxide. The flame retardant (V) may be used alone or in combination of two or more kinds. When the composition contains a flame retardant (V), the content of the flame retardant (V) in the solid content of the coating composition is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and preferably 20 mass % or less, more preferably 1 mass % or less.

[0120] [Thermal conductivity improver (W)] The composition may contain a thermal conductivity improver (W). Examples of the thermal conductivity improver (W) include boron nitride. The thermal conductivity improver (W) may be used alone or in combination of two or more kinds. When the present composition contains a thermal conductivity improver (W), the content of the thermal conductivity improver in the solid content of the coating composition is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and preferably 20 mass % or less, more preferably 1 mass % or less.

[0121] [Anti-fogging agent (X)] The composition may contain an antifogging agent (X). Examples of the antifogging agent (X) include nonionic surfactants such as fatty acid esters of polyhydric alcohols, amines of higher fatty acids, amides of higher fatty acids, sucrose fatty acid esters, and ethylene oxide adducts of amines or amides of higher fatty acids. The antifogging agent (X) may be used alone or in combination of two or more kinds. When the present composition contains an antifogging agent (X), the content of the antifogging agent (X) in the solid content of the coating composition is preferably 0.1 mass % or more and 10 mass % or less.

[0122] [Method of preparing antifouling coating composition] The composition can be prepared by mixing the components in a given ratio and dissolving or dispersing each component as necessary. The composition may be a one-component, one-liquid type paint, or a multi-component paint made up of two or more components. When a multi-liquid paint is used, each component (each liquid) contains one or more ingredients, and it is preferable that the components are packaged separately and then stored in a container such as a can. The contents of each component can be mixed at the time of painting to prepare the antifouling paint composition.

[0123] [Anti-fouling coating film and its forming method] The antifouling coating film of the present invention is obtained by curing the antifouling coating composition of the present invention. The antifouling coating film formed by the present composition is preferably used for the purpose of preventing fouling of a substrate in water, i.e., the present composition is preferably an antifouling paint composition for preventing fouling of a substrate in water. An example of the fouling of a substrate is fouling caused by aquatic organisms. The composition of the present invention is preferably a coating composition for forming an antifouling coating film used for the purpose of preventing fouling caused by aquatic organisms.

[0124] Specifically, the antifouling coating film of the present invention includes, for example, a coating step of applying the present composition to a substrate or the like, and a curing step of curing the applied coating film (the present composition) by irradiating it with active energy rays, and if necessary, a drying step and a step of attaching a cover film or the like can be combined to obtain the antifouling coating film.

[0125] <Painting process> Examples of methods for applying the present composition include known methods such as brush coating, roller coating, spraying, roll coater coating, flow coater coating, slit coater coating, gravure coater coating, spin coater coating, curtain roll coater coating, electrostatic coating, dip coating, silk printing, and spin coating. The thickness of the antifouling coating film of the present invention is set so that the finally formed antifouling coating film has a thickness described below. The coating film may be formed by one coating, or by two or more coatings (two or more coatings). The thickness of the antifouling coating film of the present invention is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 50 μm or more, and is preferably 1,000 μm or less, more preferably 500 μm or less, even more preferably 300 μm or less. When the antifouling coating film of the present invention has such an embodiment, it becomes an antifouling coating film with excellent antifouling properties.

[0126] <Curing process> The composition can be cured to form an antifouling coating film by irradiating it with active energy rays. The active energy rays may be any active energy rays that can act on the photopolymerization initiator (C) to generate active species such as radicals.

[0127] Examples of the active energy rays include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, and infrared rays, as well as electromagnetic waves such as X-rays and gamma rays, electron beams, proton beams, and neutron beams. Light beams are preferred, and among them, ultraviolet rays are preferred in terms of curing speed, ease of availability of an irradiation device, cost, and the like. In one embodiment, examples of the light source used for light irradiation include LED lamps, ultra-high pressure, high pressure, medium pressure or low pressure mercury lamps, metal halide lamps, xenon lamps, carbon arc lamps, fluorescent lamps, tungsten lamps, chemical lamps, electrodeless lamps and sunlight. The irradiation intensity of active energy rays is usually 10mW / cm 2 More than 10,000mW / cm 2 The cumulative dose is usually 50 mJ / cm or less. 2 More than 10,000mJ / cm 2 The following is the result. In the curing step, in order to suppress the influence of curing inhibition due to active oxygen generated by the active energy rays, it is preferable to irradiate the active energy rays in an inert gas atmosphere such as nitrogen or in a state in which a cover film, a separator, or the like described below is attached.

[0128] <Drying process> When the present composition contains a volatile component such as a non-reactive solvent (E), the formation of the antifouling coating film may include a drying step for the purpose of volatilizing the volatile components in the applied coating composition. The drying step may be carried out under any conditions as long as the volatile components can be evaporated. For example, the drying may be carried out by heating at a temperature of 30° C. or higher and 120° C. or lower. The drying step may be carried out before or after the curing step, or may be carried out partially before the curing step and then after the curing step.

[0129] <Attachment process> The formation of the antifouling coating film may include a step of attaching a cover film, a separator (release film, release paper), a mold film, or the like to the wet coating film of the applied paint composition or the cured antifouling coating film for the purpose of improving the curing properties in the curing step and protecting the antifouling coating film and forming a surface shape.

[0130] <Anti-fouling coating film with fine surface structure> The antifouling coating film of the present invention may have a surface microstructure for the purpose of improving water flow resistance and the like. An antifouling coating film having a surface microstructure can be formed, for example, by applying a paint composition to a substrate or the like, contacting the substrate with a mold film or mold roll having an inverted structure of the surface microstructure to be formed, and irradiating the substrate with active energy rays in that state to cause a curing reaction. As such a surface uneven structure, a riblet structure as described in WO 2019 / 189412 is preferable. The formation of antifouling coating films having such surface microstructures is often carried out by line production, but the present composition is preferable in that it has very fast curing properties and can be produced at a higher speed. In addition, the present composition is preferable in that it can be designed to have a low content of volatile components such as non-reactive solvent (E), and therefore, even in the case of a curing reaction under sealed conditions in contact with a mold film, problems such as the generation of bubbles in the coating film due to the volatilization of volatile components are unlikely to occur.

[0131] [Laminated antifouling coating film] The laminated antifouling coating film of the present invention comprises the above-mentioned antifouling coating film and an undercoat coating film which is in contact with at least a part of the antifouling coating film. The undercoat coating film of the present invention can be formed by curing an undercoat paint composition.

[0132] <Undercoat paint composition> The undercoat coating composition of the present invention may be an active energy ray curable composition, or a condensation reaction curable composition, addition reaction curable composition or other curable composition. When an active energy ray-curable composition is used as the undercoat paint composition of the present invention, the composition may be the same as that of the antifouling coating film of the present invention, and may be, for example, a composition in which the components are adjusted to prioritize adhesion over antifouling properties, weather resistance, etc. By forming a laminated antifouling coating film using such an undercoat paint composition, the antifouling coating film and the undercoat paint film complement each other in terms of their characteristics, resulting in a well-balanced laminated antifouling coating film. The undercoat coating may be a single layer or a multi-layer consisting of two or more identical or different layers.

[0133] The undercoat paint composition of the present invention may be a composition of other curing types such as a condensation reaction curing type or an addition reaction curing type. When such an undercoat paint composition is used to form a laminated antifouling coating film, it is possible to form a laminated antifouling coating film having a function that is difficult to impart in a photocurable coating film due to poor curing caused by shielding of active energy rays. For example, if such an undercoat paint composition contains one of the inorganic fillers (J) having a low transmittance of active energy rays, it is possible to form a laminated antifouling coating film having light resistance and hiding properties that could not be obtained by the antifouling coating film alone. From the viewpoint of obtaining good adhesion between the antifouling coating film and the undercoat coating film, it is preferable that such an undercoat coating composition contains the non-photocurable organopolysiloxane (N1), and from the viewpoint of gradually penetrating the antifouling coating film and thereby exhibiting high antifouling properties over the long term, it is also preferable that the undercoat coating composition contains a biological repellent (O).

[0134] [Anti-stain tape] The antifouling tape of the present invention has the above-mentioned antifouling coating film or laminated antifouling coating film and adhesive layer (v), and has an adhesive layer (v) on one side of the antifouling coating film or on the side of the undercoat coating film of the laminated antifouling coating film opposite to the side in contact with the antifouling coating film, optionally via an intermediate layer (w). The antifouling coating film or the undercoat coating film of the laminated antifouling coating film may be directly laminated to the adhesive layer (v), or the antifouling coating film or the undercoat coating film of the laminated antifouling coating film may be laminated to the adhesive layer (v) via an intermediate layer (w).

[0135] <Middle layer (w)> The intermediate layer (w) may be at least one selected from the group consisting of a bonding layer, a barrier layer, and a substrate layer. The bonding layer has a function of increasing the bonding strength between the upper and lower layers of the intermediate layer, the barrier layer has a function of reducing the movement of water and other liquids that have permeated the intermediate layer, and the substrate layer has a function of increasing the strength of the laminated antifouling coating film. A single intermediate layer (w) may have two or more of these functions. The intermediate layer (w) may be one layer or two or more layers, provided that it is provided between the undercoat coating film and the adhesive layer (v) of the antifouling coating film or laminated antifouling coating film. When two or more layers are laminated, they may be the same or different and may be laminated in any order.

[0136] As the intermediate layer (w), a layer having a function as a bonding layer can be used without limitation as long as it has excellent adhesion to the upper and lower layers of the intermediate layer, for example, a commercially available tie coat or primer that has been dried and cured can be used. In particular, when the intermediate layer is in contact with an antifouling coating film containing a curable organopolysiloxane in the upper layer, it is preferable to use a silicone resin-based tie coat or a silicone primer.

[0137] As the intermediate layer (w), any layer having a function as a barrier layer can be used without limitation as long as it has an excellent function of reducing the movement of water and other liquids that have permeated the intermediate layer. Examples of such layers include commercially available anticorrosive paints and those described as water vapor barrier layers in JP2015-224334A.

[0138] As the intermediate layer (w), a layer having a function as a substrate layer can be used without limitation as long as it has a function of increasing the strength of the laminated antifouling coating film, and for example, those described in JP 2013-194124 A can be used. Examples of the intermediate layer (w) include coatings, films, and sheets made of materials such as resin, metal, paper, nonwoven fabric, cloth, and glass, or composite materials combining these materials.

[0139] Examples of resins used as the material for the intermediate layer (w) include silicone resins; acrylic resins; polyolefin resins; polyvinyl resins; (co)polymers of unsaturated monomers such as polystyrene; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyurethane resins; epoxy resins; polyacetal; polycarbonate; acetyl cellulose; and composites thereof. Examples of the metal constituting the intermediate layer (w) include metals composed of one or more metal elements selected from the group consisting of iron, aluminum, titanium, copper, and the like. Examples of the paper constituting the intermediate layer (w) include uncoated printing paper such as fine paper and medium quality paper, and coated paper such as art paper and coated paper, as well as so-called Japanese paper and tissue paper.

[0140] Among these, for the intermediate layer (w) that mainly functions as a bonding layer, it is preferable to use a resin as the material from the viewpoints of adhesion and ease of manufacture, and it is preferable to use a silicone resin or a (co)polymer of an unsaturated monomer as the material; for the intermediate layer (w) that mainly functions as a barrier layer, it is preferable to use a resin as the material from the viewpoints of water resistance and ease of manufacture, and it is preferable to use a silicone resin, a (co)polymer of an unsaturated monomer, or an epoxy resin as the material; for the intermediate layer (w) that mainly functions as a base layer, it is preferable to use a resin, metal, or paper as the material; and when a resin is used as the base material, it is preferable to use a (co)polymer of an unsaturated monomer or a polyurethane resin.

[0141] <Adhesive layer (v)> As the adhesive layer (v), any suitable adhesive layer can be adopted as long as it does not impair the effects of the present invention, and for example, an adhesive layer as described in JP 2013-194124 A can be used. Examples of materials for such an adhesive layer (v) include acrylic resin-based adhesives, epoxy resin-based adhesives, amino resin-based adhesives, vinyl resin (vinyl acetate polymer, etc.)-based adhesives, cured acrylic resin-based adhesives, silicone resin-based adhesives, etc. The adhesive layer may be made of one type or two or more types of materials. As the adhesive layer (v), a commercially available substrate-less tape can be used, for example, substrate-less silicone tape "NSD-100" manufactured by Nippa Corporation. The thickness of the adhesive layer (v) is preferably 10 μm or more, more preferably 20 μm or more, and preferably 150 μm or less, more preferably 100 μm or less, from the viewpoints of adhesive strength and handleability.

[0142] The adhesive strength of the adhesive layer (v) in the stain-resistant tape of the present invention is preferably 5 N / 25 mm or more and 30 N / 25 mm or less. The adhesive strength of the adhesive layer is the adhesive strength to an adherend SUS304 at a peel angle of 180° according to JIS Z0237:2009.

[0143] As the antifouling tape, for example, one having the configuration described in JP-A-2013-194124 or JP-A-2016-124994 may be used.

[0144] The antifouling tape of the present invention may be produced by applying and curing the present composition to an adhesive tape in which an intermediate layer (w) and an adhesive layer (v) have been formed in advance. Commercially available products can be used as such adhesive tapes, such as "Polyester Film Adhesive Tape 631S#100" (a tape with a total thickness of 0.15 mm consisting of a polyester film with a thickness of 0.1 mm and an acrylic adhesive layer), "Glass Cloth Adhesive Tape 540S 0.18" (a tape with a total thickness of 0.13 mm consisting of a glass cloth and a silicone adhesive layer), "Kapton (registered trademark) Adhesive Tape 650S#50" (a tape with a total thickness of 0.08 mm consisting of a polyimide film with a thickness of 0.05 mm and a silicone adhesive layer), and "Silicone Rubber Adhesive Tape 9013 0.1" (a tape with a total thickness of 0.1 mm consisting of silicone rubber, polyester film, and acrylic adhesive layer laminated in this order), etc.

[0145] The stain-proofing tape of the present invention is extremely economically advantageous because the composition is photocurable and therefore the curing time is short, and therefore the tape can be produced at high speed in a production line.

[0146] [Substrate with antifouling coating film and its manufacturing method] The substrate with an antifouling coating film of the present invention has the antifouling coating film, laminated antifouling coating film, or antifouling tape of the present invention on a substrate. The method for producing the substrate with the antifouling coating film of the present invention is not particularly limited. For example, the substrate can be obtained by a method in which the composition is applied to a substrate and cured to directly obtain the substrate, a method in which a preformed antifouling coating film or a laminated antifouling coating film is adhered to the substrate, or a method in which an antifouling tape is attached to the substrate.

[0147] The substrate is preferably one that is used underwater, and more preferably used in a wide range of industrial fields such as ships, fisheries, and underwater structures in order to prevent the substrate from being fouled for a long period of time. Examples of the substrate include ships (hull panels of large steel ships such as container ships and tankers, fishing boats, FRP boats, wooden boats, yachts, and the like, including both newly built and repaired ships), fishing materials (ropes, fishing nets, fishing gear, floats, buoys, and the like), oil pipelines, water conveyance piping, circulating water pipes, diver suits, underwater goggles, oxygen cylinders, swimsuits, torpedoes, structures such as water supply and drainage outlets of thermal and nuclear power plants, undersea cables, power transmission cables, seawater utilization equipment (seawater pumps, and the like), megafloats, coastal roads, undersea tunnels, port facilities, and underwater structures such as various marine civil engineering structures in canals, waterways, and the like. Among these, ships, underwater structures, and fishing materials are preferred, and ships and underwater structures are more preferred.

[0148] The material for the substrate is not particularly limited, and examples thereof include plastics mainly composed of polyester resins such as PET (polyethylene terephthalate) and PEN (polyethylene naphthalate), polyolefin resins such as polyethylene, chlorinated polyethylene, and polypropylene, polycarbonate, polyamide, polyimide, ABS resin, polystyrene resin, polyurethane, and acrylic resin, as well as composite materials such as natural rubber, butyl rubber, halogenated butyl rubber, ethylene propylene rubber, chloroprene rubber, styrene butadiene rubber, nitrile rubber, chlorosulfonated polyethylene, epichlorohydrin rubber, acrylic rubber, silicone rubber, fluororubber, urethane rubber, glass, ceramic materials, and glass fiber reinforced plastics, wood, and paper.

[0149] In order to improve adhesion to the substrate and undercoat film, the substrate may be surface-treated before being coated with the coating composition of the present invention. Examples of such surface treatments include corona discharge treatment, plasma treatment, ultraviolet light or electron beam treatment such as excimer laser, light cleaning treatment, flame treatment, ozone treatment, cleaning treatment using water or an organic solvent, acid / alkali treatment, polishing treatment, etc.

[0150] [Anti-stain method] The antifouling method of the present invention uses the above-mentioned antifouling coating film, laminated antifouling coating film, or antifouling tape. This is a method of antifouling by providing an antifouling coating film, laminated antifouling coating film, or antifouling tape on various substrates to be antifouled. EXAMPLES

[0151] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" refers to parts by mass unless otherwise stated. In this specification, the "solid content" of each component or the present composition refers to the components excluding volatile components contained in each component or the present composition as a solvent, and is synonymous with the content obtained by drying each component or the present composition in a hot air dryer at 125°C for 1 hour.

[0152] [Components of antifouling paint composition] The components used in the coating composition are shown in Table 1.

[0153] [Table 1]

[0154] <Acrylic polymer having hydrophilic group (B2)> (Synthesis Example 1: Synthesis of Polymer (B21)) A reaction vessel equipped with a stirrer, reflux condenser, thermometer, nitrogen inlet tube, and dropping funnel was charged with 42.9 parts by mass of methyl amyl ketone, and heated under normal pressure and nitrogen atmosphere with stirring until the liquid temperature reached 100°C. While maintaining the temperature of the reaction mixture at 100±5°C, a mixture consisting of 40.0 parts by mass of NK Ester AM-90G (methoxypolyethylene glycol acrylate, average number of polyethylene glycol units: 9, manufactured by Shin-Nakamura Chemical Co., Ltd.), 60.0 parts by mass of isobutyl acrylate, and 4.0 parts by mass of 2,2'-azobis(2-methylbutyronitrile) was dropped into the reaction vessel over 4 hours. The mixture was then stirred for 2 hours while maintaining the temperature at 100±5°C, to obtain a solution of polymer (B21). The solid content of the obtained solution was 70.3% by mass, the viscosity was 109 mPa·s, and the weight average molecular weight (Mw) of polymer (B21) was 9,100.

[0155] (Synthesis Example 2: Synthesis of Polymer (B22)) A reaction vessel equipped with a stirrer, reflux condenser, thermometer, nitrogen inlet tube, and dropping funnel was charged with 42.9 parts by mass of methyl amyl ketone, and heated to a liquid temperature of 100°C under normal pressure and nitrogen atmosphere while stirring. While maintaining the temperature of the reaction mixture at 100±5°C, a mixture consisting of 30.0 parts by mass of Viscoat #MTG (methoxypolyethylene glycol acrylate, average number of polyethylene glycol units 3, manufactured by Osaka Organic Chemical Industry Co., Ltd.), 70.0 parts by mass of Silaplane FM-0711 (manufactured by JNC Corporation, methacrylate group-containing dimethylpolysiloxane, number average molecular weight 1,000), and 4.0 parts by mass of 2,2'-azobis(2-methylbutyronitrile) was dropped into the reaction vessel over 4 hours. Thereafter, the mixture was stirred for 2 hours while maintaining the temperature at 100±5°C, to obtain a solution of polymer (B22). The solid content of the obtained solution was 69.0% by mass, the viscosity was 35 mPa·s, and the weight average molecular weight (Mw) of the polymer (B22) was 11,100.

[0156] (Solid content of polymer solution) The polymer solution was dried at 125° C. and 1 atmospheric pressure for 1 hour, and the mass of the solid content obtained was divided by the mass of the polymer solution before drying to determine the solid content (mass %).

[0157] (Viscosity of polymer solution) The viscosity (mPa·s) of the polymer solution at a liquid temperature of 25°C was measured using an E-type viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.).

[0158] (Average molecular weight of polymer) The weight average molecular weight (Mw) of the polymer was measured by gel permeation chromatography (GPC) under the following conditions. (GPC conditions) Equipment: "HLC-8320GPC" (Tosoh Corporation) Column: "TSKgel guardcolumn SuperMPHZ-M" (Tosoh Corporation) x 1 + "TSKgel SuperMultiporeHZ-M" (Tosoh Corporation) x 2 Eluent: tetrahydrofuran (THF) Flow rate: 0.35ml / min Detector: RI Column thermostat temperature: 40℃ Standard material: polystyrene Sample preparation method: An eluent was added to each of the obtained polymer solutions, and the solutions were then filtered through a membrane filter to obtain filtrates, which were used as GPC measurement samples.

[0159] [Examples 1 to 16 and Comparative Examples 1 and 2] <Production of antifouling coating composition> The components were mixed and stirred according to the blending amounts (parts by mass) shown in Table 2 to prepare antifouling coating compositions.

[0160] <Preparation of coated test panels> An epoxy-based anticorrosive undercoat paint ("Banno 500", manufactured by Chugoku Paint Co., Ltd.) was applied to a sandblasted steel plate (length 100 mm x width 70 mm x thickness 2.3 mm) so that the dry film thickness was about 100 μm, and the plate was dried for one day to form an undercoat paint film. Thereafter, a silicone-based intermediate paint ("CMP Bioclean R") was applied to the intermediate paint film at 5°C so that the dry film thickness was 100 μm, and the plate was dried for two hours at 5°C to form an intermediate paint film. Next, the antifouling paint compositions of Examples 1 to 16 and Comparative Examples 1 and 2 were applied to the intermediate paint film at 5°C using a film applicator so that the film thickness after curing was 200 μm, a separator was attached, and the plate was exposed to ultraviolet light (LED-UV with a wavelength of 365 nm, irradiation intensity of about 500 mW / cm2). 2 The irradiation time was 3 seconds to obtain a test panel with a coating.

[0161] <Adhesion evaluation> Twelve hours after the preparation of the test panels, a single blade as specified in JIS K5600-5-6 was used to make a single incision reaching the undercoat coating film on the coating surface of the test panels prepared using the antifouling coating compositions of Examples 1 to 10 and Comparative Examples 1 and 2. The test panels were then rubbed 10 times perpendicularly to the incision with a paper cloth, and the occurrence of delamination between the undercoat and intermediate coating films was evaluated as adhesion (standard) according to the following criteria. (Evaluation points) 3: Delamination occurred within 1 mm of the cut 2: Delamination occurred within 1mm to 3mm from the cut 1: Continuous delamination occurred over an area of ​​3 mm or more from the cut. 0: The coating had already peeled off and was no longer present

[0162] <Anti-stain property evaluation> 24 hours after preparing the test plates using the antifouling coating compositions of Examples 1 to 16 and Comparative Examples 1 and 2, the test plates were placed in the ocean (Hiroshima Bay, Seto Inland Sea) at a depth of 1 m from the sea surface with the test surface (antifouling coating film) facing the seabed, and after 3 months, the proportion of the barnacle-adhered area to the entire test surface was evaluated by visual observation according to the following evaluation criteria. (Evaluation points) 5: No barnacles were found 4: The area of ​​barnacles attached is less than 10% of the entire test surface. 3: The area of ​​barnacles attached is between 10% and 30% of the entire test surface. 2: The area of ​​barnacles attached is 30% or more but less than 80% of the entire test surface. 1: Barnacles are attached to more than 80% of the entire test surface

[0163] <Adhesion evaluation (immediately after irradiation)> An epoxy-based anticorrosive undercoat paint ("Banno 500", manufactured by Chugoku Paint Co., Ltd.) was applied to a sandblasted steel plate (length 100 mm × width 70 mm × thickness 2.3 mm) so that the dry film thickness was about 100 μm, and the plate was dried for one day to form an undercoat paint film. Thereafter, the antifouling paint compositions of Examples 11 to 16 were applied to the paint film at 5°C using a film applicator so that the film thickness after curing was 200 μm, a separator was attached, and the plate was exposed to ultraviolet light (LED-UV with a wavelength of 365 nm, irradiation intensity of about 500 mW / cm). 2 The exposure time was 3 seconds, and the test plate was used for evaluating the immediate adhesion. Ten seconds after the test plate was prepared, a single cut was made on the coating surface of the test plate, reaching the undercoat coating, using a single blade as specified in JIS K5600-5-6.The test plate was then rubbed 10 times perpendicularly to the cut with a paper cloth, and the occurrence of delamination with the undercoat coating was evaluated as adhesion (standard) according to the following criteria. (Evaluation points) 3: Delamination occurred within 1 mm of the cut 2: Delamination occurred within 1mm to 3mm from the cut 1: Continuous delamination occurred over an area of ​​3 mm or more from the cut. 0: The coating had already peeled off and was no longer present

[0164] [Table 2-1]

[0165] [Table 2-2]

[0166] As is clear from the results of the Examples and Comparative Examples, the composition of the present invention can form an antifouling coating film that is excellent in low-temperature adhesion and antifouling properties.

Claims

1. An antifouling coating composition comprising a photocurable organopolysiloxane (A), a slip agent (B), and a photopolymerization initiator (C), the content of the photocurable organopolysiloxane (A) in the solid content of the antifouling coating composition is 50% by mass or more and 98% by mass or less; the photocurable organopolysiloxane (A) has a (meth)acryloyl group, The antifouling coating composition further contains, as a silane coupling agent (D), at least one of a compound represented by the following formula (D1), a partial condensate thereof, and a photopolymerizable monomer (M). 【Chemistry 1】 (In formula (D1), R 21 and R 22 each independently represent an alkyl group, an alkenyl group, an aryl group, or a halogenated alkyl group having from 1 to 10 carbon atoms, R 23 represents a divalent hydrocarbon group having from 1 to 20 carbon atoms which may be interrupted by an amino group (-NR-, where R represents a hydrogen atom or a hydrocarbon group having from 1 to 10 carbon atoms), an ether group (-O-), a thioether group (-S-), an ester group (-C(=O)-O-), or an amide group (-C(=O)-NR-, where R represents a hydrogen atom or a hydrocarbon group having from 1 to 10 carbon atoms), Z represents a (meth)acryloyloxy group, and w is an integer of 2 or 3.)

2. 2. The antifouling coating composition according to claim 1, wherein the photocurable organopolysiloxane (A) is represented by the following formula (I): X p R 1 (3-p) SiO(SiR 1 2 O) m (SiX q R 1 (2-q) O) n SiX p R 1 (3-p) (I) (In formula (I), R 1 each independently represents an alkyl group, an aryl group, an aralkyl group, an alkoxy group, or a halogenated alkyl group having 1 to 10 carbon atoms; each independently represents a monovalent organic group having one or more (meth)acryloyl groups and not containing a silicon atom; m represents 10 or more and 10,000 or less; n represents 0 or more and 50 or less; each independently represents an integer of 0 to 2; each independently represents 1 or 2; and at least one of p and n is 1 or more.

3. 3. The antifouling coating composition according to claim 1, wherein the photocurable organopolysiloxane (A) has a weight average molecular weight (Mw) of 10,000 or more and 100,000 or less.

4. 4. The antifouling coating composition according to claim 1, wherein the photocurable organopolysiloxane (A) has a functional group equivalent of 300 g / mol or more and 50,000 g / mol or less.

5. The antifouling coating composition according to any one of claims 1 to 4, wherein the slipping agent (B) is at least one selected from the group consisting of phenyl-modified silicones, polyether-modified silicones, and acrylic polymers having a hydrophilic group.

6. The antifouling coating composition according to any one of claims 1 to 5, wherein the content of the slip agent (B) in the solid content of the antifouling coating composition is 0.1 mass % or more and 40 mass % or less.

7. The antifouling coating composition according to any one of claims 1 to 6, wherein the total content of the photocurable organopolysiloxane (A) and the slipping agent (B) in the solid content of the antifouling coating composition is 70 mass% or more and 99 mass% or less.

8. An antifouling coating composition according to any one of claims 1 to 7, containing a photopolymerizable monomer (M).

9. An antifouling coating film formed from the antifouling coating composition according to any one of claims 1 to 8.

10. A laminated antifouling coating film comprising an undercoat coating film and the antifouling coating film according to claim 9.

11. An antifouling tape comprising the antifouling coating film according to claim 9 or the laminated antifouling coating film according to claim 10, and an adhesive layer.

12. A substrate with an antifouling coating film, comprising the antifouling coating film according to claim 9, the laminated antifouling coating film according to claim 10, or the antifouling tape according to claim 11 on the substrate.

13. The substrate with an antifouling coating film according to claim 12, wherein the substrate is one selected from the group consisting of ships, underwater structures, fishing materials, and cables.

14. A method for producing a substrate with an antifouling coating film, comprising the steps of: applying the antifouling coating composition according to any one of claims 1 to 8 to a substrate; and irradiating the applied coating film with active energy rays.

15. An antifouling method, comprising using the antifouling coating film according to claim 9, the laminated antifouling coating film according to claim 10, or the antifouling tape according to claim 11.

Citation Information

Patent Citations

  • Enhancement of property of biofouling release coating

    JP2001002515A

  • Antifouling paint composition

    JP2006274267A

  • Solvent-free silicone rubber protective coating composition

    JP2007505166A

  • Antifouling tape manufacturing method

    JP2016203039A

  • Antifouling coating material composition

    JP2019199600A