Manufacturing method for gloves with highly abrasion-resistant and highly slip-resistant soft coating
A manufacturing method using biologically derived organic polymers enhances the anti-slip and abrasion resistance of gloves, addressing comfort and durability issues in existing technologies, and providing an environmentally friendly production process.
Patent Information
- Application Number
- JP2024071018
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-01-09
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2044-04-25
AI Technical Summary
Existing gloves with anti-slip properties either lack comfort or durability, and their production processes are environmentally harmful or costly, failing to meet the demand for high abrasion resistance and anti-slip performance in both oily and dry environments.
A manufacturing method involving the use of biologically derived organic polymers like albumin, globulin, and casein, combined with a series of chemical treatments and vulcanization processes, to create a soft coating with enhanced abrasion resistance and anti-slip properties.
The method results in a coating with improved frictional force, wear resistance, and durability, while being environmentally friendly and comfortable to use, with a delicate sandy surface effect.
Smart Images

Figure 0007574488000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of glove manufacturing, and in particular to a method for manufacturing gloves with a highly abrasion-resistant and highly slip-resistant soft coating. [Background technology]
[0002] With the development of society, enterprises are increasingly attaching importance to the safety of workers, and since production work is carried out in oily and dry environments, the requirements for grip and comfort during work are increasing, so that the market is in high demand for gloves with soft coatings that have high anti-slip properties and high abrasion resistance. Currently, various products such as latex texture gloves, embossed gloves, washable gloves, and matte gloves are on the market as such products. However, latex texture gloves / embossed gloves have excellent anti-slip properties, but are not comfortable to use, and require the use of organic solvents with pungent odors such as xylene during production, and the production process is not environmentally friendly. Washable gloves have excellent comfort, but are generally non-slip and durable, and a large amount of wastewater is generated during production, which incurs extremely high production costs for wastewater treatment. Summary of the Invention [Problem to be solved by the invention]
[0003] The present invention aims to provide a method for producing gloves with a highly abrasion-resistant and highly slip-resistant soft coating, which has a simple and reliable production process, greatly improves the slip-resistant and abrasion-resistant properties of the coating, and gives the coating a delicate sand effect, resulting in very good slip-resistant properties, durability and comfort in both oily and dry environments. [Means for solving the problem]
[0004] The above technical object of the present invention is achieved by the following technical solutions.
[0005] A method for producing gloves with a highly abrasion-resistant and highly slip-resistant soft coating, comprising the steps of: The surface of the glove core coated with impregnated latex is physically sprayed with a bio-based organic polymer material, and the surface is pre-vulcanized and then vulcanized at high temperature. The glove is then washed in this order with an alkaline solution, an acid solution, and water, and dried to obtain a highly abrasion-resistant, anti-slip soft-coated glove.
[0006] Preferably, the biological organic polymer material is selected from one or more mixtures of albumin, globulin, phosphoprotein, and casein, the particle size of the biological organic polymer material is less than 50 mesh, and the frequency of the spray fan is 10Hz to 30Hz.
[0007] Preferably, the pre-vulcanization temperature is 70° C. to 90° C., the pre-vulcanization time is 90 minutes, the high-temperature vulcanization temperature is 110° C. to 140° C., and the high-temperature vulcanization time is 90 minutes.
[0008] Preferably, the alkaline solution used in the alkaline cleaning is any one selected from a NaOH solution or a KOH solution, the mass fraction of the alkaline solution is 1% to 5%, the alkaline cleaning time is 45 to 70 minutes, the acid solution used in the acid cleaning is an acetic acid solution with a mass fraction of 1% to 5%, the acid cleaning time is 45 to 70 minutes, the acid cleaning is followed by two water washes, the water washing time is 60 minutes, and the drying temperature is 90°C.
[0009] Preferably, the impregnated latex contains, by weight, 70-100 parts of nitrile latex, 15-20 parts of styrene butadiene latex, 7-10 parts of water-based PU, 0.5-0.8 parts of KOH, 1-2 parts of surfactant, 2-3 parts of blowing agent, 1-3 parts of sulfur, 2-4 parts of accelerator, 1-3 parts of zinc oxide, 1-3 parts of titanium dioxide, 3-5 parts of film former, 4-5 parts of anti-aging agent, 7-10 parts of crosslinker, 4-5 parts of bio-composite enzyme, 1-3 parts of black pigment, 1-4 parts of thickener as raw materials.
[0010] Preferably, the surfactant is any one selected from polyoxyethylene, polyoxypropylene, sodium tripolyphosphate, and sodium sulfate, the foaming agent is any one selected from azo compounds, sulfonylhydrazides, and nitroso compounds, the accelerator is any one selected from thiazole accelerators, sulfenamide accelerators, thiuram accelerators, dithiocarbamate accelerators, guanidine accelerators, and xanthic acid accelerators, the film-forming agent is any one selected from polymer resins, acrylic resins, and nitrocellulose, and the antiaging agent is any one selected from amine-based antiaging agents, phenol-based antiaging agents, and heterocyclic antiaging agents. the cross-linking agent is any one selected from phenolic resin, epoxy resin, or polyvinyl alcohol; the bioconjugate enzyme is any one selected from enzymes amylase, protease, lipase, phytase, cellulase, or glucanase; and the thickener is any one selected from sodium carboxymethylcellulose, propylene glycol alginate, sodium starch glycolate, hydroxypropyl starch ether, sodium starch phosphate, acetylated phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, or hydroxypropylated phosphate cross-linked starch.
[0011] Preferably, the method for producing the impregnated latex coated glove core comprises the steps of: Step S1 of mixing and stirring the raw materials of each component of the impregnated latex to obtain the impregnated latex; Step S2 of placing the glove core on a hand mold and preheating it at a processing temperature of 50 to 80 ° C.; Step S3 of impregnating the core of the glove with a coagulant in the preheating process; After the coagulant is soaked for 60S to 80S, the latex is soaked and spread on 1 to 4 sides in step S4; After the latex impregnation step is completed, the method proceeds to a latex spreading step, and includes step S5 in which the latex spreading time is set to 50 S to 80 S.
[0012] Preferably, the coagulant is a mixture of acetic acid and methanol, and the volume fraction of the acetic acid in the mixture is 3% to 10%.
[0013] The present invention further provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating produced by the above-mentioned production method. Effect of the Invention
[0014] As described above, the present invention has the following beneficial effects.
[0015] 1. The present invention uses organic polymeric materials of biological origin, namely albumin, globulin, phosphoprotein, and casein, to increase the frictional force of the coating and at the same time increase the strength of the coating. These organic polymeric materials of biological origin have characteristics such as low density and high strength, so that they can be more uniformly dispersed on the surface of the coating during the spraying process, and during the vulcanization process, the biological polymeric materials react more completely with the carbonyl compounds in the impregnated latex material and the carbonyl amines of the amino compounds, so that the polymerization of the polymer becomes denser, and the physical properties of the coating, such as the wear resistance and anti-slip properties, are improved.
[0016] 2. The amino groups in the bio-based polymeric material and the impregnated latex material in the present invention react with the isocyanate groups to produce urea-based compounds, and the reaction mechanism can be divided into two steps. The first step is that the amino groups attack the isocyanate groups in the isocyanate to form an intermediate such as an amine. The second step is that the intermediate reacts with another isocyanate molecule to produce a urea-based compound. The urea-based compound can effectively fill the gaps between the rubber (coating) molecules, improve its abrasion resistance and tear resistance, and can also improve the heat resistance of the rubber and improve its stability and elasticity in a high-temperature environment. At the same time, the protein (keratin) in the bio-based organic polymeric material remaining on the surface of the coating has very good compatibility, and is tightly bound to the coating material by the intermolecular force during the coating process, greatly improving the abrasion resistance of the coating, and does not cause any irritation to the skin.
[0017] 3. The crosslinking agent used in the present invention can increase the crosslinking strength of rubber and obtain better physical performance by adding hydroxymethyl groups with double bonds such as carboxyl groups in rubber, and can increase the adhesion between rubber and impregnated substrate by reacting with functional group -N=C=N- (Carbodilite) on impregnated substrate, and can increase the durability of coating. Anti-aging agent forms a protective film on the surface of rubber, and the active ingredient of the anti-aging agent can chemically react with oxygen molecules on the surface of rubber to form a protective film, which has very high antioxidant performance, so that it can prevent further erosion of oxygen molecules and delay the aging process of rubber. Biological composite enzyme removes unreacted biological organic polymer materials remaining on the surface of the coating during production, leaving only a high-strength film layer on the surface of the coating, significantly improving the wear resistance of the coating. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a microstructure diagram of the surface layer of a glove produced according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, specific embodiments of the present invention will be described in further detail with reference to the drawings, but the present invention is not limited to these embodiments.
[0020] Example 1 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 containing, in parts by weight, as raw materials 70 parts nitrile latex, 15 parts styrene butadiene latex, 10 parts water-based PU, 0.5 parts KOH, 1 part polyoxyethylene as surfactant, 2 parts azo compound as blowing agent, 1 part sulfur, 2 parts thiazole accelerator, 1 part zinc oxide, 1 part titanium dioxide, 3 parts polymer resin as film former, 4 parts amine-based anti-aging agent, 7 parts phenolic resin as crosslinker, 4 parts enzyme amylase, 1 part black pigment, 1 part sodium carboxymethylcellulose as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which albumin is physically sprayed onto the latex coating with a fan frequency of 10 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 1% for 70 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0021] Example 2 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 containing, in parts by weight, as raw materials 70 parts nitrile latex, 15 parts styrene butadiene latex, 10 parts water-based PU, 0.5 parts KOH, 1 part polyoxyethylene as surfactant, 2 parts azo compound as blowing agent, 1 part sulfur, 2 parts thiazole accelerator, 1 part zinc oxide, 1 part titanium dioxide, 3 parts polymer resin as film former, 4 parts amine-based anti-aging agent, 7 parts phenolic resin as crosslinker, 4 parts enzyme amylase, 1 part black pigment, 1 part sodium carboxymethylcellulose as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which albumin is physically sprayed onto the latex coating with a fan frequency of 15 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 1% for 70 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0022] Example 3 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 containing, in parts by weight, as raw materials 70 parts nitrile latex, 15 parts styrene butadiene latex, 10 parts water-based PU, 0.5 parts KOH, 1 part polyoxyethylene as surfactant, 2 parts azo compound as blowing agent, 1 part sulfur, 2 parts thiazole accelerator, 1 part zinc oxide, 1 part titanium dioxide, 3 parts polymer resin as film former, 4 parts amine-based anti-aging agent, 7 parts phenolic resin as crosslinker, 4 parts enzyme amylase, 1 part black pigment, 1 part sodium carboxymethylcellulose as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which albumin is physically sprayed onto the latex coating with a fan frequency of 20 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 1% for 70 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0023] Example 4 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 comprising, in parts by weight, as raw materials 85 parts nitrile latex, 18 parts styrene butadiene latex, 8 parts waterborne PU, 0.7 parts KOH, 2 parts polyoxypropylene as surfactant, 3 parts sulfonyl hydrazide as blowing agent, 2 parts sulfur, 3 parts sulfenamide accelerator, 2 parts zinc oxide, 2 parts titanium dioxide, 4 parts acrylic resin as film former, 5 parts phenolic age inhibitor, 9 parts epoxy resin as crosslinker, 4 parts protease, 2 parts black pigment, 3 parts propylene glycol alginate as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 5%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which albumin is physically sprayed onto the latex coating with a fan frequency of 25 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 3% for 60 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0024] Example 5 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 comprising, in parts by weight, as raw materials 85 parts nitrile latex, 18 parts styrene butadiene latex, 8 parts waterborne PU, 0.7 parts KOH, 2 parts polyoxypropylene as surfactant, 3 parts sulfonyl hydrazide as blowing agent, 2 parts sulfur, 3 parts sulfenamide accelerator, 2 parts zinc oxide, 2 parts titanium dioxide, 4 parts acrylic resin as film former, 5 parts phenolic age inhibitor, 9 parts epoxy resin as crosslinker, 4 parts protease, 2 parts black pigment, 3 parts propylene glycol alginate as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 5%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which albumin is physically sprayed onto the latex coating with a fan frequency of 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 3% for 60 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0025] Example 6 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation of impregnated latex S1 comprising, in parts by weight, as raw materials 85 parts nitrile latex, 18 parts styrene butadiene latex, 8 parts waterborne PU, 0.7 parts KOH, 2 parts polyoxypropylene as surfactant, 3 parts sulfonyl hydrazide as blowing agent, 2 parts sulfur, 3 parts sulfenamide accelerator, 2 parts zinc oxide, 2 parts titanium dioxide, 4 parts acrylic resin as film former, 5 parts phenolic age inhibitor, 9 parts epoxy resin as crosslinker, 4 parts protease, 2 parts black pigment, 3 parts propylene glycol alginate as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 5%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which globulin is physically sprayed onto the latex coating with a fan frequency of 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 3% for 60 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0026] Example 7 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation S1 of impregnated latex containing, in parts by weight, as raw materials 100 parts of nitrile latex, 20 parts of styrene butadiene latex, 10 parts of water-based PU, 0.8 parts of KOH, 2 parts of sodium tripolyphosphate as surfactant, 3 parts of nitroso compound as blowing agent, 3 parts of sulfur, 4 parts of dithiocarbamate accelerator, 3 parts of zinc oxide, 3 parts of titanium dioxide, 5 parts of nitrocellulose as film former, 5 parts of heterocyclic antioxidant, 10 parts of polyvinyl alcohol as crosslinker, 5 parts of cellulase, 3 parts of black pigment, 4 parts of monoesterified phosphate crosslinked starch as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 10%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which phosphoprotein is physically sprayed onto the latex coating with a fan frequency of 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 5% for 45 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0027] Example 8 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation S1 of impregnated latex containing, in parts by weight, as raw materials 100 parts of nitrile latex, 20 parts of styrene butadiene latex, 10 parts of water-based PU, 0.8 parts of KOH, 2 parts of sodium tripolyphosphate as surfactant, 3 parts of nitroso compound as blowing agent, 3 parts of sulfur, 4 parts of dithiocarbamate accelerator, 3 parts of zinc oxide, 3 parts of titanium dioxide, 5 parts of nitrocellulose as film former, 5 parts of heterocyclic antioxidant, 10 parts of polyvinyl alcohol as crosslinker, 5 parts of cellulase, 3 parts of black pigment, 4 parts of monoesterified phosphate crosslinked starch as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 10%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which casein is physically sprayed onto the latex coating with a fan frequency of 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 5% for 45 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0028] Example 9 This embodiment provides a glove with a highly abrasion-resistant and highly slip-resistant soft coating, and the manufacturing method thereof is as follows: Preparation S1 of impregnated latex containing, in parts by weight, as raw materials 100 parts of nitrile latex, 20 parts of styrene butadiene latex, 10 parts of water-based PU, 0.8 parts of KOH, 2 parts of sodium tripolyphosphate as surfactant, 3 parts of nitroso compound as blowing agent, 3 parts of sulfur, 4 parts of dithiocarbamate accelerator, 3 parts of zinc oxide, 3 parts of titanium dioxide, 5 parts of nitrocellulose as film former, 5 parts of heterocyclic antioxidant, 10 parts of polyvinyl alcohol as crosslinker, 5 parts of cellulase, 3 parts of black pigment, 4 parts of monoesterified phosphate crosslinked starch as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 10%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment step S6 in which phosphoprotein is physically sprayed onto the latex coating with a fan frequency of 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 5% for 45 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0029] Comparative Example 1 This comparative example provides a coated glove, the manufacturing method of which is as follows: Preparation of impregnated latex S1 containing, in parts by weight, as raw materials 70 parts nitrile latex, 15 parts styrene butadiene latex, 10 parts water-based PU, 0.5 parts KOH, 1 part polyoxyethylene as surfactant, 2 parts azo compound as blowing agent, 1 part sulfur, 2 parts thiazole accelerator, 1 part zinc oxide, 1 part titanium dioxide, 3 parts polymer resin as film former, 4 parts amine-based anti-aging agent, 7 parts phenolic resin as crosslinker, 4 parts enzyme amylase, 1 part black pigment, 1 part sodium carboxymethylcellulose as thickener; A preheating process S2 in which the glove core is placed on a hand mold and preheated at a processing temperature of 50°C; A coagulant impregnation step S3 in which the core of the glove in the preheating step is impregnated with a coagulant, the coagulant being a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%; After the coagulant is soaked for 60S, the latex is soaked and spread over the four sides in a latex soaking process S4; After the latex impregnation step is completed, the process proceeds to a latex spreading step S5, in which the latex spreading time is set to 50 s; a surface treatment process S6 in which industrial salt is sprayed onto the latex coating and the fan frequency is set to 30 Hz; A pre-vulcanization process and a vulcanization process S7 in which the mixture is pre-vulcanized at a temperature of 90°C and then vulcanized at a high temperature of 110°C for a processing time of 1.5 hours, respectively; The gloves are then washed with an acetic acid solution having a mass fraction of 1% for 70 minutes, and then rinsed with water twice after the acid washing, with the rinse time being 60 minutes. The gloves are then dried at 90°C to obtain a release agent S8.
[0030] The anti-slip properties of the gloves were measured by the dry slip method, the weight was 1.5 kg, the standard unit of anti-slip properties (kgf) was used, and the mechanical performance test of the gloves was measured according to the European standard EN-388 test method.
[0031] Mechanical tests were carried out and analyzed for the above-mentioned Examples 1 to 9 and Comparative Example 1, and the specific test results are shown in Table 1.
[0032] [Table 1]
[0033] As can be seen from the above experimental data, the treatment method of the present invention can effectively produce a coating with high anti-slip and high wear resistance. As can be seen from the data, the more uniformly the bio-based organic polymer material is sprayed, the higher the anti-slip and wear resistance of the glove will be, and at the same time, when the fan frequency is 20Hz, the performance of the coating sprayed with the bio-based organic polymer material is completely superior to that of the coating sprayed with industrial salt.
[0034] As can be seen from Figure 1, the coating produced by the process of the present invention has relatively uniform pore size of bubbles, and these uniform bubbles are like suction cups, when the rubber contacts the surface of the object, the rubber can contact the small protrusions on the surface of the object over a larger area, thereby achieving a greater adsorption effect, and under the action of atmospheric pressure, a vacuum space is formed, and the suction cups are in close contact with the object, greatly improving the adsorption force and increasing the gripping force of the coating. In addition, the bio-composite enzyme in the formulation system of the present invention can decompose the excess biological macromolecular organic materials on the coating during production, leaving only a high-strength film layer on the surface of the coating, significantly improving the wear resistance of the coating.
[0035] The above content is only the preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art can make various modifications and equivalent replacements to the present invention within the essence and protection scope of the present invention, and these modifications and equivalent replacements should fall within the protection scope of the technical solutions of the present invention.
Claims
1. A method for producing a highly abrasion resistant and highly slip-resistant soft coated glove, comprising the steps of: A method for producing a highly abrasion resistant and highly slip-resistant soft-coated glove, comprising the steps of physically spraying a bio-based organic polymer material onto the surface of a glove core coated with impregnated latex, pre-vulcanizing and high-temperature vulcanizing the glove in sequence, washing the glove with an alkaline solution, an acid solution, and water in that order, and drying the glove to obtain a highly abrasion resistant and highly slip-resistant soft-coated glove.
2. The method for producing a highly abrasion-resistant and highly anti-slip soft coated glove according to claim 1, characterized in that the biological organic polymer material is selected from one or a mixture of albumin, globulin, phosphoprotein, and casein, the particle size of the biological organic polymer material is less than 50 mesh, and the frequency of the spray fan is 10 Hz to 30 Hz.
3. The method for producing a highly abrasion resistant and highly slip-resistant soft coated glove according to claim 1, characterized in that the temperature of the pre-vulcanization is 70°C to 90°C, the time of the pre-vulcanization is 90 minutes, the temperature of the high-temperature vulcanization is 110°C to 140°C, and the time of the high-temperature vulcanization is 90 minutes.
4. The method for producing a highly abrasion resistant and highly anti-slip soft coated glove according to claim 1, characterized in that the alkaline solution used in the alkaline washing is selected from a NaOH solution or a KOH solution, the mass fraction of the alkaline solution is 1% to 5%, the washing time with the alkaline solution is 45 to 70 min, the acid solution used in the acid washing is an acetic acid solution having a mass fraction of 1% to 5%, the washing time with the acid solution is 45 to 70 min, washing with water is performed twice after the washing with the acid solution, the water washing time is 60 min, and the drying temperature is 90°C.
5. The method for producing a highly abrasion resistant and highly slip-resistant soft coated glove according to claim 1, characterized in that the impregnated latex contains, as raw materials, 70-100 parts of nitrile latex, 15-20 parts of styrene butadiene latex, 7-10 parts of water-based PU, 0.5-0.8 parts of KOH, 1-2 parts of surfactant, 2-3 parts of foaming agent, 1-3 parts of sulfur, 2-4 parts of accelerator, 1-3 parts of zinc oxide, 1-3 parts of titanium dioxide, 3-5 parts of film forming agent, 4-5 parts of antioxidant, 7-10 parts of crosslinking agent, 4-5 parts of bio-composite enzyme, 1-3 parts of black pigment, and 1-4 parts of thickener, by weight.
6. The surfactant is any one selected from polyoxyethylene, polyoxypropylene, sodium tripolyphosphate, and sodium sulfate, the foaming agent is any one selected from azo compounds, sulfonylhydrazides, and nitroso compounds, the accelerator is any one selected from thiazole accelerators, sulfenamide accelerators, thiuram accelerators, dithiocarbamate accelerators, guanidine accelerators, and xanthic acid accelerators, the film-forming agent is any one selected from polymer resins, acrylic resins, and nitrocellulose, the antiaging agent is any one selected from amine-based antiaging agents, phenol-based antiaging agents, and heterocyclic antiaging agents, and the crosslinking agent is any one selected from fluorine-based antiaging agents.
6. The method for producing a highly abrasion resistant and highly slip-resistant soft coated glove according to claim 5, characterized in that the bioconjugate enzyme is any one selected from the group consisting of enzymes amylase, protease, lipase, phytase, cellulase and glucanase, and the thickener is any one selected from the group consisting of sodium carboxymethylcellulose, propylene glycol alginate, sodium starch glycolate, hydroxypropyl starch ether, sodium starch phosphate, acetylated starch phosphate cross-linked, phosphate monoesterified starch phosphate cross-linked and hydroxypropylated starch phosphate cross-linked.
7. The method for producing the glove core coated with the impregnated latex is specifically as follows: Step S1: mixing and stirring the raw materials of each component of the impregnated latex to obtain the impregnated latex; Step S2: placing the glove core on a hand mold and preheating at a processing temperature of 50 to 80°C; Step S3 of impregnating the core of the glove with a coagulant in the preheating step; Step S4: impregnating the coagulant for 60S to 80S, and then impregnating the latex and spreading it over 1 to 4 sides; The method for producing a glove with a highly abrasion resistant and highly slip-resistant soft coating according to claim 1, further comprising a step S5 of spreading the latex after the latex impregnation step is completed, the step being set to a latex spreading time of 50S to 80S.
8. The method for producing a highly abrasion resistant and highly slip-resistant soft coated glove according to claim 7, characterized in that the coagulant is a mixture of acetic acid and methanol, and the volume fraction of the acetic acid in the mixture is 3% to 10%.
Citation Information
Patent Citations
Anti-slip breathable operating gloves and preparation method thereof
CN106072923A
Flame-retardant rubber gloves and preparation method thereof
CN113698677A
Anti-cutting wrap yarn, application of anti-cutting wrap yarn, anti-cutting gloves and preparation method of anti-cutting gloves
CN114318611A
Carboxylic butyronitrile emulsion as well as preparation method and application thereof
CN114672082A
Antimicrobial elastomeric article
JP2022053532A
Cited By
Anti-cutting glove and preparation method thereof
CN119453602A