Coating composition and uses thereof
A hydrosilylation-curable silicone elastomer composition with silicon-free microparticles addresses gloss changes in silicone-based synthetic leather composites by maintaining gloss consistency through abrasion, enhancing abrasion resistance and flexibility.
Patent Information
- Application Number
- JP2023538929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-30
- Filing Date
- 2021-12-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Silicone-based synthetic leather composites experience significant changes in gloss after abrasion, either decreasing due to wear patterns or increasing due to surface smoothing, which is a common issue in polymer elastomers.
A hydrosilylation-curable silicone elastomer composition is developed, comprising organopolysiloxane polymers, reinforcing silica filler, a silicone resin crosslinking agent, a hydrosilylation catalyst, and silicon-free fine particles, forming a highly crosslinked matrix to minimize gloss changes after abrasion.
The composition maintains consistent gloss levels after abrasion by compensating for surface roughness changes with silicon-free microparticles, providing excellent abrasion resistance without compromising flexibility or conformability.
Smart Images

Figure 0007573755000006 
Figure 0007573755000007 
Figure 0007573755000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a hydrosilylation curable silicone elastomer composition as or for use as a topcoat for synthetic leather materials, particularly silicone-based synthetic leather composites, a silicone coating as a topcoat for synthetic leather materials that is a cured product of the composition, a method of making the topcoat and synthetic leather materials using the same, and the use of the synthetic leather material products. The topcoat is designed to provide a highly crosslinked silicone matrix containing silicon-free organic particulates to minimize or at least reduce gloss change after abrasion.
[0002] A variety of synthetic alternatives to natural leather have been developed, mainly using polyurethane (PU) or polyvinyl chloride (PVC)-based materials. They are used in a wide variety of applications, including furniture, decoration, handbags, luggage, clothing, footwear, car interiors, car seats, etc. However, to be used as synthetic leather, stringent physical property requirements, such as flame retardancy and smoke density, suitable adhesive strength to prevent the coating layer from peeling off during use, and heat resistance, stain resistance, solvent resistance, hydrolysis resistance, etc. are required to meet increasingly stringent safety regulations. PU and / or PVC-based materials often cannot meet the above physical property requirements.
[0003] Other alternatives to natural leather include silicone-based synthetic leather composites. Such silicone-based synthetic leather composites may have some advantages over PU and / or PVC-based material alternatives. For example, they generally do not use plasticizers or toxic heavy metals, and can be prepared using more environmentally friendly manufacturing methods, considering that the manufacture of organic synthetic leather relies on the use of environmentally problematic solvents such as dimethylformamide (DMF), which often remains at least partially in synthetic leather products after manufacture.
[0004] Silicone-based synthetic leather composites can be made via several routes, but are generally manufactured using a textile support layer, two or more layers of hydrosilylation-curable liquid silicone rubber composition, and a release liner. For example, a first liquid silicone rubber (LSR) composition may be coated onto the release liner and then cured to form a first layer or skin layer. A second LSR composition, usually having different physical properties from the first layer, is applied onto the cured first layer to form an adhesive layer, and then a textile support layer is placed on the second LSR layer and then cured, and then the second LSR composition is cured to form an adhesive layer located between the skin layer and the textile support layer. If and when necessary, the release liner is then removed. If deemed appropriate to form a silicone-based leather composite, a layer of hydrosilylation-curable silicone elastomer composition may also be applied between the release liner and the textile layer. For example, a third layer may be provided as a protective topcoat on top of the skin layer.
[0005] Such silicone-based synthetic leather composites can outperform conventional PU and PVC synthetic leathers in terms of physical properties, for example, by their ability to provide better flexibility over a wide temperature range, as well as excellent UV and heat resistance. Topcoats are particularly important because they help provide advantageous properties such as abrasion resistance and dirt resistance. They are also believed to be gentle on human skin and provide the user with an excellent feel. Unfortunately, however, topcoats made from such silicone-based materials are unable to maintain the same desired gloss appearance after abrasion. After abrasion, gloss may decrease or increase. The decrease in gloss is caused by the appearance of abrasion patterns due to adhesive contact between the solid asperities of the abrasive and the surface of the silicone-based synthetic leather composite. This is a typical wear phenomenon of polymer elastomers. Alternatively, an increase in gloss may be observed, the underlying cause of which is the smoothing of a rough surface with small grains by repeated frictional interactions with a harder material, i.e., the increase in gloss caused by the reduction in surface roughness.
[0006] Therefore, there remains a need for an improved silicone coating composition suitable for forming a topcoat for a silicone-based synthetic leather composite topcoat that, upon curing, can visually minimize the change in the level of gloss change after abrasion.
[0007] 1. A leather coating composition comprising a hydrosilylation-curable silicone elastomer composition, comprising: Component (i) one or more organopolysiloxane polymers having a viscosity of 1000 to 500,000 mPa.s at 25°C, wherein at least 5 weight percent (wt.%) of the polymer per molecule is an unsaturated group selected from an alkenyl group, an alkynyl group, or a mixture thereof; Component (ii) an inorganic reinforcing silica filler, optionally treated with one or more filler treating agents (to render the filler hydrophobic); and component (iii) a silicone resin crosslinker having terminal (M) groups containing silicone-bonded hydrogen, wherein the molar ratio of Si-H groups in component (iii) to unsaturated groups in the composition is from 0.5:1 to 20:1; Component (iv) a hydrosilylation catalyst; and Component (v) non-silicon-containing organic fine particles having a number average particle size of 0.5 to 500 μm as determined using a field emission scanning electron microscope, which are thermally stable up to a temperature of at least 180° C., and which are present in the hydrosilylation-curable silicone elastomer composition in an amount of 5 to 35% by weight of the composition; A composition comprising:
[0008] The topcoat is designed to provide a highly crosslinked silicone matrix containing silicon-free particulates to reduce gloss change after abrasion.
[0009] Also provided is a synthetic leather having a topcoat in the form of a cured layer of the leather coating composition described herein, particularly a topcoat for silicone-based synthetic leather composites.
[0010] Also provided are silicone coatings formed as a reaction product of the curing of the leather coating compositions described herein, methods of utilizing same to make topcoats and silicone-based synthetic leather composites, and uses of articles made from the silicone-based synthetic leather composites.
[0011] (i) Organopolysiloxane polymer Component (i) of the hydrosilylation curable silicone elastomer composition of the leather coating composition is one or more organopolysiloxane polymers having a viscosity of 1000 to 500000 mPa.s at 25° C., wherein at least 5% by weight of the polymer per molecule are unsaturated groups selected from alkenyl groups, alkynyl groups, or mixtures thereof as determined using quantitative infrared analysis according to ASTM E168, e.g., the organopolysiloxane polymer (i) is an organopolysiloxane polymer having a plurality of groups of formula (I): R a SiO (4-a) / 2 (I) wherein each R is independently selected from an aliphatic hydrocarbyl group, an aromatic hydrocarbyl group, or an organyl group (i.e., any organic substituent having one free valence at a carbon atom, regardless of the type of functional group). Saturated aliphatic hydrocarbyls include, but are not limited to, alkyl groups such as methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl, and cycloalkyl groups such as cyclohexyl. Unsaturated aliphatic hydrocarbyls include, but are not limited to, alkenyl groups such as vinyl, allyl, butenyl, pentenyl, cyclohexenyl, and hexenyl, and alkynyl groups. Aromatic hydrocarbon groups include, but are not limited to, phenyl, tolyl, xylyl, benzyl, styryl, and 2-phenylethyl. Examples of organyl groups include, but are not limited to, halogenated alkyl groups such as chloromethyl and 3-chloropropyl, nitrogen-containing groups such as amino, amido, imino, and imido groups, and oxygen-containing groups such as polyoxyalkylene, carbonyl, alkoxy, and hydroxyl groups. Further organyl groups may include sulfur-, phosphorus-, and / or boron-containing groups. The subscript "a" may be 0, 1, 2, or 3, but is typically predominantly 2 or 3.
[0012] Siloxy groups may be described by an abbreviated (short) nomenclature, i.e., "M", "D", "T", and "Q", when R is an organic group, typically a methyl group (further teachings on silicone nomenclature can be found in Walter Noll, Chemistry and Technology of Silicones, dated 1962, Chapter I, pages 1-9). M units are siloxy groups where a=3, i.e., RSiO 1 / 2 and the D unit is a siloxy group where a=2, i.e., RSiO 2 / 2 and the T unit is a siloxy group where a=1, i.e., RSiO 3 / 2 and the Q units are siloxy groups where a=0, i.e., SiO 4 / 2is equivalent to.
[0013] Examples of typical groups of the organopolysiloxane polymer (i) include mainly alkenyl, alkyl, and / or aryl groups. The groups may be pendant (on D or T siloxy groups) or terminal (on M siloxy groups). Thus, suitable alkenyl groups in the organopolysiloxane polymer (i) typically contain 2 to 10 carbon atoms, such as vinyl, isopropenyl, allyl, and 5-hexenyl, typically vinyl groups, and are present on the polymer in an amount of at least 5% by weight of the polymer per molecule, alternatively 5 to 15% by weight of the polymer per molecule, alternatively 6 to 15% by weight of the polymer per molecule, alternatively 7 to 15% by weight of the polymer per molecule, as previously indicated, which can be determined using quantitative infrared analysis according to ASTM E168.
[0014] Typically, the silicon-bonded organic groups bonded to the organopolysiloxane polymer (i), other than the unsaturated groups selected from alkenyl and / or alkynyl groups, are selected from monovalent saturated hydrocarbon groups, typically containing from 1 to 10 carbon atoms, and monovalent aromatic hydrocarbon groups, typically containing from 6 to 12 carbon atoms, that are unsubstituted or substituted with groups that do not interfere with the cure of the composition, such as halogen atoms. Preferred species of silicon-bonded organic groups are, for example, alkyl groups, such as methyl, ethyl, and propyl, and aryl groups, such as phenyl.
[0015] The molecular structure of the organopolysiloxane polymer (i) is typically linear, although some branching may be present due to the presence of T groups (as described above) within the molecule.
[0016] In order to achieve useful levels of physical properties in elastomers prepared by curing the hydrosilylation-curable silicone elastomer compositions as described above, the viscosity of the organopolysiloxane polymer (i) should be at least 1000 mPa.s at 25° C. The upper viscosity limit of the organopolysiloxane polymer (i) is limited to a maximum viscosity of 500,000 mPa.s at 25° C.
[0017] Generally, each organopolysiloxane contains at least 5% by weight of the polymer of unsaturated groups selected from alkenyl groups, alkynyl groups, or mixtures thereof, per molecule. The amount (by weight) of unsaturated groups present is determined using quantitative infrared analysis according to ASTM E168. Component (i) has a viscosity, unless otherwise indicated, of from 1000 mPa.s to 500,000 mPa.s at 25°C, alternatively from 1000 mPa.s to 150,000 mPa.s at 25°C, alternatively from 2000 mPa.s to 125,000 mPa.s at 25°C, alternatively from 2000 mPa.s to 100,000 mPa.s at 25°C, alternatively from 5000 mPa.s to 80,000 mPa.s, measured at 25°C according to the cup / spindle method of ASTM D1084-16 Method B using a spindle appropriate for the viscosity range.
[0018] The organopolysiloxane polymers (i) may be selected, for example, from polydimethylsiloxanes, alkylmethylpolysiloxanes, alkylarylpolysiloxanes, or copolymers thereof containing alkenyl and / or alkynyl groups, and may have any other suitable end groups, for example, they may be trialkyl terminated, alkenyldialkyl terminated, or may be terminated with any other suitable combination of end groups, provided that each organopolysiloxane polymer (i) contains at least 5% by weight of polymer per molecule as described above.
[0019] Thus, the organopolysiloxane polymer (i) may be, by way of example, a dimethylvinyl-terminated polydimethylsiloxane, a dimethylvinyl-terminated dimethylmethylphenylsiloxane, a trialkyl-terminated dimethylmethylvinylpolysiloxane, or a dialkylvinyl-terminated dimethylmethylvinylpolysiloxane copolymer, but in view of the presence of high levels of alkenyl and / or alkynyl groups, may alternatively be a trialkyl-terminated dimethylmethylvinylpolysiloxane or a dialkylvinyl-terminated dimethylmethylvinylpolysiloxane copolymer.
[0020] For example, an organopolysiloxane polymer (i) containing unsaturated groups selected from alkenyl groups and / or alkynyl groups at two ends can be represented by the general formula (II). R'R”R”'SiO-(R”R”'SiO) m -SiOR'''R”R' (II) In formula (II), each R' may be an alkenyl or alkynyl group, typically containing 2 to 10 carbon atoms. Alkenyl groups include, but are not limited to, vinyl, propenyl, butenyl, pentenyl, hexenyl, alkenylated cyclohexyl groups, heptenyl, octenyl, nonenyl, decenyl, or similar linear and branched alkenyl groups, and alkenylated aromatic ring structures. Alkenyl groups may be selected from, but are not limited to, ethynyl, propynyl, butynyl, pentynyl, hexynyl, alkenylated cyclohexyl groups, heptenyl, octenyl, nonenyl, decynyl, or similar linear and branched alkenyl groups, and alkenylated aromatic ring structures.
[0021] R" does not contain ethylenic unsaturation, and each R" may be the same or different and is independently selected from monovalent saturated hydrocarbon groups, typically containing 1 to 10 carbon atoms, and monovalent aromatic hydrocarbon groups, typically containing 6 to 12 carbon atoms. R" may be unsubstituted or substituted with one or more groups that do not interfere with the cure of the hydrosilylation-curable silicone elastomer compositions described herein, such as halogen atoms. R'" is R' or R".
[0022] The organopolysiloxane polymer (i) is typically present in an amount of from 3% or 10% by weight of the composition to 50% or 45% by weight of the composition, for example, the organopolysiloxane polymer (i) may be present in the range of 10-50% or 10-45% by weight of the composition.
[0023] (ii) Reinforcing Silica Filler Component (ii) of the leather coating composition comprising the hydrosilylation curable silicone elastomer composition is a reinforcing silica filler.Preferably, component (ii) of the leather coating composition comprising the hydrosilylation curable silicone elastomer composition is a reinforcing silica filler, preferably provided in micronized form.In order to prevent the phenomenon called "creping" or "crepe hardening" during processing of the hydrosilylation curable silicone elastomer composition, the reinforcing silica filler (ii) is often treated with one or more known filler treating agents.
[0024] Precipitated silica and / or fumed silica, or fumed silica, is typically at least 50 m 2 / g (BET method according to ISO9277:2010). 2 / g (BET method according to ISO9277:2010), or 50-300m 2Fillers with a surface area of 0.01 to 0.01 g (BET method according to ISO 9277:2010) are typically used. Both types of silica are commercially available. Preferably, they are provided in micronized form.
[0025] The amount of reinforcing silica filler (ii), e.g., finely divided silica, in the hydrosilylation curable silicone elastomer compositions herein is from 5 to 40% by weight, alternatively from 5 to 30% by weight. In some cases, the amount of reinforcing silica filler may be from 7.5 to 30% by weight, alternatively from 10 to 30% by weight, alternatively from 15 to 30% by weight, based on the weight of the composition.
[0026] If the reinforcing silica filler (ii) is originally hydrophilic (e.g. untreated silica filler), it is typically treated with a treatment agent to make it hydrophobic.The surface treatment makes the filler easily wettable by the organopolysiloxane polymer (i), so that these surface-modified reinforcing silica fillers (ii) do not aggregate and can be homogeneously incorporated into the organopolysiloxane polymer (i).As a result, the hydrosilylation curable silicone elastomer composition and the cured material obtained by curing it have improved room temperature mechanical properties.
[0027] The surface treatment may be carried out prior to introduction into the composition, or may be carried out in situ (i.e., in the presence of at least some of the other components of the compositions herein by blending these components together at room temperature or above until the filler is fully treated). Typically, untreated reinforcing silica filler (ii) is treated with a treating agent in situ in the presence of organopolysiloxane polymer (i) and after mixing, a silicone rubber base material is obtained to which other components may be added.
[0028] Typically, the reinforcing silica filler (ii) can be surface-treated with any low molecular weight organosilicon compound disclosed in the applicable art to prevent creping of the hydrosilylation-curable silicone elastomer composition during processing.For example, organosilanes, organopolysiloxanes, or organosilazanes such as hexaalkyldisilazanes, short-chain siloxane diols, or fatty acids, or fatty acid esters such as stearic acid esters, to make the filler hydrophobic, thereby making it easier to handle and obtain a homogeneous mixture with other components. Specific examples include, but are not limited to, silanol-terminated trifluoropropylmethylsiloxane, silanol-terminated ViMesiloxane, tetramethyldi(trifluoropropyl)disilazane, tetramethyldivinyldisilazane, silanol-terminated MePhsiloxane, liquid hydroxyl-terminated polydiorganosiloxanes containing an average of 2-20 diorganosiloxane repeating groups per molecule, hexaorganodisiloxane, and hexaorganodisilazane. A small amount of water may be added along with the silica treating agent as a processing aid.
[0029] The filler may be introduced into the hydrosilylation-curable silicone elastomer composition in the form of a masterbatch or base comprising the filler and an organopolysiloxane polymer. The organopolysiloxane polymer used in the masterbatch or base may be of similar structure to component (i), or alternatively, may be an organopolysiloxane polymer having a viscosity in the same range as component (i), but with an alkenyl and / or alkynyl content of <5% by weight of the polymer (ASTM E168). If necessary, the fumed silica may be rendered hydrophobic in situ by introducing a suitable hydrophobizing agent into the mixture during preparation of the masterbatch.
[0030] The hydrosilylation-curable silicone elastomer compositions described herein are cured using a hydrosilylation cure package that includes an organohydrogenpolysiloxane having three or more silicon-bonded hydrogen atoms per molecule (component iii) and a hydrosilylation catalyst (component iv).
[0031] (iii) Organohydrogenpolysiloxane Component (iii) of the leather coating composition comprising a hydrosilylation curable silicone elastomer composition is a silicone resin crosslinker having end groups containing silicone-bonded hydrogen that acts as a crosslinker for polymer (i) by addition reaction of the silicon-bonded hydrogen atoms of component (iii) with the alkenyl and / or alkynyl groups of component (i) under the catalytic activity of component (iv) described below. Component (iii) contains at least 5,000 parts per million (ppm) of silicon-bonded hydrogen (Si-H), alternatively at least 7000 ppm, alternatively between 7000 and 12,000 ppm of silicon-bonded hydrogen, alternatively between 8000 and 11,000 ppm of silicon-bonded hydrogen, such that the silicon-bonded hydrogen atoms of this component are sufficiently reactive with the alkenyl and / or alkynyl groups, typically alkenyl groups, especially vinyl groups, of component (i) to form a network therewith, thereby curing the composition. The amount of silicon-bonded hydrogen present is also determined using quantitative infrared analysis according to ASTM E168.
[0032] The molecular structure of component (iii) is resinous and contains a mixture of Q, T, D, and M groups and has a viscosity of 10 to 5000 mPa.s at 25° C., alternatively 10 to 1000 mPa.s at 25° C., alternatively 10 to 500 mPa.s at 25° C., using a Brookfield DV 3T rheometer to provide good miscibility with component (i).
[0033] Examples of component (iii) of the leather coating composition comprising the hydrosilylation-curable silicone elastomer composition include: (CH3)2HSiO 1 / 2 M groups containing Si-H, such as the (CH3)3SiO group 1 / 2 Trialkyl M groups such as the SiO 4 / 2 a silicone resin comprising or consisting of a group; (CH3)2HSiO 1 / 2 Group and SiO 4 / 2silicone resins comprising or consisting of Si-H containing M groups such as groups; (CH3)2HSiO 1 / 2 M groups containing Si-H, such as the (CH3)2SiO group 2 / 2 Group, and SiO 4 / 2 a silicone resin comprising or consisting of a group; (CH3)2HSiO 1 / 2 M groups containing Si-H such as SiO 4 / 2 Group, and (C6H5)3SiO 1 / 2 Examples of suitable silicone resins include, but are not limited to, silicone resins comprising or consisting of groups, as well as alternatives in which methyl is replaced with phenyl groups or other alkyl groups or mixtures thereof. The silicone resin may also include T and / or D groups, or T groups.
[0034] Optionally, other cross-linking agents may also be utilized. These may include: 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, Tris(hydrogendimethylsiloxy)methylsilane, Tris(hydrogendimethylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, trimethylsiloxy endblocked methylhydrogen polysiloxane, Trimethylsiloxy endblocked dimethylsiloxane / methylhydrogensiloxane copolymer, dimethylhydrogensiloxy endblocked dimethylpolysiloxane, Dimethylhydrogensiloxy endblocked dimethylsiloxane / methylhydrogensiloxane copolymer, Trimethylsiloxy endblocked methylhydrogen siloxane / diphenyl siloxane copolymer, Trimethylsiloxy endblocked methylhydrogensiloxane / diphenylsiloxane / -dimethylsiloxane copolymer, Trimethylsiloxy endblocked methylhydrogensiloxane / methylphenylsiloxane / -dimethylsiloxane copolymer, Dimethylhydrogensiloxy endblocked / dimethylsiloxane / -diphenylsiloxane copolymers, and / or Dimethylhydrogensiloxy endblocked methylhydrogensiloxane / dimethylsiloxane / -methylphenylsiloxane copolymer However, it is preferred that component (iii) is one or more of the silicone resins described above.
[0035] Component (iii) is typically present in the total composition in an amount of 5-30%, 5-20%, or 10-20% by weight of the composition, with the amount present typically being determined by the molar ratio of silicon-bonded hydrogen atoms in component (iii) to the total number of all unsaturated groups, such as alkenyl and alkynyl groups, often vinyl groups. In this composition, the molar ratio of silicon-bonded hydrogen atoms in component (iii) to the total number of all unsaturated groups is from 0.5:1 to 20:1, alternatively from 0.5:1 to 10:1, alternatively from 0.5:1 to 5:1, or alternatively from 1:1 to 5:1, preferably with an excess of Si-H.
[0036] iv) Hydrosilylation catalyst As mentioned above, the leather coating composition is cured via a hydrosilylation (addition) reaction catalyzed by a hydrosilylation (addition cure) catalyst (iv) that is a metal selected from the platinum group, i.e. platinum, ruthenium, osmium, rhodium, iridium, and palladium, or a compound of such metal. Platinum and rhodium compounds are preferred due to the high activity levels of these catalysts in the hydrosilylation reaction.
[0037] Catalyst (iv) The catalyst (iv) may be a platinum group metal, a platinum group metal supported on a support such as activated carbon, a metal oxide such as aluminium oxide or silicon dioxide, silica gel or powdered charcoal, or a compound or complex of a platinum group metal.
[0038] Examples of preferred hydrosilylation catalysts (iv) are platinum-based catalysts such as platinum black, platinum oxide (Adams' catalyst), platinum on various solid supports, chloroplatinic acid, alcohol solutions of chloroplatinic acid, and complexes of chloroplatinic acid with ethylenically unsaturated compounds such as olefins and organosiloxanes containing ethylenically unsaturated silicon-bonded hydrocarbon groups. Usable soluble platinum compounds include, for example, platinum-olefin complexes of the formula (PtCl2(olefin)2 and H(PtCl3.olefin), in which case preference is given to the use of alkenes having 2 to 8 carbon atoms, such as the isomers of ethylene, propylene, butene and octene, or cycloalkanes having 5 to 7 carbon atoms, such as cyclopentene, cyclohexene and cycloheptene. Other soluble platinum catalysts are, for example, platinum-cyclopropane complexes of the formula (PtCl2C3H6)2, reaction products of hexachloroplatinic acid with alcohols, ethers and aldehydes or mixtures thereof, or reaction products of hexachloroplatinic acid with methylvinylcyclotetrasiloxane in the presence of sodium bicarbonate in an ethanolic solution. Platinum catalysts with phosphorus, sulfur and amine ligands can also be used, for example (Ph3P)2PtCl2, and complexes of platinum with vinylsiloxanes, such as sym-divinyltetramethyldisiloxane.
[0039] Therefore, specific examples of suitable platinum-based catalysts include: (i) Complexes of chloroplatinic acid with organosiloxanes containing ethylenically unsaturated hydrocarbon groups, as described in U.S. Pat. No. 3,419,593; (ii) Chloroplatinic acid in either the hexahydrate or anhydrous form; (iii) a platinum-containing catalyst obtained by a process comprising reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound, such as divinyltetramethyldisiloxane; (iv) alkene-platinum-silyl complexes as described in U.S. Pat. No. 6,605,734, such as (COD)Pt(SiMeCl2)2, where "COD" is 1,5-cyclooctadiene; and / or (v) Karstedt's catalysts, which are complexes of platinum and divinyltetramethyldisiloxane, typically containing about 1% by weight of platinum in a solvent, such as toluene, are described in U.S. Patents 3,715,334 and 3,814,730.
[0040] The hydrosilylation catalyst (iv) of the hydrosilylation-curable silicone elastomer composition is present in the total composition in a catalytic amount, i.e., an amount or content sufficient to catalyze the addition / hydrosilylation reaction and cure the composition into an elastomeric material under desired conditions. Varying levels of the hydrosilylation catalyst (iv) can be used to adjust the reaction rate and cure rate. The catalytic amount of the hydrosilylation catalyst (iv) is generally 0.01 ppm to 10,000 ppm, alternatively 0.01 to 5000 ppm, alternatively 0.01 to 3,000 ppm, alternatively 0.01 to 1,000 ppm, by weight of platinum group metal per million parts (ppm) based on the weight of the composition. In certain embodiments, the catalytic amount of the catalyst may range from 0.01 to 1,000 ppm, alternatively 0.01 to 750 ppm, alternatively 0.01 to 500 ppm, alternatively 0.01 to 100 ppm of metal based on the weight of the composition. The ranges may relate to just the metal content in the catalyst, or to the entire catalyst (including its ligands), as specified, but typically these ranges relate to just the metal content in the catalyst. The catalyst may be added as a single species or as a mixture of two or more different species. Typically, depending on the form / concentration in which the catalyst package is provided, the amount of catalyst present is in the range of 0.001-3.0% by weight of the composition, alternatively 0.01-3.0% by weight of the composition, alternatively 0.1-3.0% by weight of the composition, alternatively 0.1-2.0% by weight of the composition, or alternatively 0.1-1.5% by weight of the composition.
[0041] (v) Silicon-free organic fine particles Component (v) of the hydrosilylation curable silicone elastomer composition herein is a silicon-free organic particulate having a number average particle size of 0.5 to 500 μm, alternatively 0.5 to 250 μm, alternatively 0.5 to 100 μm, alternatively 0.5 to 75 μm, alternatively 1.0 to 50 μm. The number average particle size can be measured using a field emission scanning electron microscope, such as the FEI Nova NanoSEM™ 630 Scanning Electron Microscope from Thermo Fisher Scientific. For example, this can be accomplished by taking a field emission scanning electron micrograph of the particles, then randomly selecting 10 particles from the photograph and measuring the diameter of each particle in the image. The average diameter is then calculated for the selected particles.
[0042] The silicon-free inorganic particulates of component (v) are thermally stable up to a temperature of at least 180°C and are present in the composition in an amount of 5-35% by weight of the composition, alternatively 5-30% by weight, alternatively 5-25% by weight. They are required to be thermally stable throughout the curing process, which is typically held at a temperature of 80°C to 180°C. By "thermally stable" it is meant that the silicon-free inorganic particulates do not thermally decompose at temperatures below 180°C. This is determined by placing a sample of the silicon-free inorganic particulates in a suitable container and then placing the container in a preheated oven at a temperature of 180°C and atmospheric pressure for 30 minutes. After 30 minutes in the oven, the sample is visually evaluated to determine whether the particulates appear to be in their original form, in which case they would be considered thermally stable up to a temperature of 180°C (pass), or whether they have decomposed in some way that is visually evident, for example by agglomeration, liquefaction, carbonization, and / or decomposition.
[0043] Component (v) silicon-free inorganic particulate is generally or preferably spherical and / or quasi-spherical in shape. Component (v) silicon-free inorganic particulate may be a thermosetting material. Furthermore, for the avoidance of doubt, component (v) silicon-free inorganic particulate is silicon-free and allows only trace amounts of contamination, i.e., silicon-free inorganic particulate does not substantially contain silicon atoms or silicon-containing compounds. The term substantially used above is intended to mean that only trace amounts of silicon, typically in the form of impurities, are present.
[0044] The component (v) silicon-free inorganic particulates can be made of any suitable organic material as long as it meets certain requirements, and the particulates can be selected from polyurethane particulates, acrylic particulates, methacrylic particulates, polytetrafluoroethylene particulates, polyester particulates, polyamide particulates, and / or polyolefin particulates, and their derivatives and / or mixtures.For example, the particulates can include, but are not limited to, polyethylene, polystyrene, polyvinyl acetate, polyvinyl chloride, polyvinylidene chloride, polyacrylonitrile, polymethylmethacrylate, polybutadiene, polychloroprene, and other vinyl polymers, and their copolymers; polyamides such as nylon 6, nylon 66; and polyethylene terephthalate, polyacetal, and their blends.The component (v) silicon-free inorganic particulates have been found to be effective as a means of minimizing the visual change of gloss after rubbing, because while small grains on the leather surface are worn away during rubbing, the particulates appear on the topcoat surface and help to compensate for the loss of surface roughness, thereby avoiding the increase in gloss. In addition, the presence of robust silicon-free inorganic particulates at the topcoat surface helps to avoid further abrasion of the matrix.
[0045] Optional Additives The leather coating composition may include one or more additives. Examples of these optional additives include cure inhibitors, cured silicone elastomer powders, These include inorganic non-reinforcing fillers, conductive additives, pot life extenders, lubricants, flame retardants, pigments, colorants, chain extenders, heat stabilizers, diluents (designed to evaporate during cure), compression set improving additives, anti-squeak agents, antioxidants, antistatic agents, stain and light stabilizers, antifreeze agents and / or biocides, and mixtures thereof.
[0046] Inhibitors Optionally, since a hydrosilylation cure system is utilized, in order to obtain a longer working or pot life of the hydrosilylation-curable silicone elastomer composition used in or as a leather coating composition, a suitable inhibitor may be incorporated into the composition to retard or inhibit the activity of the catalyst.
[0047] Inhibitors for platinum metal catalysts, and generally platinum group metal catalysts, are well known in the art. Hydrosilylation or addition reaction inhibitors include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylenic alcohols, silylated acetylenic alcohols such as methyl(tris(1,1-dimethyl-2-propynyloxy))silane, maleates, fumarates, ethylenically or aromatically unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes, unsaturated hydrocarbon monoesters and diesters, conjugated ene-ynes, hydroperoxides, nitriles, and diaziridines. Alkenyl-substituted siloxanes, such as those described in U.S. Pat. No. 3,989,667, may also be used, of which cyclic methylvinylsiloxanes are preferred.
[0048] Another known class of platinum catalyst inhibitors includes the acetylenic compounds disclosed in U.S. Patent No. 3,445,420. Acetylenic alcohols, such as 2-methyl-3-butyn-2-ol, are a preferred class of inhibitors that suppress the activity of platinum-containing catalysts at 25° C. Hydrosilylation-curable silicone elastomer compositions containing these inhibitors typically must be heated to temperatures of 70° C. or above to cure at a practical rate.
[0049] Examples of acetylenic alcohols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof.
[0050] In some cases, when present, inhibitor concentrations as low as 1 mole of inhibitor per mole of metal of catalyst (iv) provide satisfactory storage stability and cure rates. In other cases, inhibitor concentrations of up to 500 moles of inhibitor per mole of metal of catalyst (iv) are required. The optimum concentration for a given inhibitor in a given composition is readily determined by routine experimentation. When present in the composition, the inhibitor is typically present in an amount of 0.0125-10% by weight of the composition, depending on the concentration and form in which the selected inhibitor is provided / commercially available. Mixtures of the above may also be used.
[0051] Cured Silicone Elastomer Powder Another optional additive that may be included in the hydrosilylation curable silicone elastomer composition is a suitable cured silicone elastomer powder. The cured silicone elastomer powder may have any suitable average particle size, for example, 0.01 to 100 μm, alternatively 0.01 to 50 μm, alternatively 0.01 to 25 μm, as measured using Dow Silicone Corporation Corporate Test Method CTM 1138, which is publicly available upon request. They may contain chemical functional groups, for example, epoxy groups, (meth)acryloxy groups, or may be coated, for example, with a silica-treated coating.
[0052] The cured silicone elastomer powder is made from a suitable curable silicone composition. The curable silicone composition may include, for example, an addition (hydrosilylation) reaction curing silicone composition, a condensation reaction curing silicone composition, an organic peroxide curing silicone composition, and an ultraviolet light curing silicone composition. The addition reaction curing and condensation reaction curing silicone compositions are preferred due to their ease of handling.
[0053] Commercial examples that can be utilized as component (v) include, by way of example, Dowsil® 23N Additive, Dowsil® 603T additive, and Dowsil® 9701 Cosmetic Powder, manufactured by Dow Silicones Corporation.
[0054] When present, the cured silicone rubber powder is present in the hydrosilylation curable silicone elastomer composition in an amount from 2.5 to 20% by weight of the composition, alternatively from 2.5 to 15% by weight of the composition, alternatively from 2.5 to 10% by weight of the composition.
[0055] Inorganic non-reinforcing fillers Inorganic non-reinforcing silica fillers in the hydrosilylation curable silicone elastomer composition, when present, may include crushed quartz, diatomaceous earth, barium sulfate, iron oxide, titanium dioxide and carbon black, wollastonite, and platelet-type fillers such as graphite, graphene, talc, mica, clay, layered silicates, kaolin, montmorillonite, and mixtures thereof. Other inorganic non-reinforcing fillers that may be used alone or in addition to the above fillers include aluminite, calcium sulfate (anhydrite), gypsum, calcium sulfate, magnesium carbonate, aluminum trihydroxide, magnesium hydroxide (hydrotalcite), graphite, copper carbonates such as malachite, nickel carbonates such as zarachite, barium carbonates such as witherite, and / or strontium carbonates such as strontianite.
[0056] The inorganic non-reinforcing fillers, when present, may alternatively or additionally be selected from aluminum oxide, silicates from the group consisting of: olivine family, garnet family; aluminosilicates; cyclic silicates; chain silicates; and layered silicates. The olivine family includes silicate minerals such as, but not limited to, forsterite and Mg2SiO4. The garnet family includes red garnet; Mg3Al2Si3O 12 ; green garnet; and Ca2Al2Si3O 12 The aluminosilicates include ground silicate minerals such as, but not limited to, sillimanite; Al2SiO5; mullite; 3Al2O32SiO2; kyanite, and Al2SiO5. The cyclic silicate family includes cordierite and Al3(Mg,Fe)2[Si4AlO 18 The chain silicate family includes ground silicate minerals such as, but not limited to, wollastonite and Ca[SiO3].
[0057] Suitable layered silicates, for example silicate minerals that can be utilized include: mica, KAl 14 [Si6Al2O 20 ](OH)4;phyllite;Al4[Si8O 20 ](OH)4;Talc;Mg6[SiO 20 ](OH)4; serpentine, e.g. asbestos; kaolinite; Al4[Si4O 10
[0033] (OH)8; and vermiculite. When present, non-reinforcing fillers are present in a cumulative amount of from 1 to 50% by weight of the composition.
[0058] In any case deemed necessary, the non-reinforcing silica filler can also be treated as described above for the reinforcing silica filler (ii) to make it hydrophobic, thereby making it easier to handle and obtain a homogeneous mixture with other components. As in the case of the reinforcing silica filler (ii), the surface treatment of the non-reinforcing silica filler can make it easier to wet the organopolysiloxane polymer (i) and, if present, the silicon-free organic particulate (v), resulting in improved properties of the hydrosilylation curable silicone elastomer composition, such as better processability (e.g., lower viscosity, better mold release ability, and / or less adhesion to processing equipment such as a two-roll mill), heat resistance, and mechanical properties.
[0059] Any suitable antioxidant, antistatic agent, stain repellent, and / or light stabilizer may be utilized in the composition.
[0060] Preferably, the conductive additive that can be used herein is inorganic. Examples of conductive fillers that can be present in the composition include metal particles, metal oxide particles, metal-coated metal particles (such as silver-plated nickel), metal-coated non-metal core particles (such as silver-coated talc or mica or quartz), and combinations thereof. Metal particles can be in the form of powder, flakes or filaments, and mixtures or derivatives thereof.
[0061] A pot-time extender, such as a triazole, may be used but is not considered essential within the scope of the present invention, and thus the hydrosilylation-curable silicone elastomer composition may be free of a pot-time extender.
[0062] In the case of lubricants, the lubricants may be reactive or non-reactive with other components of the composition. These may include organopolysiloxanes having a similar basic structure as component (i) but with only one unsaturated group, e.g., one alkenyl group, per molecule. Alternatively, the lubricants may be organic waxes, etc. If reactive, the wax may be, for example, an alkenylated wax having 15-30 carbons per molecule, or 15-30 carbons per molecule, with at least one alkenylated group, e.g., a vinyl group, per molecule.
[0063] If desired, non-reactive lubricants may be present in the composition and may include, but are not limited to, boron nitride, graphite, molybdenum sulfide, and the like, or mixtures thereof.
[0064] Examples of flame retardants include aluminum trihydrate, magnesium hydroxide, calcium carbonate, zinc borate, wollastonite, mica and chlorinated paraffins, hexabromocyclododecane, triphenyl phosphate, dimethyl methylphosphonate, tris(2,3-dibromopropyl)phosphate (tris)brominated, and mixtures or derivatives thereof.
[0065] Examples of pigments include carbon black, iron oxide, titanium dioxide, chromium oxide, bismuth vanadium oxide, and mixtures or derivatives thereof.
[0066] Examples of colorants include vat dyes, reactive dyes, acid dyes, mordant dyes, disperse dyes, cationic dyes, and mixtures thereof.
[0067] When optional additives may be used for more than one reason, e.g., as a non-reinforcing silica filler and as a flame retardant, they can function in both roles when present. When or if present, the aforementioned additional components are present in an amount, cumulatively, of 0.1 to 30 weight percent, alternatively 0.1 to 20 weight percent of the composition.
[0068] To prevent premature curing during storage, the composition is stored in two parts, Part A and Part B, before use. Typically, Part A contains the organopolysiloxane polymer (i) and a portion of the reinforcing silica filler (ii), as well as the hydrosilylation catalyst (iv), and Part B contains the remaining organopolysiloxane polymer (i) and reinforcing silica filler (ii) together with the component organohydrogenpolysiloxane (iii), and usually, if present, an inhibitor, although this may vary depending on the selection of inhibitor used. The two-part composition may be designed to be mixed together in any suitable ratio depending on the amount of organopolysiloxane polymer (i) and reinforcing silica filler (ii) in Part B, and thus may be mixed in a weight ratio of Part A:Part B of 15:1 to 1:2, but preferably in a weight ratio of Part A:Part B of 2:1 to 1:2, alternatively 1.5:1 to 1:1.5, alternatively 1:1.
[0069] Optional additives may be introduced into either the Part A or Part B silicone elastomer composition as desired, so long as they do not cause adverse effects on any of the other components of the respective parts.
[0070] The individual parts of the hydrosilylation curable silicone elastomer composition used in the leather coating composition can be prepared in any suitable manner. Any mixing technique and device described in the prior art can be used for this purpose. The specific device used is determined by the viscosity of the components and the final curable coating composition. Suitable mixers include, but are not limited to, paddle-type mixers, such as planetary mixers, or kneader-type mixers. It may be desirable to cool the components during mixing to avoid premature curing of the composition.
[0071] As previously discussed, component (ii) the reinforcing silica filler may be introduced into the composition in the form of a fumed silica masterbatch used to introduce fumed silica into either Part A or Part B of the composition, which may contain 25-45% by weight of fumed silica and 55-75% by weight of an organopolysiloxane containing at least two alkenyl and / or alkynyl groups per molecule. The organopolysiloxane may be component (i) above, and / or an organopolysiloxane in the same viscosity range as component (i), but having an alkenyl and / or alkynyl content of <5% by weight of the polymer. In one embodiment, the organopolysiloxane containing at least two alkenyl and / or alkynyl groups per molecule in the fumed silica masterbatch is a dimethylvinyl terminated polydimethylsiloxane having a viscosity of 30,000 to 80,000 mPa.s at 25° C. and a vinyl content of 0.05 to 0.2% by weight of the polymer, alternatively 0.05 to 0.15% by weight of the polymer, as determined using quantitative infrared analysis according to ASTM E 168. Such a masterbatch may contain only fumed silica and polymer, but may optionally contain small amounts of other components such as hexamethyldisilazane (HMDZ), divinyltetramethyldisiloxane, dimethylhydroxy terminated methylvinylsiloxane polymers, and / or water, having a viscosity of 10 to 100 mPa.s and a vinyl content of 5 to 20% by weight of the polymer, alternatively 7.5 to 15% by weight of the polymer, as determined using quantitative infrared analysis according to ASTM E 168.
[0072] Thus, when Part A and Part B are mixed together, the hydrosilylation-curable silicone elastomer composition may comprise:
[0073] Component (i) one or more organopolysiloxane polymers, wherein at least 5% by weight of the polymer per molecule, alternatively 5-15% by weight of the polymer per molecule, alternatively 6-15% by weight of the polymer per molecule, alternatively 7-15% by weight of the polymer per molecule, are alkenyl groups, alkynyl groups, or mixtures thereof, in an amount from 3% by weight of the composition, alternatively 10% by weight of the composition up to 50% by weight of the composition, alternatively 45% by weight of the composition. and wherein the unsaturated group is selected from the group consisting of, and having a viscosity of from 1000 to 500,000 mPa.s at 25° C., alternatively from 1000 to 150,000 mPa.s at 25° C., alternatively from 2000 to 125,000 mPa.s at 25° C., alternatively from 2000 to 100,000 mPa.s at 25° C., alternatively from 5000 to 80,000 mPa.s measured at 25° C. For example, organopolysiloxane polymer (i) may be present in the range of 10 to 50% by weight of the composition, alternatively from 10 to 45% by weight.
[0074] Component (ii) a reinforcing silica filler, preferably hydrophobically treated, which may be introduced directly into the composition or in the form of a masterbatch, and which has a BET surface area of generally at least 50 m 2 / g (BET method according to ISO 9277:2010). The filler has a viscosity of 50-450m 2 / g (BET method according to ISO 9277:2010) or 50-300m 2 / g surface area, and the amount of reinforcing silica filler (ii), e.g., finely divided silica, in the hydrosilylation curable silicone elastomer composition herein is 5 to 40 wt%, alternatively 5 to 30 wt%. In some cases, the amount of reinforcing silica filler may be 7.5 to 30 wt% of the composition, alternatively 10 to 30 wt% of the composition, alternatively 15 to 30 wt% of the composition, and when in the form of a masterbatch, the masterbatch may comprise 25 to 45 wt% fumed silica, 55 to 75 wt% of component (i), and / or a dimethylvinyl terminated polydimethylsiloxane having a viscosity of 50,000 to 80,000 mPa at 25°C and a vinyl content of 0.05 to 0.2 wt% of the polymer, alternatively 0.05 to 0.15 wt% of the polymer, alternatively 55 to 75 wt% of a dimethylvinyl terminated polydimethylsiloxane as described above. The masterbatch composition may also initially include a treating agent to treat the filler in situ to render it hydrophobic and thereby more easily blended with the polymer.
[0075] Component (iii), a silicone resin crosslinker, present in the total composition in an amount from 10 to 30% by weight of the Part B composition, alternatively from 10 to 20% by weight, alternatively from 12 to 20% by weight of the Part B composition, the amount present typically being determined by the molar ratio of silicon-bonded hydrogen atoms of component (iii) to the total number of all unsaturated groups, from 0.5:1 to 20:1, alternatively from 0.5:1 to 10:1, alternatively from 0.5:1 to 5:1, alternatively from 1:1 to 5:1, and preferably with an excess of Si-H and having end groups containing at least 5,000 parts per million (ppm) silicon-bonded hydrogen (Si-H), alternatively at least 7000 ppm, alternatively from 7000 to 12,000 ppm silicon-bonded hydrogen, alternatively from 8000 ppm to 11,000 ppm silicon-bonded hydrogen. The viscosity of component (iii) is from 15 to 50 mPa.s at 25°C, alternatively from 15 to 40 mPa.s at 25°C, alternatively from 20 to 35 mPa.s at 25°C.
[0076] The amount of catalyst present provided by component (iv) a hydrosilylation catalyst composition is in the range of 0.01 to 3.0% by weight of the composition, alternatively 0.1 to 3.0% by weight of the composition, alternatively 0.1 to 2.0% of the composition, alternatively 0.1 to 1.5% of the composition, and contains 0.01 ppm to 10,000 ppm, alternatively 0.01 to 7,500 ppm, alternatively 0.01 to 3,000 ppm, alternatively 100 to 6,000 ppm, by weight of platinum group metal, based on the combined weight of components (i) and (ii) and, if present, (v); Component (v) is a silicon-free inorganic particulate having a number average particle size (determined by the method described above, as appropriate) of 0.5 to 500 μm, alternatively 0.5 to 250 μm, alternatively 0.5 to 100 μm, alternatively 0.5 to 75 μm, alternatively 1.0 to 50 μm, and is thermally stable (determined using the method described above) to a temperature of at least 180° C. Component (v) is present in the composition in an amount of 5 to 35% by weight of the composition, alternatively 5 to 30% by weight of the composition, alternatively 5 to 25% by weight of the composition.
[0077] The total weight percent of the composition including components (i)-(v) and any optional additives is 100 weight percent, but may be any suitable combination of the above.
[0078] The order of mixing the components in the hydrosilylation curable silicone elastomer composition of the leather coating composition is not important.Prepare the appropriate part A and part B, then mix part A and part B together in a predetermined ratio of 15:1 to 1:2, for example, 1:1 ratio just before use.
[0079] Curing of the hydrosilylation-curable silicone elastomer composition of the leather coating composition can be carried out at a temperature suitable for hydrosilylation curing, such as a cure temperature of about 80°C to 180°C, alternatively 80°C to 150°C, alternatively 80°C to 130°C.
[0080] The leather coating composition described above provides excellent abrasion and scratch resistance protection after curing, and is therefore utilized as a topcoat for synthetic leather materials, particularly silicone-based synthetic leather composites. The leather coating composition can also be applied to various other types of leather, such as conventional leather, nubuck, or suede. As mentioned above, the leather coating composition may be applied to finished leather or during the final wet stage in leather finishing, but is preferably used as a topcoat for synthetic leather, particularly silicone-based synthetic leather composites. Leather with a topcoat in the form of a reaction product from the curing of the leather coating composition described above has significantly improved abrasion resistance. This improvement in abrasion resistance is achieved without compromising the compatibility and flexibility of the final coating, and other additives often used to improve abrasion resistance can make the coated leather rough to the touch and improve resistance to bending, which can cause cracks in the structure of the coating. [Brief description of the drawings]
[0081] The application and use of the above-described leather coating composition will become more apparent from the following further description taken in conjunction with the accompanying drawing figures 1-4, which are cross-sectional views showing the layers in the structure of a silicone-based synthetic leather composite during and after manufacture.
[0082] A detailed description of a method for making a silicone-based synthetic leather composite using the aforementioned hydrosilylation-curable silicone elastomer composition in conjunction with the aforementioned figures.
[0083] A silicone-based synthetic leather composite comprising a coating that is a reaction product from the curing of the aforementioned leather coating composition (5) may comprise several layers (3, 4) of cured liquid silicone rubber, each having a different function, as well as a textile support layer (2). Except for the topcoat made from the leather coating composition described herein, the silicone-based synthetic leather composite comprises at least a textile support layer (2), an adhesive layer (3) made from a first liquid silicone rubber material, and a second or skin layer (4) made from a second liquid silicone rubber material. The adhesive layer (3) is provided between the textile support layer (2) and the second (skin) layer (4) as an effective adhesive. In use, the adhesive layer or first layer (3) is adhered to the textile support layer (2) and adhered or laminated to the skin layer (4). The aforementioned leather coating composition functions as a protective topcoat (5), which is a third layer that overlies and is bonded to the skin layer (4), i.e., the second layer (4) is located between the adhesive layer (3) and the topcoat layer (5).
[0084] Typically, a release liner (1) is provided to protect the outer surface of the silicone-based synthetic leather composite until it is needed. Depending on the process relied upon to make the silicone-based synthetic leather composite, the release liner (1) may be included in the initial layer combination adhered to a skin layer (4) or a topcoat (5), depending on the preferred process. In the former case, the release liner (1) may be removed before applying the topcoat. In the latter case, the topcoat is applied onto the skin before applying the release liner onto the topcoat, or the topcoat is first applied onto the release liner before applying additional layers.
[0085] The textile support layer (2) can be made of any suitable textile material, such as woven, knitted textile, or nonwoven fabrics made from synthetic resin fibers, natural fibers, and / or microfibers. These can include, but are not limited to, polyester fibers, viscose rayon fibers, polyamide fibers, nylon, acrylic fibers, polyolefin fibers, cellulose fibers such as cotton, and elastic textile materials such as spandex, which may be used as a mixture of any two or more of the above. The textile support layer is designed to improve the mechanical strength of the silicone leather.
[0086] The leather coating composition (i.e., topcoat layer (5)) is typically applied at a wet film thickness of 10 to 100 μm, alternatively 10 to 60 μm, corresponding to a dry coating thickness of about 2 to 50 μm, alternatively 2 to 30 μm, alternatively 5 to 25 μm. It may be cured at any suitable temperature, for example, about 80° C. to 180° C., alternatively 80° C. to 160° C., alternatively 80° C. to 130° C., for a suitable period of time, for example, 30 seconds to 20 minutes, alternatively 30 seconds to 10 minutes, alternatively 30 seconds to 5 minutes, alternatively 30 seconds to 2.5 minutes.
[0087] Any suitable liquid silicone rubber composition may be utilized as the adhesive layer or first layer (3), which will be capable of adhering to the textile support layer (2) and will typically have a low durometer Shore A hardness, for example 20-40, and a soft feel when touched, once cured. A commercial example of a suitable hydrosilylation curable liquid silicone rubber composition designed to function as the adhesive layer (3) is Dowsil™ LCF 8400 Binder, manufactured by Dow Silicones Corporation. Dowsil™ LCF 8400 Binder remains the standard for hydrosilylation curable compositions to avoid premature curing, and is provided to consumers in a two-part form, so that the two parts of Dowsil™ LCF 8400 Binder are mixed together immediately prior to use.
[0088] The adhesive layer (3) may be of any desired dry thickness, for example, from 50 μm to 1 mm, alternatively from 50 to 750 μm, alternatively from 50 to 500 μm, alternatively from 100 to 500 μm, alternatively from 100 to 300 μm, and may be cured at any suitable temperature, for example from 125 to 180° C., alternatively from 130 to 170° C., alternatively from 135 to 160° C., for a suitable period of up to 20 minutes, alternatively from 1 to 10 minutes, alternatively from 1.5 to 5 minutes, alternatively from 1.5 to 4 minutes.
[0089] As previously indicated, the first or adhesive layer (3) is designed to be sandwiched between and adhered to the textile support layer (2) and the second or skin coating layer (4).
[0090] The second or skin coating composition (4) mentioned above is usually designed as a protective synthetic leather that is bonded to the adhesive layer (3). It can be used alone or with a suitable topcoat (5) such as those described herein. Any suitable liquid silicone rubber composition can be utilized to form the second or skin layer (4), which typically has a higher durometer Shore A hardness, such as (≧) 50 or more, or (≧) 60 or more, after curing, than the first or adhesive layer (3). Commercial examples of suitable liquid silicone rubber compositions that can be cured to function as the second or skin layer (4) are Dowsil® LCF 8300 Skin and Dowsil® LCF 8500 Skin, both from Dow Silicones Corporation, which are both hydrosilylation curable liquid silicone rubber compositions, and are similarly provided to users in two parts that are mixed together immediately before use to avoid premature curing during storage before use. Dowsil™ LCF 8300 Skin has a high Shore A durometer value of about 65, provides abrasion resistance, and has a relatively low viscosity compared to Dowsil™ LCF 8500 Skin. The latter is a fumed silica reinforced version of the former with high mechanical strength, and therefore has a much higher viscosity. Often, a mixture of Dowsil™ LCF 8300 Skin and Dowsil™ LCF 8500 Skin is used as the second or skin layer (4) to benefit from the advantages of both compositions.
[0091] The skin layer (4) may be of any suitable dry thickness, for example the adhesive layer may be of any desired thickness, for example from 50 μm to 1 mm thick, from 50 to 750 μm, alternatively from 50 to 500 μm, alternatively from 50 to 350 μm, alternatively from 50 to 250 μm thick. Where the skin layer was applied directly onto the release paper and the average thickness of the skin layer was determined, this was determined by measuring the length and width of a sample of the release paper, coating the release paper with the skin layer composition in this case, curing it, weighing the resulting coated release paper, and calculating the average thickness based on the following formula:
[0092] Average dry thickness of skin layer = weight of skin layer / (density x width x length) Where indicated, the average dry coat thickness of each of the other layers was similarly determined by determining the weight of each layer and using the formula above. In each case, density was determined in accordance with ASTM D792. The skin layer may be cured at any suitable temperature, for example, from about 100° C. to 150° C., alternatively from 110° C. to 135° C., alternatively from 110° C. to 125° C., for a period of time from 30 seconds to 5 minutes, alternatively from 30 seconds to 2.5 minutes.
[0093] If desired, the final silicone leather article may be post-cured at a temperature of about 75°C to 180°C, generally, but not necessarily, towards the lower end of the range if desired, e.g., 75 to 120°C, for 2 to 48 hours, alternatively 6 to 36 hours, alternatively 10 to 24 hours.
[0094] The aforementioned leather coating composition may be applied as a topcoat by any suitable coating method, such as spraying, rolling, brushing, spin coating, dip coating, solution casting, slot die coating, spray coating, knife coating, or gravure coating, onto a preformed silicone-based synthetic leather composite, such as (2, 3, 4), as shown in Figure 2. The adhesive layer (3) and skin layer (4) may be applied via the same means.
[0095] The fabric layer may be attached to the adhesive layer in any suitable manner, for example, by lamination.
[0096] In such circumstances, preformed silicone-based synthetic leather composites have typically been prepared by several alternative processes. (i) applying a liquid silicone rubber skin-type composition (4) onto a release liner (1); (ii) curing the skin layer composition of (i) on the release liner (1) to form a cured skin layer (4); (iii) applying a silicone adhesive composition onto the cured skin layer (4); (iv) placing the textile support layer (2) on the adhesive layer (3) before or during curing of the adhesive layer (3) such that the adhesive layer (3) is sandwiched between the skin layer (4) and the textile support layer (2); (v) curing the adhesive layer (3); and (vi) Removing the release liner (1) if necessary. The above is shown in Figures 1 and 2, which show a silicone-based synthetic leather composite with (Figure 1) and without (Figure 2) a release liner. In the case of Figure 2, the silicone-based synthetic leather composite has been prepared and is now ready for applying a topcoat as described above over the skin layer (4) by any suitable application means as described above (e.g., spraying, rolling, brushing, spin coating, dip coating, solvent casting, slot die coating, spray coating, knife coating, or gravure coating).
[0097] The leather coating composition described above is then applied onto the surface of the skin layer (4) from which the release liner (1) has been removed, and cured to form a protective topcoat on the silicone-based synthetic leather composite.
[0098] In an alternative embodiment, the silicone-based synthetic leather composite may be prepared in a continuous process with a topcoat using the aforementioned leather coating composition in a continuous process. In this case, the following process may be: (i) applying the aforementioned leather coating composition onto a release liner (1); (ii) curing said leather coating composition on the release liner (1) to form a cured topcoat (5); (iii) applying a silicone skin layer over the cured topcoat (5); (iv) curing the silicone skin layer to form a cured skin layer (4) such that the cured topcoat layer (5) is sandwiched between the release liner (1) and the cured skin layer (4); (v) applying a silicone adhesive composition onto the cured skin layer (4); (vi) placing or laminating a textile support layer (2) onto the uncured or cured adhesive layer (3) and preferably operatively laminating said textile support layer to said adhesive layer; (vii) curing the adhesive layer (3) such that the cured adhesive layer (3) is sandwiched between the skin layer (4) and the textile support layer (2); (viii) removing the release liner (1) if necessary;
[0099] The different layers of such a process are shown in Figures 3 and 4, where Figure 3 shows the release liner (1) present and Figure 4 shows the final silicone-based synthetic leather composite with the release liner removed.
[0100] Any suitable release liner may be used, such as the ultra-matt release paper ARX175DM from Asahi, the release papers DE-7, DE-90, DE-43C, DE-73J from Japan Dai Nippon Printing, or the semi-matt release paper DE-73M, also from Dai Nippon Printing. Each curing step may be carried out by curing and drying in a suitable oven, such as a hot air oven, or in the case of a continuous process in a conveyor oven.
[0101] The above process shows the preparation of a silicone-based synthetic leather composite material. The reader can understand that it will become necessary to introduce additional layers into the material if desired.
[0102] Synthetic leather, especially silicone-based synthetic leather composites, can be designed to have a wide variety of properties considering the contents of different layers, such as excellent flame retardancy, smoke density, heat resistance, stain resistance, solvent resistance, hydrolysis resistance, etc., depending on the end use requirements of the leather. Contemplated end uses include, but are not limited to, furniture, decoration, handbags, binders, luggage, clothing, phone covers, covers for electronic goods, book covers, footwear, automotive interiors, automotive seats, wearable devices, and / or medical beds / sheets. EXAMPLES
[0103] In the following examples, hydrosilylation curable silicone elastomer compositions forming leather coating compositions and some comparative examples were tested to show the benefits of the coatings described herein in terms of maintaining gloss after abrasion. All viscosities are measured at 25°C using a Brookfield® rotational viscometer with spindle LV-4 (designed for viscosities in the range of 1,000 to 2,000,000 mPa.s) or a Brookfield® rotational viscometer with spindle LV-1 (designed for viscosities in the range of 15 to 20,000 mPa.s) at a rotation speed of 10 rpm, according to the cup / spindle method of ASTM D1084-16 Method B, unless otherwise specified.
[0104] Alkyl and / or alkynyl content and Si-H content were determined using quantitative infrared analysis according to ASTM E168.
[0105] The ingredients used in the leather coating composition are defined below, as used with the names given in the tables / examples below: The vinyl-terminated siloxane polymer is a dimethylvinyl-terminated polydimethylsiloxane having a vinyl content of about 0.08% by weight, with a viscosity of 65,000 mPa.s at 25° C. The high vinyl siloxane polymer is a dimethylvinyl terminated dimethylmethylvinyl polysiloxane copolymer having a viscosity of 15,000 mPa.s at 25° C. and a vinyl content of about 8.0% by weight; Vinyl-terminated siloxane copolymer 2 is a dimethylvinyl-terminated dimethylmethylvinyl polysiloxane copolymer having a viscosity of 300 mPa.s at 25° C. and a vinyl content of about 1.15% by weight; Fumed silica is 300m 2 HDK® T30P pyrogenic silica (Wacker Chimie) with a BET surface area of 1.0 g / g; HMDZ is hexamethyldisilazane; MVD (methyl vinyl diol) is a dimethylhydroxy terminated polydimethylmethylvinyl siloxane having a viscosity of about 30 mPa.s at 25° C. and a vinyl content of about 12.0% by weight; the platinum catalyst being a platinum catalyst in a solution of polydimethylsiloxane having about 5000 ppm platinum metal relative to the remainder of the composition; The inhibitor is methyl(tris(1,1-dimethyl-2-propynyloxy))silane; The silicone elastomer powder was Dowsil® 23N Additive (Dow Silicones Corporation); The resinous Si-H crosslinker is a Si-H dimethyl terminated resinous Si-H polysiloxane having a viscosity of 25 mPa.s at 25° C. and a silicon-bonded hydrogen content of about 9,000 ppm; The polyurethane microparticles are RHU-5070D polyurethane microparticles manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., with an average particle size of 1 to 10 μm (source information). Acrylic microparticles 1 are Chemisnow (registered trademark) MZ-5HN manufactured by Soken Chemical & Engineering Co., Ltd., with an average particle size of 1 to 10 μm (supplier information); The acrylic microparticles 2 are Chemisnow® MX-40T by Soken Chemical & Engineering, with an average particle size of about 0.4 μm (supplier information); The lubricant is a C24-28 olefin manufactured by Nanjing Chemical Material Corp.
[0106] Table 1 provides details of the starting materials used for a silica masterbatch of the following composition: The fumed silica was mixed with a vinyl terminated siloxane polymer in the presence of a small molecule that acts as a hydrophobizing agent for the silica, treating the silica in situ while the silica and polymer were mixed. As indicated previously, the polymer used can be component (i), or a mixture of component (i) with another polymer if desired, in which case component (i) is not present in the masterbatch.
[0107] [Table 1]
[0108] Several LSR compositions were prepared as examples (Examples 1-4) and comparative examples (Comparative Examples 1-5) using two-part compositions. The total composition of each composition after mixing Part A and Part B is shown in Table 2a (Examples) and Table 3a (Comparative Examples).
[0109] Prior to mixing, the Part A composition incorporated the following: High vinyl siloxane copolymers, Part of the master batch, platinum catalyst, the lubricant (if present) and a portion of the particulate and diluent (if present), the diluent being designed to evaporate during the curing process.
[0110] The Part B composition incorporated the following: The remainder of the masterbatch, Resinous SiH crosslinker, The inhibitor, if present, and the remainder of the microparticles and any diluents present.
[0111] Diluents: Diluents are designed to evaporate during the curing process.
[0112] Immediately prior to use, the Part A composition and its respective Part B composition were mixed together in a 1:1 weight ratio to produce the final hydrosilylation-curable silicone elastomer composition under test.
[0113] [Table 2]
[0114] Once prepared, the topcoat composition was utilized in the preparation of a silicone-based synthetic leather composite through the following process: the skin layer (4) used was a mixture of Dowsil® LCF 8300 Skin and Dowsil® LCF 8500 Skin, and the adhesive layer (3) was in the form of Dowsil® LCF 8400 Binder, which was subjected to a lamination bonding process to a microfiber-based textile layer (2) before curing, and then the combination was cured at a temperature of 150° C. for 3 minutes. 1) The topcoat mixture was applied onto a release liner and cured for 1.4 minutes (min) at a temperature of 120° C. The dry film thickness was determined to be approximately ∼10 μm. 2) The skin layer was then applied onto the topcoat and cured under the same conditions. The thickness of the adhesive layer was 100-150 μm. 3) An adhesive layer was applied on top of the skin layer and the fabric was attached using a lamination bonding process. The combination was then cured at 150°C for 3 minutes, resulting in an adhesive layer thickness of 150-250μm. 4) The release liner was then removed to obtain the top-coated silicone leather sample; 5) Finally, the silicone leather material was post-cured at a temperature of 80°C for 16-20 hours.
[0115] The resulting silicone leather was then analyzed using the Taber Scratch Test, which used a TABER® Abraser (Abrader) model 5131 for testing. The Taber Scratch Test is used to evaluate the abrasion resistance performance of leather samples. Three samples of each example or comparative example were subjected to 500 cycles of rubbing using a CS-10 wheel and a 1 kg weight. After the rubbing process, the rubbed surface was washed with deionized water and air-dried before evaluation. Each sample was then visually evaluated, and any undesirable changes in gloss, color, or texture were recorded. To pass the test, there must be substantially no wear of the coating or any undesirable changes in gloss, color, or grain.
[0116] Results for examples having a topcoat according to the present disclosure are provided in Table 2b.
[0117] [Table 3]
[0118] (SC) indicates slight change.
[0119] It is believed that the high crosslink density due to the nature of the polymer and crosslinker limits chain mobility, thus minimizing adhesive contact. As a result, wear patterns are avoided, and gloss does not decrease after abrasion. Meanwhile, fine particles in the topcoat appear on the surface after abrasion. As a result, small grains are worn off, but the fine particles that appear help to compensate for the loss of surface roughness, thus avoiding gloss increase.
[0120] Similar tests were then carried out on silicone leather topcoated with the comparative composition using the same process and test methods as above. The composition for the topcoat is shown in Table 3a and the results are shown in Table 3b.
[0121] [Table 4]
[0122] [Table 5]
[0123] SDG represents the noticeable decrease in gloss and ΔGrey value represents the change in grey value.
[0124] Examples 1, 2, and 3 passed the Taber test with no obvious change in gloss. Comparative Examples 1, 3, 4, and 5 failed due to a significant decrease in gloss, while Comparative Example 2 failed due to a significant increase in gloss. Comparative Example 5 shows that the particle size of the microparticles must be at least 5 μm. Comparative Example 1 uses vinyl-terminated siloxane copolymer 2 instead of the high vinyl siloxane copolymer used in the examples. The elastomer obtained by curing Comparative Example 1 has a lower crosslink density, and therefore, in view of the results in Table 3b, it can be seen that the high vinyl siloxane copolymer is essential. The present invention includes the following embodiments. [1] A leather coating composition comprising a hydrosilylation-curable silicone elastomer composition, Component (i) one or more organopolysiloxane polymers having a viscosity of 1000 to 500,000 mPa.s at 25° C., wherein at least 5% by weight of said polymer are unsaturated groups selected from alkenyl groups, alkynyl groups, or mixtures thereof, as determined using quantitative infrared analysis in accordance with ASTM E168; Component (ii) a reinforcing silica filler which may be optionally hydrophobically treated; and component (iii) a silicone resin crosslinker having terminal (M) groups containing silicone-bonded hydrogen, wherein the molar ratio of Si-H groups in component (iii) to unsaturated groups in said composition is from 0.5:1 to 20:1; Component (iv) a hydrosilylation catalyst; and Component (v) silicon-free inorganic particles having a number average particle size of 0.5 to 500 μm as determined using a field emission scanning electron microscope, which are thermally stable up to a temperature of at least 180° C. using the test method disclosed herein, and which are present in the leather coating composition in an amount of 5 to 35% by weight; A composition comprising: [2] The hydrosilylation-curable silicone elastomer composition, wherein component (iii) is one of the following: M groups containing Si-H, (CH 3 ) 3 SiO 1 / 2 Group, and SiO 4 / 2 a silicone resin comprising or consisting of a group; Si-H containing M groups and SiO 4 / 2 a silicone resin comprising or consisting of a group; M groups containing Si-H, (CH 3 ) 2 SiO 2 / 2 Group, and SiO 4 / 2 a silicone resin comprising or consisting of a group; M group containing Si-H, SiO4 / 2 Groups, and (C 6 H 5 ) 3 SiO 1 / 2 Silicone resins containing or consisting of groups, as well as alternatives in which the methyl is replaced with a phenyl group or other alkyl group or mixtures thereof; The leather coating composition according to [1] above, comprising one or more of the following, each of which may comprise one or more T groups: [3] The leather coating composition according to [1] or [2], wherein the silicon-free organic fine particles of component (v) of the hydrosilylation-curable silicone elastomer composition are selected from polyurethane fine particles, acrylic fine particles, methacrylic fine particles, polytetrafluoroethylene fine particles, polyester fine particles, polyamide fine particles, polyolefin fine particles, and derivatives and / or mixtures thereof. [4] The leather coating composition according to [1] or [2], wherein the silicon-free organic particulate of component (v) of the hydrosilylation-curable silicone elastomer composition includes, but is not limited to, one or more of polyethylene, polystyrene, polyvinyl acetate, polyvinyl chloride, polyvinylidene chloride, polyacrylonitrile, polymethyl methacrylate, polybutadiene, polychloroprene, and other vinyl polymers and copolymers thereof; polyamides such as nylon 6, nylon 66; and polyethylene terephthalate, polyacetal, and blends thereof. [5] The leather coating composition according to any one of the above [1] to [4], further comprising one or more of the following additives: a cure inhibitor, a cured silicone elastomer powder, a pot life extender, a lubricant, a diluent, a flame retardant, a pigment, a colorant, a heat stabilizer, a compression set improving additive, an anti-squeak agent, and mixtures thereof. [6] The leather coating composition according to [5], wherein, when present, the lubricant is a reactive lubricant. [7] The leather coating composition according to any one of [1] to [6], wherein the silicon-free organic fine particles have a number average particle size of 0.5 to 100 μm as determined using a field emission scanning electron microscope. [8] The leather coating composition according to any one of the above [1] to [7], which is a top coat composition for a silicone-based synthetic leather composite material. [9] A silicone-based synthetic leather composite material comprising a top coat which is a reaction product of the composition described in any one of [1] to [8] above obtained upon curing.
[10] The silicone-based synthetic leather composite material according to [9], further comprising a textile support layer selected from one or more of polyester fibers, viscose rayon fibers, polyamide fibers, nylon, acrylic fibers, polyolefin fibers, cellulose fibers, and elastic textile materials.
[11] A method for preparing a silicone-based synthetic leather composite material having a top coat which is a cured product of the leather coating composition according to any one of the above [1] to [8], comprising the following steps: (i) applying said leather coating composition onto a release liner; (ii) curing the leather coating composition on the release liner to form a cured topcoat; (iii) applying a silicone skin layer over the cured topcoat; (iv) curing the silicone skin layer to form a cured skin layer such that the cured topcoat layer is sandwiched between the release liner and the cured skin layer; (v) applying a silicone adhesive composition onto the cured skin layer; (iv) placing the textile support layer on the adhesive layer such that the adhesive layer is sandwiched between the skin layer and the textile support layer, preferably such that the textile support layer is operatively laminated to the adhesive layer; (vii) curing the adhesive layer; (viii) optionally removing the release liner; Method by.
[12] A method of applying a silicone-based synthetic leather composite having a topcoat comprising or consisting of the leather coating composition according to
[11] above, wherein the leather coating composition is applied at a wet film thickness of 10-100 μm and dries to a corresponding dry coating thickness of about 2-50 μm.
[13] A method of applying the topcoat according to
[11] or
[12] to a silicone-based synthetic leather composite by one or more means selected from spraying, rolling, brushing, spin coating, dip coating, solvent casting, slot-die coating, spray coating, knife coating, or gravure coating.
[14] Use of the silicone-based synthetic leather composite material according to [9] or
[10] in or for furniture, decoration, handbags, binders, luggage, clothing, phone covers, covers for electronic goods, book covers, footwear, automobile interiors, automobile seats, wearable devices, and / or medical beds / sheets.
[15] Use of the leather coating composition according to any one of [1] to [8] above as a topcoat for synthetic leather to minimize gloss change after curing and abrasion.
Claims
1. 1. A leather coating composition comprising a hydrosilylation-curable silicone elastomer composition, comprising: Component (i) one or more organopolysiloxane polymers having a viscosity of 1000 to 500,000 mPa.s at 25°C, wherein at least 5% by weight of said polymer are unsaturated groups selected from alkenyl groups, alkynyl groups, or mixtures thereof, as determined using quantitative infrared analysis in accordance with ASTM E168; Component (ii) a reinforcing silica filler, optionally hydrophobically treated, present in said leather coating composition in an amount of 7.5 to 30% by weight; component (iii) a silicone resin crosslinker having terminal (M) groups containing silicone-bonded hydrogen, wherein the molar ratio of Si-H groups in component (iii) to unsaturated groups in said composition is from 0.5:1 to 20:1; Component (iv) a hydrosilylation catalyst; and Component (v) a silicon-free inorganic particulate having a number average particle size of 0.5 to 500 μm as determined using a field emission scanning electron microscope, which is thermally stable up to a temperature of at least 180° C. using the test method disclosed herein, and which is present in said leather coating composition in an amount of 5 to 35% by weight, the silicon-free organic fine particles selected from polyurethane fine particles, acrylic fine particles, methacrylic fine particles, polytetrafluoroethylene fine particles, polyester fine particles, polyolefin fine particles, or mixtures thereof; A composition comprising:
2. Component (iii) of the hydrosilylation-curable silicone elastomer composition is M groups containing Si—H, (CH 3 ) 3 SiO 1/2 group, and SiO 4/2 a silicone resin comprising or consisting of a group; M groups containing Si-H and SiO 4/2 a silicone resin comprising or consisting of a group; M groups containing Si—H, (CH 3 ) 2 SiO 2/2 group, and SiO 4/2 a silicone resin comprising or consisting of a group; M group containing Si-H, SiO 4/2 Groups, and (C 6 H 5 ) 3 SiO 1/2 Silicone resins containing or consisting of groups, as well as alternatives in which the methyl is replaced with a phenyl group or other alkyl group or mixtures thereof; 10. The leather coating composition of claim 1, comprising one or more of:
3. 10. The leather coating composition of claim 1, further comprising one or more of the following additives: cure inhibitors, cured silicone elastomer powder, pot life extenders, lubricants, diluents, flame retardants, pigments, colorants, heat stabilizers, compression set improving additives, anti-squeak agents, and mixtures thereof.
4. 4. The leather coating composition of claim 3, wherein said lubricant, when present, is a reactive lubricant.
5. 3. The leather coating composition according to claim 1, wherein the silicon-free inorganic fine particles have a number average particle size of 0.5 to 100 μm as determined using a field emission scanning electron microscope.
6. 3. The leather coating composition according to claim 1 or 2, which is a topcoat composition for a silicone-based synthetic leather composite material.
7. 3. A silicone-based synthetic leather composite comprising a topcoat which upon curing is the reaction product of the composition of claim 1 or 2.
8. 8. The silicone-based synthetic leather composite of claim 7, comprising a textile support layer selected from one or more of polyester fibers, viscose rayon fibers, polyamide fibers, nylon, acrylic fibers, polyolefin fibers, cellulose fibers, and elastic textile materials.
9. 10. A method for preparing a silicone-based synthetic leather composite having a topcoat that is a cured product of the leather coating composition of claim 1, comprising the steps of: (i) applying said leather coating composition onto a release liner; (ii) curing the leather coating composition on the release liner to form a cured topcoat; (iii) applying a silicone skin layer over the cured topcoat; (iv) curing the silicone skin layer to form a cured skin layer such that the cured topcoat layer is sandwiched between the release liner and the cured skin layer; (v) applying a silicone adhesive composition onto the cured skin layer; (iv) placing the textile support layer on the adhesive layer such that the adhesive layer is sandwiched between the skin layer and the textile support layer; (vii) curing the adhesive layer; (viii) optionally removing the release liner; Method by.
10. 10. A method of applying a silicone based synthetic leather composite having a topcoat comprising or consisting of the leather coating composition of claim 9, wherein the leather coating composition is applied at a wet film thickness of 10-100 μm and dries to a corresponding dry coating thickness of 2-50 μm.
11. 11. A method of applying the topcoat of claim 9 or 10 to a silicone-based synthetic leather composite by one or more of the means selected from spraying, rolling, brushing, spin coating, dip coating, solvent casting, slot die coating, spray coating, knife coating, or gravure coating.
12. Use of the silicone based synthetic leather composite material according to claim 7 or 8 in or for furniture, decoration, handbags, binders, luggage, clothing, phone covers, covers for electronic goods, book covers, footwear, car interiors, car seats, wearable devices, and / or medical beds / sheets.
13. 3. Use of the leather coating composition according to claim 1 or 2 as a topcoat for synthetic leather, once cured, to minimize gloss change after abrasion.
Citation Information
Patent Citations
Storageestable organosilicone compound
JP1977119659A
Room temperature curable organopolysiloxane composition
JP2004536920A
Wear-resistant multilayer composite materials
JP2023509654A