Martensitic stainless steel seamless pipe
The seamless martensitic stainless steel pipe addresses corrosion and toughness issues by optimizing element composition and microstructure, ensuring high strength and resistance to low temperatures and corrosive environments.
Patent Information
- Application Number
- JP2024538747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Martensitic stainless steel pipes used in oil country tubular goods and CCS injection pipes face challenges with insufficient corrosion resistance and low-temperature toughness, particularly in environments with carbon dioxide and chloride ions at high temperatures and pressures, and require improved strength and toughness to withstand pressure drops and maintain ductility.
A seamless martensitic stainless steel pipe composition with specific ranges of elements such as Ni (6-9%), Cr (15.0-17.5%), and controlled relational expressions to ensure high strength, low-temperature toughness, and corrosion resistance, including a microstructure predominantly composed of martensite with optional retained austenite and ferrite phases.
The solution provides a seamless martensitic stainless steel pipe with yield stress of 758 MPa or more, absorbed energy of 100 J or more at -80°C, and excellent corrosion resistance, suitable for CCS press-fit pipes and oil country tubular applications.
Smart Images

Figure 0007574975000001 
Figure 0007574975000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a martensitic stainless steel seamless pipe. [Background technology]
[0002] In conventional oil and gas fields, martensitic stainless steel pipes such as 13% Cr steel (steel containing about 13% by mass of Cr) and 17% Cr steel (steel containing about 17% by mass of Cr) are widely used as oil well tubular goods for mining. In recent years, carbon capture and storage (CCS) technology has been promoted worldwide in order to achieve carbon neutrality. In CCS, martensitic stainless steel pipes are also used for injection pipes (hereinafter referred to as CCS injection pipes) when injecting captured carbon dioxide into aquifers or depleted oil fields.
[0003] Oil well tubular goods and CCS injection pipes are steel pipes that are connected to depths of several thousand meters underground, so they must be strong enough to withstand their own weight. In addition, both oil well tubular goods and CCS injection pipes must be corrosion resistant in environments where high-temperature, high-pressure carbon dioxide and chloride ions are present. In particular, with CCS, carbon dioxide containing highly corrosive impurities such as oxygen, sulfur oxides, and nitrogen oxides may be injected, so the material for the CCS injection pipes must be highly corrosion resistant.
[0004] In addition, when oil well tubular goods and CCS injection pipes are used in cold regions, they need to be able to withstand low temperatures without becoming brittle, and so low-temperature toughness is required. In particular, with CCS injection pipes, the pressure of the fluid passing through the steel pipe is high, so there is concern that if a sudden drop in pressure occurs due to a leak or other reason, the temperature will drop due to the Joule-Thomson effect. For this reason, toughness at even lower temperatures may be required.
[0005] Patent Document 1 proposes a seamless steel pipe with high strength and high toughness, having a composition with a Cr content of 14 mass% or less. Patent Documents 2 to 4 propose seamless steel pipes with high strength, high toughness and high corrosion resistance, having a composition with a Cr content of about 17 mass% and a Ni content of 6.0 mass% or less, and a structure containing a certain amount of ferrite phase. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2009 / 004741 [Patent Document 2] JP 2017-14543 A [Patent Document 3] International Publication No. 2019 / 035329 [Patent Document 4] International Publication No. 2020 / 202957 Summary of the Invention [Problem to be solved by the invention]
[0007] In the technology described in Patent Document 1, a corrosion test is conducted for one week in a 20 mass % NaCl aqueous solution at a liquid temperature of 80°C and in a CO atmosphere at 30 atmospheres. However, it may not be said that the corrosion resistance is sufficient in the more severe corrosive environments of oil country tubular goods and CCS injection pipes.
[0008] In Patent Documents 2 and 3, excellent low-temperature toughness is defined as an absorbed energy of 80 J or more at -60°C and an absorbed energy of 40 J or more at -40°C in a Charpy impact test, respectively. In addition, in Patent Document 4, excellent low-temperature toughness is defined as an absorbed energy of 300 J or more at -10°C in a Charpy impact test and a ductile-brittle transition temperature of -40°C or less. However, in applications for CCS press-in pipes, the usage environment may be -60°C or less, so toughness at even lower temperatures may be required.
[0009] Thus, martensitic stainless steels containing about 13 mass% Cr can provide high strength and toughness, but may not have sufficient corrosion resistance.On the other hand, martensitic stainless steels containing about 17 mass% Cr, which have relatively high corrosion resistance, have the problem of reduced low-temperature toughness due to the inclusion of a ferrite phase.
[0010] An object of the present invention is to provide a martensitic stainless steel seamless pipe having a yield stress of 758 MPa or more, an absorbed energy of 100 J or more in a Charpy impact test at -80°C, and excellent corrosion resistance.
[0011] In the present invention, "having excellent corrosion resistance" means that the corrosion rate of a test piece when immersed in a 20 mass % NaCl aqueous solution at 200°C for 336 hours in a CO2 gas atmosphere at 30 atmospheres is 0.127 mm / y or less. [Means for solving the problem]
[0012] In order to achieve the above-mentioned object, the present inventors have intensively studied the components of martensitic stainless steel that achieves both high strength, high toughness, and high corrosion resistance. As a result, it has been revealed that by increasing Ni to 6 to 9 mass% and reducing the ferrite phase compared to conventional 17% Cr steel, it is possible to obtain toughness at lower temperatures while maintaining high corrosion resistance. However, if the content of alloys such as Cr and Ni increases, the Ms point, which is the temperature at which martensitic transformation begins, drops to room temperature or lower, and there is a risk that sufficient strength cannot be obtained even if quenching is performed. Therefore, it has been found that a martensitic stainless steel seamless steel pipe having the desired strength, excellent low-temperature toughness, and excellent corrosion resistance can be obtained by defining C, Cu, Ni, Cr, Mo, Nb, N, and W by an appropriate relational expression and further adjusting the composition so that the value calculated by the relational expression satisfies a predetermined range.
[0013] The present invention was completed based on these findings and further investigations. [1] In mass percent, C: 0.005~0.100%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0-9.0%, Cr: 15.0-17.5%, Al: 0.001 to 0.10%, Nb: 0.001 to 0.20%, N: 0.1% or less, O: 0.01% or less, Cu:3.5% or less, Mo: less than 1.0%, and W: 1.0% or less and the balance being Fe and unavoidable impurities, and having a chemical composition that satisfies the following formulas (1) and (2): 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W> 50.00...(1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C> 20.00 ···(2) Here, each element symbol in formula (1) and formula (2) indicates the content (mass%) of the corresponding element, and when the element is not contained, it is set to 0. [2] The composition further includes, in mass%, Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less The martensitic stainless steel seamless pipe according to [1], which contains one or more selected from the following: [3] A martensitic stainless steel seamless pipe according to [1] or [2], having a yield strength of 758 MPa or more and an absorbed energy of 100 J or more in a Charpy impact test at -80°C. Effect of the Invention
[0014] According to the present invention, it is possible to provide a martensitic stainless steel seamless pipe having a yield stress of 758 MPa or more, an absorbed energy of 100 J or more in a Charpy impact test at -80°C, and excellent corrosion resistance.
[0015] According to the present invention, it has become possible to use martensitic stainless steel seamless pipes for CCS press-in pipe applications, which require superior low-temperature toughness and high corrosion resistance compared to conventional oil well tubular goods applications. Furthermore, according to the present invention, it is possible to provide martensitic stainless steel seamless pipes that are less expensive and have superior toughness even for applications in which duplex stainless steels such as 25% Cr steel are used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The martensitic stainless steel seamless pipe of the present invention (hereinafter also simply referred to as the seamless steel pipe of the present invention) contains, by mass%, C: 0.005 to 0.100%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0 to 9.0%, Cr: 15.0 to 17.5%, Al: 0.001 to 0.10%, Nb: 0.001 to 0.20%, N: 0.1% or less, O: 0.01% or less, Cu: 3.5% or less, Mo: less than 1.0%, and W: 1.0% or less, with the balance being Fe and unavoidable impurities, and has a component composition that satisfies the following formulas (1) and (2). 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W> 50.00...(1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C> 20.00 ···(2) Here, each element symbol in the above formula (1) and formula (2) indicates the content (mass %) of the corresponding element, and when the element is not contained, it is set to 0.
[0017] The reasons for limiting the chemical composition of the seamless steel pipe of the present invention will be explained below. Note that hereinafter, unless otherwise specified, mass% will simply be abbreviated as %.
[0018] C: 0.005 to 0.100% C improves hardenability and increases the strength of steel. To obtain this effect, the C content is set to 0.005% or more. On the other hand, if the C content is too high, the Ms point decreases, martensitic transformation does not occur at room temperature, and strength cannot be ensured. Therefore, the C content is set to 0.100% or less. The C content is preferably 0.007% or more. In addition, the C content is preferably 0.050% or less, more preferably 0.030% or less, and further preferably 0.020% or less.
[0019] Silicon: 0.05 to 1.00% Si acts as a deoxidizer. To obtain this effect, the Si content is set to 0.05% or more. On the other hand, if the Si content exceeds 1.00%, the corrosion resistance and hot workability are reduced due to the precipitation of δ-ferrite. Therefore, the Si content is set to 1.00% or less. The Si content is preferably 0.50% or less. On the other hand, from the viewpoint of ensuring stable strength, the Si content is preferably 0.10% or more.
[0020] Mn: 0.05 to 1.00% Mn is an element that improves hot workability and strength. To obtain this effect, the Mn content is set to 0.05% or more. On the other hand, excessive Mn content causes MnS to precipitate, which reduces the resistance to sulfide stress corrosion cracking. Therefore, the Mn content is set to 1.00% or less. The Mn content is preferably 0.50% or less. Moreover, the Mn content is preferably 0.10% or more.
[0021] P:0.05% or less P is an impurity that is inevitably contained. P is an element that reduces corrosion resistance, and in the present invention, it is desirable to reduce it as much as possible. However, an extreme reduction in P increases production costs. Therefore, the P content is limited to 0.05% or less as a range that does not cause an extreme decrease in characteristics and is industrially feasible at low cost. The P content is preferably 0.03% or less. In addition, although there is no particular lower limit for the P content, since excessive de-P increases production costs, from the viewpoint of production costs, the P content is preferably 0.005% or more.
[0022] S: 0.005% or less S is an impurity that is inevitably contained. Since S is an element that significantly reduces hot workability, it is desirable to reduce it as much as possible. By reducing the S content to 0.005% or less, pipe manufacturing by the Mannesmann method becomes possible, so the S content in the present invention is limited to 0.005% or less. The S content is preferably 0.002% or less. In addition, although there is no particular limit to the lower limit of the S content, since excessive de-S leads to an increase in manufacturing costs, from the viewpoint of manufacturing costs, the S content is preferably 0.0005% or more.
[0023] Ni: 6.0~9.0% Ni is an element that strengthens the protective film to improve corrosion resistance, and further increases the strength of steel by dissolving in solid solution. In addition, since Ni is an element that stabilizes the austenite phase at the quenching temperature, the Ni content is set to 6.0% or more. If the Ni content is less than 6.0%, the amount of ferrite increases and the toughness decreases. On the other hand, if the Ni content exceeds 9.0%, the Ms point decreases and the strength decreases. Therefore, the Ni content is limited to 6.0 to 9.0%. The Ni content is preferably 6.5% or more. In addition, the Ni content is preferably 8.0% or less, and more preferably 7.5% or less.
[0024] Cr: 15.0~17.5% Cr is an element that forms a protective film to improve corrosion resistance, and a content of 15.0% or more can provide the desired corrosion resistance. On the other hand, if Cr is contained in excess of 17.5%, the Ms point decreases and the amount of ferrite increases, making it impossible to achieve both strength and low-temperature toughness. Therefore, the Cr content is limited to 15.0 to 17.5%. The Cr content is preferably 15.5% or more, and more preferably 16.0% or more. The Cr content is preferably 17.0% or less.
[0025] Al: 0.001 to 0.10% Al acts as a deoxidizer. To obtain this effect, the Al content is set to 0.001% or more. However, an Al content exceeding 0.10% adversely affects toughness due to the precipitation of excess oxides, so the Al content in the present invention is limited to 0.10% or less. The Al content is preferably 0.01% or more. The Al content is preferably 0.04% or less.
[0026] Nb: 0.001 to 0.20% Nb can form carbides, thereby reducing solute carbon and improving the Ms point. To obtain this effect, the Nb content is set to 0.001% or more. On the other hand, if the Nb content exceeds 0.20%, coarse carbides may precipitate, lowering toughness. Therefore, the Nb content is set to 0.20% or less. The Nb content is preferably 0.01% or more. The Nb content is preferably 0.10% or less.
[0027] N: 0.1% or less N is an impurity that is inevitably contained. N has the effect of dissolving in steel and increasing strength. However, if the N content exceeds 0.1%, various nitride-based inclusions are generated in large amounts, and corrosion resistance decreases. Therefore, the N content in the present invention is limited to 0.1% or less. The N content is preferably 0.005% or more. The N content is preferably 0.05% or less, and more preferably 0.03% or less.
[0028] O: 0.01% or less O is an impurity that is inevitably contained. Since O exists as an oxide in steel, it adversely affects various properties. Therefore, in the present invention, it is desirable to reduce it as much as possible. In particular, if the O content exceeds 0.01%, the hot workability, corrosion resistance, and toughness decrease. Therefore, the O content is set to 0.01% or less. The O content is preferably 0.005% or less. There is no particular lower limit for the O content, but since excessive de-O leads to an increase in manufacturing costs, from the viewpoint of manufacturing costs, the O content is preferably 0.001% or more.
[0029] Cu:3.5% or less Cu strengthens the protective coating and improves corrosion resistance. However, a Cu content exceeding 3.5% reduces hot workability due to precipitation of metallic Cu. Therefore, the Cu content is set to 3.5% or less. The Cu content is preferably 3.0% or less. The seamless steel pipe of the present invention does not necessarily need to contain Cu. The Cu content is preferably 0.5% or more.
[0030] Mo: Less than 1.0% Mo is an element that improves corrosion resistance. On the other hand, excessive Mo content of 1.0% or more leads to a decrease in the Ms point, which reduces hardenability and makes ferrite more likely to form, thereby reducing toughness. For this reason, the Mo content is limited to less than 1.0% in the present invention. The Mo content is preferably 0.8% or less. The seamless steel pipe of the present invention does not necessarily need to contain Mo. The Mo content is preferably 0.1% or more.
[0031] W: 1.0% or less W is an element that improves corrosion resistance. On the other hand, an excessive W content of more than 1.0% leads to a decrease in the Ms point, so in the present invention, the W content is limited to 1.0% or less. The W content is preferably 0.8% or less. The seamless steel pipe of the present invention does not need to contain W. The W content is preferably 0.1% or more.
[0032] The chemical composition of the seamless steel pipe of the present invention further contains each element so as to satisfy the following formula (1). 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W> 50.00...(1) Here, each element symbol in formula (1) indicates the content (mass%) of the corresponding element, and when the element is not contained, it is set to 0. Formula (1) is a formula that correlates with the Ms point, and when the value calculated on the left side of formula (1) is more than 50.00, martensitic transformation occurs even when cooled to room temperature, and sufficient strength can be ensured. Therefore, the value calculated on the left side of formula (1) is set to more than 50.00. The value calculated on the left side of formula (1) is preferably 55.00 or more. In addition, the value calculated on the left side of formula (1) is preferably 300.00 or less.
[0033] The chemical composition of the seamless steel pipe of the present invention further contains each element so as to satisfy the following formula (2). Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C> 20.00 ···(2) Here, each element symbol in formula (2) indicates the content (mass%) of the corresponding element, and when the element is not contained, it is set to 0. Equation (2) is an equation related to corrosion resistance. When the value calculated on the left side of equation (2) exceeds 20.00, the corrosion rate of the test piece immersed in a 20 mass% NaCl aqueous solution at a liquid temperature of 200°C for 336 hours in a CO2 gas atmosphere at 30 atmospheres can be 0.127 mm / y or less. Therefore, the value calculated on the left side of equation (2) is set to exceed 20.00. The value calculated on the left side of equation (2) is preferably 20.50 or more, and more preferably 21.00 or more. In addition, since excessive alloy addition promotes the precipitation of intermetallic compounds, the value calculated on the left side of equation (2) is preferably 30.00 or less.
[0034] The balance other than the above components may be Fe and unavoidable impurities.
[0035] The composition of the seamless steel pipe of the present invention may further contain, as optional elements, one or more selected from Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less. The composition of the seamless steel pipe of the present invention may not contain these optional elements (it may be 0%).
[0036] Co: 1% or less Co is an element that enhances corrosion resistance and hardenability. On the other hand, a Co content of more than 1% reduces low-temperature toughness. Therefore, when Co is contained, the Co content is set to 1% or less. The Co content is preferably 0.5% or less. Furthermore, when Co is contained, the Co content is preferably 0.01% or more.
[0037] V: 0.1% or less V is an element that increases the strength of steel by precipitation strengthening. On the other hand, a V content of more than 0.1% reduces low-temperature toughness. Therefore, when V is contained, the V content is set to 0.1% or less. The V content is preferably 0.08% or less. Furthermore, when V is contained, the V content is preferably 0.01% or more.
[0038] Ti: 0.1% or less Ti is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Ti content of more than 0.1% reduces low-temperature toughness. Therefore, when Ti is contained, the Ti content is set to 0.1% or less. The Ti content is preferably 0.02% or less. Furthermore, when Ti is contained, the Ti content is preferably 0.001% or more.
[0039] Zr: 0.2% or less Zr is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Zr content of more than 0.2% reduces low-temperature toughness. Therefore, when Zr is contained, the Zr content is set to 0.2% or less. The Zr content is preferably 0.15% or less. Furthermore, when Zr is contained, the Zr content is preferably 0.01% or more.
[0040] Ta: 0.2% or less Ta is an element that forms carbonitrides and increases the strength and corrosion resistance of steel. On the other hand, a Ta content of more than 0.2% reduces low-temperature toughness. Therefore, when Ta is contained, the Ta content is set to 0.2% or less. The Ta content is preferably 0.15% or less. Furthermore, when Ta is contained, the Ta content is preferably 0.01% or more.
[0041] Hf: 0.2% or less Hf is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Hf content of more than 0.2% reduces low-temperature toughness. Therefore, when Hf is contained, the Hf content is set to 0.2% or less. The Hf content is preferably 0.15% or less. Furthermore, when Hf is contained, the Hf content is preferably 0.01% or more.
[0042] Ca: 0.01% or less Ca is an element that improves the hot workability of steel by fixing S in the steel as sulfides. On the other hand, a Ca content of more than 0.01% coarsens inclusions and reduces toughness and corrosion resistance. Therefore, when Ca is contained, the Ca content is set to 0.01% or less. The Ca content is preferably 0.005% or less. Furthermore, when Ca is contained, the Ca content is preferably 0.0001% or more.
[0043] REM: 0.01% or less REM (rare earth metal) is an element that improves the hot workability of steel by fixing S in the steel as sulfide. On the other hand, the content of REM exceeding 0.01% causes inclusions to become coarse, and reduces toughness and corrosion resistance. Therefore, when REM is contained, the REM content is set to 0.01% or less. The REM content is preferably 0.005% or less. Furthermore, when REM is contained, the REM content is preferably 0.0001% or more. In the present invention, REM refers to a collective term for 17 elements, including Sc with atomic number 21, Y with atomic number 39, and 15 elements from La with atomic number 57 to Lu with atomic number 71. Furthermore, the REM content refers to the total content of these elements.
[0044] Mg: 0.01% or less Mg is an element that improves the hot workability of steel by fixing S in the steel as sulfides. On the other hand, a Mg content of more than 0.01% coarsens inclusions and reduces toughness and corrosion resistance. Therefore, when Mg is contained, the Mg content is set to 0.01% or less. The Mg content is preferably 0.005% or less. Furthermore, when Mg is contained, the Mg content is preferably 0.0001% or more.
[0045] B: 0.01% or less B is an element that improves the hot workability of steel by suppressing segregation of S to grain boundaries in the steel. On the other hand, a B content of more than 0.01% forms coarse nitrides and reduces the toughness of the steel. Therefore, when B is contained, the B content is set to 0.01% or less. The B content is preferably 0.005% or less. Furthermore, when B is contained, the B content is preferably 0.0001% or more.
[0046] Sn: 0.2% or less Sn is an element that enhances the corrosion resistance of steel. On the other hand, a Sn content of more than 0.2% reduces the hot workability of steel. Therefore, when Sn is contained, the Sn content is set to 0.2% or less. The Sn content is preferably 0.1% or less. Furthermore, when Sn is contained, the Sn content is preferably 0.01% or more.
[0047] Sb: 0.2% or less Sb is an element that enhances the corrosion resistance of steel. On the other hand, an Sb content of more than 0.2% reduces the hot workability of steel. Therefore, when Sb is contained, the Sb content is set to 0.2% or less. The Sb content is preferably 0.1% or less. Furthermore, when Sb is contained, the Sb content is preferably 0.01% or more.
[0048] Next, a preferred method for manufacturing the seamless steel pipe of the present invention will be described. In the present invention, a steel pipe material having the above-mentioned composition is used, but the method for manufacturing the seamless steel pipe does not need to be particularly limited, and any known method for manufacturing a seamless steel pipe can be applied. It is preferable to melt the molten steel having the above-mentioned composition by a melting method such as a converter, and make a steel pipe material such as a billet by a method such as a continuous casting method or an ingot-making-blooming rolling method. Next, the steel pipe material is heated, and hot worked and pipe-made in a pipe-making process by the Mannesmann plug mill method or the Mannesmann mandrel mill method, which are known pipe-making methods, and then quenched and tempered to obtain a seamless steel pipe having the above-mentioned composition.
[0049] The microstructure of the seamless steel pipe of the present invention has martensite as the main phase. In this specification, having martensite as the main phase means that the volume fraction of martensite in the microstructure is 60% or more. The balance may be one or two selected from a volume fraction of 0 to 40% retained austenite and a volume fraction of 0 to 10% ferrite. The volume fraction of martensite is preferably 80% or more, and more preferably 90% or more. The microstructure of the seamless steel pipe of the present invention may be a single martensite phase.
[0050] The seamless steel pipe of the present invention preferably has a yield strength of 758 MPa or more. The yield strength is more preferably 792 MPa or more, and even more preferably 827 MPa or more. Although not particularly limited, as an example, the yield strength is 1034 MPa or less.
[0051] The seamless steel pipe of the present invention preferably has an absorbed energy of 100 J or more in a Charpy impact test at −80° C. The absorbed energy is preferably 150 J or more, and more preferably 180 J or more. EXAMPLES
[0052] 50 kg of molten steel having the composition shown in Table 1 was melted in a vacuum furnace, and an ingot was produced by ingot casting. The following process was then carried out to simulate the manufacturing process of martensitic stainless steel seamless steel pipes. That is, the ingot was heated at 1250°C for 60 minutes and rolled to a thickness of 105 mm. After that, it was heated again at 1250°C for 60 minutes and rolled to a thickness of 15 mm to produce a plate material. The plate material was heated at 1000°C for 20 minutes, quenched by water cooling to 25°C, and then heated at 570°C for 30 minutes, and tempered by air cooling to room temperature to obtain a test material (plate material).
[0053] Tensile Test A round bar tensile test specimen with a parallel section diameter of 6 mm and a parallel section length of 25 mm was taken from the center of the plate thickness of each test material (corresponding to the center of the plate thickness of a seamless steel pipe) in accordance with API regulations. The longitudinal direction of the parallel section of this test specimen was the rolling direction of the plate material. Using this test specimen, a tensile test was performed at room temperature (25°C) to determine the yield strength YS (MPa). Yield strength YS was defined as the 0.2% proof stress. A yield strength YS of 758 MPa or more was considered to have passed, and one less than 758 MPa was considered to have failed.
[0054] Impact Testing V-notch test pieces (full size) were taken from the center of each test material in the thickness direction so that the longitudinal direction of the test piece was perpendicular to the rolling direction, and a Charpy impact test was performed in accordance with the provisions of JIS Z 2242: 2018. The test temperature was -80°C, and those with absorbed energy of 100 J or more were considered to have passed, and those with absorbed energy of less than 100 J were considered to have failed.
[0055] Corrosion Resistance Test A 30mm x 40mm x 3mm test piece was taken from each test material. The test piece was immersed in a test liquid held in an autoclave: a 20% by mass NaCl aqueous solution (liquid temperature 200°C, CO2 gas atmosphere at 30 atm), and a corrosion test was performed for 336 hours. The weight of the test piece after the test was measured, and the corrosion rate was calculated from the weight difference before and after the corrosion test. A corrosion rate of 0.127mm / y or less was considered to be a pass, and a corrosion rate of more than 0.127mm / y was considered to be a fail.
[0056] Tissue observation A test piece for microstructure observation and a test piece for X-ray diffraction were taken from each test material at the center position of the plate thickness (corresponding to the center position of the wall thickness of a seamless steel pipe). The cross section of the test piece for microstructure observation perpendicular to the longitudinal direction (rolling direction) of the steel material was etched using a Villela etching solution. The cross section was then observed using an optical microscope at an appropriate magnification of 100 to 1000 times. The obtained image was analyzed to calculate the area ratio of the ferrite phase. This area ratio was considered to be the volume ratio of the ferrite phase. The volume ratio of the retained austenite phase was determined by chemically polishing the cross section of the test piece for X-ray diffraction perpendicular to the thickness direction of the steel material. A Co-Kα radiation source was used for the incident X-rays, and the area ratio of the retained austenite phase was calculated from the intensity ratio of the (200), (211) planes of ferrite to the (200), (220), and (311) planes of austenite. This area ratio was considered to be the volume ratio of the retained austenite phase. The results are shown in Table 2. In Table 2, the remainder other than the ferrite phase and the retained austenite phase is defined as the martensite phase. In the present invention, the martensite phase may contain a precipitate phase of 5% or less in volume fraction in addition to the ferrite phase and the retained austenite phase.
[0057] [Table 1]
[0058] [Table 2]
[0059] All of the examples of the present invention have high strength (yield strength YS: 758 MPa or more), high toughness (absorbed energy of 100 J or more in a Charpy impact test at -80°C), and low resistance to CO2, Cl - The samples had excellent corrosion resistance in a high-temperature corrosive environment containing ions at 200° C. On the other hand, the comparative examples outside the scope of the present invention did not achieve the desired values in at least one of the yield strength YS, absorbed energy in a Charpy impact test at -80° C., and corrosion resistance.
[0060] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. [Industrial Applicability]
[0061] The martensitic stainless steel seamless pipe of the present invention is useful as oil country tubular goods and CCS press-in pipes, which require high strength, excellent low-temperature toughness, and excellent corrosion resistance, and is particularly suitable as CCS press-in pipes.
Claims
1. In mass percent, C: 0.005-0.100%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0 to 9.0%, Cr: 15.0-17.5%, Al: 0.001-0.10%, Nb: 0.001-0.20%, N: 0.1% or less, O: 0.01% or less, Cu: 3.5% or less, Mo: less than 1.0%, and W: 1.0% or less and the balance being Fe and unavoidable impurities, and having a chemical composition that satisfies the following formulas (1) and (2): 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W> 50.00...(1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C> 20.00...(2) Here, each element symbol in formula (1) and formula (2) indicates the content (mass%) of the corresponding element, and when the element is not contained, it is set to 0.
2. The composition further includes, in mass%, Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less 2. The martensitic stainless steel seamless pipe according to claim 1, comprising one or more selected from the following:
3. 3. The martensitic stainless steel seamless pipe according to claim 1 or 2, having a yield strength of 758 MPa or more and an absorbed energy in a Charpy impact test at -80°C of 100 J or more.
Citation Information
Patent Citations
Martensitic welded stainless steel pipe and producing method therefor
JP2001179485A
High-strength stainless steel pipe superior in corrosion resistance for oil well
JP2005105357A
Stainless steel pipe for oil well excellent in enlarging characteristic and its production method
JP2007169776A
Cr-CONTAINING STEEL PIPE FOR MEMBER FOR CARBON DIOXIDE INJECTION
JP2011252222A
High-strength stainless steel seamless pipe for oil wells and method for manufacturing same
WO2023053743A1
Cited By
Low-cost ultrahigh-strength martensitic steel material as well as preparation method and application thereof
CN122013070A