Anode and method for producing same
The introduction of an auxiliary agent with Si-C and Si-O bonds in the manufacturing process addresses the dispersion issues of negative electrode components, enhancing slurry uniformity and reducing defects in electrochemical devices.
Patent Information
- Application Number
- JP2022519826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-25
AI Technical Summary
The uniform dispersion of negative electrode active materials, dispersants, and binders in electrochemical devices is challenging, leading to non-uniform surface tension, which causes repelling, denting, or shrinkage phenomena, affecting the properties and safety of the electrodes and increasing production costs.
A manufacturing method for negative electrodes that involves adding an auxiliary agent with Si-C and Si-O bonds, mixing with solvents, and applying vibration treatment to improve compatibility and surface tension, resulting in a uniform slurry.
The method enhances the uniformity of the negative electrode slurry, reducing surface defects and improving the quality and safety of electrochemical devices.
Smart Images

Figure 0007575451000005 
Figure 0007575451000006 
Figure 0007575451000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of energy storage, and in particular to anodes and methods for their manufacture. [Background technology]
[0002] With the development of technology and the increasing demand for portable devices, the demand for electrochemical devices (e.g., lithium ion batteries) is increasing significantly. Electrochemical devices with high safety and long life are being investigated.
[0003] During the preparation of the negative electrode of the electrochemical device, the negative electrode active material, the dispersant, the binder, the conductive agent, etc. are dissolved in a solvent to form a negative electrode slurry. However, it is generally difficult to uniformly disperse the negative electrode active material, the dispersant, the binder, the conductive agent, etc., and the surface tension of the negative electrode slurry is non-uniform. The difference in surface tension causes repelling, denting, or shrinkage, which adversely affect the apparent properties of the negative electrode and the properties of the electrochemical device, affect the safety and yield rate of the product, and further increase the production cost.
[0004] In view of this situation, there is a need to provide an improved anode and method for making the same. Summary of the Invention
[0005] SUMMARY OF THE DISCLOSURE Embodiments of the present invention aim to alleviate, to some extent, at least one of the problems existing in the related art by providing a negative electrode and a method for making the same.
[0006] According to one aspect of the present invention, there is provided a method for producing a negative electrode, the method including the step of adding an auxiliary agent having Si-C and Si-O bonds.
[0007] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is mixed with a solvent.
[0008] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is added after the addition of the binder.
[0009] According to some embodiments of the invention, the method comprises the steps of: a mixing step S1 of uniformly mixing a negative electrode active material, a dispersant, a binder, a solvent, and the auxiliary having Si-C and Si-O bonds to obtain a negative electrode slurry; A coating step S2 in which the negative electrode slurry prepared in S1 is coated on a negative electrode current collector at a coating speed of 10 m / min to 100 m / min to obtain an initial electrode piece; The initial electrode piece obtained in S2 is placed in a vacuum drying apparatus and dried at a drying temperature of 80° C. to 150° C., and a drying step S3 is included to obtain the negative electrode.
[0010] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is (a) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (b) the surface tension of an aqueous solution containing 0.1% of the auxiliary having Si-C and Si-O bonds is 30 mN / m or less; It has at least one of the following characteristics.
[0011] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds includes polyether siloxane.
[0012] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds includes at least one of a complex silicone polyether complex, a polyether modified trisiloxane, and a polyether modified silicone polyether siloxane.
[0013] According to some embodiments of the present invention, the negative electrode active material includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-oxygen material, silicon-carbon material, silicon, and tin alloy.
[0014] According to some embodiments of the invention, the solvent is deionized water or N-methylpyrrolidone.
[0015] According to some embodiments of the present invention, in any of steps S1, S2, or S3, a vibration treatment, which is at least one of mechanical vibration and ultrasonic vibration, is performed simultaneously.
[0016] According to some embodiments of the present invention, any of steps S1, S2 or S3 is followed by a vibration treatment, which may be at least one of mechanical vibration and ultrasonic vibration.
[0017] According to some embodiments of the present invention, the vibration treatment has a vibration frequency of 100 Hz to 800 Hz, an amplitude of 0.01 mm to 0.5 mm, and a vibration time of 1 minute to 5 minutes.
[0018] According to some embodiments of the present invention, the vibration process is performed multiple times, and the vibration frequency of at least one of the vibration processes is lower than the vibration frequency of a previous vibration process.
[0019] According to a further aspect of the present invention, there is provided a negative electrode obtained by the method for producing a negative electrode of the present invention.
[0020] According to some embodiments of the present invention, the content of the auxiliary material having Si-C and Si-O bonds in the negative electrode is 500 ppm or less, preferably 300 ppm or less.
[0021] According to some embodiments of the present invention, the negative electrode has a surface contact angle with diethyl carbonate that is reduced by 10% or more compared to a negative electrode prepared without adding an additive having Si-C and Si-O bonds.
[0022] According to a further aspect of the present invention, there is provided an electrochemical device comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode is obtained by the negative electrode manufacturing method of the present invention, or the negative electrode is the negative electrode of the present invention.
[0023] According to a further aspect of the invention there is provided an electronic device comprising an electrochemical device of the invention.
[0024] Other aspects and advantages of embodiments of the invention will be set forth in the following, in part, and / or will be explained by the practice of the embodiments of the invention. [Brief description of the drawings]
[0025] In the following, in order to explain the embodiments of the present invention, the drawings necessary for explaining the embodiments of the present invention or the prior art will be briefly described. It is obvious that the drawings described below are only a part of the embodiments of the present invention. Those skilled in the art can still obtain drawings of other embodiments according to the structures illustrated in these drawings without making creative efforts.
[0026] [Figure 1] FIG. 1 is a surface appearance diagram of the negative electrode of Comparative Example 1. As shown in FIG. [Diagram 2] FIG. 2 is a surface appearance diagram of the negative electrode of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Examples of the present invention will be described in detail below. The examples of the present invention should not be construed as limiting the present invention.
[0028] As used herein, the following terms have the meanings indicated below, unless otherwise specified.
[0029] In the detailed description and claims, a list of terms connected by the term "at least one of" or other similar terminology can mean any combination of the listed terms. For example, if terms A and B are listed, the term "at least one of A and B" means A only, B only, or A and B. In another example, if terms A, B, and C are listed, the term "at least one of A, B, and C" means A only; or B only; C only; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Term A can include a single element or multiple elements. Term B can include a single element or multiple elements. Term C can include a single element or multiple elements. The term "at least one of" has a similar meaning to the term "at least one of."
[0030] In the process of preparing the negative electrode, generally, the negative electrode active material, dispersant, binder, conductive agent, etc. are dissolved in a solvent to form a negative electrode slurry, and then the negative electrode slurry is applied onto a negative electrode current collector and dried to form a negative electrode. Due to poor compatibility between the negative electrode active material and the solvent, the dispersant often does not function well, making it difficult to uniformly disperse the negative electrode active material, dispersant, binder, conductive agent, etc. in the solvent, and the negative electrode slurry cannot be made sufficiently uniform. Non-uniform negative electrode slurry results in non-uniform surface tension. The difference in surface tension causes repelling, denting, or shrinkage (as shown in FIG. 1), which adversely affect the apparent characteristics of the negative electrode and the characteristics of the electrochemical device, affect the safety and yield rate of the product, and further increase the production cost.
[0031] The present invention uses a specific manufacturing method to improve the compatibility between the negative electrode active material and the solvent, and further improve the surface tension of the negative electrode slurry, thereby reducing the phenomenon of cissing, dents, or shrinkage on the negative electrode surface (as shown in FIG. 2), thereby improving the quality of the negative electrode and improving the characteristics of the electrochemical device.
[0032] 1. Negative electrode manufacturing method In one embodiment, the present invention provides a method for producing a negative electrode, comprising the step of adding an auxiliary agent having Si-C and Si-O bonds.
[0033] According to some embodiments of the invention, the method comprises the following steps.
[0034] S1: Mixing step In this step, the negative electrode active material, the dispersant, the binder, the solvent, and the auxiliary having the Si-C and Si-O bonds are uniformly mixed to obtain a negative electrode slurry.
[0035] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is mixed with a solvent.
[0036] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is added after the addition of the binder.
[0037] According to some embodiments of the present invention, the negative electrode active material includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-oxygen material, silicon-carbon material, silicon alloy, and tin alloy.
[0038] According to some embodiments of the invention, the solvent is deionized water or N-methylpyrrolidone.
[0039] According to some embodiments of the invention, the dispersing agent comprises at least one of carboxymethyl cellulose, carboxymethyl cellulose derivatives, alginic acid, alginic acid derivatives, polyacrylic acid, polyacrylic acid derivatives, polyamic acid, polyamic acid derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, starch, starch derivatives, hydroxypropyl cellulose, and hydroxypropyl cellulose derivatives.
[0040] According to some embodiments of the invention, the binder comprises at least one of styrene-butadiene rubber, polyacrylate, polytetrafluoroethylene, polyvinyl alcohol, polyurethane, polyvinylidene fluoride, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, hexafluoropropylene-tetrafluoroethylene copolymer, and vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer.
[0041] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds is (c) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (d) the surface tension of an aqueous solution containing 0.1% of the auxiliary having Si-C and Si-O bonds is 30 mN / m or less.
[0042] In some embodiments, the auxiliary agent having Si-C and Si-O bonds has an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less. In some embodiments, the auxiliary agent having Si-C and Si-O bonds has an oxidation potential of 5 V or more and a reduction potential of 0.3 V or less. The auxiliary agent having the above oxidation / reduction potential has stable electrochemical properties and contributes to improving the cycle and high-temperature storage properties of the electrochemical device.
[0043] In some embodiments, the surface tension of the aqueous solution containing 0.1 wt% of the auxiliary agent having Si-C and Si-O bonds is 30 mN / m or less. In some embodiments, the surface tension of the aqueous solution containing 0.1 wt% of the auxiliary agent having Si-C and Si-O bonds is 25 mN / m or less. In some embodiments, the surface tension of the aqueous solution containing 0.1 wt% of the auxiliary agent having Si-C and Si-O bonds is 20 mN / m or less. In some embodiments, the surface tension of the aqueous solution containing 0.1 wt% of the auxiliary agent having Si-C and Si-O bonds is 15 mN / m or less. In some embodiments, the surface tension of the aqueous solution containing 0.1 wt% of the auxiliary agent having Si-C and Si-O bonds is 10 mN / m or less. When the surface tension of the auxiliary agent having Si-C and Si-O bonds is within the above range, the interface of the negative electrode mixture layer is good.
[0044] The surface tension of the auxiliary having Si-C and Si-O bonds can be measured by the following method: use a JC2000D3E contact angle measuring device to measure the aqueous solution of the auxiliary with a solid content of 1%, measure each sample at least three times, select at least three data, and calculate the average value to obtain the surface tension of the auxiliary.
[0045] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds includes polyether siloxane.
[0046] According to some embodiments of the present invention, the coagent having Si-C and Si-O bonds includes at least one of a complex silicone polyether complex, a polyether modified trisiloxane, and a polyether modified silicone polyether siloxane.
[0047] According to some embodiments of the present invention, the amount of the auxiliary agent having Si-C and Si-O bonds is 3000 ppm or less. In some embodiments, the amount of the auxiliary agent having Si-C and Si-O bonds is 2500 ppm or less. In some embodiments, the amount of the auxiliary agent having Si-C and Si-O bonds is 2000 ppm or less. In some embodiments, the amount of the auxiliary agent having Si-C and Si-O bonds is 1500 ppm or less. In some embodiments, the amount of the auxiliary agent having Si-C and Si-O bonds is 1000 ppm or less. In some embodiments, the amount of the auxiliary agent having Si-C and Si-O bonds is 500 ppm or less. When the amount of the auxiliary agent having Si-C and Si-O bonds is within the above range, the surface tension of the negative electrode slurry can be effectively reduced.
[0048] The ratios of the negative electrode active material, dispersant, binder, solvent, and auxiliary agent having Si-C and Si-O bonds added in this step are not particularly limited as long as they are known ratios that can be used in the process of preparing a negative electrode slurry.
[0049] S2: Coating step In this step, the negative electrode slurry prepared in S1 is applied onto a negative electrode current collector at a coating speed of 10 m / min to 100 m / min to obtain an initial electrode piece.
[0050] S3: Drying step In this step, the initial electrode piece obtained in S2 is placed in a vacuum drying apparatus and dried at a drying temperature of 80° C. to 150° C. to obtain the negative electrode.
[0051] According to some embodiments of the present invention, in any of steps S1, S2, or S3, a vibration treatment, which is at least one of mechanical vibration and ultrasonic vibration, is performed simultaneously. According to some embodiments of the present invention, after any of steps S1, S2, or S3, a vibration treatment, which is at least one of mechanical vibration and ultrasonic vibration, is performed. The vibration treatment can effectively prevent non-uniformity of the negative electrode slurry due to differences in density.
[0052] According to some embodiments of the present invention, the vibration treatment has a vibration frequency of 100 Hz to 800 Hz, an amplitude of 0.01 mm to 0.5 mm, and a vibration time of 1 minute to 5 minutes.
[0053] According to some embodiments of the present invention, the vibration treatment is performed multiple times, and the vibration frequency of at least one of the vibration treatments is lower than the vibration frequency of a previous vibration treatment.
[0054] 2, negative electrode In another embodiment, the present invention provides an anode obtained by the method for producing an anode of the present invention.
[0055] According to some embodiments of the present invention, the content of the auxiliary agent having Si-C and Si-O bonds in the negative electrode is 500 ppm or less. In some embodiments, the content of the auxiliary agent having Si-C and Si-O bonds in the negative electrode is 400 ppm or less. In some embodiments, the content of the auxiliary agent having Si-C and Si-O bonds in the negative electrode is 300 ppm or less. In some embodiments, the content of the auxiliary agent having Si-C and Si-O bonds in the negative electrode is 200 ppm or less.
[0056] According to some embodiments of the present invention, the negative electrode has a surface contact angle with diethyl carbonate that is reduced by more than 10% compared to a negative electrode prepared without adding an additive having Si-C and Si-O bonds (contact angle of more than 70°).
[0057] The contact angle is the contact angle measured within 10 seconds after dropping a drop of diethyl carbonate onto the negative electrode mixture layer. Diethyl carbonate is a commonly used electrolyte solvent. By using diethyl carbonate as a measurement index for the contact angle, the wettability of the electrolyte to the negative electrode mixture layer can be examined. A smaller contact angle of the negative electrode surface with diethyl carbonate indicates improved wettability of the electrolyte to the negative electrode mixture layer and improved liquid retention of the negative electrode mixture layer.
[0058] The contact angle can be measured using an automatic contact angle meter manufactured by Kyowa Interface Science Co., Ltd. The contact angle θ can be determined, for example, by the θ / 2 method. In the θ / 2 method, when the angle between the baseline of the droplet and a straight line passing through the apex and one end point of the droplet is θ′, the contact angle θ=2θ′. Therefore, the contact angle θ can be calculated by measuring θ′ using the distance 2r between the two end points of the baseline of the droplet and the height h of the droplet. At this time, the droplet needs to be dropped in an amount that is not affected by gravity. As the non-aqueous solvent used for contact angle measurement, a commonly used electrolyte solvent such as diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, methyl propyl carbonate, or methyl isopropyl carbonate can be used.
[0059] According to some embodiments of the present invention, the contact angle of the negative electrode active material layer to the non-aqueous solvent is 60° or less. In some embodiments, the contact angle of the negative electrode active material layer to the non-aqueous solvent measured by a contact angle measurement method is 50° or less. In some embodiments, the contact angle of the negative electrode active material layer to the non-aqueous solvent measured by a contact angle measurement method is 30° or less. When the contact angle of the negative electrode active material layer to the non-aqueous solvent is within the above range, defects at the interface of the negative electrode active material layer are reduced, the stability of the electrochemical device in the charge / discharge cycle is improved, and the cycle characteristics of the electrochemical device can be ensured.
[0060] 3, positive electrode There are no particular limitations on the positive electrode, separator, and electrolyte, so long as they are known positive electrodes, separators, and electrolytes used in electrochemical devices (for example, lithium ion batteries).
[0061] The positive electrode that can be used in the embodiments of the present invention has a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The type of the positive electrode active material is not particularly limited as long as it is a known positive electrode active material used in an electrochemical device (for example, a lithium-ion battery). For example, a lithium-containing compound that can impart a high energy density to the electrochemical device can be used. The lithium-containing compound includes one or more of a lithium transition metal composite oxide and a lithium transition metal phosphate compound. The lithium transition metal composite oxide includes lithium and an oxide containing one or more transition metal elements. The lithium transition metal phosphate compound is a phosphate compound containing lithium and one or more transition metal elements. The transition metal element includes one or more of Co, Ni, Mn, and Fe, and these elements enable the electrochemical device to have a higher voltage. The lithium-containing compound is a compound represented by the chemical formula LixM1O2 or LiyM2PO4, where M1 and M2 represent one or more transition metal elements, and the values of x and y change according to the charge / discharge state. Typically, they are in the range of 0.05 ≦ x ≦ 1.10 and 0.05 ≦ y ≦ 1.10. In some embodiments, the lithium transition metal composite oxide includes, but is not limited to, lithium nickel-based transition metal composite oxides represented by LiCoO2, LiNiO2, and LiNi 1-z MzO2 (where M is selected from one or more of Co, Mn, Fe, Al, V, Sn, Mg, Ti, Sr, Ca, Zr, Mo, Tc, Ru, Ta, W, Re, Yb, Cu, Zn, Ba, B, Cr, Si, Ga, P, Sb, and Nb, and z satisfies 0.005 < z < 0.5). In some embodiments, the lithium transition metal phosphate compound includes, but is not limited to, LiFePO4 and a compound represented by the formula LiFe 1-u Mn u PO4 (where u < 1). By using these compounds as the active material of the positive electrode, the obtained electrochemical device has a high battery capacity and excellent cycle characteristics.
[0062] 4. Electrolyte The type of electrolyte is not particularly limited as long as it is a known electrolyte used in electrochemical devices (for example, lithium ion batteries).
[0063] The electrolyte may include any non-aqueous solvent known in the art for use as an electrolyte solvent, including, but not limited to, one or more of cyclic carbonates, linear carbonates, cyclic carboxylic acid esters, linear carboxylic acid esters, cyclic ethers, linear ethers, phosphorus-containing organic solvents, sulfur-containing organic solvents, and aromatic fluorine-containing solvents.
[0064] Examples of the cyclic carbonate include, but are not limited to, one or more of ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate. In some embodiments, the cyclic carbonate has 3 to 6 carbon atoms.
[0065] Examples of the linear carbonate include, but are not limited to, one or more of linear carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate (DEC), methyl-n-propyl carbonate, ethyl-n-propyl carbonate, di-n-propyl carbonate, etc. Examples of the fluorine-substituted linear carbonate include, but are not limited to, one or more of bis(fluoromethyl)carbonate, bis(difluoromethyl)carbonate, bis(trifluoromethyl)carbonate, bis(2-fluoroethyl)carbonate, bis(2,2-difluoroethyl)carbonate, bis(2,2,2-trifluoroethyl)carbonate, 2-fluoroethylmethylcarbonate, 2,2-difluoroethylmethylcarbonate, and 2,2,2-trifluoroethylmethylcarbonate.
[0066] Examples of the cyclic carboxylic acid ester include, but are not limited to, one or more of γ-butyrolactone and γ-valerolactone. In some embodiments, some of the hydrogen atoms of the cyclic carboxylic acid ester may be replaced with fluorine.
[0067] Examples of the chain carboxylic acid ester include, but are not limited to, one or more of methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, sec-butyl acetate, isobutyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, methyl isobutyrate, ethyl isobutyrate, methyl valerate, ethyl valerate, methyl pivalate, and ethyl pivalate. In some embodiments, a portion of the hydrogen atoms of the chain carboxylic acid ester may be substituted with fluorine. In some embodiments, examples of the chain carboxylic acid ester substituted with fluorine include, but are not limited to, methyl trifluoroacetate, ethyl trifluoroacetate, propyl trifluoroacetate, butyl trifluoroacetate, and 2,2,2-trifluoroethyl trifluoroacetate.
[0068] Examples of such cyclic ethers include, but are not limited to, one or more of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 2-methyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and dimethoxypropane.
[0069] Examples of the chain ether include, but are not limited to, one or more of dimethoxymethane, 1,1-dimethoxyethane, 1,2-dimethoxyethane, diethoxymethane, 1,1-diethoxyethane, 1,2-diethoxyethane, ethoxymethoxymethane, 1,1-ethoxymethoxyethane, and 1,2-ethoxymethoxyethane.
[0070] Examples of the phosphorus-containing organic solvent include, but are not limited to, one or more of trimethyl phosphate, triethyl phosphate, dimethylethyl phosphate, methyldiethyl phosphate, ethylenemethyl phosphate, ethyleneethyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl) phosphate, and tris(2,2,3,3,3-pentafluoropropyl) phosphate.
[0071] Examples of the sulfur-containing organic solvent include, but are not limited to, one or more of sulfolane, 2-methylsulfolane, 3-methylsulfolane, dimethylsulfone, diethylsulfone, ethylmethylsulfone, methylpropylsulfone, dimethylsulfoxide, methyl methanesulfonate, ethyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, dimethyl sulfate, diethyl sulfate, and dibutyl sulfate. In some embodiments, some of the hydrogen atoms of the sulfur-containing organic solvent may be replaced with fluorine.
[0072] The aromatic fluorine-containing solvent includes, but is not limited to, one or more of fluorobenzene, difluorobenzene, trifluorobenzene, tetrafluorobenzene, pentafluorobenzene, hexafluorobenzene, and trifluoromethylbenzene.
[0073] In some embodiments, the solvent used in the electrolyte of the present invention includes at least one of cyclic carbonate, linear carbonate, cyclic carboxylic acid ester, and linear carboxylic acid ester. In some embodiments, the solvent used in the electrolyte of the present invention includes at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, n-propyl acetate, and ethyl acetate. In some embodiments, the solvent used in the electrolyte of the present invention includes at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, and γ-butyrolactone.
[0074] The electrolyte used in the electrolyte solution of the embodiment of the present invention is, for example, an inorganic lithium salt such as LiClO4, LiAsF6, LiPF6, LiBF4, LiSbF6, LiSO3F, LiN(FSO2)2; for example, LiCF3SO3, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium cyclic 1,3-hexafluoropropane disulfonimide, lithium cyclic 1,2-tetrafluoroethane disulfonimide, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiPF4(CF3)2, LiPF4 Fluorine-containing organic lithium salts such as (C2F5)2, LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2; dicarboxylic acid-containing complex lithium salts such as lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium tris(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate, but are not limited thereto. The electrolytes described above may be used alone or in combination of two or more. For example, in some embodiments, the electrolyte includes a combination of LiPF6 and LiBF4. In some embodiments, the electrolyte comprises a combination of an inorganic lithium salt, such as LiPF6 or LiBF4, and a fluorine-containing organic lithium salt, such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, etc. In some embodiments, the concentration of the electrolyte is in the range of 0.8-3 mol / L, e.g., in the range of 0.8-2.5 mol / L, in the range of 0.8-2 mol / L, in the range of 1-2 mol / L, or, for example, 1 mol / L, 1.15 mol / L, 1.2 mol / L, 1.5 mol / L, 2 mol / L, or 2.5 mol / L.
[0075] 5. Separator The type of separator is not particularly limited as long as it is a known separator used in electrochemical devices (for example, lithium ion batteries).
[0076] The separator that can be used in the embodiment of the present invention includes a polymer or an inorganic material formed from a material stable to the electrolyte of the present invention. For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a nonwoven fabric, a membrane, or a composite membrane having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene glycol terephthalate, and polyimide. Specifically, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane can be selected and used.
[0077] A surface treatment layer is provided on at least one surface of the base layer. The surface treatment layer may be a polymer layer or an inorganic layer, or may be a layer obtained by mixing a polymer and an inorganic material.
[0078] The inorganic layer includes inorganic particles and a binder, the inorganic particles include one or more of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium oxide, tin oxide, cerium oxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate, and the binder includes one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylic acid ester, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene.
[0079] The polymer layer includes a polymer, the polymeric material including at least one of polyamide, polyacrylonitrile, acrylic ester polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(polyvinylidene fluoride-hexafluoropropylene).
[0080] 6. Electrochemical equipment The electrochemical device of the present invention includes any device in which an electrochemical reaction can occur, and specific examples thereof include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery. In some embodiments, the electrochemical device of the present invention includes a positive electrode piece having a positive electrode active material capable of absorbing and releasing metal ions, a negative electrode according to the embodiments of the present invention, an electrolyte, and a separator disposed between the positive electrode and the negative electrode.
[0081] 7, electronic equipment The use of the electrochemical device of the present invention is not particularly limited, and may be used in any electronic device known in the prior art. In some embodiments, the electrochemical device of the present invention is used in, but is not limited to, notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, mobile fax machines, mobile copy machines, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, portable cleaners, portable CD players, mini CDs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, automobiles, motorcycles, auxiliary bicycles, bicycles, lighting equipment, toys, game equipment, watches, power tools, strobes, cameras, large-scale household storage batteries, and lithium ion capacitors.
[0082] Hereinafter, the preparation of a lithium ion battery is described with reference to specific examples, and those skilled in the art should understand that the preparation method described in the present invention is merely exemplary, and any other suitable preparation method is within the scope of the present invention.
[0083] Working Example Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples and comparative examples. However, the embodiments of the present invention are not limited to these examples.
[0084] 1. Preparation of lithium-ion batteries 1. Preparation of the negative electrode S1: Mixing step Artificial graphite, styrene-butadiene rubber, and carboxymethyl cellulose were mixed with deionized water in a mass ratio of 96%:3%:1%, and the order of addition was as follows: Step 1. Artificial graphite and carboxymethyl cellulose Step 2. Deionized water Step 3. Carboxymethylcellulose Step 4. Styrene-butadiene rubber
[0085] As described below, in the examples, 2000 ppm of an auxiliary agent having Si-C and Si-O bonds was added, while in the comparative examples, no auxiliary agent was added or 2000 ppm of an auxiliary agent having no Si-C and Si-O bonds was added. The auxiliary agents having Si-C and Si-O bonds used in the examples of the present invention are as shown in the table below.
[0086] JPEG0007575451000001.jpg39131
[0087] The components were mixed uniformly to obtain a negative electrode slurry.
[0088] S2: Coating step The negative electrode slurry prepared in S1 was applied onto a 12 μm copper foil at a coating speed of 10 m / min to 100 m / min to obtain an initial pole piece.
[0089] S3: Drying step The initial electrode piece obtained in S2 was placed in a vacuum drying apparatus and dried at a drying temperature of 80 to 150° C. to obtain a negative electrode.
[0090] 2. Preparation of the positive electrode Lithium cobalt oxide (LiCoO2), conductive material (Super-P), and polyvinylidene fluoride (PVDF) were mixed with N-methylpyrrolidone (NMP) in a mass ratio of 95%:2%:3% and stirred uniformly to obtain a positive electrode slurry. The positive electrode slurry was applied to 12μm aluminum foil, dried, cold pressed, punched out, and tabs were welded to obtain a positive electrode.
[0091] 3. Preparation of electrolyte In a dry argon gas atmosphere, EC, PC and DEC (weight ratio 1:1:1) were mixed, LiPF6 was added and mixed uniformly to obtain an electrolyte solution. The concentration of LiPF6 in the electrolyte solution was 1.15 mol / L.
[0092] 4. Preparation of the separator A polyethylene (PE) porous polymer membrane was used as the separator.
[0093] 5. Preparation of Lithium-ion Battery The obtained positive electrode, separator, and negative electrode were wound in this order, and placed on an exterior foil, leaving an inlet for injecting electrolyte. The inlet was then sealed, and a lithium-ion battery was obtained through processes such as formation and test capacity.
[0094] II. Method for detecting defects on the surface of negative electrodes of lithium-ion batteries The pole piece after cold pressing was scanned and photographed using a CCD scanner, and the defects were identified using the gray level differences at different positions. Area 0.2mm 2 Any location where the gradation level difference is greater than 10 is regarded as a pole piece defect, and the number of defects is counted.
[0095] 3. Measurement results Table 1 shows the effect of additives and their addition order on defects on the negative electrode surface of lithium ion batteries.
[0096] [Table 1]
[0097] As shown in Comparative Example 1, when the negative electrode was prepared, no auxiliary was added, so the number of defects on the negative electrode surface was large. As shown in Examples 1 to 5, when the negative electrode was prepared, the surface tension of the negative electrode slurry was significantly improved by adding an auxiliary having Si-C and Si-O bonds, and the number of defects on the negative electrode surface was significantly reduced. Regarding the addition of an auxiliary during the preparation of the negative electrode, when the auxiliary having Si-C and Si-O bonds was mixed with a solvent, when the auxiliary having Si-C and Si-O bonds was mixed with a binder, and when the auxiliary having Si-C and Si-O bonds was added after the binder was added, the number of defects on the negative electrode surface was extremely reduced. Figures 1 and 2 show pole pieces obtained in Comparative Example 1 and Example 2, respectively. In Figure 1, the positions where the color difference is noticeable (for example, the positions indicated by the black circles in Figure 1) are defective parts of the pole pieces, and in Figure 2, there are almost no spots of color difference.
[0098] Table 2 shows the effect of different additives on the defects on the negative electrode surface of a lithium-ion battery. In the examples in Table 2, each additive was mixed with deionized water in step 2.
[0099] [Table 2]
[0100] As shown in Comparative Examples 2 to 4, the number of defects on the negative electrode surface was not significantly improved even when a typical organic solvent (e.g., ethanol, acetone, or ethylene carbonate, which does not have Si-C and Si-O bonds) was added as an auxiliary during preparation of the negative electrode. As shown in Examples 2 and 6 to 9, the surface tension of the negative electrode slurry can be significantly reduced and the number of defects on the negative electrode surface can be significantly reduced by adding an auxiliary having Si-C and Si-O bonds during preparation of the negative electrode.
[0101] Table 3 shows the effects of coating speed, drying temperature and vibration treatment on defects on the surface of the negative electrode of a lithium ion battery. In the examples in Table 3, the auxiliary agent 1 was mixed with deionized water in step 2. The vibration treatment is performed by ultrasonic treatment after step S2.
[0102] [Table 3]
[0103] The results show that the number of defects on the negative electrode surface can be further reduced by setting the coating speed to 10 m / min to 100 m / min and the drying temperature to 80° C. to 150° C. The number of defects on the negative electrode surface can be further reduced by setting the coating speed to 20 m / min to 100 m / min and the drying temperature to 80° C. to 150° C. In particular, a higher effect can be obtained when vibration treatment is added.
[0104] Throughout the specification, references to "embodiments," "some embodiments," "one embodiment," "another embodiment," "an example," "embodiment," or "several examples" mean that at least one embodiment or example of the invention includes a particular feature, structure, material, or characteristic described in that embodiment or example. Thus, the appearances of, for example, "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in one example," "in a particular example," or "an example" in various places throughout the specification do not necessarily refer to the same embodiment or example of the invention. Furthermore, particular features, structures, materials, or characteristics herein may be combined in any suitable manner in one or more embodiments or examples.
[0105] Although illustrative embodiments have been disclosed and described, those skilled in the art should understand that the above-described embodiments are not to be construed as limiting the present invention, and that modifications, substitutions, and alterations to the embodiments are possible without departing from the spirit, principle, and scope of the present invention.
Claims
1. A method for producing a negative electrode, comprising the steps of: The method for producing the negative electrode includes the steps of: A negative electrode active material, a dispersant, a binder, and a solvent are mixed to obtain a mixed solution, and then an auxiliary agent having Si-C and Si-O bonds is added to the mixed solution and mixed uniformly to obtain a negative electrode slurry, the auxiliary agent including polyether siloxane, or After mixing the negative electrode active material and the dispersant, a mixture of the auxiliary agent having Si-C and Si-O bonds and a solvent is added to obtain a mixed liquid, and then the dispersant and binder are added to the mixed liquid and mixed uniformly to obtain a negative electrode slurry; A mixing step S1; A coating step S2 of coating the negative electrode slurry prepared in S1 onto a negative electrode current collector at a coating speed of 10 m / min to 100 m / min to obtain an initial electrode piece; A drying step S3 in which the initial electrode piece obtained in S2 is placed in a vacuum drying apparatus and dried at a drying temperature of 80° C. to 150° C. to obtain the negative electrode; The negative electrode active material is artificial graphite, the solvent is deionized water; The dispersant is carboxymethyl cellulose, The method for producing a negative electrode, wherein the binder is styrene-butadiene rubber.
2. The auxiliary agent having Si—C and Si—O bonds is (a) an oxidation potential of 4.5 V or more and a reduction potential of 0.5 V or less; (b) the surface tension of an aqueous solution containing 0.1% of the auxiliary having Si-C and Si-O bonds is 30 mN / m or less; The method for producing a negative electrode according to claim 1 , wherein the negative electrode is formed of a material selected from the group consisting of fluorine, fluorine, arsenic ...
3. The method for producing a negative electrode according to claim 1, wherein the auxiliary agent having Si-C and Si-O bonds includes at least one of a composite silicone polyether composite and a polyether modified trisiloxane.
4. 2. The method for producing a negative electrode according to claim 1, wherein the auxiliary having Si—C and Si—O bonds is selected from the group consisting of trisiloxane surfactants, silicone surfactants, dihydroxypolydimethylsiloxanes, N-β-aminoethyl-Y-aminopropyldimethoxymethylsilanes, and methylsilicone oil polydimethylsiloxanes.
5. 2. The method for producing a negative electrode according to claim 1, wherein the amount of the auxiliary having Si--C and Si--O bonds added is 3000 ppm or less.
6. The method for producing a negative electrode according to claim 1 , wherein a vibration treatment of at least one of mechanical vibration and ultrasonic vibration is simultaneously performed in any one of steps S1, S2, and S3.
7. The method for producing a negative electrode according to claim 1 , further comprising the step of performing a vibration treatment, which is at least one of mechanical vibration and ultrasonic vibration, after any one of steps S1, S2 and S3.
8. The method for producing a negative electrode according to claim 6 or 7, wherein the vibration treatment has a vibration frequency of 100 Hz to 800 Hz, an amplitude of 0.01 mm to 0.5 mm, and a vibration time of 1 minute to 5 minutes.
9. The method for producing a negative electrode according to claim 6 or 7, wherein the vibration treatment is performed a plurality of times, and the vibration frequency of at least one of the vibration treatments is lower than the vibration frequency of a previous vibration treatment.
Citation Information
Patent Citations
Method for preparing lithium ion battery negative pole piece
CN106848202A
Lithium ion battery cathode slurry and preparation method thereof
CN109037676A
Controller of synchronous motor
JP1986052177A
Lithium-ion battery negative electrode additive and method for producing the same, lithium-ion battery negative electrode sheet and lithium-ion battery
JP2015523699A
Anode slurry for lithium-ion batteries
JP2019535110A