Polarizing plate, optical device, and method for manufacturing polarizing plate

The polarizing plate with a wire grid structure and ion beam assisted vapor deposition antireflection layer addresses durability issues, ensuring high reliability and optical performance in high-temperature and intense light environments.

JP7575192B2Active Publication Date: 2024-10-29DEXERIALS CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020007241
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-21
Publication Date
2024-10-29
Estimated Expiration
2040-01-21

AI Technical Summary

Technical Problem

Existing polarizing plates face issues with durability in high-temperature environments and high-intensity light conditions, and their antireflection layers may decompose, leading to reduced performance.

Method used

A polarizing plate with a wire grid structure featuring convex portions and an antireflection layer composed of alternating high and low refractive index layers, formed using ion beam assisted vapor deposition, which includes a reflective, dielectric, and absorbing layer, enhancing durability and optical properties.

Benefits of technology

The solution provides improved reliability with enhanced heat resistance, moisture resistance, and scratch resistance, maintaining optical performance under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575192000001
    Figure 0007575192000001
  • Figure 0007575192000002
    Figure 0007575192000002
  • Figure 0007575192000003
    Figure 0007575192000003
Patent Text Reader

Abstract

To provide a polarizing plate and an optical apparatus with excellent reliability.SOLUTION: This polarizing plate has a wire grid structure and includes a transparent substrate, a plurality of protrusions protruding from the first surface of the transparent substrate, and an antireflection layer laminated on the second surface opposite to the first surface of the transparent substrate, wherein the plurality of protrusions are periodically arranged at a pitch shorter than a wavelength of light in a use band, each of the protrusions extends in a first direction and includes a reflective layer, a dielectric layer, and an absorption layer in order from the first surface, the antireflection layer has high refractive index layers and low refractive index layers that are alternately laminated, and the antireflection layer is an ion beam assisted vapor deposition film or an ion beam sputtering film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate, an optical device, and a method for manufacturing a polarizing plate. [Background technology]

[0002] Polarizing plates are used in liquid crystal displays, etc. In recent years, attention has been focused on wire grid polarizing plates in which reflective layers are arranged at a period shorter than the wavelength of light in the band used.

[0003] For example, Patent Document 1 describes a polarizing plate having an antireflection layer and a wire grid in this order on a substrate.

[0004] Furthermore, for example, Patent Document 2 describes a wire grid polarizer in which an anti-reflection coating is applied to the surface on which the wire grid is formed and the surface opposite to the surface of the substrate.

[0005] Furthermore, for example, Patent Document 3 describes a polarizing element having an antireflection layer on the surface of the substrate opposite to the surface on which the wire grid is formed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2016-38537 A [Patent Document 2] JP 2005-242080 A [Patent Document 3] JP 2010-60587 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, there has been a demand for higher brightness and higher definition in liquid crystal projectors, etc., and there is a demand for polarizing plates that are durable even in environments with high luminosity and strong light, and also have high transmittance characteristics.

[0008] The antireflection layer of the polarizing plate described in Patent Document 1 is composed of hollow particles, a solvent, and a binder, and the organic matter remaining in the antireflection layer may decompose in a high-temperature environment, resulting in a deterioration in characteristics. The antireflection layers of the polarizers described in Patent Documents 2 and 3 are not described in detail, and may not have sufficient durability.

[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide a polarizing plate and an optical device having excellent reliability. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides the following means.

[0011] A polarizing plate according to a first aspect is a polarizing plate having a wire grid structure, comprising a transparent substrate, a plurality of convex portions protruding from a first surface of the transparent substrate, and an antireflection layer laminated on a second surface of the transparent substrate opposite the first surface, wherein the plurality of convex portions are periodically arranged at a pitch shorter than the wavelength of light in the used band, each convex portion extends in a first direction, and comprises, in order from the first surface, a reflective layer, a dielectric layer, and an absorbing layer, wherein the antireflection layer has a high refractive index layer and a low refractive index layer laminated alternately, and the antireflection layer is an ion beam assisted deposition film or an ion beam sputtering film.

[0012] A polarizing plate according to a second aspect is a polarizing plate having a wire grid structure, comprising a transparent substrate, a plurality of convex portions protruding from a first surface of the transparent substrate, and an antireflection layer laminated on a second surface of the transparent substrate opposite the first surface, wherein the plurality of convex portions are periodically arranged at a pitch shorter than the wavelength of light in the used band, and each convex portion extends in a first direction, and comprises, in order from the first surface, a reflective layer, a dielectric layer, and an absorbing layer, wherein the antireflection layer has high refractive index layers and low refractive index layers laminated alternately, and the contrast reduction rate after 1000 hours at a temperature of 250°C is less than 40%.

[0013] A polarizing plate according to a third aspect is a polarizing plate having a wire grid structure, comprising a transparent substrate, a plurality of convex portions protruding from a first surface of the transparent substrate, and an antireflection layer laminated on a second surface of the transparent substrate opposite the first surface, wherein the plurality of convex portions are periodically arranged at a pitch shorter than the wavelength of light in the used band, and each convex portion extends in a first direction, and comprises, in order from the first surface, a reflective layer, a dielectric layer, and an absorbing layer, wherein the antireflection layer has a high refractive index layer and a low refractive index layer laminated alternately, and wherein the antireflection layer has a peel load of 33 mN or more in a microscratch test in accordance with JIS R3255 at a scratch speed of 10 μm / sec.

[0014] An optical device according to a fourth aspect includes the polarizing plate according to the above aspect.

[0015] A manufacturing method for a polarizing plate according to a fifth aspect is a manufacturing method for a polarizing plate having a wire grid structure, and includes the steps of forming high refractive index layers and low refractive index layers alternately on one surface of a transparent substrate by ion beam assisted deposition or ion beam sputtering, and laminating an anti-reflection layer, laminating a reflective layer, a dielectric layer, and an absorbing layer, in that order, on the surface of the transparent substrate opposite to the surface on which the anti-reflection layer is laminated, to form a laminate, and processing the laminate to form a plurality of convex portions that are periodically arranged at a pitch shorter than the wavelength of light in the band of light used. Effect of the Invention

[0016] According to the polarizing plate and the optical device according to the above aspect, the reliability can be improved. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a perspective view of a polarizing plate according to a first embodiment. [Diagram 2] 1 is a cross-sectional view of a polarizing plate according to a first embodiment. [Diagram 3] 1 is a cross-sectional view of a characteristic portion of a polarizing plate according to a first embodiment. [Figure 4] 1 is a cross-sectional photograph of an antireflection layer. [Diagram 5]FIG. 4 is a graph showing the change over time in wettability of an antireflection layer. [Figure 6] FIG. 4 is a diagram showing the absorption axis transmittance of a polarizing plate. [Figure 7] FIG. 4 is a diagram showing the transmission axis transmittance of a polarizing plate. [Figure 8] FIG. 13 is a diagram showing the results of a heat resistance test of a polarizing plate. [Figure 9] FIG. 13 is a diagram showing the results of a scratch test on the polarizing plate according to Comparative Example 1. [Figure 10] FIG. 4 is a diagram showing the results of a scratch test on the polarizing plate according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. They may be modified as appropriate within the scope of the effects of the present invention.

[0019] "Polarizing plate" 1 is a perspective view of a polarizing plate 100 according to a first embodiment. The polarizing plate 100 includes a transparent substrate 10, a plurality of protrusions 20, and an antireflection layer 30. The plurality of protrusions 20 protrude from a first surface 10A of the transparent substrate 10. The antireflection layer 30 is laminated on a second surface 10B of the transparent substrate 10. The second surface 10B is the surface of the transparent substrate 10 opposite to the first surface 10A.

[0020] Here, the directions are defined. The plane in which the transparent substrate 10 extends is defined as the XY plane, and the direction in which the protrusions 20 extend is defined as the Y direction. The direction perpendicular to the Y direction is defined as the X direction. The direction perpendicular to the X and Y directions is defined as the Z direction. The Y direction is an example of a first direction.

[0021] The polarizing plate 100 attenuates polarized waves (TE waves (S waves)) having an electric field component parallel to the Y direction in which the convex portions 20 extend, and transmits polarized waves (TM waves (P waves)) having an electric field component perpendicular to the Y direction. The polarizing plate 100 has an absorption axis in the Y direction and a transmission axis in the X direction. The polarizing plate 100 attenuates TE waves and transmits TM waves through four actions: transmission, reflection, interference, and selective optical absorption of polarized waves due to optical anisotropy.

[0022] (Transparent substrate) The transparent substrate 10 is transparent to light having a wavelength in the band used by the polarizing plate 100. The term "transparent" does not necessarily mean that the substrate transmits 100% of the light having a wavelength in the band used, but only needs to transmit enough light to maintain its function as a polarizing plate. The average thickness of the transparent substrate 10 is preferably 0.3 mm or more and 1 mm or less.

[0023] The refractive index of the transparent substrate 10 is, for example, not less than 1.1 and not more than 2.2. The transparent substrate 10 is, for example, glass, quartz crystal, sapphire, etc. The component composition of the glass material used as the transparent substrate 10 is not particularly limited.

[0024] For example, silicate glass is widely distributed as optical glass and is inexpensive. Quartz glass (refractive index 1.46) and soda-lime glass (refractive index 1.51) are also inexpensive and have excellent transparency. In contrast, quartz and sapphire have excellent thermal conductivity. The material of the transparent substrate 10 can be appropriately selected depending on the performance required of the polarizing plate 100. For example, polarizing plates for the optical engine of a projector are irradiated with strong light, so light resistance and heat dissipation are required. It is preferable to use quartz or sapphire for the transparent substrate 10 used for projectors.

[0025] When the transparent substrate 10 is an optically active crystal such as quartz or sapphire, the optical characteristics are improved by making the extension direction of the convex portion 20, which will be described later, parallel or perpendicular to the optical axis of the crystal. The optical axis is the directional axis in which the difference in refractive index between the ordinary ray and the extraordinary ray of light traveling in that direction is the smallest.

[0026] (Convex part) The protrusions 20 protrude from the transparent substrate 10 in the Z direction and extend in the Y direction. The protrusions 20 are periodically arranged in the X direction. The pitch P of adjacent protrusions 20 in the X direction is shorter than the wavelength of light in the band used by the polarizing plate 100. For example, the pitch P is 100 nm or more and 200 nm or less. If the pitch P is within this range, the protrusions 20 can be easily manufactured, and the mechanical stability and stability of the optical properties of the protrusions 20 are improved.

[0027] The pitch P between adjacent protrusions 20 can be measured as an average value using a scanning electron microscope or a transmission electron microscope. For example, the distance in the X direction between adjacent protrusions 20 is measured at any four points, and the pitch P is found by taking the arithmetic average. The measurement method of averaging the measurement values ​​at any four points among the multiple protrusions 20 is called the electron microscopy method.

[0028] The protrusions 20 protrude from the transparent substrate 10. The protrusions 20 protrude, for example, with the Z direction as the main direction. The average width of the protrusions 20 in the X direction is, for example, 20% to 50% of the pitch P. The average width of the protrusions 20 means the average value of the widths at each point obtained by dividing the protrusions 20 into 10 in the Z direction. The height of the protrusions 20 is, for example, 250 nm to 400 nm. The aspect ratio obtained by dividing the height of the protrusions 20 by the average width is, for example, 5 to 13.3.

[0029] Fig. 2 is a cross-sectional view of the polarizing plate 100 according to the first embodiment. Fig. 2 is a cross-sectional view of the polarizing plate 100 cut along the XZ plane. The protrusion 20 includes a reflective layer 22, a dielectric layer 24, and an absorbing layer 26, in this order from the first surface 10A.

[0030] A portion of the light incident on the polarizing plate 100 from the first surface 10A side is absorbed and attenuated as it passes through the absorbing layer 26 and the dielectric layer 24. TM (P waves) of the light that has passed through the absorbing layer 26 and the dielectric layer 24 passes through the reflective layer 22. In contrast, TE (S waves) of the light that has passed through the absorbing layer 26 and the dielectric layer 24 is reflected by the reflective layer 22. A portion of the reflected TE waves is absorbed as it passes through the absorbing layer 26 and the dielectric layer 24, and a portion is reflected again and returns to the reflective layer 22. The TE waves reflected by the reflective layer 22 interfere with each other as they pass through the absorbing layer 26 and the dielectric layer 24, and are attenuated. The polarizing plate 100 exhibits polarization characteristics due to the selective attenuation of the TE waves as described above.

[0031] <Reflective layer> The reflective layer 22 is on the first surface 10A of the transparent substrate 10. Another layer may be inserted between the transparent substrate 10 and the reflective layer 22. The reflective layer 22 protrudes in the Z direction relative to the transparent substrate 10 and extends in a strip shape in the Y direction. The reflective layer 22 reflects TE waves (S waves) and transmits TM waves (P waves). The height of the reflective layer 22 is, for example, not less than 100 nm and not more than 300 nm.

[0032] The reflective layer 22 includes a material that is reflective to light of a wavelength in the used band. The reflective layer 22 includes, for example, a simple metal such as Al, Ag, Cu, Mo, Cr, Ti, Ni, W, Fe, Si, Ge, or Ta, or an alloy thereof. The reflective layer 22 is made of, for example, aluminum or an aluminum alloy. The reflective layer 22 is not limited to a metal, and may be an inorganic film or a resin film whose surface reflectance is increased by coloring or the like.

[0033] The reflective layer can be formed at a high density by, for example, vapor deposition or sputtering, and may be made up of two or more layers made of different materials.

[0034] <Dielectric layer> The dielectric layer 24 is laminated, for example, on the reflective layer 22. The dielectric layer 24 does not necessarily need to be in contact with the reflective layer 22, and another layer may be present between the dielectric layer 24 and the reflective layer 22. The dielectric layer 24 extends in a strip shape in the Y direction.

[0035] The thickness of the dielectric layer 24 is determined according to the polarized wave reflected by the absorbing layer 26. The thickness of the dielectric layer 24 is such that the phase of the polarized wave reflected by the absorbing layer 26 and the phase of the polarized wave reflected by the reflecting layer 22 are shifted by half a wavelength. The thickness of the dielectric layer 24 is, for example, 1 nm or more and 500 nm or less. Within this range, the phase relationship between the two reflected polarized waves can be adjusted, and the interference effect can be enhanced. The thickness of the dielectric layer 24 is determined using the above-mentioned electron microscopy method.

[0036] The dielectric layer 24 includes, for example, a metal oxide, magnesium fluoride (MgF2), cryolite, germanium, silicon, boron nitride, carbon, or a combination thereof. The metal oxide is, for example, a Si oxide such as SiO2, Al2O3, beryllium oxide, bismuth oxide, boron oxide, tantalum oxide, etc. The dielectric layer 24 is, for example, a Si oxide or a Ti oxide.

[0037] The refractive index of the dielectric layer 24 is, for example, greater than 1.0 and equal to or less than 2.5. Since the optical characteristics of the reflective layer 22 are also affected by the refractive index of the surroundings (for example, the refractive index of the dielectric layer 24), the polarization characteristics can be controlled by adjusting the refractive index of the dielectric layer 24.

[0038] The dielectric layer 24 can be formed by, for example, evaporation, sputtering, chemical vapor deposition (CVD), or atomic layer deposition (ALD). The dielectric layer 24 may be two or more layers.

[0039] <Absorption layer> The absorbing layer 26 is, for example, laminated on the dielectric layer 24. The absorbing layer 26 extends in a strip shape in the Y direction. The thickness of the absorbing layer 26 is, for example, 5 nm or more and 50 nm or less. The thickness of the absorbing layer 26 can be measured by the above-mentioned electron microscope method.

[0040] The absorbing layer 26 includes one or more substances having a light absorbing effect and an optical constant whose extinction constant is not zero. The absorbing layer 26 includes, for example, a metal material or a semiconductor material. The material used for the absorbing layer 26 is appropriately selected depending on the wavelength range of the light in the band used.

[0041] When a metal material is used for the absorption layer 26, the metal material is, for example, a single metal such as Ta, Al, Ag, Cu, Au, Mo, Cr, Ti, W, Ni, Fe, or Sn, or an alloy containing one or more of these elements. When a semiconductor material is used for the absorption layer 26, the semiconductor material is, for example, Si, Ge, Te, ZnO, or a silicide material. Examples of the silicide material include β-FeSi2, MgSi2, NiSi2, BaSi2, CrSi2, and TaSi. A polarizing plate 100 using these materials for the absorption layer 26 has a high extinction ratio in the visible light range. The absorption layer 26 also contains, for example, Fe or Ta and Si.

[0042] When the absorption layer 26 is a semiconductor material, the band gap energy of the semiconductor contributes to the light absorption. The band gap energy of the semiconductor material is, for example, equal to or less than the value obtained by converting the wavelength of the band used into energy. For example, when the band used is the visible light range, the absorption layer 26 is made of a semiconductor material having a band gap energy of 3.1 eV or less, which corresponds to the absorption energy at wavelengths of 400 nm or more.

[0043] The absorption layer 26 is not limited to one layer, and may be composed of two or more layers. When the absorption layer 26 is composed of two or more layers, the materials of each layer may be different. The absorption layer 26 can be formed by a method such as vapor deposition or sputtering.

[0044] (Anti-reflection layer) The antireflection layer 30 is laminated on a second surface 10B opposite to the first surface 10A on which the convex portions 20 of the transparent substrate 10 are formed. Fig. 3 is a cross-sectional view of a characteristic portion of the polarizing plate 100 according to the first embodiment. Fig. 3 is an enlarged cross-sectional view of the antireflection layer 30 of the polarizing plate 100.

[0045] The anti-reflection layer 30 prevents reflection by utilizing the interference of light. The anti-reflection layer 30 is formed by alternately stacking low-refractive index layers 31 and high-refractive index layers 32. The low-refractive index layers 31 have a lower refractive index than the adjacent layers. The high-refractive index layers 32 have a higher refractive index than the adjacent layers. The low-refractive index layers 31 have a lower refractive index than the transparent substrate 10, for example, greater than 1.0. The high-refractive index layers 32 have a higher refractive index than the low-refractive index layers 31, for example. The thicknesses of the low-refractive index layers 31 and the high-refractive index layers 32 are appropriately selected depending on the wavelength range of the light in the band of use, etc. The thicknesses of the low-refractive index layers 31 and the high-refractive index layers 32 are, for example, 1 nm or more and 500 nm or less. The thicknesses of the low-refractive index layers 31 and the high-refractive index layers 32 may be different from each other.

[0046] The low refractive index layer 31 and the high refractive index layer 32 are dielectric layers. The low refractive index layer 31 and the high refractive index layer 32 are made of, for example, oxides such as Si oxide, Ti oxide, Zr oxide, Al oxide, Nb oxide, Ta oxide, Bi oxide, and Be oxide, magnesium fluoride, cryolite, germanium, silicon, and carbon. For example, the low refractive index layer 31 is made of SiO2, and the high refractive index layer 32 is made of TiO2 or NbO2.

[0047] The anti-reflection layer 30 is, for example, an ion beam assisted deposition film or an ion beam sputtering film. The ion beam assisted deposition film is a film formed by an ion beam assisted deposition (IAD) method. The ion beam sputtering film is a film formed by an ion beam sputtering (IBS) method.

[0048] Figure 4 shows cross-sectional photographs of an antireflection layer. Figure 4(a) shows an antireflection layer 30 formed by ion-beam assisted deposition, and Figure 4(b) shows an antireflection layer formed by vacuum deposition. The black part is a TiO2 layer 32A, the white part is a SiO2 layer 31A, and the gray part is a transparent substrate 10.

[0049] As shown in Figure 4(b), the anti-reflection layer formed by the vacuum deposition method has multiple white lines in the Z direction, and grain boundaries can also be seen. Also, altered layers that look different from other parts were found in various places within the layer. The altered layers are probably affected by moisture or heat during the manufacturing process. Furthermore, the results of energy dispersive X-ray analysis showed that the oxygen distribution at the interface of each layer in the anti-reflection layer formed by the vacuum deposition method was unclear. Furthermore, evaluation by electron energy loss spectroscopy (EELS) showed that the TiO2 layer 32A of the anti-reflection layer formed by the vacuum deposition method was composed of polycrystals containing TiO2 with an anatase type crystal structure.

[0050] In contrast, the anti-reflection layer 30 formed by the ion beam assisted deposition method is homogeneous, has no visible grain boundaries, and is dense. The anti-reflection layer 30 formed by the ion beam assisted deposition method also has a smoother interface than the anti-reflection layer formed by the vacuum deposition method. In addition, the results of energy dispersive X-ray analysis confirmed that the anti-reflection layer 30 formed by the ion beam assisted deposition method had a clear oxygen distribution, with differences in oxygen concentration even at the interfaces of each layer.

[0051] (protective layer, water-repellent layer) The polarizing plate 100 may have other components in addition to the transparent substrate 10, the convex portions 20, and the anti-reflection layer 30. For example, the polarizing plate 100 may have a protective layer on the light incident surface side. The protective layer improves the reliability of the polarizing plate 100, such as heat resistance. In addition, for example, the surface of the convex portions 20 may have a water-repellent film. The water-repellent film is made of a fluorine-based silane compound such as perfluorodecyltriethoxysilane (FDTS). The water-repellent film can be formed by, for example, a CVD method or an ALD method. The water-repellent film improves the reliability of the polarizing plate 100, such as moisture resistance.

[0052] "Method of manufacturing polarizing plate" The method for manufacturing the polarizing plate 100 according to this embodiment includes a step of forming the antireflection layer 30, a step of laminating a laminate that serves as the base of the protrusions, and a step of processing the laminate into the protrusions 20.

[0053] First, low refractive index layers 31 and high refractive index layers 32 are alternately laminated on the second surface 10B of the transparent substrate 10. The low refractive index layers 31 and high refractive index layers 32 are formed by ion beam assisted deposition or ion beam sputtering. The number of low refractive index layers 31 and high refractive index layers 32 can be changed as appropriate. The thickness of each of the low refractive index layers 31 and high refractive index layers 32 is appropriately selected depending on the wavelength range of the light in the band of use, etc. The low refractive index layers 31 and high refractive index layers 32 are alternately laminated to form an anti-reflection layer 30 on the second surface 10B.

[0054] Next, in the film formation process, a layer to be a reflective layer, a layer to be a dielectric layer, and a layer to be an absorbing layer are laminated in this order on the first surface 10A of the transparent substrate 10 to form a laminate. These layers are formed by, for example, a sputtering method or a vapor deposition method.

[0055] Finally, the laminate is processed. For example, a photolithography method, a nanoimprint method, or the like is used for processing the laminate. For example, a mask pattern is formed in a one-dimensional lattice shape with resist on one surface of the laminate. The convex portion 20 is formed by selectively etching the portion where the resist is not formed. The etching is performed by, for example, dry etching. Furthermore, after forming the convex portion 20, a protective layer and a water-repellent layer may be formed thereon.

[0056] The polarizing plate 100 according to this embodiment has excellent reliability. The reliability includes, for example, moisture resistance, heat resistance, and scratch resistance.

[0057] Fig. 5 is a diagram showing the change over time in wettability of the antireflection layers of Example 1 and Comparative Example 1. The horizontal axis indicates the time elapsed since the surface of the antireflection layer was plasma-treated with O2, and the vertical axis indicates the contact angle of water calculated by the θ / 2 method. Example 1 is an antireflection layer produced by ion beam assisted deposition method as shown in Fig. 4a, and Comparative Example 1 is an antireflection layer produced by vacuum deposition method as shown in Fig. 4b. Both antireflection layers are made of nine layers of SiO2 and TiO2 stacked alternately.

[0058] The wettability was evaluated by treating the surface of the anti-reflection layer with O2 plasma, dripping water on it after a certain time had passed, and measuring the contact angle of the dripped water. The O2 plasma treatment was performed to ensure that the initial surface condition of the anti-reflection layer was consistent.

[0059] In both Example 1 and Comparative Example 1, the wettability was high immediately after the O2 plasma treatment. This is believed to be because the surface of the antireflective layer was activated by the O2 plasma treatment, exposing hydrophilic groups. The antireflective layer of Comparative Example 1 did not change in wettability even after time had passed. In contrast, the antireflective layer of Example 1 decreased in wettability over time, and water repellency increased. The antireflective layer of Example 1 had a water contact angle of 20 degrees or more after 300 hours had passed. This is believed to be because the effect of the O2 plasma treatment decreased over time after the O2 plasma treatment, and the water contact angle was affected by the surface condition of the antireflective layer. The antireflective layer of Example 1 was dense and highly smooth because it was produced by ion beam assisted deposition.

[0060] The antireflection layer according to Example 1 has better water repellency than the antireflection layer according to Comparative Example 1, and therefore the polarizing plate according to Example 1 has better moisture resistance than the polarizing plate according to Comparative Example 1.

[0061] 6 and 7 are diagrams showing the optical characteristics of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1. Each polarizing plate has a reflective layer made of Al and having a height of 250 nm from the transparent substrate side as a convex portion on the surface of the transparent substrate opposite to the surface having the antireflection layer, a dielectric layer made of SiO2 and having a thickness of 5 nm, and an absorption layer made of FeSi and having a thickness of 25 nm. FIG. 6 shows the results of the absorption axis transmittance of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1. The horizontal axis of FIG. 6 is the wavelength, and the vertical axis is the absorption axis transmittance. FIG. 7 shows the results of the transmission axis transmittance of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1. The horizontal axis of FIG. 7 is the wavelength, and the vertical axis is the transmission axis transmittance.

[0062] The polarizing plates having the antireflection layers of Example 1 and Comparative Example 1 differ only in the manufacturing method of the antireflection layer as described above, and the transparent substrate 10 and the convex portion 20 are the same. The fact that the shape of the convex portion 20 is the same can be confirmed by the fact that the absorption axis transmittance of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1 is approximately the same. The difference in the transmission axis transmittance of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1 is due to the difference in the antireflection layers. As shown in FIG. 7, the polarizing plate having the antireflection layer of Example 1 has superior optical properties to the polarizing plate having the antireflection layer of Comparative Example 1 over the entire visible light range.

[0063] FIG. 8 shows the results of a heat resistance test of the polarizing plates having the antireflection layers of Example 1 and Comparative Example 1. The horizontal axis indicates the evaluation time, and the vertical axis indicates the rate of change in contrast. In the heat resistance test, the polarizing plate was left in a clean oven heated to 250° C., and the difference in contrast before and after leaving it was evaluated. The contrast was calculated by dividing the transmission axis transmittance by the absorption axis transmittance. The evaluation was performed using, as an example, the case where the incident light was in the green band of the visible light range (wavelength of 520 nm to 590 nm).

[0064] As shown in Fig. 8, the contrast reduction rate of the polarizing plate having the antireflection layer of Example 1 was smaller than that of Comparative Example 1. The polarizing plate having the antireflection layer of Example 1 had a contrast reduction rate of less than 40% after 1000 hours at a temperature of 250°C. This is believed to be because the antireflection layer of Example 1 was dense as it was produced by ion beam assisted deposition and was therefore less susceptible to heat effects. Heat effects include excessive oxidation caused by oxygen penetrating into the interior.

[0065] 8, the case where the incident light is in the green band of the visible light range (wavelength of 520 nm or more and 590 nm or less) was taken as an example, but similar results were obtained when the incident light is in the red band of the visible light range (wavelength of 600 nm or more and 680 nm or less) and when the incident light is in the blue band of the visible light range (wavelength of 430 nm or more and 510 nm or less), although the rate of change in contrast is slightly different. In other words, the polarizing plate having the antireflection layer of Example 1 is more excellent in heat resistance than the polarizing plate having the antireflection layer of Comparative Example 1.

[0066] Figures 9 and 10 are diagrams showing the results of the scratch test on the polarizing plates of Example 1 and Comparative Example 1. Figure 9 shows the result of the scratch test on the polarizing plate of Comparative Example 1, and Figure 10 shows the result of the scratch test on the polarizing plate of Example 1. The lower part of Figures 9 and 10 shows the surface state of the antireflection layer after evaluation. The scratch test was performed using a Rhesca CSR-2000 (manufactured by Rhesca Co., Ltd.).

[0067] The scratch test was performed by placing a stylus on the surface of the anti-reflection layer of the polarizing plate. The scratch test was performed in accordance with JIS R-3255. The excitation amplitude of the stylus was 100 μm, the excitation frequency was 45 Hz, the scratch speed was 10 μm / sec, the initial load was 0 mN, the maximum load was 75 mN, the measurement time was 60 seconds, and the stylus diameter was 15 μm. Sensor 1 is an integral processing of the delay in the movement of the stylus relative to the horizontal excitation, and corresponds to the friction force in a theoretical approximation formula. Sensor 2 indicates the vibration acceleration of the stylus in the vertical direction. The load indicates the load applied to the thin film.

[0068] As shown in Fig. 9, the antireflection layer according to Comparative Example 1 peeled off when a load of 33 mN was applied. That is, the peeling load of the antireflection layer according to Comparative Example 1 was 33 mN. In contrast, as shown in Fig. 10, the antireflection layer according to Example 1 did not peel off even when a load of 75 mN was applied. That is, the polarizing plate having the antireflection layer of Example 1 is more excellent in abrasion resistance than the polarizing plate having the antireflection layer of Comparative Example 1.

[0069] "Optical equipment" The optical device according to the second embodiment includes the polarizing plate 100 according to the first embodiment. Examples of optical devices include liquid crystal projectors, head-up displays, and digital cameras. The polarizing plate 100 according to the first embodiment is highly reliable and can be used for various purposes. The polarizing plate 100 is made of an inorganic material. The polarizing plate 100 is particularly suitable for use in liquid crystal projectors, head-up displays, and the like, which require higher heat resistance than organic polarizing plates.

[0070] When an optical device includes a plurality of polarizing plates, at least one of the plurality of polarizing plates may be the polarizing plate 100 according to the first embodiment. For example, when the optical device is a liquid crystal projector, polarizing plates are arranged on the entrance side and exit side of a liquid crystal panel. The polarizing plate 100 according to the first embodiment is used for one of the polarizing plates.

[0071] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the specific embodiment, and various modifications and changes are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0072] 10 Transparent substrate 10A 1st side 10B 2nd side 20 Convex 22 Reflective layer 24 Dielectric layer 26 Absorbing Layer 30 Anti-reflection layer 31 Low refractive index layer 32 High refractive index layer 100 Polarizing Plate

Claims

1. A polarizing plate having a wire grid structure, A transparent substrate; A plurality of protrusions protruding from a first surface of the transparent substrate; an anti-reflection layer laminated on a second surface of the transparent substrate opposite to the first surface; the plurality of protrusions are periodically arranged at a pitch shorter than the wavelength of light in the used band, Each of the protrusions extends in a first direction and includes a reflective layer, a dielectric layer, and an absorbing layer in this order from the first surface, The reflective layer has a thickness of 100 nm or more and 300 nm or less, and is made of Al; The dielectric layer has a thickness of SiO 2 of 1 nm to 500 nm, The thickness of the absorption layer is FeSi from 5 nm to 50 nm, The antireflection layer is made up of nine layers of low refractive index layers and high refractive index layers stacked alternately, The anti-reflection layer is an ion-beam assisted deposition film or an ion-beam sputtering film, A polarizing plate having a contrast reduction rate of less than 40% after 1000 hours at a temperature of 250°C.

2. 2. The polarizing plate according to claim 1, wherein the antireflection layer has a peel load of 33 mN or more in a microscratch test at a scratch speed of 10 μm / sec according to JIS R3255.

3. An optical device comprising the polarizing plate according to claim 1 or 2.

4. A method for producing a polarizing plate having the wire grid structure according to claim 1 or 2, comprising the steps of: A step of depositing a high refractive index layer and a low refractive index layer alternately on one surface of a transparent substrate by an ion beam assisted deposition method or an ion beam sputtering method, and laminating an anti-reflection layer; forming a laminate by sequentially laminating a reflective layer, a dielectric layer, and an absorbing layer on a surface of the transparent substrate opposite to the surface on which the anti-reflection layer is laminated; and processing the laminate to form a plurality of convex portions that are periodically arranged at a pitch shorter than the wavelength of light in the band of use.

Citation Information

Patent Citations

  • Plastic optical member and production thereof

    JP1989197701A

  • Optical article having antireflection layer

    JP1998123301A

  • Sputter source, sputter film forming apparatus, sputtering method, optical multi-layer film, optical member projection exposure apparatus

    JP2003193231A

  • Optical element having antireflection film and medical application optical equipment

    JP2005208519A

  • Wire grid polarizer

    JP2005242080A