High-index, curved-cap wire grid polarizers

A wire grid polarizer design with a high index, low index, and reflective layer, along with a convex wire end, addresses manufacturing inconsistencies, resulting in stable and efficient reflection performance.

JP7575210B2Active Publication Date: 2024-10-29MOXTEK INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020121257
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-17
Filing Date
2020-07-15
Publication Date
2024-10-29
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Existing wire grid polarizers face challenges in manufacturing consistency, particularly in achieving stable and low variation in reflection performance (Rs) due to difficulties in controlling nanometer-sized wires, leading to fluctuations in performance across and within wafers.

Method used

The implementation of a wire grid polarizer design with a high index layer, low index layer, and reflective layer, combined with a convex shape at the distal end of each wire, and optimized layer configurations to minimize manufacturing variations and enhance reflection performance.

Benefits of technology

The proposed design achieves improved and consistent reflection performance (Rs) with reduced variations, enhancing the overall efficiency and manufacturability of wire grid polarizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575210000003
    Figure 0007575210000003
  • Figure 0007575210000004
    Figure 0007575210000004
  • Figure 0007575210000005
    Figure 0007575210000005
Patent Text Reader

Abstract

To improve performance of a wire grid polarizer (WGP) by reducing variation in reflection (RS) of a polarization opposite to a predominant polarization.SOLUTION: Each wire 12 of a wire grid polarizer (WGP) can include the following layers moving outwards from a substrate 11: a high-index layer HL, a low-index layer LL, and a reflective layer RL. Each wire 12 can have a distal end 12D, farthest from the substrate 11, with a convex shape. These layers and the convex shape can be combined for a more stable and improved RS.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application relates generally to wire grid polarizers. [Background technology]

[0002] Wire grid polarizers (WGPs) can divide light into two different polarization states. One polarization state can be primarily transmitted through the WGP, while the other polarization state can be primarily absorbed or reflected. The effectiveness or performance of a WGP is based on high transmission of the predominantly-transmitted polarization (sometimes called Tp), minimal transmission of the opposite polarization (sometimes called Ts), and a desired reflection of the opposite polarization (sometimes called Rs). The contrast (Tp / Ts) is a useful indicator of WGP performance.

[0003] If a reflected light beam is to be used, it can be helpful to have a high reflectance (e.g., high Rs) of the opposite polarization. For reflective WGPs, a high Rs is desirable, and the efficiency (Tp * Rs) is a useful indicator of WGP performance. It can be helpful to have a low Rs when a reflected light beam is not used and the reflected light would interfere with the optical system. Due to the difficulties in manufacturing nanometer sized wires, there can be excessive variation in Rs from wafer to wafer or even within each wafer. It would be beneficial to reduce such variation.

[0004] It has been recognized that it would be advantageous to improve wire grid polarizer (WGP) performance and reduce the variation in Rs. The present invention is directed to various embodiments of WGPs that meet these needs. Summary of the Invention

[0005] The WGP can comprise an array of wires on a surface of a substrate, with channels between adjacent wires, each wire can include the following layers moving outwardly from the substrate: a high index layer, a low index layer, and a reflective layer. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic cross-sectional side view of a wire grid polarizer (WGP) 10 comprising an array of wires 12 on a face 11F of a substrate 11, each wire 12 including a high index layer HL, a low index layer LL, and a reflective layer RL, in accordance with one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional side view of a WGP 20 similar to WGP 10, but further including distal ends 12D of each wire 12 having a convex shape, in accordance with one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional side view of a WGP 30, similar to WGPs 10 and 20, except that the reflective layer RL of WGP 20 is located at the distal end 12D of each wire 12, and the reflective layer RL has a convex shape, in accordance with one embodiment of the present invention. [Figure 4] FIG. 1 is a schematic diagram of a method of using a WGP 40 to polarize light, according to one embodiment of the present invention, comprising emitting a light beam 42 from a light source 41 to the WGP 40, with the substrate 11 of the WGP 40 facing the light source 41.

[0007] The following definitions, including plural equivalents, apply throughout this patent application.

[0008] The metal oxides referred to herein include combinations of metal and oxygen in any ratio, including non-stoichiometric combinations.

[0009] Unless otherwise expressly stated herein, all n and k values ​​(the real part of the refractive index, n, and the extinction coefficient, k) are values ​​over the wavelength range of 450 nm to 700 nm.

[0010] As used herein, the phrase "consists essentially of" and related phrases, in reference to a wire structure, means that the wire includes the mentioned thin film(s) for optical performance, but does not include other thin film(s). However, the wire may also include impurities or coatings for protection, such as from corrosion or oxidation. Substrate ribs under the wire 12 are not included in the wire for purposes of this definition.

[0011] As used herein, the term "elongated" refers to the length of the wire 12 (into the paper and across the wire width W 12 or wire thickness Th 12 (perpendicular to the wire) length L is the wire width W 12 or wire thickness Th 12 (e.g., L is substantially larger than the wire width W 12 and / or wire thickness Th 12 ≧10-fold, ≧100-fold, ≧1000-fold, or ≧10,000-fold compared to . See FIG. 1.

[0012] As used herein, the term "nm" means nanometer(s).

[0013] As used herein, the terms "on," "located on," "located at," and "located over" mean located directly on or over, with some other solid material in between. The terms "located directly on," "adjoin," "adjoins," and "adjoining" mean direct and immediate contact.

[0014] As used herein, the term "parallel" means exactly parallel, parallel within standard manufacturing tolerances, or nearly parallel, such that any deviation from exactly parallel has a negligible effect on the normal use of the device.

[0015] As used herein, the term "substrate" refers to a base material, such as a glass wafer. The substrate may be optically thick, which may mean substantially thicker than the maximum wavelength of light in the wavelength range of use, if the claims explicitly state so. For example, the thickness of the substrate, Th 11 can be ≧0.1 mm, ≧0.35 mm, or ≧0.6 mm.

[0016] As used herein, the term "ultraviolet spectrum" means ≧10 nm and <400 nm, the term "visible spectrum" means ≧400 nm and <700 nm, and the term "infrared spectrum" means ≧700 nm and <1 mm.

[0017] As used herein, the term "refractive index" means the real part of the refractive index (n) and the term "extinction coefficient" means the imaginary part of the refractive index (k).

[0018] Materials used in optical constructions can absorb some light, reflect some light, and transmit some light. The following definitions distinguish between materials that are primarily absorptive, primarily reflective, and primarily transmissive. Each material can be considered to be absorptive, reflective, or transmissive within the wavelength range of intended use, across the ultraviolet spectrum, across the visible spectrum, across the infrared spectrum, or a combination of the spectrum, and can have different properties within different wavelength ranges. Thus, whether a material is absorptive, reflective, or transmissive depends on the intended wavelength range of use. Materials are divided into absorptive, reflective, and transmissive based on the reflectance R, the real part of the refractive index n, and the imaginary part of the refractive index / extinction coefficient k. Equation 1 is used to determine the reflectance R of an interface between air and a uniform slab of material at normal incidence: TIFF0007575210000001.tif11170Unless otherwise expressly specified herein, materials with k≦0.1 within the wavelength range are "transparent" materials, materials with k>0.1 and R≦0.6 within the specified wavelength range are "absorptive", and materials with k>0.1 and R>0.6 within the specified wavelength range are "reflective". If expressly so stated in a patent claim, materials with k>0.1 and R≧0.7, R≧0.8, or R≧0.9 are "reflective" materials within the specified wavelength range.

[0019] Unless otherwise expressly stated herein, all temperature dependent values ​​are at 25°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] As shown in FIG. 1, a wire grid polarizer (WGP) 10 is shown, which is an array of wires 12, with channels 13 between adjacent wires 12, attached to a surface 11 of a substrate 11. FThe array of wires 12 may be parallel and elongated. The pitch P of the wires 12 may be less than half the lowest wavelength of the desired range of polarized light (e.g., P<200 nm for visible light polarized light). Each wire 12 may comprise or consist essentially of the following layers proceeding outwardly from the substrate 11: a high index layer HL, a low index layer LL, and a reflective layer RL. The high index layer HL is offset by the low refractive index n of the low index layer LL. L High refractive index compared to n H may have the following structure:

[0021] The following are exemplary refractive index and extinction coefficient values ​​and relationships, which may be values ​​or relationships across the ultraviolet spectrum, across the infrared spectrum, across the visible spectrum, or across a combination thereof. The following refractive index and extinction coefficient values ​​and relationships may be values ​​or relationships across a portion of the visible spectrum, such as at least 50 nm, at least 100 nm, or at least 150 nm of the visible spectrum.

[0022] Refractive index n of high index layer HL H is the refractive index n of the low index layer LL L can be higher (n H >n L ); the extinction coefficient k of the high index layer HL H is the extinction coefficient k of the low index layer LL L can be higher (k H >k L ); or both. The refractive index n of the low index layer LL L is the refractive index n of the high index layer HL H can be lower than (n L <n H ); the extinction coefficient k of the low index layer LL L is the extinction coefficient k of the high index layer HL H can be lower (k L <k H ); or both. For a reflective WGP, the extinction coefficient kH and the extinction coefficient k of the low index layer LL L For example, k H ≦0.01 and k L It can be very small, such as ≦0.01.

[0023] Refractive index n of high index layer HL H can be higher than the refractive index of any other layer in the wire. For example, the refractive index n H is n H ≧2, n H ≥ 3, or n H ≧4. In one embodiment, all layers in the wire may have a refractive index <2 or <3, except for the high index layer HL.

[0024] Extinction coefficient k of high index layer HL H can be ≦0.01 for a reflective WGP or ≧0.1 for an absorptive WGP. The extinction coefficient k L can be ≦0.01.

[0025] The extinction coefficient k of the reflective layer RL R can be higher than the extinction coefficient of any other layer in the wire. The extinction coefficient k of the reflective layer RL R is the extinction coefficient k of the high index layer HL H Higher extinction coefficient k of the low index layer LL L higher, or both (k R >k H , k R >k L , or both).

[0026] Below are exemplary materials for each of these layers, whether the exemplary materials are classified as reflective (R), absorbing (A), or transmissive (T) in the visible spectrum, and their refractive index (n) and extinction coefficient (k) values: TIFF0007575210000002.tif45170

[0027] WGP 10 can be fabricated as follows: The following layers, with the thickness of each layer in parentheses, can be applied to substrate 11 in the following order: titanium dioxide thin film (80 nm), silicon dioxide thin film (80 nm), aluminum thin film (80 nm), silicon dioxide hard mask (290 nm), aluminum hard mask (290 nm), then a resist layer. The thickness of the resist layer can vary depending on the type of resist and the lithography method.

[0028] The resist layer can be etched with fluorine, the aluminum hard mask can be etched with chlorine or bromine, the silicon dioxide hard mask can be etched with fluorine, the aluminum thin film can be etched with chlorine or bromine to form the reflective layer RL, the silicon dioxide thin film can be etched with fluorine to form the low index layer LL, and the titanium dioxide thin film can be etched with chlorine or bromine to form the high index layer HL. At this stage of the etch process, the resist and aluminum hard mask should be consumed, but there will probably still be some residual silicon dioxide hard mask. Any residual silicon dioxide hard mask can then be removed by fluorine. In addition to the above, a polymer film or oxygen can be used to passivate the sides of the wires 12.

[0029] WGPs 20 and 30 shown in FIGS. 2-3 are similar to WGP 10, except that WGPs 20 and 30 have a distal end 12 of each wire 12 that has a convex shape. D As shown in FIG. 2, the top layer 24 on the reflective layer RL can have a convex shape. As shown in FIG. 3, the reflective layer RL is disposed on the distal end 12 of each wire 12. Dand the reflective layer RL may have a convex shape. WGPs 20 and 30 may be made similar to WGP 10, except that a final fluorine etch to remove residual silicon dioxide may be reduced or skipped, thus eliminating or reducing one etch step and reducing manufacturing costs.

[0030] The convex shape can be a semicircle or a semi-ellipse. The other half of the ellipse is shown by line 25 in Figures 2-3. The major axis 27 of the semi-ellipse is aligned with the surface 11 of the substrate 11 as shown in Figure 2. F Parallel to the surface 11 of the substrate 11 as shown in FIG. F It may extend perpendicular to the

[0031] The semi-elliptical shape can have an eccentricity ratio >0, ≥0.1, ≥0.25, ≥0.5, ≥0.1, ≥0.75, or ≥0.9; and ≤0.6, ≤0.75, ≤0.9, ≤0.95, ≤0.97, ≤0.98, or <0.1. For example, the WGP 20 of FIG. F 3 has a semi-elliptical major axis 27 parallel to the surface 11 of the substrate 11 and an eccentricity of about 0.91. F 2 and has a semi-elliptical major axis 27 perpendicular to the axis of curvature and an eccentricity of about 0.76.

[0032] When the top layer 24 has a convex shape as shown in Figure 2, it may be preferred that the reflective layer RL has a rectangular shape (e.g., minimal or no etch to the sides of the reflective layer RL). This can be achieved by the use of an anisotropic etch, a thick top layer 24 or a hard mask over the top layer 24, reduced etch time, higher etch bias power, lower chamber pressure, or a combination thereof. Additionally, a higher etch selectivity between the top layer 24 and the reflective layer RL can help achieve this.

[0033] Furthermore, if the top layer 24 is transmissive and has a convex shape, such convex shape can be tuned along with the thickness of the top layer 24 to improve the WGP performance, in particular to increase the transmission of the desired polarization (e.g., increase Tp) and reduce the variation in the reflection of the opposite polarization (Rs). The preferred shape of the convex shape of the top layer 24 depends on the overall WGP structure and wavelength range; however, it can be fabricated without etching to the side of the reflective layer RL, in which case the major axis 27 of the semi-elliptical shape of the convex shape is aligned with the surface 11 of the substrate 11 as shown in FIG. F , and generally preferably extends parallel to the reflective layer RL. Generally, a more anisotropic etch in combination with a higher etch selectivity between the top layer 24 and the reflective layer RL can be used to achieve this. The top layer 24 can be a remaining portion of a hard mask, or the material of the top layer 24 can be sandwiched between the hard mask and the reflective layer RL.

[0034] Depending on the use of the WGP and the material and thickness of the top layer 24, the convex shape of the top layer 24 may have a semicircular shape or the major axis 27 of the semi-elliptical shape of the convex shape of the top layer 24 may be aligned with the surface 11 of the substrate 11. F It may be preferable for the upper layer 24 to extend perpendicular to the upper surface of the reflective layer RL. This shape may provide good protection for the high index layer HL, the low index layer LL, and the reflective layer RL. To form such a structure, a thicker layer of material for the upper layer 24 may be applied along with using an etch that has lower anisotropic properties.

[0035] When the reflective layer RL has a convex shape as shown in FIG. 3, the transmission of the desired polarization (e.g., an increase in Tp) occurs when the major axis 27 of the convex semi-ellipse is aligned with the surface 11 of the substrate 11. F This can be achieved when the hard mask extends perpendicular to the reflective layer RL. This can be achieved by using a thinner hard mask, reduced bias power, increased chamber pressure, and lower selectivity of the etch chemistry between the hard mask and the material of the reflective layer RL.

[0036] If the reflective layer RL has a convex shape, and low transmission (e.g., low Ts) and high contrast (e.g., high Tp / Ts) of the opposite polarization is desired over a high Tp, then the major axis 27 of the convex semi-elliptical shape is aligned with the surface 11 of the substrate 11. F For the etch in the above section, the following can be achieved: a thicker hard mask, increased bias power, reduced chamber pressure, and higher selectivity of the etch chemistry between the hard mask and the material of the reflective layer RL.

[0037] Thus, in the WGP 30 in which the reflective layer RL has a convex shape, the high Tp (the principal axis 27 is located on the surface 11 F ) and low Ts (principal axis 27 is parallel to surface 11 F There is a trade-off between Tp and Ts (perpendicular to Ts). Each WGP can thus be tuned for an increase in Tp or a decrease in Ts, depending on which is most useful for a particular application.

[0038] WGP30 can have a higher Tp than WGP10 and 20; however, WGP10 and 20 can have a higher contrast (Tp / Ts) than WGP30. WGP10 can have an improved Rs than WGP20 and 30. WGP20 and 30 can be easier to manufacture compared to WGP10. For each WGP application, a different combination of Tp, Ts, Rs, and cost is preferred.

[0039] WGPs 10, 20, and 30 can have high Rs if the high index layer HL is transmissive (e.g., titanium dioxide) or low Rs if the high index layer HL is absorbing (e.g., silicon or germanium). Furthermore, such Rs can be stable with minimal variation in Rs from wafer to wafer or within a wafer. This improvement in Rs is due to a combination of factors including the order of layers within the wire 12, the particular materials of the layers, the particular refractive indices of the layers, the particular extinction coefficients of the layers, limiting to only a small number of such layers (e.g., three, four, or five layers) within each wire 12, and the number of layers at the distal end 12 of each wire 12. D and the rectangular cross-sectional shapes of the high index layer HL and the low index layer LL. It is the synergistic combination of these factors that provides improved and consistent Rs.

[0040] Each of the high index layer HL and the low index layer LL can have a rectangular cross-sectional shape, as shown in Figures 1-3. Fabrication of a WGP with high index layer HL and low index layer LL having a rectangular cross-sectional shape is particularly useful for reducing the variation of Rs between wafers fabricated or even within each wafer. This can be achieved by sandwiching the high index layer HL and the low index layer LL between the substrate 11 and the reflective layer RL (thus protecting the high index layer HL and the low index layer LL during the etch), and then positioning the light source 41 to face the substrate 11 instead of facing the wires 12, as described in the following section.

[0041] 4 shows a method of using WGP 40, the method including emitting a light beam 42 from a light source 41 to WGP 40, with substrate 11 of WGP 40 facing light source 41. WGP 40 can be any of the WGPs described herein. In prior art WGPs, the wires typically face the light source for minimal variation in Rs, but it is preferred to use the WGPs herein with substrate 11 facing light source 41.

Claims

1. A wire grid polarizer (WGP), comprising: an array of wires on a surface of a substrate, the array having channels between adjacent wires; each wire has a distal end furthest from the substrate, the distal end having a convex shape; each wire includes, from the substrate outwardly, the following layers, in that order: a high index layer, a low index layer, a reflective layer, and a transmissive top layer, the transmissive top layer having a convex shape; the refractive index of the high index layer is higher than the refractive index of the low index layer across the visible spectrum; the refractive index of the high index layer is higher than the refractive index of any other layer in the wire across the visible spectrum; the top layer being permeable and having a convex shape, is located at the distal end; the high index layer, the low index layer, and the reflective layer each have a rectangular cross-sectional shape; Across the visible spectrum: the refractive index of the high index layer is ≧2, WGP.

2. The high index layer and the low index layer each have a rectangular cross-sectional shape, k R >k H and k R >k L where k R is the extinction coefficient of the reflective layer, k H is the extinction coefficient of the high index layer, k L The WGP of claim 1 , wherein:

3. 2. The WGP of claim 1, wherein across the visible spectrum: the refractive index of the high index layers is ≧2, the extinction coefficient of the high index layers is ≦0.01, and the extinction coefficient of the low index layers is ≦0.

01.

4. 2. The WGP of claim 1, wherein over at least 50 nm of the visible spectrum: the refractive index of the high index layers is ≧3, the extinction coefficient of the high index layers is ≧0.1, and the extinction coefficient of the low index layers is ≦0.

01.

5. The WGP of claim 1 , wherein the convex shape of the distal end of each wire has a semi-elliptical or semi-circular shape.

6. 2. The WGP of claim 1, wherein the convex shape of the distal end of each wire has a semicircular or semi-elliptical shape, the semi-elliptical shape having a major axis extending perpendicular to the plane of the substrate and an eccentricity > 0 and < 0.

6.

7. 2. The WGP of claim 1, wherein the convex shape of the distal end of each wire has a semi-elliptical shape having a major axis extending perpendicular to a plane of the substrate and an eccentricity of > 0.6 and < 0.

98.

8. The WGP of claim 1 , wherein the convex shape of the distal end of each wire has a semicircular or semi-elliptical shape, the semi-elliptical shape having a major axis extending parallel to a plane of the substrate.

9. 13. A method of using the WGP of claim 1 to polarize light, comprising emitting a beam of light from a light source onto the WGP, the substrate facing the light source.

Citation Information

Patent Citations

  • Reflection-suppressing wire grid polarizer

    JP2010530995A

  • Optical element and projection type liquid crystal display device

    JP2012103469A

  • Polarization element

    JP2012181420A

  • Sheet polarizer and sheet polarizer manufacturing method

    JP2015034959A

  • Sheet polarizer, sheet polarizer manufacturing method, and bundle structure manufacturing method