METHOD FOR PATTERNING METAL CERAMIC SUBSTRATE AND PATTERNED METAL CERAMIC SUBSTRATE
A method for patterning metal-ceramic substrates using two etchants and strategic substrate arrangement enhances efficiency and completeness of active metal removal, addressing inefficiencies in existing methods.
Patent Information
- Application Number
- JP2021197576
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-22
- Filing Date
- 2021-12-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-06
AI Technical Summary
Existing methods for patterning metal-ceramic substrates are inefficient, resource-intensive, and require high temperatures, and do not effectively remove active metals in a timely manner.
A method involving the use of two etchants to remove metals with different melting points from a metal-ceramic substrate, where the substrates are arranged to minimize shading during etching, allowing for efficient and complete removal of active metals using optimized etching solution application.
The method enables faster, more efficient, and less resource-consuming patterning of metal-ceramic substrates with complete removal of active metals, suitable for power electronics applications.
Smart Images

Figure 0007575369000002 
Figure 0007575369000003 
Figure 0007575369000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for patterning a metal-ceramic substrate and to a patterned metal-ceramic substrate. [Background technology]
[0002] Metal-ceramic substrates play an important role in the field of power electronics. They are a key element in the construction of electronic components and ensure that the large amounts of heat generated during their operation can be quickly dissipated. Metal-ceramic substrates usually consist of a ceramic layer and a metal layer bonded on top of the ceramic layer.
[0003] Several methods for bonding metal layers to ceramic layers are known from the prior art. The so-called DCB (Direct Copper Bonding) method involves reacting copper with a reactive gas (usually oxygen) and applying a copper compound (usually copper oxide) with a lower melting point than copper to the surface of the copper foil. When the treated copper foil is applied to a ceramic body and fired, the copper compound melts and wets the surface of the ceramic body, forming a stable bond between the copper foil and the ceramic body. This method is described, for example, in patent document 1 or 2.
[0004] While the DCB method has obvious advantages, it has two main disadvantages. First, the method needs to be carried out at a relatively high temperature, slightly below the melting point of copper. Second, the method can only be used with aluminum-based ceramics, such as aluminum oxide or aluminum nitride. Therefore, an alternative method for producing metal-ceramic substrates under less stringent conditions is required. Alternatively, the metal foil can be bonded to the ceramic body at a temperature of about 650-1000°C using special solders containing silver and / or copper and active metals. The role of the active metal is to react with the ceramic material and bond the ceramic material to the rest of the solder to form a reaction layer, and the copper and / or silver serve to bond this reaction layer to the metal foil. For example, Patent Document 3 proposes bonding the copper foil to the ceramic body using a solder containing 50-89% silver by weight and further containing copper, bismuth, and an active metal. This method has been successfully used to reliably bond the copper foil to the ceramic body. To avoid problems related to silver migration, it may be advantageous to use a silver-free solder to bond the metal foil to the ceramic body. Such a technique is proposed, for example, in Patent Document 4. The metal-ceramic substrate thus produced has, in addition to a metal layer and a ceramic layer, a bonding layer that is located between the metal layer and the ceramic layer and contains an active metal.
[0005] After bonding the metal foil to the ceramic body, it is common to pattern the metal-ceramic substrate to form conductive tracks. Conventional etching techniques are usually used for this purpose. In a typical method, the metal side of the metal-ceramic substrate is masked, for example with a polymer. This masking protects the parts of the metal-ceramic substrate that will not be removed during the etching process, while leaving the unmasked parts available for etching. The metal of the metal foil and components of the bonding layer are dissolved by an etching solution and removed from the metal-ceramic substrate to form the conductive tracks. The masking is then removed, and the patterned metal-ceramic substrate is obtained.
[0006] In the conventional method, the metal of the metal foil and the solder components of the joining layer are removed during treatment with a first etching solution, leaving at least the active metal. The active metal is then dissolved and removed by treatment with a second etching solution. To achieve high throughput, the metal-ceramic substrates are usually stacked in a holding device and are contacted with the etching solution in the holding device. In particular, it has been found to be practically advantageous to stack the metal-ceramic substrates vertically. To achieve complete etching, the metal-ceramic substrates need to be in contact with the etching solution for a long period of time.
[0007] In principle, it is necessary to reduce the residence time of the metal-ceramic substrate in the etching solution, so that the method for patterning the metal-ceramic substrate can be carried out more quickly, more efficiently, with fewer resources and with less energy consumption. Furthermore, it is required that the material to be removed during etching, especially the active metal, is removed as completely as possible in a given time. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] U.S. Pat. No. 3,744,120 [Patent Document 2] German Patent No. 2319854 [Patent Document 3] Patent No. 4812985 [Patent Document 4] DE 102017114893 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention therefore aims to provide a method for convenient patterning of metal-ceramic substrates, which is preferably faster, more efficient and less resource- and / or energy-intensive than methods known from the prior art, and more preferably, which allows the material removed during etching, in particular the active metal, to be removed as completely as possible in a given time. [Means for solving the problem]
[0010] This problem is solved by the method according to claim 1.
[0011] The present invention therefore provides a method for patterning a metal-ceramic substrate, the method comprising the following steps: a) providing a first metal-ceramic substrate and a second metal-ceramic substrate, each of which comprises: A ceramic layer; A metal layer; a bonding layer located between the ceramic layer and the metal layer, the bonding layer comprising (i) a metal having a melting point of at least 700° C. and (ii) an active metal; b) providing an etchant 1 capable of removing metal from the metal layer and at least partially removing metal having a melting point of at least 700° C. from the bonding layer; c) providing an etchant 2 capable of removing the active metal from the bonding layer; d) masking areas on the metal layer of the first metal-ceramic substrate and on the metal layer of the second metal-ceramic substrate that are not intended to be ablated; e) contacting the first metal-ceramic substrate and the second metal-ceramic substrate with the etching solution 1; f) contacting the first metal ceramic substrate and the second metal ceramic substrate with the etching solution 2, wherein the first metal ceramic substrate and the second metal ceramic substrate are arranged such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 60% or less; Includes.
[0012] The present invention further provides a metal-ceramic substrate obtainable by this method.
[0013] The method according to the invention relates to the patterning of metal-ceramic substrates.
[0014] To this end, first, a first metal-ceramic substrate and a second metal-ceramic substrate are provided.
[0015] The first metal ceramic substrate and the second metal ceramic substrate each have a metal layer. The metal of the metal layer is preferably selected from the group consisting of copper, aluminum and molybdenum. According to a particularly preferred embodiment, the metal of the metal layer is selected from the group consisting of copper and molybdenum. According to a very particularly preferred embodiment, the metal of the metal layer is copper. The metal layer preferably has a thickness in the range of 0.01 to 10 mm, more preferably in the range of 0.03 to 5 mm, and particularly preferably in the range of 0.05 to 3 mm.
[0016] The first and second metal ceramic substrates each have a ceramic layer. The ceramic of the ceramic layer is preferably an insulating ceramic. The ceramic may be, for example, an oxide-based ceramic, a nitride-based ceramic, a carbide-based ceramic, etc. Preferably, the ceramic is a metal oxide ceramic, a silicon oxide ceramic, a metal nitride ceramic, a silicon nitride ceramic, a boron nitride ceramic, or a boron carbide ceramic. According to a preferred embodiment, the ceramic is selected from the group consisting of aluminum nitride ceramic, silicon nitride ceramic, and aluminum oxide ceramic (such as ZTA ("zirconia toughened alumina") ceramic). The ceramic layer preferably has a thickness in the range of 0.05 to 10 mm, more preferably in the range of 0.1 to 5 mm, and even more preferably in the range of 0.15 to 3 mm.
[0017] The first metal-ceramic substrate and the second metal-ceramic substrate each have a bonding layer located between the ceramic layer and the metal layer, the bonding layer preferably providing a physical bond between the ceramic layer and the metal layer.
[0018] The bonding layer includes (i) a metal having a melting point of 700°C or more and (ii) an active metal. The metal having a melting point of 700°C or more is preferably a melting point of 850°C or more, more preferably a melting point of 1000°C or more. According to a preferred embodiment, the metal having a melting point of at least 700°C is selected from the group consisting of copper, silver, nickel, tungsten, molybdenum and mixtures thereof. According to a particularly preferred embodiment, the metal having a melting point of at least 700°C is selected from the group consisting of copper, nickel, tungsten, molybdenum and mixtures thereof. According to a particularly very preferred embodiment, the metal having a melting point of at least 700°C is copper. The content of the at least one metal having a melting point of at least 700°C is preferably 55 to 93 atomic %, particularly preferably 60 to 85 atomic %, most preferably 65 to 80 atomic %, based on the number of atoms in the bonding layer.
[0019] The active metal is preferably selected from the group consisting of titanium, zirconium, niobium, tantalum, vanadium, hafnium and mixtures thereof. According to a particularly preferred embodiment, the active metal is titanium. The content of the active metal is preferably 1 to 10 atomic %, particularly preferably 2 to 8 atomic %, and most preferably 3 to 7 atomic %, based on the number of atoms in the bonding layer.
[0020] According to a preferred embodiment, the bonding layer may contain (i) a metal having a melting point of at least 700° C. and (ii) an active metal, and may further contain (iii) an additional element as a remaining element. According to a particularly preferred embodiment, the content of the additional element in the bonding layer is 5 to 40 atomic %, more preferably 7 to 35 atomic %, and particularly preferably 10 to 35 atomic %, based on the number of atoms in the bonding layer.
[0021] Therefore, according to a further preferred embodiment, the bonding layer is made of a metal having a melting point of less than 700°C. The metal having a melting point of less than 700°C is preferably less than 600°C, more preferably less than 550°C. According to a preferred embodiment, the metal having a melting point of less than 700°C is selected from the group consisting of tin, bismuth, indium, gallium, zinc, antimony, magnesium, and mixtures thereof. According to a particularly preferred embodiment, the metal having a melting point of less than 700°C is selected from the group consisting of tin, bismuth, and mixtures thereof. The content of at least one metal having a melting point of less than 700°C is preferably 5 to 40 atomic %, more preferably 7 to 35 atomic %, and particularly preferably 10 to 35 atomic %, based on the number of atoms in the bonding layer.
[0022] According to a preferred embodiment, the bonding layer has a region adjacent to the metal layer and a region adjacent to the ceramic layer. The region adjacent to the metal layer is preferably richer in metals having a melting point of 700° C. or more than the region adjacent to the ceramic layer. The region adjacent to the ceramic layer is preferably richer in active metals than the region adjacent to the metal layer. According to a particularly preferred embodiment, the region adjacent to the metal layer is thicker than the region adjacent to the ceramic layer of the bonding layer. In addition, the ratio of the thickness of the region adjacent to the metal layer of the bonding layer to the thickness of the region adjacent to the ceramic layer of the bonding layer is preferably 2:1 or more, more preferably 3:1 or more, and may be particularly preferably 5:1 or more.
[0023] According to a preferred embodiment, the maximum content of silver is preferably 15.0 at.%, more preferably 1.0 at.%, even more preferably 0.5 at.%, very particularly preferably 0.1 at.%, based on the number of atoms in the bonding layer. It may therefore be preferred that the bonding layer is free of silver or low in silver. Surprisingly, it has been found that the mere absence of silver in the bonding layer or a low content of silver in the bonding layer leads to the fact that a reliable and complete removal of the active metal from the area of the bonding layer to be etched can be achieved in a short time by the method according to the invention. Without being bound by theory, it is believed that this effect is due to the fact that the presence of silver favors the formation of areas near the metal layer that are difficult to remove by etching. The formation of this area near the metal layer containing silver may ultimately lead to an effective prevention of contact between the area near the ceramic layer containing active metal and the etching solution 2. It is believed that this prevention is reduced or eliminated by reducing the proportion of silver in the bonding layer, making the removal of the active metal easier.
[0024] According to a preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate each comprise: a second metal layer; a second bonding layer located between the ceramic layer and the second metal layer, the second bonding layer comprising: (i) a metal having a melting point of at least 700° C.; and (ii) an active metal; Equipped with.
[0025] Such a metal-ceramic substrate is also called a double-sided metal-ceramic substrate. With regard to the characteristics of the second metal layer and the second bonding layer, reference can be made to the description of the metal layer and the bonding layer described herein. Preferably, the second metal layer is thus formed as a metal layer described herein, and the second bonding layer is formed as a bonding layer described herein.
[0026] The metal-ceramic substrate can be produced by the usual methods known in the prior art. Preferably, the metal-ceramic substrate is produced by a soldering method. According to a preferred embodiment, the metal-ceramic substrate is produced by the AMB ("Active Metal Brazing") method. In this method, a metal foil is brazed to a ceramic body using a brazing material that usually consists of copper, silver and an active metal (e.g. titanium). Such a method is disclosed, for example, in US Pat. No. 4,591,535. According to another preferred embodiment, the metal-ceramic substrate is produced by a method of soldering a metal foil to a ceramic body using a solder material that includes a metal having a melting point of at least 700° C. (e.g. copper), a metal having a melting point of less than 700° C. (e.g. tin) and an active metal (e.g. titanium). Such a method is disclosed, for example, in US Pat. No. 4,591,535.
[0027] In the method according to the invention, an etching solution 1 is provided that is capable of removing the metal of the metal layer and at least partially the metal with a melting point of 700° C. from the bonding layer. The etching solution 1 may for example be an etching solution known from the prior art and suitable for etching copper. Thus, the etching solution 1 may be, for example, FeCl 3 Etchant and CuCl 2 The etching solution may be selected from the group consisting of:
[0028] The method according to the invention further provides an etchant 2 capable of removing active metals from the bonding layer. Etchant 2 may be an etchant for active metals known in the prior art. Exemplary etchants are disclosed in EP 3 688 835 A1 and EP 3 684 148 A1. According to a preferred embodiment, etchant 2 is selected from the group consisting of an etchant comprising hydrogen peroxide and an etchant comprising ammonium peroxodisulfate. For example, etchant 2 may be a mixture of ammonium fluoride and fluoroboric acid (e.g. HBF 4 ) and hydrogen peroxide and / or ammonium peroxodisulfate.
[0029] According to the invention, the first metal-ceramic substrate and the second metal-ceramic substrate are masked in areas where ablation is not intended. The masking is not further limited and can be performed by a method known to a person skilled in the art from the prior art. For example, an etching resist can be used for the masking. For example, an etching resist can be applied to the metal layer of the metal-ceramic substrate, and only the areas where ablation is not intended are exposed for curing. Then, when contacting with an etching solution, the masked areas are protected so that the action of the etching solution does not remove material in these areas. On the other hand, the unmasked (uncured) areas can be etched in a subsequent etching step.
[0030] According to the present invention, the first metal-ceramic substrate and the second metal-ceramic substrate are then contacted with the etching solution 1. In this step, under the action of the etching solution 1, in the unmasked areas of the metal-ceramic substrate, the metal is removed from the metal layer and the metal having a melting point of at least 700°C is at least partially removed from the bonding layer. Furthermore, the etching solution 1 can also be designed such that, in addition to the metal of the metal layer and the metal having a melting point of at least 700°C, other metals (if present) of the bonding layer are also removed, except for the active metal. The method of contacting the metal-ceramic substrate with the etching solution 1 is not particularly limited. It may be preferably provided that the metal-ceramic substrate is immersed or sprayed in the etching solution 1.
[0031] Next, the first metal ceramic substrate and the second metal ceramic substrate are contacted with the etching solution 2. In this step, the active metal is removed in the unmasked areas of the metal ceramic substrate by the action of the etching solution 2. At this time, the first metal ceramic substrate and the second metal ceramic substrate are arranged so that when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 60% or less. According to a preferred embodiment, the first metal ceramic substrate and the second metal ceramic substrate are contacted with the etching solution 2, and the first metal ceramic substrate and the second metal ceramic substrate are arranged so that when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 50% or less, particularly preferably 40% or less, very particularly preferably 30% or less, for example 15% or less.
[0032] The orthogonal projection of the first metal-ceramic substrate is on a projection plane parallel to the metal layer of the first metal-ceramic substrate. Preferably, the projection plane spans an image obtained by translating the first metal-ceramic substrate. Preferably, the displacement is in a direction perpendicular to the metal layer of the first metal-ceramic substrate. This translation can be in one direction, but also in the opposite direction. The distance between the metal layer of the first metal-ceramic substrate and the projection plane parallel thereto is preferably selected such that the distance between the metal layer of the first metal-ceramic substrate and the projection plane parallel thereto is equal to or greater than the distance between the metal layer of the first metal-ceramic substrate and the plane spanned by the second metal-ceramic substrate, and the distance between the metal layer of the first metal-ceramic substrate and the plane spanned by the second metal-ceramic substrate is preferably determined along a perpendicular line passing through the center of gravity of the metal layer of the first metal-ceramic substrate. It is therefore preferred that the distance between the metal layer of the first metal-ceramic substrate and the projection plane parallel thereto is large enough to achieve partial shading of the second metal-ceramic substrate in the orthogonal projection, insofar as this is at all possible due to the arrangement of the first and second metal-ceramic substrates. The distance between the metal layer of the first metal-ceramic substrate and the projection plane parallel thereto may be 20 cm, 30 cm or 50 cm. For example, the distance between the metal layer of the first metal-ceramic substrate and the projection plane parallel thereto may correspond to the length of the largest side of the first metal-ceramic substrate.
[0033] If the second metal-ceramic substrate is placed between the metal layer of the first metal-ceramic substrate and a projection plane parallel thereto, the metal layer can be shaded by orthogonal projection, if necessary. According to the invention, shading occurs regardless of whether the metal layer of the first metal-ceramic substrate faces or is away from the metal layer of the second metal-ceramic substrate. Thus, shading of the metal layer of the second metal-ceramic substrate can be achieved even if the ceramic layer of the first metal-ceramic substrate, the ceramic layer of the second metal-ceramic substrate, the ceramic layers of the first and second metal-ceramic substrates, or, if appropriate, objects connected to the ceramic layers of the first or second metal-ceramic substrates (e.g. further metal layers on the first and / or second metal-ceramic substrates) still remain in the orthogonal projection between the metal layer of the first metal-ceramic substrate and the metal layer. The shading ratio preferably results from the ratio of (a) to (b). Here, (a) shows the area of the region on the second metal-ceramic substrate intersected by an orthogonal projection of the first metal-ceramic substrate onto a projection plane parallel to the metal layer of the first metal-ceramic substrate, and (b) shows the area of the metal layer of the second metal-ceramic substrate. When calculating the area, it is not necessary to take into account the masking of the metal layer. It is therefore preferable to calculate the area using the area of the metal layer that results without masking and etching. Similarly, further metal layers on the second metal-ceramic substrate, for example in the case of metallizing both sides, do not need to be taken into account when calculating the area. [Brief description of the drawings]
[0034] [Figure 1] The arrangement of a first metal ceramic substrate 10 and a second metal ceramic substrate 20 is shown, and it is shown that even when the first metal ceramic substrate 10 is orthogonally projected onto projection planes 40, 40 parallel to the mask metal layer 11 of the first metal ceramic substrate 10, the shading of the metal layer 21 of the second metal ceramic substrate 20 is 0%. [Diagram 2]The arrangement of a first metal ceramic substrate 100 and a second metal ceramic substrate 200 is shown, and when the first metal ceramic substrate 100 is orthogonally projected onto a projection plane 400 parallel to the mask metal layer 110 of the first metal ceramic substrate 100, it is shown that more than 60% of the metal layer 210 of the second metal ceramic substrate 200 is shaded. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] FIG. 1 shows an arrangement of a first metal-ceramic substrate 10 and a second metal-ceramic substrate 20, and shows that when the first metal-ceramic substrate 10 is orthogonally projected onto a projection plane 40, 40 parallel to the mask metal layer 11 of the first metal-ceramic substrate 10, the shading of the metal layer 21 of the second metal-ceramic substrate 20 is 0%. Shown is a first metal-ceramic substrate 10 having a mask (not shown) metal layer 11 bonded to a ceramic layer 12. The ceramic layer 12 has a larger dimension than the metal layer 11 and may therefore extend beyond the metal layer 11. Also shown is a second metal-ceramic substrate 20 having a metal layer 21 bonded to a ceramic layer 22. The first metal-ceramic substrate 10 and the second metal-ceramic substrate 20 lie horizontally on their entire surfaces on a carrier 30. When the first metal ceramic substrate 10 is translated perpendicularly to the metal layer 11 of the first metal ceramic substrate 10, images 50, 50' of the first metal ceramic substrate 10 are displayed straddling the projection planes 40, 40'. The orthogonal projections (indicated by dashed arrows) of the first metal ceramic substrate 10 onto the projection planes 40, 40' do not intersect with the metal layer 21 of the second metal ceramic substrate 20. Therefore, even if the first metal ceramic substrate 10 is orthogonally projected onto the projection planes 40, 40' parallel to the metal layer 11 of the first metal ceramic substrate 10, the shading of the second metal ceramic substrate 20 is 0%.
[0036] FIG. 2 shows an arrangement of a first metal ceramic substrate 100 and a second metal ceramic substrate 200, in which the first metal ceramic substrate 100 is orthogonally projected onto a projection plane 400 parallel to the mask metal layer 110 of the first metal ceramic substrate 100, shading more than 60% of the metal layer 210 of the second metal ceramic substrate 200. Shown is a first metal ceramic substrate 100 having a mask (not shown) metal layer 110 bonded to a ceramic layer 120. Also shown is a second metal ceramic substrate 200 having a metal layer 210 bonded to a ceramic layer 220. The first metal ceramic substrate 100 and the second metal ceramic substrate 200 are arranged at an angle on a carrier 300 (e.g., a conveyor belt). The angled arrangement can be achieved, for example, by using a carrier (not shown). The second metal ceramic substrate 200 is arranged behind the first metal ceramic substrate 100 and oriented parallel thereto. The projection plane 400 is arranged parallel to and spaced from the mask metal layer 110 of the first metal ceramic substrate 100. Here, for example, it is arranged parallel to the mask metal layer 110 of the first metal ceramic substrate 100, so that it may straddle the second metal ceramic substrate 200. However, the position of the projection plane is not further limited. The projection plane can therefore alternatively be displaced parallel to the projection plane 400 shown here. In particular, the projection plane can be selected to be at a greater distance from the metal surface 110 of the metal ceramic substrate 100 than the projection plane 400. When the first metal ceramic substrate 100 is orthogonally projected onto a projection plane parallel to the metal layer 110 of the first metal ceramic substrate 100, the amount of shading of the second metal ceramic substrate 200 does not depend in this respect on the exact position of the projection plane. The orthogonal projection of the first metal ceramic substrate 100 onto the projection plane 400 (shown by the dashed arrow) intersects with the metal layer 210 of the second metal ceramic substrate 200 in the light-shielding region 500. When the first metal ceramic substrate 100 is orthogonally projected onto a projection plane 400 parallel to the metal layer 110 of the first metal ceramic substrate 100, the shading of the second metal ceramic substrate 200 is 60% or more.
[0037] Surprisingly, it was found that the effect of etching with the etching solution 2 is greatly influenced by the relative positions of the individual metal-ceramic substrates. According to the invention, it is advantageous to position the metal-ceramic substrates such that the surfaces with the unmasked areas (i.e., areas not occupied by, for example, an etching mask) of the metal-ceramic substrates are as freely accessible as possible to the etching solution 2. Without being bound by theory, it is believed that this is because the etching solution 2 can be very ideally perfused to the unmasked areas. By effectively flowing the etching solution 2, contact with the etching solution 2 occurs, which may allow the active metal to be completely removed from the bonding layer in a very short time.
[0038] There is no further limitation on the arrangement of the first metal ceramic substrate and the second metal ceramic substrate when they are contacted with the etching solution 2. According to a preferred embodiment, the first metal ceramic substrate and the second metal ceramic substrate can be contacted with the etching solution 2 while moving the first metal ceramic substrate and the second metal ceramic substrate. Preferably, the movement is a continuous movement.
[0039] According to a preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged on a carrier for contacting with the etching solution 2. Particularly preferably, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged on the same carrier. The carrier may be, for example, a conveyor belt. According to a preferred embodiment, the carrier is a conveyor belt which is moved in the conveying direction. Alternatively, it may be a holder for the metal-ceramic substrates to rest on the conveyor belt. Thus, the first metal-ceramic substrate and the second metal-ceramic substrate may be arranged, for example, directly on the conveyor belt as a carrier, or the first metal-ceramic substrate and the second metal-ceramic substrate may be arranged on a further carrier (for example a holder), which in turn is arranged on the conveyor belt as a carrier.
[0040] The arrangement of the first and second metal-ceramic substrates on the carrier is not further limited. According to a preferred embodiment, it is provided that the first and second metal-ceramic substrates rest on one carrier over their entire surface. According to an alternative, it may be provided that the first and second metal-ceramic substrates rest substantially only on the guide rails of a conveyor belt. According to a further alternative, the first and second metal-ceramic substrates may rest on the guide rails of a further carrier (e.g., a holder) or be clamped to the frame of a further carrier (e.g., a holder), which may be placed on the conveyor belt.
[0041] Preferably, the metal-ceramic substrate lies on the carrier in such a way that the metal layers of the first and second metal-ceramic substrates, which are masked and which are preferably intended for treatment with the etching solution 2, face away from the carrier. According to a further preferred embodiment, the first and second metal-ceramic substrates are respectively double-sided metallized metal substrates, with particularly preferred masking of the areas on the metal layers of the first and second metal-ceramic substrates being carried out on both sides. In this embodiment, it may be advantageous for the metal-ceramic substrates for treatment with the etching solution to rest only at their ends on the carrier, for example on the guide rails of a conveyor belt or on the guide rails of a holder, or to be clamped to the frame of a holder.
[0042] Further, but not limited to, the possibility of arranging the first metal ceramic substrate and the second metal ceramic substrate such that when the etching solution 2 is contacted, the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, shading the metal layer of the second metal ceramic substrate by 60% or less.
[0043] According to a preferred embodiment, when contacting with the etching solution 2, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged on a carrier, preferably on the same carrier, in at least one of the following ways, the carrier being particularly preferably a conveyor belt moving in the conveying direction: a) A method in which a first metal-ceramic substrate and a second metal-ceramic substrate are not laminated; b) placing the first metal-ceramic substrate and the second metal-ceramic substrate in a substantially horizontal position; c) the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially perpendicular position and one behind the other in the transport direction; and d) A method of arranging the first metal ceramic substrate and the second metal ceramic substrate so that the first metal ceramic substrate forms an angle of 45° or less with the conveying direction, more preferably 30° or less, and even more preferably 20° or less with the second metal ceramic substrate, and so that the second metal ceramic substrate forms an angle of 45° or less with the conveying direction, more preferably 30° or less, and even more preferably 20° or less with the conveying direction. It is.
[0044] Therefore, when contacted with the etching solution 2 according to one embodiment, the first metal ceramic substrate and the second metal ceramic substrate do not have to be stacked. In this case, the first metal ceramic substrate and the second metal ceramic substrate are preferably disposed adjacent to each other. Preferably, the first metal ceramic substrate and the second metal ceramic substrate are disposed parallel to each other.
[0045] According to a further preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially horizontal position. In this case, the first metal-ceramic substrate and the second metal-ceramic substrate are preferably arranged side by side. Preferably, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged parallel to each other. For example, in this case, the first metal-ceramic substrate and the second metal-ceramic substrate can be arranged lying on one of the metal layers, and particularly preferably lying on the unmasked metal layer.
[0046] According to a further preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially vertical position and one behind the other with respect to the transport direction. In this case, the first metal-ceramic substrate and the second metal-ceramic substrate can be arranged, for example, in a holder on a conveyor belt. In this case, the first metal-ceramic substrate and the second metal-ceramic substrate can be arranged in the same holder or the first metal-ceramic substrate and the second metal-ceramic substrate can be arranged in different holders. In this case, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged one behind the other with respect to the transport direction, so that an ideal flow of the etching solution 2 can be achieved.
[0047] According to a further preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged such that the first metal-ceramic substrate forms an angle of 45° or less, more preferably 30° or less, even more preferably 20° or less with the conveying direction, and the second metal-ceramic substrate forms an angle of 45° or less, more preferably 30° or less, even more preferably 20° or less with the conveying direction. According to yet another preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are arranged such that the first metal-ceramic substrate forms an angle of at least 1°, more preferably at least 3°, particularly preferably at least 5° with the conveying direction, and the second metal-ceramic substrate forms an angle of at least 1°, more preferably at least 3°, particularly preferably at least 5° with the conveying direction. Such an angle between the first or second metal-ceramic substrate and the conveying direction of the conveyor belt can be advantageous for simplifying the outflow of the etching solution 2. According to yet another preferred embodiment, the first metal ceramic substrate and the second metal ceramic substrate are arranged so that the first metal ceramic substrate forms an angle with the transport direction within a range of 1 to 45°, more preferably an angle with a range of 3 to 30°, and particularly preferably an angle with a range of 5 to 20°, and the second metal ceramic substrate is arranged so that the first metal ceramic substrate forms an angle with the transport direction within a range of 1 to 45°, more preferably an angle with a range of 3 to 30°, and particularly preferably an angle with a range of 5 to 20°.
[0048] According to a further preferred embodiment, the method according to the invention is operated continuously.
[0049] There is no further limitation on the method of contacting the first metal ceramic substrate and the second metal ceramic substrate with the etching solution 2. According to a preferred embodiment, the contacting of the first metal ceramic substrate and the second metal ceramic substrate with the etching solution 2 is carried out by spraying the etching solution 2 onto the first metal ceramic substrate and the second metal ceramic substrate, immersing the first metal ceramic substrate and the second metal ceramic substrate in the etching solution 2, or passing the first metal ceramic substrate and the second metal ceramic substrate through the etching solution 2.
[0050] According to yet another preferred embodiment, the first metal-ceramic substrate and the second metal-ceramic substrate are ultrasonically contacted when contacted with the etching solution 2.
[0051] According to a preferred embodiment, the masking is removed from the first metal ceramic substrate and the second metal ceramic substrate. For example, the masking can be removed from the first metal ceramic substrate and the second metal ceramic substrate after contacting with the etching solution 2. On the other hand, it is also possible to remove the masking from the first metal ceramic substrate and the second metal ceramic substrate already after contacting with the etching solution 1. The removal of the masking is not further limited and can be performed by any method known to those skilled in the art.
[0052] Furthermore, it may be advantageous if cleaning is carried out before, between and / or after the individual steps of the method according to the invention. Cleaning is preferably carried out with water. Particularly preferably, cleaning of the first metal-ceramic substrate and the second metal-ceramic substrate is carried out with: Before masking, Before treating with etching solution 1, Before treating with etching solution 2, Before removing the masking and / or After removing the masking, It will be held.
[0053] After cleaning, the first metal-ceramic substrate and the second metal-ceramic substrate are preferably dried.
[0054] The metal ceramic substrate obtained by the above method has a particularly fine patterned structure and is highly suitable for power electronics applications. EXAMPLES
[0055] (Example of manufacturing metal ceramic substrate) To prepare the metal-ceramic substrate, 19.8 wt% tin powder (7-11 μm), 3.7 wt% titanium hydride, and 6.5 wt% organic vehicle were mixed in a stand mixer at 1930 rpm for 30 min. Then, 3.0 wt% Texanol and 67 wt% copper powder (7-11 μm) were added stepwise. The resulting mixture was stirred at high speed until a homogenous paste was obtained.
[0056] The paste thus obtained was used to bond the ceramic body to both opposing sides of the metal foil. For this purpose, a ceramic body (obtained from Toshiba Materials) with dimensions 174 x 139 x 0.32 mm and identical front and back faces was used. This paste was screen-printed on the back face of the ceramic body with a 280 mesh screen over an area of dimensions 168 x 130 mm and pre-dried at 125 ° C for 15 minutes. The paste thickness after pre-drying was 25 ± 5 μm. A copper foil made of oxygen-free highly conductive copper with a purity of 99.99% and dimensions 170 x 132 x 0.3 mm was then placed on the pre-dried paste. The structure thus produced was turned over and the paste was printed evenly on the front face of the ceramic body, pre-dried, and then the copper foil was placed on top to form a sandwich structure. Next, a silicon carbide plate weighing 1 kg was placed on this sandwich structure, which was then fired at a maximum temperature of 910°C (measured with a thermocouple) for 20 minutes and cooled to room temperature to obtain a metal ceramic substrate comprising a ceramic layer bonded on both sides to a copper layer via a bonding layer.
[0057] Example of etching of metal-ceramic substrate: An etching mask having a masked region and an unmasked region was provided on the upper surface of the metal ceramic substrate obtained by the above manufacturing example. After rinsing with water, the metal ceramic substrate was treated with etching solution 1 to remove copper from the copper layer and copper and tin from the bonding layer. Thereafter, the metal ceramic substrate was washed according to the following examples and comparative examples, and treated with etching solution 2 to remove titanium from the bonding layer.
[0058] Example 1: The metal-ceramic substrate was placed horizontally on the conveyor belt and transported through a bath of etching solution 2 by the conveyor belt.
[0059] Example 2: The metal-ceramic substrate was placed horizontally on a conveyor belt and transported through a bath of etching solution 2 by the conveyor belt while being subjected to ultrasonic treatment.
[0060] Example 3: The metal-ceramic substrate was placed horizontally on a conveyor belt and transported under a spray nozzle, from which the etching solution 2 was sprayed onto the metal-ceramic substrate.
[0061] Example 4: The metal-ceramic substrate was placed horizontally on a conveyor belt and the etching solution 2 was sprayed onto it while it was stationary.
[0062] Example 5: The metal-ceramic substrate was placed on a conveyor belt, which transported it through a bath of etching solution 2 while subjecting it to ultrasonic treatment. The transport directions of the metal-ceramic substrate and the conveyor belt were at an angle of 15°. The inclined position of the metal-ceramic substrate was achieved by a support. The metal-ceramic substrate was positioned so that when a certain metal-ceramic substrate was orthogonally projected onto a projection plane parallel to the mask metal layer of this metal-ceramic substrate, the metal layer of the other (adjacent) metal-ceramic substrate was shaded by a maximum of 15%.
[0063] Example 6: The metal-ceramic substrate was placed on a conveyor belt, which transported it through a bath of etching solution 2 while subjecting it to ultrasonic treatment. The transport directions of the metal-ceramic substrate and the conveyor belt each formed an angle of 10°. The inclined position of the metal-ceramic substrate was achieved by a support. The metal-ceramic substrate was positioned so that when a certain metal-ceramic substrate was orthogonally projected onto a projection plane parallel to the mask metal layer of this metal-ceramic substrate, the metal layer of the other (adjacent) metal-ceramic substrate was shaded by up to 50%.
[0064] Comparative Example 1: The metal-ceramic substrate was placed vertically on a holder on a conveyor belt and transported through a bath of etching solution 2 by the conveyor belt.
[0065] Comparative Example 2: The metal-ceramic substrate was placed vertically on a holder on a conveyor belt and transported by the conveyor belt through a bath of etching solution 2 while being subjected to ultrasonic treatment.
[0066] Comparative Example 3: The metal-ceramic substrate was placed vertically on a holder on a conveyor belt and transported under a spray nozzle from which the etchant 2 was sprayed onto the metal-ceramic substrate.
[0067] Comparative Example 4: The metal-ceramic substrate was placed vertically on a holder on a conveyor belt and the etching solution 2 was sprayed on it while it was stationary.
[0068] Comparative Example 5: The metal-ceramic substrate was placed on a conveyor belt, which transported it through a bath of etching solution 2 while subjecting it to ultrasonic treatment. The transport directions of the metal-ceramic substrate and the conveyor belt each formed an angle of 10°. The inclined position of the metal-ceramic substrate was achieved by a support. The metal-ceramic substrate was positioned so that when a certain metal-ceramic substrate was orthogonally projected onto a projection plane parallel to the mask metal layer of this metal-ceramic substrate, the metal layer of the other (adjacent) metal-ceramic substrate was shaded by 70%.
[0069] evaluation: Each example and comparative example was repeated with different types of metal-ceramic substrates, different types of etchant 2, and different conveyor belt speeds. The same parameters were used for each example and comparative example. The amount of titanium remaining in the bonding layer of the metal-ceramic substrate was qualitatively measured. The results are shown in Table 1. Table 1: [Table 1] Legend: +++: Very low residual titanium content ---: Very high residual titanium content o: Residual titanium content is easily detectable
[0070] The results show that such an arrangement of the metal-ceramic substrate during contact with the etching solution 2, i.e. such that when the metal-ceramic substrate is orthogonally projected onto a projection plane parallel to the mask metal layer of the metal-ceramic substrate, the metal layer of the further metal-ceramic substrate is shaded by no more than 60%, as for example when the metal-ceramic substrate is positioned horizontally or nearly horizontally, allows for particularly effective removal of the active metal. The results also show that in the metal-ceramic substrate obtained according to the method of the invention, the free active metal is substantially completely removed.
Claims
1. A method for patterning a metal-ceramic substrate, comprising the steps of: a) providing a first metal-ceramic substrate and a second metal-ceramic substrate, each of which comprises: - a ceramic layer; A metal layer; a bonding layer located between the ceramic layer and the metal layer, the bonding layer comprising: (i) a metal having a melting point of at least 700° C.; and (ii) an active metal; b) providing an etchant 1 capable of removing metal from said metal layer and at least partially removing metal having a melting point of at least 700° C. from said bonding layer; c) providing an etchant 2 capable of removing said active metal from said bonding layer; d) masking areas on the metal layer of the first metal-ceramic substrate and on the metal layer of the second metal-ceramic substrate that are not intended to be ablated; e) contacting the first metal-ceramic substrate and the second metal-ceramic substrate with the etching solution 1; f) contacting the first metal ceramic substrate and the second metal ceramic substrate with the etching solution 2, the first metal ceramic substrate and the second metal ceramic substrate being arranged such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 60% or less; Including, The method of claim 1, wherein the maximum silver content is 10.0 atomic %, based on the atomic number of said bonding layer.
2. 2. The method of claim 1, wherein the ceramic of the ceramic layer is selected from the group consisting of aluminum nitride ceramic, silicon nitride ceramic, and aluminum oxide ceramic.
3. 3. The method according to claim 1 or 2, characterized in that the metal of the metal layer is copper.
4. A method according to any one of claims 1 to 3, characterized in that the metal having a melting point of at least 700°C is copper.
5. The method according to any one of claims 1 to 4, characterized in that the bonding layer consists of a metal having a melting point below 700°C.
6. 6. The method of claim 5, wherein the metal having a melting point below 700° C. is selected from the group consisting of tin, bismuth, indium, gallium, zinc, antimony and magnesium.
7. The method according to any one of claims 1 to 6, characterized in that the active metal is selected from the group consisting of titanium, zirconium, niobium, tantalum, vanadium and hafnium.
8. The method according to any one of claims 1 to 7, characterized in that the maximum silver content is 1.0 atomic % based on the atomic number of the bonding layer.
9. The method according to any one of claims 1 to 8, characterized in that, when the first metal ceramic substrate and the second metal ceramic substrate are brought into contact with the etching solution 2, the first metal ceramic substrate and the second metal ceramic substrate are arranged such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 50% or less.
10. A method according to any one of claims 1 to 8, characterized in that when the first metal ceramic substrate and the second metal ceramic substrate are brought into contact with the etching solution 2, the first metal ceramic substrate and the second metal ceramic substrate are positioned such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 40% or less.
11. A method according to any one of claims 1 to 8, characterized in that when the first metal ceramic substrate and the second metal ceramic substrate are brought into contact with the etching solution 2, the first metal ceramic substrate and the second metal ceramic substrate are positioned such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 30% or less.
12. A method according to any one of claims 1 to 8, characterized in that when the first metal ceramic substrate and the second metal ceramic substrate are contacted with the etching solution 2, the first metal ceramic substrate and the second metal ceramic substrate are positioned such that, when the first metal ceramic substrate is orthogonally projected onto a projection plane parallel to the metal layer of the first metal ceramic substrate, the metal layer of the second metal ceramic substrate is shaded by 15% or less.
13. 13. The method according to any one of the preceding claims, characterized in that during contact with the etching solution 2, the first metal-ceramic substrate and the second metal-ceramic substrate are placed on a carrier, preferably on the same carrier.
14. 14. The method according to claim 13, characterized in that the carrier is a conveyor belt moved in a conveying direction.
15. When the first metal-ceramic substrate and the second metal-ceramic substrate are contacted with the etching solution 2, a) a method in which the first metal-ceramic substrate and the second metal-ceramic substrate are not laminated; b) placing the first metal-ceramic substrate and the second metal-ceramic substrate in a substantially horizontal position; c) the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially vertical position and one behind the other with respect to the transport direction; and d) a method of arranging the first metal ceramic substrate and the second metal ceramic substrate such that the first metal ceramic substrate forms an angle of 45° or less with the conveying direction and the second metal ceramic substrate forms an angle of 45° or less with the conveying direction; 15. The method according to claim 14, characterized in that the method further comprises arranging the first and second electrodes in at least one of the following ways:
16. When contacted with the etching solution 2, the first metal-ceramic substrate and the second metal-ceramic substrate are a) a method in which the first metal-ceramic substrate and the second metal-ceramic substrate are not laminated; b) placing the first metal-ceramic substrate and the second metal-ceramic substrate in a substantially horizontal position; c) the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially vertical position and one behind the other with respect to the transport direction; and d) a method of arranging the first metal ceramic substrate and the second metal ceramic substrate such that the first metal ceramic substrate forms an angle of 30° or less with the transport direction and the second metal ceramic substrate forms an angle of 30° or less with the transport direction; 15. The method according to claim 14, characterized in that the method further comprises arranging the first and second electrodes in at least one of the following ways:
17. When contacted with the etching solution 2, the first metal-ceramic substrate and the second metal-ceramic substrate are a) a method in which the first metal-ceramic substrate and the second metal-ceramic substrate are not laminated; b) placing the first metal-ceramic substrate and the second metal-ceramic substrate in a substantially horizontal position; c) the first metal-ceramic substrate and the second metal-ceramic substrate are arranged in a substantially vertical position and one behind the other with respect to the transport direction; and d) a method of arranging the first metal ceramic substrate and the second metal ceramic substrate such that the first metal ceramic substrate forms an angle of 20° or less with the conveying direction and the second metal ceramic substrate forms an angle of 20° or less with the conveying direction; 15. The method according to claim 14, characterized in that the method further comprises arranging the first and second electrodes in at least one of the following ways:
Citation Information
Patent Citations
Soldering material for active soldering and methods for active soldering
DE102017114893A1
Method of joining a metal part directly to a substrate made of non-metallic material
DE2319854A1
JP1973012985B1
Ceramic circuit board and method for manufacturing the same
JP2003285195A
Ceramic circuit board and power semiconductor module using the same
JP2009170930A