Lap fillet arc welding method and method for manufacturing welded joint
The lap fillet arc welding method addresses corrosion issues at welds in high-strength steel plates by using short-circuit transfer and controlled parameters, achieving stable weld bead shapes and reduced slag generation for improved corrosion resistance and manufacturing efficiency.
Patent Information
- Application Number
- JP2023570389
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-31
- Filing Date
- 2023-09-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-09-11
AI Technical Summary
Conventional welding methods fail to effectively prevent corrosion at welds in high-strength steel plates used in automotive components, leading to corrosion-related strength reduction and increased manufacturing complexity due to the use of toxic chemicals and special equipment.
A lap fillet arc welding method using short-circuit transfer and specific welding parameters, including a high Ar gas ratio, controlled welding angles, and pulse welding, to stabilize the weld bead shape and reduce slag generation, thereby enhancing corrosion resistance without requiring special equipment or toxic chemicals.
Stabilizes the weld bead shape and reduces slag formation, improving corrosion resistance and manufacturing efficiency while maintaining component strength and rigidity, thus enhancing the durability of automotive components.
Smart Images

Figure 0007574948000003 
Figure 0007574948000004 
Figure 0007574948000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a lap fillet arc welding method for obtaining an arc welded joint having a good weld toe shape while suppressing slag, and a method for manufacturing a welded joint. [Background technology]
[0002] In recent years, there has been an increasing need for automobiles to simultaneously increase the strength and rigidity of the components used in the body in order to improve the safety and reliability of the body, and to reduce the weight of the components in order to improve fuel efficiency. As a result, the use of high-strength steel plates has led to the thinning of steel plates used in components. On the other hand, among the various components used in automobiles, thicker steel plates are used for suspension components (such as lower arms) compared to the body in terms of component strength and rigidity. Therefore, if the strength of the steel plates used in suspension components can be increased and the thickness of the steel plates can be reduced, the weight of the vehicle body can be further reduced. This will achieve improved fuel efficiency while maintaining the strength and rigidity of the components.
[0003] In general, for the purpose of ensuring corrosion resistance, components used in a corrosive environment are subjected to anti-rust treatments such as chemical conversion coating and electrochemical coating after welding. However, over time, rust and corrosion may be observed at the welded part and its vicinity. As described above, corrosion occurring in components with electrochemical coating tends to occur at the welded part, and over time, it spreads with the blistering of the coating film over a wide area of the welded part and its periphery, and also progresses in the plate thickness direction. When corrosion progresses in this way, the plate thickness of the welded part and its vicinity decreases, resulting in a decrease in the strength of the welded part and ultimately a decrease in the strength of the component. In other words, when corrosion occurs and progresses in a component (such as an automobile suspension component) where a load acts on the welded part, it may lead to the destruction of the component.
[0004] When performing electrodeposition coating, in order to improve the adhesion between the base steel sheet and the weld metal and the electrodeposition coating, a chemical conversion treatment (e.g., zinc phosphate treatment, etc.) is performed as a pretreatment on the base steel sheet and the weld metal, and then the electrodeposition coating is performed. Zinc phosphate treatment, which is a widely used example of a chemical conversion treatment, is a technique for growing zinc phosphate crystals on the surface of the base steel sheet and the weld metal to improve the adhesion of the coating in the electrodeposition coating. However, with conventional techniques, even in components that have been subjected to a chemical conversion treatment prior to electrodeposition coating, coating blistering frequently occurs over a wide area at and around the weld over time. In other words, with the technique of performing the above-mentioned chemical conversion treatment as a pretreatment and then performing electrodeposition coating, it is difficult to completely suppress the occurrence of corrosion originating from the weld.
[0005] Furthermore, when arc welding is performed on components using steel sheets with a plated layer, the plated layer evaporates at the welded parts exposed to high heat from the heat source, the arc plasma (hereinafter referred to as "arc"), and non-plated parts are locally exposed. Therefore, a significant improvement in corrosion resistance that would justify the increased cost associated with the use of steel sheets with a plated layer cannot be expected.
[0006] As explained above, various manufacturing technologies have been developed to improve the corrosion resistance of components, but each has both advantages and disadvantages. From the perspective of improving corrosion resistance while suppressing increases in manufacturing costs, technologies that more effectively prevent the occurrence and progression of corrosion starting from welds are being studied.
[0007] The starting point of corrosion from the weld is (a) Slag adhering to the weld (mainly the surface of the weld bead), (b) Welding fumes adhering to the welded parts, (c) Oxides formed on the surface of steel plates exposed to high temperatures by welding; Even if a member having the above-mentioned deposits (a) and (b) or oxides (c) present in the welded portion is subjected to chemical conversion treatment, regions that are not covered with the chemical conversion layer made of zinc phosphate crystals will remain locally, originating from these deposits and products.
[0008] In areas not covered by the chemical conversion coating, the formation of the coating film is insufficient even if electrocoating is applied, and the adhesion of the coating film is insufficient, resulting in a significant decrease in corrosion resistance. This results in a decrease in plate thickness due to the occurrence and progression of corrosion. Therefore, the following technologies are being considered as a way to prevent the occurrence of the above-mentioned deposits (a) and (b) and oxides (c).
[0009] For example, Patent Document 1 discloses a technique in which after arc welding and before electrocoating, a weld and its vicinity are sprayed or immersed in a non-oxidizing acidic solution with a pH of 2 or less and a liquid temperature of 30 to 90° C. This technique removes the above-mentioned (a) slag, (b) welding fumes, and (c) oxides by dissolving the weld beads and steel plate in the non-oxidizing solution.
[0010] However, in the technology disclosed in Patent Document 1, the acid solution must be washed off before electrocoating, which complicates the manufacturing process of the component. In addition, the component formed into the desired shape is made by overlapping and joining steel plates of various shapes, so the acid solution remaining in the gaps between the overlapping plates causes severe corrosion. Furthermore, since a large amount of acid solution is used, the manufacturing equipment is exposed to a corrosive environment, making it prone to corrosion and failure, and it is also necessary to prevent the scattering of fumes to ensure the safety of workers.
[0011] Patent Document 2 discloses a technique for improving the post-painting corrosion resistance of a weld and its vicinity by reducing the total Si content of the welding wire and base metal used in arc welding and increasing the total Mn content of the welding wire and base metal.
[0012] However, if the Si content is reduced in order to suppress the generation of slag, the strength of the steel plate is inevitably reduced. In other words, with the technology disclosed in Patent Document 2, thick steel plates must be used to ensure the strength of the components, making it difficult to achieve a reduction in the weight of the car body.
[0013] Patent Document 3 discloses a technique for forming a sufficient chemical conversion coating layer by adjusting the components of the treatment solution used in the chemical conversion coating, even in the case of a weld bead containing slag, welding fumes, and oxides. This technique facilitates the formation of a chemical conversion coating layer by performing surface treatment using a surface conditioning solution containing zinc phosphate colloid. Furthermore, by performing chemical conversion treatment using a zinc phosphate treatment solution with an F content of 100 mass ppm or more, slag, welding fumes, and oxides are dissolved and removed, improving the adhesion of the coating film formed by electrodeposition coating.
[0014] However, the technology disclosed in Patent Document 3 uses a zinc phosphate treatment solution that contains fluorine, which is designated as a toxic substance, so when the wastewater is discharged outside the factory, the fluorine content must be reduced to a level that satisfies environmental standards, which requires large-scale wastewater treatment facilities in addition to the parts manufacturing facilities. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] Japanese Patent Application Publication No. 9-20994 [Patent Document 2] Japanese Patent Application Publication No. 8-33997 [Patent Document 3] Patent No. 5549615 Summary of the Invention [Problem to be solved by the invention]
[0016] The present invention has been made in consideration of these problems, and has an object to provide a lap fillet arc welding method and a manufacturing method for a welded joint that can prevent oxygen from being mixed into the weld metal and suppress the generation of slag without using special equipment, and can stably obtain a welded joint with an excellent weld bead shape. [Means for solving the problem]
[0017] The inventors have found that in order to improve the corrosion resistance of the welded portion and stably obtain a welded joint with a good bead shape, it is most effective to set the welding target position at the end of the upper sheet of two steel sheets and within a predetermined range in the direction perpendicular to the weld line of the lower sheet from the overlap corner, which is the corner formed by the two steel sheets. Here, in order to suppress the amount of slag generated that affects the corrosion resistance of the welded portion, it is important to suppress the oxidation of Si, Mn, Ti, etc. contained in the steel sheet and the welding wire, and if a shielding gas with a reduced content of oxidizing gas is used, the oxidation of these elements can be suppressed and the amount of slag generated can be reduced. However, in gas-shielded arc welding with a high Ar gas ratio in the shielding gas, after the oxide film on the surface of the steel sheet is removed by the cleaning action, the cathode spot crawls on the surface of the steel sheet, making the arc unstable, and the dissolution of O (oxygen), which reduces the surface tension, into the molten metal is extremely small, so that the weld bead shape is likely to be convex, which creates a new problem of reduced joint strength. Therefore, the inventors came up with the idea that regular droplet transfer is effective for a stable supply of deposited metal to the weld, and decided to utilize short-circuit transfer, which is less affected by arc fluctuation. Also, from the viewpoint of smoothing the weld bead shape, they thought that by offsetting the welding target position, which is the end of the upper sheet of two steel sheets and is also the corner of the overlapping portion formed by the two steel sheets, in a direction perpendicular to the weld line of the lower sheet, it would be possible to increase the contact area between the weld surface and the arc even without an element that reduces surface tension, and therefore it would be possible to increase the weld metal width and reduce the weld metal height for a constant deposition amount.
[0018] The present invention is based on the above findings, and the gist of the present invention is as follows. [1] A fillet arc welding method for joining a corner consisting of at least two steel sheets, comprising: a lap fillet arc welding method in which joining is performed using short-circuit transfer, the welding target position is the end of the upper sheet of the two steel sheets and is 0.2 mm to 1.8 mm in a direction perpendicular to the weld line of the lower sheet, starting from the corner of the overlapping portion which is an angle formed by the two steel sheets, a gas containing 98 volume % or more of Ar is used as a shielding gas, and the weld metal height H (mm) and weld metal width W (mm) of the weld satisfy the following formula (1). 0.2 ≦ H / W ≦ 1.2 (1) [2] The lap fillet arc welding method according to [1], wherein pulse welding is performed in which a pulse peak current (Ip) and a pulse base current (Ib) are periodically repeated, and the pulse peak current (Ip) of the pulse welding is 300 A or more and 600 A or less, and the pulse frequency is 30 Hz or more and 200 Hz or less. [3] A method for manufacturing a welded joint using the lap fillet arc welding method described in [1] or [2] above. Effect of the Invention
[0019] According to the present invention, it is possible to stably obtain a welded joint with a good bead shape, and it is also possible to suppress the intrusion of oxygen into the weld metal and the generation of slag without making special changes to the specifications of the welding equipment used in conventional MAG welding using an oxidizing gas or MIG welding using a gas mainly composed of an inert gas. [Brief description of the drawings]
[0020] [Figure 1-1] FIG. 2 is a schematic diagram showing an example of a welded joint produced by lap fillet arc welding. [Figure 1-2] FIG. [Figure 1-3] FIG. 2 is a cross-sectional view of a weld bead. [Diagram 2] 2(a) and 2(b) are schematic diagrams showing droplet transfer in conventional arc welding. [Diagram 3] 3(a) and 3(b) are schematic diagrams illustrating short-circuit transfer according to the present invention. [Figure 4]FIG. 2 is a schematic diagram showing a pulse current waveform in arc welding according to the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing the bead area and slag coverage area of a weld bead. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the present invention will be described in detail with reference to the drawings. Fig. 1-1 is a schematic diagram showing an example of a welded joint produced by lap fillet arc welding, showing an example of an embodiment of the present invention. The above is a representative example, and the shape of the welded joint and the welding position are not limited.
[0022] In the present invention, as shown in FIG. 1-1, for example, the welding wire 1 continuously fed from the welding torch 2 through the center of the welding torch 2 to the base metal 3 (more specifically, for example, a weld line consisting of a corner of a step formed by stacking two base metals 3) is used as the anode, and the base metal 3 is used as the cathode, and a welding voltage is applied from a welding power source (not shown). A part of the Ar shielding gas (not shown) supplied from the welding torch 2 is ionized and turned into plasma to form an arc 5 between the welding wire 1 and the base metal 3. The part of the Ar shielding gas that is not ionized and flows from the welding torch 2 to the base metal 3 plays a role of insulating the arc 5 and the molten pool (not shown in FIG. 1-1) formed by melting the base metal 3 from the outside air. The tip of the welding wire 1 melts and becomes a molten droplet due to the heat input from the arc 5, and the molten droplet is transported to the molten pool by electromagnetic force, gravity, etc. This phenomenon occurs continuously as the welding torch 2 or the base metal 3 moves, causing the molten pool to solidify behind the weld line, forming a weld bead 6. This achieves the joining of at least two steel sheets. The solidified molten pool is the weld metal.
[0023] Figure 1-2 is a diagram showing the welding target position in Figure 1-1. The welding target position is the intersection of the welding wire 1 and the base material 3, which is the end of the upper sheet of the two steel sheets, and is a corner of the overlapping portion 19 formed by the two steel sheets. The welding target position is determined as a target line 20 a predetermined distance away from the starting point of the overlapping portion corner 19.
[0024] Fig. 1-3 is a diagram showing a cross section of a weld bead. Welding is performed while ensuring a predetermined weld metal height (H) 25, weld metal width (W) 26, and flank angle (θ) 27 in the weld bead 6 (weld portion). The details of the above will be described later.
[0025] On the other hand, when conventional MIG welding is performed on carbon steel, which is the subject of the present invention, there is a problem that the welding is extremely unstable. MAG welding or MIG welding is a reverse polarity welding in which the electrode (wire) is the anode, so cathode spots are formed starting from areas on the surface of the base steel sheet that have a low work function like oxides and are prone to electron emission. For example, in an aluminum alloy that has a strong oxide film on the surface of the base material, cathode spots are stably formed starting from the oxide film on the weld line, making good welding possible. However, in steel that is difficult to form an oxide film, the O 2 or CO 2 In MIG welding, which does not produce oxides derived from the metal, the cathode spot is not fixed and moves around vigorously on the surface of the base material in search of a location with a low work function, which results in unstable welding and a welded joint with a meandering or wavy weld bead 6.
[0026] Regarding this phenomenon, the inventors observed the arc behavior in welding experiments and concluded that the main cause of the meandering and wavy shape of the weld bead, which was cited as a problem in MIG welding of carbon steel, was unstable metal transfer. Figures 2(a) and 2(b) show schematic diagrams explaining droplet transfer in conventional MIG welding. In conventional MIG welding, droplet transfer involves a mixture of two modes: the welding wire 1 melts and is transported continuously from a long, thin liquid column to the molten pool 8, as shown in Figure 2(a). In order to suppress this unstable droplet transfer, it is considered effective to regularly separate droplets 7 from the tip of the welding wire 1, but in the case of Ar shielding gas, the electromagnetic pinch force acting on the welding wire 1 is small, making it difficult for droplets 7 to detach.
[0027] Therefore, in the present invention, it has been discovered that, as a means for stabilizing the droplet transfer, it is effective to regularly repeat the non-short-circuit state of FIG. 3(a) and the short-circuit state of FIG. 3(b) between the tip of the welding wire 1 and the base metal 3, and to complete the joining by so-called periodic short-circuit transfer, in which the droplet 7 is transferred to the base metal 3 during the short-circuit state.
[0028] Gas containing 98% or more Ar by volume In order to improve the corrosion resistance of the welded portion, it is necessary to suppress the amount of slag produced that adheres to the welded portion, and for this purpose, it is important to suppress the oxidation of Si, Mn, Ti, and the like contained in the steel sheet and the welding wire 1. For this reason, it is necessary to use a gas containing 98% or more by volume of Ar as the shielding gas. It is preferable to use 99% or more by volume of Ar. There is no particular upper limit, and Ar may be 100% by volume.
[0029] 0.2 ≦ H / W ≦ 1.2 (1) As shown in FIG. 1-3, 25 is the weld metal height (H), 26 is the weld metal width (W), and 27 is the flank angle (θ). By defining the relationship between the weld metal height (H) 25 and the weld metal width (W) 26 within the range of the above formula (1), a weld bead 6 with a smooth toe shape can be obtained. If H / W is less than 0.2, the heat input is dispersed over a wide range, so that the upper sheet end is difficult to melt, and undercut occurs, or the penetration of the lower sheet may be insufficient. Therefore, H / W is set to 0.2 or more. Preferably, H / W is 0.25 or more, more preferably 0.3 or more, and even more preferably 0.35 or more. If H / W is more than 1.2, the weld bead 6 becomes convex and the flank angle 27 becomes excessively small. Therefore, H / W is set to 1.2 or less. Preferably, H / W is 1.1 or less, more preferably 1.0 or less, and even more preferably 0.9 or less. The units of H and W are both mm.
[0030] The molten metal height (H) and weld metal width (W) are measured according to the following method. The molten metal height (H) 25 and weld metal width (W) 26 were measured on a cross section in the plate thickness direction perpendicular to the weld line at five arbitrary points of the weld bead 6 in an area excluding the bead start and end portions 10 (each 15 mm long) of the weld bead 6 shown in FIG. 6, as described below. However, the arbitrary five points were located at positions 5 mm or more apart from each other. Here, the weld bead 6 was cut at arbitrary points in the plate thickness direction perpendicular to the weld line, and the molten metal height 25 and weld metal width 26 of each were found, and their average values were taken as the "molten metal height (H)" and the "weld metal width (W)." Although not particularly limited, it is preferable that the molten metal height (H) is such that, when the thickness of the upper plate is T (mm), H / T is 0.8 or more. More preferably, H / T is 0.9 or more. It is preferable that the upper limit of H / T is 1.8 or less. More preferably, H / T is 1.6 or less. It is preferable that the weld metal width (W) is such that, when the thickness of the upper plate is T (mm), W / T is 1.5 or more. More preferably, W / T is 1.6 or more. It is preferable that the upper limit of W / T is 3.0 or less. More preferably, W / T is 2.8 or less.
[0031] The welding target position is the end of the upper sheet of the two steel sheets, and is located between 0.2 mm and 1.8 mm from the overlap corner, which is the corner of the two steel sheets, in the direction perpendicular to the weld line of the lower sheet. The welding target position in the present invention is a point where an extension line of the welding wire 1 intersects with the base material 3 as shown in FIG. 1-2. By shifting the target position from the overlap corner 19 in a direction perpendicular to the weld line of the lower plate (hereinafter, also referred to as offsetting, the direction is referred to as offset direction 21, and the amount is referred to as offset value 22), the weld metal width 26 can be increased and the weld metal height 25 can be reduced even in gas-shielded arc welding with a high Ar ratio in which the surface tension of the molten metal is increased, and 0.2≦H / W≦1.2 can be satisfied. In other words, when the offset value 22 is less than 0.2 mm, the welding region is limited to a narrow range, so that the weld bead tends to be convex, and H / W may be excessive. For this reason, the offset value 22 is set to 0.2 mm or more, that is, the welding target position is set to 0.2 mm or more in a direction perpendicular to the weld line of the lower plate from the overlap corner. The offset value 22 is preferably 0.3 mm or more, more preferably 0.4 mm or more, and even more preferably 0.5 mm or more. On the other hand, if the offset value 22 is greater than 1.8 mm, the current path at the overlap corner becomes unstable, causing the arc plasma to fluctuate more, making stable welding difficult. In addition, there is concern that the amount of slag may increase due to air entrainment. For this reason, the offset value 22 is set to 1.8 mm or less, that is, the welding target position is set to 1.8 mm or less in the direction perpendicular to the weld line of the lower sheet from the overlap corner. The offset value 22 is preferably 1.7 mm or less, more preferably 1.6 mm or less, and even more preferably 1.5 mm or less.
[0032] Pulse peak current (Ip) is 300A or more and 600A or less (optimal condition) FIG. 4 shows a schematic diagram of a pulse current waveform in the arc welding of the present invention. Pulse welding is a method in which a pulse peak current (Ip) and a pulse base current (Ib) are periodically repeated to perform welding. If the pulse peak current (Ip) is too small, the droplet 7 formed at the tip of the welding wire 1 cannot be pushed down to the molten pool 8, and the short circuit may become unstable, or sufficient heat input may not be ensured, resulting in deterioration of the bead shape. Therefore, the pulse peak current (Ip) is preferably 300 A or more. More preferably, it is 350 A or more. Even more preferably, it is 380 A or more. Most preferably, it is 400 A or more. On the other hand, if it is too large, it causes burn-through and increases spatter. Therefore, the pulse peak current (Ip) is preferably 600 A or less. More preferably, it is 590 A or less. Even more preferably, it is 580 A or less. Most preferably, it is 570 A or less. Since a short circuit occurs during the pulse peak current, the pulse peak current time (tp) per cycle is preferably 0.5 ms or more. The pulse peak current time (tp) per cycle is more preferably 0.7 ms or more, and even more preferably 0.8 ms or more. If the pulse peak current time (tp) per cycle is too large, the arc 5 and molten pool 8 may become too turbulent during a short circuit, which may result in poor weld bead shape, so the pulse peak current time (tp) per cycle is desirably 3.5 ms or less. The pulse peak current time (tp) per cycle is more preferably 3.3 ms or less, and even more preferably 3.2 ms or less.
[0033] If the pulse base current (Ib) is too small, the arc discharge during the pulse base period becomes unstable, causing deterioration of the bead shape and insufficient penetration. For this reason, the pulse base current (Ib) is preferably 30 A or more. The pulse base current (Ib) is more preferably 35 A or more. Even more preferably 40 A or more, and most preferably 45 A or more. On the other hand, if it is too large, burn-through occurs, and the difference between the pulse peak current (Ip) and the pulse base current (Ib) cannot be sufficiently secured, and the effect of pushing down the droplet 7 formed at the tip of the welding wire 1 to the molten pool 8 and short-circuiting it cannot be obtained sufficiently, and the welding may not be stable. For this reason, the pulse base current (Ib) is preferably 120 A or less. The pulse base current (Ib) is more preferably 110 A or less. The pulse base current (Ib) is further preferably 100 A or less, and most preferably 90 A or less. If the pulse base current time (tb) per cycle is too short, the droplet 7 cannot grow to the ideal size, and periodic short circuiting may not be realized. Therefore, the pulse base current time (tb) per cycle is preferably 1.0 ms or more. The pulse base current time (tb) per cycle is more preferably 1.5 ms or more, even more preferably 2.0 ms or more, and most preferably 2.5 ms or more. If the pulse base current time (tb) per cycle is too long, the short circuit may not be controlled as intended at the pulse peak, or the arc 5 and molten pool 8 may become significantly disturbed during the short circuit. Therefore, the pulse base current time (tb) per cycle is preferably 10.0 ms or less. The pulse base current time (tb) per cycle is more preferably 9.0 ms or less, even more preferably 8.5 ms or less, and most preferably 8.0 ms or less. In addition, if the rise time (tup) and fall time (tdown) are too small, it will induce wobbling of the arc 5, and if they are too large, it will cause deterioration of the bead shape, so it is preferable that they are each 0.1 to 3.0 ms. That is, it is preferable that tup is 0.1 ms or more. It is more preferable that it is 0.3 ms or more, and even more preferable that it is 0.4 ms or more. It is most preferable that it is 0.5 ms or more. It is preferable that tdown is 3.0 ms or less.More preferably, it is 2.8 ms or less, further preferably, it is 2.6 ms or less, and most preferably, it is 2.5 ms or less.
[0034] Pulse frequency is 30Hz or more and 200Hz or less (optimal condition) By setting the pulse frequency within the above range, the movement of the droplet 7 can be stabilized and the deposition amount can be made uniform, thereby making it possible to obtain a stable and appropriate flank angle 27. If the pulse frequency is less than 30 Hz, the short circuit transfer period becomes large, and large droplets 7 move to the molten pool 8, or droplet transfer modes other than short circuit transfer (such as streaming transfer) are irregularly mixed. Therefore, the pulse frequency is preferably 30 Hz or more. The pulse frequency is more preferably 40 Hz or more, and even more preferably 50 Hz or more. On the other hand, if the pulse frequency is more than 200 Hz, although the droplets 7 are small, the arc 5 is excessively re-ignited due to short circuit, and the arc 5 becomes unstable. Therefore, the pulse frequency is preferably 200 Hz or less. The pulse frequency is more preferably 180 Hz or less, and even more preferably 160 Hz or less.
[0035] When the welding speed is high, it is difficult to keep the deposition amount constant, and it is difficult to control a continuous and stable weld bead shape, which may induce welding defects such as undercut. The above phenomenon becomes particularly noticeable under welding conditions of 200 cm / min or more, and it becomes necessary to limit the welding speed to the contents described below. Therefore, the welding speed is preferably 200 cm / min or less. More preferably, it is 160 cm / min or less, and even more preferably, it is 120 cm / min or less. On the other hand, when the welding speed is low, the heat input and deposition amount become excessive, and burn-through may occur. Therefore, the welding speed is preferably 20 cm / min or more. More preferably, it is 30 cm / min or more, and even more preferably, it is 40 cm / min or more.
[0036] The average frequency (short circuit frequency) F (Hz) of the short circuit transfer affects the volume of the droplet 7 at the end of the welding wire 1, and is not particularly limited, but is preferably 20 Hz or more. The average frequency (short circuit frequency) F (Hz) of the short circuit transfer is more preferably 30 Hz or more, and even more preferably 40 Hz or more. As an upper limit, the average frequency (short circuit frequency) F (Hz) of the short circuit transfer is preferably 200 Hz or less. More preferably, it is 180 Hz or less, and even more preferably, it is 150 Hz or less. Specifically, the short circuit frequency refers to the number of occurrences per unit time of the phenomenon (short circuit phenomenon) in which the droplet 7 at the tip of the wire comes into contact with the molten pool 8 and the arc 5 is extinguished. The average frequency (short circuit frequency) F (Hz) of the short circuit transfer can be measured, for example, by monitoring the transition of the arc voltage during welding with an oscilloscope, counting the number of times it becomes zero, and dividing the count number by the monitoring time to obtain the number of counts per second. If the monitoring time is too short, the variation in the count number becomes large, so it is preferable to set the monitoring time to 0.5 s or more. The monitoring time is more preferably 0.8 s or more, and even more preferably 1.0 s or more. There is no particular upper limit, but it is preferably 3.0 s or less because a large amount of measurement data requires a lot of time for counting and reduces workability. For example, when measuring the short circuit frequency in-process and performing feedback control of the welding conditions, if the monitoring time is too long, it becomes difficult to perform instantaneous feedback control according to the welding situation.
[0037] In addition, when one short circuit occurs per pulse period, the average frequency of the short circuit transition (short circuit frequency) F (Hz) will be the same as the pulse frequency described above, but the short circuit period does not necessarily need to be synchronized with the pulse period, and the average frequency of the short circuit transition (short circuit frequency) F (Hz) may differ from the pulse frequency.
[0038] In addition, the preferable range of the welding conditions is, for example, a welding current of 150A to 300A, an arc voltage of 20V to 35V, a distance between the base metal and the tip (contact tip) of 5mm to 30mm, and an Ar shielding gas flow rate of 10L / min to 25L / min. That is, the welding current is preferably 150A or more. More preferably, it is 170A or more, and more preferably, it is 180A or more. The welding current is preferably 300A or less. More preferably, it is 280A or less, and more preferably, it is 270A or less. The arc voltage is preferably 20V or more. More preferably, it is 21V or more, and more preferably, it is 22V or more. The arc voltage is preferably 35V or less. More preferably, it is 32V or less, and more preferably, it is 30V or less. The distance between the base metal 3 and the contact tip is preferably 5mm or more. More preferably, it is 8mm or more, and more preferably, it is 10mm or more. The distance between the base metal 3 and the contact tip is preferably 30mm or less. More preferably, it is 25mm or less, and more preferably, it is 20mm or less. It is preferable that the Ar shielding gas flow rate is 10 L / min or more. More preferably, it is 12 L / min or more, and even more preferably, it is 15 L / min or more. It is preferable that the Ar shielding gas flow rate is 25 L / min or less. More preferably, it is 24 L / min or less, and even more preferably, it is 22 L / min or less. The welding current and arc voltage are average values in each welding pass, and more specifically, the welding current is the average value of the pulse peak current and the pulse base current. By managing this, it is possible to grasp the total heat input during welding. The contact tip is attached inside the welding torch, and serves to supply power to the welding wire 1 and to guide the wire feed.
[0039] The welding wire used in the present invention is not particularly limited. For example, a solid wire such as YGW12 or YGW16 described in JIS Z 3312 can be used.
[0040] The base material 3 of the present invention is intended for steel sheets and plated steel sheets. The composition of the steel sheets is not particularly limited, but for example, a steel sheet containing C: 0.02 mass% to 0.3 mass%, Si: 0.01 mass% or more, Mn: 0.5% mass% or more, P: 0.05 mass% or less, and S: 0.05 mass% or less is preferable, and other alloy elements such as Cu, Ni, Cr, and Ti may be contained. In the above steel sheets, Si is preferably 3.0 mass% or less, and Mn is preferably 5.0 mass% or less. The lower limit of P is not particularly limited, but is preferably 0.0005 mass% or more, and the lower limit of S is not particularly limited, but is preferably 0.0005 mass% or more. The plating composition of the plated steel sheets is not particularly limited, but for example, Zn can be mentioned.
[0041] By using the lap fillet arc welding method limited as described above, it is possible to suppress the generation of slag in the welded portion and to manufacture a welded joint having a good bead shape, and it is possible to obtain the welded joint. In addition to the above, the present invention is also characterized by its high robustness, which is a useful feature. Note that high robustness means that the method is less susceptible to disturbances such as the environment and plate shape, and that the suitable welding conditions are wide. EXAMPLES
[0042] Examples of the present invention will be described below. Two steel plates (each with a thickness of 2.6 mm) having the components shown in Table 1 were stacked together, and fillet welding was performed, for example, by the method shown in FIG. 1-1. Components other than those shown in Table 1 include Fe and alloy elements such as Ni, Cr, Ti, and Mo. Welding was performed under the welding conditions shown in Table 2. YGW16 described in JIS Z 3312 was used as the welding wire.
[0043] The welded steel plate obtained as described above was subjected to the following test method to measure the slab coverage ratio (S RATIO ), flank angle (θ) and the presence or absence of undercut were evaluated.
[0044] (Slag coverage area rate) FIG. 5 is a schematic diagram showing the bead area and the slag-covered area in a weld bead. The bead surface area S BEAD and the slag covering surface area S SLAG is calculated by photographing the surface of the area excluding the bead start and end portions 10 of the weld bead 6 (each 15 mm long) from directly above and measuring the projected areas from the top of the weld bead 6 and slag. If the length of the weld bead 6 is less than 130 mm, the entire surface length excluding the bead start and end portions 10 is photographed. If the length of the weld bead 6 is 130 mm or more, the surface of any portion (100 mm long) excluding the bead start and end portions 10 is photographed. The calculated slag surface area S SLAG The value of the bead surface area S BEAD The slag coverage area ratio S RATIO S RATIO A passing grade was 30% or less.
[0045] (Flank angle) The flank angle (θ) 27 was measured by observing a cross section in the plate thickness direction perpendicular to the weld line (parallel to the line AA in FIG. 5) at five arbitrary points of the weld bead 6 as shown in FIG. 1-3 in an area excluding the bead start and end portions 10 (each 15 mm long). However, the five arbitrary points were positioned at least 5 mm apart from each other. Here, the weld bead was cut at arbitrary points in the plate thickness direction perpendicular to the weld line, and each flank angle 27 was found, and the average value was taken as the "flank angle θ (°)". A θ of 95° or more was considered to be acceptable.
[0046] (Evaluation of the presence or absence of undercuts) The presence or absence of undercut was determined based on the definition described in JIS Z 3001-4 by visually confirming that there was no undercut (weld defect) at the end of weld bead 6 in the area excluding the bead start and end portions 10 (each 15 mm long) of weld bead 6.
[0047] In addition, "S RATIO is 30% or less, θ is 110° or more, and there is no undercut. RATIOis 30% or less, θ is 95° or more and less than 110°, and there is no undercut. RATIO The evaluation was given an F (fail) when at least one of the following conditions was satisfied: θ is greater than 30%, θ is less than 95°, and there is an undercut.
[0048] From Table 2, the welding conditions No. 1 to No. 9, which are examples of the invention, are S RATIO The requirements of θ being 30% or less, θ being 95° or more, and no undercut were met, and a good weld joint shape was obtained while suppressing slag.
[0049] In the welding conditions Nos. 1 to 3, 5, and 6 of the above-mentioned invention examples, θ was 110° or more, and more stable welded joint shapes were obtained. In contrast, in the welding conditions Nos. 10 to 13, which are comparative examples, RATIO Any one of the following conditions was not satisfied: θ was 30% or less, θ was 95° or more, and there was no undercut. Therefore, a good weld bead was not obtained, and a good weld joint shape was not obtained.
[0050] [Table 1]
[0051] [Table 2] [Explanation of symbols]
[0052] 1 Welding wire 2. Welding torch 3 Base material 5. Arc 6 Weld Bead 7 droplets 8 Molten Pool 10 Bead start and end 19 Stacked Corner 20 Target Line 21 Offset direction 22 Offset Value 25 Weld metal height (H) 26 Weld metal width (W) 27 Flank angle (θ) tup Rise time tp Pulse peak current time tdown Fall time tb Pulse base current time tup+tp+tdown+tb Pulse 1 period S BEAD Bead Surface Area S SLAG Slag Coverage Surface Area W MAX Maximum bead width W min Bead width minimum
Claims
1. 1. A fillet arc welding method for joining a corner made of at least two steel sheets, comprising the steps of: a lap fillet arc welding method in which joining is performed using short-circuit transfer, a welding target position is an end portion of an upper sheet of the two steel sheets, and is 0.2 mm to 1.8 mm in a direction perpendicular to the weld line of the lower sheet, starting from a corner of the overlapping portion that is a corner formed by the two steel sheets, a gas containing 98 volume % or more of Ar is used as a shielding gas, and a weld metal height H (mm) and a weld metal width W (mm) of the weld portion satisfy the following formula (1): 0.2 ≦ H / W ≦ 1.2 ... (1)
2. 2. The lap fillet arc welding method according to claim 1, wherein pulse welding is performed in which a pulse peak current (Ip) and a pulse base current (Ib) are periodically repeated, and the pulse peak current (Ip) of the pulse welding is 300 A or more and 600 A or less, and the pulse frequency is 30 Hz or more and 200 Hz or less.
3. A method for manufacturing a welded joint using the lap fillet arc welding method according to claim 1 or 2.
4. A lap fillet arc welding method as described in claim 1 or 2, wherein the formula (1) satisfies 0.2 ≦ H / W ≦ 0.
9.
5. A lap fillet arc welding method as described in claim 1 or 2, wherein the weld metal width W (mm) is W / T of 1.5 or more when the plate thickness of the upper plate is T (mm).
6. A method for manufacturing a welded joint using the lap fillet arc welding method described in claim 4.
7. A method for manufacturing a welded joint using the lap fillet arc welding method described in claim 5.
Citation Information
Patent Citations
Ultrasonic combustion apparatus
JP1980049615A
Lap fillet welding method
JP1986144270A
Gas shielded metal arc welding method which enhances corrosion resistance after coating of weld zone and near this zone
JP1996033997A
Improvement of corrosion resistance after coating in arc weld zone and its vicinity
JP1997020994A
MIG welding method
WO2021085544A1