Separator and secondary battery including same

The separator with a carbon nanotube structure addresses the conductive path issue in lithium secondary batteries, improving electrode conductivity and battery performance.

JP7575168B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2023512414
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-04
Filing Date
2021-08-31
Publication Date
2024-10-29
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

Conventional methods using current collectors and conductive materials are insufficient to improve the conductive path of electrodes in lithium secondary batteries, affecting the input/output characteristics and lithium ion diffusion.

Method used

A separator is developed with a conductive layer comprising a carbon nanotube structure where single-walled carbon nanotube units are aligned and bonded, enhancing the conductive path while maintaining lithium ion diffusion.

Benefits of technology

The conductive path is improved, reducing battery resistance and enhancing input/output characteristics and lifespan, with minimal impact on lithium ion diffusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575168000003
    Figure 0007575168000003
  • Figure 0007575168000004
    Figure 0007575168000004
  • Figure 0007575168000005
    Figure 0007575168000005
Patent Text Reader

Abstract

The present invention relates to a separator and a secondary battery including the same, which includes a porous substrate and a conductive layer disposed on the porous substrate, the conductive layer including a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are bonded to each other in parallel, and an average diameter of the carbon nanotube structure is 2 nm to 500 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0112867, filed on September 4, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a separator including a porous substrate and a conductive layer disposed on the porous substrate, the conductive layer including a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are bonded to each other in parallel, and the carbon nanotube structure has an average diameter of 2 nm to 500 nm, and a secondary battery including the separator. [Background technology]

[0003] Recently, as the technological development and demand for mobile devices increases, the demand for batteries as energy sources is rapidly increasing, and accordingly, research on batteries that can meet various needs is being actively conducted. In particular, research on lithium secondary batteries that have high energy density as a power source for such devices and have excellent life and cycle characteristics is being actively conducted.

[0004] The lithium secondary battery refers to a battery including an electrode assembly including a positive electrode including a positive electrode active material capable of inserting / extracting lithium ions, a negative electrode including a negative electrode active material capable of inserting / extracting lithium ions, and a separator interposed between the positive electrode and the negative electrode, and an electrolyte containing lithium ions.

[0005] Since the movement of electrons must be smooth between the positive electrode and the negative electrode (hereinafter referred to as electrodes), the conductive path of the electrodes must be reliably secured. For this purpose, the electrodes use current collectors with active material layers located on their surfaces, and the active material layers contain conductive materials. In addition, in order to improve the conductive path of the electrodes, techniques for modifying the surface of the current collectors or uniformly dispersing conductive materials have been introduced. However, conventional methods using current collectors and conductive materials alone are insufficient to improve the conductive path of the electrodes.

[0006] Therefore, this specification introduces a separator capable of improving the conductive path of an electrode and a secondary battery including the same. Summary of the Invention [Problem to be solved by the invention]

[0007] One problem to be solved by the present invention is to provide a separator that can improve the input / output characteristics of a battery by improving the conductive path of an electrode while maintaining the degree of diffusion of lithium ions in the separator.

[0008] Another problem to be solved by the present invention is to provide a secondary battery including the separator. [Means for solving the problem]

[0009] According to one embodiment of the present invention, there is provided a separator comprising a porous substrate and a conductive layer disposed on the porous substrate, the conductive layer comprising a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are bonded in parallel to each other, and the carbon nanotube structure has an average diameter of 2 nm to 500 nm.

[0010] According to another embodiment of the present invention, there is provided a secondary battery including the separator. Effect of the Invention

[0011] Since the separator according to the present invention includes a conductive layer including a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are bound to each other in a row, the conductive path of the electrode in contact with the conductive layer can be improved, and the battery resistance can be reduced to improve the input / output characteristics of the battery. In addition, since the conductive layer has almost no effect on the pore structure of the porous substrate (or the porous substrate and the inorganic coating layer) in the separator, the conductive path can be improved while minimizing the reduction in the diffusion degree of lithium ions in the separator. [Brief description of the drawings]

[0012] [Figure 1] 2 is a SEM photograph of the separator of Comparative Example 1. [Diagram 2] 2 is a SEM photograph of the separator of Example 1. [Diagram 3] 1 is a SEM photograph of the separator of Example 2. [Figure 4] 1 is a SEM photograph of the separator of Comparative Example 3. [Diagram 5] 1 is a TEM photograph of the carbon nanotube structure of Production Example 1. [Figure 6] 1 is a TEM photograph of a single-walled carbon nanotube unit of Production Example 2. [Figure 7] FIG. 1 is a schematic diagram of a battery according to one embodiment of the present invention. [Figure 8] FIG. 1 is a schematic diagram of a portion of a battery according to one embodiment of the present invention. [Figure 9] FIG. 1 is a schematic diagram of a portion of a battery according to one embodiment of the present invention. [Figure 10] FIG. 1 is a schematic diagram of a portion of a battery according to one embodiment of the present invention. [Figure 11] FIG. 1 is a schematic diagram of a portion of a battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The terms and words used in this specification and the claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that are consistent with the technical idea of ​​the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.

[0014] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise.

[0015] In this specification, the terms "comprise", "comprise", or "have" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0016] In this specification, the "specific surface area" is measured by the BET method, and specifically, it can be calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mini II made by BEL Japan.

[0017] The average particle size D in this specification 50 The average particle size D can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve. 50 can be measured by using, for example, a laser diffraction method. The laser diffraction method generally allows measurement of particle diameters from the submicron range to about several mm, and can provide results with high reproducibility and high resolution.

[0018] In the present invention, a single-walled carbon nanotube unit refers to a tubular unit having one wall made of carbon atoms, and a multi-walled carbon nanotube unit refers to a tubular unit having multiple walls made of carbon atoms stacked on one tube.

[0019] The present invention will be specifically described below.

[0020] Separator The separator according to the present invention includes a porous substrate and a conductive layer disposed on the porous substrate, the conductive layer including a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are bonded together in parallel, and the carbon nanotube structure may have an average diameter of 2 nm to 500 nm.

[0021] 1) Porous base material The porous substrate may be a porous polymeric film substrate or a porous polymeric nonwoven fabric substrate.

[0022] The porous polymer film substrate may be a porous polymer film made of a polyolefin such as polyethylene, polypropylene, polybutylene, or polypentene, and such a polyolefin porous polymer film substrate exhibits a shutdown function at a temperature of, for example, 80 to 130°C.

[0023] In this case, the polyolefin porous polymer film can be formed from a polyolefin polymer such as polyethylene (such as high density polyethylene, linear low density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination of two or more of these.

[0024] In addition, the porous polymer film substrate can be manufactured by forming various polymers such as polyester, in addition to polyolefin, into a film shape. The porous polymer film substrate can be formed into a structure in which two or more film layers are laminated, and each film layer can be formed of the above-mentioned polymers such as polyolefin and polyester alone or a mixture of two or more of them.

[0025] In addition, the porous polymer film substrate and the porous nonwoven fabric substrate may be formed of a polymer selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, and the like, either alone or in combination.

[0026] The thickness of the porous substrate is not particularly limited, but is preferably 1 to 100 μm, and more preferably 5 to 50 μm. The pore size and porosity of the porous substrate are also not particularly limited, but are preferably 0.01 to 50 μm and 10 to 95%, respectively.

[0027] 2) Conductive layer The conductive layer may be disposed on the porous substrate. Specifically, the conductive layer may be disposed on one side of the porous substrate, and more specifically, the conductive layer may be disposed on only one side of the porous substrate.

[0028] The conductive layer may include a carbon nanotube structure, and more specifically, the conductive layer may be made of the carbon nanotube structure.

[0029] The carbon nanotube structure may include a plurality of single-walled carbon nanotube units. Specifically, the carbon nanotube structure may be a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are aligned and bonded to each other. More specifically, in consideration of the durability of the conductive layer and the conductive network of the electrode, the carbon nanotube structure may be a carbon nanotube structure in which 2 to 4,500, preferably 50 to 4,500, more preferably 1,000 to 4,500 single-walled carbon nanotube units are bonded to each other. In consideration of the improvement of the dispersibility of the carbon nanotube structure and the durability of the conductive layer, the carbon nanotube structure may be a carbon nanotube structure in which 1,000 to 4,500 single-walled carbon nanotube units are aligned and bonded to each other.

[0030] In the carbon nanotube structure, the single-walled carbon nanotube units may be arranged side by side and bonded together (long axes of the units are bonded together in parallel to form a flexible bundled cylindrical structure) to form the carbon nanotube structure. In the conductive layer, the carbon nanotube structures may be connected to each other to form a network structure.

[0031] The carbon nanotube structure is different from a general carbon nanotube. Specifically, a general carbon nanotube refers to a carbon nanotube unit formed by dispersing a bundle type or entangled type carbon nanotube (single-walled carbon nanotube unit or multi-walled carbon nanotube unit attached to or entangled with each other) in a dispersion medium to the maximum extent (conductive material dispersion). In this case, the carbon nanotube is completely dispersed in the conventional conductive material dispersion, and exists as a conductive material dispersion in which a single carbon nanotube unit is dispersed. In the conventional conductive material dispersion, the carbon nanotube unit is easily cut due to an excessive dispersion process, and has a shorter length than the initial length. In this case, when a separator is coated using the conductive material dispersion, carbon nanotube units having a small average diameter are located in the pores in the separator, so that the pore volume on the surface and inside of the separator is excessively reduced, and lithium ions in the separator do not diffuse smoothly. In addition, the carbon nanotube units are connected to each other through pores in the separator, which may cause a local short circuit between the positive and negative electrodes that are sandwiched between the separator. Furthermore, the multi-walled carbon nanotube units have a high degree of structural defects due to the mechanism of nodal growth (no smooth linear growth, but nodes due to defects that occur during the growth process). Therefore, the multi-walled carbon nanotube units are more easily cut during the dispersion process, and the short cut multi-walled carbon nanotube units are more likely to aggregate with each other due to π-π stacking of the carbon of the units. This makes it difficult for them to be more uniformly dispersed in the conductive layer of the separator.

[0032] In contrast, the carbon nanotube structure included in the conductive layer of the separator of the present invention has a rope-like shape in which a plurality of single-walled carbon nanotube units having relatively high crystallinity and no structural defects are arranged side by side and connected to each other. Since the carbon nanotube structure has a large average diameter, it is not easily disposed inside the pores of the porous substrate (or the porous substrate and the inorganic coating layer) of the separator, and the pore structure can be maintained. As a result, the decrease in lithium ion diffusion in the separator can be minimized, and the input / output characteristics of the battery can be maintained. In addition, since the carbon nanotube structure forms a network structure in the conductive layer, the conductive layer can function as a kind of current collector for the electrode in contact with the conductive layer due to the network structure. Specifically, the conductive layer may be in contact with not only the electrode but also a current application part (e.g., a lower can in a coin cell, an electrode tab in a general full cell) connected to the electrode, so that when a current is applied from the outside, a current can move along the conductive layer in addition to the current collector in the electrode. Therefore, since the current can move uniformly over the entire surface of the electrode along the conductive layer, the resistance of the battery can be significantly improved, and the input / output characteristics and life characteristics of the battery can be improved. In particular, since the conductive network of the carbon nanotube structure can be formed very uniformly and firmly based on the long length and large diameter of the carbon nanotube structure, the improvement effect of the conductive path is more excellent than when a general carbon nanotube unit is used.

[0033] In the carbon nanotube structure, the average diameter of the single-walled carbon nanotube units may be 0.5 nm to 10 nm, specifically 1 nm to 9 nm. When the average diameter is satisfied, even if a small amount of the carbon nanotube structure is used, the improvement effect of the conductive path in the electrode via the conductive layer can be maximized. The average diameter corresponds to the average value of the diameters of the top 100 single-walled carbon nanotube units and the bottom 100 single-walled carbon nanotube units when the surface of the manufactured separator is observed by TEM.

[0034] In the carbon nanotube structure, the average length of the single-walled carbon nanotube units may be 1 μm to 100 μm, specifically 5 μm to 50 μm. When the average length is satisfied, a conductive path can be formed on the electrode via the conductive layer, and a unique network structure can be formed in the conductive layer, so that even a very small amount of carbon nanotube structures can maximize the conductivity in the electrode. The average length corresponds to the average value of the lengths of the top 100 single-walled carbon nanotube units and the bottom 100 single-walled carbon nanotube units when the surface of the manufactured separator is observed by TEM.

[0035] The specific surface area of ​​the single-walled carbon nanotube unit is 500 m 2 / g~1,000m 2 / g, specifically 600m 2 / g~800m 2 When the range is satisfied, the wide specific surface area can smoothly secure a conductive path in the electrode, so that even a small amount of carbon nanotube structure can maximize the conductivity in the electrode. The specific surface area of ​​the single-walled carbon nanotube unit can be calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using BELSORP-mini II manufactured by BEL Japan.

[0036] The average diameter of the carbon nanotube structure may be 2 nm to 500 nm, specifically 10 nm to 500 nm, more specifically 100 nm to 500 nm. If the average diameter is less than 2 nm, the carbon nanotube structure is easily broken during the dispersion process, the conductive network is not smoothly formed, the carbon nanotube structure may block the pore structure of the porous substrate (or the porous substrate and the inorganic coating layer), and the performance of the battery may be reduced. There is a problem that an internal short circuit occurs because the conductive network is allowed to form as a path penetrating the separator. If the average diameter exceeds 500 nm, the excessive diameter may block the pore structure on the surface of the porous substrate (or the porous substrate and the inorganic coating layer), and the performance of the battery may be reduced. When the same content of carbon nanotube structure is used, the number of tubes forming the conductive network is small, and the desired effect cannot be smoothly achieved. The average diameter corresponds to an average value of the diameters of the top 100 carbon nanotube structures having the largest diameter and the bottom 100 carbon nanotube structures having the smallest diameter when the surface of the manufactured separator is observed by SEM.

[0037] The average length of the carbon nanotube structures may be 1 μm to 500 μm, specifically 5 μm to 300 μm, and more specifically 10 μm to 100 μm. When this range is satisfied, a conductive network is effectively formed and current in the electrode can be uniformly transmitted, thereby reducing battery resistance and improving overall battery performance such as input / output characteristics and life characteristics of the battery. The average length corresponds to the average value of the lengths of the top 100 carbon nanotube structures and the bottom 100 carbon nanotube structures when the surface of the manufactured separator is observed by SEM.

[0038] Meanwhile, depending on the case, the single-walled carbon nanotube unit may be surface-treated by oxidation or nitridation in order to improve the affinity with the dispersant.

[0039] The carbon nanotube structure may be included in an amount of 0.01 to 20 parts by weight, specifically 0.01 to 10 parts by weight, based on 100 parts by weight of the porous substrate. When the above range is satisfied, the pore structure of the porous substrate may be exposed on the surface, and the surface of the separator may have a porous structure. In addition, the conductive layer may function as a kind of current collector on the surface of the electrode in contact with the separator, thereby reducing the resistance of the battery and improving the input / output characteristics of the battery.

[0040] Meanwhile, the carbon nanotube structure is a highly crystalline carbon-based material and has high high temperature stability and chemical resistance, so that the carbon nanotube structure can maintain a strong net-like network structure even when the temperature inside the battery increases rapidly.

[0041] The thickness of the conductive layer may be 10 nm to 2000 nm, specifically 50 nm to 2000 nm, and more specifically 100 nm to 1000 nm. When the above range is satisfied, the pore structure of the porous substrate can be exposed on the surface, and the surface of the separator can have a porous structure. In addition, the conductive layer can act as a kind of current collector on the surface of the electrode in contact with the separator, so that the resistance of the battery can be reduced and the input / output characteristics of the battery can be improved. In particular, in order to obtain the above-mentioned effects while maintaining a high energy density of the battery, the thickness of the conductive layer is most preferably 100 nm to 1,000 nm. The thickness can be measured by observing the cross section of the separator by SEM.

[0042] The surface resistance of the conductive layer is 5×10 -1 Ω / □~5×10 4 It may be Ω / □, specifically 5×10Ω / □ to 5×10 4The range may be Ω / □. This range can be derived from the high electrical conductivity of the carbon nanotube structure and the formation of a long, sturdy, rope-like conductive network due to the use of the carbon nanotube structure. When this range is satisfied, the conductive layer can act as a kind of current collector on the surface of the electrode in contact with the separator while the surface of the separator maintains a porous structure, thereby reducing the resistance of the battery and improving the input / output characteristics of the battery.

[0043] The conductive layer may further include an additive covering at least a portion of the surface of the carbon nanotube structure. The additive may play a role in appropriately dispersing bundled or entangled carbon nanotubes when forming the carbon nanotube structure. Since the additive is present while covering at least a portion of the surface of the carbon nanotube structure, the conductive layer is unlikely to be detached from the separator and can be strongly bonded to the porous substrate.

[0044] The additive may be at least one selected from the group consisting of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, hydrogenated nitrile butadiene rubber, polystyrene, pyrene butyric acid, pyrene sulfonic acid, tannic acid, pyrene methylamine, sodium dodecyl sulfate, carboxymethylcellulose, styrene butadiene rubber, and fluororubber, and specifically may be carboxymethylcellulose.

[0045] 3) Inorganic coating layer Depending on the case, the separator may further include the inorganic coating layer. The inorganic coating layer may be disposed between the porous substrate and the conductive layer. In this case, even if heat generation / ignition occurs or temperature rises suddenly due to various reasons in the battery, the inorganic coating layer can maintain the shape of the separator, prevent short circuit between the positive electrode and the negative electrode, and improve the safety of the battery.

[0046] The inorganic coating layer can include inorganic particles. The inorganic particles are not particularly limited as long as they do not cause an oxidation and / or reduction reaction, i.e., an electrochemical reaction, with the positive or negative electrode current collector in the operating voltage range of the battery (e.g., 0 to 5 V based on Li / Li+) and do not reduce the electrical conductivity. Examples of the inorganic particles include Al2O3, BaTiO3, CaO, CeO2, NiO, MgO, SiO2, SnO2, SrTiO3, TiO2, Y2O3, ZnO, ZrO2, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y TiyO3(PLZT), Pb(Mg3Nb 2 / 3 The inorganic material may be one or more inorganic materials selected from the group consisting of PMN-PT, PbTiO3, and hafnia (HfO2).

[0047] The inorganic coating layer may further include a binder. The binder serves to strengthen the binding force of the inorganic particles. Examples of the binder include polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples of suitable cellulose acetate copolymers include, but are not limited to, cyanoethyl propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose.

[0048] Meanwhile, the carbon nanotube structure is a highly crystalline carbon-based material, and therefore has high high-temperature stability and chemical resistance. Therefore, even if the temperature inside the battery rises suddenly, the carbon nanotube structure can maintain a strong net-like network structure. In addition, when the inorganic coating layer and the carbon nanotube structure are combined, even if heat generation / ignition occurs or the temperature rises suddenly due to various reasons inside the battery, the inorganic coating layer and the carbon nanotube structure maintain the shape of the separator, preventing short circuit between the positive and negative electrodes, and further improving the safety of the battery.

[0049] The air permeability of the separator may be 50s / 100cc to 500s / 100cc, specifically 100s / 100cc to 300s / 100cc, and more specifically 150s / 100cc to 250s / 100cc. The air permeability means the time it takes for 100cc of air to permeate the separator. Meeting the air permeability means that the pore structure of the separator is effectively constructed, in other words, that the pore structure of the separator can be maintained even if the conductive layer is formed. When the range of the air permeability of the separator is met, lithium ions can easily diffuse, and the input / output characteristics of the battery can be improved.

[0050] Manufacturing method of separator Next, a method for producing the separator of the present invention will be described.

[0051] The method for producing a separator of the present invention includes the steps of preparing a carbon nanotube structure and disposing the carbon nanotube structure on the porous substrate, the carbon nanotube structure including a structure in which a plurality of single-walled carbon nanotube units are bonded to each other in parallel, and the carbon nanotube structure may have an average diameter of 2 nm to 500 nm. The porous substrate and the carbon nanotube structure may be the same as the porous substrate and the carbon nanotube structure described in the separator of the above embodiment.

[0052] 1) Preparation of carbon nanotube structures The preparation of the carbon nanotube structure may include a step (S1-1) of preparing a mixture containing a dispersion medium, a dispersant, and bundled single-walled carbon nanotubes (a combination or aggregate of single-walled carbon nanotube units), and a step (S1-2) of applying a shear force to the mixture to disperse the bundled single-walled carbon nanotubes and form a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are combined in a line.

[0053] In the step S1-1, the mixture can be prepared by adding the bundled single-walled carbon nanotubes and a dispersant to a dispersion medium. The bundled single-walled carbon nanotubes are the above-mentioned single-walled carbon nanotube units that are combined to form a bundle, and typically contain 2 or more, substantially 500 or more, for example 5,000 or more single-walled carbon nanotube units.

[0054] The specific surface area of ​​the bundled single-walled carbon nanotubes is 500 m 2 / g~1,000m 2 / g, specifically 600m 2 / g~800m 2 When the above range is satisfied, a conductive path in the electrode can be smoothly secured due to the large specific surface area, so that even with a very small amount of conductive material, the conductivity in the electrode can be maximized.

[0055] The bundled single-walled carbon nanotubes may be contained in the mixture at 0.1 wt % to 1.0 wt %, specifically, 0.2 wt % to 0.5 wt %. When the range is satisfied, the bundled single-walled carbon nanotubes are dispersed at an appropriate level, a carbon nanotube structure at an appropriate level may be formed, and dispersion stability may be improved.

[0056] Examples of the dispersion medium include water, amide polar organic solvents such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP); alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol, and octanol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, and hexylene glycol; polyhydric alcohols such as glycerin, trimethylolpropane, pentaerythritol, and sorbitol. Examples of the dispersion medium include, but are not limited to, alcohols, glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, and tetraethylene glycol monobutyl ether, ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, and cyclopentanone, and esters such as ethyl acetate, γ-butyrolactone, and ε-propiolactone, and any one or a mixture of two or more of these may be used. More specifically, the dispersion medium may be water.

[0057] The dispersant may include at least one of hydrogenated nitrile butadiene rubber, polyvinylidene fluoride, and carboxymethyl cellulose, and may be specifically carboxymethyl cellulose. The dispersant may correspond to the additive of the above-mentioned embodiment.

[0058] In the dispersion of the conductive material, the weight ratio of the bundled carbon nanotubes to the dispersant may be 1:0.1 to 1:10, specifically, 1:1 to 1:10. When the ratio is within this range, the bundled single-walled carbon nanotubes are dispersed at an appropriate level, a carbon nanotube structure at an appropriate level may be formed, and dispersion stability may be improved.

[0059] The solid content in the mixture may be 0.1 wt% to 20 wt%, specifically 1 wt% to 10 wt%. When the above range is satisfied, the bundled single-walled carbon nanotubes are dispersed at an appropriate level, a carbon nanotube structure of an appropriate level is formed, and dispersion stability is improved. In addition, the electrode slurry may have viscosity and elasticity suitable for the electrode manufacturing process, which also contributes to increasing the solid content of the electrode slurry.

[0060] In the step S1-2, the process of dispersing the bundled carbon nanotubes in the mixture can be performed using a mixer such as a homogenizer, a bead mill, a ball mill, a basket mill, an attrition mill, a universal mixer, a clear mixer, a spike mill, a TK mixer, or an ultrasonic dispersion (sonification) device, etc. Among them, the bead mill method is preferred because it can precisely control the diameter size of the carbon nanotube structure, can achieve uniform distribution of the carbon nanotube structure, and has an advantage in terms of cost.

[0061] The bead mill method is as follows: the mixture is placed in a container containing beads, and the container is rotated to disperse the bundled single-walled carbon nanotubes.

[0062] At this time, the conditions for carrying out the bead mill method are as follows.

[0063] The average particle size of the beads may be 0.5 mm to 1.5 mm, specifically 0.5 mm to 1.0 mm. When the above range is satisfied, the diameter size of the carbon nanotube structure can be appropriately controlled without being broken during the dispersion process, and a dispersion solution with a uniform composition can be produced.

[0064] The rotation speed of the container may be 500 RPM to 10,000 RPM, specifically 2,000 RPM to 6,000 RPM. When the rotation speed is within the above range, the diameter size of the carbon nanotube structure can be appropriately controlled without being broken during the dispersion process, and a dispersion solution with a uniform composition can be produced.

[0065] The time for which the bead mill is performed may be 0.5 to 2 hours, specifically 0.5 to 1.5 hours, and more specifically 0.8 to 1 hour. When the above range is satisfied, the diameter size of the carbon nanotube structure can be appropriately controlled without being broken during the dispersion process, and a dispersion solution with a uniform composition can be produced. The execution time of the bead mill means the total time for which the bead mill is applied, and therefore, for example, if the bead mill is performed several times, it means the total time over the several times.

[0066] The bead mill conditions are for dispersing the bundled single-walled carbon nanotubes to an appropriate level, specifically excluding the case where the bundled single-walled carbon nanotubes are completely dispersed into a single single-walled carbon nanotube. That is, the bead mill conditions are for dispersing the bundled single-walled carbon nanotubes to an appropriate level to form a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are aligned and bonded to each other in the conductive material dispersion liquid produced. This can be achieved only when the composition of the mixture liquid, the conditions of the dispersion process (e.g., the bead mill process), etc. are strictly controlled.

[0067] Through the above process, a carbon nanotube structure dispersion liquid can be formed.

[0068] (2) disposing a carbon nanotube structure on a porous substrate; The carbon nanotube structure dispersion liquid may be coated on the porous substrate, and the coated carbon nanotube structure dispersion liquid may be solidified to dispose the carbon nanotube structure on the porous substrate. The porous substrate may or may not include the inorganic coating layer described above, but it is preferable for the porous substrate to include an inorganic coating layer in order to improve safety. The carbon nanotube structure dispersion liquid may be coated using a conventional method such as a Mayer bar, a die coater, a reverse roll coater, or a gravure coater.

[0069] secondary battery A secondary battery according to another embodiment of the present invention may include the electrodes and the separator according to the above-described embodiment.

[0070] The electrodes may include a positive electrode and a negative electrode.

[0071] The electrode may include an electrode active material layer. The electrode may further include a current collector, in which case the electrode active material layer may be disposed on one or both sides of the current collector.

[0072] The current collector is not particularly limited as long as it is a material that has conductivity without inducing a chemical change in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, alloys thereof, those having their surfaces treated with carbon, nickel, titanium, silver, or the like, or calcined carbon may be used.

[0073] The current collector may typically have a thickness of 3 μm to 500 μm, and may have fine irregularities on its surface to enhance the bonding strength of the electrode active material. The electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0074] The electrode active material layer may include an electrode active material and a conductive material.

[0075] The electrode active material may be a positive electrode active material or a negative electrode active material generally used in the art, and its type is not particularly limited.

[0076] For example, as the positive electrode active material, a lithium oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium may be used. More specifically, the lithium oxide is a lithium-manganese-based oxide (for example, LiMnO2, LiMn2O, etc.), a lithium-cobalt-based oxide (for example, LiCoO2, etc.), a lithium-nickel-based oxide (for example, LiNiO2, etc.), a lithium-nickel-manganese-based oxide (for example, LiNi 1-Y1 Mn Y1 O2 (where 0 < Y1 < 1), LiNi Z1 Mn 2-Z1 O4 (where 0 < Z1 < 2), etc.), a lithium-nickel-cobalt-based oxide (for example, LiNi 1-Y2 Co Y2 O2 (where 0 < Y2 < 1), etc.), a lithium-manganese-cobalt-based oxide (for example, LiCo 1-Y3 Mn Y3 O2 (where 0 < Y3 < 1), LiMn 2-Z2 Co Z2 O4 (where 0 < Z2 < 2), etc.), a lithium-nickel-cobalt-manganese-based oxide (for example, Li(Ni P1 Co Q1 Mn R1 )O2 (where 0 < P1 < 1, 0 < Q1 < 1, 0 < R1 < 1, P1 + Q1 + R1 = 1) or Li(Ni P2 Co Q2 Mn R2 )O4 (where 0 < P2 < 2, 0 < Q2 < 2, 0 < R2 < 2, P2 + Q2 + R2 = 2), etc.), or a lithium-nickel-cobalt-manganese-other metal (M) oxide (for example, Li(Ni P3 Co Q3 Mn R3 M 1 S )O2 (where M 1is selected from the group consisting of Al, Cu, Fe, V, Cr, Ti, Zr, Zn, Ta, Nb, Mg, B, W, and Mo, and P3, Q3, R3, and S are atomic fractions of independent elements, respectively, where 0 < P3 < 1, 0 < Q3 < 1, 0 < R3 < 1, 0 < S < 1, and P3 + Q3 + R3 + S = 1), etc.), and one or more of these compounds can be included.

[0077] On the other hand, as the negative electrode active material, for example, carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO v (0 < v < 2), metal oxides such as SnO2, vanadium oxide, and lithium vanadium oxide that can be doped and undoped with lithium; or composites containing the metallic compound and the carbonaceous material such as Si-C composite or Sn-C composite, etc. may be mentioned, and one or more mixtures of these may be used. Also, a thin film of metallic lithium can be used as the negative electrode active material. Note that as the carbon material, both low-crystalline carbon and highly crystalline carbon can be used.

[0078] The electrode active material may be contained in an amount of 70% by weight to 99.5% by weight, preferably 80% by weight to 99% by weight, based on the total weight of the electrode active material layer. When the content of the electrode active material satisfies the above range, excellent energy density, electrode adhesion, and electrical conductivity can be achieved.

[0079] The conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0080] The electrode may further include a binder, which may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, and may include various copolymers thereof.

[0081] The electrodes are connected to a current applying portion.

[0082] Specifically, when the secondary battery is a coin cell, an external current is applied to an electrode in contact with the lower can through a lower can, and in this case, the lower can corresponds to the current application part. When the secondary battery is a mono cell (or a pouch-type or cylindrical battery having more than one stack) instead of a coin cell, an external current is applied to the electrode through an electrode tab, and in this case, the electrode tab corresponds to the current application part. When the electrode is a positive electrode in the mono cell, an end of a positive electrode current collector in the positive electrode (an end region of a portion (plain portion) where a positive electrode active material layer is not formed) may correspond to the current application part.

[0083] The separator may be disposed between the positive electrode and the negative electrode. The positive electrode includes a positive electrode current collector and a positive electrode active material layer, and the negative electrode includes a negative electrode current collector and a negative electrode active material layer. The positive electrode current collector and the negative electrode current collector each include a non-coated portion where the positive electrode active material layer and the negative electrode active material layer are not disposed (not overlapping with the positive electrode active material layer). When the positive electrode is in contact with the conductive layer of the separator (in some cases, the negative electrode, not the positive electrode, may be in contact with the conductive layer of the separator), the conductive layer of the separator may be in contact with the non-coated portion of the positive electrode current collector and the current application portion (corresponding to the positive electrode tab). As a result, the current flowing into the secondary battery through the current application portion can be uniformly transmitted to the positive electrode active material layer not only through the positive electrode current collector but also through the conductive layer.

[0084] 7, when manufacturing the coin cell, the separator 130 including the porous substrate 131 and the conductive layer 132 is disposed between the negative electrode 120 and the positive electrode 110, and the conductive layer 132 of the separator 130 is in contact with the upper surface of the positive electrode 110. In addition, the lower cap 111a is disposed to be in contact with the lower surface of the positive electrode 110, and a portion of the lower cap 111a is in contact with the conductive layer 132 during the assembly of the coin cell. Therefore, the current applied through the lower cap 111a, which is a current application unit, can be uniformly spread not only to the lower surface of the positive electrode 110 along the lower cap 111a, but also to the upper surface of the positive electrode 110 along the conductive layer 132. As a result, the battery resistance can be reduced, and the input / output characteristics of the battery can be significantly improved.

[0085] The case of a mono cell will be described below. Referring to FIG. 8, a mono cell includes a positive electrode 110 including a positive electrode collector 111 and a positive electrode active material layer 112, a negative electrode 120 including a negative electrode collector 121 and a negative electrode active material layer 122, and a separator 130 including a porous substrate 131 and a conductive layer 132. The end portion of the positive electrode collector 111 protrudes long without the positive electrode active material layer 112 disposed on the surface to form a positive electrode tab 111a which is a current application portion, and the positive electrode tabs 111a are in contact with each other. At this time, a portion of the conductive layer 132 is in contact with a portion of the positive electrode tab 111a (C). Therefore, the current applied through the positive electrode tab 111a flows not only to the positive electrode collector 111 but also to the conductive layer 132, so that the current can flow uniformly in the positive electrode active material layer 112. As a result, the battery resistance can be reduced, and the input / output characteristics of the battery can be significantly improved.

[0086] FIG. 9 is a schematic diagram illustrating the positional relationship of a positive electrode collector 111, a positive electrode active material layer 112, a positive electrode tab 111a, and a separator conductive layer 132 in an unwound battery state before completing a jelly roll battery. The positive electrode collector 111 includes a plain portion that does not overlap with the positive electrode active material layer, and the plain portion and a part of the positive electrode tab 111a are in contact with the conductive layer 132 (area corresponding to C). Therefore, the current applied through the positive electrode tab 111a flows not only to the positive electrode collector 111 but also to the conductive layer 132, so that the current can flow uniformly in the positive electrode active material layer 112. This can reduce the battery resistance and greatly improve the input / output characteristics of the battery.

[0087] 10 and 11 are similar to FIG. 9, but there are a plurality of positive electrode tabs 111a and a plurality of positive electrode active material layers 112 in separate regions. In this case, the area of ​​the positive electrode tabs 111a and the uncoated area in contact with the conductive layer increases, so that the current applied through the positive electrode tabs 111a flows more uniformly to the conductive layer 132 and the current flows more uniformly to the positive electrode active material layer 112. As a result, the battery resistance can be further reduced and the input / output characteristics of the battery can be significantly improved.

[0088] In the above-mentioned FIGS. 7 to 11, the positions of the positive and negative electrodes can be interchanged.

[0089] The secondary battery may further include an electrolyte, which may be used in the manufacture of a lithium secondary battery, including, but not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, and a molten inorganic electrolyte.

[0090] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0091] Examples of the non-aqueous organic solvent include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0092] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, are highly viscous organic solvents having a high dielectric constant and easily dissociating lithium salts, and therefore can be preferably used. When such a cyclic carbonate is mixed with a linear carbonate having a low viscosity and a low dielectric constant, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte having high electrical conductivity can be prepared, and therefore the cyclic carbonate can be more preferably used.

[0093] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of:

[0094] In addition to the constituent components of the electrolyte, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0095] According to yet another embodiment of the present invention, there is provided a battery module including the secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate-limiting characteristics and high cycle characteristics, and therefore can be used as a power source for a medium- to large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system.

[0096] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications fall within the scope of the appended claims.

[0097] Production Example 1: Production of carbon nanotube structure dispersion A bundle-type carbon nanotube (specific surface area: 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more. 2 0.4 parts by weight of cellulose acetate (1.0% by weight / g) and 0.6 parts by weight of carboxymethyl cellulose (weight average molecular weight: 400,000 g / mol, degree of substitution: 1.0) were mixed with 99.0 parts by weight of water as a dispersion medium to produce a mixture with a solid content of 1.0% by weight.

[0098] The mixture was stirred using a bead mill to disperse the bundled single-walled carbon nanotubes in the solvent, producing a carbon nanotube structure dispersion. The beads had a particle size of 1 mm, the stirring vessel containing the beads was rotated at 3,000 RPM, and the stirring was performed for 60 minutes. The carbon nanotube structure dispersion contained carbon nanotube structures in which 2 to 5,000 single-walled carbon nanotube units were bound together in a line (see FIG. 5). In the carbon nanotube structure dispersion, the carbon nanotube structure was 0.4 wt % and the carboxymethyl cellulose was 0.6 wt %.

[0099] Preparation Example 2: Preparation of Single-Walled Carbon Nanotube Unit Dispersion A bundle-type carbon nanotube (specific surface area: 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more. 2 0.2 parts by weight of cellulose acetate (1.0 g / g) and 1.2 parts by weight of carboxymethyl cellulose (weight average molecular weight: 100,000 g / mol, degree of substitution: 1.0) were mixed with 98.6 parts by weight of water as a dispersion medium to produce a mixture with a solid content of 1.4% by weight.

[0100] The mixture was stirred in a bead mill to disperse the bundled single-walled carbon nanotubes in the solvent, producing a conductive material dispersion. At this time, the particle size of the beads was 1 mm, and the rotation speed of the stirring vessel containing the beads was 3,000 RPM. Stirring was performed for a total of 4 cycles (with 60 minutes of natural cooling between each cycle) under the above conditions, with 60 minutes of stirring being one cycle. Thus, a single-walled carbon nanotube unit dispersion was produced. In the dispersion, the bundled single-walled carbon nanotubes were completely dispersed, and only single-walled carbon nanotube units were present as individual units, and the above-mentioned carbon nanotube structure was not detected (see FIG. 6). In addition, the single-walled carbon nanotube units were 0.2 wt % and the carboxymethyl cellulose was 1.2 wt % in the single-walled carbon nanotube unit dispersion.

[0101] Examples and Comparative Examples Example 1: Manufacture of separator and secondary battery (1) Separator manufacturing A polymer solution (solid content 5wt% concentration) was prepared by mixing acetone and PVDF-HFP binder (weight average molecular weight: 300,000g / mol). Al2O3 (Nippon Light Metal, LS235) was added to the polymer solution at 20wt% of the total content, and dispersed using a ball mill to prepare a slurry for an inorganic porous coating layer. The slurry was coated on a porous substrate (Toray B12PA1, thickness 12μm) using a dip coating method, and humid phase separation was induced at a relative humidity (RH) level of 40%. A separator including an inorganic coating layer was manufactured in this manner. The carbon nanotube structure dispersion of Manufacturing Example 1 was coated on the separator manufactured in the above manner using a doctor blade coating method to a thickness of 500nm on the cross section basis, and the separator was manufactured by drying in an oven at 120℃ for 1 minute.

[0102] As a positive electrode active material, Li[Ni 0.6 Mn 0.2 Co 0.2 The positive electrode active material, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a weight ratio of 94:4:2 in N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode slurry.

[0103] The prepared slurry was applied to a positive electrode current collector (Al) with a thickness of 15 μm at a loading amount of 5 mAh / cm 2 The coating was applied and dried so that the temperature of the circulating air was 110° C. The coating was then rolled and dried in a vacuum oven at 130° C. for 2 hours to form a positive electrode active material layer.

[0104] The negative electrode active material, artificial graphite, the negative electrode conductive material, carbon black, the negative electrode binders, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were mixed in a weight ratio of 96.1:0.5:2.3:1.1 with distilled water to prepare a negative electrode slurry. The prepared slurry was applied to a negative electrode current collector (Cu) with a thickness of 20 μm at a loading amount of 6 mAh / cm. 2 The negative electrode current collector on which the negative electrode slurry was disposed was rolled by a roll rolling method so that the total thickness of the negative electrode slurry and the negative electrode current collector was 80 μm. The negative electrode slurry and the negative electrode current collector were then dried at 110° C. for 6 hours to prepare a negative electrode.

[0105] Then, the prepared positive and negative electrodes and the separators of the Examples and Comparative Examples were combined to prepare a monocell, and then an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC)=1 / 2 (volume ratio), lithium hexafluorophosphate (LiPF61 mol) was injected into the monocell to finally prepare a lithium secondary battery. A part of the conductive layer in the separator and a part of the positive electrode tab, which is the end of the positive electrode current collector of the positive electrode, were in contact with each other.

[0106] Example 2: Separator and battery manufacture A separator and a battery were produced in the same manner as in Example 1, except that the thickness of the conductive layer was 250 nm.

[0107] Example 3: Separator and battery manufacture The loading of the positive electrode is 2.5mAh / cm 2 A separator and a battery were produced in the same manner as in Example 1, except that the separator and the battery were produced in the same manner as in Example 1.

[0108] Example 4: Separator and battery manufacture The conductive layer is 250 nm thick and the loading of the positive electrode is 2.5 mAh / cm 2 A separator and a battery were produced in the same manner as in Example 1, except that the separator and the battery were produced in the same manner as in Example 1.

[0109] Comparative Example 1: Manufacture of separator and battery A separator and a battery were produced in the same manner as in Example 1, except that no conductive layer was formed.

[0110] Comparative Example 2: Manufacture of separator and battery A separator and a battery were produced in the same manner as in Example 3, except that no conductive layer was formed.

[0111] Comparative Example 3: Manufacture of separator and battery A separator and a battery were manufactured in the same manner as in Example 1, except that the single-walled carbon nanotube unit dispersion liquid of Preparation Example 2 was used instead of the carbon nanotube structure dispersion liquid of Preparation Example 1.

[0112] Comparative Example 4: Production of separator A separator and a battery were manufactured in the same manner as in Example 2, except that the single-walled carbon nanotube unit dispersion liquid of Preparation Example 2 was used instead of the carbon nanotube structure dispersion liquid of Preparation Example 1.

[0113] Comparative Example 5: Production of separator A separator and a battery were manufactured in the same manner as in Example 3, except that the single-walled carbon nanotube unit dispersion liquid of Preparation Example 2 was used instead of the carbon nanotube structure dispersion liquid of Preparation Example 1.

[0114] Comparative Example 6: Production of separator A separator and a battery were manufactured in the same manner as in Example 4, except that the single-walled carbon nanotube unit dispersion liquid of Preparation Example 2 was used instead of the carbon nanotube structure dispersion liquid of Preparation Example 1.

[0115] [Table 1]

[0116] In Examples 1 to 4, the carbon nanotube structures had an average diameter of 100 nm and an average length of 15.6 μm. The average diameter and average length correspond to the average values ​​of the top 100 carbon nanotube structures with the largest diameter (or length) and the bottom 100 carbon nanotube structures when the manufactured negative electrodes are observed by TEM. In Comparative Examples 2 and 4, the single-walled carbon nanotube units had an average diameter of 1.6 nm and an average length of 1.8 μm. The average diameter and average length correspond to the average values ​​of the top 100 single-walled carbon nanotube units with the largest diameter (or length) and the bottom 100 single-walled carbon nanotube units when the manufactured negative electrodes are observed by TEM.

[0117] Experimental example 1: Observation of the separator The separators of Example 1 and Comparative Example 2 were observed by SEM. 1 is an SEM photograph of the separator of Comparative Example 1, FIG. 2 is an SEM photograph of the separator of Example 1, FIG. 3 is an SEM photograph of the separator of Example 2, and FIG.

[0118] 2 and 3, thick rope-like carbon nanotube structures (2 to 5,000 single-walled carbon nanotube structures are connected to each other in a line) are located on the surface of the inorganic coating layer in a network shape, and the carbon nanotube structures are uniformly entangled in a network structure without blocking the pore structure on the surface of the inorganic coating layer. In addition, carboxymethyl cellulose is disposed on the carbon nanotube structures. In contrast, referring to FIG. 4, thick and long carbon nanotube structures are not observed, and thin and short single-walled carbon nanotube units exist as individual units. Therefore, when the same amount is used, the number of single-walled carbon nanotube units increases exponentially compared to the carbon nanotube structure, and in this case, the single-walled carbon nanotube units are densely packed to the extent that the pore structure on the surface is completely blocked, and the inorganic layer is coated and disposed in the form of a kind of surface film with no gaps or inside the pores.

[0119] Experimental Example 2: Evaluation of separator air permeability The separators produced in Examples 1 to 4 and Comparative Examples 1 to 6 were evaluated for air permeability as follows.

[0120] Using an air permeability meter (manufacturer: Asahi Seiko, product name: EG01-55-1MR), the time (sec) it took for 100ml of air to pass through the separator at a constant pressure (0.05MPa) was measured. Measurements were taken at three points, one on each side of the left / middle / right of each separator, and the average was calculated. The results are shown in Table 2. A rate of 500s / 100cc or more may cause a decrease in battery output and cycle characteristics.

[0121] Experimental Example 3: Evaluation of the surface resistance of the separator's conductive layer For the separators produced in Examples 1 to 4 and Comparative Examples 1 to 6, the surface resistance of the conductive layer was evaluated as follows.

[0122] The surface resistance of the conductive layer of the separator was measured using a surface resistance measuring instrument (manufacturer: Mitsubishi, product name: MCP-T610) equipped with a 4-pin probe. Measurements were taken at one point each on the left, middle, and right parts of each separator (a total of three points), and the average was calculated. The results are shown in Table 2.

[0123] Experimental Example 4: Evaluation of discharge capacity by C-Rate The output characteristics of the batteries of Examples 1 to 4 and Comparative Examples 1 to 6 were evaluated as follows.

[0124] The charge C-rate was fixed at 0.2C, and the discharge C-rate was increased from 0.2C to 2.0C. The discharge capacity (%) at 2.0C relative to the discharge capacity at 0.2C was measured for each lithium secondary battery, and the results are shown in Table 2.

[0125] [Table 2]

Claims

1. a porous substrate and a conductive layer disposed on the porous substrate; The conductive layer includes a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are connected to each other in parallel, The carbon nanotube structure has an average diameter of 2 nm to 500 nm; The conductive layer further comprises an additive covering at least a portion of a surface of the carbon nanotube structure.

2. A method for manufacturing a semiconductor device comprising: The conductive layer includes a carbon nanotube structure in which a plurality of single-walled carbon nanotube units are connected to each other in parallel, The carbon nanotube structure has an average diameter of 2 nm to 500 nm; The separator further comprises an inorganic coating layer between the porous substrate and the conductive layer, the inorganic coating layer comprising inorganic particles.

3. The separator according to claim 1 , wherein the carbon nanotube structures are interconnected to each other in the conductive layer to form a network structure.

4. 4. The separator according to claim 1, wherein the carbon nanotube structure has an average length of 1 μm to 500 μm.

5. The separator according to any one of claims 1 to 4, wherein the conductive layer has a thickness of 10 nm to 2000 nm.

6. The surface resistance of the conductive layer is 5×10 -1 Ω / □~5×10 4 The separator according to claim 1 , wherein the resistance is Ω / □.

7. The separator of claim 1 , wherein the additive comprises carboxymethyl cellulose.

8. The separator according to any one of claims 1 to 7, having an air permeability of 50s / 100cc to 500s / 100cc.

9. The separator according to claim 1 , wherein the conductive layer is disposed on one side of the porous substrate.

10. A secondary battery comprising an electrode and the separator according to any one of claims 1 to 9.

11. The electrodes include a positive electrode and a negative electrode, the separator is disposed between the positive electrode and the negative electrode; The positive electrode includes a positive electrode current collector and a positive electrode active material layer, the positive electrode current collector includes a non-coated portion that is not overlapped with the positive electrode active material layer, the non-coated portion including a current application portion corresponding to an end region of the non-coated portion, The secondary battery according to claim 10 , wherein the conductive layer is in contact with the current application portion.

Citation Information

Patent Citations

  • A composite electrode material, an electrode for a battery containing this material, and a lithium battery having this electrode.

    JP2012501515A

  • Multilayer porous film having electroconductive layer, and separator for battery

    JP2014208448A

  • Negative electrode for lithium ion secondary battery and for lithium ion capacitor

    JP2015156293A

  • Multilayer porous film, separator for electricity storage device, and electricity storage device

    JP2016007816A

  • Lithium-sulfur battery diaphragm and lithium-sulfur battery

    JP2018037407A

Cited By

  • Laminates and energy storage devices

    JP2026154590A