How Stainless Steel is Made

Applying a magnetic field during stainless steel cooling or hardening suppresses embrittlement, addressing spinodal decomposition and sigma phase issues, resulting in improved mechanical properties.

JP7574423B2Active Publication Date: 2024-10-28OUTOKUMPU OY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023518187
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-09
Filing Date
2021-10-08
Publication Date
2024-10-28
Estimated Expiration
2041-10-08

AI Technical Summary

Technical Problem

Existing stainless steel production methods fail to adequately suppress embrittlement during cooling and quenching, particularly in duplex and ferrite grades, leading to reduced mechanical properties due to spinodal decomposition and sigma phase formation.

Method used

Applying a magnetic field during the cooling or hardening process of stainless steel production to suppress embrittlement, using a magnetic field strength of at least 0.2T, preferably 1.5-3.0T, to prevent spinodal decomposition and sigma phase formation.

Benefits of technology

The application of a magnetic field significantly reduces spinodal decomposition and embrittlement, ensuring high-quality stainless steel products with improved impact toughness and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574423000002
    Figure 0007574423000002
  • Figure 0007574423000003
    Figure 0007574423000003
  • Figure 0007574423000004
    Figure 0007574423000004
Patent Text Reader

Abstract

1. A method for inhibiting embrittlement of stainless steel in a stainless steel production process, comprising: producing stainless steel in a conventional stainless steel production process; Annealing the stainless steel in an annealing step; - cooling the steel in a cooling step or quenching the steel in a quenching step; applying a magnetic field to the stainless steel during the cooling or quenching step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for inhibiting embrittlement of steels, in particular the method includes inhibiting embrittlement of duplex and ferritic grades by external magnetic fields. [Background technology]

[0002] The superior properties of stainless steels are due in part to the heat treatments performed during the final processing steps. In order for a stainless steel product to have the required properties, such as good corrosion resistance, formability and strength, for a long service life, the heat treatments performed need to be tightly controlled. Heat treatments improve these desired properties, but can also "sensitize" the part if not performed properly. The risk of sensitization generally increases as the stainless steel grades become more highly alloyed, i.e., higher Cr and Mo levels. For example, dwell times in the range of 700°C to 950°C must be avoided to prevent the formation of sigma phases and chromium carbides, both of which can reduce the corrosion resistance and mechanical properties of highly alloyed austenitic and duplex stainless steel grades. To avoid this, cooling after heat treatment is preferably performed by water quenching in a water bath or by water spraying, depending on the product form. Another temperature region to be avoided as much as possible for duplex stainless steels is between 250°C and 500°C. Within this temperature region, a phenomenon known as spinodal decomposition can occur.

[0003] Spinodal decomposition, often referred to as 475°C embrittlement, is a degradation of duplex materials that dramatically impairs toughness. At 475°C, for example, decomposition and embrittlement of the ferrite phase can occur in duplex and ferritic grades to the extent that impact toughness can decrease by 50% after a 3 minute hold at that temperature. At lower temperatures, 250-350°C, decomposition still occurs, but at a much slower rate, and up to tens of thousands of hours at that temperature are required to have the same level of adverse effect on properties.

[0004] More recently, it has been recognized that for thick gauge parts (such as quarto plate), some degree of spinodal decomposition may occur during cooling / quenching of the part after solution annealing. Cooling / quenching is most typically performed in a batch (or in-line bulk spray) in a water bath. However, even in a bath with high agitation of the water, the part may cool too slowly, resulting in undesirable material properties. Air-cooled parts, which cool more slowly than quenched parts, are even more susceptible to spinodal decomposition, as the material takes longer to cool through the critical temperature region. It is well established that highly alloyed duplex grades and ferritic systems may be susceptible to precipitation of undesirable phases such as sigma phase during cooling, but as mentioned above, the fact that spinodal decomposition may also play a significant role in property degradation during the cooling / quenching step is novel. Low alloyed duplex and ferritic grades that do not undergo sigma phase precipitation may still be susceptible to spinodal decomposition when quenched in water, although to a lesser extent. However, some low alloy grades, such as bars, can be air cooled to produce the as-rolled product. Because the cooling rate is relatively slow when cooling in air, the grades produced in this manner are susceptible to spinodal decomposition.

[0005] Japanese Patent Application No. 09217149A shows that 475°C embrittlement can occur during cooling of thick gauge castings with grain sizes larger than 50 μm. They teach that advanced cooling schedules are necessary to suppress sigma phase, 475°C embrittlement and induced stresses, including that the cooling rate needs to be higher than 10°C / min from 500°C to 300°C to limit 475°C embrittlement. However, such a cooling approach is not possible in an in-line quenching process and is not practical for industrial-scale batch annealing using large tanks for quenching. Furthermore, 10°C / min is still too slow to avoid spinodal decomposition in some materials, for example, in thick gauge materials with grain sizes most exceeding 50 μm. Due to material properties, the highest possible cooling rate at large plate thicknesses is not fast enough to fully suppress 475°C embrittlement.

[0006] JP 2006212674A describes how ferritic grades can suffer from brittleness due to 475°C embrittlement in hot rolled coils if not properly cooled during coiling. A solution is proposed by starting the coiling at a specific temperature so that the tip of the coil enters the mandrel just above the embrittlement temperature range and is then rapidly cooled during coiling by a mandrel with built-in cooling. However, this approach is practically impossible on e.g. plate material or bar. Nor is it possible in an in-line process where pickling is performed immediately after e.g. annealing.

[0007] China Patent No. 108315549A claims a method for removing age embrittlement in duplex stainless steel by subjecting aged duplex stainless steel to electric pulse treatment, characterized in that the parameters of the pulse treatment range as follows: frequency 1-200Hz, pulse width 20μs-1ms, current 10-2000A, function time 1-6h. The method is said to restore aged duplex stainless steel after long exposure to 475°C range, but does not prevent the occurrence of embrittlement during processing of the steel. Summary of the Invention

[0008] The inventors have recently found that 475°C embrittlement can even occur during the cooling / quenching step. It has been confirmed that the properties of materials subjected to 475°C embrittlement during cooling are somewhat degraded in terms of impact toughness, although not to the same extent as the above-mentioned isothermal aging at 475°C. However, in combination with the presence of sigma phases (which are also formed during the same cooling / quenching), the impact toughness can be further degraded below acceptable levels, thus limiting the thickness or quality of the material supplied. Suppressing this embrittlement is therefore essential to achieve high-standard products.

[0009] The invention is defined by what is disclosed in the independent claims. Preferred embodiments are set forth in the dependent claims.

[0010] It is an object of the present invention to overcome at least some of the shortcomings of the prior art and to provide a method for inhibiting embrittlement of stainless steels.

[0011] According to a first aspect of the present invention, there is provided a method of inhibiting embrittlement of stainless steel in a stainless steel production process, the method comprising the steps of producing stainless steel in a conventional stainless steel production process, annealing the stainless steel, cooling / quenching the steel, and applying a magnetic field to the steel, wherein the magnetic field is applied to the steel during the cooling or quenching step.

[0012] The present invention provides considerable advantages: It has surprisingly been found that the embrittlement of stainless steel can be inhibited, and therefore high quality stainless steel products can be provided.

[0013] Further features and advantages will become apparent from the following description. [Brief description of the drawings]

[0014] The invention will now be illustrated in more detail with reference to the accompanying drawings, in which: [Figure 1]1 shows different cooling curves obtained by using a GLEEBLE test apparatus. The GLEEBLE apparatus is generally used for thermomechanical testing of materials and to simulate physical processes such as industrial heat treatment and subsequent cooling. This apparatus is therefore ideal for simulating different cooling conditions related to the 475°C phenomenon. The specimen is heated to the desired annealing temperature, in this example 1100°C, and then controlled cooled to simulate cooling conditions typical for industrial production of square plates, bars, etc. In FIG. 1, a typical industrial cooling curve is shown in dashed lines, with an average cooling rate of 60°C / min throughout the entire cooling from 1100°C to below 100°C, and a rapid cooling curve is shown in solid lines, with a normal industrial cooling of 60°C / min up to the beginning of the critical embrittlement temperature range (550°C), followed by rapid cooling at above 500°C / min throughout this range. [Diagram 2] Plot of SANS data (intensity I(Q) [cm-1] vs. inverse wavelength Q [nm-1]) showing evidence of phase separation (increase in peak intensity and shift to lower wavelengths with longer exposure times) at 450°C for a super duplex grade. The figure also shows how an external magnetic field (1.5 T) suppresses the peaks (spinodal decomposition) and therefore embrittlement. [Diagram 3] FIG. 3 is a plot of SANS data (intensity I(Q) [cm-1] versus inverse wavelength Q [nm-1]) showing evidence of phase separation (increase in peak intensity with longer exposure times and shift to lower wavelengths) at 450° C. for a two-phase grade. FIG. 3 also shows how an external magnetic field (1.5 T) suppresses the peaks and therefore embrittlement. [Figure 4] Plot of SANS data (intensity I(Q) [cm-1] vs inverse wavelength Q [nm-1]) showing how initial typical industrial cooling of material at 60 °C / min (identified as "Slow" in the plot) affects the nanostructure already in the as-received state, compared to more rapid cooling conditions, over 500 °C / min (identified as "Fast" in the plot), over 550-350 °C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention relates to a method for inhibiting embrittlement of stainless steel in a stainless steel production process, comprising the steps of producing stainless steel in a conventional stainless steel production process, annealing the stainless steel in an annealing step having an annealing temperature range of 900-1250°C, quenching the steel in a water bath or any other suitable quenching medium / process, including air cooling with or without forced air, over a critical temperature range of 350°C-550°C and below 350°C, in particular below 200°C, preferably below 150°C, suitably up to 100°C, and applying a magnetic field to the steel during either the annealing step or the cooling / quenching step, or during both the annealing step and the cooling / quenching step.

[0016] Figure 1 shows that different cooling rates can affect the properties of duplex stainless steels with respect to 475°C embrittlement. Regular industrial process cooling (dashed line) gives low impact toughness strength, since some spinodal decomposition has already occurred during this cooling period. If the material is rapidly quenched from 550°C to 350°C (solid black line), the impact toughness is significantly higher (Table 1), since there was no time for spinodal decomposition to occur. For the air-cooled specimen, the residence time in the critical region is significantly longer than for regular process cooling, so the impact toughness is logically even lower than for the process-cooled specimen.

[0017] The curves in Fig. 2 represent different heat treatment and process conditions for the super-duplex material. The material aged at 450°C for 500 hours had a Q of 0.007 nm. -1 After 6 hours at this temperature, the peak intensity becomes smaller and the peak intensity becomes smaller at higher inverse wavelengths (Q 0.01 nm). -1), indicating less phase separation, as might be expected considering the shorter exposure time. This trend continues for the sample held for 2 hours, with a smaller but still very significant peak. In comparison, materials held for 6 and 2 hours at 450°C in the presence of a magnetic field (1.5T) show no signs of phase separation, as no peak intensity is observed above background levels. This indicates that in the presence of a magnetic field, 475°C embrittlement is completely suppressed at isothermal aging conditions up to at least 6 hours.

[0018] Figure 3 shows the same findings as in Figure 2, except for the duplex grade 2205 rather than the superduplex grade 2507. Despite the fact that the duplex grades are less susceptible to embrittlement than the superduplex grades due to the fact that they have less Cr. Figure 3 still shows that at 450°C for 6 hours there is a significant degree of spinodal decomposition and even after 30 minutes some affected nanostructure can be observed. Also, even for this grade, in the presence of an external magnetic field, phase separation is significantly suppressed.

[0019] Figure 4 shows the SANS data (intensity I(Q) [cm-1] vs. inverse wavelength Q [nm -1 ]) are plotted. The total exposure time to the 475°C temperature range is shorter than that in Figure 2. The typical background intensity differs between the "slow" and "fast" cooling sample curves due to typical microstructural differences, e.g., different austenite intervals. However, the average background intensity is about 0.01 nm. -1The slight curvature of the intensity at (data points show higher intensity than the background reference line added to the plot) measures the change in nanostructure and indicates that the slowly cooled sample shows incipient phase separation, whereas the fast cooled sample appears to be unaffected. The process cooling rate of the slowly cooled sample in Figure 4 was similar to that of the slowly cooled sample in Figure 1 (50-70 °C / min and Table 1), which also had low impact toughness. This indicates that the material produced by production may already have some degree of phase separation and embrittlement in the as-received state. The degree of phase separation, and therefore embrittlement, becomes more severe in air-cooled parts when the cooling rate is much less than 50 °C / min. The "fast" cooled sample in Figure 4 was rapidly cooled (>500 °C / min) faster than would be possible under normal process quenching conditions. Thus, in a practical process, it is not possible to cool a thick plate, such as a square plate, fast enough to avoid the onset of embrittlement. The application of an external magnetic field overcomes this problem and allows the material to be delivered without spinodal decomposition / embrittlement.

[0020] Embodiment The present invention relates to a method for inhibiting embrittlement of stainless steel in a stainless steel production process. In an embodiment, the process comprises the steps of providing an annealed stainless steel, cooling or quenching the steel in a cooling or quenching step, and applying a magnetic field to the stainless steel. The cooling / quenching is most typically performed in a batch in a water bath (or mass spray in-line) or air cooling. A magnetic field is applied to the stainless steel during the cooling or quenching step. It has been found that embodiments of the present invention are suitable for all types of stainless steel. Thus, in another embodiment, providing an annealed stainless steel includes, but is not limited to, stainless steel produced by any process such as melting raw material and / or scrap material, casting into stainless steel ingots, slabs, blooms or atomized metal powder, or rolling into stainless steel billets, plates, sheets, strips, coils, bars, rods, wires, profiles and shapes, seamless and welded tubes and / or pipes, formed shapes, near net shape powder metallurgy and profiles, further processing by pressing or molding, followed by casting either by ingot casting or continuous casting, followed by hot rolling and / or cold rolling, or forging ready for final annealing in the temperature range of 900°C to 1250°C. In a further embodiment, the stainless steel melt can be used to produce metal powder for isostatic pressing or additive manufacturing for annealing and cooling or quenching.

[0021] In one embodiment, raw materials such as nickel and molybdenum are melted with scrap metal in an electric arc furnace, with or without vacuum oxygen decarburization. Electric arc furnaces are particularly efficient for purposes of embodiments of the present invention.

[0022] In some embodiments, the stainless steel is tapped into a mold. The mold may be made from a variety of materials known to those skilled in the art. In one embodiment, the stainless steel is tapped into a copper mold. In a further embodiment, the stainless steel is continuously cast into a slab.

[0023] As mentioned above, the stainless steel manufacturing process includes an annealing step. Such a process may include one or more annealing steps in the temperature range of 900°C to 1250°C. In some embodiments, the annealing step has the purpose of homogenizing the stainless steel and softening and dissolving secondary phases, such as carbides, nitrides, and intermetallic compounds such as sigma phases. Thus, in some embodiments, the annealing step includes increasing the temperature of the steel to a temperature above 900°C. The annealing step may be performed in an embodiment in a batch furnace for batch annealing or by in-line annealing.

[0024] The stainless steel manufacturing process also includes a cooling or quenching step. The number of quenching steps is usually equal to the number of annealing steps. In some embodiments, the cooling or quenching step reduces the temperature of the steel to maintain the material properties of the steel.

[0025] In some embodiments, the quenching step reduces the temperature of the steel from the annealing temperature below a temperature at which secondary phases or embrittlement can no longer form or occur, i.e. below 350°C, in particular below 200°C, preferably below 150°C, suitably below 100°C, by a quenching method selected from batch quenching in a water bath, in-line quenching, spraying, and other suitable quenching techniques as used in the stainless steel industry in producing duplex stainless steels. In some embodiments, the quenching step reduces the temperature of the steel to room temperature or to a temperature in the range of room temperature to 350°C. For the purposes of this application, room temperature means a temperature in the range of 20 to 25°C. Cooling below 20°C has no particular advantage.

[0026] In another embodiment, the cooling step involves air cooling, either by forced air or natural cooling, to reduce the temperature of the steel to room temperature.

[0027] In a further embodiment, the magnetic field has a field strength greater than 0.2 T, preferably greater than 1.0, most preferably in the range of 1.5-3.0 T. Increasing the magnetic strength above 3.0 T does not provide any special advantage since the material will reach magnetic saturation. The magnetic field inhibits embrittlement of stainless steels.

[0028] As mentioned above, embodiments of the present invention are suitable for all stainless steels, in particular embodiments, the stainless steel is a ferritic stainless steel or a martensitic stainless steel.

[0029] The following non-limiting examples illustrate at least some embodiments of the present invention.

[0030] Working Example Duplex grades are sensitive to 475°C embrittlement. Impact toughness testing (Charpy impact test) is a standardized test method (e.g., well established as a test method for determining the presence of deleterious phases in duplex grades as described in ASTM A923 method B, in accordance with ISO 148-1:2016, ISO 17781) and is ideally suited to determine whether a material has been sensitized in some way, for example, by 475°C embrittlement. Impact toughness tests were performed at -40°C on duplex grades that were subjected to cooling conditions different from the normal annealing temperature, as shown in Figure 1. For this purpose, a GLEEBLE instrument was used to simulate the typical cooling curve of a plate material when quenched in a water bath, and thus the cooling through the critical temperature range 550-350°C was at a normal rate (dashed line in Figure 1). In comparison, other samples were cooled to 550°C under the same conditions and then rapidly quenched through the critical temperature range to completely eliminate the onset of 475°C embrittlement (solid line in Figure 1). The specimens used for this GLEEBLE simulation and impact toughness test were of standard size 55x10x6mm with a v-notch for impact testing. The 6mm thickness allowed for precise temperature control throughout the cooling step. The results in Table 1 from the cooling conditions in Figure 1 show that with normal process quenching, the impact toughness is lower than for specimens where rapid quenching was used to avoid embrittlement, indicating that embrittlement exists at 475°C under normal cooling conditions for heavy plate.

[0031] Small angle neutron scattering (SANS) has been applied to highlight the evolution of the nanostructure resulting from spinodal decomposition in dual-phase steels after exposure to temperatures of about 475 °C, either isothermally or during process cooling. Similarly, SANS has been used to show that spinodal decomposition is suppressed after the same exposure by an applied external magnetic field. Specifically, SANS measures the spinodal decomposition in the nanostructure, i.e. at the atomic level, that is present when dual-phase steels are exposed to temperatures between 250 and 500 °C, with the development of Fe-rich and Cr-rich (segregation) domains. This phase separation leads to embrittlement, limiting for example the impact toughness. A sample size of 10 x 10 x 1 mm was used. The 1 mm thickness allows for good signal strength and also avoids multiple scattering that may otherwise be experienced with thicker samples. The 10 x 10 mm dimensions are ideal to give a uniform temperature throughout the sample when heated samples are required.

[0032] Using a SANS apparatus, several tests have been carried out to highlight the presence of spinodal decomposition in a dual-phase steel under different conditions, showing how sensitive this material is to this phenomenon of 475°C embrittlement and how it can be suppressed in the presence of a magnetic field of, for example, 1.5 T.

[0033] Figures 2 and 3 show how phase separation can be clearly detected using SANS for two different austenitic-ferritic duplex stainless steels. The previously annealed and quenched materials were held at 450°C for 6 and 500 hours. With increasing time, the peak intensity increases and the position of the peak shifts to a lower Q (nm -1), indicating that spinodal decomposition progresses with time. This is more evident in Fig. 2 compared to Fig. 3 due to the higher alloy content, especially chromium, of the super duplex grade in this Fig. 2. Tests were also carried out on samples held at 475 °C for up to 6 hours in the presence of an applied external magnetic field of strength 1.5 T. These tests showed that the degree of phase separation, and therefore embrittlement, can be suppressed to very low and insignificant levels, as indicated by the absence of intensity peaks that would otherwise be observed without a magnetic field. This is true for both the duplex grades in Fig. 2 and Fig. 3, indicating that even if a large amount of spinodal decomposition is potentially present (Fig. 2), this can be suppressed in the presence of a magnetic field.

[0034] Figure 4 shows that under normal process quenching with relatively slow cooling (approximately 60°C / min) as in the case of thick plate material, there is some phase separation as indicated by the slight intensity peak in the as-received condition compared to the rapidly cooled material. As already mentioned, rapid cooling (>500°C / min) as fast as the "fast sample" in Figure 4 is not possible for many plates, thus deemphasizing the need for a means to suppress 475°C embrittlement, such as using a magnetic field.

[0035] It has been shown that in the presence of an applied external magnetic field, the decomposition kinetics in the two-phase alloy should be significantly suppressed and embrittlement should also be significantly delayed.

[0036] For this purpose, an external magnetic field of >0.2 T should be applied to the stainless steel being cooled or quenched during the entire cooling or quenching process of the part, preferably during cooling or quenching from below 600° C. The magnetic field is applied such that the entire material to be cooled or quenched is surrounded by a magnetic field of >0.2 T.

[0037] [Table 1]

Claims

1. 1. A method for inhibiting embrittlement of stainless steel in a stainless steel production process, comprising: Producing stainless steel in a conventional stainless steel production process; - annealing the stainless steel in an annealing step; - cooling the steel in a cooling step or quenching the steel in a quenching step; applying a magnetic field to the stainless steel; the magnetic field is applied to the stainless steel during the cooling or quenching step; A method characterized in that the cooling or quenching step reduces the temperature of the steel from the annealing temperature to below 350°C either by a quenching step (batch quenching in a water tank or in-line spraying) or by a cooling step (as air cooling, either by forced air or natural cooling).

2. The stainless steel production process comprises: Melting raw / scrap materials for stainless steel production; Casting stainless steel into ingots, slabs, blooms or atomized metal powder; The method of claim 1, comprising further processing the stainless steel by rolling, pressing or forming into billets, plates, sheets, strip, coils, bars, rods, wires, shapes and forms, seamless and welded tubes and / or pipes, formed shapes, near net shape powder metallurgy and shapes.

3. 3. The method of claim 2, wherein the raw materials are melted in an electric arc furnace with or without vacuum oxygen decarburization.

4. The method of any one of claims 1 to 3, wherein the stainless steel is tapped into a mould.

5. The method of any one of claims 1 to 4, wherein the stainless steel is tapped into a copper mould.

6. The method according to any one of claims 1 to 5, wherein the stainless steel is continuously cast into slabs.

7. A method according to any one of the preceding claims, wherein the annealing step comprises increasing the temperature of the steel to above 900°C for homogenization, softening and dissolution of secondary phases.

8. A method according to any one of the preceding claims, wherein the cooling or quenching step reduces the temperature of the steel in order to maintain its material properties.

9. The method according to any one of claims 1 to 8, wherein the annealing step is carried out in a batch furnace for batch annealing or in-line annealing.

10. The method according to any one of the preceding claims, wherein the magnetic field applied during quenching has a field strength of more than 0.2 T.

11. The method according to any one of claims 1 to 10, wherein the stainless steel is a ferritic stainless steel or a martensite containing stainless steel.

Citation Information

Patent Citations

  • Production of cr-series stainless steel sheet by using thin thickness casting method

    JP1989197046A

  • Production of cu-containing ferritic stainless steel strip

    JP1998273731A

  • Steel alloy, plastic molding tool holder or holder detail, hardened blank for holder or holder detail, steel alloy production method

    JP2010503770A

  • Low nickel austenitic stainless steel and method for manufacturing hot-rolled steel sheet of the same