Crosslinked polyolefin separation membrane and method for producing same

The controlled production of crosslinked polyolefin separation membranes with uniform crosslinking addresses non-uniformity issues, improving resistance and meltdown temperature, thus enhancing the safety and performance of lithium secondary batteries.

JP7575425B2Active Publication Date: 2024-10-29LG CHEM LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2022092282
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-12
Filing Date
2022-06-07
Publication Date
2024-10-29
Estimated Expiration
2039-06-11

AI Technical Summary

Technical Problem

Existing crosslinked polyolefin separation membranes in lithium secondary batteries face issues with non-uniform crosslinking, leading to increased surface resistance and difficulty in achieving a consistent meltdown temperature, which affects the safety and performance of the batteries.

Method used

A method for producing a crosslinked polyolefin separation membrane involving controlled addition of diluents and a silane crosslinking reaction to ensure uniform crosslinking throughout the membrane thickness, reducing surface reactions and maintaining consistent meltdown temperature.

Benefits of technology

The method results in a separation membrane with reduced surface resistance and improved mechanical and thermal properties, enhancing the safety and performance of electrochemical devices by ensuring uniform crosslinking and higher meltdown temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575425000004
    Figure 0007575425000004
  • Figure 0007575425000005
    Figure 0007575425000005
  • Figure 0007575425000006
    Figure 0007575425000006
Patent Text Reader

Abstract

The present invention provides a separation membrane containing a silane-crosslinked polyolefin that has a uniform degree of crosslinking in the thickness direction by reducing over-crosslinking on the surface of the separation membrane, or in which the degree of crosslinking inside the separation membrane is higher than that on the surface. The present invention relates to a crosslinked polyolefin separation membrane, the separation membrane comprising a silane-crosslinked polyolefin, and having a predetermined silane-crosslinked IR (infrared spectroscopy) peak intensity in the thickness direction of the separation membrane, and a method for manufacturing the same. The present invention can provide a separation membrane in which intensive silane crosslinking reactions on the separation membrane surface are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crosslinked polyolefin separation membrane and a method for producing the same.

[0002] This application claims priority to Korean Patent Application No. 10-2018-0067719, filed on June 12, 2018, the entire contents of which are incorporated herein by reference in their entirety in the specification and drawings. [Background technology]

[0003] In recent years, interest in energy storage technology has been increasing. As the fields of application expand to include mobile phones, camcorders, and laptops, as well as the energy of electric vehicles, efforts in the research and development of electrochemical elements have been increasingly realized. Electrochemical elements are the field that has attracted the most attention from this perspective, and in particular, the development of rechargeable secondary batteries has attracted attention. In recent years, in the development of such batteries, research and development related to the design of new electrodes and batteries has been conducted in order to improve the capacity density and specific energy.

[0004] Among the secondary batteries currently in use, lithium secondary batteries, developed in the early 1990s, have been attracting attention due to their advantages of high operating voltage and significantly higher energy density compared to conventional batteries that use aqueous electrolytes, such as Ni-MH, Ni-Cd, and sulfuric acid-lead batteries.

[0005] Such lithium secondary batteries are composed of a positive electrode, a negative electrode, an electrolyte, and a separator. In particular, the separator is required to have insulating properties to separate and electrically insulate the positive electrode and the negative electrode, and high ionic conductivity to increase the permeability of lithium ions based on high porosity.

[0006] In addition, if the difference between the shutdown temperature and meltdown temperature of the separator is large, the safety of the lithium secondary battery including the separator is ensured. To widen the gap between the two, the shutdown temperature must be adjusted to decrease and the meltdown temperature to increase.

[0007] One method for increasing the meltdown temperature is to use a crosslinked polyolefin porous membrane. However, when a crosslinking reaction is used, there is a risk of a side reaction occurring between the diluent required for pore formation and the crosslinking agent required for the crosslinking reaction. In particular, the crosslinking agent that reacts with the diluent migrates to the surface of the separator together with the diluent during extrusion / stretching, causing a problem of the crosslinking reaction occurring only on the surface of the finally produced separator. When the crosslinking reaction occurs only on the surface of the separator in this way, it is difficult to produce a crosslinked polyolefin separator having a uniform meltdown temperature in the thickness direction, and there is a problem of the resistance increasing because it is difficult to form pores on the surface of the separator due to over-crosslinking on the surface of the separator. Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to provide a separation membrane containing a silane-crosslinked polyolefin having a uniform degree of crosslinking in the thickness direction by reducing over-crosslinking on the surface of the separation membrane, or a higher degree of crosslinking inside the separation membrane than on the surface.

[0009] Therefore, one aspect of the present invention aims to provide a cross-linked polyolefin separation membrane which has a uniform meltdown temperature in the thickness direction of the separation membrane, and which has a higher meltdown temperature and a reduced resistance value than conventional membranes.

[0010] Another object of the present invention is to provide a method for producing the above-mentioned separation membrane. [Means for solving the problem]

[0011] One aspect of the present invention provides a crosslinked polyolefin separation membrane according to the following embodiment.

[0012] The first embodiment is A crosslinked polyolefin separation membrane, The separation membrane comprises a silane-crosslinked polyolefin, The separation membrane has a silane crosslinking IR (infrared spectroscopy) peak intensity of 0.001 to 0.012 in the thickness direction; The present invention relates to a crosslinked polyolefin separation membrane, characterized in that the ratio (B / A) of the silane crosslinking IR peak intensity (B) at the center in the thickness direction of the separation membrane to the silane crosslinking IR peak intensity (A) on one surface of the separation membrane is 0.8 to 1.2.

[0013] The second embodiment is A crosslinked polyolefin separation membrane, The separation membrane comprises a silane-crosslinked polyolefin, The separation membrane has a silane crosslinking IR peak intensity of 0.001 to 0.012 in the thickness direction; The present invention relates to a crosslinked polyolefin separation membrane, characterized in that the ratio (C / A) of the silane crosslinking IR peak intensity (A) on one surface of the separation membrane to the silane crosslinking IR peak intensity (C) at a point from one surface of the separation membrane to 1 / 4 of the total thickness of the separation membrane is 0.9 to 1.5.

[0014] The third embodiment is A crosslinked polyolefin separation membrane, The separation membrane comprises a silane-crosslinked polyolefin, In the thickness direction of the separation membrane, the IR peak is 2847 cm -1 Intensity (D) of IR peak 1030cm -1 The intensity ratio ((A, B or C) / D) is 0.001 to 0.012, The present invention relates to a crosslinked polyolefin separation membrane, characterized in that the ratio (B / A) of the silane crosslinking IR peak intensity (B) at the center in the thickness direction of the separation membrane to the silane crosslinking IR peak intensity (A) on one surface of the separation membrane is 0.8 to 1.2.

[0015] The fourth embodiment is the first or second embodiment, The silane crosslinking IR peak is at 1030 cm -1 The present invention relates to a crosslinked polyolefin separation membrane, characterized in that

[0016] A fifth embodiment relates to a crosslinked polyolefin separation membrane, wherein the silane (Si) content in the separation membrane is 150 ppm to 900 ppm by weight per 100 parts by weight of the separation membrane in any one of the above-mentioned embodiments.

[0017] A sixth embodiment is any one of the above-mentioned embodiments, The present invention relates to a crosslinked polyolefin separation membrane, characterized in that the degree of crosslinking of the separation membrane is 15 to 90%.

[0018] A seventh embodiment is any one of the above-mentioned embodiments, The present invention relates to a crosslinked polyolefin separation membrane having a crosslink density (the number of Si-O-Si crosslinking points per unit volume) of 0.01 mol / L or more.

[0019] Another aspect of the present invention provides a method for producing a crosslinked polyolefin separation membrane according to the following embodiment.

[0020] The eighth embodiment is: (S1) introducing and mixing a polyolefin having a weight average molecular weight of 200,000 to 1,000,000, a first diluent, an alkoxysilane having a carbon-carbon double bond group, an initiator and a crosslinking catalyst into an extruder; (S2) adding and mixing a second diluent into the extruder to reactively extrude the silane-grafted polyolefin composition; (S3) forming and stretching the reactively extruded silane-grafted polyolefin composition into a sheet; (S4) extracting the first diluent and the second diluent from the stretched sheet to prepare a silane-grafted polyolefin porous membrane; (S5) heat fixing the porous membrane; (S6) crosslinking the porous membrane in the presence of moisture.

[0021] The ninth embodiment is the eighth embodiment, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, characterized in that the ratio (t2 / t1) of the elapsed time (t2) from the addition of the second diluent to the elapsed time (t1) from the addition of the first diluent to the extrusion is 0.1 to 0.7.

[0022] A tenth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein a weight ratio of the first diluent to the second diluent is 50:50 to 80:20.

[0023] An eleventh embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the first diluent and the second diluent each independently contain liquid paraffin oil, solid paraffin oil, mineral oil, wax, soybean oil, phthalate esters, aromatic ethers, fatty acids having 10 to 20 carbon atoms, fatty acid alcohols having 10 to 20 carbon atoms, fatty acid esters, or two or more of these.

[0024] A twelfth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the kinetic viscosity of the second diluent is the same as or lower than the kinetic viscosity of the first diluent.

[0025] The thirteenth embodiment is the twelfth embodiment, The first diluent and the second diluent each have a kinematic viscosity of 5 cSt to 100 cSt at 40°C; In this case, the difference in kinetic viscosity between the first diluent and the second diluent is 5 cSt or more.

[0026] The fourteenth embodiment is the thirteenth embodiment, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the difference in kinetic viscosity between the first diluent and the second diluent is 10 cSt or more.

[0027] A fifteenth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the total content of the first diluent and the second diluent is 100 to 350 parts by weight based on 100 parts by weight of the polyolefin.

[0028] A sixteenth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the carbon-carbon double bond group-containing alkoxysilane contains a compound represented by the following chemical formula 1.

[0029] [ka]

[0030] In Chemical Formula 1, R1, R2, and R3 are each independently an alkoxy group having 1 to 10 carbon atoms or an alkyl group having 1 to 10 carbon atoms, in which case at least one of R1, R2, and R3 is an alkoxy group, and R is a vinyl group, an acryloxy group, a methacryloxy group, or an alkyl group having 1 to 20 carbon atoms, in which case at least one hydrogen atom of the alkyl group is substituted with a vinyl group, an acryl group, an acryloxy group, a methacryloxy group, or a methacryl group.

[0031] The seventeenth embodiment is the sixteenth embodiment, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the carbon-carbon double bond group-containing alkoxysilane includes trimethoxyvinylsilane, triethoxyvinylsilane, vinyltriacetoxysilane, (3-methacryloxypropyl)trimethoxysilane, (3-methacryloxypropyl)triethoxysilane, vinylmethyldimethoxysilane, vinyl-tris(2-methoxyethoxy)silane, vinylmethyldiethoxysilane, or at least two of these.

[0032] An eighteenth embodiment is any one of the above-mentioned embodiments, The content of the carbon-carbon double bond group-containing alkoxysilane is 0.1 to 3.0 parts by weight based on 100 parts by weight in total of the polyolefin, the first diluent and the second diluent, and the content of the initiator is 0.1 to 20 parts by weight based on 100 parts by weight of the carbon-carbon double bond group-containing alkoxysilane.

[0033] A nineteenth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the content of the crosslinking catalyst is 0.1 to 20 parts by weight based on 100 parts by weight of the alkoxysilane containing a carbon-carbon double bond group.

[0034] A twentieth embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the crosslinking catalyst contains dibutyltin dilaurate, dibutyltin diacetate, stannous acetate, stannous caprylate, zinc naphthenate, zinc caprylate, cobalt naphthenate, ethylamine, dibutylamine, hexylamine, pyridine, sulfuric acid, hydrochloric acid, toluene, sulfonic acid, acetic acid, stearic acid, maleic acid, or two or more of these.

[0035] A twenty-first embodiment is any one of the above-mentioned embodiments, The present invention relates to a method for producing a crosslinked polyolefin separation membrane, wherein the heat setting temperature is 100 to 140°C. Effect of the Invention

[0036] According to one aspect of the present invention, a separator having a uniform degree of crosslinking in the thickness direction of the separator or a greater degree of crosslinking in the interior than on the surface thereof can be provided, which can reduce the resistance of the separator surface and improve the physical properties of an electrochemical device, such as output and cycle characteristics.

[0037] According to one embodiment of the present invention, in the production method of a crosslinked polyolefin separation membrane, in the production of a silane-grafted polyolefin composition, a certain amount of a first diluent is added together with an initiator, a crosslinking agent, etc. in the first half of reactive extrusion, and a second diluent is added alone in the second half of reactive extrusion, thereby reducing the phenomenon in which crosslinking occurs mainly on the surface of the separation membrane. [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 is a schematic diagram illustrating a method for analyzing the degree of cross-linking in the thickness direction of a separation membrane by IR after exposing the separation membrane specimen through oblique cutting (1°). [Diagram 2] 1 is a diagram showing a separation membrane according to an embodiment of the present invention and an IR spectrum of the separation membrane in a thickness direction. [Diagram 3] FIG. 2 is a diagram showing silane bridge (Si-0) stretching peak intensity in the thickness direction of a separator according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing a change in crosslink structure over time in terms of crosslink density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] The present invention will be described in detail below. The terms and words used in the specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings and concepts that correspond to the technical ideas of the present invention, based on the principle that the inventor himself can appropriately define the concepts of terms in order to best describe the invention.

[0040] Throughout this specification, when a moiety is referred to as being "connected" to another moiety, this includes not only a "direct connection" but also an "indirect connection" via another element. Furthermore, "connection" includes not only a physical connection but also an electrochemical connection.

[0041] Throughout this specification, when a part "comprises" another component, it means that the part may further include the other component, not excluding the other component, unless otherwise specified.

[0042] Additionally, as used in this specification, "comprising" specifies the presence of a referenced shape, number, step, operation, member, element, and / or group thereof, but does not exclude the presence or addition of one or more other shapes, numbers, operations, members, elements, and / or groups.

[0043] As used throughout this specification, the terms "about," "substantially," and the like are used to mean a numerical value or close to a numerical value when given the manufacturing and material tolerances inherent in the recited value, and are used to prevent an unconscionable infringer from unfairly taking advantage of the disclosure in which precise or absolute numerical values ​​are recited to aid in the understanding of this application.

[0044] Throughout this specification, the term "combinations thereof" in a Markush form surface refers to a mixture or combination of one or more selected from the group of components recited in the Markush form expression, and is meant to include one or more selected from the group of recited components.

[0045] Throughout this specification, the phrase "A and / or B" means "A, B, or all of these."

[0046] One aspect of the present invention relates to a crosslinked polyolefin separation membrane and a method for producing the crosslinked polyolefin separation membrane.

[0047] The separator used in a lithium secondary battery has excellent safety when the difference between the shutdown temperature and the meltdown temperature is large. In order to widen the gap between the two, the shutdown temperature must be decreased and the meltdown temperature must be increased.

[0048] Therefore, the present inventors used a silane crosslinking reaction to produce a separator with a higher meltdown temperature. In this case, the meltdown temperature can be controlled by the crosslinking degree of the crosslinked polyolefin porous membrane. For example, a higher crosslinking degree increases the meltdown temperature, and a lower crosslinking degree decreases the meltdown temperature.

[0049] Such crosslinked polyolefin porous membranes can be manufactured by reactive extrusion of a mixture of polyolefin, a diluent, and a crosslinking agent (e.g., a carbon-carbon double bond group-containing alkoxysilane, an initiator, a crosslinking catalyst, etc.), but if the diluent and the crosslinking agent are added at the same time, there is a risk of a side reaction between the diluent and the crosslinking agent. The present inventors have found that, particularly in the case of a diluent with low viscosity, the diluent migrates to the surface of the separation membrane during reactive extrusion, causing a side reaction between the diluent and the crosslinking agent, resulting in a concentrated crosslinking reaction on the surface of the separation membrane.

[0050] The present inventors have focused on this problem and provide a separation membrane in which intensive cross-linking reactions on the surface of the separation membrane are reduced, and a method for manufacturing the same.

[0051] According to one embodiment of the present invention, there is provided a crosslinked polyolefin separation membrane, the separation membrane comprising a silane-crosslinked polyolefin, the separation membrane has a silane-crosslinked IR (infrared spectroscopy) peak intensity in the thickness direction of the separation membrane of 0.001 to 0.012, and the ratio (B / A) of the silane-crosslinked IR peak intensity (B) at the center of the separation membrane in the thickness direction to the silane-crosslinked IR peak intensity (A) on one surface of the separation membrane is 0.8 to 1.2.

[0052] At this time, the silane crosslinking IR peak is at 1030 cm -1 The above is in the vicinity of 1030cm. -1 The peak at indicates the presence of -Si-O-Si.

[0053] According to one aspect of the present invention, the crosslinked polyolefin separator has a silane crosslink IR peak intensity of 0.001 to 0.012 in the thickness direction of the separator. The presence of silane crosslinks (Si-O-Si) in the separator as in the above numerical range increases the meltdown temperature to about 175°C or higher, improving the safety of the electrochemical device. In one aspect of the present invention, the above numerical range indicates the presence or absence of -Si-O-Si in the separator. In other words, when the IR peak of the separator is measured, the IR peak intensity of the separator at 1030 cm -1 If the IR peak in the vicinity does not show the above peak intensity, it means that there is no Si-O-Si cross-linking in the separator, and in this case, the desired meltdown temperature cannot be achieved by one embodiment of the present invention.

[0054] Meanwhile, when preparing a silane crosslinked polyolefin separator, the ratio (B / A) of the silane crosslinked IR peak intensity (A) at one surface of the separator to the silane crosslinked IR peak intensity (B) at the center of the thickness direction of the separator is controlled to be 0.8 to 1.2 by controlling the time, type and amount of the diluent. As a result, in the separator according to one embodiment of the present invention, the silane crosslinked IR peak intensity at the surface and the silane crosslinked IR peak intensity at the inside are maintained equal or similar to each other, and the resistance value of the separator surface is reduced, so that a separator having uniform mechanical or thermal properties in the thickness direction of the separator can be provided. If the B / A ratio is less than 0.8, the resistance value of the separator surface is high, and when used as a separator for an electrochemical element, the output improvement may not be sufficient. If the B / A ratio is more than 1.2, the resistance value of the separator inside is high, and when used as a separator for an electrochemical element, the output improvement may not be sufficient.

[0055] In the present invention, the silane crosslinking IR peak intensity can be measured by the following method, but is not limited thereto.

[0056] First, a separation membrane specimen to be measured was prepared in a predetermined size, and then the separation membrane was cut at a predetermined inclination using a bevel cutting analyzer.

[0057] The cut separation membrane is divided into equal parts at predetermined intervals in the thickness direction of the separation membrane using an FT-IR spectrometer, and the silane crosslinking IR peak intensity from the surface to the inside of the separation membrane is measured three times and the average value is calculated.

[0058] At this time, the size of the specimen, the inclination angle, the equal intervals, and the number of measurements may be changed according to the thickness and size of the manufactured separator in order to reduce the error range.

[0059] FIG. 1 is a schematic diagram showing a method for analyzing the degree of cross-linking in the thickness direction of a separator by IR after exposing the separator by oblique cutting (1°) in the thickness direction of the separator.

[0060] Meanwhile, a crosslinked polyolefin separation membrane of one embodiment of the present invention in which intensive crosslinking reactions on the surface are reduced is determined by the ratio (C / A) of the silane crosslinking IR peak intensity (A) on one surface of the separation membrane to the silane crosslinking IR peak intensity (C) at a point from one surface of the separation membrane to 1 / 4 of the total thickness of the separation membrane.

[0061] Specifically, a separation membrane according to one embodiment of the present invention is a crosslinked polyolefin separation membrane, the separation membrane comprising a silane-crosslinked polyolefin, characterized in that the separation membrane has a silane crosslinking IR peak intensity of 0.001 to 0.012 in the thickness direction thereof, and a ratio (C / A) of the silane crosslinking IR peak intensity (C) at a point from one surface of the separation membrane to a 1 / 4 point of the total thickness of the separation membrane to the silane crosslinking IR peak intensity (A) on one surface of the separation membrane is 0.9 to 1.5.

[0062] In this way, by controlling the silane crosslinking IR peak intensity at 1 / 4 of the total thickness of the separator to be equal or similar to the silane crosslinking IR peak intensity on one surface of the separator, a crosslinked polyolefin separator with reduced intensive crosslinking reaction on the surface can be provided. If the C / A ratio is less than 0.9, the resistance value of the separator surface is high, and when used as a separator for electrochemical devices, the output improvement may not be sufficient. If the C / A ratio is more than 1.5, the resistance value inside the separator is high, and when used as a separator for electrochemical devices, the output improvement may not be sufficient.

[0063] Meanwhile, another aspect of the present invention is a crosslinked polyolefin separation membrane, the separation membrane comprising a silane-crosslinked polyolefin, and an IR peak of 2847 cm in the thickness direction of the separation membrane. -1 Intensity (D) of IR peak 1030cm -1 The ratio ((A, B or C) / D) of the silane crosslinking IR peak intensity (A) on one surface of the separation membrane is 0.001 to 0.012, and the ratio (B / A) of the silane crosslinking IR peak intensity (B) at the center in the thickness direction of the separation membrane to the silane crosslinking IR peak intensity (A) on one surface of the separation membrane is 0.8 to 1.2.

[0064] In the crosslinked polyolefin separation membrane according to one embodiment of the present invention, the IR peak at 2847 cm -1 indicates a CH stretching bond, with an IR peak at 2847 cm -1 The value of converges to approximately 1. In other words, the crosslinked polyolefin separation membrane according to one embodiment of the present invention has an IR peak of 2847 cm in the thickness direction. -1 Intensity (D) of IR peak 1030cm -1 The ratio ((A, B or C) / D) of the strengths (A, B or C) of the crosslinked polyolefins is 0.001 to 0.012. In this case, (A, B or C) / D may indicate the ratio of the silane crosslinking bond to the polyolefin main chain.

[0065] In one specific embodiment of the present invention, the separation membrane may have a silane crosslinking IR peak intensity in the thickness direction of the membrane of 0.002 to 0.010, or 0.003 to 0.008.

[0066] In a specific embodiment of the present invention, the silane (Si) content in the separator may be 150 ppm to 900 ppm, 250 ppm to 800 ppm, or 350 ppm to 750 ppm based on 100 parts by weight of the separator. Within the above numerical ranges, the desired mechanical and thermal properties of the separator of the present invention can be achieved. Furthermore, since the amount of silane crosslinking is appropriate, a resistance value suitable for use as a separator for an electrochemical device can be maintained.

[0067] The silane content in the separator can be measured by the following method, but is not limited thereto. As a non-limiting example, the silane content in the separator can be measured using an Axiom model inductively coupled plasma mass spectrometer (ICP-MS, inductively coupled plasma with mass spectrometer, here MC-ICP-MS, Axiom is an AXIOM MC model manufactured by Thermo Elemental in the UK, and is a form that also has a high resolution function).

[0068] According to an embodiment of the present invention, a separation membrane having a uniform IR peak in the thickness direction of the separation membrane can be provided by controlling the timing, type and amount of the first diluent and the second diluent.

[0069] One aspect of the present invention provides a separator having a uniform IR peak in the thickness direction of the separator or a higher IR peak value in the interior than in the surface. That is, the over-crosslinking of silane on the surface of the separator is prevented. That is, by preventing the over-crosslinking of silane on the surface of the separator, which would otherwise cause a decrease in porosity, a separator having a relatively low resistance can be provided.

[0070] In addition, the uniformity of the IR peak in the thickness direction of the separator indicates that the silane crosslinking is uniform in the thickness direction, which makes it possible to provide a separator having uniform thermal shrinkage and mechanical strength in the thickness direction.

[0071] The separation membrane according to one embodiment of the present invention described above has a degree of crosslinking of 15 to 90%, 20 to 80%, or 25 to 75%. When the degree of crosslinking is within the above numerical range, the meltdown temperature can be increased to a desired range, and the possibility of breakage and gel generation during the stretching process is low.

[0072] Meanwhile, in one specific embodiment of the present invention, the separation membrane has a crosslink density (the number of Si-O-Si crosslinking points per unit volume) of 0.01 mol / L or more, and may be 0.01 to 0.10 mol / L, 0.02 to 0.08 mol / L, or 0.03 to 0.07 mol / L.

[0073] The present inventors found that when the degree of crosslinking is equal to or greater than a certain value, the separator exhibits excellent heat resistance and has an increased meltdown temperature. If the meltdown temperature is high, the separator according to the present invention can be applied to fields such as automobiles, which have large capacities and where safety is important.

[0074] On the other hand, the present inventors have studied the correlation between the change in the degree of crosslinking and the change in the crosslinking structure, which is indicated by the crosslinking density.

[0075] As described above, in a specific embodiment of the present invention, the crosslink density of the separator may be 0.01 mol / L or more. If the crosslink density is less than 0.01 mol / L, the degree of crosslinking is coarse, and if the crosslink density is 0.01 mol / L or more, the degree of crosslinking is dense. This is shown in Figure 4. As a result, the mechanical strength is high and the shrinkage rate at high temperatures is reduced, and especially if the crosslink density is 0.01 mol / L or more, the high temperature shrinkage rate is reduced slowly.

[0076] A method for producing a crosslinked polyolefin separation membrane according to one aspect of the present invention includes the steps of: (S1) introducing and mixing a polyolefin having a weight average molecular weight of 200,000 to 1,000,000, a first diluent, an alkoxysilane having a carbon-carbon double bond group, an initiator and a crosslinking catalyst into an extruder; (S2) adding and mixing a second diluent into the extruder to reactively extrude the silane-grafted polyolefin composition; (S3) forming and stretching the reactively extruded silane-grafted polyolefin composition into a sheet; (S4) extracting the first diluent and the second diluent from the stretched sheet to prepare a silane-grafted polyolefin porous membrane; (S5) heat fixing the porous membrane; (S6) crosslinking the porous membrane in the presence of moisture.

[0077] The method for producing the separation membrane according to the present invention will now be described in detail.

[0078] First, a polyolefin having a weight average molecular weight of 200,000 to 1,000,000, a first diluent, an alkoxysilane containing a carbon-carbon double bond group, an initiator and a crosslinking catalyst are charged into an extruder and mixed (S1).

[0079] Conventionally, polyolefin, diluent, crosslinking agent, etc. are mixed in an extruder at the same time to produce a silane-grafted polyolefin composition. However, this process has the problem that the silane crosslinking reaction occurs only on the surface of the separator, and the mechanical and thermal properties of the separator are not uniform in the thickness direction.

[0080] Meanwhile, in the present invention, by controlling the type, amount and / or addition time of the diluent, it is possible to provide a separator having uniform mechanical and thermal properties, such as the degree of crosslinking and meltdown temperature, in the thickness direction of the separator.

[0081] In a specific embodiment of the present invention, the polyolefin may be polyethylene; polypropylene; polybutylene; polypentene; polyhexene; polyoctene; a copolymer of two or more of ethylene, propylene, butene, pentene, 4-methylpentene, hexene, hebsen, and octene; or a mixture thereof.

[0082] In particular, the polyethylene may be low density polyethylene (LDPE), linear low density polyethylene (LLDPE), high density polyethylene (HDPE), etc., among which high density polyethylene having a high crystallinity and a high melting point of the resin is most preferable.

[0083] In a specific embodiment of the present invention, the weight average molecular weight of the polyethylene may be 200,000 to 1,000,000, 220,000 to 700,000, or 250,000 to 500,000. In the present invention, a high molecular weight polyolefin having a weight average molecular weight of 200,000 to 1,000,000 is used as a starting material for producing a separation membrane, thereby ensuring uniformity of the separation membrane film and membrane production processability, and finally obtaining a separation membrane having excellent strength and heat resistance.

[0084] In a specific embodiment of the present invention, the first diluent may be liquid or solid paraffin oil, mineral oil, wax, soybean oil, etc., which are commonly used in the manufacture of wet separation membranes.

[0085] In a specific embodiment of the present invention, the first diluent may be a diluent capable of liquid-liquid phase separation from polyolefin, and examples of the diluent include phthalates such as dibutyl phthalate, dihexyl phthalate, and dioctyl phthalate; aromatic ethers such as diphenyl ether and benzyl ether; fatty acids having 10 to 20 carbon atoms such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid; fatty alcohols having 10 to 20 carbon atoms such as palmitic alcohol, stearic alcohol, and oleic alcohol; and fatty acid esters in which one or more fatty acids having a fatty acid group with a carbon number of 4 to 26, such as palmitic acid mono-, di-, or triester, stearic acid mono-, di-, or triester, oleic acid mono-, di-, or triester, and linoleic acid mono-, di-, or triester, are esterified with an alcohol having 1 to 10 carbon atoms and having 1 to 8 hydroxyl groups.

[0086] The first diluent may be any of the above-mentioned components, either alone or in the form of a mixture of two or more of them.

[0087] In a specific embodiment of the present invention, the carbon-carbon double bond group-containing alkoxysilane is a crosslinking agent that undergoes a silane crosslinking reaction, and is grafted to a polyolefin via the carbon-carbon double bond group, specifically the vinyl group, and crosslinks the polyolefin by undergoing a water crosslinking reaction via the alkoxy group.

[0088] In a specific embodiment of the present invention, the carbon-carbon double bond group-containing alkoxysilane may include a compound represented by the following Chemical Formula 1:

[0089] [ka]

[0090] In Chemical Formula 1, R1, R2, and R3 are each independently an alkoxy group having 1 to 10 carbon atoms or an alkyl group having 1 to 10 carbon atoms, in which case at least one of R1, R2, and R3 is an alkoxy group, and R is a vinyl group, an acryloxy group, a methacryloxy group, or an alkyl group having 1 to 20 carbon atoms, in which case at least one hydrogen atom of the alkyl group is substituted with a vinyl group, an acryl group, an acryloxy group, a methacryloxy group, or a methacryl group.

[0091] Meanwhile, R may additionally include an amino group, an epoxy group, or an isocyanate group.

[0092] In a specific embodiment of the present invention, the carbon-carbon double bond group-containing alkoxysilane may include trimethoxyvinylsilane, triethoxyvinylsilane, vinyltriacetoxysilane, (3-methacryloxypropyl)trimethoxysilane, (3-methacryloxypropyl)triethoxysilane, vinylmethyldimethoxysilane, vinyl-tris(2-methoxyethoxy)silane, vinylmethyldiethoxysilane, or a mixture of at least two of them.

[0093] In a specific embodiment of the present invention, the content of the carbon-carbon double bond group-containing alkoxysilane may be 0.1 to 3.0 parts by weight, 0.2 to 2.0 parts by weight, or 0.5 to 1.5 parts by weight based on 100 parts by weight in total of the polyolefin, the first diluent, and the second diluent. When the content of the carbon-carbon double bond group-containing alkoxysilane satisfies the above numerical range, problems such as a low silane content resulting in a low grafting rate and a low crosslinking degree, or a high silane content resulting in unreacted silane remaining and poor appearance of the extruded sheet can be prevented.

[0094] In a specific embodiment of the present invention, the initiator can be used without limitation as long as it is an initiator capable of generating radicals. Non-limiting examples of the initiator include 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP), benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, dicumyl peroxide, cumyl peroxide, hydrogen peroxide, potassium persulfate, etc.

[0095] In a specific embodiment of the present invention, the content of the initiator may be 0.1 to 20 parts by weight, specifically 1 to 10 parts by weight, more specifically 2 to 5 parts by weight, based on 100 parts by weight of the carbon-carbon double bond group-containing alkoxysilane. When the content of the initiator satisfies the above numerical range, it is possible to prevent a problem in which the silane grafting rate is reduced due to a low content of the initiator, or a problem in which polyethylene is crosslinked in the extruder due to a high content of the initiator.

[0096] In one particular embodiment of the present invention, the crosslinking catalyst is added to promote the silane crosslinking reaction.

[0097] In a specific embodiment of the present invention, the crosslinking catalyst may be a carboxylate of a metal such as tin, zinc, iron, lead, or cobalt, an organic base, an inorganic acid, or an organic acid. Non-limiting examples of the crosslinking catalyst include the carboxylate of a metal such as dibutyltin dilaurate, dibutyltin diacetate, stannous acetate, stannous caprylate, zinc naphthenate, zinc caprylate, and cobalt naphthenate, the organic base may be ethylamine, dibutylamine, hexylamine, and pyridine, the inorganic acid may be sulfuric acid, hydrochloric acid, and the organic acid may be toluene, sulfonic acid, acetic acid, stearic acid, and maleic acid. The crosslinking catalyst may be used alone or in a mixture of two or more of these.

[0098] In a specific embodiment of the present invention, the content of the crosslinking catalyst may be 0.1 to 20 parts by weight, 1 to 10 parts by weight, or 2 to 5 parts by weight based on 100 parts by weight of the carbon-carbon double bond group-containing alkoxysilane. When the content of the crosslinking catalyst satisfies the above numerical range, a desired level of silane crosslinking reaction occurs, and undesired side reactions do not occur in the lithium secondary battery. In addition, there is no cost problem such as waste of the crosslinking catalyst.

[0099] Next, the second diluent is added to the extruder and mixed to reactively extrude the silane-grafted polyolefin composition (S2).

[0100] That is, a polyolefin having a weight average molecular weight of 200,000 to 1,000,000, a first diluent, a carbon-carbon double bond group-containing alkoxysilane, an initiator, and a crosslinking catalyst are added to an extruder and mixed, and after a certain period of time has elapsed, a second diluent is additionally added to the mixture and mixed.

[0101] As described above, the present invention can reduce the occurrence of concentrated silane crosslinking reaction on the surface of the separator by controlling the introduction and mixing times of the first diluent and the second diluent to be different from each other.

[0102] The type of the second diluent is the same as that described above for the first diluent.

[0103] In a specific embodiment of the present invention, the second diluent may be the same as or different from the first diluent. In particular, the second diluent added alone after a certain time has elapsed, i.e., without a cross-linking additive (cross-linking agent, cross-linking catalyst, etc.), is preferably added to the surface side of the separation membrane to be formed, so that the second diluent has a kinetic viscosity that is the same as or lower than that of the first diluent.

[0104] When the kinetic viscosity of the second diluent is lower than that of the first diluent, the second diluent can easily move to the surface side and prevent clogging of surface pores. In addition, when the kinetic viscosity of the second diluent used is relatively low, the pore size of the crosslinked polyolefin separation membrane produced is small and the shutdown temperature can be lowered. As a result, pore clogging occurs at a lower temperature, and a crosslinked polyolefin separation membrane with improved safety can be provided.

[0105] Therefore, in a specific embodiment of the present invention, the kinematic viscosity of the first diluent and the second diluent may be independently 5 cSt to 100 cSt, 10 cSt to 90 cSt, 15 cSt to 85 cSt, or 19.08 cSt to 67.84 cSt at 40°C, and the difference in kinematic viscosity between the first diluent and the second diluent may be 5 cSt or more, or 10 cSt or more.

[0106] In a specific embodiment of the present invention, the total content of the first diluent and the second diluent may be 100 to 350 parts by weight, 125 to 300 parts by weight, or 150 to 250 parts by weight based on 100 parts by weight of the polyolefin. When the total content of the diluent satisfies the above numerical range, problems such as reduced porosity, small pore size, and lack of interconnection between pores, greatly reduced permeability, and increased extrusion load due to increased viscosity of the polyolefin solution, which is difficult to process, can be prevented, and problems such as breakage and thickness variation during stretching caused by the low polyolefin content, which is caused by the low polyolefin content, which is caused by the polyolefin not being thermodynamically mixed with the diluent, and extruding in a gel form, can be reduced.

[0107] In a specific embodiment of the present invention, the weight ratio of the first diluent to the second diluent may be 50:50 to 80:20, 65:45 to 75:25, or 60:40 to 70:30. When the weight ratio of the first diluent to the second diluent satisfies the above numerical range, the first diluent can migrate to the surface of the separator during the extrusion / stretching step, thereby reducing the phenomenon in which the crosslinking reaction occurs only in the surface area.

[0108] In a specific embodiment of the present invention, the ratio (t2 / t1) of the elapsed time (t2) from the addition of the second diluent to the elapsed time (t1) from the addition of the first diluent to the extrusion may be 0.1 to 0.7, 0.2 to 0.65, or 0.3 to 0.63.

[0109] When the time elapsed from the addition of the first diluent and the second diluent to extrusion is as described above, the first diluent causes the intended reaction in the extruder, that is, the graft reaction between the polyolefin and the carbon-carbon double bond group-containing alkoxysilane, to occur uniformly, and subsequently, the second diluent, which is added separately, can be reduced in that it migrates to the wall side (outer shell) in the barrel and / or die of the extruder, causing an additional crosslinking reaction on the surface during the separation membrane formation stage.

[0110] In a specific embodiment of the present invention, the silane-grafted polyolefin composition may further contain general additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, an antistatic agent, and a nucleating agent, if necessary.

[0111] In a specific embodiment of the present invention, the reactive extrusion step may use a single screw extruder or a twin screw extruder.

[0112] Next, the reactively extruded silane-grafted polyolefin composition is formed into a sheet and stretched (S3).

[0113] For example, the reactively extruded silane-grafted polyolefin composition can be extruded using an extruder equipped with a T-die or the like, and then cooled extrudates can be formed using conventional casting or calendaring methods using water or air cooling.

[0114] In a specific embodiment of the present invention, a separator having improved mechanical strength and puncture strength can be provided by undergoing the stretching step as described above.

[0115] In a specific embodiment of the present invention, the stretching can be performed by sequential or simultaneous stretching using a roll or a tenter. The stretching ratio can be 3 times or more, or 4 to 10 times in each of the machine direction and the transverse direction, and the total stretching ratio can be 14 to 100 times. When the stretching ratio satisfies the above numerical range, it is possible to prevent problems such as insufficient orientation in one direction and at the same time, deterioration of tensile strength and puncture strength due to imbalance of physical properties between the machine direction and the transverse direction. In addition, when the total stretching ratio satisfies the above numerical range, it is possible to prevent problems such as unstretched or no formation of pores.

[0116] In one specific embodiment of the present invention, the stretching temperature may vary depending on the melting point of the polyolefin used, the concentration and type of diluent.

[0117] In a specific embodiment of the present invention, for example, when the polyolefin used is polyethylene, the diluent is liquid paraffin, the kinetic viscosity of the first diluent is 40-100 cSt at 40° C., and the kinetic viscosity of the second diluent is 5-60 cSt, the stretching temperature may be 70-160° C., 90-140° C., or 100-130° C. in the case of longitudinal stretching, 90-180° C., 110-160° C., or 120-150° C. in the case of transverse stretching, and 90-180° C., 110-160° C., or 120-150° C. in the case of simultaneous stretching in both directions. When the stretching temperature satisfies the above numerical range, problems of breakage or understretching due to lack of flexibility caused by low stretching temperature can be prevented, and partial overstretching or physical property difference caused by high stretching temperature can be prevented.

[0118] Then, the first diluent and the second diluent are extracted from the formed and stretched sheet to produce a silane-grafted polyolefin porous membrane (S4).

[0119] In a specific embodiment of the present invention, the first diluent and the second diluent may be extracted from the porous membrane using an organic solvent, and the porous membrane may be dried.

[0120] In a specific embodiment of the present invention, the organic solvent is not particularly limited as long as it can extract the diluent, and methyl ethyl ketone, methylene chloride, hexane, etc., which have high extraction efficiency and quick drying, are suitable.

[0121] In a specific embodiment of the present invention, the extraction method may be any of the common solvent extraction methods, such as an immersion method, a solvent spray method, and an ultrasonic method, which may be used alone or in combination. The content of the residual diluent after the extraction process is preferably 1% by weight or less. If the content of the residual diluent exceeds 1% by weight, the physical properties are degraded and the permeability of the porous membrane is reduced. The content of the residual diluent is affected by the extraction temperature and extraction time, and the extraction temperature is preferably high to increase the solubility of the diluent and the organic solvent, but is preferably 40° C. or less in consideration of safety issues caused by boiling of the organic solvent. If the extraction temperature is below the freezing point of the diluent, the extraction efficiency is significantly reduced, so the extraction temperature must be higher than the freezing point of the diluent.

[0122] The extraction time varies depending on the thickness of the porous membrane to be manufactured, but in the case of a separation membrane having a thickness of 5 to 15 μm, 1 to 3 minutes is appropriate.

[0123] Thereafter, the porous membrane is heat-set (S5).

[0124] The heat fixing is a step of fixing the porous membrane and applying heat to the porous membrane to forcibly fix the porous membrane that tends to shrink, thereby removing residual stress.

[0125] In a specific embodiment of the present invention, when the polyolefin is polyethylene, the heat setting temperature may be 100 to 140°C, 105 to 135°C, or 110 to 130°C. When the polyolefin is polyethylene, if the heat setting temperature satisfies the above numerical range, the rearrangement of polyolefin molecules occurs, which can remove residual stress in the porous membrane and reduce the problem of clogging of pores in the porous membrane due to partial melting. The higher the heat setting temperature, the better the heat shrinkage rate of the produced separator, and the lower the heat setting temperature, the lower the resistance of the separator.

[0126] In a specific embodiment of the present invention, the heat setting time may be 10 to 120 seconds, 20 to 90 seconds, or 30 to 60 seconds. When heat setting is performed for the above times, rearrangement of polyolefin molecules occurs, which can eliminate residual stress in the porous membrane and reduce the problem of pore clogging in the porous membrane due to partial melting.

[0127] Next, the heat-set porous membrane is crosslinked in the presence of moisture (S6).

[0128] In a specific embodiment of the present invention, the crosslinking can be carried out at 60 to 100°C, 65 to 95°C, or 70 to 90°C.

[0129] In one specific embodiment of the present invention, the crosslinking can be carried out at a humidity of 60 to 95% for 6 to 50 hours.

[0130] The present invention will be described in detail below with reference to specific examples. However, the examples according to the present invention can be modified into many other forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those skilled in the art.

[0131] Example 1 First, 10.5 kg of high density polyethylene (VH035 manufactured by Daehan Petrochemicals) having a weight average molecular weight of 380,000 as polyolefin, 13.65 kg of liquid paraffin oil (LP350F manufactured by Kyokudong Petrochemicals, kinematic viscosity at 40°C 67.89 cSt) as the first diluent, 450 g of trimethoxyvinylsilane as the carbon-carbon double bond group-containing alkoxysilane, 6 g of dibutyltin dilaurate as the crosslinking catalyst, and 6 g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP) as the initiator were put into the extruder and mixed.

[0132] Then, 5.85 kg of liquid paraffin oil (LP150F manufactured by Kyokuto Petrochemical, kinematic viscosity at 40°C 29.34 cSt) was added as a second diluent to the extruder and mixed. At this time, the ratio (t2 / t1) of the elapsed time (t2) from the addition of the second diluent to the elapsed time (t1) from the addition of the first diluent to the extrusion was 62% (0.62). That is, the elapsed time (t2) from the addition of the second diluent to the extrusion was about 0.62 times the elapsed time (t1) from the addition of the first diluent to the extrusion. Specifically, the elapsed time (t1) from the addition of the first diluent to the extrusion was 52 seconds, and the elapsed time (t2) from the addition of the second diluent to the extrusion was 32 seconds. Then, reactive extrusion was performed at a temperature condition of 210°C to produce a silane-grafted polyethylene composition.

[0133] The silane-grafted polyethylene composition thus produced was molded into a sheet using a T-die and a cooling casting roll, and then sequentially stretched in MD and then TD using a tenter-type sequential stretching machine. The MD and TD stretch ratios were both 7.5 times. The stretching temperatures were 108°C in MD and 121°C in TD.

[0134] The first diluent and the second diluent were extracted from the stretched sheet using methylene chloride, and the sheet from which the diluents were extracted was heat-set at 124°C to produce a porous membrane. The porous membrane was crosslinked for 48 hours under conditions of 85°C and 85% humidity to produce a crosslinked polyethylene separator. The results are shown in Table 1.

[0135] Example 2 A separation membrane was produced in the same manner as in Example 1, except that the second diluent was changed to LP100F (kinematic viscosity at 40° C.: 19.08 cSt) manufactured by Kyokuto Petrochemical Co., Ltd.

[0136] Example 3 A separation membrane was produced in the same manner as in Example 1, except that LP150F (kinematic viscosity at 40°C: 29.34 cSt) manufactured by Kyokuto Petrochemical Co., Ltd. was used as the first diluent, and LP100F (kinematic viscosity at 40°C: 19.08 cSt) manufactured by Kyokuto Petrochemical Co., Ltd. was used as the second diluent.

[0137] Comparative Example 1 A non-crosslinked polyolefin separator was produced without adding vinyl-containing alkoxysilane, initiator, and crosslinking catalyst to the extruder.

[0138] Specifically, 10.5 kg of high density polyethylene (VH035 manufactured by Daehan Petrochemicals) having a weight average molecular weight of 380,000 as polyolefin and 19.5 kg of liquid paraffin oil (LP350F manufactured by Kyokudong Petrochemicals, kinematic viscosity at 40°C of 67.89 cSt) as diluent were added to an extruder at once and mixed.

[0139] Thereafter, the mixture was extruded at a temperature of 210° C. to produce a polyethylene composition.

[0140] The polyethylene composition thus produced was molded into a sheet using a T-die and a cooling casting roll, and then successively stretched in MD and then TD using a tenter-type successive stretching machine. The MD and TD stretch ratios were both 7.5 times. The stretching temperatures were 108°C in MD and 121°C in TD.

[0141] The diluent was extracted from the stretched sheet using methylene chloride, and the sheet was heat-set at 124° C. to produce a non-crosslinked polyethylene separator. The shutdown temperature of the separator produced was 140.3° C. Meanwhile, in the case of Comparative Example 1, since no vinyl-containing alkoxysilane was added, no IR peak due to silane crosslinking was observed.

[0142] Comparative Example 2 A separation membrane was produced in the same manner as in Example 1, except that 10.5 kg of high density polyethylene (VH035 manufactured by Daehan Petrochemicals) having a weight average molecular weight of 380,000 as a polyolefin, 19.5 kg of liquid paraffin oil (LP350F manufactured by Kukdong Petrochemicals, kinematic viscosity at 40°C of 67.89 cSt) as a diluent, 450 g of trimethoxyvinylsilane as an alkoxysilane containing a carbon-carbon double bond group, 6 g of dibutyltin dilaurate as a crosslinking catalyst, and 6 g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP) as an initiator were added to the extruder at once and mixed.

[0143] Comparative Example 3 10.5 kg of silane-grafted polyolefin (HYUNDAI EP XP650) and 19 kg of liquid paraffin oil (Kyokuto Petrochemical LP350F, kinematic viscosity at 40° C. 67.89 cSt) were charged into an extruder and mixed at 180° C., followed by extrusion.

[0144] The extruded material was then molded into a sheet using a T-die and a cooling casting roll, and then sequentially stretched in a tenter-type sequential stretching machine, with MD stretching followed by TD stretching. The MD stretch ratio and TD stretch ratio were both 7.5 times. The stretching temperatures were 108°C in MD and 121°C in TD.

[0145] Then, a 30 wt% aqueous dispersion containing 6 g of dibutyltin dilaurate as a crosslinking catalyst was applied to both sides of the resultant product, and the product was then immersed in warm water maintained at 85°C for 1 hour to complete silane crosslinking. The resultant product was then immersed in methylene chloride at room temperature for 30 minutes to extract liquid paraffin oil, and then dried in an oven at 80°C for 30 minutes to remove the extraction solvent. The results are shown in Table 1.

[0146] Experimental Example (1) Measurement of IR peak intensity The silane crosslinking IR peaks of the surface and inner surfaces of the separation membranes according to Examples 1 to 3 and Comparative Examples 2 and 3 were measured by the following method. Specifically, after preparing a separation membrane specimen, a slope cutting was performed in the thickness direction of the separation membrane at a slope of 1° using a slope cutting analyzer (SAICAS). The cut separation membrane was then divided into 30 equal parts in the thickness direction of the separation membrane and analyzed using a Fourier transform infrared spectrophotometer (FTIR, Agilent Cary620). FIG. 3 shows the results of measuring the silane crosslinking IR peak intensity twice at 30 equal positions in the thickness direction of the separation membrane, and all of the IR peak intensities measured twice were within the range of 0.004 to 0.006 cm. -1 This indicates that the crosslinking reaction occurred uniformly in the thickness direction of the separator of Example 1.

[0147] (2) Measurement of shutdown temperature First, the separators prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were placed in an electrolyte (ethylene carbonate:ethyl methyl carbonate=5:5, LiPF61M). Thereafter, while raising the temperature from 30° C. at a rate of 5° C. / min, the point at which the ionic conductivity became 0 was defined as the shutdown temperature, and the temperature at this point was measured.

[0148] (3) Measurement of meltdown temperature The meltdown temperature was measured by a ThermoMechanical Analyzer (TMA) after taking samples from the porous membrane in the machine direction (MD) and transverse direction (TD). Specifically, a 10 mm long sample was placed in a TMA device (TA Instruments Q400) and exposed to a temperature rise (from 30°C at 5°C / min) with a tension of 19.6 mN applied. The length of the sample changes with increasing temperature, and the temperature at which the length increases rapidly and the sample breaks is measured. MD and TD were measured, and the higher temperature was determined as the meltdown temperature of the sample.

[0149] (4) Measuring the resistance of the separation membrane After the separator was placed in a coin cell (CR2032), a non-aqueous electrolyte (ethylene carbonate: diethyl carbonate = 3:7, LiPF61M) was poured in to prepare a coin cell. After storing the cell at room temperature for 6 hours to ensure that the electrolyte was sufficiently impregnated, the impedance was measured in the range of 10 kHz to 100 kHz using an electrochemical measurement device (multipotentiostat / galvanostat, Ametech Co., Ltd., VersaSTAT4), and the real value of the impedance when the imaginary value of the impedance was 0 was calculated as the resistance using linear interpolation.

[0150] (5) Battery safety evaluation Batteries containing the separators of Examples 1 to 3 and Comparative Examples 1 to 3 were prepared, and the manufactured batteries were fully charged and then subjected to a nail penetration test under GB / T conditions (nail diameter 5 mm, penetration speed 25 mm / sec). If the battery did not ignite within 12 hours after the nail penetration, it was judged to have passed.

[0151] (6) Capacity retention rate evaluation Lithium secondary batteries containing the separators of Examples 1 to 3 and Comparative Examples 1 to 3 were prepared, and the lithium secondary batteries were initially charged and discharged once using an electrochemical charger / discharger. At this time, charging was performed at a current density of 0.1C-rate up to a voltage of 4.3V, and discharging was performed at the same current density up to 2.5V. Such charging and discharging was performed a total of 200 times.

[0152] During the above-mentioned charging and discharging process, the voltage and capacity of the positive and negative electrodes included in each battery were measured.

[0153] The capacity retention rate of each battery was calculated as follows. Capacity retention rate (%) = (Capacity after 200 cycles / Initial capacity) x 100

[0154] (7) Measurement of cross-linking degree The degree of crosslinking (or gel fraction) was measured using a xylene solvent according to ASTM D 2765. Specifically, the separation membrane specimen was immersed in refluxing xylene for 12 hours to dissolve the polymer, and then dried and weighed.

[0155] (8) Measurement of silane (Si) content in the separation membrane First, the separation membrane specimen was reacted with sulfuric acid and sulfurized on a hot plate, after which the sulfuric acid was removed.Then, it was incinerated in an electric furnace (temperature: 600℃) for 4 hours and decomposed into nitric acid and hydrogen peroxide.The specimen was then dissolved transparently and diluted with tertiary ultrapure water to prepare an analysis sample.

[0156] The silane content in the separation membrane was measured using an Axiom model inductively coupled plasma mass spectrometer (ICP-MS, inductively coupled plasma with mass spectrometer, MC-ICP-MS, Axiom is the AXIOM MC model manufactured by Thermo Elemental, UK, and is a form equipped with high resolution capabilities).

[0157] (9) Measurement of cross-link density in the membrane The crosslink density was calculated using the swelling ratio based on the Flory-Huggins theory and the Flory-Rehner equation. The interaction parameter (χ) was calculated based on the Flory-Huggins theory, where the mixing free energy (ΔG) is a function of the polymer volume fraction (υp) and the interaction parameter (χ), and the equilibrium swelling condition is when the mixing free energy is zero (ΔG = 0).

[0158] [Number 1] ΔG = RT {ln(1-υp) + υp + χυp 2} ... Flory-Huggins theory The Flory-Lehner equation was used to determine the crosslink density: where N is the crosslink density (mol / L) and Vs is the molar volume of the solvent (L / mol). [Number 2] -[ln(1-υp) + υp + χυp2 ] = NVs[υp 1 / 3 - υp / 2] … Flory-Lehner formula

[0159] (10) Measurement of tensile strength The separators prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were cut to 15 mm x 100 mm to prepare samples. The prepared samples were pulled in the MD direction at a speed of 500 mm / min according to ASTM-D882, and the strength at the point when the specimen broke was measured.

[0160] (11) Measurement of heat shrinkage rate The heat shrinkage rate was calculated by (initial length-120°C / length after 1 hour of heat shrinkage treatment) / (initial length)×100. [Table 1]

Claims

1. A crosslinked polyolefin separation membrane, The separation membrane comprises a silane-crosslinked polyolefin, The separation membrane has an IR peak of 2847 cm -1 Intensity (D) of IR peak 1030 cm -1 The ratio of the intensities is 0.001 to 0.012, a ratio (C / A) of a silane crosslinking IR peak intensity (C) at a point from one surface of the separation membrane to a 1 / 4 point of the total thickness of the separation membrane to a silane crosslinking IR peak intensity (A) at one surface of the separation membrane is 0.93 to 0.98; The silicon (Si) content in the separation membrane is 150 ppm to 710 ppm; The crosslinked polyolefin separation membrane has a crosslink density (the number of Si-O-Si crosslinking points per unit volume) of 0.040 mol / L or more and 0.048 mol / L or less.

2. A crosslinked polyolefin separation membrane, The separation membrane comprises a silane-crosslinked polyolefin, The separation membrane has an IR peak of 2847 cm -1 Intensity (D) of IR peak 1030 cm -1 The ratio of the intensities is 0.001 to 0.012, the ratio (B / A) of the silane cross-linking IR peak intensity (B) at the center in the thickness direction of the separation membrane to the silane cross-linking IR peak intensity (A) at one surface of the separation membrane is 0.96 to 0.99; The silicon (Si) content in the separation membrane is 150 ppm to 710 ppm; The crosslinked polyolefin separation membrane has a crosslink density (the number of Si-O-Si crosslinking points per unit volume) of 0.040 mol / L or more and 0.048 mol / L or less.

3. The silane crosslinking IR peak is 1030 cm -1 The crosslinked polyolefin separation membrane according to claim 1 or 2,

4. The crosslinked polyolefin separation membrane according to any one of claims 1 to 3, wherein the separation membrane has a gel fraction indicating a degree of crosslinking measured using a xylene solvent according to ASTM D2765 of 15 to 90%.

Citation Information

Patent Citations

  • Porous film, and separator for cell and cell using the same

    JP1997216964A